Block copolymer, and production method of the same, as well as resin composition comprising the same
A benzotriazole-based block copolymer with alkane chain and UV-absorbing blocks addresses photostability and bleed-out issues, providing enhanced UV absorption and durability in resin compositions.
Patent Information
- Application Number
- JP2023062938
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing ultraviolet absorbers for resins face issues with poor long-term photostability, bleed-out, and compatibility, particularly in high humidity environments, leading to appearance defects and insufficient ultraviolet absorption in the long-wave region.
A block copolymer is developed with specific monomers (A and B) that are benzotriazole-based, featuring a polymer block (A) with an alkane chain and a UV-absorbing block (B), produced through living polymerization, ensuring high molecular weight and compatibility with resins like polyolefins, thereby preventing bleed-out and enhancing UV absorption in the 300 to 400 nm range.
The block copolymer exhibits excellent UV absorption in the long-wave region and remains stable in high humidity conditions, maintaining long-term weather resistance and preventing surface bleed-out, thus improving the appearance and durability of resin compositions.
Smart Images

Figure 2024149206000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel block copolymer, a method for producing the same, and a resin composition containing the same. [Background technology]
[0002] In order to improve light shielding properties and light resistance, resin articles are usually added with ultraviolet absorbents and light stabilizers. Such ultraviolet absorbents and light stabilizers with various chemical structures are commercially available. In particular, as the ultraviolet absorbent, inorganic ultraviolet absorbents and organic ultraviolet absorbents may be used.
[0003] Inorganic ultraviolet absorbers are described in, for example, Patent Documents 1 to 3. Inorganic ultraviolet absorbers are excellent in durability such as weather resistance and heat resistance, but the degree of freedom of selection is limited because the absorption wavelength is determined by the band gap of the compound, and there is no inorganic ultraviolet absorber that can absorb up to the long-wave ultraviolet (UV-A) region of 320 to 400 nm without absorbing visible light. Inorganic ultraviolet absorbers that absorb long-wave ultraviolet rays are accompanied by coloring because they have absorption up to the visible region.
[0004] On the other hand, organic ultraviolet absorbers have a high degree of freedom in the design of the absorber structure, so that various absorption wavelengths can be obtained by devising the absorber structure. Up to now, systems using various organic ultraviolet absorbers such as benzotriazole-based, benzophenone-based, triazine-based, and cyan-based have been studied, and when absorbing up to the long-wave ultraviolet region, two methods have been considered: using one with a maximum absorption wavelength in the long-wave ultraviolet region, or increasing the concentration. However, those with a maximum absorption wavelength in the long-wave ultraviolet region described in Patent Documents 4 and 5, etc., have poor light resistance and their absorption ability decreases over time. On the other hand, benzotriazole-based ultraviolet absorbers have relatively good light resistance, and by increasing the concentration, they can relatively clearly cut up to the long-wave region (see Patent Document 6, for example).
[0005] However, since these organic ultraviolet absorbents generally have low molecular weights, when added at high concentrations, they may precipitate over time from the surface of a resin article, or may be eluted in the environment of use by rain or water containing detergent, etc. For this reason, it is known that resin articles containing organic ultraviolet absorbents deteriorate the appearance of the product over time, and it is difficult to impart long-term photostability to the product.
[0006] To solve such problems, a method has been developed in which a curable resin is laminated on the layer on the surface side of the ultraviolet absorbent-containing layer to suppress the elution and precipitation (hereinafter also referred to as "bleed-out") of the ultraviolet absorbent. For example, Patent Document 7 proposes a method of laminating a photocurable acrylic resin. However, this attempt has the disadvantages that there are limitations on the type of resin used and that it can only be applied to multi-layer products.
[0007] In order to solve such problems, an ultraviolet absorber made of a bisbenzotriazolylphenol compound having two addition polymerization side chains has been developed (Patent Document 8). Since this compound has two addition polymerization side chains, it functions as both an ultraviolet absorber and a crosslinking agent. Since this compound has a carbamoyloxy unit in the molecule, it is said that the compound imparts flexibility to a cured resin using the compound as a crosslinking agent. However, the compound described in Patent Document 8 is prone to bleeding out in a usage environment where moisture is present, which may impair the appearance of the product, and there is still a problem with weather resistance, i.e., long-term sustainability of light stability in a usage environment where the compound is simultaneously affected by light and moisture.
[0008] Furthermore, in order to solve such problems, attempts have been made to give a group having a polymerizable double bond such as a vinyl group to an ultraviolet absorber, polymerize the resulting compound to increase its molecular weight, and improve compatibility with the resin to prevent the ultraviolet absorber from volatilizing, thermally decomposing, seeping out, etc. (Patent Documents 9 to 11). However, these ultraviolet absorbing polymers also have the following drawbacks, and there is still room for improvement. That is, depending on the type of resin to which they are added, the compatibility is insufficient, which reduces the transparency of the resin. This tendency is particularly noticeable in non-polar thermoplastic resins such as polyolefins. In addition, they are still unsatisfactory in terms of long-term light resistance. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 5-339033 [Patent Document 2] Japanese Patent Application Publication No. 5-345639 [Patent Document 3] Japanese Patent Application Publication No. 6-56466 [Patent Document 4] Japanese Patent Application Publication No. 6-145387 [Patent Document 5] JP 2003-177235 A [Patent Document 6] JP 2005-517787 A [Patent Document 7] Patent Application No. 2013-523010 [Patent Document 8] JP 2004-2317 A [Patent Document 9] Japanese Patent Application Publication No. 60-38411 [Patent Document 10] Japanese Patent Publication No. 181360 / 1983 [Patent Document 11] Japanese Patent Application Publication No. 3-281685 Summary of the Invention [Problem to be solved by the invention]
[0010] The object of the present invention, which has been made in consideration of the above-mentioned conventional problems, is to provide a block copolymer that has excellent ultraviolet absorption properties in the long-wave ultraviolet region of 300 to 400 nm and is unlikely to bleed out even when contained in a resin such as a polyolefin and exposed to a high-humidity environment, and a resin composition containing the same. [Means for solving the problem]
[0011] As a result of intensive research, the present inventors have found that the following invention meets the above-mentioned object, and have completed the present invention. [1] A block copolymer comprising: a polymerization block (A) having a repeating unit derived from a monomer (A) selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, the monomer (A) having an alkane chain having 8 or more carbon atoms; and a polymerization block (B) having a repeating unit derived from a monomer (B) which is a benzotriazole-based monomer represented by the following general formula (1): [ka] (In the above general formula (1), R 1 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, R 2 represents a linear or branched alkylene group having 1 to 6 carbon atoms; R 3 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, a halogen group, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group. [2] The block copolymer according to [1], characterized in that the block copolymer has crystallinity. [3] The block copolymer according to [1] or [2], wherein the monomer (A) is one selected from the group consisting of stearyl acrylate, behenyl acrylate, hexadecyl acrylate, and lauryl acrylate. [4] The block copolymer according to any one of [1] to [3], containing the monomer (A) in an amount of 35 to 95% by mass relative to 100% by mass of the block copolymer. [5] The block copolymer according to any one of [1] to [4], having a number average molecular weight of 2,000 to 20,000. [6] The block copolymer according to any one of [1] to [5], having a molecular weight distribution (Mw / Mn) of 2.5 or less. [7] A method for producing the block copolymer according to any one of [1] to [6], comprising: a monomer (A) polymerization step of subjecting a monomer (A) having an alkane chain having 8 or more carbon atoms, the monomer (A) being one selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, to living polymerization to obtain a polymerization block (A) having a repeating unit derived from the monomer (A); and a monomer (B) polymerization step of subjecting the polymerization block (A) to living polymerization with a monomer (B) which is a benzotriazole-based monomer represented by the following general formula (1), to obtain a copolymer comprising the polymerization block (A) and a polymerization block (B) having a repeating unit derived from the monomer (B). [ka] (In the above general formula (1), R 1 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, R 2 represents a linear or branched alkylene group having 1 to 6 carbon atoms; R 3 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, a halogen group, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group. [8] A method for producing the block copolymer according to any one of [1] to [6], comprising: a monomer (B) polymerization step of subjecting a monomer (B), which is a benzotriazole-based monomer represented by the following general formula (1), to living polymerization to obtain a polymerization block (B) having a repeating unit derived from the monomer (B); and a monomer (A) polymerization step of subjecting the polymerization block (B) to living polymerization, the monomer (A) being one selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, having an alkane chain having 8 or more carbon atoms, to obtain a copolymer comprising the polymerization block (A) having a repeating unit derived from the monomer (A) and the polymerization block (B). [ka] (In the above general formula (1), R 1 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, R 2 represents a linear or branched alkylene group having 1 to 6 carbon atoms; R 3 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, a halogen group, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group. [9] An ultraviolet absorbent comprising the block copolymer according to any one of [1] to [6].
