Method for producing power cable
The resin composition with a tailored elastic modulus distribution in power cables addresses water tree propagation and bending resistance issues by incorporating a sea phase and two island phases, enhancing insulation properties and maintaining strength under stress.
Patent Information
- Application Number
- JP2023139163
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-08-29
- Publication Date
- 2024-10-18
AI Technical Summary
Existing power cables using cross-linked polyethylene insulating layers face issues with water tree formation and bending resistance due to phase structures that allow propagation of water trees from microscopic foreign objects or microvoids, leading to reduced insulation properties.
A resin composition for power cables is developed, comprising propylene and styrene units, with a specific elastic modulus distribution that includes a sea phase and two island phases of different sizes, optimized to suppress water tree propagation and maintain bending resistance.
The solution effectively limits water tree growth to 200 μm or less and maintains AC breakdown electric field strength at 50 kV/mm or more even after bending, ensuring high insulation properties under stress.
Smart Images

Figure 2024149339000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a resin composition and a power cable. [Background technology]
[0002] Cross-linked polyethylene has excellent insulating properties and has therefore been widely used as a resin component constituting the insulating layer in power cables and the like (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 57-69611 Summary of the Invention
[0004] According to one aspect of the present disclosure, A resin composition constituting an insulating layer of a power cable, Contains propylene units and styrene units, The resin composition comprises In the elastic modulus distribution obtained by measuring the elasticity of a small area using a scanning probe microscope at 25°C, a marine phase having an elastic modulus of more than 100 MPa; A first island phase having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less; A second island phase having an elastic modulus of 100 MPa or less and a size of more than 100 nm and not more than 2000 nm; Equipped A resin composition is provided. [Brief description of the drawings]
[0005] [Figure 1] FIG. 1 is a schematic cross-sectional view perpendicular to the axial direction of a power cable according to an embodiment of the present disclosure. [Diagram 2]FIG. 2 shows the elastic modulus distribution of sample A1 obtained by measuring the elasticity of a small area at 25° C. using a scanning probe microscope. [Diagram 3] FIG. 3 shows the elastic modulus distribution of sample B5 obtained by micro-area elasticity measurement using a scanning probe microscope at 25° C. [Figure 4] FIG. 4 shows the elastic modulus distribution of sample B2 obtained by micro-area elasticity measurement using a scanning probe microscope at 25° C. [Diagram 5] FIG. 5 shows the elastic modulus distribution of sample B3 obtained by micro-area elasticity measurement using a scanning probe microscope at 25° C. [Figure 6] FIG. 6 is a schematic cross-sectional view showing a water needle test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] [Problem that this disclosure aims to solve] The present inventors have focused on propylene-based resin (polypropylene) as a resin component constituting an insulating layer, and have conducted extensive research to improve the characteristics of power cables.
[0007] An object of the present disclosure is to suppress the occurrence of water trees originating from minute foreign objects or minute voids in an insulating layer while ensuring the bending resistance of the insulating layer.
[0008] [Effects of this disclosure] According to the present disclosure, it is possible to suppress the occurrence of water trees originating from minute foreign objects or minute voids in the insulating layer while ensuring the bending resistance of the insulating layer.
[0009] [Description of the embodiments of the present disclosure] <Inventor's findings> First, the findings of the inventors will be outlined.
[0010] The propylene-based resin itself has a high crystal content and tends to be hard.
[0011] Therefore, in order to control the crystallinity of the propylene-based resin and improve the flexibility of the insulation layer of the power cable, the inventors considered mixing a propylene-based resin with a low-crystalline resin as the resin component that constitutes the insulation layer.
[0012] However, the inventors have found the following new problem in an insulating layer containing a propylene-based resin and a low-crystalline resin.
[0013] (Water trees originating from tiny foreign objects or tiny voids) In the conventional water tree test, an electric field is applied to the insulation layer of a power cable while the cable is immersed in water. In the water tree test, water pressure is applied uniformly to the insulation layer, and an electric field is applied uniformly.
[0014] However, it has been found that even in power cables in which water trees did not occur in the above-mentioned water tree tests, when tiny foreign objects or tiny voids are mixed into the insulation layer, the water tree resistance of the insulation layer may be reduced depending on the phase structure of the insulation layer as follows.
[0015] (i) In the case where the phase structure of the insulating layer is a bicontinuous structure, when a minute foreign object or a minute void is mixed into the insulating layer, the minute foreign object or the minute void may be incorporated into a relatively flexible phase (hereinafter also referred to as a flexible phase) containing a low crystalline resin in the bicontinuous structure. In this case, when a water tree is generated starting from a minute foreign object or a minute void, the water tree is likely to propagate along the flexible phase of the bicontinuous structure.
[0016] (ii) In the case where the phase structure of the insulating layer is a sea-island structure having only a sea phase and small islands having a size of 100 nm or less as a soft phase, coarse crystals grow in the sea phase containing the propylene-based resin. Therefore, when a minute foreign object or a minute void is mixed into the insulating layer, water trees are likely to propagate at the interface of the coarse crystals.
[0017] (Deterioration of insulation when bent) Conventionally, in order to evaluate the insulation of an insulating layer, for example, the AC breakdown field strength has been measured. The measurement has been performed on a sheet taken from the insulating layer of a power cable immediately after production, without applying any particular stress.
[0018] However, it was found that even if the power cable has a high AC breakdown field strength in the above-mentioned measurement, the AC breakdown field strength decreases when the power cable is bent. Specifically, it was found that the bending resistance of the insulating layer may decrease depending on the phase structure of the insulating layer as follows.
[0019] (iii) In the case where the phase structure of the insulating layer is a sea-island structure having only a sea phase and a large island phase having a size of more than 100 nm as a soft phase, the elasticity of the sea phase containing the propylene-based resin is maintained at a high level. Therefore, when the power cable is bent, cracks are generated in the sea phase or the crystals are separated from each other. This may result in a decrease in the insulating properties of the insulating layer.
[0020] Therefore, the inventors conducted intensive research into the above-mentioned new problem, and as a result, by optimizing the phase structure of the insulating layer, they succeeded in suppressing the occurrence of water trees originating from tiny foreign objects or tiny voids in the insulating layer while ensuring the bending resistance of the insulating layer.
[0021] The present disclosure is based on the above-mentioned findings discovered by the inventors.
[0022] <Embodiments of the present disclosure> Next, embodiments of the present disclosure will be listed and described.
[0023] [1] A resin composition according to one embodiment of the present disclosure, A resin composition constituting an insulating layer of a power cable, Contains propylene units and styrene units, The resin composition comprises In the elastic modulus distribution obtained by measuring the elasticity of a small area using a scanning probe microscope at 25°C, a marine phase having an elastic modulus of more than 100 MPa; A first island phase having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less; A second island phase having an elastic modulus of 100 MPa or less and a size of more than 100 nm and not more than 2000 nm; Equipped with. According to this configuration, by optimizing the phase structure of the insulating layer, it is possible to ensure the bending resistance of the insulating layer while suppressing the occurrence of water trees originating from tiny foreign objects or tiny voids in the insulating layer.
[0024] [2] A power cable according to one embodiment of the present disclosure includes: A conductor; an insulating layer provided so as to cover an outer periphery of the conductor; Equipped with The insulating layer includes a propylene unit and a styrene unit, The insulating layer is In the elastic modulus distribution obtained by measuring the elasticity of a small area using a scanning probe microscope at 25°C, a marine phase having an elastic modulus of more than 100 MPa; A first island phase having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less; A second island phase having an elastic modulus of 100 MPa or less and a size of more than 100 nm and not more than 2000 nm; Equipped with. According to this configuration, by optimizing the phase structure of the insulating layer, it is possible to ensure the bending resistance of the insulating layer while suppressing the occurrence of water trees originating from tiny foreign objects or tiny voids in the insulating layer.
[0025] [3] In the power cable according to the above [2], The maximum length of the water tree in the insulation layer generated by the water needle test is 200 μm or less. Here, the water needle test is providing a plate electrode on a first surface of the block taken from the insulating layer; forming a needle-shaped gap having a tip with a radius of curvature of 10 μm at a position facing the first surface with a gap of 1 mm; A step of forming a water needle in the block by injecting artificial seawater having a salinity of 3.8% by mass into the gap; applying an AC voltage of 1000 Hz and 4 kV between the plate electrode and the tip of the water needle for 200 hours; Includes. According to this configuration, even if minute foreign matter or minute voids are mixed into the insulating layer, excessive propagation of water trees can be suppressed.
[0026] [4] The power cable according to the above [2] or [3], The AC breakdown field strength of the insulating layer at 25°C after a predetermined bending test is 50 kV / mm or more. Here, the bending test is a first step of bending the power cable so that a bending ratio of a bending radius of the power cable to an outer diameter of the insulating layer is 7 or less; a second step of bending the power cable in a direction opposite to the bending direction of the first step at a bending ratio equal to the bending ratio of the first step; Includes. According to this configuration, even if the power cable is bent, it is possible to maintain high insulation properties of the insulating layer.
