Centrifugal atomizer and method of producing impalpable powder
The centrifugal spray device addresses disk damage and yield issues by using a protective member and magnetic flux transmission to preheat the disk inductively, ensuring stable fine powder production.
Patent Information
- Application Number
- JP2024060861
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-07
- Filing Date
- 2024-04-04
- Publication Date
- 2024-10-18
AI Technical Summary
The formation of metal coagulum on the disk in centrifugal spray devices leads to poor yield and disk damage due to temperature differences and excessive centrifugal force, causing splashing and unbalanced rotation.
A centrifugal spray device using a cold crucible melting furnace with a protective member and magnetic flux transmission to preheat the disk inductively, preventing temperature drops and rebounding of molten metal, ensuring consistent temperature and stable production.
Stabilizes the production of fine powder by preventing disk damage and improving yield through controlled temperature management and reduced splashing, ensuring efficient atomization.
Smart Images

Figure 2024149438000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a centrifugal atomizer and method for producing fine powder that addresses the problem of metal precipitates forming on the disk. [Background technology]
[0002] Known methods for producing fine metal powders include water atomization (water atomization), gas atomization (gas atomization), and centrifugal atomization (disk atomization). Among these, centrifugal atomization produces fine powder by pouring molten metal from a crucible onto a disk placed in the direction of the flow of the molten metal, and has the advantage that the particle size can be easily controlled to, for example, 100 μm or less, and that it is easy to produce perfect spheres.
[0003] 7(a) is a principle diagram showing a centrifugal atomizer for carrying out centrifugal atomization (disk atomization) of fine metal powder. This device is composed of a refractory crucible 101 and a rotating disk mechanism 102 (for example, Patent Document 1).
[0004] In the refractory crucible 101, a tapping section 101a is provided at the bottom, and molten metal 103 heated by a heating means (not shown) is tapped from the bottom of the tapping section 101a. The molten metal 103 is then dripped onto a disk 102a rotating at high speed. The molten metal 103 is then sprayed horizontally from the outer periphery of the disk 102a, and is cooled and solidified by the surrounding gas, thereby producing spherical metal powder 103a.
[0005] In this case, since the refractory crucible 101 needs to deliver the molten metal 103 to the disk 102a at or above its melting point, it is considered preferable to use a heating means to heat the molten metal 103 to a temperature sufficiently higher than the melting point before pouring it out. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2021-4393 Summary of the Invention [Problem to be solved by the invention]
[0007] Incidentally, one possible embodiment of the centrifugal atomizer is to employ a cold crucible (CC) melting furnace 104 shown in FIG. 7(b) instead of the refractory crucible 101.
[0008] The cold crucible melting furnace 104 has the advantage that it can melt active metals and metals with high melting points without reducing the purity, compared to the conventional bottom tapping of the refractory crucible 101.
[0009] In this cold crucible melting furnace 104, the furnace side walls 104a and the bottom floor 104b are made of water-cooled copper segments. By cooling, a skull (solidified portion) 104c is formed on the furnace side walls 104a and the hearth floor 104b. Part of the skull 104c is melted by the tapping coil 104d, and the molten metal 106 is tapped from the bottom through the tapping portion 104e.
[0010] The hot water outlet coil 104d shown in FIG. 7(b) is configured as a flat coil (one turn, four layers).
[0011] However, when the cold crucible melting furnace 104 and the rotating disk mechanism 105 are combined to form a centrifugal atomization device, the skull 104c cannot be completely melted, and therefore, in principle, it is difficult to heat the supplied molten metal 106 to a temperature sufficiently higher than the melting point. Therefore, if the temperature of the disk 105a is lower than that of the molten metal, the supplied molten metal 106 is cooled on the disk 105a and does not spread in a thin film on the upper surface of the disk 105a, which may cause the following problem.
