Optical film, circularly polarizing plate, and organic electroluminescence display device

The optical film with specific layer configurations addresses black discoloration issues in organic EL display devices by using vertically aligned discotic and rod-shaped liquid crystal layers, improving display quality through reduced black tinting.

JP2024149527AInactive Publication Date: 2024-10-18FUJIFILM CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024121148
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-01-25
Filing Date
2024-07-26
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing optical films used as circularly polarizing plates in organic electroluminescent (EL) display devices suffer from black discoloration issues in the front and diagonal directions.

Method used

The optical film is configured with three optically anisotropic layers: a layer formed by fixing a vertically aligned discotic liquid crystal compound, a layer formed by fixing a rod-shaped liquid crystal compound twisted with the thickness direction as the helical axis, and a layer formed by fixing vertically aligned rod-shaped liquid crystals, with specific alignments and retardations to suppress black tinting.

Benefits of technology

The configuration effectively suppresses black tinting in both the front and diagonal directions when used as a circularly polarizing plate in organic EL display devices, enhancing display quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149527000051
    Figure 2024149527000051
  • Figure 2024149527000052
    Figure 2024149527000052
  • Figure 2024149527000053
    Figure 2024149527000053
Patent Text Reader

Abstract

To provide an optical film with which coloring by black color in a front direction and an oblique direction is restricted when used in an organic EL display device as a circularly polarizing plate, and to provide a circularly polarizing plate and an organic EL display device.SOLUTION: An optical film is long-sized and includes an optical anisotropic layer (A), an optical anisotropic layer (B), and an optical anisotropic layer (C) in this order. In the optical anisotropic layer (A), a vertically oriented disk-shaped liquid crystal compound is fixed. In the optical anisotropic layer (B), a rod-like liquid crystal compound with a twisted orientation using a thickness direction as a helical axis is fixed. In the optical anisotropic layer (C), a vertically oriented rod-like liquid crystal compound is fixed. An in-plane slow axis of the optical anisotropic layer (A) is parallel to an in-plane slow axis on a surface on an optical anisotropic layer (A) side of the optical anisotropic layer (B). In the optical film, the optical anisotropic layer (A) and the optical anisotropic layer (B) are arranged so that mutual in-plane slow axes satisfy a prescribed positional relationship.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical film, a circular polarizing plate, and an organic electroluminescence display device. [Background technology]

[0002] 2. Description of the Related Art Optically anisotropic layers having refractive index anisotropy are used in various applications, such as antireflection films for organic electroluminescence (EL) display devices and optical compensation films for liquid crystal display devices. For example, Patent Document 1 discloses a retardation plate in which two types of optically anisotropic layers exhibiting predetermined optical characteristics are laminated. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5960743 Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have studied an optical film having the optically anisotropic layer described in Patent Document 1 laminated thereon, and have found that when the optically anisotropic layer is used as a circular polarizer in an organic EL display device, there is room for improvement in suppressing the occurrence of black tinting in the front direction and oblique directions.

[0005] An object of the present invention is to provide an optical film that, when used as a circular polarizing plate in an organic EL display device, suppresses black tinting in the front direction and oblique directions. Another object of the present invention is to provide a circular polarizing plate and an organic EL display device. [Means for solving the problem]

[0006] The present inventors have found that the above problems can be solved by the following configuration.

[0007] [1] A long optical film having an optically anisotropic layer (A), an optically anisotropic layer (B), and an optically anisotropic layer (C) in this order, the optically anisotropic layer (A) is a layer in which a vertically aligned discotic liquid crystal compound is fixed, the optically anisotropic layer (B) is a layer in which rod-like liquid crystal compounds are fixed and twisted in a helical axis along the thickness direction; The optically anisotropic layer (C) is a layer in which vertically aligned rod-like liquid crystal compounds are fixed, an in-plane slow axis of the optically anisotropic layer (A) is parallel to an in-plane slow axis of the optically anisotropic layer (B) on the surface facing the optically anisotropic layer (A); When observed from the optically anisotropic layer (C) side toward the optically anisotropic layer (A) side, if the in-plane slow axis of the optically anisotropic layer (A) rotates clockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (A) rotates counterclockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (A) side, When observed from the optically anisotropic layer (C) side towards the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite the optically anisotropic layer (A) side rotates clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) facing the optically anisotropic layer (A). [2] The in-plane retardation of the optically anisotropic layer (A) at a wavelength of 550 nm is 140 to 220 nm; the value of the product Δnd of the refractive index anisotropy Δn of the optically anisotropic layer (B) measured at a wavelength of 550 nm and the thickness d of the optically anisotropic layer (B) is 140 to 220 nm; The optical film according to [1], wherein the optically anisotropic layer (C) has an in-plane retardation of 0 to 10 nm at a wavelength of 550 nm and a thickness direction retardation of −120 to −20 nm at a wavelength of 550 nm. [3] The angle between the longitudinal direction of the long optical film and the in-plane slow axis of the optically anisotropic layer (A) is 40 to 85°; The twist angle of the twisted liquid crystal compound in the optically anisotropic layer (B) is 90±30°, When observed from the optically anisotropic layer (C) side toward the optically anisotropic layer (A) side, the in-plane slow axis of the optically anisotropic layer (A) rotates 40 to 85° clockwise with respect to the longitudinal direction of the long optical film; the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (A) rotates counterclockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (A) side; The optical film according to [1] or [2], wherein, when observed from the optically anisotropic layer (C) side towards the optically anisotropic layer (A) side, with respect to the longitudinal direction of the long optical film, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise by 40 to 85°, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (A) side rotates clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (A) side. [4] A long optical film having an optically anisotropic layer (A), an optically anisotropic layer (C), and an optically anisotropic layer (B) in this order, the optically anisotropic layer (A) is a layer in which horizontally aligned rod-like liquid crystal compounds are fixed, The optically anisotropic layer (C) is a layer in which a vertically aligned rod-like liquid crystal compound is fixed, the optically anisotropic layer (B) is a layer in which rod-like liquid crystal compounds are fixed and twisted in a helical axis along the thickness direction; an in-plane slow axis of the optically anisotropic layer (A) is parallel to an in-plane slow axis of the optically anisotropic layer (B) on the surface facing the optically anisotropic layer (C); When observed from the optically anisotropic layer (B) side toward the optically anisotropic layer (A) side, if the in-plane slow axis of the optically anisotropic layer (A) rotates clockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (C) side rotates clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) facing the optically anisotropic layer (C), When observed from the optically anisotropic layer (B) side towards the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite the optically anisotropic layer (C) side rotates counterclockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) facing the optically anisotropic layer (C). [5] The in-plane retardation of the optically anisotropic layer (A) at a wavelength of 550 nm is 140 to 220 nm; the value of the product Δnd of the refractive index anisotropy Δn of the optically anisotropic layer (B) measured at a wavelength of 550 nm and the thickness d of the optically anisotropic layer (B) is 140 to 220 nm; The optical film according to [4], wherein the optically anisotropic layer (C) has an in-plane retardation of 0 to 10 nm at a wavelength of 550 nm and a thickness direction retardation of −150 to −50 nm at a wavelength of 550 nm. [6] The angle between the longitudinal direction of the long optical film and the in-plane slow axis of the optically anisotropic layer (A) is 5 to 50°; The twist angle of the twisted liquid crystal compound in the optically anisotropic layer (B) is 90±30°, When observed from the optically anisotropic layer (B) side toward the optically anisotropic layer (A) side, with the longitudinal direction of the long optical film as a reference, if the in-plane slow axis of the optically anisotropic layer (A) rotates clockwise by 5 to 50°, with the in-plane slow axis of the surface of the optically anisotropic layer (B) facing the optically anisotropic layer (C) as a reference, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (C) side rotates clockwise, The optical film according to [4] or [5], wherein, when observed from the optically anisotropic layer (B) side towards the optically anisotropic layer (A) side, with the longitudinal direction of the long optical film as a reference, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise by 5 to 50°, with the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite the optically anisotropic layer (C) side rotates counterclockwise with the in-plane slow axis of the surface of the optically anisotropic layer (B) facing the optically anisotropic layer (C) side as a reference. [7] An optical film according to any one of [1] to [6] and a polarizer, A circularly polarizing plate in which a polarizer is disposed adjacent to an optically anisotropic layer (A) of an optical film. [8] The circular polarizing plate according to [7], wherein the polarizer has a luminous efficiency-corrected single transmittance of 44% or more. [9] The circularly polarizing plate according to [7] or [8], wherein the polarizer is formed using a composition containing a polymerizable liquid crystal compound.