[0027] [5] In the power cable according to any one of [2] to [4] above, The insulating layer further comprises a butene unit, The content of the butene units in the insulating layer is not less than 9 mass % and less than 20 mass %. According to this configuration, the above-mentioned sea-island structure can be stably formed.
[0028] [6] The power cable according to any one of [2] to [5] above, The insulating layer is A propylene-based resin, a first styrenic elastomer comprising propylene units or butene units and styrene units; a second styrenic elastomer containing propylene units or butene units and styrene units and different from the first styrenic elastomer; has. According to this configuration, two island phases having different sizes can be stably formed in the insulating layer.
[0029] [Details of the embodiment of the present disclosure] Next, an embodiment of the present disclosure will be described below with reference to the drawings. Note that the present disclosure is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.
[0030] <One embodiment of the present disclosure> (1) Resin composition The resin composition of the present embodiment constitutes, for example, an insulating layer 130 of a power cable 10 described later.
[0031] The resin composition of the present embodiment contains, for example, a propylene-based resin and a low crystalline resin as resin components. The term "resin component" as used herein means a resin material (polymer) that constitutes the main component of the resin composition. The term "main component" means a component that is contained in the largest proportion.
[0032] By mixing the propylene-based resin with a low-crystalline resin, excessive crystal growth of the propylene-based resin can be inhibited, and the flexibility of the insulating layer 130 can be improved.
[0033] (Propylene-based resin) The propylene-based resin of the present embodiment constitutes the main component of the insulating layer and contains at least propylene units as the main chain. Examples of the propylene-based resin include homopolypropylene (homo PP), random polypropylene (random PP), and block polypropylene (block PP).
[0034] By analyzing the resin composition of the present embodiment with a nuclear magnetic resonance (NMR) device, for example, when the propylene-based resin is random PP or block PP, propylene units and ethylene units are detected, and when the low crystalline resin is homo PP, propylene units are detected.
[0035] From the viewpoint of obtaining high insulation in the insulating layer 130, the propylene-based resin may be random PP. Homo PP has a larger amount of crystals than random PP, and can obtain high insulation. However, the insulating layer 130 containing homo PP may cause cracks in the crystals or between the crystals. For this reason, the inherent insulation properties of homo PP may not be obtained. In contrast, since random PP contains ethylene units, the amount of crystals is small. However, the insulating layer 130 containing random PP is less likely to cause cracks due to coarse crystallization. As a result, the random PP can obtain high insulation properties compared to homo PP.
[0036] When the propylene-based resin is random PP, the ethylene unit content in the random PP may be, for example, 0.5% by mass or more and 15% by mass or less. By making the ethylene unit content 0.5% by mass or more, it is possible to suppress the growth of coarse spherulites. On the other hand, by making the ethylene unit content 15% by mass or less, it is possible to suppress the decrease in melting point and stably realize the use in a non-crosslinked or slightly crosslinked state.
[0037] In this embodiment, the stereoregularity of the polypropylene is not particularly limited, but may be, for example, isotactic. Isotactic polypropylene is polymerized with a Ziegler-Natta catalyst and is versatile. When the stereoregularity is isotactic, the melting point can be suppressed from decreasing in a composition in which a propylene-based resin and a low-crystalline resin are mixed. This allows the high insulating properties inherent to the propylene-based resin to be obtained.
[0038] In this embodiment, the storage modulus of the propylene-based resin alone is, for example, 300 MPa or more and 2500 MPa or less.
[0039] The "storage modulus" referred to here is measured by dynamic mechanical analysis (DMA) in accordance with JIS K7244-4:1999.
[0040] The dynamic viscoelasticity measurement is carried out under the following conditions. Measurement mode: Tensile mode Distortion: 0.08% Frequency: 10Hz Temperature range: 0℃ to 200℃ Heating rate: 10℃ / min The above-mentioned "storage modulus" is a value measured at 25°C by the dynamic viscoelastic measurement.
[0041] By setting the storage modulus of the propylene-based resin alone to 300 MPa or more, it is possible to ensure the rigidity of the insulating layer 130. On the other hand, by setting the storage modulus of the propylene-based resin alone to 2500 MPa or less, it is possible to ensure the flexibility of the insulating layer 130.
[0042] The melt flow rate (MFR) of the propylene-based resin is not particularly limited, but may be, for example, 0.1 g / 10 min to 10.0 g / 10 min, or 0.1 g / 10 min to 5.0 g / 10 min. The "MFR" here is a value measured in accordance with JIS K7210 at a temperature of 230° C. and a load of 2.16 kg. By setting the MFR of the propylene-based resin within the above range, a sea-island structure, which will be described later, can be easily formed in the insulating layer 130.
[0043] The melting point of the propylene-based resin is not particularly limited, but may be, for example, 130° C. or higher and 165° C. or lower. This makes it possible to easily form a sea-island structure, which will be described later, when the propylene-based resin is mixed with the low-crystalline resin.
[0044] (Low crystalline resin) The low crystalline resin of the present embodiment is configured to control the crystallinity of the propylene-based resin and impart flexibility to the insulating layer. For example, the low crystalline resin does not have a melting point, or the melting point of the low crystalline resin is less than 100° C. The heat of fusion of the low crystalline resin may be, for example, 50 J / g or less, or 30 J / g or less.
[0045] The low crystalline resin of the present embodiment is, for example, a styrene-based elastomer, which can form island phases, which will be described later.
[0046] The styrene-based elastomer as the low crystalline resin contains a styrene unit as a hard segment and at least a propylene unit or a butene unit as a soft segment. The styrene-based elastomer may contain at least one monomer unit selected from, for example, an ethylene unit and an isoprene unit as another soft segment.
[0047] Examples of styrene-based elastomers include: Styrene butadiene styrene block copolymer (SBS), Hydrogenated styrene butadiene styrene block copolymer, Styrene ethylene propylene copolymer (SEP), Styrene-isoprene-styrene copolymer (SIS), Hydrogenated styrene-isoprene styrene copolymer, Hydrogenated styrene butadiene rubber, Hydrogenated styrene isoprene rubber, Styrene ethylene butene olefin crystalline block copolymer, Among these, two or more kinds may be used in combination.
[0048] Here, "hydrogenated" means that hydrogen has been added to the double bond. For example, "hydrogenated styrene butadiene styrene block copolymer" means a polymer in which hydrogen has been added to the double bond of a styrene butadiene styrene block copolymer. Note that no hydrogen has been added to the double bond of the aromatic ring of styrene. "Hydrogenated styrene butadiene styrene block copolymer" can be rephrased as styrene ethylene butene styrene block copolymer (SEBS).
[0049] Among styrene-based elastomers, hydrogenated materials that do not contain double bonds in the chemical structure excluding aromatic rings may be used. When a non-hydrogenated material is used, the resin component may be thermally deteriorated during molding of the resin composition, and the properties of the resulting molded product may be reduced. In contrast, the use of a hydrogenated material can improve resistance to thermal deterioration. This allows the properties of the molded product to be maintained at a higher level.
[0050] In this embodiment, the resin composition contains two styrene-based elastomers (a first styrene-based elastomer and a second styrene-based elastomer) as low crystalline resins. The first styrene-based elastomer contains a propylene unit or a butene unit, and a styrene unit. The second styrene-based elastomer contains a propylene unit or a butene unit, and a styrene unit, and is different from the first styrene-based elastomer. The content of at least one monomer unit in the second styrene-based elastomer is different from the content of at least one monomer unit in the first styrene-based elastomer. This allows two island phases having different sizes to be stably formed in the insulating layer 130.
[0051] The content of propylene units or butene units in the second styrene-based elastomer is, for example, less than the content of propylene units or butene units in the first styrene-based elastomer. Since the second styrene-based elastomer contains relatively few propylene units or butene units, which have good compatibility with propylene-based resins, the second styrene-based elastomer can be aggregated to form a large island phase containing the second styrene-based elastomer (second island phase described below). On the other hand, since the first styrene-based elastomer contains relatively many propylene units or butene units, the first styrene-based elastomer can be finely dispersed to form a small island phase containing the first styrene-based elastomer (first island phase described below).
[0052] Specifically, the content of propylene units or butene units in the first styrene-based elastomer is, for example, 40% by mass or more and 80% by mass or less. By making the content of propylene units or butene units in the first styrene-based elastomer 40% by mass or more, the first styrene-based elastomer can be finely dispersed. On the other hand, by making the content of propylene units or butene units in the first styrene-based elastomer 80% by mass or less, the rigidity of the insulating layer 130 can be ensured.