[0012] (1) The molten metal 106 splashes on the upper surface of the disk 105a and is not sprayed, resulting in a decrease in yield. (2) The solidified material 106a of the molten metal 106 continues to grow on the upper surface of the disk 105a, unevenly relative to the central axis of rotation, and the disk 105a is damaged by the excessive centrifugal force. On the other hand, if the strength of the disk 105a is made stronger, it will rotate in an unbalanced state, generating excessive vibration and load, which will lead to motor failure.
[0013] One possible solution to this problem is to heat the disk 105a. In order to deal with this problem without increasing the number of parts or costs, it is possible to bring the disk 105a close to the discharge coil 104d and use the discharge coil 104d to heat the surface of the disk 105a. However, this raises the risk of damage or breakage of the discharge coil 104d due to the rebound of the molten metal 106 from the disk 105a.
[0014] An object of the present invention is to provide a centrifugal atomizer and a method for producing fine powder that can effectively solve these problems. [Means for solving the problem]
[0015] In order to achieve the above object, the present invention takes the following measures.
[0016] In other words, the centrifugal atomization device of the present invention melts skull using a discharge coil arranged around the discharge part of a cold crucible melting furnace, discharges molten metal from the discharge part, and supplies the molten metal onto a disk arranged in the direction of the downward flow of the molten metal to produce fine powder by centrifugal atomization.The centrifugal atomization device is characterized in that a protective member is arranged between the discharge coil and the disk to prevent the molten metal from bouncing back from the disk to the discharge coil, and at least a part of the protective member is provided with a magnetic flux permeable portion for applying the magnetic flux of the discharge coil to the disk.
[0017] In this way, even if the tapping coil and the disk are brought close to each other, the protective member can prevent the molten metal from bouncing off the disk. The magnetic flux of the tapping coil can be applied to the disk through the magnetic flux permeable portion of the protective member. Therefore, even without using a separate heat source, the tapping coil effectively heats the disk by induction heating during preheating, bringing the disk temperature close to the molten metal temperature, and the molten metal is induction heated during disk atomization, preventing the molten metal temperature from dropping below its melting point. This can eliminate problems such as a decrease in yield rate in the production of fine powder and damage or breakage of the disk due to the growth of solidified matter.
[0018] It is preferable that the protective member is a metal shielding plate, and the magnetic flux transmission portion is a ceramic plate fitted to the inner periphery of the shielding plate. In this way, the shielding plate can be made strong, can be water-cooled as necessary, and can have a structure that makes it easy to attach the shielding plate (the mechanism itself).
[0019] In this case, it is preferable that the outer diameter of the ceramic plate is larger than the diameter of the disk, and the ceramic plate is provided with a molten metal passage portion having an inner diameter substantially equal to or smaller than the inner diameter of the tapping coil, thereby making it possible to appropriately prevent the molten metal from bouncing back and to appropriately transmit the magnetic flux.
[0020] The tapping coil is preferably provided with a plurality of turns along the tapping direction of the molten metal from the tapping section, thereby making it possible to suppress a temperature drop of the molten metal toward the disk after tapping.
[0021] In addition, the method for producing fine powder according to the present invention is characterized in that, in melting metal in a crucible of a cold crucible melting furnace with a melting coil, melting skull with a discharge coil arranged around the discharge part to discharge molten metal from the discharge part, and supplying the molten metal onto a disk arranged in the direction of flow of the molten metal to produce fine powder by centrifugal atomization, the method comprises carrying out a preheating process in which the inside of the crucible is heated by the melting coil to keep the molten metal from solidifying, while preheating the disk with the discharge coil to an extent that the molten metal does not discharge from the discharge part, and a discharge process in which the disk is heated while the molten metal is discharged from the discharge part after the preheating process.