[10] An organic electroluminescence display device comprising the optical film according to any one of [1] to [6] or the circular polarizing plate according to any one of [7] to [9]. Effect of the Invention

[0008] According to the present invention, it is possible to provide an optical film that, when used as a circular polarizing plate in an organic EL display device, suppresses black tinting in the front direction and oblique directions. Furthermore, according to the present invention, a circular polarizing plate and an organic EL display device can be provided. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the first embodiment of the optical film of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of the second embodiment of the optical film of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing one example of an embodiment of the circularly polarizing plate of the present invention. [Figure 4] FIG. 4 is a schematic cross-sectional view showing one example of an embodiment of the circularly polarizing plate of the present invention. [Diagram 5] FIG. 5 is an example of a schematic cross-sectional view of the first embodiment of the optical film of the present invention. [Figure 6] FIG. 6 is a diagram showing the relationship between the longitudinal direction of a long optical film and the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B) in one mode of the first embodiment of the optical film of the present invention. [Figure 7]FIG. 7 is a diagram showing the relationship between the longitudinal direction of a long optical film when observed from the direction of the white arrow in FIG. 5 and the angle between the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B). [Figure 8] FIG. 8 is a schematic cross-sectional view of another example of the first embodiment of the optical film of the present invention. [Figure 9] FIG. 9 is a diagram showing the relationship between the longitudinal direction of a long optical film and the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B) in another aspect of the first embodiment of the optical film of the present invention. [Figure 10] FIG. 10 is a diagram showing the relationship between the longitudinal direction of a long optical film when observed from the direction of the white arrow in FIG. 8 and the angle between the longitudinal direction and the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B). [Figure 11] FIG. 11 is an example of a schematic cross-sectional view of the second embodiment of the optical film of the present invention. [Figure 12] FIG. 12 is a diagram showing the relationship between the longitudinal direction of a long optical film and the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B) in one mode of the second embodiment of the optical film of the present invention. [Figure 13] FIG. 13 is a diagram showing the relationship between the longitudinal direction of a long optical film when observed from the direction of the white arrow in FIG. 11 and the angle between the longitudinal direction and the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B). [Figure 14] FIG. 14 is a schematic cross-sectional view of another example of the second embodiment of the optical film of the present invention. [Figure 15] FIG. 15 is a diagram showing the relationship between the longitudinal direction of a long optical film and the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B) in another aspect of the second embodiment of the optical film of the present invention. [Figure 16] FIG. 16 is a diagram showing the relationship between the longitudinal direction of a long optical film when observed from the direction of the white arrow in FIG. 14 and the angle between the longitudinal direction and the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In the present specification, each component may be used alone or in combination of two or more substances corresponding to each component. When two or more substances are used in combination for each component, the content of the component refers to the total content of the substances used in combination, unless otherwise specified. In addition, in this specification, "(meth)acrylic" is a notation representing "acrylic" or "methacrylic". Next, the terms used in this specification will be explained.

[0011] The slow axis is defined at 550 nm unless otherwise specified.

[0012] In the present invention, Re(λ) and Rth(λ) respectively represent the in-plane retardation and the retardation in the thickness direction at a wavelength λ, which is set to 550 nm unless otherwise specified. In the present invention, Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx+ny+nz) / 3) and the film thickness (d(μm)) into AxoScan, Slow axis direction (°) Re(λ)=R0(λ) Rth(λ)=((nx+ny) / 2-nz)×d is calculated. Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ).

[0013] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., Ltd.) and a sodium lamp (λ=589 nm) as a light source. In addition, when measuring wavelength dependency, it can be measured using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Co., Ltd.) in combination with an interference filter. In addition, values ​​from the Polymer Handbook (JOHN WILEY & SONS, INC.) and catalogs of various optical films can be used. The average refractive index values ​​of major optical films are shown below as examples: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).

[0014] In this specification, "light" refers to actinic rays or radiation, such as the emission line spectrum of a mercury lamp, far ultraviolet rays represented by excimer lasers, extreme ultraviolet rays (EUV light: Extreme Ultraviolet), X-rays, ultraviolet rays, and electron beams (EB). Among these, ultraviolet light is preferable.