[0053] On the other hand, the content of propylene units or butene units in the second styrene-based elastomer is, for example, 5% by mass or more and less than 40% by mass. By making the content of propylene units or butene units in the second styrene-based elastomer 5% by mass or more, it is possible to ensure the flexibility of the insulating layer 130. On the other hand, by making the content of propylene units or butene units in the second styrene-based elastomer less than 40% by mass, it is possible to aggregate the second styrene-based elastomer and stably form large island phases containing the second styrene-based elastomer (second island phases described later).
[0054] The content of styrene units in the second styrene elastomer is, for example, higher than the content of styrene units in the first styrene elastomer. This allows the compatibility of the second styrene elastomer with the propylene resin to be lower than that of the first styrene elastomer. As a result, the island phase containing the second styrene elastomer (the second island phase described below) can be easily made larger than the island phase containing the first styrene elastomer (the first island phase described below).
[0055] Specifically, the content of the styrene unit in the first styrene elastomer may be, for example, 20% by mass or less, or 10% by mass or less. By setting the content of the styrene unit in the first styrene elastomer to 20% by mass or less, the first styrene elastomer can be finely dispersed. Furthermore, by setting the content of the styrene unit in the first styrene elastomer to 10% by mass or less, the first styrene elastomer can be finely dispersed while efficiently softening the insulating layer 130.
[0056] On the other hand, the content of the styrene unit in the second styrene-based elastomer is, for example, more than 20 mass% and not more than 70 mass%. By making the content of the styrene unit in the second styrene-based elastomer more than 20 mass%, the second styrene-based elastomer can be aggregated. On the other hand, by making the content of the styrene unit in the second styrene-based elastomer not more than 70 mass%, the flexibility of the insulating layer 130 can be ensured.
[0057] In this embodiment, the storage modulus of the styrene-based elastomer alone is, for example, 0.1 MPa or more and 100 MPa or less. The measurement method and conditions for the "storage modulus of the styrene-based elastomer alone" are the same as those for the storage modulus of the propylene-based resin described above. By setting the storage modulus of the styrene-based elastomer alone to 0.1 MPa or more, the rigidity of the insulating layer 130 can be ensured. On the other hand, by setting the storage modulus of the styrene-based elastomer alone to 400 MPa or less, the flexibility of the insulating layer 130 can be ensured.
[0058] The MFR of the styrene-based elastomer is not particularly limited, but may be, for example, 0.1 g / 10 min to 30.0 g / 10 min, or 0.1 g / 10 min to 10.0 g / 10 min. The measurement conditions for the MFR of the styrene-based elastomer are the same as those described for the MFR of the propylene-based resin. When the MFR of the styrene-based elastomer is within the above range, the sea-island structure described below can be easily formed in the insulating layer 130.
[0059] (Monomer unit content in resin composition) The content of the monomer units in the resin composition (insulating layer 130 described below) is measured by subjecting the resin composition to an NMR device, where the total content of the monomer units in the resin composition is taken as 100 mass %.
[0060] The content of the propylene unit in the resin composition is, for example, more than 50% by mass and 80% by mass or less. The propylene-based resin phase can be formed as a sea phase throughout the entire insulating layer. This makes it possible to ensure the insulating properties of the propylene-based resin as the main component while making the insulating layer 130 non-crosslinked. On the other hand, by making the content of the propylene unit 80% by mass or less, it is possible to ensure an island phase containing a low crystalline resin in the insulating layer 130. This makes it possible to suppress excessive crystal growth of the propylene-based resin.
[0061] In this embodiment, when the resin composition contains propylene units, butene units, and styrene units, the content of butene units in the resin composition is, for example, 9% by mass or more and less than 20% by mass. This allows a sea-island structure, which will be described later, to be stably formed in the insulating layer 130. The phase structure will be described in detail later.
[0062] In this embodiment, the content of the styrene unit in the resin composition is, for example, 0.1 mass% or more and less than 15%. By making the content of the styrene unit 0.1 mass% or more, it is possible to stabilize the insulating property of the insulating layer 130. On the other hand, by making the content of the styrene unit less than 15 mass%, it is possible to ensure the flexibility of the insulating layer 130.
[0063] The resin composition may contain, as a monomer unit other than the propylene unit, the butene unit, and the styrene unit, for example, an ethylene unit derived from a propylene-based resin or a low-crystalline resin.
[0064] In this embodiment, the content of each of the first styrene-based elastomer and the second styrene-based elastomer as low crystalline resins in the resin composition is adjusted based on the content of the above-mentioned monomer units in the resin composition when the resin components are mixed.
[0065] (Crosslinking agent) In this embodiment, the resin component constituting the insulating layer 130 may be non-crosslinked from the viewpoint of recycling. In this case, the resin composition may not contain a crosslinking agent.
[0066] On the other hand, the resin composition may contain a small amount of a crosslinking agent so as to reduce the gel fraction (degree of crosslinking). Specifically, the resin composition may contain a crosslinking agent so that the crosslinking agent residue in the insulating layer 130 is less than 300 ppm. The "residue of the crosslinking agent (decomposition residue)" here means a decomposition product generated by the decomposition of the crosslinking agent due to the crosslinking reaction. When dicumyl peroxide is used as the crosslinking agent, the residue is, for example, cumyl alcohol, α-methylstyrene, etc.
[0067] (Other additives) In addition to the above-mentioned resin components, the resin composition may contain, for example, an antioxidant, a heat stabilizer, a copper inhibitor, a lubricant, and a colorant.
[0068] The resin composition may not contain a metal hydroxide that serves as a flame retardant. Alternatively, even if the resin composition contains a metal oxide, the content of the metal oxide in the resin composition may be 1 part by mass or less when the content of the resin component in the resin composition is 100 parts by mass. This allows the insulating layer 130 to have stable insulation properties.
[0069] (2) Power cable Next, the power cable of this embodiment will be described with reference to FIG.
[0070] The power cable 10 of this embodiment is configured as a so-called solid insulated power cable. The power cable 10 of this embodiment is configured to be laid, for example, on land (in a pipe), underwater, or at the bottom of the water. The power cable 10 may be used, for example, for AC or DC.
[0071] Specifically, the power cable 10 includes, for example, a conductor 110 , an inner semiconductive layer 120 , an insulating layer 130 , an outer semiconductive layer 140 , a shielding layer 150 , and a sheath 160 .
[0072] (Conductor (conductive part)) The conductor 110 is formed by twisting together a plurality of conductor core wires (conductive core wires) containing, for example, pure copper, a copper alloy, aluminum, or an aluminum alloy.
[0073] (internal semiconductive layer) The internal semiconductive layer 120 is provided so as to cover the outer periphery of the conductor 110. The internal semiconductive layer 120 has semiconductivity and is configured to suppress electric field concentration on the surface of the conductor 110. The internal semiconductive layer 120 contains, for example, at least one of an ethylene-based copolymer such as an ethylene-ethyl acrylate copolymer, an ethylene-methyl acrylate copolymer, an ethylene-butyl acrylate copolymer, and an ethylene-vinyl acetate copolymer, an olefin-based elastomer, and the above-mentioned low crystalline resin, and conductive carbon black.
[0074] (insulating layer) The insulating layer 130 is provided so as to cover the outer periphery of the internal semiconductive layer 120. The insulating layer 130 is, for example, extrusion molded from a resin composition as described above. The phase structure of the insulating layer 130 and the cable characteristics will be described in detail later.
[0075] (Outer semiconducting layer) The outer semiconductive layer 140 is provided so as to cover the outer periphery of the insulating layer 130. The outer semiconductive layer 140 has semiconductivity and is configured to suppress electric field concentration between the insulating layer 130 and the shielding layer 150. The outer semiconductive layer 140 is configured, for example, from the same material as the inner semiconductive layer 120.
[0076] (shielding layer) The shielding layer 150 is provided so as to cover the outer periphery of the outer semiconductive layer 140. The shielding layer 150 is formed, for example, by winding a copper tape, or is formed as a wire shield in which a plurality of soft copper wires or the like are wound. Note that a tape made of a material such as a rubber-coated cloth may be wound on the inside or outside of the shielding layer 150.
[0077] (sheath) The sheath 160 is provided so as to cover the outer periphery of the shielding layer 150. The sheath 160 is made of, for example, polyvinyl chloride or polyethylene.
[0078] If the power cable 10 of this embodiment is an underwater cable or an underwater cable, it may have a metal waterproof layer such as an aluminum sheath or an iron wire armor outside the shielding layer 150.
[0079] On the other hand, the power cable 10 of the present embodiment may not have a water-impermeable layer outside the shielding layer 150. In other words, the power cable 10 of the present embodiment may be configured to have a non-completely water-impermeable structure.
