Quantum dot composition, method of preparing the same, cured product thereof, and display device including the same

A quantum dot composition with optimized photopolymerizable monomers and surface-modified ligands addresses viscosity and aggregation issues, enabling efficient electrohydrodynamic inkjet printing and improved display performance.

JP2024149460AActive Publication Date: 2024-10-18SAMSUNG ELECTRONICS CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024061476
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2024-04-05
Publication Date
2024-10-18
Estimated Expiration
2044-04-05

AI Technical Summary

Technical Problem

Existing quantum dot compositions for electrohydrodynamic inkjet printing face challenges with high viscosity, aggregation, and poor electrical conductivity, making them unsuitable for efficient patterning and display applications.

Method used

A quantum dot composition is formulated with specific ratios of photopolymerizable monomers and oligomers containing carbon-carbon double bonds and thiol groups, along with surface modification using primary and secondary ligands, to achieve suitable viscosity and prevent aggregation, enhancing electrical conductivity and ejection properties.

Benefits of technology

The composition exhibits excellent optical properties, prevents aggregation, and supports efficient inkjet printing, reducing material waste and manufacturing costs while maintaining high light conversion efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149460000001_ABST
    Figure 2024149460000001_ABST
Patent Text Reader

Abstract

To provide a quantum dot composition, a method of preparing the same, a cured product thereof, and a display device including the same.SOLUTION: The disclosure relates to a quantum dot composition, a method of preparing the same, a cured product thereof, and a display device including the same, and more particularly, to a quantum dot composition for electrohydrodynamic inkjet printing, a method of preparing the same, a cured product thereof, and a display device including the same.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a quantum dot composition, a manufacturing method thereof, a cured product thereof, and a display device including the same, and more particularly to a quantum dot composition for electrohydrodynamic inkjet printing, a manufacturing method thereof, a cured product thereof, and a display device including the same. [Background technology]

[0002] Quantum dots (QDs) are so-called semiconductor nanocrystals, and can produce various colors by generating light of different wavelengths according to particle size without changing the type of material. They have advantages of higher color purity and light stability than existing light-emitting bodies, so they are attracting attention as a next-generation light-emitting device.

[0003] In particular, quantum dots, which have become a new trend in the display field, are dispersed in a polymer matrix and can be applied to various displays and electronic devices in the form of a complex in addition to TVs and LEDs. Quantum dots, represented by CdSe and InP, have made rapid progress in terms of luminous efficiency (quantum yield), and a synthesis method with a luminous efficiency of nearly 100% has been introduced. Based on this, TVs using quantum dot sheets are currently being commercialized. In the next stage, quantum dots are included in the color filter layer of existing LED TVs (excluding pigments and dyes), and quantum dot TVs are being developed that are self-emitting versions rather than filtering type in the color filter layer. The key to developing such quantum dot TVs is to focus on how much the luminous efficiency of quantum dots can be maintained in the process of forming pixels with quantum dots and the manufacturing process.

[0004] Meanwhile, materials for color filters are required to have high sensitivity, adhesion to substrates, chemical resistance, heat resistance, etc. Conventionally, color filters applied to displays have generally been formed through a patterning process in which a desired pattern is formed using a photosensitive resist composition through an exposure process using a photomask, and then non-exposed areas are dissolved and removed through a development process, but this has led to a problem of increased costs due to waste materials.

[0005] Recently, in order to solve the problem of increasing the quality of materials used for pixels and the associated cost increases, methods that use materials only in desired areas and minimize the use of materials have been attracting attention, rather than the conventional patterning methods such as spin coating or slit coating. The most representative method is the inkjet method, which can be broadly classified into the bubble jet method and the piezo method. The inkjet method uses materials only in desired pixels, thereby preventing unnecessary waste of materials.

[0006] However, since the quantum dot composition used in the inkjet method is required to have a viscosity of 100 cps or less, preferably 50 cps or less, it is difficult to apply a high-viscosity ink having a viscosity exceeding 100 cps.

[0007] To overcome the drawbacks of the inkjet method, the electrohydrodynamic (EHD) inkjet method, which is capable of fine patterning, has been developed. The EHD inkjet method applies an electric potential difference between the ink ejection nozzle and the substrate, enabling fine ink printing through the electric field.

[0008] As a related prior art, Korean Patent Publication No. 10-2020-0137977 discloses a solution used in an electrohydrodynamic printing method.

[0009] The above-mentioned prior art is characterized by improving light efficiency by forming a lens shape using fine printing, so the solvent must be evaporated to form a quantum dot-polymer resin to improve viscosity. Also, if the ratio of quantum dots is high, good light conversion efficiency is obtained, but if the ratio of quantum dots is low, aggregation between quantum dots occurs, and there is a problem that the light conversion efficiency is poor.

[0010] To solve this problem, an appropriate ratio of polymer to quantum dots has been proposed, but the weight ratio is about 1:100 to 1:1000, which requires an excessively large amount of polymer, and this has resulted in problems such as the quantum dot-polymer mixing process and the quantum dot-polymer resin formation process taking a considerable amount of time. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Korean Patent Publication No. 10-2020-0137977 Summary of the Invention [Problem to be solved by the invention]

[0012] The problem to be solved by the present invention is to provide a quantum dot composition having a high viscosity suitable for the EHD inkjet method, good electrical conductivity, no aggregation between quantum dots, and excellent ejection properties and inkjetability, and a method for producing the same.

[0013] Another object of the present invention is to provide a quantum dot composition that exhibits excellent optical properties while preventing aggregation between quantum dots, and a method for producing the same.

[0014] Another object of the present invention is to provide a cured product of the quantum dot composition and a display device including the same. [Means for solving the problem]

[0015] According to one aspect of the present invention for solving the above-mentioned problems, a photopolymerizable composition comprising quantum dots, a photopolymerizable monomer and an oligomer, The oligomer provides a quantum dot composition, which is characterized in that it contains a compound containing a carbon-carbon double bond and a compound containing a thiol group.

[0016] Preferably, the oligomer comprises The present invention provides a quantum dot composition comprising two or more of the compounds containing a carbon-carbon double bond.

[0017] Preferably, the quantum dot composition is characterized in that the compound containing a carbon-carbon double bond includes one type each of a compound containing 2 to 3 carbon-carbon double bonds per molecule and a compound containing one carbon-carbon double bond per molecule.

[0018] Preferably, the quantum dot composition is provided, wherein the compound containing a carbon-carbon double bond includes one or more compounds containing a phenol group.

[0019] Preferably, the quantum dot composition is provided, wherein the compound containing a thiol group contains two to four functional groups.

[0020] Preferably, the compound containing a carbon-carbon double bond comprises triallyl isocyanurate and phenol acrylate; The quantum dot composition is characterized in that the compound containing a thiol group contains ethylene glycol di(3-mercaptopropionate).

[0021] Preferably, the quantum dot composition is characterized in that the molar ratio of the compound containing a carbon-carbon double bond to the compound containing a thiol group is 2.75:1 to 5:1.

[0022] Preferably, the quantum dot composition is characterized in that the molar ratio of the compound containing 2 to 3 carbon-carbon double bonds per molecule to the compound containing one carbon-carbon double bond per molecule is 0.01:1 to 1.5:1.

[0023] Preferably, the quantum dot composition is characterized in that the carbon-carbon double bond is one or more selected from the group including a vinyl group, an allyl group, a (meth)acrylic group, an isopropenyl group, and a 2-butenyl group.

[0024] Preferably, a quantum dot composition is provided that has a viscosity in the range of 200 to 1000 cps at room temperature.

[0025] Preferably, the quantum dot composition is characterized in that the quantum dots are surface-modified with a primary ligand represented by the following chemical formula 1 and a secondary ligand having 3 to 40 carbon atoms and including a carboxyl group.

[0026] [ka] (In the above Chemical Formula 1, M is a divalent to tetravalent metal; m is an integer of 1 to 4, and X is independently an organic group having 3 to 20 carbon atoms; n is an integer from 2 to 4.