[0015] In this specification, "visible light" refers to light having a wavelength of 380 to 780 nm. In addition, in this specification, unless otherwise specified, the measurement wavelength is 550 nm. In this specification, the angular relationship (e.g., "perpendicular", "parallel", etc.) is assumed to include the range of error permitted in the technical field to which the present invention pertains. Specifically, this means that the angle is within a range of less than ±10° from the exact angle, and the error from the exact angle is preferably within a range of ±5° or less, and more preferably within a range of ±3° or less.

[0016] In this specification, the horizontal alignment of rod-like liquid crystal compounds refers to a state in which the major axes of the liquid crystal compounds are aligned parallel to and in the same direction as the layer surface. Here, "horizontal" does not necessarily mean strictly horizontal, but means an orientation in which the inclination angle between the average molecular axis of the liquid crystal compound in the layer and the layer surface is less than 20°. In addition, the same orientation does not require the orientation to be strictly the same, but rather means that when the orientations of the slow axes are measured at any 20 positions within the plane, the maximum difference between the slow axis orientations at the 20 positions (the difference between the two slow axis orientations with the largest difference among the 20 slow axis orientations) is less than 10°. The vertical alignment of a discotic liquid crystal compound refers to a state in which the disc axis of the liquid crystal compound is aligned perpendicular to and in the same direction as the layer surface. Here, the term "vertical" does not necessarily mean strictly vertical, but means an orientation in which the inclination angle between the disc plane of the liquid crystal compound in the layer and the layer surface is 70 to 110°. In addition, the same orientation does not require the orientation to be strictly the same, but rather means that when the orientations of the slow axes are measured at any 20 positions within the plane, the maximum difference between the slow axis orientations at the 20 positions (the difference between the two slow axis orientations with the largest difference among the 20 slow axis orientations) is less than 10°.

[0017] In this specification, the optically anisotropic layer may be any layer that exhibits predetermined optical properties, and is preferably, for example, a layer in which the alignment state of aligned liquid crystal compounds is fixed. The "fixed" state is a state in which the alignment of the liquid crystal compound is maintained. Specifically, it is more preferable that the layer has no fluidity in a temperature range of usually 0 to 50° C., or under more severe conditions, −30 to 70° C., and that the alignment state is not changed by an external field or external force, and the fixed alignment state can be stably maintained.

[0018] The optically anisotropic layer contained in the optical film of the present invention is preferably a layer in which vertically aligned rod-like liquid crystal compounds or horizontally aligned discotic liquid crystal compounds are fixed. In view of their usefulness as compensation layers for circular polarizers and display devices, the layer in which vertically aligned rod-shaped liquid crystal compounds are fixed is preferably a positive C plate, and the layer in which horizontally aligned discotic liquid crystal compounds are fixed is preferably a negative C plate.

[0019] Here, the positive C plate and the negative C plate are defined as follows. When the refractive index in the slow axis direction in the film plane (the direction in which the in-plane refractive index is maximum) is nx, the refractive index in the direction perpendicular to the in-plane slow axis is ny, and the refractive index in the thickness direction is nz, the positive C plate satisfies the relationship in formula (C1), and the negative C plate satisfies the relationship in formula (C2). Note that the positive C plate has a negative Rth value, and the negative C plate has a positive Rth value. Formula (C1) nz>nx≒ny Formula (C2) nz <nx≒ny It should be noted that the above "≒" includes not only the case where the two are completely identical, but also the case where the two are substantially identical. The term "substantially the same" means that, for example, the absolute value of (nx-ny) x d (where d is the thickness of the film) is 0 to 10 nm, preferably 0 to 5 nm, is also included in "nx ≈ ny".

[0020] A characteristic feature of the optical film of the present invention is that three layers, namely, optically anisotropic layer (A), optically anisotropic layer (B) and optically anisotropic layer (C), each of which is formed by fixing a predetermined liquid crystal compound in a predetermined orientation, are arranged in a predetermined order, and the in-plane slow axes of the optically anisotropic layer (A) and the optically anisotropic layer (B) are arranged in a predetermined positional relationship. In Patent Document 1, as shown in Comparative Example 1 described later, when used as a circular polarizer in an organic EL display device, there is room for improvement in suppressing black coloring in the front direction and oblique directions. Therefore, in the present invention, as described above, the optically anisotropic layer (A), the optically anisotropic layer (B) and the optically anisotropic layer (C) are arranged in a predetermined order, and the optically anisotropic layer (A) and the optically anisotropic layer (B) are arranged in a predetermined positional relationship, so that it is considered that when applied to an organic EL display device as a circular polarizer, the black coloring in the front direction and oblique directions is suppressed.

[0021] [Optical film (first embodiment)] The optical film according to the first embodiment of the present invention is a long optical film having an optically anisotropic layer (A), an optically anisotropic layer (B), and an optically anisotropic layer (C) in this order, the optically anisotropic layer (A) is a layer in which a vertically aligned discotic liquid crystal compound is fixed, the optically anisotropic layer (B) is a layer in which rod-like liquid crystal compounds are fixed and twisted in a helical axis along the thickness direction; The optically anisotropic layer (C) is a layer in which vertically aligned rod-like liquid crystal compounds are fixed, an in-plane slow axis of the optically anisotropic layer (A) is parallel to an in-plane slow axis of the optically anisotropic layer (B) on the surface facing the optically anisotropic layer (A); When observed from the optically anisotropic layer (C) side toward the optically anisotropic layer (A) side, if the in-plane slow axis of the optically anisotropic layer (A) rotates clockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (A) rotates counterclockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (A) side, When observed from the optically anisotropic layer (C) side towards the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite the optically anisotropic layer (A) side rotates clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) facing the optically anisotropic layer (A).

[0022] [Optical film (second embodiment)] The optical film according to the second embodiment of the present invention is a long optical film having an optically anisotropic layer (A), an optically anisotropic layer (C), and an optically anisotropic layer (B) in this order, the optically anisotropic layer (A) is a layer in which horizontally aligned rod-like liquid crystal compounds are fixed, The optically anisotropic layer (C) is a layer in which a vertically aligned rod-like liquid crystal compound is fixed, the optically anisotropic layer (B) is a layer in which rod-like liquid crystal compounds are fixed and twisted in a helical axis along the thickness direction; an in-plane slow axis of the optically anisotropic layer (A) is parallel to an in-plane slow axis of the optically anisotropic layer (B) on the surface facing the optically anisotropic layer (C); When observed from the optically anisotropic layer (B) side toward the optically anisotropic layer (A) side, if the in-plane slow axis of the optically anisotropic layer (A) rotates clockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (C) side rotates clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) facing the optically anisotropic layer (C), When observed from the optically anisotropic layer (B) side towards the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite the optically anisotropic layer (C) side rotates counterclockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) facing the optically anisotropic layer (C).