[0080] (Specific dimensions, etc.) Although there are no particular limitations on the specific dimensions of the power cable 10, for example, the diameter of the conductor 110 is 5 mm or more and 60 mm or less, the thickness of the inner semiconductive layer 120 is 0.5 mm or more and 3 mm or less, the thickness of the insulating layer 130 is 3 mm or more and 35 mm or less, the thickness of the outer semiconductive layer 140 is 0.5 mm or more and 3 mm or less, the thickness of the shielding layer 150 is 0.1 mm or more and 5 mm or less, and the thickness of the sheath 160 is 1 mm or more. The AC voltage applied to the power cable 10 of this embodiment is, for example, 20 kV or more.
[0081] (3) Phase structure of the insulating layer The inventors have discovered a phase structure of the insulating layer 130 that can solve the above-mentioned new problems by measuring the micro-area elasticity of the insulating layer 130 that contains a resin composition.
[0082] The "micro-area elasticity measurement" referred to here is performed using a scanning probe microscope (SPM). In this measurement, for example, a sheet having a predetermined thickness cut out from the center in the thickness direction of the insulating layer 130 is used. In the micro-area elasticity measurement, for example, at 25°C, the elastic modulus is measured under the condition that a cantilever made of silicon (single crystal) and having a tip with a radius of curvature of 1 nm or more and less than 20 nm is used to tap the sample 16,000 times within a 1 μm square range.
[0083] Such micro-area elasticity measurement makes it possible to obtain the elastic modulus distribution in the insulating layer 130. This makes it possible to grasp the phase structure of the insulating layer 130 based on the elastic modulus distribution.
[0084] For example, by observing the elastic modulus distribution with a threshold value of 200 MPa, it is possible to know whether the phase structure of the insulating layer 130 is a co-continuous structure or not. Here, the propylene unit or butene unit in the styrene-based elastomer easily mixes with the propylene-based resin. The portion where the styrene-based elastomer and the propylene-based resin are mixed has an elastic modulus of, for example, 200 MPa or less as an intermediate elastic modulus between the elastic modulus of the propylene-based resin and the elastic modulus of the styrene-based resin. When such a phase with an elastic modulus of 200 MPa or less is connected as a continuous phase, water trees tend to extend in the phase. Therefore, by observing the elastic modulus distribution with a threshold value of 200 MPa, it is possible to determine whether the insulating layer 130 has a co-continuous structure in which water trees tend to extend.
[0085] Furthermore, for example, by observing the elastic modulus distribution with a threshold elastic modulus of 100 MPa, it is possible to measure the size of the island phases when the phase structure of the insulating layer 130 is an island structure. That is, since the styrene-based elastomer exhibits an elastic modulus of less than 100 MPa in the micro-area elasticity measurement, it is possible to measure the size of the island phases derived from the styrene-based elastomer by observing with a threshold elastic modulus of 100 MPa.
[0086] In this embodiment, the insulating layer 130 has, in the elastic modulus distribution obtained by micro-area elasticity measurement using an SPM at 25°C, for example, a sea phase having an elastic modulus of more than 100 MPa, a first island phase having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less, and a second island phase having an elastic modulus of 100 MPa or less and a size of more than 100 nm and 2000 nm or less.
[0087] In this embodiment, the resin composition constituting the insulating layer 130 can stably form the above-mentioned phase structure in the insulating layer 130 by, for example, satisfying the following requirements. The (A) resin composition contains a propylene-based resin and two styrene-based elastomers as low-crystalline resins. (B) When the resin composition contains propylene units, butene units, and styrene units, the content (mass percent concentration) of butene units in the resin composition is 9 mass % or more and less than 20 mass %. (C) The new mixing method described below is applied.
[0088] The phase structure of the insulating layer 130 of this embodiment will be described below with reference to Figs. 2 to 5. As an example, the phase structure of the insulating layer 130 of this embodiment will be compared with that of a reference example in the case where the resin composition constituting the insulating layer 130 contains propylene units, butene units, and styrene units. Figs. 2 to 5 show the elastic modulus distribution obtained by measuring the elasticity of a small area using an SPM at 25°C. In Figs. 2 to 5, the gray areas indicate areas having an elastic modulus equal to or lower than the threshold value shown at the top of each figure.
[0089] (Reference Example 1: Co-continuous structure) For example, in Reference Example 1, in which the content of butene units in the resin composition is 20 mass% or more, regardless of whether the resin composition contains two styrene-based elastomers as low-crystalline resins, the phase structure of the insulating layer 130 is a co-continuous structure as shown in Figure 3.
[0090] As shown in the elastic modulus distribution in Figure 3, the bicontinuous structure of Reference Example 1 has, for example, a first continuous phase CP1 having an elastic modulus of more than 200 MPa and a second continuous phase CP2 having an elastic modulus of less than 200 MPa. The first continuous phase CP1 is derived from a propylene-based resin. The second continuous phase CP2 is mainly derived from a styrene-based elastomer as a low-crystalline resin.
[0091] In the bicontinuous structure, the first continuous phase CP1 and the second continuous phase CP2 are each long and continuous. In the elastic modulus distribution with a threshold elastic modulus of 200 MPa, the length between both ends of the second continuous phase CP2 is, for example, 5 μm or more. The "length between both ends of the second continuous phase CP2" here refers to the length of a straight line connecting the first end of the second continuous phase CP2 to the second end that is the furthest from the first end.
[0092] In the case where the insulating layer 130 has a phase structure of the above-mentioned co-continuous structure, when minute foreign matter or minute voids are mixed into the insulating layer 130, the minute foreign matter or minute voids may be incorporated into the soft second continuous phase CP2 containing a styrene-based elastomer. In this case, when water trees are generated starting from the minute foreign matter or minute voids, the water trees are likely to propagate along the second continuous phase CP2 of the co-continuous structure.
[0093] (Reference Example 2: Sea-island structure with only microisland phases) For example, in Reference Example 2, in which the resin composition contains only a styrene-based elastomer with a high butene unit content as the low crystalline resin and the content of butene units in the resin composition is less than 20 mass%, the phase structure of the insulating layer 130 is, for example, a sea-island structure having only the microisland phase SIP shown in Figure 4.
[0094] As shown in the elastic modulus distribution in Figure 4, the sea-island structure of Reference Example 2 has, for example, a sea phase SP having an elastic modulus of more than 100 MPa and a microisland phase SIP having an elastic modulus of less than 100 MPa. The sea phase SP is derived from a propylene-based resin. The microisland phase SIP is derived from a styrene-based elastomer as a low-crystalline resin. The size of the microisland phase SIP is, for example, 100 nm or less.
[0095] In the case where the phase structure of the insulating layer 130 is a sea-island structure having only the micro-island phases SIP as described above, coarse crystals grow in the sea phase SP containing the propylene-based resin. Therefore, when minute foreign matter or minute voids are mixed into the insulating layer 130, water trees tend to propagate at the interfaces of the coarse crystals.
[0096] (Reference Example 3: Sea-island structure having only coarse island phases) For example, in Reference Example 3, in which the resin composition contains only a styrene-based elastomer with a low butylene unit content as the low crystalline resin and the content of butene units in the resin composition is less than 9 mass%, the phase structure of the insulating layer 130 is, for example, a sea-island structure having only the coarse island phase LIP as shown in Figure 5.
[0097] In the elastic modulus distribution shown in Figure 5, the sea-island structure of Reference Example 3 has, for example, a sea phase SP having an elastic modulus of more than 100 MPa and a fine island phase SIP having an elastic modulus of less than 100 MPa. The sea phase SP is derived from a propylene-based resin. The coarse island phase LIP is derived from a styrene-based elastomer as a low-crystalline resin. The size of the coarse island phase LIP is, for example, more than 100 nm.
[0098] When the insulating layer 130 has a sea-island structure having only the coarse island phases LIP as described above, the elasticity of the sea phase SP containing the propylene-based resin is maintained at a high level. Therefore, when the power cable 100 is bent, the sea phase SP may crack or the crystals may separate from each other. This may result in a decrease in the insulating properties of the insulating layer 130.
[0099] In addition, for example, even when the resin composition constituting insulating layer 130 does not contain a styrene-based elastomer, or when the resin composition constituting insulating layer 130 satisfies the above-mentioned (A) and (B) but does not satisfy (C), the phase structure of insulating layer 130 will be a sea-island structure similar to that of Reference Example 3.
[0100] (This embodiment: a sea-island structure having two islands of different sizes) In contrast, in this embodiment, the resin composition constituting the insulating layer 130 satisfies, for example, the above-mentioned requirements (A), (B), and (C), and the phase structure of the insulating layer 130 becomes, for example, a sea-island structure as shown in FIG. 2.
[0101] That is, in this embodiment, the resin composition (A) contains a propylene-based resin and two styrene-based elastomers as low-crystalline resins, and thus it is possible to form two island phases (a first island phase IP1 and a second island phase IP2) of different sizes.
[0102] In this embodiment, by making the content of butene units in the (B) resin composition 9% by mass or more, the compatibility of each styrene-based elastomer with the propylene-based resin is ensured, and excessive aggregation of each styrene-based elastomer can be suppressed. This allows the first island phase IP1 to be finely dispersed in the sea phase SP. Furthermore, excessive aggregation of the second island phase IP2 can be suppressed.