[0027] Preferably, the quantum dot composition is provided for use in electrohydrodynamic inkjet printing.

[0028] According to another aspect of the present invention, the surface of the quantum dots is modified, then dispersed in a photopolymerizable monomer to obtain a quantum dot dispersion, which is then mixed with an oligomer; The oligomer is produced by mixing a compound containing a carbon-carbon double bond and a compound containing a thiol group.

[0029] Preferably, the present invention provides a method for producing a quantum dot composition, wherein the oligomer contains two or more types of compounds containing the carbon-carbon double bond.

[0030] Preferably, the method for producing a quantum dot composition is provided, wherein the compound containing a carbon-carbon double bond includes one type each of a compound containing 2 to 3 carbon-carbon double bonds per molecule and a compound containing one carbon-carbon double bond per molecule.

[0031] Preferably, the method for producing a quantum dot composition is provided, wherein the compound containing a carbon-carbon double bond includes one or more compounds containing a phenol group.

[0032] Preferably, the present invention provides a method for producing a quantum dot composition, wherein the compound containing a thiol group contains two to four functional groups.

[0033] Preferably, the present invention provides a method for producing a quantum dot composition, characterized in that the compound containing a carbon-carbon double bond and the compound containing a thiol group are mixed at a molar ratio of 2.75:1 to 5:1.

[0034] Preferably, the present invention provides a method for producing a quantum dot composition, characterized in that the compound containing 2 to 3 carbon-carbon double bonds per molecule and the compound containing one carbon-carbon double bond per molecule are mixed in a molar ratio of 0.01:1 to 1.5:1.

[0035] Preferably, the method for producing a quantum dot composition is characterized in that modifying the surface of the quantum dots includes performing a primary surface modification by adding a primary ligand represented by the following chemical formula 1, and then performing a secondary surface modification by adding a secondary ligand having 3 to 40 carbon atoms and containing a carboxyl group.

[0036] [ka] (In the above Chemical Formula 1, M is a divalent to tetravalent metal; m is an integer of 1 to 4, and X is independently an organic group having 3 to 20 carbon atoms; n is an integer from 2 to 4.

[0037] Preferably, the oligomer further comprises a thermal initiator and a polymerization inhibitor; The oligomer is stirred at room temperature before being mixed with the quantum dot dispersion, and then polymerized to produce an oligomer.

[0038] Preferably, the present invention provides a method for producing a quantum dot composition, which further comprises adding a photopolymerizable monomer, and adding and mixing a polymerization inhibitor, a photoinitiator, and a diffusing agent.

[0039] According to yet another aspect of the present invention, there is provided a cured film produced using the quantum dot composition.

[0040] According to yet another aspect of the present invention, there is provided a light-emitting device comprising the quantum dot composition.

[0041] According to yet another aspect of the present invention, there is provided a display device including the light emitting device. Effect of the Invention

[0042] Conventionally, it has been difficult to realize excellent optical properties while preventing aggregation between quantum dot particles, but the quantum dot composition and the manufacturing method thereof according to the present invention have the advantage of making it possible to achieve this, thereby making the manufacturing process convenient and simple and reducing costs.

[0043] In addition, the quantum dot composition according to the present invention has good electrical conductivity, does not cause aggregation between particles, and has excellent dischargeability, suitable viscosity, and excellent inkjetting properties, particularly as a quantum dot ink composition for EHD inkjet printing.

[0044] In addition, the quantum dot composition has excellent transparency and excellent optical properties.

[0045] In addition, the quantum dot composition according to the present invention can reduce out-gas emitted during curing due to the ligand, etc., thereby improving the quality of products manufactured therefrom. [Brief description of the drawings]

[0046] [Figure 1] 1 is a diagram showing some of the results of Experimental Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0047] The present invention will now be described.

[0048] All terms (including technical and scientific terms) used in this specification may be used as commonly understood by those having ordinary knowledge in the technical field to which the present invention belongs, unless otherwise defined. Furthermore, terms defined in commonly used dictionaries are not interpreted ideally or excessively unless otherwise clearly defined.

[0049] Furthermore, throughout this specification, when a part "comprises" a certain component, this does not mean to exclude other components, but means that it may further include other components, unless specifically stated to the contrary.

[0050] In addition, in this specification, "(meth)acrylate" means acrylate and methacrylate, "(meth)acrylic" means acrylic and methacrylic, and "(meth)acryloyl" means acryloyl and methacryloyl.

[0051] In addition, in this specification, "monomer" and "monomer" have the same meaning. In the present invention, a monomer is distinguished from an oligomer and a polymer, and refers to a compound having a weight average molecular weight of 1,000 or less. In this specification, a "photopolymerizable monomer" refers to a group involved in a polymerization reaction, such as a (meth)acrylate group.

[0052] In this specification, "substitution" means that a hydrogen atom in a compound or functional group is replaced with a C1-C30 alkyl group, a C2-C30 alkenyl group, a C2-C30 alkynyl group, a C1-C30 alkoxy group, a C1-C30 heteroalkyl group, a C3-C30 heteroalkylaryl group, a C3-C30 cycloalkyl group, a C3-C15 cycloalkenyl group, a C6-C30 cycloalkynyl group, a C2-C30 heterocycloalkyl group, a halogen (-F, -Cl, -Br or -I), a hydroxy group (-OH), a nitro group (-NO 2 ), a cyano group (-CN), an ester group (-C(=O)OR, where R is a C1-C10 alkyl or alkenyl group), an ether group (-OR, where R is a C1-C10 alkyl or alkenyl group), a carbonyl (-C(=O)-R, where R is a C1-C10 alkyl or alkenyl group), a carboxyl group (-COOH), and combinations thereof.

[0053] In this specification, the term "organic group" refers to a C1-C30 linear or branched alkyl group, a C2-C30 linear or branched alkenyl group, or a C2-C30 linear or branched alkynyl group, each of which may be substituted or unsubstituted.

[0054] As used herein, "alkyl" refers to a monovalent substituent derived from a straight or branched chain saturated hydrocarbon having 1 to 40 carbon atoms. Examples include, but are not limited to, methyl, ethyl, propyl, isobutyl, sec-butyl, pentyl, iso-amyl, hexyl, and the like.

[0055] As used herein, "alkenyl" refers to a monovalent substituent derived from a straight or branched unsaturated hydrocarbon having 2 to 40 carbon atoms and one or more carbon-carbon double bonds. Examples include, but are not limited to, vinyl, allyl, isopropenyl, 2-butenyl, etc.

[0056] <Quantum dot composition> A quantum dot composition according to one embodiment of the present invention includes quantum dots, photopolymerizable monomers and oligomers, where the oligomers include compounds containing carbon-carbon double bonds and compounds containing thiol groups.

[0057] The quantum dot composition according to one embodiment of the present invention is used for electrohydrodynamic inkjet printing and has a viscosity of 5000 cps or less, preferably in the range of 200 to 1000 cps, and more preferably in the range of 300 to 800 cps.

[0058] The composition of the quantum dot composition will be specifically described below.

[0059] Quantum dots Quantum dots (QDs) are nano-sized semiconductor materials that can have different energy band gaps depending on their size and composition, and can therefore emit light of various emission wavelengths.

[0060] Such quantum dots may have a homogeneous single layer structure, a multilayer structure such as a core-shell structure, a gradient structure, or a mixture of these. In the core-shell structure, the shell may be multilayered (e.g., core / shell / shell), where each layer may comprise a different component, e.g., a (semi)metal oxide.

[0061] The quantum dots can be freely selected from II-VI group compounds, III-V group compounds, IV-VI group compounds, group IV elements, group IV compounds, and combinations thereof. When the quantum dots have a core-shell structure, the core and shell can be freely composed of the following exemplary components.

[0062] By way of example, the II-VI compound may be a binary compound selected from the group consisting of CdO, CdS, CdSe, CdTe, ZnO, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, MgSe, MgS and mixtures thereof; CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdH ternary compounds selected from the group consisting of CdZnSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, MgZnSe, MgZnS, and mixtures thereof; and quaternary compounds selected from the group consisting of CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe, and mixtures thereof.