[0023] [First embodiment] A first embodiment of the optical film of the present invention will be described below with reference to the drawings.

[0024] FIG. 1 is a schematic cross-sectional view showing an example of the first embodiment of the optical film of the present invention. An optical film 10 shown in FIG. 1 has an optically anisotropic layer (A) 1a, an optically anisotropic layer (B) 1b, and an optically anisotropic layer (C) 1c, in this order. Here, the optically anisotropic layer (A) 1a is a layer in which a vertically aligned discotic liquid crystal compound is fixed. The optically anisotropic layer (B) 1b is a layer in which rod-like liquid crystal compounds are fixed and helically aligned with the thickness direction as the helical axis. The optically anisotropic layer (C) 1c is a layer in which vertically aligned rod-like liquid crystal compounds are fixed.

[0025] Next, a description will be given with reference to FIGS. 5 has an optically anisotropic layer (A) 11a, an optically anisotropic layer (B) 11b, and an optically anisotropic layer (C) 11c in this order. The optically anisotropic layer (B) 11b is a layer in which a liquid crystal compound LC is fixed and twisted in a helical axis along the thickness direction.

[0026] The arrows in the optically anisotropic layer (A) 11a in Fig. 6 represent the in-plane slow axis on each surface, and the dashed line represents the longitudinal direction of the long optical film. As shown in Fig. 6, the in-plane slow axis on the surface 111a of the optically anisotropic layer (A) 11a opposite to the optically anisotropic layer (B) 11b side is parallel to the in-plane slow axis on the surface 112a of the optically anisotropic layer (A) 11a on the optically anisotropic layer (B) 11b side, and the angle between each in-plane slow axis and the longitudinal direction of the long optical film is represented by θ1. As shown in Fig. 7, when observed from the white arrow side in Fig. 5 [when observed from the optically anisotropic layer (C) 11c toward the optically anisotropic layer (A) 11a], the in-plane slow axis of the optically anisotropic layer (A) 11a rotates clockwise by θ1° with respect to the longitudinal direction of the long optical film indicated by the dashed line. In other words, the in-plane slow axis of the optically anisotropic layer (A) 11a is located at a position rotated clockwise by θ1°.

[0027] In addition, the arrows in the optically anisotropic layer (B) 11b in FIG. 6 indicate the in-plane slow axes on the respective surfaces. The in-plane slow axis of the optically anisotropic layer (A) 11a is parallel to the in-plane slow axis of the optically anisotropic layer (B) 11b on the surface of the optically anisotropic layer (A) 11a side. In other words, the angle between the in-plane slow axis of the optically anisotropic layer (B) 11b on the surface of the optically anisotropic layer (A) 11a side and the longitudinal direction of the long optical film corresponds to the above-mentioned θ1. In addition, the in-plane slow axis of the optically anisotropic layer (B) 11b on the surface 111b on the optically anisotropic layer (A) 11a side and the in-plane slow axis of the optically anisotropic layer (B) 11b on the surface 112b on the opposite side to the optically anisotropic layer (A) 11a side form a twist angle described later. In other words, when observed from the white arrow side in Fig. 5 (when observed from the optically anisotropic layer (C) 11c toward the optically anisotropic layer (A) 11a side), the in-plane slow axis of the optically anisotropic layer (B) 11b on the surface 111b on the optically anisotropic layer (A) 11a side of the optically anisotropic layer (B) 11b rotates at a predetermined angle counterclockwise based on the in-plane slow axis of the optically anisotropic layer (B) 11b on the surface 112b on the opposite side to the optically anisotropic layer (A) 11a side. That is, as shown in Figure 7, when observed from the side indicated by the white arrow in Figure 5 (when observed from the optically anisotropic layer (C) 11c toward the optically anisotropic layer (A) 11a), the in-plane slow axis of the optically anisotropic layer (A) 11a is located at a position rotated by a predetermined angle θ2° counterclockwise based on the in-plane slow axis of the optically anisotropic layer (A) 11a.

[0028] Next, a description will be given with reference to FIGS. 8 includes an optically anisotropic layer (A) 12a, an optically anisotropic layer (B) 12b, and an optically anisotropic layer (C) 12c in this order. The optically anisotropic layer (B) 12b is a layer formed by fixing a liquid crystal compound LC that is twisted and aligned with the thickness direction as the helical axis.

[0029] The arrows in the optically anisotropic layer (A) 12a in Fig. 9 represent the in-plane slow axis on each surface, and the dashed line represents the longitudinal direction of the long optical film. As shown in Fig. 9, the in-plane slow axis on the surface 121a of the optically anisotropic layer (A) 12a opposite to the optically anisotropic layer (B) 12b side is parallel to the in-plane slow axis on the surface 122a of the optically anisotropic layer (A) 12a on the optically anisotropic layer (B) 12b side, and the angle between each in-plane slow axis and the longitudinal direction of the long optical film is represented by θ1. As shown in Fig. 10, when observed from the white arrow side in Fig. 8 [when observed from the optically anisotropic layer (C) 11c toward the optically anisotropic layer (A) 11a side], the in-plane slow axis of the optically anisotropic layer (A) 12a rotates counterclockwise by θ1° with respect to the longitudinal direction of the long optical film indicated by the dashed line. In other words, the in-plane slow axis of the optically anisotropic layer (A) 12a is located at a position rotated counterclockwise by θ1°.