[10] A resin composition comprising the block copolymer according to any one of [1] to [6] and a resin.
[11] The resin composition according to
[10] , wherein the resin is a polyolefin.
[12] The resin composition according to
[10] or
[11] , wherein the resin is polyethylene and / or cyclic polyolefin.
[13] The resin composition according to any one of
[10] to
[12] , wherein the content of the block copolymer is 0.5 to 3.0 mass% relative to 100 mass% of the resin composition, and the content of the resin is 97.0 to 99.5 mass% relative to 100 mass% of the resin composition.
[14] The resin composition according to any one of
[10] to
[13] , characterized in that the ultraviolet ray transmittance at a wavelength of 340 nm is 5% or less, and the block copolymer does not bleed out to the surface when left to stand for 28 days in an atmosphere having a temperature of 40°C and a relative humidity of 75%. Effect of the Invention
[0012] According to the present invention, it is possible to provide a block copolymer that has excellent ultraviolet absorption in the long-wave ultraviolet region of 300 to 400 nm and is unlikely to bleed out even when contained in a resin such as a polyolefin and exposed to a high-humidity environment, and a resin composition containing the same. Furthermore, the resin composition of the present invention containing such a block copolymer has excellent long-term weather resistance and can suppress poor appearance caused by bleeding out of the block copolymer. [Brief description of the drawings]
[0013] [Figure 1] 1 is an image of the film of Example 1 observed by an optical microscope. [Diagram 2] 1 is an image of the film of Comparative Example 1 observed by an optical microscope. [Diagram 3] 1 is an image of the film of Comparative Example 2 observed by an optical microscope. [Figure 4] 1 is an image of the film of Comparative Example 3 observed by an optical microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] An embodiment of the present invention will be described below.
[0015] The block copolymer of the present embodiment is a copolymer having a polymerization block (A) and a polymerization block (B). The polymerization block (A) is a polymerization block (polymer) that is likely to have a structure exhibiting crystallinity, and the polymerization block (B) is a polymerization block (polymer) that has a structure exhibiting an ultraviolet absorbing effect in the long-wave ultraviolet region of 300 to 400 nm (hereinafter also simply referred to as the "long-wave ultraviolet region"). The copolymer of the present embodiment that contains such a polymerization block can form a portion where a part of the copolymer interpenetrates a resin such as a polyolefin to which the copolymer is added.
[0016] The polymerization block (A) contained in the block copolymer of this embodiment has a repeating unit (structural unit) derived from a monomer (A) having an alkane chain with 8 or more carbon atoms. The polymerization block (B) contained in the copolymer of this embodiment has a repeating unit (structural unit) derived from a monomer (B) that is an ultraviolet absorbing monomer. In other words, the polymerization block (A) is a polymer of the monomer (A) having an alkane chain with 8 or more carbon atoms (polymer of monomer (A)), and the polymerization block (B) is a polymer of the monomer (B) that is an ultraviolet absorbing monomer (polymer of monomer (B)). The copolymer of this embodiment is a block copolymer of the polymer of the monomer (A) and the polymer of the monomer (B).
[0017] First, the polymer block (A) contained in the copolymer of the present embodiment will be specifically described.
[0018] The polymer block (A) is a polymer block having a repeating unit derived from a monomer (A) having an alkane chain having 8 or more carbon atoms. The monomer (A) relating to the repeating unit of the polymer block (A) is one monomer having an alkane chain having 8 or more carbon atoms and selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene.
[0019] The (meth)acrylate having an alkane chain having 8 or more carbon atoms is a compound represented by the following general formula (2): When the monomer (A) is a (meth)acrylate having an alkane chain having 8 or more carbon atoms (hereinafter also simply referred to as "(meth)acrylate"), the polymer block (A) has a repeating unit represented by the following general formula (3). [ka] [ka] In the general formulas (2) and (3), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group having 8 or more carbon atoms, and n represents an integer of 2 or more.
[0020] The (meth)acrylamide having an alkane chain with 8 or more carbon atoms is a compound represented by the following general formula (4): When the monomer (A) is a (meth)acrylamide having an alkane chain with 8 or more carbon atoms, the polymer block (A) has a repeating unit represented by the following general formula (5). [ka] [ka] In the general formulas (4) and (5), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group having 8 or more carbon atoms, and R 6 represents a hydrogen atom or an alkyl group, and n represents an integer of 2 or more.
[0021] The vinyl ether having an alkane chain with 8 or more carbon atoms is a compound represented by the following general formula (6): When the monomer (A) is a vinyl ether having an alkane chain with 8 or more carbon atoms, the polymer block (A) has a repeating unit represented by the following general formula (7). [ka] [ka] In the general formulas (6) and (7), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group having 8 or more carbon atoms, and n represents an integer of 2 or more.
[0022] The vinyl ester having an alkane chain with 8 or more carbon atoms is a compound represented by the following general formula (8): When the monomer (A) is a vinyl ester having an alkane chain with 8 or more carbon atoms, the polymer block (A) has a repeating unit represented by the following general formula (9). [ka] [ka] In the general formulas (8) and (9), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group having 8 or more carbon atoms, and n represents an integer of 2 or more.
[0023] The siloxane having an alkane chain with 8 or more carbon atoms is a compound represented by the following general formula (10): When the monomer (A) is a siloxane having an alkane chain with 8 or more carbon atoms, the polymer block (A) has a repeating unit represented by the following general formula (11). [ka] [ka] In the general formulas (10) and (11), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group having 8 or more carbon atoms, and n represents an integer of 2 or more.
[0024] The α-olefin having an alkane chain with 8 or more carbon atoms is a compound represented by the following general formula (12): When the monomer (A) is an α-olefin having an alkane chain with 8 or more carbon atoms (hereinafter also simply referred to as "α-olefin"), the polymer block (A) has a repeating unit represented by the following general formula (13). [ka] [ka] In the general formulas (12) and (13), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group having 8 or more carbon atoms, and n represents an integer of 2 or more.
[0025] The substituted styrene having an alkane chain with 8 or more carbon atoms is a compound represented by the following general formula (14): When the monomer (A) is a substituted styrene having an alkane chain with 8 or more carbon atoms, the polymer block (A) has a repeating unit represented by the following general formula (15). [ka] [ka] In the general formulas (14) and (15), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group having 8 or more carbon atoms, and n represents an integer of 2 or more.