[0063] As another example, the III-V compound may be selected from the group consisting of binary compounds selected from the group consisting of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, and mixtures thereof; ternary compounds selected from the group consisting of GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, and mixtures thereof; and quaternary compounds selected from the group consisting of GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, and mixtures thereof.

[0064] As another example, the IV-VI compound may be selected from the group consisting of binary compounds selected from the group consisting of SnS, SnSe, SnTe, PbS, PbSe, PbTe, and mixtures thereof; ternary compounds selected from the group consisting of SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, and mixtures thereof; and quaternary compounds selected from the group consisting of SnPbSSe, SnPbSeTe, SnPbSTe, and mixtures thereof.

[0065] As another example, the group IV element may be selected from the group consisting of Si, Ge, and mixtures thereof. The group IV compound may also be a binary compound selected from the group consisting of SiC, SiGe, and mixtures thereof.

[0066] As another example, the alloy type compound is a ternary compound selected from InZnP, etc.

[0067] The two-element compound, three-element compound, or four-element compound may be present in a particle at a uniform concentration, or may be present in the same particle with a concentration distribution that is partially different. A quantum dot may also have a core / shell structure in which one quantum dot surrounds another. The interface between the core and the shell may have a concentration gradient in which the concentration of the element present in the shell decreases toward the center.

[0068] The shape of the quantum dots is not particularly limited as long as it is a shape commonly used in the art. For example, the shapes of the quantum dots may be spherical, rod-shaped, pyramidal, disk-shaped, multi-arm, or cubic nanoparticles, nanotubes, nanowires, nanofibers, nanoplate particles, and the like.

[0069] In addition, the size of the quantum dots is not particularly limited and can be appropriately adjusted within a normal range known in the art. As an example, the average particle size (D50) of the quantum dots is about 2 to 10 nm. In this way, when the particle size of the quantum dots is controlled in the range of about 2 to 10 nm, light of a desired hue can be emitted. For example, when the particle size of the quantum dot core / shell containing InP is about 5 to 6 nm, light of a wavelength of about 520 to 550 nm can be emitted, while when the particle size of the quantum dot core / shell containing InP is about 7 to 8 nm, light of a wavelength of about 620 to 640 nm can be emitted. For example, as the blue light-emitting QD, non-cadmium (Cd)-based III-V group QD (e.g., InP, InGaP, InZnP, GaN, GaAs, GaP) can be used.

[0070] In addition, the quantum dots may have a full width of half maximum (FWHM) of an emission wavelength spectrum of about 40 nm or less, and color purity and color reproducibility may be improved within this range. In addition, the light emitted through such quantum dots is emitted in all directions, and thus a wide viewing angle may be improved.

[0071] According to one embodiment of the present invention, the content of the quantum dots is 1 to 60 wt %, preferably 20 to 50 wt %, based on the total weight of the quantum dot composition depending on the properties of the quantum dots.

[0072] Oligomers In the quantum dot composition according to the present invention, the oligomer includes a compound containing a carbon-carbon double bond and a compound containing a thiol group. Preferably, the oligomer includes two or more compounds containing a carbon-carbon double bond, and may include, for example, one compound containing 2 to 3 carbon-carbon double bonds per molecule and one compound containing one carbon-carbon double bond per molecule.

[0073] In the case where the compound contains 2 to 3 carbon-carbon double bonds per molecule, the molecular weight is about 200 to 1000 g / mol, preferably about 200 to 800 g / mol, and more preferably about 200 to 500 g / mol. For example, triallyl isocyanurate can be used.

[0074] At this time, the compound containing a carbon-carbon double bond may contain one or more compounds containing a phenol group, and preferably, the compound containing a phenol group may be a compound containing one carbon-carbon double bond per molecule. After the quantum dot composition is cured, in the subsequent process, the ligands on the surface of the quantum dots are discharged in gas form (hereinafter, outgassing), which may cause problems such as cracking of the cured film, the light-emitting element, and the display device, and product defects such as poor paper lamination. However, when one or more compounds containing a phenol group are contained, there is an advantage that the generation of outgassing can be reduced. For example, phenol acrylate can be used.

[0075] The compound containing a thiol group contains 2 to 4 functional groups, preferably 2 to 4 thiol groups per molecule, and more preferably 2 to 3 thiol groups per molecule. For example, ethylene glycol di(3-mercaptopropionate) can be used.

[0076] The molar ratio of the compound containing a carbon-carbon double bond to the compound containing a thiol group is 2.75:1 to 5:1, preferably 2.75:1 to 4:1, and more preferably 2.75:1 to 3.5:1.

[0077] The molar ratio of the compound containing 2 to 3 carbon-carbon double bonds per molecule to the compound containing one carbon-carbon double bond per molecule is 0.01:1 to 1.5:1, preferably 0.1:1 to 1.5:1, and more preferably 0.3:1 to 1.2:1.

[0078] In compounds containing carbon-carbon double bonds, the carbon-carbon double bonds are independently one or more selected from the group including, but not limited to, an allyl group, a vinyl group, a (meth)acrylic group, an isopropenyl group, and a 2-butenyl group.

[0079] According to an embodiment of the present invention, the content of the oligomer is 1 to 50 wt %, preferably 10 to 45 wt %, based on the total weight of the quantum dot composition depending on the properties of the quantum dots.

[0080] Ligand In the quantum dot composition according to the present invention, the ligand serves to modify the surface of the quantum dots. Quantum dots have a barrier to dispersion in photopolymerizable monomers due to their hydrophobic surface characteristics, but the surface of the quantum dots can be modified with an appropriate ligand to improve the compatibility of the quantum dots with the photopolymerizable monomers.

[0081] According to one embodiment of the present invention, the ligand may include a primary ligand represented by the following Chemical Formula 1, and a secondary ligand having 3 to 40 carbon atoms and including a carboxyl group.

[0082] [ka] In the above Chemical Formula 1, M is a divalent to tetravalent metal, m is an integer of 1 to 4, and X is independently an organic group having 3 to 20 carbon atoms; n is an integer from 2 to 4.

[0083] The primary ligand may also be a metal-thiol compound formed by reacting a metal salt with a thiol compound.

[0084] In the primary ligand, M is a metal having a valence of 2 to 4. For example, M is a metal of Groups 2 to 14, such as Mg, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Cd, In, or Sn. In Chemical Formula 1, n is determined by the valence of M and is an integer of 2 to 4.

[0085] In addition, in the above Chemical Formula 1, X is also independently an organic group having 3 to 20 carbon atoms. For example, X is an ester (-C(=O)O-), an ether (-O-), a carbonyl (-C(=O)-), a carboxyl group (-C(=O)-OH), a sulfonyl (-SO 2 -), sulfide (-S-), sulfoxide (-SO-), alkoxy group (C n H 2n+1 X may also be an alkylene or alkenylene group having 3 to 20 carbon atoms containing one or more functional groups selected from the group consisting of an ester (-C(=O)O-) and a hydroxyl group (-OH). Specifically, X may also be an organic group having 4 to 20 carbon atoms containing an ester (-C(=O)O-) functional group.

[0086] In the primary ligand, the thiol group has excellent affinity with the surface of the quantum dot, and therefore can improve the dispersibility of the quantum dot in the photopolymerizable monomer. In addition, the primary ligand can include not only a thiol group but also an ester, ether, carbonyl, carboxyl group, alkoxy group, cycloalkoxy group, or hydroxyl group, thereby maximizing the dispersibility of the surface-modified quantum dot in the polar monomer having hydrophobicity. In addition, the quantum dot composition including such quantum dots can have advantageous properties (e.g., low viscosity) for the display process. Meanwhile, when a thiol-based compound having 3 or less carbon atoms is used, the surface of the quantum dots can be modified, but the high polarity of the surface-modified quantum dots makes it difficult to disperse them in general solvents and monomers.