[0030] In addition, the arrows in the optically anisotropic layer (B) 12b in FIG. 9 indicate the in-plane slow axes on the respective surfaces. The in-plane slow axis of the optically anisotropic layer (A) 12a is parallel to the in-plane slow axis of the optically anisotropic layer (B) 12b on the surface of the optically anisotropic layer (A) 12a side. That is, the angle between the in-plane slow axis of the optically anisotropic layer (B) 12b on the surface of the optically anisotropic layer (A) 12a side and the longitudinal direction of the long optical film corresponds to the above-mentioned θ1. In addition, the in-plane slow axis of the optically anisotropic layer (B) 12b on the surface 121b on the optically anisotropic layer (A) 12a side and the in-plane slow axis of the optically anisotropic layer (B) 12b on the surface 122b opposite to the optically anisotropic layer (A) 12a side form a twist angle described later. In other words, when observed from the white arrow side in Fig. 8 [when observed from the optically anisotropic layer (C) 11c toward the optically anisotropic layer (A) 11a side], the in-plane slow axis of the optically anisotropic layer (B) 12b on the surface 121b on the optically anisotropic layer (A) 12a side of the optically anisotropic layer (B) 12b rotates at a predetermined angle clockwise based on the in-plane slow axis of the optically anisotropic layer (B) 12b on the surface 122b opposite to the optically anisotropic layer (A) 12a side. That is, as shown in Figure 10, when observed from the side indicated by the white arrow in Figure 8 (when observed from the optically anisotropic layer (C) 11c toward the optically anisotropic layer (A) 11a), the in-plane slow axis of the optically anisotropic layer (A) 12a is located at a position rotated a predetermined angle (twist angle) of θ2° clockwise based on the in-plane slow axis of the optically anisotropic layer (A) 12a.

[0031] [Second embodiment] A second embodiment of the optical film of the present invention will be described below with reference to the drawings.

[0032] FIG. 2 is a schematic cross-sectional view showing an example of the second embodiment of the optical film of the present invention. The optical film 20 shown in FIG. 2 has an optically anisotropic layer (A) 2a, an optically anisotropic layer (C) 2c, and an optically anisotropic layer (B) 2b in this order. Here, the optically anisotropic layer (A) 2a is a layer in which horizontally aligned rod-like liquid crystal compounds are fixed. The optically anisotropic layer (C) 2c is a layer in which vertically aligned rod-like liquid crystal compounds are fixed. The optically anisotropic layer (B) 2b is a layer in which rod-like liquid crystal compounds are fixed and helically aligned with the thickness direction as the helical axis.

[0033] Next, a description will be given with reference to FIGS. 11 includes an optically anisotropic layer (A) 21a, an optically anisotropic layer (C) 21c, and an optically anisotropic layer (B) 21b in this order. The optically anisotropic layer (B) 21b is a layer formed by fixing a liquid crystal compound LC that is twisted and aligned with the thickness direction as the helical axis.

[0034] The arrows in the optically anisotropic layer (A) 21a in Fig. 12 represent the in-plane slow axis on each surface, and the dashed line represents the longitudinal direction of the long optical film. As shown in Fig. 12, the in-plane slow axis on the surface 211a of the optically anisotropic layer (A) 21a opposite to the optically anisotropic layer (B) 21b side is parallel to the in-plane slow axis on the surface 212a of the optically anisotropic layer (A) 21a facing the optically anisotropic layer (B) 21b, and the angle between each in-plane slow axis and the longitudinal direction of the long optical film is represented by θ1. As shown in Fig. 13, when observed from the white arrow side in Fig. 11 [when observed from the optically anisotropic layer (B) 21b toward the optically anisotropic layer (A) 21a], the in-plane slow axis of the optically anisotropic layer (A) 11a rotates clockwise by θ1° with respect to the longitudinal direction of the long optical film indicated by the dashed line. In other words, the in-plane slow axis of the optically anisotropic layer (A) 11a is located at a position rotated clockwise by θ1°.

[0035] In addition, the arrows in the optically anisotropic layer (B) 21b in FIG. 12 indicate the in-plane slow axes on the respective surfaces. The in-plane slow axis of the optically anisotropic layer (A) 21a is parallel to the in-plane slow axis of the optically anisotropic layer (B) 21b on the surface facing the optically anisotropic layer (A) 21a. In other words, the angle between the in-plane slow axis of the optically anisotropic layer (B) 21b on the surface facing the optically anisotropic layer (A) 21a and the longitudinal direction of the long optical film corresponds to the above-mentioned θ1. In addition, the in-plane slow axis of the optically anisotropic layer (B) 21b on the surface 211b on the optically anisotropic layer (A) 21a side and the in-plane slow axis of the optically anisotropic layer (B) 21b on the surface 212b opposite to the optically anisotropic layer (A) 21a side form a twist angle described later. In other words, when observed from the white arrow side in Fig. 11 (when observed from the optically anisotropic layer (B) 21b toward the optically anisotropic layer (A) 21a side), the in-plane slow axis of the optically anisotropic layer (B) 21b on the surface 211b on the optically anisotropic layer (A) 21a side of the optically anisotropic layer (B) 21b rotates at a predetermined angle clockwise based on the in-plane slow axis of the optically anisotropic layer (B) 21b on the surface 212b opposite to the optically anisotropic layer (A) 21a side. That is, as shown in Figure 13, when observed from the side indicated by the white arrow in Figure 11 (when observed from the optically anisotropic layer (B) 21b toward the optically anisotropic layer (A) 21a), the in-plane slow axis of the optically anisotropic layer (A) 21a on the surface 212b of the optically anisotropic layer (B) 21b opposite the optically anisotropic layer (A) 21a is located at a position rotated a predetermined angle θ2° clockwise with respect to the in-plane slow axis of the optically anisotropic layer (A) 21a.

[0036] Next, a description will be given with reference to FIGS. 14 includes an optically anisotropic layer (A) 22a, an optically anisotropic layer (C) 22c, and an optically anisotropic layer (B) 22b in this order. The optically anisotropic layer (B) 22b is a layer formed by fixing a liquid crystal compound LC that is twisted and aligned with the thickness direction as the helical axis.

[0037] The arrows in the optically anisotropic layer (A) 22a in Fig. 15 represent the in-plane slow axis on each surface, and the dashed line represents the longitudinal direction of the long optical film. As shown in Fig. 15, the in-plane slow axis on the surface 221a of the optically anisotropic layer (A) 22a opposite to the optically anisotropic layer (B) 22b side is parallel to the in-plane slow axis on the surface 222a of the optically anisotropic layer (A) 22a on the optically anisotropic layer (B) 22b side, and the angle between each in-plane slow axis and the longitudinal direction of the long optical film is represented by θ1. As shown in Fig. 16, when observed from the white arrow side in Fig. 14 [when observed from the optically anisotropic layer (B) 22b toward the optically anisotropic layer (A) 22a], the in-plane slow axis of the optically anisotropic layer (A) 22a rotates counterclockwise by θ1° with respect to the longitudinal direction of the long optical film indicated by the dashed line. In other words, the in-plane slow axis of the optically anisotropic layer (A) 22a is located at a position rotated counterclockwise by θ1°.

