Method for producing epoxy resin and recycled fiber, method for producing fiber-containing epoxy resin composition, and method for producing fiber-containing epoxy resin cured product

The direct reaction of fiber-containing polycarbonate resin with epihalohydrin in the presence of a metal hydroxide or alkoxide simplifies the recycling process, producing epoxy resin and regenerated fibers, addressing the complexity of conventional recycling methods and achieving efficient recycling of fiber-containing polycarbonate resins.

JP2024149214APending Publication Date: 2024-10-18MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023062948
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Conventional chemical recycling of polycarbonate resin, especially when containing reinforcing fibers, is complicated and difficult due to insolubility of fibers during decomposition and purification processes, necessitating additional steps like polycondensation and functionalization.

Method used

A method involving the direct reaction of fiber-containing polycarbonate resin with epihalohydrin in the presence of a metal hydroxide or alkoxide, followed by decomposition and solid-liquid separation, to produce an epoxy resin and regenerated fibers, simplifying the recycling process.

Benefits of technology

This method efficiently produces an industrially useful epoxy resin and recycles fibers, offering a simpler and more effective chemical recycling process for fiber-containing polycarbonate resins.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a new production method which can chemically recycle a fiber-containing polycarbonate resin more easily than conventional production methods.SOLUTION: A method for producing an epoxy resin and a recycled fiber includes a reaction step of reacting a fiber-containing polycarbonate resin with epihalohydrin to yield an epoxy resin and a recycled fiber.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an epoxy resin and recycled fibers, a method for producing a fiber-containing epoxy resin composition containing the obtained epoxy resin and recycled fibers, and a method for producing a cured product of the fiber-containing epoxy resin composition. [Background technology]

[0002] Polycarbonate resin has excellent mechanical properties, electrical properties, heat resistance, cold resistance, transparency, etc., and is a material used for various applications. The demand for polycarbonate resin is increasing, and the amount of discarded polycarbonate resin is also increasing accordingly. Therefore, it is becoming important to reuse the discarded polycarbonate resin.

[0003] Under these circumstances, a method has been disclosed in which an aromatic polycarbonate resin is decomposed with an aqueous metal hydroxide solution to obtain an aqueous solution of an alkali metal salt of an aromatic dihydroxy compound, and the aromatic dihydroxy compound is recovered from the aqueous solution (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2006 / 114893 Summary of the Invention [Problem to be solved by the invention]

[0005] As described in Patent Document 1, in conventional chemical recycling techniques for discarded polycarbonate resin, only dihydroxy compounds such as bisphenol A are recovered, and in order to obtain industrially useful chemical products, further processes such as polycondensation and functionalization are required. In particular, chemical recycling technology for polycarbonate resins that contain reinforcing materials such as fibers to strengthen plastics has been complicated to implement and difficult to recycle because the reinforcing materials such as fibers are insoluble in the decomposition and purification processes. The present invention provides an industrially useful epoxy resin, and also provides a new production method that enables chemical recycling of fiber-containing polycarbonate resin in a simpler manner than conventional methods. [Means for solving the problem]

[0006] As a result of intensive research into providing the above-mentioned new production method, the present inventors have found a method for directly obtaining an epoxy resin by reacting a fiber-containing polycarbonate resin with epihalohydrin. In addition, they have found that by simultaneously obtaining recycled fibers, a polycarbonate resin containing recycled fibers can be easily obtained. That is, the present invention relates to the following inventions.