[0026] In the above general formulas (2) to (15), n may be an integer of 2 or more, and may be appropriately determined in a range that does not impair compatibility with the resin, depending on the length of the alkyl group having 8 or more carbon atoms (alkane chain having 8 or more carbon atoms), the sequence of the monomer (A) and the monomer (B), the degree of polymerization, etc. From the viewpoint that the block copolymer of the present embodiment is more likely to have a structure that exhibits crystallinity and is more likely to be compatible with the resin, n is more preferably 5 or more, and even more preferably 10 or more. The upper limit of n may be appropriately set in a range that does not impair the effects of the present invention, and may be, for example, 1000 or less, 800 or less, or 500 or less.
[0027] In the above general formulas (4) and (5), R 6 represents a hydrogen atom or an alkyl group. The number of carbon atoms in the alkyl group in the above general formulas (4) and (5) is not particularly limited, but from the viewpoint that the block copolymer of the present embodiment is more likely to have a structure exhibiting crystallinity, the number of carbon atoms in the alkyl group is preferably 1 to 3.
[0028] As described above, the monomer (A) has an alkane chain having 8 or more carbon atoms. In other words, the alkane chain having 8 or more carbon atoms is an alkyl group having 8 or more carbon atoms, and R 5 The block copolymer of the present embodiment is easily crystalline because the monomer (A) has an alkane chain having 8 or more carbon atoms, and is easily able to interact with resins such as polyolefins. This makes the block copolymer of the present embodiment more compatible with resins. The fact that the block copolymer has crystallinity can be confirmed by measuring the melting point and the heat of fusion using a differential scanning calorimeter (DSC). If the melting point and heat of fusion can be measured using a differential scanning calorimeter (DSC), it can be determined that the block copolymer has crystallinity.
[0029] The alkane chain having 8 or more carbon atoms (alkyl group having 8 or more carbon atoms) is, in other words, a linear, branched, or cyclic alkyl group having 8 or more carbon atoms, and among these, a linear alkyl group having 8 or more carbon atoms is preferable. Furthermore, the alkane chain having 8 or more carbon atoms (alkyl group having 8 or more carbon atoms) is preferably a decyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group (stearyl group), or a docosyl group (behenyl group) among linear groups. When the alkane chain having 8 or more carbon atoms (alkyl group having 8 or more carbon atoms) is linear, the block copolymer of the present embodiment is more likely to have a structure that exhibits crystallinity, and the block copolymer of the present embodiment is more likely to be compatible with resins such as polyolefins.
[0030] The alkane chain having 8 or more carbon atoms (alkyl group having 8 or more carbon atoms) possessed by monomer (A) may have 8 or more carbon atoms, but since the block copolymer of the present embodiment is more likely to have a structure exhibiting crystallinity and the interaction between the block copolymer and resins such as polyolefins can be further improved, the alkane chain is preferably an alkane chain having 12 or more carbon atoms, and more preferably an alkane chain having 16 or more carbon atoms. Note that this alkane chain is preferably a linear alkane chain.
[0031] The alkane chain having 8 or more carbon atoms contained in monomer (A) may have any number of carbon atoms, but since this makes it easier for the copolymer to have an appropriate three-dimensional structure and improves interpenetration with resins such as polyolefins, the alkane chain is preferably an alkane chain having 50 or less carbon atoms, more preferably an alkane chain having 40 or less carbon atoms, and even more preferably an alkane chain having 30 or less carbon atoms. In addition, when the alkane chain has 50 or less carbon atoms, it becomes easier to set the polymerization conditions for producing a block copolymer.
[0032] The monomer (A) relating to the repeating unit of the polymer block (A) is preferably a (meth)acrylate (compound represented by the above general formula (2)) or an α-olefin (compound represented by the above general formula (12)) among the above-mentioned monomers (A) from the viewpoint of further increasing the ultraviolet absorbing property in the long-wave ultraviolet region of 300 to 400 nm and further suppressing bleeding out from the resin. In other words, the polymer block (A) preferably has either a repeating unit derived from a (meth)acrylate (repeating unit represented by the above general formula (3)) or a repeating unit derived from an α-olefin (repeating unit represented by the above general formula (13)) among the above-mentioned repeating units.
[0033] Among the above-mentioned monomers (A), it is more preferable that the monomer (A) is a (meth)acrylate (a compound represented by the above general formula (2)) from the viewpoints of ease of obtaining the monomer, ease of controlling the polymerization conditions, ease of interaction between alkane chains having 8 or more carbon atoms, etc. In other words, it is more preferable that the polymer block (A) has a repeating unit derived from a (meth)acrylate (a repeating unit represented by the above general formula (3)) among the above-mentioned repeating units. Specific examples of the (meth)acrylate represented by the above general formula (2) include hexadecyl acrylate, dodecyl acrylate (lauryl acrylate), dodecyl methacrylate (lauryl methacrylate), octadecyl acrylate (stearyl acrylate), octadecyl methacrylate (stearyl methacrylate), docosyl acrylate (behenyl acrylate), docosyl methacrylate (behenyl methacrylate), etc. From the viewpoint of further enhancing the ultraviolet absorbency in the long-wave ultraviolet region and further suppressing bleeding out from the resin, it is preferable that the monomer (A) is one selected from the group consisting of octadecyl acrylate (stearyl acrylate), docosyl acrylate (behenyl acrylate), hexadecyl acrylate, and dodecyl acrylate (lauryl acrylate) among (meth)acrylates (compounds represented by the above general formula (2)).
[0034] The content of monomer (A) in the copolymer (content of polymer block (A)) is preferably 35 to 95% by mass, more preferably 38 to 85% by mass, and particularly preferably 40 to 80% by mass, based on 100% by mass of the copolymer of this embodiment. By setting the content of monomer (A) to 35% by mass or more, the block copolymer of this embodiment is more likely to have a more crystalline structure and is more likely to be compatible with resins such as polyolefins. Note that, by setting the content of monomer (A) to 95% by mass or less, it is more likely to achieve both ultraviolet absorbing properties and compatibility with resins such as polyolefins.
[0035] The block copolymer of the present embodiment may have at least one of the above-mentioned polymerization blocks (A), and may have two or more polymerization blocks (A). When the block copolymer has two or more polymerization blocks (A), the monomers (A) related to the repeating units between the two or more polymerization blocks (A) may be the same or different. When the block copolymer has two or more polymerization blocks (A), the polymerization degrees of the two or more polymerization blocks (A) may be different or the same from each other.
[0036] Next, the polymer block (B) contained in the block copolymer of the present embodiment will be described.
[0037] Polymer block (B) is a polymer block having a repeating unit derived from monomer (B). Monomer (B) relating to the repeating unit of polymer block (B) is a benzotriazole-based monomer (ultraviolet absorbing monomer) represented by the following general formula (1). The repeating unit derived from the benzotriazole-based monomer represented by the following general formula (1) (i.e., monomer (B)) is represented by the following general formula (16). [ka] [ka] In the above general formulas (1) and (16), R 1represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, R 2 represents a linear or branched alkylene group having 1 to 6 carbon atoms; R 3 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, a halogen group, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group.
[0038] In the above general formulas (1) and (16), R 1 In other words, the hydrocarbon group having 1 to 8 carbon atoms in R and X is a methyl group, an ethyl group, or a linear, branched, or cyclic hydrocarbon group having 3 to 8 carbon atoms. 1 and R 3 Specific examples of the hydrocarbon group having 1 to 8 carbon atoms in the above formula include a methyl group, an ethyl group, a propyl group, an isopropyl group, a cyclopropyl group, a butyl group, a 1-methylpropyl group, a 2-methylpropyl group, a 1,1-dimethylethyl group, a cyclobutyl group, a pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1,1-dimethylpropyl group, a 2,2-dimethylpropyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a cyclobutylmethyl group, a cyclopentyl group, a hexyl group, and a 1-methylpentyl group. , 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 1-ethylbutyl group, 2-ethylbutyl group, cyclohexyl group, heptyl group, 1-methylhexyl group, 1-ethylpentyl group, cyclohexylmethyl group, cycloheptyl group, octyl group, 1-methylheptyl group, 2-ethylhexyl group, phenyl group, o-tolyl group, m-tolyl group, p-tolyl group, benzyl group, 2-phenylethyl group, allyl group, 3-butenyl group, 4-pentenyl group, 5-hexenyl group, or propargyl group.