[0038] In addition, the arrows in the optically anisotropic layer (B) 22b in FIG. 15 indicate the in-plane slow axes on the respective surfaces. The in-plane slow axis of the optically anisotropic layer (A) 22a is parallel to the in-plane slow axis of the optically anisotropic layer (B) 22b on the surface facing the optically anisotropic layer (A) 22a. In other words, the angle between the in-plane slow axis of the optically anisotropic layer (B) 22b on the surface facing the optically anisotropic layer (A) 22a and the longitudinal direction of the long optical film corresponds to the above-mentioned θ1. In addition, the in-plane slow axis of the optically anisotropic layer (B) 22b at the surface 221b on the optically anisotropic layer (A) 22a side and the in-plane slow axis of the optically anisotropic layer (B) 22b at the surface 222b opposite to the optically anisotropic layer (A) 22a side form a twist angle described later. In other words, when observed from the white arrow side in Fig. 14 (when observed from the optically anisotropic layer (B) 22b toward the optically anisotropic layer (A) 22a side), the in-plane slow axis of the optically anisotropic layer (B) 22b at the surface 222b opposite to the optically anisotropic layer (A) 22a side rotates counterclockwise at a predetermined angle based on the in-plane slow axis of the optically anisotropic layer (B) 22b at the surface 221b on the optically anisotropic layer (A) 22a side. That is, as shown in Figure 16, when observed from the side indicated by the white arrow in Figure 14 (when observed from the optically anisotropic layer (B) 22b toward the optically anisotropic layer (A) 22a), the in-plane slow axis of the optically anisotropic layer (A) 22a on the surface 222b of the optically anisotropic layer (B) 22b opposite the optically anisotropic layer (A) 22a is located at a position rotated a predetermined angle (twist angle) of θ2° counterclockwise based on the in-plane slow axis of the optically anisotropic layer (A) 22a.

[0039] <Optical anisotropic layer (A)> As described above, in the first embodiment, the optically anisotropic layer (A) is a layer in which vertically aligned discotic liquid crystal compounds are fixed, and in the second embodiment, the optically anisotropic layer (A) is a layer in which horizontally aligned rod-shaped liquid crystal compounds are fixed. In addition, the in-plane retardation of the optically anisotropic layer (A) at a wavelength of 550 nm is preferably 140 to 220 nm in both the first and second embodiments, and more preferably 150 to 200 nm in order to further suppress black tinge when an organic EL display device to which the optical film of the present invention is applied as a circular polarizer is viewed from the front or oblique direction (hereinafter, simply referred to as "black tinge is further suppressed").

[0040] In the first embodiment, the angle θ1 between the longitudinal direction of the long optical film and the in-plane slow axis of the optically anisotropic layer (A) is preferably from 40 to 85°, more preferably from 50 to 85°, and even more preferably from 65 to 85°. On the other hand, in the second embodiment, the angle θ1 between the longitudinal direction of the long optical film and the in-plane slow axis of the optically anisotropic layer (A) is preferably from 5 to 50°, more preferably from 5 to 40°, and even more preferably from 5 to 25°.

[0041] <Optical anisotropic layer (B)> In both the first and second embodiments, the optically anisotropic layer (B) is a layer in which a liquid crystal compound is fixed that is twisted and aligned with the thickness direction as the helical axis, and is preferably a layer in which a chiral nematic phase having a so-called helical structure is fixed. When forming the phase, it is preferable to use a mixture of a liquid crystal compound exhibiting a nematic liquid crystal phase and a chiral agent described later. The meaning of the "fixed" state is as described above.

[0042] In both the first and second embodiments, the value of the product Δnd of the refractive index anisotropy Δn of the optically anisotropic layer (B) measured at a wavelength of 550 nm and the thickness d of the optically anisotropic layer (B) is preferably 140 to 220 nm, more preferably 150 to 210 nm, and even more preferably 160 to 200 nm, in that black tinge is further suppressed. The refractive index anisotropy Δn means the refractive index anisotropy of the optically anisotropic layer. The above Δnd is measured using an AxoScan (polarimeter) device manufactured by Axometrics and the device analysis software of the same company.

[0043] The twist angle of the liquid crystal compound (the twist angle of the alignment direction of the liquid crystal compound) is preferably 90±30° (within a range of 60 to 120°), and from the viewpoint of further suppressing black coloring, is more preferably 90±20° (within a range of 70 to 110°), and further preferably 90±10° (within a range of 80 to 100°). The torsion angle is measured using an AxoScan (polarimeter) device manufactured by Axometrics Inc. and the device analysis software of the same company. The liquid crystal compound is twisted around the thickness direction of the optically anisotropic layer (B) as an axis, from one main surface to the other main surface of the optically anisotropic layer (B). Accordingly, the orientation direction (in-plane slow axis direction) of the liquid crystal compound differs depending on the position in the thickness direction of the optically anisotropic layer (B).

[0044] The in-plane slow axis of the optically anisotropic layer (A) is parallel to the in-plane slow axis of the optically anisotropic layer (B) on the surface of the optically anisotropic layer (A). In other words, the angle between the in-plane slow axis of the optically anisotropic layer (B) on the surface of the optically anisotropic layer (A) and the longitudinal direction of the long optical film corresponds to the above-mentioned θ1. In addition, the in-plane slow axis of the optically anisotropic layer (B) on the surface on the optically anisotropic layer (A) side and the in-plane slow axis of the optically anisotropic layer (B) on the surface opposite to the optically anisotropic layer (A) side preferably form the above-mentioned twist angle (within the range of 90±30°). Based on the in-plane slow axis of the optically anisotropic layer (B) on the surface on the optically anisotropic layer (A) side, the in-plane slow axis of the optically anisotropic layer (B) on the surface opposite to the optically anisotropic layer (A) side rotates a predetermined angle (within the range of 90±30°) clockwise.

[0045] (Chiral Agents) Various known chiral agents can be used to form a twisted alignment of a liquid crystal compound. The chiral agent has the function of inducing a helical structure of a liquid crystal compound. Since the sense or pitch of the helix induced by the chiral compound varies depending on the compound, the chiral compound may be selected according to the purpose. As the chiral agent, known compounds can be used, but it is preferable to have a cinnamoyl group.As examples of the chiral agent, the compounds described in Liquid Crystal Device Handbook (Chapter 3, Section 4-3, Chiral Agent for TN, STN, page 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989) and JP-A-2003-287623, JP-A-2002-302487, JP-A-2002-80478, JP-A-2002-80851, JP-A-2010-181852 and JP-A-2014-034581 can be exemplified.