[0007] [1] A method for producing an epoxy resin and a recycled fiber, comprising a reaction step of reacting a fiber-containing polycarbonate resin with an epihalohydrin to obtain an epoxy resin and a recycled fiber. [2] The method for producing an epoxy resin and a regenerated fiber according to [1], wherein the reaction step includes a decomposition reaction for decomposing a polycarbonate resin, and the decomposition reaction is carried out in the presence of a metal hydroxide or a metal alkoxide. [3] The method for producing an epoxy resin and a recycled fiber according to [1] or [2], wherein the fiber is a carbon fiber. [4] The method for producing an epoxy resin and a regenerated fiber according to any one of [1] to [3], wherein the reaction step includes a separation step of performing solid-liquid separation into fibers and a solution. [5] The method for producing an epoxy resin and a regenerated fiber according to any one of [1] to [4], wherein the polycarbonate resin is an aromatic polycarbonate resin. [6] The method for producing an epoxy resin and a regenerated fiber according to any one of [1] to [5], wherein in the reaction step, 1 to 20 moles of the epihalohydrin are used per mole of carbonate groups contained in the polycarbonate resin. [7] The method for producing an epoxy resin and a regenerated fiber according to any one of [2] to [6], wherein in the reaction step, 1 to 10 moles of the metal hydroxide or metal alkoxide are used per mole of carbonate groups contained in the polycarbonate resin. [8] The method for producing an epoxy resin and a regenerated fiber according to any one of [1] to [7], wherein the epoxy resin obtained by the reaction step has an epoxy equivalent of 50 to 10,000 g / eq. [9] A method for producing a fiber-containing epoxy resin composition, comprising a step of mixing the epoxy resin obtained by the method according to any one of [1] to [8] with recycled fibers.

[10] A method for producing a fiber-containing epoxy resin composition, comprising a step of mixing an epoxy resin obtained by the method according to any one of [1] to [8], recycled fibers, and a curing agent.

[11] The method for producing a fiber-containing epoxy resin composition according to

[10] , further comprising mixing 0.1 to 1000 parts by mass of the curing agent with respect to 100 parts by mass of the epoxy resin.

[12] The method for producing a fiber-containing epoxy resin composition according to

[10] or

[11] , wherein the curing agent is at least one selected from the group consisting of polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, mercaptan compounds, cationic polymerization initiators, and organic phosphines.

[13] A method for producing a fiber-containing cured epoxy resin product, comprising a step of curing a fiber-containing epoxy resin composition obtained by the method according to any one of

[10] to

[12] . Effect of the Invention

[0008] The present invention provides an industrially useful epoxy resin, and also provides a new method that enables chemical recycling of fiber-containing polycarbonate resin in a simpler manner than conventional methods. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following description, and can be modified as desired without departing from the gist of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after "~", the values ​​before and after the "~" are included.

[0010] One aspect of the present invention is a method for producing an epoxy resin and a recycled fiber, comprising a reaction step of reacting a fiber-containing polycarbonate resin with an epihalohydrin to obtain an epoxy resin and a recycled fiber. In this specification, the term "recycled fiber" refers to a fiber that was once contained in a resin, extracted from the resin, and regenerated so that it can be reused. For example, it is a fiber extracted from a composite material of polycarbonate resin and fiber, such as fiber-reinforced plastic (FRP).

[0011] <Reaction process> The reaction step is a step of reacting the fiber-containing polycarbonate resin with epihalohydrin to obtain an epoxy resin and regenerated fibers. In this step, the fiber-containing polycarbonate resin is reacted with epihalohydrin to obtain an epoxy resin and regenerated fibers, and a highly efficient chemical recycling method can be provided.

[0012] (Polycarbonate resin) The polycarbonate resin includes a polymer containing a carbonate bond (-OC(=O)-O-). Although there is no limitation on the polycarbonate resin, it is preferable to use an aromatic polycarbonate resin in terms of availability of raw materials and usefulness of the epoxy resin to be produced.

[0013] The aromatic polycarbonate resin may be a polycarbonate resin containing a structural unit derived from an aromatic dihydroxy compound. Examples of the aromatic dihydroxy compound include bisphenols such as bisphenol A, bisphenol C, bisphenol F, bisphenol E, bisphenol Z, bisphenol S, bisphenol AD, bisphenol acetophenone, bisphenol trimethylcyclohexane, bisphenol fluorene, tetramethyl bisphenol A, tetramethyl bisphenol F, tetra-t-butyl bisphenol A, and tetramethyl bisphenol S; biphenol, tetramethyl biphenol, dimethyl biphenol, and tetra-t-butyl bisphenol; Examples of phenolic compounds include biphenols such as tylbiphenol; benzenediols such as hydroquinone, methylhydroquinone, dibutylhydroquinone, resorcin, and methylresorcin (here, "benzenediols" are compounds having one benzene ring, and two hydroxyl groups are directly bonded to the benzene ring); dihydroanthrahydroquinones such as dihydroanthrahydroquinone; dihydroxydiphenyl ethers such as dihydroxydiphenyl ether; thiodiphenols such as thiodiphenol; dihydroxynaphthalenes such as dihydroxynaphthalene; and dihydroxystilbenes such as dihydroxystilbene. The aromatic polycarbonate resin may be a homopolymer using one of these aromatic dihydroxy compounds alone, or a copolymer using two or more of them.