[0087] The secondary ligand may have a carbon number of 3 to 40 and may include a carboxyl group. According to one embodiment of the present invention, the secondary ligand does not include a thiol group.

[0088] According to one embodiment of the present invention, the secondary ligand is represented by Formula 2: [ka] In the above Chemical Formula 2, L is a single bond or is selected from the group consisting of a substituted or unsubstituted C1-C20 alkylene group and a substituted or unsubstituted C1-C20 alkenylene group; A is a single bond or an ester (-C(=O)O-), ether (-O-), carbonyl (-C(=O)-), sulfonyl (-SO 2 a C1-C20 alkylene or alkenylene group containing one or more functional groups selected from the group consisting of aryl, aryloxy ... R is hydrogen or is selected from the group consisting of a substituted or unsubstituted C1-C20 alkyl group, and a substituted or unsubstituted C1-C20 alkenyl group.

[0089] Preferably, in the secondary ligand, A may include ester (-COO-), ether (-O-) and combinations thereof. Also, A may be a C2-C15 alkylene or alkenylene group, preferably a C2-C10 alkylene or alkenylene group.

[0090] In general, thiol-based ligands are known to have high reactivity with the surface of quantum dots. However, quantum dot compositions containing only thiol-based ligands have problems such as harmful odor generation and increased viscosity, which reduces storage stability, making them unsuitable for use in inkjet compositions. The quantum dot composition according to the present invention exhibits low viscosity and excellent storage stability by using a primary ligand containing a thiol-based ligand together with a secondary ligand not containing a thiol group. In addition, the secondary ligand has excellent dispersibility in photopolymerizable monomers by containing functional groups such as ester (-C(=O)O-), ether (-O-), carbonyl (-C(=O)-), and carboxyl group (-C(=O)-OH). On the other hand, if the secondary ligand has 16 or more carbon atoms, problems may occur in which the surface of the quantum dots is not modified or dispersibility in general solvents and monomers is impaired.

[0091] According to one embodiment of the present invention, the molar ratio of the primary ligand to the secondary ligand is 1:30-20:1, preferably 1:15-10:1, and more preferably 1:8-5:1, but is not limited thereto.

[0092] According to one embodiment of the present invention, the mixing ratio of the quantum dots to the ligand is 1:1 to 20 by weight, preferably 1:1 to 10 by weight, and more preferably 1:5 to 10 by weight. Here, the ligand means the sum of the primary ligand and the secondary ligand.

[0093] Photopolymerizable Monomer In the quantum dot composition according to the present invention, the photopolymerizable monomer controls the overall crosslink density of the polymer matrix, which is the formulation in which the quantum dots (QDs) are dispersed, thereby expressing the structure and various physical properties of the matrix. It can also improve flexibility and adhesiveness and adhesion to other materials.

[0094] The photopolymerizable monomer may include a (meth)acrylate monomer. The monomer that can be used is not particularly limited as long as it is a monomer that is commonly used in the relevant field.

[0095] As an example, the (meth)acrylate monomer may include at least one of a (meth)acrylic group, a vinyl group, and an allyl group. Specifically, there are 1,6-hexanediol diacrylate, 1,6-cyclohexanediol diacrylate, 2,2-dimethyl-1,3-propanediol diacrylate, diethylene glycol diacrylate, dipropylene glycol diacrylate, 1,3-butylene glycol dimethacrylate, trimethylolpropane trimethacrylate, isobornyl acrylate, isobornyl methacrylate, tetrahydrofuryl acrylate, acryloylmorpholine, 2-phenoxyethyl acrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol mono(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol hexaacrylate, and dipentaerythritol hexamethacrylate. These may be used alone or in a mixture of two or more. In the present invention, 1,6-hexanediol diacrylate is preferred as the photopolymerizable monomer to achieve the viscosity characteristics of the quantum dot composition.

[0096] In the present invention, the content of the (meth)acrylamide monomer is 1 to 50% by weight, preferably 3 to 40% by weight, based on the total weight of the quantum dot composition, depending on the properties of the quantum dots.

[0097] Photoinitiators In the quantum dot composition according to the present invention, the photoinitiator is a component that is excited by a light source such as ultraviolet (UV) light to initiate photopolymerization, and any photopolymerization initiator commonly used in the art can be used without limitation. Examples of such compounds include acetophenone-based compounds, benzophenone-based compounds, thioxanthone-based compounds, benzoin-based compounds, triazine-based compounds, and oxime-based compounds.

[0098] Non-limiting examples of photoinitiators that can be used include ethyl (2,4,6-trimethylbenzoyl)phenylphosphinate, Irgacure 184, Irgacure 369, Irgacure 651, Irgacure 819, Irgacure 907, benzion alkyl ether, benzophenone, benzyl dimethyl acetone, hydroxycyclohexyl phenyl acetone, chloroacetophenone, 1,1-dichloroacetophenone, diethoxyacetophenone, hydroxyacetophenone, 2-chlorothioxanthone, 2-ethylanthraquinone (2-ETAQ), 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone, methyl benzoylformate, etc. These may be used alone or in combination of two or more.

[0099] The content of the photoinitiator may be appropriately adjusted within a range known in the art. For example, it is 0.01 to 10 wt %, preferably 0.1 to 5 wt %, based on the total weight of the quantum dot composition. When the content of the photoinitiator falls within the above range, the photopolymerization reaction can be sufficiently carried out without deteriorating the physical properties of the matrix.

[0100] Diffusion Agent In the quantum dot composition according to the present invention, the diffusing agent reflects light that is not absorbed by the light conversion material and allows the light conversion material to absorb the reflected light again, i.e., the diffusing agent increases the amount of light absorbed by the light conversion material, thereby increasing the light conversion efficiency.

[0101] The diffusing agent may be any diffusing agent component known in the art without any restrictions. Such a diffusing agent may be a solid diffusing agent powder or a dispersion liquid in which the diffusing agent is dispersed.

[0102] A non-limiting example of a diffusing agent that can be used is barium sulfate (BaSO 4 ), calcium carbonate (CaCO 3 ), titanium dioxide (TiO 2 ), zirconia (ZrO 2 ) or a combination thereof. The average particle size and shape of the diffusing agent are not particularly limited and may be appropriately selected from among those known in the art. As an example, the average particle size (D50) is 150 nm to 250 nm, specifically, 180 nm to 230 nm. When the average particle size of the diffusing agent is within the above range, a more excellent light diffusing effect can be obtained, and the light conversion efficiency can be increased.

[0103] The content of the diffusing agent may be appropriately adjusted within a range known in the art. For example, it is 0.01 to 10 wt % based on the total weight of the quantum dot composition, and preferably 0.1 to 5 wt %. When the content of the diffusing agent falls within the above range, it can exhibit an effect of improving the light conversion efficiency without deteriorating the physical properties of the matrix.

[0104] Polymerization Inhibitor In the quantum dot composition according to the present invention, the polymerization inhibitor is a substance that reacts with radicals to form low-reactivity radicals or compounds that do not cause a polymerization reaction, and can control the rate of the photopolymerization reaction.

[0105] The polymerization inhibitor may be any known substance in the art without limitation, for example, a quinone compound, a phenol or aniline compound, or an aromatic nitro or nitroso compound. Specifically, there are hydroquinone (HQ), methylhydroquinone (THQ), hydroquinone monomethyl ether (MEHQ), hydroquinone monoethyl ether (EEHQ), 1,4-benzoquinone (BQ), 2,5-diphenylbenzoquinone (DPBQ), methyl-1,4-benzoquinone (MBQ), phenyl-1,4-benzoquinone (PBQ), 2,6-di-tert-butyl-4-methylphenol (BHT), 2,6-diphenyl-4-octadecyloxyphenol, catechol, phenothiazine, bis(α-methylbenzyl)phenothiazine, 3,7-dioctylphenothiazine, bis(α,α-dimethylbenzyl)phenothiazine, dimethyldithiocarbamic acid, diethyldithiocarbamic acid, dipropyldithiocarbamic acid, dibutyldithiocarbamic acid, diphenyldithiocarbamic acid, etc. These may be used alone or in combination of two or more.