[0039] In the above general formulas (1) and (16), R 2 Examples of the linear or branched alkylene group having 1 to 6 carbon atoms in the formula include a methylene group, an ethylene group, a trimethylene group, a propylene group, and various butylene groups.
[0040] In the above general formulas (1) and (16), the alkoxy group having 1 to 4 carbon atoms in X is, in other words, a methoxy group, an ethoxy group, or a linear, branched, or cyclic alkoxy group having 3 to 4 carbon atoms. 3 Specific examples of the alkoxy group in include a methoxy group, an ethoxy group, a 1-propyloxy group, a 2-propyloxy group, a 1-butoxy group, and a t-butoxy group.
[0041] Specific examples of the monomer (B) (benzotriazole-based monomer represented by general formula (1)) relating to the repeating unit of the polymer block (B) include 2-[2'-hydroxy-5'-(methacryloyloxymethyl)phenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(methacryloyloxypropyl)phenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(methacryloyloxypropyl)phenyl]-2H-benzotriazole, 2-[2'-hydroxy-3'-t-butyl-5'-(methacryloyloxyethyl)phenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-t-butyl-3'-(methacryloyloxyethyl)phenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-t-butyl-3'-(methacryloyloxyethyl)phenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-5- Examples of the methoxy-2H-benzotriazole include 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-5-cyano-2H-benzotriazole, 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-5-t-butyl-2H-benzotriazole, and 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-5-nitro-2H-benzotriazole, but are not limited thereto. These may be used alone or in combination of two or more.
[0042] The block copolymer of the present embodiment may have at least one of the above-mentioned polymerization blocks (B), and may have two or more polymerization blocks (B). When the block copolymer has two or more polymerization blocks (B), the monomers (B) related to the repeating units between the two or more polymerization blocks (B) may be the same or different. When the block copolymer has two or more polymerization blocks (B), the polymerization degrees of the two or more polymerization blocks (B) may be different or the same from each other.
[0043] The content of monomer (B) in the copolymer (content of polymer block (B)) is preferably 5 to 65 mass%, more preferably 15 to 62 mass%, and particularly preferably 20 to 60 mass%, based on 100 mass% of the copolymer of this embodiment. By setting the content of monomer (B) to 65 mass% or less, the block copolymer of this embodiment is more likely to have crystallinity and is more likely to be compatible with resins such as polyolefins. Note that, by setting the content of monomer (B) to 5 mass% or more, it is more likely to achieve both ultraviolet absorbing properties and compatibility with resins such as polyolefins.
[0044] The block copolymer of this embodiment has at least one each of the above-mentioned polymerization block (A) and polymerization block (B). As long as the block copolymer of this embodiment has at least one each of the above-mentioned polymerization block (A) and polymerization block (B), it may further have other polymerization blocks (hereinafter also simply referred to as "other blocks") different from the polymerization block (A) and the polymerization block (B). In addition, the block copolymer of this embodiment may have a molecular structure in which the polymerization block (A) and the polymerization block (B) are directly linked, or may have a molecular structure in which the polymerization block (A) and the polymerization block (B) are linked via another block.
[0045] From the viewpoints of further improving the ultraviolet absorbing property in the long-wave ultraviolet region and further suppressing bleeding out from the resin, the block copolymer of this embodiment is preferably a copolymer represented by the following general formula (17): This copolymer is a copolymer containing a polymerization block (A) having a repeating unit derived from a (meth)acrylate represented by the above general formula (2) (the repeating unit represented by the above general formula (3)) and a polymerization block (B) having a repeating unit derived from a benzotriazole-based monomer represented by the above general formula (1) (the repeating unit represented by the above general formula (16)).
[0046] [ka] In the general formula (17), R 1 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, R 2 represents a linear or branched alkylene group having 1 to 6 carbon atoms; R 3 represents a hydrogen atom or a methyl group, X represents a hydrogen atom, a halogen group, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, x represents an integer of 2 or more, R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group having 8 or more carbon atoms, and y represents an integer of 2 or more.
[0047] The number average molecular weight (Mn) of the copolymer of the present embodiment is not particularly limited, but from the viewpoint of further suppressing bleed-out from the resin, it is preferably 2,000 to 20,000.
[0048] The molecular weight distribution (Mw / Mn) of the copolymer of the present embodiment is not particularly limited, but is preferably 2.5 or less from the viewpoint of further suppressing bleeding out from the resin. The lower limit of the molecular weight distribution (Mw / Mn) can be, for example, 1.1 or more, or can be 1.5 or more.
[0049] In this specification, the number average molecular weight (Mn) and weight average molecular weight (Mw) of the block copolymer are values measured by gel permeation chromatography (GPC). The measurement conditions may be, for example, the conditions described in the Examples below. The molecular weight distribution (Mw / Mn) of the copolymer can be determined by dividing the weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) by the number average molecular weight (Mn).
[0050] The block copolymer of the present embodiment is not particularly limited, but in the molecular weight distribution measured using gel permeation chromatography (GPC), the proportion of components having a molecular weight of 1000 or less is preferably 1% by mass or less relative to 100% by mass of the block copolymer. By making the proportion of components having a molecular weight of 1000 or less 1% by mass or less, bleeding out from the resin can be further suppressed, and ultraviolet absorbency in the long-wave ultraviolet region can be more easily improved.
[0051] Next, a method for producing the block copolymer of this embodiment will be described.
[0052] The block copolymer of the present embodiment is not particularly limited in its manufacturing method, and can be manufactured by a known method. For example, the copolymer of the present embodiment can be manufactured by a living polymerization method such as a living cationic polymerization method, a living anionic polymerization method, or a living radical polymerization method. Specific examples of the living radical polymerization method include a polymerization method mediated by nitroxide (NMP method), an atom transfer radical polymerization method (ATPR method), and a reversible addition-fragmentation chain transfer polymerization method (RAFT method).
[0053] In the narrow sense, living polymerization refers to polymerization in which the terminals always remain active, but in general, it also includes pseudo-living polymerization in which inactivated and activated terminals are in equilibrium. In this specification, living polymerization refers to the latter.
[0054] Hereinafter, the method for producing the copolymer of this embodiment using living polymerization will be described.
[0055] The method for producing the copolymer of the present embodiment using a living polymerization method includes at least a monomer (A) polymerization step of living polymerizing a monomer (A) to obtain a polymerization block (A) (a polymerization block having a repeating unit derived from monomer (A)), and a monomer (B) polymerization step of living polymerizing a monomer (B) with the polymerization block (A) to obtain a copolymer including the polymerization block (A) and polymerization block (B) (a polymerization block having a repeating unit derived from monomer (B)).
[0056] The living polymerization of the monomer (A) in the monomer (A) polymerization step can be carried out in a polymerization solvent containing the monomer (A) and a polymerization initiator. The polymerization solvent can be an organic solvent capable of dissolving the monomer (A). Examples of the organic solvent capable of dissolving the monomer (A) include aromatic compounds such as benzene, toluene, xylene, and anisole, ester compounds such as methyl acetate, propyl acetate, and butyl acetate, and ketone compounds such as acetone, methyl ethyl ketone, and cyclohexanone. The polymerization solvent may be used alone or in combination of two or more. The polymerization initiator contained in the polymerization solvent and the content thereof may be a conventionally known polymerization initiator and the content thereof according to the type of living polymerization used. The content of the monomer (A) contained in the polymerization solvent may be a conventionally known monomer content according to the type of living polymerization used.