[0014] Among the above-mentioned aromatic dihydroxy compounds, those having bisphenol A or bisphenol C as the main structural unit are particularly preferred from the viewpoints of reactivity, ease of availability of raw materials, and versatility of the resulting epoxy resin. These aromatic polycarbonates may be used alone or in combination of two or more.

[0015] Further, the polycarbonate resin is not limited to a polycarbonate resin alone, and may be a composition containing one or more resins other than polycarbonate, such as polyester resins, polyarylate resins, etc. When a composition containing a resin other than polycarbonate resin is used, the polycarbonate resin composition preferably contains 50% by mass or more of the polycarbonate resin, more preferably 70% by mass or more, and even more preferably 90% by mass or more.

[0016] (fiber) The fibers contained in the fiber-containing polycarbonate resin are not particularly limited as long as they can be contained in the polycarbonate resin, and examples thereof include glass fiber and carbon fiber. The fibers are preferably capable of improving the mechanical strength of the cured polycarbonate resin, and are preferably carbon fibers. The shape, diameter, aspect ratio, etc. of the fibers are not particularly limited as long as they can be contained in the polycarbonate.

[0017] (epihalohydrin) Examples of epihalohydrins include epichlorohydrin, β-methylepichlorohydrin, epibromohydrin, etc. Among these, epichlorohydrin is particularly preferred from the viewpoints of reactivity, ease of availability of raw materials, and versatility of the resulting epoxy resin. These epihalohydrins may be used alone or in combination. .

[0018] The amount of epihalohydrin used in the reaction step is not particularly limited, but is preferably 1 to 20 moles, more preferably 3 to 16 moles, and particularly preferably 6 to 14 moles per mole of carbonate bond in the raw material polycarbonate resin. If the amount of epihalohydrin used is equal to or more than the lower limit, it is preferable in that undesirable side reactions such as crosslinking reactions can be suppressed. In addition, if the amount of epihalohydrin used is equal to or less than the upper limit, it is preferable in that industrial production efficiency is improved.

[0019] (Decomposition reaction) The reaction step includes a decomposition reaction for decomposing the polycarbonate resin, and the decomposition reaction is preferably carried out in the presence of a metal hydroxide or a metal alkoxide.

[0020] (metal hydroxide) Examples of metal hydroxides include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide; and alkaline earth metal hydroxides such as magnesium hydroxide, calcium hydroxide, strontium hydroxide, and barium hydroxide. These may be used alone or in combination of two or more. From the viewpoint of raw material availability, alkali metal hydroxides are preferred, and sodium hydroxide is particularly preferred.

[0021] The metal hydroxide is continuously supplied as an aqueous metal hydroxide solution within the reaction time, and the supply amount of the metal hydroxide is preferably 1 to 10 moles, more preferably 2.4 to 8 moles, and particularly preferably 3 to 6 moles per mole of carbonate bond in the polycarbonate resin. When the amount of the metal hydroxide used is equal to or more than the lower limit, the reaction rates of the decomposition reaction and the epoxy group formation reaction can be sufficiently ensured, which is preferable from the viewpoint of the quality and production efficiency of the obtained epoxy resin. In addition, when the amount is equal to or less than the upper limit, it is preferable from the viewpoint of suppressing excessive reaction and side reactions such as crosslinking reaction.

[0022] From the viewpoint of availability, the metal hydroxide concentration of the aqueous metal hydroxide solution is preferably 5 to 50 mass %.

[0023] (Metal alkoxide) Examples of the metal in the metal alkoxide include alkali metals such as lithium, sodium, potassium, rubidium, and cesium; and alkaline earth metals such as magnesium, calcium, strontium, and barium. Examples of the alkoxide include methoxide, ethoxide, and propoxide. Examples of the alkoxide include methoxide, ethoxide, propoxide, and glycoxide. The alcohol of the metal alkoxide is not particularly limited, and may be a monoalcohol or a polyol such as a glycol-based compound, but is preferably a monoalcohol. Examples of the monoalcohol include methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, s-butanol, and t-butanol. Examples of the polyol include ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, cyclohexanedimethanol, and glycerin. The glycol compound is a compound in which one hydroxyl group is bonded to each of two carbon atoms of an alkyl group having two or more carbon atoms, and examples of the glycol compound include ethylene glycol and propylene glycol. Metal alkoxides may be used alone or in combination of two or more. Among these, sodium methoxide is preferred from the viewpoint of industrial availability.