[0022] In this way, the disk can be preheated in advance, so that the temperature difference between the molten metal and the disk can be made small when the molten metal is supplied to the disk from the tapping portion. Effect of the Invention
[0023] According to the present invention as described above, it is possible to provide a centrifugal atomizer and a method for producing fine powder which effectively addresses the problem of metal solidification on the disk, improves the yield in the production of fine powder, and prevents damage and breakage of the disk. [Brief description of the drawings]
[0024] [Figure 1] 1 is a schematic diagram of a centrifugal spray device according to an embodiment of the present invention; [Diagram 2] FIG. 2 is an enlarged view corresponding to a main part of FIG. [Diagram 3] FIG. [Figure 4] FIG. [Diagram 5] FIG. 5 is a configuration explanatory diagram corresponding to FIG. 4 . [Figure 6] FIG. 13 is a diagram showing another modified example of the present invention. [Figure 7] 1A and 1B are diagrams showing a conventional example and an improved example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0026] The centrifugal atomization device A shown in FIG.
[0027] The cold crucible melting furnace 1 comprises a furnace side wall 11 and a hearth 12. The furnace side wall 11 is made of copper and is water-cooled by a mechanism not shown, and a crucible 1a is made up of a collection of rectangular segments 11a, and a melting coil 13 for induction heating is wound spirally around the outer periphery of the crucible 1a, to which high-frequency power is supplied from a first power supply unit 14. The magnetic field induced by the current of the melting coil 13 induces eddy currents in the metal 3 in the crucible 1a through the gap between the segments 11a, 11a, and the metal 3 self-heats and melts.
[0028] The hearth 12 is a flat plate larger than the outer periphery of the furnace side wall 11 which constitutes the bottom of the cold crucible melting furnace 1. Like the furnace side wall 11, the hearth 12 is made of water-cooled copper and is an assembly of segments 12a which are divided approximately in the circumferential direction.
[0029] The hearth 12 is provided with a tapping part (so-called bottom tapping part) 15 capable of discharging the metal 3 from the center to the outside of the crucible 1a.
[0030] When the metal 3 is heated by the melting coil 13, the metal 3 melts and becomes molten metal 3a, which solidifies from the outside facing the water-cooled furnace side wall 11 and from the contact surface with the hearth 12. The solidified metal lump is called skull 3b. The tapping part 15 is covered with skull 3b. In order to tap the molten metal 3a from the tapping part 15 of the hearth 2, it is necessary to melt the skull 3b near the tapping part 15.
[0031] Therefore, a molten metal discharge coil 16 wound around the molten metal discharge section 15 is placed on the underside of the hearth 12, and high-frequency power is supplied from a second power supply unit 17 to melt a portion of the skull 3b formed on the hearth 12, including the skull 3b at the molten metal discharge section 15, by induction heating.
[0032] As a result, a part of the skull 3b melts, and the outlet 15 that was blocked by the skull 3b opens, allowing the molten metal 3a to be tapped from the opening. The tapping direction is the vertical direction (Z direction).
[0033] The first and second power supply devices 14 and 17 are controlled by a coil control unit 18 in terms of on / off, power supply, etc.
[0034] On the other hand, the rotating disk mechanism 2 includes a disk-shaped disk 21, a motor 22 that drives the disk 21 around the central axis 2a, and a motor control unit 23 that controls the motor 22. The disk 21 is disposed so that its upper surface is perpendicular to the central axis 2a and the center of the upper surface corresponds to the center of the tapping nozzle 15. In this embodiment, the disk 21 is made of carbon and disposed in a horizontal position so as to receive at its center the molten metal 3a that is tapped vertically from above. The motor 22 is, for example, a servo motor, and the on / off and rotation speed of the disk 21 are controlled via the motor control unit 23.
[0035] Before the molten metal is discharged from the cold crucible melting furnace 1, the disk 21 is rotated at high speed by the motor 22, and then the molten metal 3a discharged from the discharge nozzle 15 is supplied to the upper surface of the disk 21. The molten metal 3a then moves along the upper surface of the disk 21 toward the periphery of the disk 21 due to the centrifugal force of the disk 21, and is sprayed from the periphery outward in the radial direction. The sprayed molten metal 3a is cooled by the gas surrounding the disk 21 and solidifies to form fine powder 3c. The gas is, for example, an inert gas.