[0106] The content of the polymerization inhibitor can be appropriately adjusted within a range known in the art, for example, 0.01 to 2% by weight, preferably 0.05 to 1 part by weight, based on the total weight of the quantum dot composition.

[0107] Other additives In addition to the above-mentioned components, the quantum dot composition of the present invention may contain additives known in the art without limitation, as long as the additives do not impair the effects of the present invention. In this case, the content of the additives may be appropriately adjusted within the range known in the art.

[0108] Examples of usable additives include silane compounds, siloxane compounds, antioxidants, polymerization inhibitors, lubricants, surface conditioners, surfactants, adhesion promoters, defoamers, slip agents, solvents, wetting agents, light stabilizers, stain inhibitors, softeners, thickeners, polymers, etc. These may be used alone or in combination of two or more.

[0109] The silane-based compound serves to impart adhesiveness to the matrix, and the siloxane-based compound serves to impart wetting properties. Such silane-based compounds and siloxane-based compounds may be any compounds known in the art without limitation.

[0110] The antioxidant suppresses discoloration caused by heat or light exposure, and by various oxidizing gases such as ozone, active oxygen, NOx, and SOx (X is an integer), and in the present invention, the addition of the antioxidant can prevent coloring of the matrix and reduce a decrease in film thickness caused by decomposition. Examples of usable antioxidants include hydrazides, hindered amine antioxidants, nitrogen-containing heterocyclic mercapto compounds, thioether antioxidants, hindered phenol antioxidants, ascorbic acids, zinc sulfate, thiocyanates, thiourea derivatives, sugars, nitrites, sulfites, thiosulfates, and hydroxylamine derivatives.

[0111] The leveling agent may be included for the purpose of increasing the adhesive strength within the composition by leveling the quantum dot composition so that the composition is coated evenly and smoothly. The leveling agent may include an acrylic or silicone-based agent alone or in combination of two or more types. As an example, the leveling agent may include polyether-modified polydimethylsiloxane, and may include a (meth)acryloyl group added to the polyether chain.

[0112] A surfactant may be included for the purpose of mixing and coating uniformity of the quantum dot composition. The surfactant may be a typical cationic, anionic, zwitterionic, or nonionic surfactant known in the art, and may be, for example, one or more of a fluorosurfactant, a silicone surfactant, and a fluorosilicone surfactant.

[0113] The light stabilizer is an ultraviolet absorbing agent and has the effect of increasing the weather resistance of the matrix, while the softening agent is for mitigating the occurrence of cracks in the dried polymer matrix, and can improve the impact resistance and flex resistance by mitigating the occurrence of cracks in the cured matrix.

[0114] <Method of manufacturing quantum dot composition> In another embodiment of the present invention, a method for producing a quantum dot composition includes modifying the surface of quantum dots, dispersing the quantum dots in a photopolymerizable monomer to obtain a quantum dot dispersion, and mixing the quantum dot dispersion with an oligomer. The oligomer may be produced by mixing a compound containing a carbon-carbon double bond and a compound containing a thiol group.

[0115] The method may include mixing the compound containing the carbon-carbon double bond and the compound containing the thiol group in a molar ratio of 2.75:1 to 5:1.

[0116] In this case, the mixture may contain two or more types of compounds containing a carbon-carbon double bond, may contain one type each of a compound containing 2 to 3 carbon-carbon double bonds per molecule and a compound containing one carbon-carbon double bond per molecule, or may include mixing the compound containing 2 to 3 carbon-carbon double bonds per molecule and the compound containing one carbon-carbon double bond per molecule in a molar ratio of 0.01:1 to 1.5:1.

[0117] The oligomer may further include a thermal initiator and a polymerization inhibitor, and may be prepared as an oligomer through a polymerization reaction after stirring at room temperature before being mixed with the quantum dot dispersion.

[0118] In addition, the compound containing a carbon-carbon double bond and the compound containing a thiol group are as described above in the quantum dot composition to the extent that they overlap.

[0119] Modifying the surface of the quantum dot may include performing a primary surface modification by adding a primary ligand represented by the following chemical formula 1, and then performing a secondary surface modification by adding a secondary ligand having 3 to 40 carbon atoms and including a carboxyl group.

[0120] [ka] (In the above Chemical Formula 1, M is a divalent to tetravalent metal; m is an integer of 1 to 4, and X is independently an organic group having 3 to 20 carbon atoms; n is an integer from 2 to 4.

[0121] Specifically, quantum dots are synthesized, a primary ligand is added to the solution in which the quantum dots are synthesized to perform primary surface modification, and the solution is then centrifuged to obtain quantum dots with primary surface modification. The quantum dots with primary surface modification are then dispersed in a photopolymerizable monomer, and a secondary ligand having 3 to 40 carbon atoms and including a carboxyl group is then added to perform secondary surface modification of the quantum dots.

[0122] Here, the quantum dots can be produced by any method known in the art (eg, a high-temperature injection method, a microfluidic reactor method, a method using microwave radiation, etc.).

[0123] The quantum dots can be synthesized by adding a primary ligand to a solution in which the quantum dots are synthesized while maintaining the temperature at about 60°C, stirring and reacting for 30 minutes to 3 hours to primarily modify the surface of the quantum dots, and then adding a secondary ligand and stirring and reacting for 30 minutes to 3 hours to secondary modify the surface of the quantum dots.

[0124] The surface modification of the quantum dots is carried out in two stages to prevent the formation of an addition product due to the reaction between the primary ligand and the secondary ligand. Meanwhile, when the primary ligand and the secondary ligand are simultaneously added to the quantum dots, an addition product may be formed by a thiol-ene reaction between the thiol group of the primary ligand and the acrylate of the secondary ligand. Such an addition product may increase the viscosity of the quantum dot composition when the surface-modified quantum dots are dispersed in a photopolymerizable monomer.

[0125] After the surface of the quantum dots is modified by the above method, the surface-modified quantum dots are obtained by centrifugation, and the quantum dot dispersion liquid can be prepared by dispersing the surface-modified quantum dots obtained in a photopolymerizable monomer.

[0126] In addition, the method may further include adding a photopolymerizable monomer to the quantum dot dispersion and the oligomer, and adding and mixing a polymerization inhibitor, a photoinitiator, and a diffusing agent.

[0127] <Cured product, light-emitting element, and display device> The present invention can provide a cured product containing the quantum dot composition. The cured product according to the present invention has excellent optical properties, specifically, a light absorption rate of 85% or more, preferably 90% or more. In addition, the cured product has a light conversion rate of 30% or more, specifically, 35% or more.

[0128] The cured product may be prepared by applying the quantum dot composition onto a substrate using an EHD inkjet spraying method to form a pattern, and curing the pattern.

[0129] The present invention provides a light-emitting device comprising the quantum dot composition. For example, a color filter is a thin-film optical component that extracts three colors, red, green, and blue, from white light emitted from a backlight source on a pixel-by-pixel basis to realize colors on a liquid crystal display.

[0130] Such color filters are manufactured by methods such as dyeing, pigment dispersion, printing, and electrodeposition. Also, color filters containing quantum dot compositions are manufactured by inkjet printing. In the inkjet printing, materials are used only for desired pixels, so that waste of unnecessary materials can be prevented.

[0131] The present invention also provides a display device including the quantum dot composition, which may be, but is not limited to, a liquid crystal display (LCD), an electroluminescent display (EL), a plasma display panel (PDP), a field emission display (FED), an organic light emitting device (OLED), and the like.

[0132] The present invention will be described in more detail with reference to the following examples. However, the following examples are for illustrative purposes only and are not intended to limit the scope of the present invention.