[0024] In the reaction step, the metal alkoxide is continuously supplied within the reaction time, and is preferably 1 to 10 moles, more preferably 2.4 to 8 moles, and particularly preferably 3 to 6 moles per mole of carbonate group contained in the polycarbonate resin. When the amount of metal alkoxide used is equal to or more than the above lower limit, the reaction rate of the decomposition reaction and the epoxy group formation reaction can be sufficiently ensured, which is preferable from the viewpoint of the quality and production efficiency of the obtained epoxy resin. In addition, when the amount is equal to or less than the above upper limit, it is preferable from the viewpoint of suppressing excessive reaction and side reactions such as crosslinking reaction.

[0025] In the reaction process, the decomposition reaction of the fiber-containing polycarbonate is carried out by azeotroping the reaction liquid while maintaining a predetermined temperature as necessary to obtain volatile steam. The steam obtained is then cooled to obtain a condensate, which is then subjected to oil / water separation, and the oil component with the water removed is returned to the reaction system, whereby the water generated by the glycidylation and the water derived from the aqueous metal hydroxide solution are dehydrated. This reduces the amount of water in the system, and promotes the formation of epoxy groups by the metal hydroxide.

[0026] The method for separating epihalohydrin from the azeotropic condensate is not particularly limited, but for example, the azeotropic condensate can be subjected to static separation in a static separation device and only the epihalohydrin in the lower layer is continuously returned to the system, thereby circulating epihalohydrin. In order to maintain the molar ratio of epihalohydrin in the system, the amount of epihalohydrin retained in the static separation device is preferably 5 mass% or less based on the total amount of charged epihalohydrin.

[0027] The reaction step can be carried out under reduced pressure as necessary. The pressure in the reaction system is not particularly limited, but is preferably 380 to 760 mmHg. By carrying out the reaction under reduced pressure, it is possible to promote the azeotropy of water and epihalohydrin.

[0028] In the reaction step, the reaction temperature is preferably 30 to 100° C. in order to ensure a sufficient reaction rate, and the reaction time is preferably 10 to 360 minutes, more preferably 20 to 300 minutes, and particularly preferably 30 to 240 minutes in order to allow the reaction to proceed sufficiently.

[0029] After the reaction is completed, a post-treatment step is carried out as necessary. In the post-treatment, insoluble by-product salts are removed by filtration or by washing with water, and then unreacted epihalohydrin is removed by distillation under reduced pressure to obtain the desired epoxy resin and regenerated fibers.

[0030] In addition, in the reaction step, catalysts such as quaternary ammonium salts such as tetramethylammonium chloride and tetraethylammonium bromide; tertiary amines such as benzyldimethylamine and 2,4,6-tris(dimethylaminomethyl)phenol; imidazoles such as 2-ethyl-4-methylimidazole and 2-phenylimidazole; phosphonium salts such as ethyltriphenylphosphonium iodide; and phosphines such as triphenylphosphine may be used.

[0031] In addition, in the reaction step, inert organic solvents such as alcohols such as ethanol and isopropanol; glycols such as ethylene glycol, diethylene glycol, propylene glycol and polyethylene glycol; ketones such as acetone and methyl ethyl ketone; ethers such as dioxane and ethylene glycol dimethyl ether; glycol ethers such as propylene glycol monomethyl ether; aprotic polar solvents such as dimethyl sulfoxide and dimethylformamide; and aromatic hydrocarbon solvents such as toluene and xylene may be used.