[0057] The polymerization solvent used in the monomer (A) polymerization step should contain at least the monomer (A) and a polymerization initiator, and may contain other components in addition to these.For example, when the ATRP method is used as the living radical polymerization method, the polymerization solvent may further contain a catalyst such as metallic copper or a copper compound.Also, for example, when the TERP method is used as the living radical polymerization method, the polymerization solvent may further contain an organic tellurium compound.
[0058] The polymerization conditions of the monomer (A) in the monomer (A) polymerization step are not particularly limited, and conventionally known polymerization conditions according to the living polymerization method used can be used. As a specific example, when a living radical polymerization method is used, the polymerization temperature of the monomer (A) can be -20 to 120°C, the atmosphere in which the monomer (A) is polymerized can be a nitrogen atmosphere, and the polymerization time of the monomer (A) can be 1 to 48 hours. The polymerization of the monomer (A) may be carried out while stirring the polymerization solvent.
[0059] The living polymerization of monomer (B) in the monomer (B) polymerization step can be carried out in a polymerization solvent obtained by mixing monomer (B) with the polymerization solvent used in the monomer (A) polymerization step (i.e., the polymerization solvent containing the generated polymerization block (A)). This polymerization solvent contains at least a polymerization initiator, polymerization block (A), and monomer (B). In order to carry out the living polymerization by monomer (B) more efficiently, the polymerization solvent may further contain a polymerization solvent in addition to monomer (B). The content of monomer (B) contained in the polymerization solvent can be the content of a conventionally known monomer according to the type of living polymerization used.
[0060] The polymerization conditions of the monomer (B) in the monomer (B) polymerization step are not particularly limited, and conventionally known polymerization conditions according to the living polymerization method used can be used. As a specific example, when a living radical polymerization method is used, the polymerization temperature of the monomer (B) can be -20 to 120°C, the atmosphere in which the monomer (B) is polymerized can be a nitrogen atmosphere, and the polymerization time of the monomer (B) can be 2 to 48 hours. The polymerization of the monomer (B) may be carried out while stirring the polymerization solvent.
[0061] A copolymer including the polymerized block (A) and the polymerized block (B) can be obtained by the above-mentioned monomer (B) polymerization step. The obtained copolymer can be the copolymer of the present embodiment.
[0062] In the above-mentioned production method, the monomer (A) polymerization step is followed by the monomer (B) polymerization step, but the order of carrying out the monomer (A) polymerization step and the monomer (B) polymerization step can be changed depending on the type of monomer to be polymerized, the weight average molecular weight, the polymerization conditions, etc. That is, the block copolymer of this embodiment may be produced by a production method including a monomer (B) polymerization step of living polymerizing the monomer (B) to obtain a polymerization block (B), and a monomer (A) polymerization step of living polymerizing the monomer (A) to the polymerization block (B) to obtain a copolymer containing the polymerization block (A) and the polymerization block (B). In this production method, the monomer (A) can be living polymerized to the polymerization block (B) in a polymerization solvent obtained by mixing the monomer (A) with the polymerization solvent used in the monomer (B) polymerization step (i.e., the polymerization solvent containing the generated polymerization block (B)).
[0063] In the above-mentioned production method, the copolymer containing the polymerization block (A) and the polymerization block (B) obtained by the monomer (B) polymerization step or the monomer (A) polymerization step is regarded as the block copolymer of this embodiment, but the copolymer containing the polymerization block (A) and the polymerization block (B) obtained by the monomer (B) polymerization step or the monomer (A) polymerization step may be subjected to at least one treatment consisting of heating, drying (spray drying, etc.), and concentration, and the copolymer subjected to the treatment may be regarded as the block copolymer of this embodiment. By performing these treatments, the copolymer containing the polymerization block (A) and the polymerization block (B) can be made into a paste or powder, and the block copolymer of this embodiment in the form of a paste or powder can be produced.
[0064] The block copolymer of the present embodiment described above can exhibit excellent ultraviolet absorbing properties in the long-wave ultraviolet region of 300 to 400 nm because the polymerization block (B) has a constitutional unit (repeating unit) derived from the monomer (B) that exhibits ultraviolet absorbing properties in the long-wave ultraviolet region. In addition, the block copolymer of the present embodiment can exhibit excellent ultraviolet absorbing properties in the long-wave ultraviolet region of 300 to 400 nm because the polymerization block (A) has a constitutional unit derived from the monomer (A) that contains an alkane chain having 8 or more carbon atoms. Therefore, the block copolymer is easily compatible with resins such as polyolefins, and does not easily bleed out even when the block copolymer is contained in a resin such as polyolefins and exposed to a high humidity environment.
[0065] As described above, the block copolymer of the present embodiment exhibits excellent ultraviolet absorption in the long-wave ultraviolet region of 300 to 400 nm, and therefore can be used as an ultraviolet absorbent. The ultraviolet absorbent containing the block copolymer of the present embodiment may be composed only of the block copolymer of the present embodiment, but may also contain other components in addition to the block copolymer. Examples of other components include solvents such as water and alcohol, oils and fats such as silicone oil, and ultraviolet absorbents other than the block copolymer of the present embodiment. When such other components are included, the block copolymer of the present embodiment and the other components can be appropriately mixed to produce an ultraviolet absorbent containing the other components.
[0066] Furthermore, as described above, the block copolymer of the present embodiment exhibits excellent ultraviolet absorption properties in the long-wave ultraviolet region, and is less likely to bleed out even when incorporated into a resin such as polyolefin and exposed to a high-humidity environment. Therefore, the block copolymer may be incorporated into a resin and used as a resin composition.
[0067] The resin composition containing the block copolymer of the present embodiment contains at least the block copolymer of the present embodiment and a resin. The resin composition may contain other components other than the block copolymer of the present embodiment and the resin. The resin contained in the resin composition is not particularly limited, but it is preferable to use polyolefins such as polyethylene, polypropylene, and cycloolefin polymer (cyclic polyolefin). The resin contained in the resin composition may be two or more kinds of resins. The resin contained in the resin composition is preferably a cycloolefin polymer (cyclic polyolefin) and / or polyethylene among polyolefins, since the resin composition has excellent dispersibility of the block copolymer of the present embodiment and has excellent ultraviolet absorption in the long-wave ultraviolet region.
[0068] The polyethylene may be any polyethylene generally referred to as polyethylene, and examples thereof include ethylene-α-olefin copolymers such as high-density polyethylene, low-density polyethylene, linear low-density polyethylene, ethylene-propylene copolymers, ethylene-butene copolymers, ethylene-hexene copolymers, and ethylene-octene copolymers, ethylene-acrylate copolymers, ethylene-methacrylate copolymers, and ethylene-vinyl acetate copolymers, and may contain two or more of these.
[0069] The polyethylene preferably has a melt flow rate (MFR) of 0.1 to 15 g / 10 min, more preferably 0.5 to 10.0 g / 10 min, measured under conditions of 190°C and a load of 2.16 kg according to JIS K6922-1. When the MFR is 0.1 g / 10 min or more, the load when using an extruder during molding can be reduced more than when the MFR is less than 0.1 g / 10 min, and the occurrence of roughness on the surface of the resin composition during molding can be suppressed more. Furthermore, when the MFR is 15 g / 10 min or less, the melt tension is increased and molding stability is improved more than when the MFR is more than 15 g / 10 min.