[0036] In such a configuration, as described above, in the cold crucible melting furnace 1, the skulls 3b between the segments 11a, 11a and between the segments 12a, 12a cannot be completely melted when the melt is discharged, so in principle it is difficult to heat the supplied molten metal to a temperature sufficiently higher than the melting point. On the other hand, the disk 21 is not particularly heated. For this reason, if the temperature of the disk 21 is low when the molten metal 3a is supplied onto the disk 21, the temperature of the molten metal 3a drops below the melting point and the molten metal 3a does not spread in a thin film on the upper surface of the disk 21. This not only reduces the yield in the production of fine powder, but also causes the molten metal 3a to solidify on the disk 21, which leads to damage and failure of the disk and the motor.
[0037] In this embodiment, as shown in Figure 2, in order to heat the disk 21 using the magnetic flux Φ of the tapping coil 16, a protective member 4 is placed between the tapping coil 16 and the disk 21, and a magnetic flux permeable portion 41 is provided in part of the protective member 4 to inductively heat the disk 21, while the tapping coil 16 is wound in a way that prevents a drop in the temperature of the molten metal 3a during tapping.
[0038] The tapping nozzle 15 is funnel-shaped and comprises an inverted cone-shaped expanded diameter section 15a and a cylindrical straight section 15b, and is detachably attached to a through hole 12b provided in the hearth 12. Specifically, a part of the through hole 12b has a tapered structure that opens upward, and the expanded diameter section 15a of the tapping nozzle 15 is attached to this tapered section, with the lower end of the cylindrical section 15b protruding downward from the hearth 12. A dissimilar material nozzle suitable for the molten metal 3a is used for the tapping nozzle 15.
[0039] The protective member 4 is composed of a copper shielding plate 40 having excellent heat dissipation and durability, and a part of the shielding plate 40 is composed of a magnetic flux transmission part 41 that is not affected by magnetic flux, specifically, a ceramic plate 41a using a magnetically permeable material (e.g., boron nitride, etc.). This is because if only the copper shielding plate 40 is used, the magnetic flux Φ of the discharge coil 16 is blocked by the shielding plate 40 and does not reach the disk 21. Here, the shielding plate 40 is formed in an annular shape, its inner circumference is made into a stepped hole 40a, and the ceramic plate 41a is fitted into the stepped hole 40a. The ceramic plate 41a is positioned at a predetermined distance (e.g., about 1 mm) from the lower end 16b of the discharge coil 16, and is placed with a predetermined distance (e.g., 10 mm) between it and the disk 21 that does not hinder atomization. The ceramic plate 41a is provided with a molten metal passage hole 41a1 in the center to pass the molten metal 3a.
[0040] The discharge coil 16 is a copper tube 16a with four turns, and is not flat wound, but is composed of an inner circumferential portion with two turns in the axial direction and one layer in the radial direction, and an outer circumferential portion with two turns in the axial direction and one layer in the radial direction. Specifically, the inner circumferential portion is wound with two turns in the axial direction, and the second layer is wound with two turns in the axial direction in a stepped manner in the radial direction, resulting in a two-turn, two-layer structure. The outer diameter r1 of the discharge coil 16 is slightly larger than or approximately equal to the diameter r2 of the disk 21. The upper end 16c of the discharge coil 16 is disposed in close proximity to or in contact with the lower surface 12a of the hearth 12, which is a water-cooled copper segment structure.
[0041] The tapping coil 16 has two turns and two layers, and is disposed under the hearth 12, so that the ceramic plate 41a is located between the hearth 12 and the disk 21 (here, approximately in the middle position).
[0042] In addition, the diameter r3 of the ceramic plate 41a is approximately twice the diameter r2 of the disk 21, ensuring the magnetic path space necessary for the magnetic flux Φ generated by the discharge coil 16 to circulate without being blocked by the copper shielding plate 40.
[0043] The hole diameter r4 of the molten metal passing hole 41a1 of the ceramic plate 41a is set to be approximately the same as the inner diameter r5 of the tapping coil 16. Of course, the hole diameter r4 of the molten metal passing hole 41a1 may be set to be smaller than the inner diameter r5 of the tapping coil 16.