[0032] Furthermore, if the amount of saponifiable halogen in the epoxy resin obtained as described above is too high, Then, by reprocessing, a purified epoxy resin having a sufficiently reduced amount of saponifiable halogen can be obtained. That is, the crude epoxy resin obtained by the reaction is redissolved in an inert organic solvent such as isopropyl alcohol, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, dioxane, methoxypropanol, or dimethyl sulfoxide, and an alkali metal hydroxide or metal alkoxide is added as a solid or aqueous solution to carry out a ring-closing reaction at a temperature of about 30 to 120°C, more preferably 40 to 110°C, and even more preferably 50 to 100°C for 0.1 to 8 hours, more preferably 0.3 to 7 hours, and even more preferably 0.5 to 6 hours. Then, the excess alkali metal hydroxide or metal alkoxide and the secondary salt are removed by a method such as washing with water, and the organic solvent is distilled off under reduced pressure and / or steam distillation is carried out to obtain an epoxy resin having a reduced amount of hydrolyzable halogen. If the reaction temperature is too low or the reaction time is too short, the ring-closing reaction may not proceed, whereas if the reaction temperature is too high or the reaction time is too long, the reaction may proceed, but may result in problems such as high molecular weight, high epoxy equivalent, and high viscosity.

[0033] (separation process) The reaction step preferably includes a separation step of separating the fibers and the solution into a solid-liquid separation, whereby the epoxy resin solution and the regenerated fibers can be separated and each can be obtained. In the separation step, an organic solvent such as toluene and water are added to the reaction liquid, and the mixture is filtered to separate the regenerated fibers.

[0034] (Obtained epoxy resin) The epoxy equivalent of the epoxy resin obtained through the reaction step is preferably 50 to 10,000 g / eq, more preferably 100 to 5,000 g / eq, and particularly preferably 150 to 3,000 g / eq, as measured according to JIS K7236. When the epoxy equivalent of the obtained epoxy resin is within the above range, the crosslink density increases when cured with various curing agents, and a cured product having excellent chemical resistance and the like can be obtained.

[0035] <Fiber-containing epoxy resin composition> A fiber-containing epoxy resin composition can be produced by mixing the obtained epoxy resin with recycled fibers. Also, a fiber-containing epoxy resin composition can be produced by mixing the obtained epoxy resin with recycled fibers and a curing agent. If necessary, other epoxy compounds, curing accelerators, other components, etc. may be appropriately blended into the fiber-containing epoxy resin composition.

[0036] (hardening agent) A curing agent is a substance that contributes to the crosslinking reaction and / or chain extension reaction between epoxy groups of an epoxy compound. In this specification, even substances that are usually called "curing accelerators" are considered to be curing agents as long as they contribute to the crosslinking reaction and / or chain extension reaction between epoxy groups of an epoxy compound.

[0037] The amount of the curing agent is preferably 0.1 to 1000 parts by mass, more preferably 100 parts by mass or less, further preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less, based on 100 parts by mass of the epoxy resin.

[0038] When the fiber-containing epoxy resin composition contains an epoxy compound other than the above epoxy resin, the amount of the curing agent is preferably 0.1 to 1000 parts by mass, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less, based on 100 parts by mass of the total epoxy resin components as solids. The more preferable amount of the curing agent is as described below according to the type of the curing agent.

[0039] In this specification, "solid content" means the components excluding the solvent, and includes not only solid epoxy compounds but also semi-solid and viscous liquid substances. Moreover, "total epoxy resin components" means the sum of the above epoxy resins and other epoxy resins described below.

[0040] In the method for producing a fiber-containing epoxy resin composition, it is preferable to use as the curing agent at least one selected from the group consisting of polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, cationic polymerization initiators, and organic phosphines.

[0041] Examples of polyfunctional phenols include bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol B, bisphenol AD, bisphenol Z, and tetrabromobisphenol A; biphenols such as 4,4'-biphenol and 3,3',5,5'-tetramethyl-4,4'-biphenol; catechol, resorcin, hydroquinone, and dihydroxynaphthalenes; and compounds in which the hydrogen atoms bonded to the aromatic rings of these compounds are substituted with non-interfering substituents such as halogen groups, alkyl groups, aryl groups, ether groups, ester groups, and organic substituents containing hetero elements such as sulfur, phosphorus, and silicon. Further examples include novolaks and resols which are polycondensates of these phenols, or monofunctional phenols such as phenol, cresol, and alkylphenols with aldehydes.

[0042] Examples of polyisocyanate compounds include polyisocyanate compounds such as tolylene diisocyanate, methylcyclohexane diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, trimethylhexamethylene diisocyanate, lysine triisocyanate, etc. Furthermore, polyisocyanate compounds obtained by reacting these polyisocyanate compounds with compounds having at least two active hydrogen atoms such as amino groups, hydroxyl groups, carboxyl groups, water, etc., or trimers to pentamers of the above polyisocyanate compounds, etc., can be mentioned.