[0046] Chiral agents generally contain asymmetric carbon atoms, but axially asymmetric compounds or planarly asymmetric compounds that do not contain asymmetric carbon atoms can also be used as chiral agents. Examples of axially asymmetric compounds or planarly asymmetric compounds include binaphthyl, helicene, paracyclophane and their derivatives. Chiral agents may have a polymerizable group. When both the chiral agent and the liquid crystal compound have a polymerizable group, a polymer having a repeating unit derived from the polymerizable liquid crystal compound and a repeating unit derived from the chiral agent can be formed by a polymerization reaction between the polymerizable chiral agent and the polymerizable liquid crystal compound. In this embodiment, the polymerizable group of the polymerizable chiral agent is preferably the same as the polymerizable group of the polymerizable liquid crystal compound. Therefore, the polymerizable group of the chiral agent is also preferably an unsaturated polymerizable group, an epoxy group or an aziridinyl group, more preferably an unsaturated polymerizable group, and particularly preferably an ethylenically unsaturated polymerizable group. The chiral agent may also be a liquid crystal compound.

[0047] As the chiral agent, isosorbide derivatives, isomannide derivatives, binaphthyl derivatives, etc. can be preferably used. As the isosorbide derivative, a commercially available product such as LC-756 manufactured by BASF may be used. The content of the chiral agent in the liquid crystal composition is preferably 0.01 to 200 mol %, more preferably 1 to 30 mol %, of the amount of the liquid crystal compound.

[0048] <Optical anisotropic layer (C)> In both the first and second embodiments, the optically anisotropic layer (C) is a layer in which vertically aligned rod-like liquid crystal compounds are fixed, and is preferably a layer containing a photoalignable polymer described later. In both the first and second embodiments, the in-plane retardation of the optically anisotropic layer (C) at a wavelength of 550 nm is preferably 0 to 10 nm. Further, the retardation in the thickness direction of the optically anisotropic layer (C) at a wavelength of 550 nm is preferably −120 to −20 nm in the first embodiment, and preferably −150 to −50 nm in the second embodiment. The in-plane retardation is more preferably 0 to 5 nm in order to further suppress black coloring. In the first embodiment, the retardation in the thickness direction is more preferably −110 to −30 nm, and more preferably −100 to −40 nm, in order to further suppress black coloring. In the second embodiment, the retardation is more preferably −140 to −60 nm, and more preferably −130 to −70 nm.

[0049] <Method of manufacturing optical film> The method for producing the optical film is not particularly limited, and any known method can be used. In particular, the method for producing the optical film can be carried out continuously by roll-to-roll. For example, an optically anisotropic layer (A) to an optically anisotropic layer (C) each exhibiting a predetermined optical property are prepared, and the optically anisotropic layers are bonded to a long support in a predetermined order via an adhesive layer (e.g., a pressure-sensitive adhesive layer or a bonding layer), thereby producing an optical film. Alternatively, the optically anisotropic layer (A) to the optically anisotropic layer (C) may be successively formed on a long support using a polymerizable liquid crystal composition described later to produce an optical film. For example, the polymerizable liquid crystal composition may be applied onto a long support to form the optically anisotropic layer (C), and then the polymerizable liquid crystal composition may be applied onto the optically anisotropic layer (C) to form the optically anisotropic layer (B), and the polymerizable liquid crystal composition may be further applied onto the optically anisotropic layer (B) to form the optically anisotropic layer (A). Furthermore, the above-mentioned method of laminating an optically anisotropic layer and the method of forming an optically anisotropic layer using a polymerizable liquid crystal composition may be combined. As a combined method, a polymerizable liquid crystal composition is applied onto a long support to form an optically anisotropic layer (C), a polymerizable liquid crystal composition is then applied onto the optically anisotropic layer (C) to form an optically anisotropic layer (B) to obtain a laminate, and then an optically anisotropic layer (A) formed by separately applying the polymerizable liquid crystal composition onto a long support is bonded to the optically anisotropic layer (B) via an adhesive layer (e.g., a pressure-sensitive adhesive layer or a bonding layer) to produce an optical film. As another combined method, a polymerizable liquid crystal composition is applied onto a long support to form an optically anisotropic layer (C), and then a polymerizable liquid crystal composition is applied onto the optically anisotropic layer (C) to form an optically anisotropic layer (A) to obtain a laminate, and then an optically anisotropic layer (B) formed by separately applying the polymerizable liquid crystal composition onto a long support is bonded to the optically anisotropic layer (C) via an adhesion layer (e.g., a pressure-sensitive adhesive layer or adhesive layer), thereby producing an optical film. Each component will be described in detail below.

[0050] (liquid crystal compound) The above-mentioned optically anisotropic layer (A), optically anisotropic layer (B) and optically anisotropic layer (C) are each a layer in which the above-mentioned liquid crystal compound is fixed in a predetermined alignment state, and it is preferable that the layer is formed using a composition containing a liquid crystal compound having a polymerizable group (hereinafter also referred to as "polymerizable liquid crystal composition"). Here, as the above-mentioned rod-shaped liquid crystal compound, for example, those described in claim 1 of JP-T-11-513019 and paragraphs 0026 to 0098 of JP-A-2005-289980 can be preferably used. As the above-mentioned discotic liquid crystal compound, for example, those described in paragraphs 0020 to 0067 of JP-A No. 2007-108732 and paragraphs 0013 to 0108 of JP-A No. 2010-244038 can be preferably used.

[0051] In the present invention, the rod-shaped liquid crystal compound may be a liquid crystal compound having forward wavelength dispersion or a liquid crystal compound having reverse wavelength dispersion. When the liquid crystal compound has forward wavelength dispersion, the production cost of the optical film is reduced and durability is improved, which is preferable. In this specification, a liquid crystal compound with forward wavelength dispersion is one in which, when the in-plane retardation (Re) value in the visible light range of an optically anisotropic layer prepared using this liquid crystal compound is measured, the Re value decreases as the measured wavelength increases, whereas a liquid crystal compound with reverse wavelength dispersion is one in which, when the Re value is similarly measured, the Re value increases as the measured wavelength increases.

[0052] The type of polymerizable group possessed by the liquid crystal compound is not particularly limited, and is preferably a functional group capable of an addition polymerization reaction, more preferably a polymerizable ethylenically unsaturated group or a ring-polymerizable group, and further preferably a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group.