[0070] The density of polyethylene, measured according to JIS K6922-1, is 900 to 970 kg / m 3 is preferably 910 to 960 kg / m 3 The density is 900kg / m 3 If it is more than 900kg / m 3 In addition, the mechanical strength of the resulting resin composition can be increased compared to when the density is less than 970 kg / m 3 If it is less than 970kg / m 3 In comparison with the case where it exceeds 100%, the transparency of the obtained resin composition can be further improved.
[0071] The cyclic polyolefin may be any cyclic polyolefin that is generally referred to as a cyclic polyolefin, and examples thereof include cycloolefin copolymers, which are copolymers of ethylene and norbornenes, and cycloolefin polymers, which are hydrogenated products of ring-opening metathesis polymers of unsaturated cyclic olefin monomers. Specific examples of cycloolefin copolymers include "TOPAS" manufactured by TOPAS Advanced Polymers and "ARTON (registered trademark)" manufactured by JSR Corporation. Specific examples of cycloolefin polymers include "Zeonex (registered trademark)" and "Zeonor (registered trademark)" manufactured by Zeon Corporation, and "APEL (registered trademark)" manufactured by Mitsui Chemicals, Inc.
[0072] The cyclic polyolefin preferably has a melt flow rate (MFR) of 10 to 60 g / 10 min, measured under conditions of 280°C and a load of 2.16 kg according to ISO 1133. When the MFR is 10 g / 10 min or more, the load when using an extruder during molding can be reduced more than when the MFR is less than 10 g / 10 min, and the occurrence of roughness on the surface of the resin composition during molding can be suppressed more. Also, when the MFR is 60 g / 10 min or less, the melt tension is increased and molding stability is improved more than when the MFR is more than 60 g / 10 min.
[0073] The cyclic polyolefin preferably has a glass transition temperature of 80 to 170°C as measured by a differential scanning calorimeter at a temperature rise rate of 20°C / min in accordance with JIS K7121. When the glass transition temperature is 80°C or higher, the heat resistance of the molded article is improved and dimensional changes due to expansion during heating and shrinkage during cooling can be suppressed compared to when the glass transition temperature is lower than 80°C. Furthermore, when the glass transition temperature is 170°C or lower, low-temperature processability is improved compared to when the glass transition temperature is higher than 170°C, and oxidation deterioration due to heat during molding can be suppressed, allowing a molded article with excellent transparency to be obtained.
[0074] The content of the copolymer of this embodiment in the resin composition is preferably 0.5 to 3.0 mass%, and more preferably 0.7 to 2.0 mass%, relative to 100 mass% of the resin composition, since this improves the dispersibility of the copolymer in the resin composition and results in a resin composition with excellent UV absorption properties.
[0075] From the viewpoints of further increasing the ultraviolet absorbing properties in the long-wave ultraviolet region and further suppressing bleed-out from the resin, the content of the resin in the resin composition is preferably 97.0 to 99.5 mass%, and more preferably 98.0 to 99.3 mass%, relative to 100 mass% of the resin composition.
[0076] The method for producing a resin composition containing the block copolymer of the present embodiment is not particularly limited as long as the copolymer of the present embodiment can be dispersed in a resin. For example, the block copolymer of the present embodiment can be produced by kneading the block copolymer of the present embodiment with a resin.
[0077] The block copolymer of the present embodiment and the resin can be kneaded using a kneading device that is typically used for kneading resins, such as a single-screw extruder, a twin-screw extruder, a multi-screw extruder, a Banbury mixer, a pressure kneader, a rotating roll, an internal mixer, etc. The block copolymer of the present embodiment and the resin can be kneaded by heating, for example, at 160 to 260°C.
[0078] The block copolymer of this embodiment and the resin may be kneaded after premixing using a tumbler, a Henschel mixer, or the like. Alternatively, the block copolymer of this embodiment and the resin may be kneaded to produce a master batch containing the block copolymer at a high concentration, and then the master batch and the resin may be kneaded to produce a resin composition. The resin composition obtained by kneading the block copolymer of this embodiment and the resin may be molded into a predetermined shape by a conventionally known method.
[0079] As described above, the copolymer of the present embodiment exhibits excellent ultraviolet absorption in the long-wave ultraviolet region, and is less likely to bleed out even when contained in a resin and exposed to a high-humidity environment. Therefore, a resin composition containing the copolymer of the present embodiment has excellent long-term weather resistance, and can also suppress poor appearance caused by bleeding out of the block copolymer. EXAMPLES
[0080] The present invention will be described in more detail below by showing examples, but the present invention is not limited to these examples.
[0081] The properties of the samples used in the examples and comparative examples were evaluated by the following methods.
[0082] <Molecular weight, molecular weight distribution> The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured by gel permeation chromatography (GPC). The molecular weight distribution (Mw / Mn) was calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) measured by GPC. A GPC device (HLC-8320GPC, Tosoh Corporation (trade name)) and a column (TSKgel GMHhr-H (6.0 mml.D x 4 cm) and TSKgel GMHhr-H (7.8 mml.D x 30 cm), Tosoh Corporation (trade name)) were used, the column temperature was set to 40°C, and chloroform was used as the eluent. The measurement sample was prepared at a concentration of 0.002 to 1.0 mg / ml, and 0.3 ml was injected and measured. The molecular weight calibration curve was calibrated using a polystyrene sample with a known molecular weight. Mw and Mn were calculated as linear polyethylene equivalent values.
[0083] <Monomer content in copolymer> A UV detector (338 nm) was used for the GPC detector to measure the UV absorption peak area derived from the copolymer. The content of monomer (B) in the copolymer was calculated based on the concentration-UV absorption peak area calibration curve for the UV absorbing monomer (monomer (B)) and the UV absorption peak area value of the copolymer. The content of monomer (A) was calculated assuming that the copolymer consists of two components, monomer (A) and monomer (B).
[0084] <Melting point, heat of fusion> The melting point and heat of fusion were measured by a differential scanning calorimeter (DSC). After filling an aluminum pan with 5 mg of sample, the sample was placed in the heat sink of a DSC device (manufactured by Hitachi High-Tech Science Co., Ltd. (product name) AS-3) using an autosampler, and the heater temperature was set to -30°C. The heater temperature was raised from -30°C to 210°C at 10°C / min and held for 5 min, then lowered to -30°C at 10°C / min and held for 5 min, and then raised again to 210°C at 10°C / min to measure the melting point and heat of fusion of the sample. An empty aluminum pan was used as a reference material.
[0085] <Absorption peak wavelength> The absorption peak wavelength (peak top wavelength of the absorption peak) was measured by ultraviolet-visible spectroscopy (UV-VIS). After dissolving the sample in chloroform to 10 mg / L, an appropriate amount was poured into a quartz cell to prepare a sample for absorption peak measurement. After placing the sample for absorption peak measurement in a UV-VIS measurement device (product name V-770 manufactured by JASCO Corporation), measurements were performed in a wavelength scanning range of 190 to 450 nm and at scanning intervals of 0.5 nm.
[0086] The commercially available products and the methods for producing the copolymers used in the examples and comparative examples are shown below.