[0043] Examples of the amine compounds include aliphatic primary, secondary, and tertiary amines, aromatic primary, secondary, and tertiary amines, cyclic amines, guanidines, and urea derivatives. Specific examples include triethylenetetramine, diaminodiphenylmethane, diaminodiphenyl ether, metaxylenediamine, dicyandiamide, 1,8-diazabicyclo(5,4,0)-7-undecene, 1,5-diazabicyclo(4,3,0)-5-nonene, dimethylurea, and guanylurea.

[0044] Examples of the acid anhydride compound include phthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, and condensates of maleic anhydride and unsaturated compounds.

[0045] Examples of the imidazole-based compound include 1-isobutyl-2-methylimidazole, 2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, benzimidazole, etc. Although the imidazole-based compound also functions as a curing accelerator, which will be described later, in the present invention it is classified as a curing agent.

[0046] Examples of the amide-based compounds include dicyandiamide and its derivatives, polyamide resins, and the like.

[0047] A cationic polymerization initiator generates cations when exposed to heat or active energy rays. and aromatic onium salts. Specifically, SbF6 - , BF4 - , AsF6 - , PF6 - , CF3SO3 2- , B(C6F5)4 - and an aromatic cation component containing an atom of iodine, sulfur, nitrogen, phosphorus, etc. Diaryliodonium salts and triarylsulfonium salts are particularly preferred.

[0048] Examples of organic phosphines include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine. Examples of phosphonium salts include tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate. Examples of tetraphenylboron salts include 2-ethyl-4-methylimidazole tetraphenylborate and N-methylmorpholine tetraphenylborate.

[0049] The above curing agents may be used either individually or in combination of two or more of the same or different types.

[0050] When polyfunctional phenols, amine compounds, or acid anhydride compounds are used as the curing agent, it is preferable to use them in such a manner that the equivalent ratio of the functional groups in the curing agent (hydroxyl groups of polyfunctional phenols, amino groups of amine compounds, or acid anhydride groups of acid anhydride compounds) to the total epoxy groups in the epoxy resin composition is in the range of 0.8 to 1.5. When polyisocyanate compounds are used, it is preferable to use them in such a range that the equivalent ratio of the number of isocyanate groups in the polyisocyanate compounds to the number of hydroxyl groups in the epoxy resin composition is in the range of 1:0.01 to 1:1.5. When imidazole compounds are used, it is preferable to use them in the range of 0.5 to 10 parts by mass with respect to 100 parts by mass of the total epoxy resin components as solid contents in the epoxy resin composition. When amide compounds are used, it is preferable to use them in the range of 0.1 to 20% by mass with respect to the total amount of the total epoxy resin components and amide compounds as solid contents in the epoxy resin composition. When a cationic polymerization initiator is used, it is preferably used in the range of 0.01 to 15 parts by mass based on 100 parts by mass of all epoxy resin components as solid contents in the epoxy resin composition.When an organic phosphine is used, it is preferably used in the range of 0.1 to 20% by mass based on the total amount of all epoxy resin components as solid contents in the epoxy resin composition and the organic phosphines.

[0051] In addition to the curing agents listed above, the fiber-containing epoxy resin composition may also contain other curing agents such as mercaptan compounds, organic acid dihydrazides, boron halide amine complexes, etc. These curing agents may be used alone or in combination of two or more.

[0052] (Other epoxy resins) In the method for producing a fiber-containing epoxy resin composition, epoxy resins other than the above-mentioned epoxy resins (sometimes referred to as "other epoxy resins" in this specification) can be used. Examples of the other epoxy resins include glycidyl ether type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, biphenyl type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, tetrabromobisphenol A type epoxy resins, and other polyfunctional phenol type epoxy resins, epoxy resins obtained by hydrogenating the aromatic rings of the above-mentioned aromatic epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, linear aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. The above-mentioned other epoxy resins may be used alone or in combination of two or more.