[0103] In this embodiment, by making the content of butene units in the (B) resin composition less than 20% by mass, it is possible to prevent each styrene-based elastomer from being excessively compatible with the propylene-based resin, thereby preventing the formation of a co-continuous structure.
[0104] In this embodiment, by applying a novel mixing method described later, it is possible to apply a high shear force to the resin composition and ensure a sufficient residence time of the resin composition in the cylinder, thereby stably forming the sea-island structure of this embodiment.
[0105] Specifically, as shown in the elastic modulus distribution in FIG. 2, the sea-island structure of this embodiment includes, for example, a sea phase SP, a first island phase IP1, and a second island phase IP2.
[0106] The marine SP has a modulus of elasticity above 100 MPa. The marine SP is derived from a propylene-based resin. The marine SP spans the entire modulus distribution.
[0107] The first island phase IP1 has an elastic modulus of 100 MPa or less and a size of 0.1 nm to 100 nm. The "size of the first island phase IP1" here refers to the maximum length of a straight line connecting the first end of the first island phase IP1 to the second end, which is the furthest end.
[0108] The first island phase IP1 is, for example, mainly derived from the first styrene-based elastomer. That is, the first island phase IP1 contains at least a styrene unit. The styrene unit in the first island phase IP1 can be observed by staining a sample taken from the insulating layer 130 with a heavy metal using a transmission electron microscope (TEM).
[0109] The second island phase IP2 has an elastic modulus of 100 MPa or less and a size of more than 100 nm and not more than 2000 nm. The method for measuring the size of the second island phase IP2 is the same as the method for measuring the size of the first island phase IP1 described above.
[0110] The second island phase IP2 is mainly derived from the second styrene-based elastomer, for example. That is, the second island phase IP2 contains at least styrene units. The styrene units in the second island phase IP2 can be observed by TEM using the same method as described for the first island phase IP1.
[0111] The ratio of the total area of the first island phase IP1 and the second island phase IP2 to the unit area of the elastic modulus distribution (hereinafter also referred to as the "island phase total area ratio") is, for example, 10% or more and 70% or less. By setting the island phase total area ratio to 10% or more, it is possible to suppress the formation of coarse crystals in the sea phase SP. This makes it possible to make the insulating layer 130 flexible. On the other hand, by setting the island phase total area ratio to 70% or less, it is possible to ensure the insulating properties of the sea phase SP.
[0112] The ratio of the area of the first island phase IP1 to the unit area of the elastic modulus distribution (hereinafter also referred to as "first island phase area ratio") is, for example, 1% or more and 40% or less. By setting the first island phase area ratio to 1% or more, the first island phase IP1 can be sufficiently dispersed in the sea phase SP. This makes it possible to make the insulating layer 130 flexible. On the other hand, by setting the total first island phase area ratio to 40% or less, the insulating properties of the sea phase SP can be ensured.
[0113] The ratio of the area of the second island phase IP2 to the unit area of the elastic modulus distribution (hereinafter also referred to as the "second island phase area ratio") is, for example, 5% or more and 30% or less. By setting the second island phase area ratio to 5% or more, the formation of coarse crystals of the sea phase SP can be suppressed. On the other hand, by setting the second island phase total area ratio to 30% or less, the insulating properties of the sea phase SP can be ensured.
[0114] Furthermore, in the sea phase SP, the diameter of the circular island phase free region (region within the dashed line in the figure) that does not include the first island phase IP1 and the second island phase IP2 is, for example, 5 nm or more and 400 nm or less. When the diameter of the island phase free region is 5 nm or more, the insulating properties of the sea phase SP can be ensured. On the other hand, when the diameter of the island phase free region is 400 nm or less, the formation of coarse crystals of the sea phase SP can be suppressed. This makes it possible to make the insulating layer 130 flexible.
[0115] (4) Cable characteristics In this embodiment, since the insulating layer 130 has the above-mentioned sea-island structure, the bending resistance of the insulating layer 130 can be ensured while suppressing the occurrence of water trees originating from micro-foreign objects or micro-voids in the insulating layer 130.
[0116] (Water tree resistant) The inventors evaluated the water tree resistance of the insulating layer 130 by performing a water tree test (hereinafter also referred to as a “water needle test”) using a water needle that simulates a micro-foreign object or micro-void that has been trapped in the insulating layer 130.
[0117] The "water needle test" referred to here is performed in the following procedure, as shown in Figure 6.
[0118] First, a hexahedral block IB is cut from the insulating layer 130. After the block IB is cut, a plate electrode FE is provided on a first surface S1 of the block IB.
[0119] After the plate electrode FE is provided, a needle-shaped gap is formed along the normal direction from the second surface S2 opposite to the first surface S1 of the block IB. At this time, the needle-shaped gap is formed at a position facing the first surface S1 of the block IB with a distance d of 1 mm, so that the tip of the needle-shaped gap has a curvature radius of 10 μm.
[0120] After forming a gap in block IB, artificial seawater with a salinity of 3.8% by mass is injected into the gap, forming a water needle WN in block IB.
[0121] In the above-mentioned state, an AC voltage of 1000 Hz and 4 kV is applied between the plate electrode FE and the tip of the water needle WN for 200 hours.
[0122] After the water needle test, the length of the water tree that has developed at the tip of the water needle WN is measured.
[0123] Thus, in the water needle test of this embodiment, the tip of the water needle WN is sharpened to simulate a minute foreign object or a minute void trapped in the insulating layer 130. Therefore, a high electric field is applied locally near the tip of the water needle WN. Therefore, the water needle test of this embodiment makes it much easier for water trees to occur compared to the conventional water tree test in which an electric field is applied uniformly to the insulating layer.
[0124] In this embodiment, the maximum length of the water tree in the insulating layer 130 caused by the water needle test is, for example, 200 μm or less. That is, even in the test in which water treeing is likely to occur as described above, the maximum length of the water tree in the insulating layer 130 can be shortened.
[0125] (Insulation after bending test) In this embodiment, the insulating layer 130 has the above-mentioned sea-island structure, and thus has resistance to a predetermined bending test.
[0126] The "bending test" here includes, for example, a first step of bending the power cable 10 so that the bending ratio (hereinafter also simply referred to as the "bending ratio") of the bending radius of the power cable 10 to the outer diameter of the insulating layer 130 is 7 or less, and a second step of bending the power cable 10 in the direction opposite to the bending direction of the first step at the same bending ratio as the bending ratio of the first step.
[0127] In a bending test according to normal cable standards, the bending ratio of the bending radius of the power cable to the outer diameter of the insulating layer is set to, for example, about 20.
[0128] In contrast, the bending ratio in the bending test of this embodiment is smaller than the bending ratio in the bending test of the normal cable standard. Therefore, in the bending test of this embodiment, the bending stress applied to the insulating layer 130 is strong. As a result, defects are likely to occur in the insulating layer 130 due to the bending test.
[0129] In this embodiment, even after the bending test described above, the AC breakdown field strength is maintained high.
[0130] That is, in this embodiment, the AC breakdown field strength of the insulating layer 130 at room temperature (eg, 25° C.) after the above-mentioned bending test may be, for example, 50 kV / mm or more, or 60 kV / mm or more.
[0131] The "AC breakdown field strength" referred to here is measured at room temperature (25°C) by applying an AC voltage of commercial frequency (e.g., 60 Hz) of 10 kV to a sample with a thickness of 0.4 mm for 10 minutes, and then increasing the voltage by 1 kV in increments of 10 minutes, repeating this cycle.
[0132] In this embodiment, the AC breakdown field strength of the insulating layer 130 at room temperature (eg, 25° C.) before the bending test is also naturally, for example, 50 kV / mm or more, or 60 kV / mm or more.
[0133] (5) Manufacturing method of power cables Next, a method for manufacturing the power cable of this embodiment will be described.
[0134] The method for producing a power cable of this embodiment includes, for example, a conductor preparing step S120, a resin composition preparing step S140, a cable core forming step 300, a shielding layer forming step S400, and a sheath forming step S500.
[0135] (S120: Conductor preparation process) Conductor 110 is prepared by twisting together a plurality of conductor core wires.
[0136] (S140: Resin composition preparation step) On the other hand, a resin composition containing propylene units and styrene units is prepared.
[0137] At this time, the resin composition is mixed so that, in the elastic modulus distribution obtained by micro-area elasticity measurement using an SPM at 25°C, the resin composition comprises a sea phase SP having an elastic modulus of more than 100 MPa, a first island phase IP1 having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less, and a second island phase IP2 having an elastic modulus of 100 MPa or less and a size of more than 100 nm and 2000 nm or less.