[0044] Next, the process for producing the fine powder will be described.
[0045] Cooling of the crucible 1a is started, and when the crucible 1a has cooled, the metal 3 is put into the crucible 1a, and the process of inductively heating the metal 3 is started by energizing the melting coil 13 through the coil control unit 18. When the metal 3 melts to become the molten metal 3a as shown in FIG. 1 and a skull 3b is formed in the part in contact with the furnace side wall 11 and the hearth 12, the coil control unit 18 starts the preheating process of energizing the melting coil 13 while maintaining the melting coil 13 in a state in which the molten metal 3a does not solidify. At this time, the coil control unit 18 maintains the power below the level at which the molten metal 3a does not discharge from the discharge nozzle 15. As a result, the magnetic flux Φ of the discharge coil 16 reaches the disk 21 through the ceramic plate 41a, which is the magnetic flux permeable unit 41. The magnetic flux Φ passes through the surface of the disk 21 and heats only the disk surface (skin effect), and heat is transferred to the inside of the disk 21 by thermal conduction, so that the entire disk 21 including the surface is preheated.
[0046] The preheating temperature at this time is set so that the surface of the disk 21 has a temperature close to the melting point of the metal 3. The disk control unit 23 rotates the disk 21 at a predetermined rotation speed before or after the start of preheating.
[0047] After the preheating process is completed, the atomization process begins, and the disk control unit 23 rotates the disk at a predetermined speed, which is faster than the preheating process. The coil control unit 18 increases the power of the discharge coil 16, melting the skull 3b and discharging the molten metal 3a from the discharge nozzle 15. The molten metal 3a passes through the inner circumference of the discharge coil 16 and is supplied to the disk 21 through the molten metal passage hole 41a1 of the ceramic plate 41a.
[0048] At this stage, the surface of the disk 21 is preheated to a temperature close to the melting point of the metal 3, and the molten metal 3a that reaches the disk 21 while being prevented from dropping in temperature by passing through the axially arranged molten metal coil 16 after being tapped is no longer immediately cooled by the disk 21. As a result, the molten metal 3a spreads in a thin film on the upper surface of the disk 21 and is centrifugally atomized, becoming fine powder 3c without generating solidification on the upper surface of the disk 21. Furthermore, the molten metal 3a does not splash on the upper surface of the disk 21 and the disk 21 does not break, making it possible to produce stable fine powder 3c.
[0049] As described above, the centrifugal atomization device A of this embodiment melts the skull 3b using the discharge coil 16 arranged around the discharge nozzle 15, which is the discharge part of the cold crucible melting furnace 1, and discharges molten metal 3a from the discharge nozzle 15. The molten metal 3a is then supplied onto a disk 21 arranged in the downstream direction of the molten metal 3a, and fine powder 3c is produced by centrifugal atomization. A protective member 4 is arranged between the discharge coil 16 and the disk 21 to prevent the molten metal 3a from bouncing back from the disk 21 to the discharge coil 16, and a magnetic flux permeable portion 41 is provided in at least a part of the protective member 4 to apply the magnetic flux Φ of the discharge coil 16 to the disk 21.
[0050] In this way, even if the discharge coil 16 and the disk 21 are brought close to each other, the protective member 4 can prevent the molten metal 3a from bouncing off the disk 21. The magnetic flux Φ of the discharge coil 16 can be applied to the disk 21 through the magnetic flux permeable portion 41 of the protective member 4. Therefore, even without using a separate heat source, the discharge coil 16 effectively inductively heats the disk 21 during preheating, bringing the disk temperature close to the molten metal temperature, and the molten metal is inductively heated during disk atomization, preventing the molten metal temperature from dropping below its melting point, thereby eliminating problems such as a decrease in yield in the production of the fine powder 3c and damage or breakage of the disk 21 due to the growth of solidified matter.