[0053] When the fiber-containing epoxy resin composition contains the above-mentioned epoxy resin and other epoxy resins, the ratio of the other epoxy resins in the total epoxy resin components as solids in the fiber-containing epoxy resin composition is preferably 1% by mass or more, more preferably 5% by mass or more, and on the other hand, is preferably 99% by mass or less, more preferably 95% by mass or less. By having the ratio of the other epoxy resins be equal to or more than the lower limit, the physical property improvement effect by blending the other epoxy resins can be sufficiently obtained. On the other hand, by having the ratio of the other epoxy resins be equal to or less than the upper limit, the effect of chemical recyclability by the epoxy resins can be sufficiently obtained.

[0054] The fiber-containing epoxy resin composition may contain other components in addition to the components listed above. Examples of other components include curing accelerators (excluding those corresponding to the above-mentioned curing agents), coupling agents, flame retardants, antioxidants, light stabilizers, plasticizers, reactive diluents, pigments, inorganic fillers, organic fillers, etc. The other components listed above can be used in appropriate combinations depending on the desired physical properties of the fiber-containing epoxy resin composition.

[0055] [Cured product] The fiber-containing epoxy resin composition can be cured to obtain a cured product. The term "curing" used here means intentionally curing an epoxy compound by heat and / or light, and the degree of curing can be controlled depending on the desired physical properties and applications.

[0056] The method of curing the fiber-containing epoxy resin composition to produce a cured product varies depending on the components and amounts of the components in the fiber-containing epoxy resin composition and the shape of the compound, but typically includes heating conditions of 5 seconds to 180 minutes at 50 to 200° C. This heating is preferably performed in two stages, consisting of a primary heating at 50 to 160° C. for 5 seconds to 30 minutes and a secondary heating at 90 to 200° C., which is 40 to 120° C. higher than the primary heating temperature, for 1 minute to 150 minutes, in order to reduce poor curing.

[0057] When producing a cured product as a semi-cured product, the curing reaction of the fiber-containing epoxy resin composition may be allowed to proceed to an extent that allows the shape to be maintained by heating, etc. When the fiber-containing epoxy resin composition contains a solvent, most of the solvent is removed by techniques such as heating, reducing pressure, and air drying, but 5% by mass or less of the solvent may remain in the semi-cured product. EXAMPLES

[0058] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples. Note that the values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​of the examples. The epoxy equivalent of the epoxy resin obtained in the following examples was measured in accordance with JIS K 7236.

[0059] [Confirmation of epoxy resin production] The production of the epoxy resin was confirmed by high performance liquid chromatography according to the following procedure and conditions. Equipment: JASCO RHPLC, JASCO 03150-3M Unifinepak C18 3μm 150mm×3.0mmID Method: Gradient method ·Analysis temperature: 40℃ ·Eluent composition: Solution A: Acetonitrile Solution B: Distilled water At 0 min of analysis time, the ratio of liquid A: liquid B was 30:70 (volume ratio, the same applies below), and gradually changed to liquid A: liquid B = 100:0 from 0 to 25 min of analysis time. ·Flow rate: 0.40mL / min Detection wavelength: 280nm

[0060] Example 1 A separable flask reactor having a thermometer, a dropping funnel, a stirrer, a nitrogen inlet tube, and a cooling tube was charged with 93 parts by weight of Pyrofil pellets PC-C-20 (carbon fiber-containing BPA type polycarbonate manufactured by Mitsubishi Chemical) and 327 parts by weight of epichlorohydrin (epichlorohydrin was supplied so that the amount was 12 moles per mole of carbonate bonds in the polycarbonate), and the mixture was heated to 100°C to dissolve the polycarbonate resin, and then cooled to about 40°C under a nitrogen gas atmosphere. Then, the mixture was heated to 65°C while continuously dropping 136 parts by weight of a 28% sodium methoxide methanol solution (sodium methoxide was supplied so that the amount was 2.4 moles per mole of carbonate bonds in the polycarbonate), and the reaction was carried out for 120 minutes. Then, 230 parts by weight of water was added, and the oil-water separated water layer was separated to remove salts generated by the reaction from the resin solution, residual sodium methoxide, etc., and the reaction was stopped.