[0138] Specifically, in this embodiment, a propylene-based resin is mixed with two styrene-based elastomers as low-crystalline resins: a first styrene-based elastomer containing propylene units or butene units and styrene units, and a second styrene-based elastomer containing propylene units or butene units and styrene units and different from the first styrene-based elastomer.
[0139] At this time, in this embodiment, when the resin composition contains propylene units, butene units, and styrene units, the propylene-based resin is mixed with the first styrene-based elastomer and the second styrene-based elastomer as low crystalline resins so that the content of butene units in the resin composition is 9 mass% or more and less than 20 mass%.
[0140] At this time, in the present embodiment, for example, a twin-screw mixer is used to mix the resin composition. By using the twin-screw mixer, the resin composition can be mixed with a higher shear force than with a kneader.
[0141] At this time, in this embodiment, the resin composition is mixed at a temperature of, for example, less than 220°C. If the resin composition is mixed at a temperature of 220°C or higher, the viscosity of the resin composition decreases due to the high temperature. This makes it difficult to apply a predetermined shear force to the resin composition. In contrast, in this embodiment, the mixing temperature is set to less than 220°C, so that the viscosity of the resin composition can be maintained high. This makes it possible to apply a high shear force to the resin composition. As a result, the above-mentioned sea-island structure can be stably formed.
[0142] At this time, in this embodiment, for example, the installation conditions of the kneading disk in the twin-screw mixer are adjusted, and the rotation speed in the twin-screw mixer is adjusted. Here, the shear force in the twin-screw mixer can be changed, for example, by changing the kneading disk or changing the rotation speed. For example, if the kneading disks are installed at more than five places and each rotation speed is 200 rpm or more, the temperature is likely to rise during mixing. In contrast, in this embodiment, for example, the number of kneading disks installed is set to 2 or more and 5 or less, and each rotation speed is set to 20 rpm or more and less than 200 rpm. This makes it possible to suppress the temperature rise to 220 ° C. or more during mixing. By suppressing the temperature rise, it is possible to suppress the decrease in the viscosity of the resin composition. As a result, it is possible to maintain a high shear force in the twin-screw mixer.
[0143] In this embodiment, for example, the filling rate of the resin composition in the cylinder of the twin-screw mixer (the ratio of the volume of the resin composition to the volume of the cylinder) is increased to ensure the residence time of the resin composition in the cylinder. Usually, the filling rate of the resin composition in the cylinder of the twin-screw mixer is set to 20% or less to reduce the load on the equipment (the torque applied to the screw) and ensure the discharge amount. In contrast, in this embodiment, the filling rate of the resin composition in the cylinder of the twin-screw mixer is set to more than 20%, so that the residence time of the resin composition in the cylinder can be sufficiently ensured. This allows the above-mentioned sea-island structure to be stably formed.
[0144] In this manner, in this embodiment, the above-described sea-island structure can be formed in the resin composition.
[0145] After mixing the resin composition, the resin composition is granulated by an extruder, thereby forming a pellet-like resin composition that will form the insulating layer 130. Note that the steps from mixing to granulation may be performed in one go.
[0146] (S300: Cable core forming process (extrusion process, insulation layer forming process)) After the conductor preparing step S120 and the resin composition preparing step S140 are completed, the insulating layer 130 is formed so as to cover the outer periphery of the conductor 110 using the above-mentioned resin composition.
[0147] At this time, in this embodiment, by extrusion molding the insulating layer 130 using the above-mentioned resin composition, the above-mentioned sea-island structure is also formed in the insulating layer 130.
[0148] At this time, in this embodiment, for example, a three-layer co-extruder is used to simultaneously form the inner semiconductive layer 120, the insulating layer 130 and the outer semiconductive layer 140.
[0149] Specifically, for example, the composition for the inner semiconductive layer is charged into extruder A, which forms the inner semiconductive layer 120, of the three-layer co-extruder.
[0150] The above-mentioned pellet-shaped resin composition is fed into the extruder B which forms the insulating layer 130. The set temperature of the extruder B is set to a temperature which is, for example, 10° C. to 50° C. higher than the desired melting point. The set temperature is appropriately adjusted based on the linear speed and extrusion pressure.
[0151] An outer semiconductive layer composition containing the same materials as the inner semiconductive layer resin composition charged in extruder A is charged in extruder C which forms the outer semiconductive layer 140 .
[0152] Next, the extrudates from the extruders A to C are guided to a common head, and the inner semiconductive layer 120, the insulating layer 130, and the outer semiconductive layer 140 are simultaneously extruded from the inside to the outside around the periphery of the conductor 110. This forms an extruded material that will become the cable core.
[0153] The extrusion is then cooled, for example with water.
[0154] Through the above cable core formation step S300, a cable core composed of the conductor 110, the inner semiconductive layer 120, the insulating layer 130 and the outer semiconductive layer 140 is formed.
[0155] (S400: Shielding layer formation process) Once the cable core is formed, a shielding layer 150 is formed on the outside of the outer semiconducting layer 140, for example by wrapping copper tape around it.
[0156] (S500: Sheath forming process) After the shielding layer 150 is formed, vinyl chloride is put into an extruder and extruded to form a sheath 160 around the outer periphery of the shielding layer 150 .
[0157] In this manner, the power cable 10 is manufactured as a solid insulated power cable.
[0158] (6) Summary of this embodiment According to this embodiment, one or more of the following advantages are achieved.
[0159] (a) In this embodiment, the insulating layer 130 comprises, in the elastic modulus distribution obtained by microarea elasticity measurement using an SPM at 25°C, a sea phase SP having an elastic modulus of more than 100 MPa, a first island phase IP1 having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less, and a second island phase IP2 having an elastic modulus of 100 MPa or less and a size of more than 100 nm and 2000 nm or less.
[0160] By dispersing the flexible and fine first island phase IP1 in the sea phase SP containing the propylene-based resin, the propylene-based resin can be efficiently made flexible, and the insulating layer 130 as a whole can be made flexible. This makes it possible to suppress cracks in the sea phase SP even if bending stress is applied to the insulating layer 130 when the power cable 10 is bent. As a result, the insulating properties of the insulating layer 130 can be ensured even if the power cable 10 is bent.
[0161] In this state, by further dispersing the soft and large second island phase IP2 in the sea phase SP containing the propylene-based resin, even if a water tree occurs starting from a minute foreign object or a minute void, the water tree propagation can be stopped within the second island phase IP2. As a result, excessive propagation of the water tree caused by the minute foreign object or the minute void in the insulating layer 130 can be suppressed.
[0162] As described above, according to this embodiment, it is possible to suppress the occurrence of water trees originating from minute foreign particles or minute voids in the insulating layer 130 while ensuring the bending resistance of the insulating layer 130.
[0163] (b) In this embodiment, in a water needle test simulating a minute foreign object or a minute void introduced into the insulating layer 130, the maximum length of the water tree in the insulating layer 130 is 200 μm or less. That is, even in a test in which water treeing is likely to occur, the maximum length of the water tree in the insulating layer 130 can be shortened. As a result, even if a minute foreign object or a minute void is mixed into the actual insulating layer 130, excessive propagation of the water tree can be suppressed.
[0164] (c) In this embodiment, after a bending test with a bending ratio of 7 or less, the AC breakdown field strength of the insulating layer 130 at room temperature (e.g., 25°C) is 50 kV / mm or more. That is, even in a test in which a bending stress stronger than the bending stress in a bending test according to a normal cable standard is applied to the insulating layer 130, the AC breakdown field strength can be maintained high. As a result, even if the actual power cable 10 is bent, it is possible to maintain the insulation properties of the insulating layer 130 at a high level.
[0165] <Other embodiments of the present disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above-described embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.
[0166] In the above embodiment, the case where the power cable 10 does not need to have a water-impermeable layer has been described, but the present disclosure is not limited to this case. The power cable 10 may have a simple water-impermeable layer. Specifically, the simple water-impermeable layer is made of, for example, a metal laminate tape. The metal laminate tape has, for example, a metal layer made of aluminum or copper, and an adhesive layer provided on one or both sides of the metal layer. The metal laminate tape is, for example, wound vertically so as to surround the outer periphery of the cable core (outer periphery than the outer semiconductive layer). The water-impermeable layer may be provided outside the shielding layer, or may also serve as the shielding layer. With such a configuration, the cost of the power cable 10 can be reduced.
[0167] In the above embodiment, the power cable 10 is configured to be laid on land, underwater, or on the bottom of the water, but the present disclosure is not limited to this. For example, the power cable 10 may be configured as a so-called overhead electric wire (overhead insulated electric wire).
[0168] In the above embodiment, three layers are simultaneously extruded in the cable core forming step S300, but each layer may be extruded one at a time. EXAMPLES
[0169] Next, examples according to the present disclosure will be described. These examples are merely examples of the present disclosure, and the present disclosure is not limited to these examples.
[0170] (1) Power cable production Power cables of samples A1 to A3 and B1 to B8 were manufactured according to the following procedure.