[0087] (1) Ultraviolet absorbers Y-1: 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-2H-benzotriazole (a compound represented by the following formula (18)) (manufactured by Otsuka Chemical Co., Ltd., RUVA-93 (product name) (melting point = 98°C, molecular weight = 323g / mol)) [ka] Y-2: 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole (ADEKA Corporation, Adeka STAB (registered trademark) LA-36 (product name) (melting point = 138 to 141°C, molecular weight = 315 g / mol) Y-3: 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol] (ADEKA Corporation, Adeka STAB (registered trademark) LA-31RG (product name) (melting point = 194 to 200 ° C, molecular weight = 659 g / mol))
[0088] (2) Monomer (A) Monomer (A-1): Stearyl acrylate (hereinafter also referred to as "STA") The monomer (A-1) is a monomer represented by the following formula (19) having an alkane chain having 18 carbon atoms (a linear alkyl group having 18 carbon atoms) on the side chain. [ka]
[0089] (3) Monomer (B) Monomer (B-1): 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-2H-benzotriazole (compound represented by the following formula (18)) (Otsuka Chemical Co., Ltd. RUVA-93 (product name) (melting point = 98°C, molecular weight = 323g / mol)) [ka] The monomer (B-1) is a methacrylate monomer having a benzotriazole structure in the main chain.
[0090] (4) Polymerization initiator: Bloc Builder MA No. 33 (manufactured by Arkema)
[0091] (5) Polymerization solvent: butyl acetate
[0092] (6) Copolymer Production Examples <Production example 1 (copolymer (X-1))> A solution containing 10.23 g of STA, 10.03 g of butyl acetate, and 1.53 g of initiator was stirred at a polymerization temperature of about 110° C. and a reactor stirring speed of 75 rpm for 1.5 hours, and living radical polymerization was performed under a nitrogen atmosphere to produce a polymerization block (A) (polymer (A)) having a repeating unit derived from STA (monomer (A-1)) which is monomer (A). Furthermore, 10.01 g of RUVA-93 (monomer (B-1)) which is monomer (B) and 10.68 g of butyl acetate were added to the solution of the polymerization block (A) obtained in this way, and the solution was stirred at a polymerization temperature of about 110° C. and a reactor stirring speed of 75 rpm for 10.5 hours, thereby living radical polymerization of RUVA-93 (monomer (B-1)) which is monomer (B) to the polymerization block (A). As a result, a block copolymer (X-1) containing the polymerization block (A) and a polymerization block (B) having a repeating unit derived from RUVA-93 (monomer (B-1)) was obtained. This block copolymer (X-1) was a block copolymer represented by the following formula (20). [ka] In the above formula (20), x and y represent the degree of polymerization.
[0093] In the block copolymer (X-1), the content of monomer (A-1) was 71.4% by mass (1,500 (g / mol)) based on 100% by mass of the block copolymer (X-1), and the content of monomer (B-1) was 28.6% by mass (600 (g / mol)) based on 100% by mass of the block copolymer (X-1). The number average molecular weight, molecular weight distribution (Mw / Mn), melting point, heat of fusion, and absorption peak wavelength of the block copolymer (X-1) are shown in Table 1 below.
[0094] <Production example 2 (copolymer (X-2))> A block copolymer (X-2) was produced in the same manner as in Production Example 1, except that the polymerization reaction time in Production Example 1 was changed (first reaction: 3 hours, second reaction: 21 hours). The block copolymer (X-2) was a block copolymer represented by the above formula (20). In the obtained block copolymer (X-2), the content of the monomer (A-1) was 61.7% by mass (2,900 (g / mol)) relative to 100% by mass of the block copolymer (X-2), and the content of the monomer (B-1) was 38.3% by mass (1,800 (g / mol)) relative to 100% by mass of the block copolymer (X-2). The number average molecular weight, molecular weight distribution (Mw / Mn), melting point, heat of fusion, and absorption peak wavelength of the block copolymer (X-2) were as shown in Table 1 below.
[0095] <Production example 3 (copolymer (X-3))> A block copolymer (X-3) was produced in the same manner as in Production Example 1, except that the polymerization reaction time in Production Example 1 was changed (first reaction: 6 hours, second reaction: 42 hours). The block copolymer (X-3) was a block copolymer represented by the above formula (20). In the obtained block copolymer (X-3), the content of the monomer (A-1) was 47.7% by mass (6,200 (g / mol)) relative to 100% by mass of the block copolymer (X-3), and the content of the monomer (B-1) was 52.3% by mass (6,800 (g / mol)) relative to 100% by mass of the block copolymer (X-3). The number average molecular weight, molecular weight distribution (Mw / Mn), melting point, heat of fusion, and absorption peak wavelength of the block copolymer (X-3) were as shown in Table 1 below.
[0096] <Production example 4 (copolymer (X-4))> A block copolymer (X-4) was produced in the same manner as in Production Example 1, except that the amounts of monomers charged in Production Example 1 were changed (STA: 10.03 g, RUVA-93: 19.86 g) and the polymerization reaction time was changed (first reaction: 5 hours, second reaction: 43 hours). The block copolymer (X-4) was a block copolymer represented by the above formula (20). In the obtained block copolymer (X-4), the content of monomer (A-1) was 43.1 mass% (5,600 (g / mol)) relative to 100 mass% of the block copolymer (X-4), and the content of monomer (B-1) was 56.9 mass% (7,400 (g / mol)) relative to 100 mass% of the block copolymer (X-4). The number average molecular weight, molecular weight distribution (Mw / Mn), melting point, heat of fusion, and absorption peak wavelength of the block copolymer (X-4) were as shown in Table 1 below.
[0097] [Table 1]
[0098] (7) Polyolefin (C) Linear low-density polyethylene (C-1): FY12 manufactured by Tosoh Corporation, density 916 kg / m 3 The melt flow rate (MFR) measured under conditions of 190°C and a load of 2.16 kg in accordance with JIS K6922-1 is 1.0 g / 10 min. Linear low-density polyethylene (C-2): Nipolon-L M55 manufactured by Tosoh Corporation, density 920 kg / m 3 The melt flow rate (MFR) measured under the conditions of 190°C and a load of 2.16 kg in accordance with JIS K6922-1 is 8.0 g / 10 min. Low-density polyethylene (C-3): Petrothene 175K manufactured by Tosoh Corporation, density 922 kg / m 3 The melt flow rate (MFR) measured under conditions of 190°C and a load of 2.16 kg in accordance with JIS K6922-1 is 0.6 g / 10 min. High density polyethylene (C-4): Nipolon Hard 5700 manufactured by Tosoh Corporation, density 954 kg / m 3The melt flow rate (MFR) measured under conditions of 190°C and a load of 2.16 kg in accordance with JIS K6922-1 is 1.0 g / 10 min. Cycloolefin polymer (C-5): Zeon Corporation (trade name) Zeonor 1020R, melt flow rate (MFR) measured under conditions of 280°C and a load of 2.16 kg in accordance with ISO 1133 = 20g / 10min, glass transition temperature measured by a differential scanning calorimeter at a heating rate of 20°C / min in accordance with JIS K7121 = 102°C
[0099] Using the copolymers (X-1, X-2, X-3, X-4) and ultraviolet absorbers (Y-1, Y-2, Y-3) shown in Table 1, resin compositions (films) of Examples 1 to 10 and Comparative Examples 1 to 3 were produced by the following method, and the evaluations described below were performed.
[0100] <Example 1> 5 parts by mass of copolymer (X-1) and 95 parts by mass of polyolefin (C-1) were mixed and kneaded in a single screw extruder (manufactured by Toyo Seiki Seisakusho Co., Ltd., product name: Labo Plastomill D2025N) using a full-flight screw with a compression ratio of 3 under conditions of a heating temperature of 180°C and a rotation speed of 40 rpm. After cooling the kneaded product, it was cut into pellets using a pelletizer to obtain a master batch.
[0101] 36 parts by mass of the obtained master batch and 64 parts by mass of polyolefin (C-1) were mixed and kneaded in a single screw extruder (manufactured by Toyo Seiki Seisakusho, product name: Labo Plastomill 2D25S) using a full-flight screw with a compression ratio of 3 under conditions of a heating temperature of 180°C and a rotation speed of 40 rpm. After cooling the kneaded product, it was cut into pellets using a pelletizer to obtain a resin composition.