[0061] The reaction solution obtained was gradually heated and the pressure in the system was reduced, and it was held for 30 minutes from when it reached 150°C and 5mmHg, and methanol, excess epichlorohydrin, and dimethyl carbonate were completely distilled out of the system. After that, the system was returned to normal pressure while nitrogen was sealed in the system, and 233 parts by weight of toluene and 500 parts by weight of water were added and filtered to separate the carbon fiber. The oil layer from which the water layer of the filtrate was separated and removed was then added with 100 parts by weight of water, and the separated and removed water layer was repeatedly washed with water several times until it became neutral, to obtain a toluene solution of epoxy resin. The toluene was distilled from this solution under heating and reduced pressure, and the toluene was completely removed by holding it for 30 minutes from when it reached 150°C and 5mmHg, to obtain a liquid epoxy resin. The epoxy equivalent of the obtained epoxy resin was 261g / eq. The carbon fiber separated by filtration was washed with water and acetone to remove the attached resin and inorganic salt, and dried at 120°C for 2 hours to obtain regenerated carbon fiber.

[0062] Example 2 A resin composition was obtained by mixing 8 parts by weight of the epoxy resin produced in Example 1, 2 parts by weight of the recycled carbon fiber produced in Example 1, and 3 parts by weight of jER Cure ST14 (amine curing agent manufactured by Mitsubishi Chemical). The resulting composition was poured into a mold and heated at 100°C for 2 hours, and then heated at 170°C for 1 hour to obtain a recycled carbon fiber reinforced plastic.

Claims

1. A method for producing an epoxy resin and a regenerated fiber, comprising: a reaction step of reacting a fiber-containing polycarbonate resin with an epihalohydrin to obtain an epoxy resin and a regenerated fiber.

2. 2. The method for producing an epoxy resin and a regenerated fiber according to claim 1, wherein the reaction step includes a decomposition reaction for decomposing a polycarbonate resin, and the decomposition reaction is carried out in the presence of a metal hydroxide or a metal alkoxide.

3. The method for producing epoxy resin and recycled fibers according to claim 1 , wherein the fibers are carbon fibers.

4. The method for producing an epoxy resin and a regenerated fiber according to claim 1 , wherein the reaction step includes a separation step of performing solid-liquid separation into fibers and a solution.

5. The method for producing an epoxy resin and a recycled fiber according to claim 1, wherein the polycarbonate resin is an aromatic polycarbonate resin.

6. 2. The method for producing an epoxy resin and a regenerated fiber according to claim 1, wherein in the reaction step, 1 to 20 moles of the epihalohydrin are used per mole of carbonate groups contained in the polycarbonate resin.

7. 3. The method for producing an epoxy resin and a regenerated fiber according to claim 2, wherein in the reaction step, 1 to 10 moles of the metal hydroxide or metal alkoxide are used per mole of carbonate groups contained in the polycarbonate resin.

8. The method for producing an epoxy resin and a regenerated fiber according to claim 1, wherein the epoxy resin obtained by the reaction step has an epoxy equivalent of 50 to 10,000 g / eq.

9. A method for producing a fiber-containing epoxy resin composition, comprising: mixing the epoxy resin obtained by the method according to any one of claims 1 to 8 with recycled fibers.

10. A method for producing a fiber-containing epoxy resin composition, comprising: mixing the epoxy resin obtained by the method according to any one of claims 1 to 8 with recycled fibers and a curing agent.

11. The method for producing a fiber-containing epoxy resin composition according to claim 10, wherein 0.1 to 1000 parts by mass of the curing agent is mixed with 100 parts by mass of the epoxy resin.

12. The method for producing a fiber-containing epoxy resin composition according to claim 10, wherein the curing agent is at least one selected from the group consisting of polyfunctional phenols, polyisocyanate-based compounds, amine-based compounds, acid anhydride-based compounds, imidazole-based compounds, amide-based compounds, mercaptan-based compounds, cationic polymerization initiators, and organic phosphines.

13. A method for producing a fiber-containing epoxy resin cured product, comprising: curing the fiber-containing epoxy resin composition obtained by the method according to claim 10.

Citation Information

Patent Citations

  • Method for producing aqueous solution of alkali metal salt of aromatic dihydroxy compound from waste aromatic polycarbonate

    WO2006114893A1

Cited By

  • Method for producing epoxy resin, method for producing epoxy resin composition, and method for producing cured product

    JP2023101259A

  • Curable carbonate composition, manufacturing method thereof and carbonate-cured product

    JP2025104282A

  • Curable carbonate composition, method for preparing the same, and cured carbonate product

    JP7874148B2