[0133] [Production Example 1-1] Production of primary ligand 1-1 1) Add about 280g of polyoxyethylene glycol methyl ether 400 and about 50g of mercaptosuccinic acid, heat to about 100°C, and react for about 12 hours. After the reaction is complete, cool to room temperature to obtain 330g of bis-(methoxypolyoxyethylene glycol) mercaptosuccinate-400. 2) In a round-bottom flask, add zinc chloride (ZnCl 2 1.7 g of Zn-bis-(methoxypolyoxyethylene glycol)mercaptosuccinate-400) and 32 g of bis-(methoxypolyoxyethylene glycol)mercaptosuccinate-400) were added to 134.5 g of hexyl acetate and dissolved by stirring at about 60° C. Then, HCl was removed under vacuum for 2 hours to produce the primary ligand Zn-bis-(methoxypolyoxyethylene glycol)mercaptosuccinate-400).

[0134] [Production Example 1-2] Production of primary ligand 1-2 In a round-bottom flask, add zinc chloride (ZnCl 2) and the compound represented by formula A-1 were added to hexyl acetate in a molar ratio of about 1:3, and then dissolved by stirring at about 60° C. Then, HCl was removed under vacuum for about 2 hours to prepare primary ligand 1-2.

[0135] [ka]

[0136] [Production Example 1-3] Production of primary ligand 1-3 Primary ligand 1-3 was prepared in the same manner as in Preparation Example 1-2, except that the compound represented by formula A-2 was used instead of the compound represented by formula A-1 in Preparation Example 1-2.

[0137] [ka]

[0138] [Production Example 1-4] Production of primary ligand 1-4 Primary ligand 1-4 was prepared in the same manner as in Preparation Example 1-2, except that the compound represented by formula A-3 was used instead of the compound represented by formula A-1 in Preparation Example 1-2.

[0139] [ka]

[0140] [Production Example 1-5] Production of primary ligand 1-5 Primary ligand 1-5 was prepared in the same manner as in Preparation Example 1-2, except that the compound represented by formula A-4 was used instead of the compound represented by formula A-1 in Preparation Example 1-2.

[0141] [ka]

[0142] [Production Example 1-6] Production of primary ligand 1-6 Primary ligand 1-6 was prepared in the same manner as in Preparation Example 1-2, except that the compound represented by formula A-5 was used instead of the compound represented by formula A-1 in Preparation Example 1-6.

[0143] [ka]

[0144] [Production Example 2-1] Production of secondary ligand 2-1 The compound represented by the chemical formula B-1 was added to hexyl acetate in a round-bottom flask and stirred at room temperature for about 1 hour to prepare secondary ligand 2-1.

[0145] [ka]

[0146] [Production Example 2-2] Production of secondary ligand 2-2 A secondary ligand 2-2 was prepared in the same manner as in Preparation Example 2-1, except that a compound represented by formula B-2 was used instead of the compound represented by formula B-1 in Preparation Example 2-1.

[0147] [ka]

[0148] [Production Example 2-3] Production of secondary ligand 2-3 Secondary ligand 2-3 was prepared in the same manner as in Preparation Example 2-1, except that the compound represented by formula B-3 was used instead of the compound represented by formula B-1 in Preparation Example 2-1.

[0149] [ka]

[0150] [Production Example 2-4] Production of secondary ligand 2-4 Secondary ligand 2-4 was prepared in the same manner as in Preparation Example 2-1, except that the compound represented by formula B-4 was used instead of the compound represented by formula B-1 in Preparation Example 2-1.

[0151] [ka]

[0152] [Production Example 2-5] Production of secondary ligand 2-5 Secondary ligand 2-5 was prepared in the same manner as in Preparation Example 2-1, except that the compound represented by formula B-5 was used instead of the compound represented by formula B-1 in Preparation Example 2-1.

[0153] [ka]

[0154] [Production Example 2-6] Production of secondary ligand 2-6 Secondary ligand 2-6 was prepared in the same manner as in Preparation Example 2-1, except that the compound represented by formula B-6 was used instead of the compound represented by formula B-1 in Preparation Example 2-1.

[0155] [ka]

[0156] [Production Example 3] Production of quantum dot (QD) dispersion 1) 750 ml of InZnP / ZnSe / ZnS (core / shell / shell) quantum dot dispersion solution (Hansol, quantum dot solid powder 20 wt%; hexyl acetate) was heated to about 60°C in a nitrogen atmosphere and stirred. About 9 g of the prepared primary ligand (1-1), Zn-bis-(methoxypolyoxyethylene glycol) mercaptosuccinate-400), was added and stirred for about 2 hours to perform primary surface modification of the quantum dots. 2) About 30 g of the prepared secondary ligand (2-2), mono(2-acryloyloxyethyl)succinate, was added to the solution containing the quantum dots that had been subjected to the primary surface modification, and the solution was stirred for about 2 hours to perform secondary surface modification of the quantum dots. 3) The solution containing the quantum dots after the surface modification was centrifuged twice with cyclohexane to obtain quantum dot powder, which was then dispersed in 1,6-hexanediol diacrylate (manufactured by MIWON) at 60 wt% to produce a QD dispersion.

[0157] [Production Example 4] Production of oligomer Production Example 4-1. Production of Oligomer A Based on 100 parts by weight of triallyl isocyanurate, 1 part by weight of 2,2'-azobis(2,4-dimethylvaleronitrile) and 0.1 parts by weight of methylhydroquinone were dissolved to prepare solution A. 25 parts by weight of solution A, 50 parts by weight of phenoxyethyl acrylate and 25 parts by weight of ethylene glycol di(3-mercaptopropionate) were mixed and stirred at room temperature for 1 hour. After stirring, the reactor temperature was set to about 80°C to prepare oligomer A by oligomer polymerization reaction.

[0158] Production Example 4-2. Production of Oligomer B Oligomer B was prepared in the same manner as in Preparation Example 4-1, except that about 42.9 parts by weight of Solution A prepared in Preparation Example 4-1, about 28.6 parts by weight of phenoxyethyl acrylate, and about 28.6 parts by weight of ethylene glycol di(3-mercaptopropionate) were mixed.

[0159] Production Example 4-3. Production of Oligomer C Oligomer C was prepared in the same manner as in Preparation Example 4-1, except that about 29.2 parts by weight of Solution A prepared in Preparation Example 4-1, about 41.7 parts by weight of phenoxyethyl acrylate, and about 29.2 parts by weight of ethylene glycol di(3-mercaptopropionate) were mixed.

[0160] Production Example 4-4. Production of Oligomer D Oligomer D was prepared in the same manner as in Preparation Example 4-1, except that 20 parts by weight of Solution A prepared in Preparation Example 4-1, 40 parts by weight of phenoxyethyl acrylate, and 40 parts by weight of ethylene glycol di(3-mercaptopropionate) were mixed.

[0161] Production Example 4-5. Production of Oligomer E Oligomer E was prepared in the same manner as in Preparation Example 4-1, except that 50 parts by weight of Solution A prepared in Preparation Example 4-1, 25 parts by weight of phenoxyethyl acrylate, and 25 parts by weight of ethylene glycol di(3-mercaptopropionate) were mixed.

[0162] <Example 1-1> Preparation of quantum dot composition A quantum dot composition was prepared by mixing 70 parts by weight of the green quantum dot dispersion (Hansol, quantum dot polymer 60 wt%: 1,6-hexanediol diacrylate 40 wt%) that had been surface-modified and 17.5 parts by weight of oligomer A, followed by mixing 5.4 parts by weight of 1,6-hexanediol diacrylate (manufactured by MIWON), 0.1 parts by weight of methylhydroquinone, 2 parts by weight of ethyl (2,4,6-trimethylbenzoyl) phenylphosphinate as a photoinitiator, and 5 parts by weight of titanium dioxide as a diffusing agent.

[0163] <Example 1-2> The procedure was the same as in Example 1, except that Oligomer B prepared in Preparation Example 4-2 was used instead of Oligomer A.

[0164] <Example 1-3> The procedure was the same as in Example 1, except that Oligomer C prepared in Preparation Example 4-3 was used instead of Oligomer A.