[0051] Specifically, the protective member 4 is a metallic shielding plate 40, and the magnetic flux permeable portion 41 is a ceramic plate 41a fitted into the inner circumference of the shielding plate 40. This gives strength to the shielding plate 40, allows the shielding plate 40 to be water-cooled if necessary, and enables the shielding plate 40 (the mechanism itself) to be easily attached.
[0052] In this case, the outer diameter r3 of the ceramic plate 41a is larger than the diameter of the disk r2, and the ceramic plate 41a is provided with a molten metal passage portion 41a1 with an inner diameter r4 that is approximately equal to the inner diameter r5 of the discharge coil 16, thereby making it possible to appropriately prevent the molten metal 3a from bouncing back and allow the magnetic flux Φ to pass through.
[0053] In addition, since the dispensing coil 16 is provided with multiple turns (2 turns) along the dispensing direction (Z direction) of the molten metal 3a from the dispensing nozzle 15, a drop in temperature of the molten metal 3a heading toward the disk 21 after being dispensed can be suppressed.
[0054] In addition, the manufacturing method of fine powder 3c according to this embodiment involves melting the metal 3 in the crucible 1a of the cold crucible melting furnace 1 with the melting coil 13, melting the skull 3b with the discharge coil 16 arranged around the discharge nozzle 15 to discharge molten metal 3a from the discharge nozzle 15, and supplying the molten metal 3a onto a disk 21 arranged in the downward direction of the flow to produce fine powder 3c by centrifugal atomization, and includes carrying out a preheating process in which the inside of the crucible 1 is heated by the melting coil 13 to keep the molten metal 3a from solidifying, while preheating the disk 21 with the discharge coil 16 to an extent that the molten metal 3a is not discharged from the discharge nozzle 15, and a discharge process in which the disk 21 is heated while the molten metal 3a is discharged from the discharge nozzle 15 after the preheating process.
[0055] In this way, the disk 21 can be preheated in advance, so that the temperature difference between the molten metal 3a and the disk 21 can be kept small when the molten metal 3a is supplied from the discharge nozzle 15 to the disk 21.
[0056] Although one embodiment of the present invention has been described above, the specific configuration of each part is not limited to the above-described embodiment.
[0057] For example, as shown in FIG. 3, the discharge coil 16 may be configured with an inner peripheral portion of 3 turns and 1 layer and an outer peripheral portion of 1 turn and 1 layer, and the upper end portion of the two layers forming a flat coil shape may be located on the bottom surface 12a side of the hearth 12 having a segment structure. In this case, while the hearth 12 is heated by the flat coil-shaped portion, the time for the molten metal 3a to pass between the discharge coil 16 from the time of tapping to the time of reaching the disk 21 is longer than that of a flat coil, so that the molten metal 3a is less likely to cool. The number of turns of the discharge coil 16 may be arbitrarily changed to match the power supply. Shielding plates and magnetic flux transmission parts are omitted in FIG. 3.
[0058] Also, as shown in FIG. 4, the tapping section 115 may be integral with the water-cooled copper segments 12a constituting the hearth 12. As described above, the hearth 12 is made of water-cooled copper, like the furnace side wall 11, and is an assembly of segments 12a divided in the circumferential direction. The shape of the tapping section 115 is substantially the same as that of the tapping nozzle 15, and as shown in FIG. 4 and FIG. 5, the tapping section 115 has a funnel shape in which a small-diameter inner diameter portion located inside an inverted cone-shaped expanded diameter portion 115a is connected to a vertical straight portion 115b. In this embodiment, the tip portion 115c protrudes downward, but the tip portion 115c may not protrude downward. The hearth 12 has a general cooling structure in which cooling water is supplied to a cooling passage provided inside a fan-shaped copper bottom segment 12a. Since the molten metal outlet 115 is an integrated segment type, it is also cooled, and therefore even if the power of the molten metal outlet coil 16 required for discharging the molten metal is increased (for example, about twice), the molten metal outlet 115 does not melt and the nozzle shape is maintained. In other words, the coil power during preheating of the disk 21 can also be increased. This makes the solidified material on the top surface of the disk even thinner and reduces imbalance due to eccentricity of the solidified material, allowing the peripheral speed of the disk to be increased, preventing the disk from breaking and obtaining atomized powder with an even smaller particle size.