[0171] (1-1) Material preparation process The following materials were prepared as the resin components of each sample.
[0172] (Propylene-based resin) Random Polypropylene (r-PP): Stereoregularity: Isotactic Ethylene unit content: 3% by mass, MFR: 1.3g / 10min (230℃, 2.16kg), Density: 0.9g / ml, Melting point: 145℃, Heat of fusion: 100J / g
[0173] (Low crystalline resin) Hydrogenated Styrene Butadiene Styrene Block Copolymer (SEBS1): Butene unit content: 65% by mass, Styrene unit content: 5% by mass, MFR:6.0g / 10min(230℃, 2.16kg), Hardness: A45, Melting point: None, Heat of fusion: None
[0174] Hydrogenated Styrene Butadiene Styrene Block Copolymer (SEBS2): Butene unit content: 25% by mass, Styrene unit content: 30% by mass, MFR: 5.0g / 10min (230℃, 2.16kg), Hardness: A84, Melting point: None, Heat of fusion: None
[0175] Hydrogenated Styrene Butadiene Styrene Block Copolymer (SEBS3): Butene unit content: 65% by mass, Styrene unit content: 12% by mass, MFR: 4.5g / 10min (230℃, 2.16kg), Hardness: A42, Melting point: None, Heat of fusion: None
[0176] Very low density polyethylene (VLDPE): ethylene-1-butene copolymer, Butene unit content: 21% by mass, MFR:6.7g / 10min(230℃, 2.16kg), Hardness: A86, Melting point: 66℃, Heat of fusion: 10J / g
[0177] (1-2) Resin composition mixing process The resin compositions for each sample were mixed using the materials described above.
[0178] (Samples A1~A3) In samples A1 to A3, r-PP, SEBS1, and SEBS2 were mixed so that the content of each monomer unit was the value shown in Table 1 below. At this time, a twin-screw mixer was used to mix the resins at a temperature of 200°C. Kneading disks were installed at three locations, each of which had a rotation speed of 100 rpm, and the filling rate of the resin composition in the cylinder was 50%. This method is also referred to as the "new mixing method" below.
[0179] (Samples B1-B7) In samples B1 to B7, resin compositions were mixed in the same manner as in sample A1, except that the low crystalline resin used and the content of each monomer unit were different.
[0180] (Sample B8) For sample B8, the resin composition was mixed in the same manner as for sample A1, except that the mixing method was different. For sample B8, the resin composition was mixed at a temperature of 220°C using a kneader.
[0181] (1-3) Post-process While mixing the resin composition as described above, a conductor core wire made of a dilute copper alloy with a diameter of 17 mm was twisted together to form a conductor having a cross-sectional area of 200 mm 2 The conductor was prepared. After the conductor was prepared, the resin composition for the internal semiconductive layer containing an ethylene-ethyl acrylate copolymer, the above-mentioned resin composition, and the resin composition for the external semiconductive layer made of the same material as the resin composition for the internal semiconductive layer were respectively fed into extruders A to C. The extrudates from the extruders A to C were guided to a common head, and the internal semiconductive layer, the insulating layer, and the external semiconductive layer were simultaneously extruded from the inside to the outside around the conductor. At this time, the thicknesses of the internal semiconductive layer, the insulating layer, and the external semiconductive layer were set to 0.5 mm, 3.5 mm, and 0.5 mm, respectively. After the extrusion process, the extruded material was cooled. As a result, the power cables of samples A1 to A3 and B1 to B8 were manufactured.
[0182] (2) Evaluation The following evaluations were performed for each sample.
[0183] (NMR) A part of the insulating layer of each of the above samples was dissolved in orthochlorobenzene and analyzed in this state at a temperature of 130° C. using a JEOL NMR device. 1 H-NMR and 13 The composition ratio of the monomer units was calculated from the peak area ratio obtained by C-NMR.
[0184] (SPM) Micro-area elasticity measurements were performed using an SPM. For these measurements, a sheet with a thickness of 1 mm cut from the center of the insulating layer of each sample in the thickness direction was used. For the micro-area elasticity measurements, the elastic modulus was measured at 25°C under the condition that a cantilever with a tip made of silicon (single crystal) and a curvature radius of 7 nm was used to tap 16,000 times within a 1 μm square area of the sample.
[0185] In the micro-area elasticity measurement, an elastic modulus distribution with an elastic modulus threshold of 200 MPa and an elastic modulus distribution with an elastic modulus threshold of 100 MPa were obtained. For each elastic modulus distribution, the field of view was set to 1.0 μm square.
[0186] In the elastic modulus distribution with a threshold elastic modulus of 200 MPa, the phase structure in which each phase is continuous without being separated was judged to be a "cocontinuous structure (B1)," and the phase structure in which each phase is separated was judged to be an "island-sea structure."
[0187] When the phase structure was judged to be an "island-sea structure," the size of the island phase was measured in the elastic modulus distribution with the threshold elastic modulus set at 100 MPa. As a result, a sea-island structure having a first island phase with an elastic modulus of 100 MPa or less and a size of 0.1 nm to 100 nm, and a second island phase with an elastic modulus of 100 MPa or less and a size of more than 100 nm to 2000 nm was evaluated as "A" as the phase structure of the present disclosure. A sea-island structure having only the first island phase was evaluated as "B2." A sea-island structure having only the second island phase was evaluated as "B3."
[0188] (Water needle test) As shown in FIG. 6, a block was taken from the insulating layer of each sample and the above-mentioned water needle test was performed.
[0189] The conditions for the water needle test were set as follows: Curvature radius of the tip of the water needle: 10μm Distance from the flat electrode on the first surface of the block to the tip of the water needle: 1 mm Salinity of artificial seawater in the water needle: 3.8% by mass Frequency: 1000MHz AC voltage: 4kV
[0190] After the water needle test, the block was dried and then boiled in a methylene blue aqueous solution to stain it. After staining the block, the block was sliced near the tip of the water needle to form a slice for observation. The slice for observation was then observed under an optical microscope to observe the water tree that had developed near the tip of the water needle in the slice for observation.
[0191] At this time, the maximum length of the water tree that occurred in the sliced specimen for observation was measured. The "maximum length of the water tree" was calculated by rounding off the length of the longest water tree in 10 blocks randomly extracted from the insulation layer of each sample.
[0192] As a result, the cases where the maximum length of the water tree was 200 μm or less were evaluated as good (A), and the cases where the maximum length of the water tree was more than 200 μm were evaluated as poor (B).
[0193] (Insulation evaluation) (i) Insulation evaluation immediately after manufacture Immediately after the manufacture of the power cables, sheets were taken from the insulation layer of each sample, with a thickness of 0.4 mm.
[0194] At room temperature (25°C), an AC voltage of 10 kV with commercial frequency (60 Hz) was applied to the insulating layer sheet for 10 minutes, and then the voltage was increased by 1 kV and applied for 10 minutes repeatedly. The electric field strength was measured when the insulating layer sheet experienced dielectric breakdown. As a result, AC breakdown strength of 50 kV / mm or more was evaluated as good (A), and AC breakdown strength of less than 50 kV / mm was evaluated as poor.
[0195] (ii) Insulation evaluation after bending test (7D bending test) First, a bending test was performed on each sample power cable.
[0196] In the first step of the bending test, a power cable with an outer diameter of 26 mm was pressed along half the circumference of a SUS ring with a radius of 180 mm. In other words, the power cable was bent so that the bending ratio of the bending radius of the power cable to the outer diameter of the insulation layer (outer diameter of the power cable) was 7 or less. In the second step that followed, the power cable was bent in the opposite direction to the bending direction in the first step, at the same bending ratio as in the first step.
[0197] (Sample collection and AC breakdown test) For each sample of power cable after the bending test, an insulating layer sheet was taken in the same manner as in the above-mentioned evaluation immediately after manufacture. For the insulating layer sheet taken after the bending test, an AC breakdown test was performed in the same manner as in the above-mentioned evaluation immediately after manufacture.
[0198] (3) Results The results of the evaluation of each sample will be described with reference to Table 1 below and FIGS.
[0199] [Table 1]
[0200] As a result of the above-mentioned NMR analysis, it was confirmed that each sample satisfied the content of each monomer unit shown in Table 1. Other evaluation results of each sample will be described below.
[0201] (Samples B1, B5 and B6) In samples B1 and B5, the insulating layer contained 20 mass % or more of butene units. In sample B6, the insulating layer did not contain styrene units and contained 20 mass % or more of butene units.
[0202] For this reason, as shown in the elastic modulus distribution in FIG. 3, in samples B1, B5 and B6, the phase structure of the insulating layer was a bicontinuous structure B1.
[0203] As a result, in the samples B1, B5 and B6, the AC breakdown electric field strength after the bending test was 50 kV / mm or more. However, in the samples B1, B5 and B6, the maximum length of the water tree in the water needle test exceeded 200 μm.