[0165] <Example 1-4> The procedure was the same as in Example 1, except that Oligomer D prepared in Preparation Example 4-4 was used instead of Oligomer A.

[0166] <Example 1-5> The procedure was the same as in Example 1, except that Oligomer E prepared in Preparation Example 4-5 was used instead of Oligomer A.

[0167] <Comparative Example 1-1> The procedure was the same as in Example 1, except that instead of Oligomer A, a monomer of 1,6-hexanediol diacrylate (manufactured by MIWON) was used.

[0168] <Comparative Example 1-2> The procedure was the same as in Example 1, except that Oligomer A was replaced with an aliphatic urethane acrylate-based oligomer, MIRAMER PU2042 (manufactured by MIWON Co., Ltd.).

[0169] <Comparative Example 1-3> The procedure was the same as in Example 1, except that instead of Oligomer A, an epoxy acrylate-based oligomer, MIRAMER SC6300 (manufactured by MIWON Co., Ltd.), was used.

[0170] <Example 2-1> A quantum dot composition was prepared by mixing 46.5 parts by weight of the red quantum dot dispersion (Hansol, quantum dot polymer 60 wt%: 1,6-hexanediol diacrylate 40 wt%) with 35.5 parts by weight of Oligomer A and then mixing 10.9 parts by weight of 1,6-hexanediol diacrylate, 0.1 parts by weight of methylhydroquinone, 2 parts by weight of ethyl (2,4,6-trimethylbenzoyl) phenylphosphinate as a photoinitiator, and 5 parts by weight of titanium dioxide as a diffusing agent.

[0171] <Example 2-2> The procedure was the same as in Example 2-1, except that Oligomer B prepared in Preparation Example 4-2 was used instead of Oligomer A.

[0172] <Comparative Example 2-1> The procedure was the same as in Example 2-1, except that a monomer of 1,6-hexanediol diacrylate (manufactured by MIWON) was used instead of Oligomer A.

[0173] The compositions of the examples and comparative examples are summarized in Table 1 below.

[0174] [Table 1]

[0175] Experimental Example 1. Evaluation of dispersibility and stability of QD dispersion and oligomer mixture In Examples 1-1 to 1-5, Examples 2-1 to 2-2, and Comparative Examples 1-2 to 1-3, which contain an oligomer in the composition, a mixture was produced by mixing only the QD dispersion and the oligomer composition. The results are shown in Table 2 below and FIG.

[0176] [Table 2]

[0177] In the mixed solutions of Examples 1-1, 1-2, 2-1 and 2-2, the QD dispersion and the oligomer have good mixability, are uniformly dispersed, and do not harden or aggregate even when left for a long time, and the mixed solutions have excellent stability.

[0178] On the other hand, it is found that the mixed liquids of Examples 1-3 to 1-5 and Comparative Examples 1-2 and 1-3 have insufficient dispersibility and stability. Specifically, it was found that in Examples 1-3 and 1-4, thermal curing occurred even at room temperature, and a part of the mixed liquid became hard like plastic, and in the case of Example 1-5, a phenomenon occurred in which the quantum dots and oligomers became entangled and aggregated, and it was found that the dispersibility was very insufficient. In addition, in Comparative Examples 1-2 and 1-3, phenomena such as curing and aggregation were not observed, but the overall mixability was not good, and the mixed liquid was found to be opaque.

[0179] Referring to FIG. 1, it can be seen that the mixed solutions of Examples 1-1 and 1-2 are transparent, whereas the mixed solutions of Comparative Examples 1-2 and 1-3 are cloudy.

[0180] Experimental Example 2: Evaluation of the light conversion rate and light absorption rate of the quantum dot cured material 1) Among the examples, the green quantum dot compositions of Examples 1-1 and 1-2 and Comparative Examples 1-1 to 1-3, which had good dispersibility and stability, were applied to a thickness of 10 μm on a 2 cm × 2 cm glass substrate using a spin coater (Mikasa Corporation, Opticoat MS-A150), and cured at 4000 mJ / cm using an LED curing device with a wavelength of 395 nm. 2 A cured film was produced by irradiating the sample with light at 1000 nm. A 2 cm x 2 cm single film specimen was then loaded into an integrating sphere device (QE-2100, manufactured by Otsuka Electronics Co., Ltd.) to measure the initial light absorption rate and the light conversion rate after curing (QE). The sample was then heat-treated (post-baked) at 180°C for 30 minutes in a nitrogen atmosphere, after which the light conversion rate (QE) was measured. The results are shown in Table 3 below.

[0181] [Table 3]

[0182] The cured films produced in Examples 1-1 and 1-2 and Comparative Examples 1-1 to 1-3 were produced with a substantially uniform thickness in the range of 10 μm to about 0.2 μm.

[0183] It was confirmed that the optical absorptance of all the examples was 87% or more, and the optical conversion rate was 35% or more, showing excellent optical properties.

[0184] On the other hand, the comparative examples, except for Comparative Example 1-1, do not exceed 87%, and even Comparative Example 1-1 shows a lower light absorption rate than the Examples. Comparative Example 1-1, in which a monomer was used instead of an oligomer, showed a light conversion rate of 32.8%, which is somewhat lower optical characteristics, and the oligomers used in Comparative Examples 1-2 to 1-3 did not have good dispersibility in the quantum dot dispersion liquid, and showed light conversion rates of 30.7% and 27.6%, which are lower than Comparative Example 1-1.

[0185] In the case of the examples, the light conversion rate after the heat treatment was maintained at 35% or more, with changes of 0.1% and 0.9%, respectively, and the change rates before and after the heat treatment were approximately 0.2% and 2.4%, respectively. On the other hand, in the comparative examples, the light conversion rate decreased by 0.1%, 0.3%, and 1.7%, respectively, and the change rates before and after the heat treatment were approximately 0.3%, 0.9%, and 6.2%, respectively.

[0186] Therefore, since the excellent optical properties of Examples 1-1 and 1-2 are well maintained both before and after heat treatment, when they are applied to light emitting devices, displays, etc. and commercialized, they will be able to maintain their optical properties for a longer period of time compared to the comparative examples.

[0187] 2) Using the red quantum dot compositions prepared in Examples 2-1, 2-2 and Comparative Example 2-1, cured films were prepared in the same manner as above, and the light absorptivity and light conversion rate were measured. In addition, the light conversion rate after heat treatment was measured in the same manner as above. The results are shown in Table 4 below.

[0188] [Table 4]

[0189] The cured films produced in Examples 2-1 and 2-2 and Comparative Example 2-1 were produced with a substantially uniform thickness in the range of 10 μm to about 0.1 μm.

[0190] It was confirmed that the optical absorptance of all the examples was 90% or more, and the optical conversion rate was 39% or more, showing excellent optical properties.

[0191] On the other hand, the comparative example in which a monomer was used instead of an oligomer had a light absorptance of less than 90% and a light conversion rate of 35%, which shows slightly lower optical properties than the examples.

[0192] In the case of the embodiment, the light conversion efficiency after the heat treatment was maintained at 39% or more, with changes of 0.1% and 0.4%, respectively, and the rates of change before and after the heat treatment were approximately 0.2% and 1.0%, respectively.

[0193] In the case of the comparative example, even if the light conversion rate after the heat treatment increased slightly, it was only at a level of 36%, and the optical characteristics were not as good as those of the examples.

[0194] In summary, the excellent optical properties of Examples 2-1 and 2-2 are well maintained both before and after heat treatment. Therefore, when they are applied to light emitting devices, displays, etc. and commercialized, they will be able to maintain their optical properties for a longer period of time than the comparative example.

[0195] Experimental Example 3. Viscosity evaluation of quantum dot composition The viscosity of the green quantum dot compositions of Examples 1-1 to 1-2 and Comparative Examples 1-1 to 1-3 was measured using a rotational rheometer (HAAKE MARS manufactured by Thermo Scientific) at room temperature (25° C.).