[0059] Furthermore, the materials are not particularly limited as long as the basic effects of the present invention can be obtained; for example, the shielding plate can be made of glass and the disk can be made of a material other than carbon.
[0060] In addition, the protective member in the above embodiment is a copper plate, and ceramic is provided on a part of it as a magnetic flux permeable portion. However, if there is no practical problem, such as no need for water cooling or the like and the mounting strength can be ensured, the protective member that prevents the molten metal from splashing back may be made of only a magnetically permeable material such as a ceramic plate, which simultaneously functions as a magnetic flux permeable portion.
[0061] Furthermore, the shape of the protective member is not necessarily limited to a plate shape. For example, the protective member 4X shown in Fig. 6 is made of a ceramic cylindrical tube 40X that also serves as a magnetic flux transmission section, and is configured to cover the periphery of the tapping space for the molten metal, thereby isolating the tapping coil 16 from the tapping space. Even in this case, it is possible to prevent the molten metal scattered from the disk 21 from adhering to the tapping coil 16.
[0062] Other configurations can also be modified in various ways without departing from the spirit of the present invention. [Explanation of symbols]
[0063] A…Centrifugal spray device 1…Cold crucible melting furnace 3a…Molten metal 3b…Skull 3c…Fine powder 4. Protective material 15…Water outlet section (water outlet nozzle) 16…Water outlet coil 21...Disc 40...Shielding plate 41...Magnetic flux permeable section 41a…Ceramic plate r2: disc diameter r3: Outer diameter of ceramic plate r4: Inner diameter of magnetic flux permeable part r5…Inner diameter of the tapping coil Z…Direction of tapping Φ...Magnetic flux
Claims
1. A centrifugal atomizer for producing fine powder by centrifugal atomization, comprising: a cold crucible melting furnace having a discharge coil disposed around a discharge part of the furnace, melting skull, discharging molten metal from the discharge part, and supplying the molten metal onto a disk disposed in a direction of the downward flow of the molten metal; A centrifugal spray device characterized in that a protective member is placed between the discharge coil and the disk to prevent the molten metal from splashing back from the disk to the discharge coil, and a magnetic flux permeable portion is provided in at least a part of the protective member to apply the magnetic flux of the discharge coil to the disk.
2. 2. The centrifugal atomizer according to claim 1, wherein the protective member is a metallic shielding plate, and the magnetic flux permeable portion is a ceramic plate fitted around the inner periphery of the shielding plate.
3. 3. The centrifugal spray device according to claim 2, wherein an outer diameter of the ceramic plate is larger than a diameter of the disk, and the ceramic plate is provided with a molten metal passage portion having an inner diameter substantially equal to or smaller than an inner diameter of the tapping coil.
4. 2. The centrifugal atomizer according to claim 1, wherein the discharge coil is provided with a plurality of turns along a direction in which the molten metal is discharged from the discharge portion.
5. A method for producing fine powder, comprising the steps of melting a metal in a crucible of a cold crucible melting furnace with a melting coil, dissolving a skull with a discharge coil disposed around the discharge part, discharging the molten metal from the discharge part, and supplying the molten metal onto a disk disposed in a direction of flow of the molten metal, thereby producing fine powder by centrifugal atomization, The inside of the crucible is heated by the melting coil to keep the molten metal from solidifying, A method for producing fine powder, characterized by carrying out a preheating process in which the disk is preheated by the tapping coil to a degree that does not cause molten metal to be tapped from the tapping section, and a tapping process in which the disk is heated while causing molten metal to be tapped from the tapping section after the preheating process.
Citation Information
Patent Citations
Centrifugal spray device and method of producing fine powder
JP2021004393A