[0204] In samples B1, B5 and B6, the phase structure of the insulating layer was the co-continuous structure B1, so when water trees were generated in the water needle test, it is believed that the water trees propagated along the flexible phase of the co-continuous structure.
[0205] (Sample B2) In sample B2, the insulating layer contained only SEBS1 having a high content of butene units as the low crystalline resin, and the content of butene units in the insulating layer 130 was less than 20 mass %.
[0206] Therefore, as shown in the elastic modulus distribution in FIG. 4, in sample B2, the phase structure of the insulating layer was a sea-island structure B2 having minute first island phases but no coarse second island phases.
[0207] As a result, in sample B2, the AC breakdown electric field strength after the bending test was 50 kV / mm or more. However, in sample B2, the maximum length of the water tree in the water needle test exceeded 200 μm.
[0208] In sample B2, the phase structure of the insulating layer was a sea-island structure B2 with only minute first island phases, and coarse crystals grew in the sea phase. Therefore, when water treeing occurred in the water needle test, it is considered that the water treeing propagated at the interface of the coarse crystals.
[0209] (Samples B3 and B4) In samples B3 and B4, the insulating layer contained only SEBS2 having a low content of butene units as the low crystalline resin, and the content of butene units in the insulating layer was less than 9 mass %.
[0210] Therefore, as shown in the elastic modulus distribution in FIG. 5, in samples B3 and B4, the phase structure of the insulating layer was a sea-island structure B3 having coarse second island phases but no minute first island phases.
[0211] As a result, in samples B3 and B4, the maximum length of the water tree in the water needle test was 200 μm or less. However, in samples B3 and B4, the AC breakdown field strength after the bending test was less than 50 kV / mm.
[0212] In the samples B3 and B4, cracks and the like occurred in the sea phase during the bending test, which is considered to have caused the insulation properties to decrease after the bending test.
[0213] (Sample B7) In sample B7, the insulating layer contained only VLDPE containing no styrene units as the low crystallinity resin.
[0214] Therefore, sample B7 had the sea-island structure B3 including only coarse island phases, similar to samples B3 and B4.
[0215] As a result, in sample B7, cracks and the like occurred in the sea phase, similarly to samples B3 and B4, and therefore the AC breakdown field strength after the bending test was less than 50 kV / mm.
[0216] (Sample B8) In sample B8, the composition of the monomer units in the insulating layer was the same as in sample A1, but the novel mixing method described above was not applied.
[0217] Therefore, in sample B8, the phase structure of the insulating layer was the sea-island structure B3 including only coarse island phases, similar to samples B3 and B4.
[0218] As a result, in sample B8, the maximum length of the water tree in the water needle test was 200 μm or less, but in sample B8, the AC breakdown field strength after the bending test was less than 50 kV / mm.
[0219] In sample B8, the new mixing method was not applied, so the shear force during mixing was insufficient and the resin composition was not mixed sufficiently. Therefore, in sample B8, the sea-island structure A like that in sample A1 was not formed. As a result, cracks occurred in the sea phase during the bending test, which is thought to have reduced the insulation properties after the bending test.
[0220] (Samples A1~A3) In the samples A1 to A3, the insulating layer contained SEBS1 and SEBS2 as the low crystalline resin. In the samples A1 to A3, the content of butene units in the insulating layer was 9 mass% or more and less than 20 mass%. Furthermore, a new mixing method was applied to the samples A1 to A3.
[0221] Therefore, as shown in FIG. 2, in Samples A1 to A3, the phase structure of the insulating layer was a sea-island structure A including minute first island phases and coarse second island phases.
[0222] As a result, in the samples A1 to A3, the AC breakdown electric field strength after the bending test was 50 kV / mm or more.Furthermore, in the samples A1 to A3, the maximum length of the water tree in the water needle test was 200 μm or less.
[0223] In samples A1 to A3, the phase structure of the insulating layer was a sea-island structure A having minute first island phases and coarse second island phases, and it was confirmed that the insulating properties of the insulating layer could be ensured even when the power cable was bent.
[0224] Furthermore, it was confirmed that by making the phase structure of the insulating layer into a sea-island structure A having a minute first island phase and a coarse second island phase, excessive propagation of water treeing from the tip of a water needle simulating a minute foreign object or minute void in the insulating layer could be suppressed.
[0225] <Additional Notes> The following additional aspects of the present disclosure.
[0226] (Appendix 1) A resin composition constituting an insulating layer of a power cable, Contains propylene units and styrene units, The resin composition comprises In the elastic modulus distribution obtained by measuring the elasticity of a small area using a scanning probe microscope at 25°C, a marine phase having an elastic modulus of more than 100 MPa; A first island phase having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less; A second island phase having an elastic modulus of 100 MPa or less and a size of more than 100 nm and not more than 2000 nm; Equipped Resin composition.
[0227] (Appendix 2) A conductor; an insulating layer provided so as to cover an outer periphery of the conductor; Equipped with The insulating layer includes a propylene unit and a styrene unit, The insulating layer is In the elastic modulus distribution obtained by measuring the elasticity of a small area using a scanning probe microscope at 25°C, a marine phase having an elastic modulus of more than 100 MPa; A first island phase having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less; A second island phase having an elastic modulus of 100 MPa or less and a size of more than 100 nm and not more than 2000 nm; Equipped Power cable.
[0228] (Appendix 3) The maximum length of the water tree in the insulation layer generated by the water needle test is 200 μm or less. Here, the water needle test is providing a plate electrode on a first surface of the block taken from the insulating layer; forming a needle-shaped gap having a tip with a radius of curvature of 10 μm at a position facing the first surface with a gap of 1 mm; A step of forming a water needle in the block by injecting artificial seawater having a salinity of 3.8% by mass into the gap; applying an AC voltage of 1000 Hz and 4 kV between the plate electrode and the tip of the water needle for 200 hours; Includes 2. A power cable as defined in claim 2.
[0229] (Appendix 4) The AC breakdown field strength of the insulating layer at 25°C after a predetermined bending test is 50 kV / mm or more. Here, the bending test is a first step of bending the power cable so that a bending ratio of a bending radius of the power cable to an outer diameter of the insulating layer is 7 or less; a second step of bending the power cable in a direction opposite to the bending direction of the first step at a bending ratio equal to the bending ratio of the first step; Includes 1. A power cable as claimed in claim 2 or 3.
[0230] (Appendix 5) The insulating layer further comprises a butene unit, The content of the butene units in the insulating layer is 9% by mass or more and less than 20% by mass. 5. The power cable according to claim 2,
[0231] (Appendix 6) The first island phase and the second island phase contain at least the styrene unit. 10. The power cable according to claim 2,
[0232] (Appendix 7) The insulating layer is A propylene-based resin, a first styrenic elastomer comprising propylene units or butene units and styrene units; a second styrenic elastomer containing propylene units or butene units and styrene units and different from the first styrenic elastomer; have 7. The power cable according to any one of appendix 2 to appendix 6.
[0233] (Appendix 8) The content of the propylene unit or the butene unit in the second styrene-based elastomer is less than the content of the propylene unit or the butene unit in the first styrene-based elastomer. 8. The power cable according to claim 7.
[0234] (Appendix 9) The content of the styrene units in the second styrene-based elastomer is greater than the content of the styrene units in the first styrene-based elastomer. 1. A power cable as claimed in claim 7 or 8.
[0235] (Appendix 10) A step of preparing a resin composition including a propylene unit and a styrene unit; forming an insulating layer from the resin composition so as to cover an outer periphery of a conductor; Equipped with In the step of preparing the resin composition, The resin composition is mixed so that, in an elastic modulus distribution obtained by measuring elasticity in a micro-area using a scanning probe microscope at 25°C, the composition has a sea phase having an elastic modulus of more than 100 MPa, a first island phase having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less, and a second island phase having an elastic modulus of 100 MPa or less and a size of more than 100 nm and 2000 nm or less. A method for manufacturing power cables. [Explanation of symbols]
[0236] 10 Power Cable 110 Conductor 120 Inner semiconducting layer 130 Insulating layer 140 Outer semiconducting layer 150 Shielding layer 160 Sheath
Claims
[Claim 1] A step of preparing a resin composition including a propylene unit and a styrene unit; forming an insulating layer from the resin composition so as to cover an outer periphery of a conductor; Equipped with In the step of preparing the resin composition, The resin composition is mixed so that, in an elastic modulus distribution obtained by measuring elasticity in a micro-area using a scanning probe microscope at 25°C, the composition has a sea phase having an elastic modulus of more than 100 MPa, a first island phase having an elastic modulus of 100 MPa or less and a size of 0.1 nm or more and 100 nm or less, and a second island phase having an elastic modulus of 100 MPa or less and a size of more than 100 nm and 2000 nm or less. A method for manufacturing power cables.