[0102] The obtained resin composition was compressed in a compression molding machine AWFA.50 (manufactured by Shinto Metal Industries Co., Ltd.) at a heating temperature of 180°C and a heating pressure of 190 kgf / cm 2 After heating and compressing for 6 minutes, the mixture was immersed in cold water at a temperature of 15° C. and rapidly cooled and solidified to obtain a film having a thickness of 100 μm. The obtained film was used as the film of Example 1.
[0103] <Example 2> 1.8 parts by mass of copolymer (X-1) and 98.2 parts by mass of polyolefin (C-1) were mixed and kneaded in a single screw extruder (manufactured by Toyo Seiki Seisakusho Co., Ltd., product name Labo Plastomill D2025N) using a full-flight screw with a compression ratio of 3 under conditions of a heating temperature of 180°C and a rotation speed of 40 rpm. After cooling the kneaded product, it was cut into pellets using a pelletizer to obtain a resin composition.
[0104] The obtained resin composition was compressed in a compression molding machine AWFA.50 (manufactured by Shinto Metal Industries Co., Ltd.) at a heating temperature of 180°C and a heating pressure of 190 kgf / cm 2 After heating and compressing for 6 minutes, the mixture was immersed in cold water at a temperature of 15° C. for rapid cooling and solidification to obtain a film having a thickness of 100 μm. The obtained film was used as the film of Example 2.
[0105] <Examples 3 to 10 and Comparative Examples 1 to 3> Films of Examples 3 to 10 and Comparative Examples 1 to 3 were produced in the same manner as in Example 2, except that the raw materials and contents of Example 2 were changed to those shown in Table 2 below.
[0106] <Film evaluation> The films were evaluated by the following methods.
[0107] (UV absorption) A test piece measuring 10 mm wide x 50 mm long was cut out from the prepared film, and the ultraviolet light transmittance at a wavelength of 340 nm was measured in pure water using an ultraviolet-visible spectrophotometer (model V-730, manufactured by JASCO Corporation). When the ultraviolet light transmittance was below 5%, the ultraviolet light absorbency was judged to be good (evaluated as ◯), and otherwise it was rated as ×.
[0108] (Bleeding resistance) The prepared film was placed in a thermo-hygrostat (Hitachi Appliances, Inc., model EC26-MHHP) and stored for one month (28 days) under conditions of a temperature of 40°C and a relative humidity of 75%. Thereafter, an arbitrarily selected spot on the film surface was observed with an optical microscope (Nikon, model LV100ND) set to an observation magnification of 50 times, and the presence or absence of bleed-out in an observation area of 2.4 mm x 1.7 mm was observed. In the entire observation image, when no precipitate (i.e., precipitate of copolymer or ultraviolet absorber) was present on the film surface, the bleed resistance was judged to be good (evaluated as ◯), and otherwise was evaluated as ×. For reference, the observation image of Example 1 in which no bleed-out occurred is shown in FIG. 1, and the observation images of Comparative Examples 1 to 3 in which bleed-out occurred are shown in FIGS. 2 to 4.
[0109] The evaluation results of the films of Examples 1 to 10 and Comparative Examples 1 to 3 are shown in Table 2 below. [Table 2]
[0110] As shown in Table 2, the films of Examples 1 to 10 were evaluated as ◯ for both UV absorbency and bleed resistance, whereas the films of Comparative Examples 1 to 3 were evaluated as ◯ for UV absorbency but x for bleed resistance. From these results, it was understood that the resin compositions (films) of Examples 1 to 10 exhibit excellent UV absorbency in the long-wave UV region of 320 to 400 nm, and are resin compositions that are excellent in long-term weather resistance and can maintain UV absorbency even under high humidity.
Claims
1. A polymer block (A) having a repeating unit derived from a monomer (A) which is one selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, and which has an alkane chain having 8 or more carbon atoms; and a polymer block (B) having a repeating unit derived from monomer (B), which is a benzotriazole-based monomer represented by the following general formula (1): [Formula 1] (In the general formula (1), R 1 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms; R 2 represents a linear or branched alkylene group having 1 to 6 carbon atoms; R 3 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, a halogen group, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group.
2. The block copolymer according to claim 1 , wherein the block copolymer has crystallinity.
3. 2. The block copolymer according to claim 1, wherein the monomer (A) is one selected from the group consisting of stearyl acrylate, behenyl acrylate, hexadecyl acrylate, and lauryl acrylate.
4. 2. The block copolymer according to claim 1, comprising the monomer (A) in an amount of 35 to 95% by mass relative to 100% by mass of the block copolymer.
5. 2. The block copolymer according to claim 1, having a number average molecular weight of 2,000 to 20,000.
6. 2. The block copolymer according to claim 1, having a molecular weight distribution (Mw / Mn) of 2.5 or less.
7. a monomer (A) polymerization step of subjecting a monomer (A) having an alkane chain having 8 or more carbon atoms, the monomer (A) being one selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, to living polymerization to obtain a polymer block (A) having a repeating unit derived from the monomer (A); a monomer (B) polymerization step of subjecting the polymerization block (A) to living polymerization with a monomer (B) which is a benzotriazole-based monomer represented by the following general formula (1) to obtain a copolymer including the polymerization block (A) and a polymerization block (B) having a repeating unit derived from the monomer (B); A method for producing the block copolymer according to any one of claims 1 to 6, comprising: [Case 2] (In the general formula (1), R 1 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms; R 2 represents a linear or branched alkylene group having 1 to 6 carbon atoms; R 3 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, a halogen group, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group.
8. a monomer (B) polymerization step of subjecting a monomer (B), which is a benzotriazole-based monomer represented by the following general formula (1), to living polymerization to obtain a polymer block (B) having a repeating unit derived from the monomer (B); a monomer (A) polymerization step of subjecting the polymer block (B) to living polymerization with a monomer (A) having an alkane chain having 8 or more carbon atoms and selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene to obtain a copolymer including a polymer block (A) having a repeating unit derived from the monomer (A) and the polymer block (B); A method for producing the block copolymer according to any one of claims 1 to 6, comprising: [C3] (In the general formula (1), R 1 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms; R 2 represents a linear or branched alkylene group having 1 to 6 carbon atoms; R 3 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, a halogen group, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group.
9. An ultraviolet absorbent comprising the block copolymer according to any one of claims 1 to 6.
10. A resin composition comprising the block copolymer according to any one of claims 1 to 6 and a resin.
11. The resin composition according to claim 10, wherein the resin is a polyolefin.
12. The resin composition according to claim 10, wherein the resin is polyethylene and / or cyclic polyolefin.
13. The content of the block copolymer is 0.5 to 3.0% by mass relative to 100% by mass of the resin composition, The resin composition according to claim 12, wherein the content of the resin is 97.0 to 99.5% by mass based on 100% by mass of the resin composition.
14. The resin composition according to any one of claims 10 to 13, characterized in that the resin composition has an ultraviolet ray transmittance of 5% or less at a wavelength of 340 nm, and the block copolymer does not bleed out to the surface when left to stand for 28 days in an atmosphere having a temperature of 40°C and a relative humidity of 75%.
Citation Information
Patent Citations
Ultraviolet absorbing polymer comprising 2-hydroxy-5-acrylyloxyalkylphenyl-2h-benzotriazoles
JP1985038411A
High polymer material composition having improved light stability
JP1987181360A
Ultraviolet absorber for plastic
JP1991281685A
Manufacture of uv shielding glass and window glass for automobile and window glass for building
JP1993339033A
Solution composition for forming transparent zinc oxide film
JP1993345639A