[0196] The viscosities of the red quantum dot compositions of Examples 2-1 to 2-2 and Comparative Example 2-1 were also measured by the same method. The results are shown in Table 5 below.

[0197] [Table 5]

[0198] The viscosities of the green quantum dot composition examples were approximately 392 cps and 417 cps, and the viscosities of the red quantum dot composition examples were approximately 495 cps and 734 cps, confirming that the viscosities are suitable for EHD inkjet printing as well as inkjet printing.

[0199] On the other hand, Comparative Examples 1-1 and 2-1, in which a monomer was used instead of an oligomer, showed low viscosities of about 35 cps and 22 cps, and were found to be unsuitable for EHD inkjet printing.

[0200] In addition, Comparative Examples 1-2 and 1-3, which used oligomers, were suitable in terms of viscosity, but considering the results of Experimental Examples 1 and 2, it was determined that they would be difficult to apply in practice.

[0201] Experimental Example 4. EHD (electrohydrodynamic) inkjet printing (inkjetting properties) evaluation The inkjetting properties (ejection properties) of the green quantum dot compositions of Examples 1-1 to 1-2 and Comparative Example 1-1 were measured. Specifically, the EHD inkjetting properties were evaluated using an iEHD printer (manufactured by ENJET) with a nozzle inner diameter of 75 μm. In addition, the inkjetting properties of the red quantum dot compositions of Examples 2-1 to 2-2 and Comparative Example 2-1 were measured by the same method, and the results are shown in Table 6 below.

[0202] [Table 6]

[0203] It was confirmed that all examples of the green quantum dot composition had no nozzle clogging and exhibited good EHD inkjet printing at a delta voltage of 1.4 kV (-0.6 kV to -2 kV), and the examples of the red quantum dot composition also had no nozzle clogging and exhibited good EHD inkjet printing at a delta voltage of 0.8 kV (-0.6 kV to -1.5 kV).

[0204] On the other hand, in Comparative Examples 1-1 and 2-1 in which a monomer was used instead of an oligomer, a problem was found in that the resin was not properly jetted only to the desired area during EHD printing due to its low viscosity.

[0205] However, in the case of Comparative Examples 1-2 and 1-3 in which oligomers were used, it was confirmed that the compositions had suitable viscosities for jetting properties based on the results of Experimental Example 3. However, taking into account the results of Experimental Example 1, the compositions were highly turbid and the raw materials were likely to precipitate, which raised concerns about nozzle clogging, so jetting properties were not evaluated.

[0206] It will be obvious to those having ordinary skill in the art to which the present invention pertains that the present invention is not limited to the above-described embodiments and can be modified or altered in various ways without departing from the technical scope of the present invention.

Claims

1. Quantum dots, photopolymerizable monomers and oligomers, The oligomer comprises a compound containing a carbon-carbon double bond and a compound containing a thiol group.

2. The quantum dot composition according to claim 1, wherein the oligomer contains two or more compounds containing the carbon-carbon double bond.

3. The compound containing a carbon-carbon double bond includes one type each of a compound containing 2 to 3 carbon-carbon double bonds per molecule and a compound containing one carbon-carbon double bond per molecule. The quantum dot composition according to claim 2.

4. 2. The quantum dot composition according to claim 1, wherein the compound containing a carbon-carbon double bond includes one or more compounds containing a phenol group.

5. The quantum dot composition according to claim 1, wherein the compound containing a thiol group contains two to four functional groups.

6. The compound containing a carbon-carbon double bond includes triallyl isocyanurate and phenol acrylate.

2. The quantum dot composition according to claim 1, wherein the compound containing a thiol group comprises ethylene glycol di(3-mercaptopropionate).

7. The quantum dot composition according to claim 3, characterized in that the molar ratio of the compound containing a carbon-carbon double bond to the compound containing a thiol group is 2.75:1 to 5:

1.

8. The molar ratio of the compound containing 2 to 3 carbon-carbon double bonds per molecule to the compound containing one carbon-carbon double bond per molecule is 0.01:1 to 1.5:

1. The quantum dot composition according to claim 7.

9. The quantum dot composition according to claim 1, wherein the carbon-carbon double bond is one or more selected from the group consisting of a vinyl group, an allyl group, a (meth)acrylic group, an isopropenyl group, and a 2-butenyl group.

10. 2. The quantum dot composition according to claim 1, wherein the viscosity at room temperature is in the range of 200 to 1000 cps.

11. The quantum dots include a primary ligand represented by the following formula 1:

2. The quantum dot composition according to claim 1, which is surface-modified with a secondary ligand having 3 to 40 carbon atoms and including a carboxyl group. 【Chemistry 1】 (In the above Chemical Formula 1, M is a divalent to tetravalent metal; m is an integer of 1 to 4, and X is independently an organic group having 3 to 20 carbon atoms; n is an integer from 2 to 4.

12. 10. The quantum dot composition of claim 1, wherein the composition is used for electrohydrodynamic inkjet printing.

13. After modifying the surface of the quantum dots, they are dispersed in a photopolymerizable monomer to obtain a quantum dot dispersion, which is then mixed with an oligomer. The method for producing a quantum dot composition, wherein the oligomer is produced by mixing a compound containing a carbon-carbon double bond and a compound containing a thiol group.

14. The method for producing a quantum dot composition according to claim 13, wherein the oligomer contains two or more compounds containing the carbon-carbon double bond.

15. The compound containing a carbon-carbon double bond includes one type each of a compound containing 2 to 3 carbon-carbon double bonds per molecule and a compound containing one carbon-carbon double bond per molecule. The method for producing a quantum dot composition according to claim 14.

16. The method for producing a quantum dot composition according to claim 13, wherein the compound containing a carbon-carbon double bond includes one or more compounds containing a phenol group.

17. The method for producing a quantum dot composition according to claim 13, characterized in that the compound containing a thiol group contains two to four functional groups.

18. The method for producing a quantum dot composition according to claim 15, characterized in that the compound containing a carbon-carbon double bond and the compound containing a thiol group are mixed in a molar ratio of 2.75:1 to 5:

1.

19. The compound containing 2 to 3 carbon-carbon double bonds per molecule and the compound containing 1 carbon-carbon double bond per molecule are mixed in a molar ratio of 0.01:1 to 1.5:

1. The method for producing a quantum dot composition according to claim 18.

20. The method for producing a quantum dot composition according to claim 13, wherein the surface modification of the quantum dots includes a primary surface modification by adding a primary ligand represented by the following Chemical Formula 1, and then a secondary surface modification by adding a secondary ligand having 3 to 40 carbon atoms and including a carboxyl group. 【Chemistry 2】 (In the above Chemical Formula 1, M is a divalent to tetravalent metal; m is an integer of 1 to 4, and X is independently an organic group having 3 to 20 carbon atoms; n is an integer from 2 to 4.

21. The oligomer further comprises a thermal initiator and a polymerization inhibitor; The method for producing a quantum dot composition according to claim 13, wherein the oligomer is prepared as an oligomer through a polymerization reaction after being stirred at room temperature before being mixed with the quantum dot dispersion liquid.

22. The method for preparing a quantum dot composition according to claim 13, further comprising: adding a photopolymerizable monomer, and adding and mixing a polymerization inhibitor, a photoinitiator, and a diffusing agent.

23. A cured film produced using the quantum dot composition of claim 1.

24. A light-emitting device comprising the quantum dot composition of claim 1.

25. A display device comprising the light emitting element of claim 24.

Citation Information

Patent Citations

  • Curable composition, photosensitive resin composition, photosensitive resin film, color filter, and method of manufacturing pixel

    CN109897449A

  • Photosensitive resin composition

    JP2013155258A

  • Self-assembled brush block copolymer nanoparticles for drug delivery

    JP2016539206A

  • Wavelength conversion member, backlight unit, image display device, resin composition for wavelength conversion member, and cured resin product

    JP2019174566A

  • Wavelength conversion member, backlight unit, image display device, and curable composition

    JP2020101804A