[0053] The optically anisotropic layer produced in the present invention is a layer formed by fixing a liquid crystal compound having a polymerizable group (a rod-shaped liquid crystal compound or a discotic liquid crystal compound having a polymerizable group) by polymerization or the like, and once formed into a layer, it no longer needs to exhibit liquid crystallinity.

[0054] The content of the liquid crystal compound in the polymerizable liquid crystal composition is not particularly limited, but is preferably 60% by mass or more, more preferably 70% by mass or more, based on the total mass (solid content) of the polymerizable liquid crystal composition, in terms of ease of controlling the alignment state of the liquid crystal compound. The upper limit is not particularly limited, but is preferably 99% by mass or less, more preferably 97% by mass or less.

[0055] (Other Ingredients) The polymerizable liquid crystal composition may contain other components in addition to the liquid crystal compound. For example, the polymerizable liquid crystal composition may contain a polymerization initiator. When the polymerizable liquid crystal composition contains a polymerization initiator, the polymerization of the liquid crystal compound having a polymerizable group proceeds more efficiently. The polymerization initiator may be a known polymerization initiator, such as a photopolymerization initiator or a thermal polymerization initiator, with a photopolymerization initiator being preferred. The content of the polymerization initiator in the polymerizable liquid crystal composition is not particularly limited, but is preferably 0.01 to 20 mass %, more preferably 0.5 to 10 mass %, based on the total mass (solid content) of the polymerizable liquid crystal composition.

[0056] The polymerizable liquid crystal composition may contain a photosensitizer. The type of photosensitizer is not particularly limited, and examples include known photosensitizers. The content of the photosensitizer in the polymerizable liquid crystal composition is not particularly limited, but is preferably 0.01 to 20 mass %, more preferably 0.5 to 10 mass %, based on the total mass (solid content) of the polymerizable liquid crystal composition.

[0057] The polymerizable liquid crystal composition may contain a polymerizable monomer different from the liquid crystal compound having a polymerizable group. The polymerizable monomer may be a radical polymerizable compound or a cationic polymerizable compound, and a polyfunctional radical polymerizable monomer is preferable. The polymerizable monomer may be, for example, the polymerizable monomer described in paragraphs 0018 to 0020 of JP-A-2002-296423. The content of the polymerizable monomer in the polymerizable liquid crystal composition is not particularly limited, but is preferably from 1 to 50% by mass, and more preferably from 5 to 30% by mass, based on the total mass of the liquid crystal compound.

[0058] The polymerizable liquid crystal composition may contain a surfactant. Examples of the surfactant include conventionally known compounds, but fluorine-based compounds are preferred. Specifically, for example, the compounds described in paragraphs 0028 to 0056 of JP-A No. 2001-330725 and the compounds described in paragraphs 0069 to 0126 of JP-A No. 2003-295212 are included.

[0059] The polymerizable liquid crystal composition may contain a polymer. Examples of the polymer include cellulose esters. Examples of the cellulose esters include those described in paragraph 0178 of JP-A-2000-155216. The content of the polymer in the polymerizable liquid crystal composition is not particularly limited, but is preferably from 0.1 to 10% by mass, and more preferably from 0.1 to 8% by mass, based on the total mass of the liquid crystal compound.

[0060] The polymerizable liquid crystal composition forming the optically anisotropic layer (C) may contain a photoacid generator when the photoalignable polymer contained in the polymerizable liquid crystal composition is a cleavage-type photoalignable polymer described below. Examples of photoacid generators include onium salt compounds, trichloromethyl-s-triazines, sulfonium salts, iodonium salts, quaternary ammonium salts, diazomethane compounds, imide sulfonate compounds, and oxime sulfonate compounds. Among these, onium salt compounds, imide sulfonate compounds, and oxime sulfonate compounds are preferred, and onium salt compounds and oxime sulfonate compounds are more preferred. The photoacid generators can be used alone or in combination of two or more.

[0061] In addition to the above, the polymerizable liquid crystal composition may contain an additive (alignment control agent) that promotes horizontal or vertical alignment in order to bring the liquid crystal compound into a horizontal or vertical alignment state.

[0062] (Photo-oriented polymer) Any photo-alignable polymer that may be contained in the optically anisotropic layer (C) of the optical film of the present invention (hereinafter, also formally abbreviated as "photo-alignable polymer of the present invention") is a polymer having a photo-alignable group.

[0063] The photo-alignable group possessed by the photo-alignable polymer of the present invention refers to a group having a photo-alignment function in which rearrangement or an anisotropic chemical reaction is induced when irradiated with anisotropic light (e.g., plane polarized light, etc.). Photo-alignable groups that undergo at least one of dimerization and isomerization due to the action of light are preferred, because they provide excellent alignment uniformity and good thermal and chemical stability.

[0064] Specific examples of the group that dimerizes by the action of light preferably include groups having a skeleton of at least one derivative selected from the group consisting of cinnamic acid derivatives, coumarin derivatives, chalcone derivatives, maleimide derivatives, and benzophenone derivatives. On the other hand, specific examples of groups that are isomerized by the action of light preferably include groups having a skeleton of at least one compound selected from the group consisting of an azobenzene compound, a stilbene compound, a spiropyran compound, a cinnamic acid compound, and a hydrazono-β-ketoester compound.

[0065] Of these photoalignable groups, a group selected from the group consisting of a cinnamoyl group, an azobenzene group, a chalconyl group, and a coumarin group is preferred, because the liquid crystal alignment of the optically anisotropic layer formed on the upper layer is better even with a small amount of exposure.

[0066] The photoalignable polymer of the present invention is preferably a photoalignable polymer that contains a repeating unit having a photoalignable group and a repeating unit having a fluorine atom or a silicon atom during the formation of the optically anisotropic layer (C). In addition, because the photoalignable polymer of the present invention provides better liquid crystal alignment properties in the optically anisotropic layer formed on the upper layer, it is preferable that the photoalignable polymer of the present invention has a repeating unit A containing a cleavage group that decomposes to produce a polar group by the action of at least one selected from the group consisting of light, heat, acid and base, and that the repeating unit A has a cleavage group in its side chain and has a fluorine atom or a silicon atom on the terminal side of the cleavage group in the side chain (hereinafter also referred to as "cleavage-type photoalignable polymer"). Here, the "polar group" contained in the repeating unit A refers to a group having at least one heteroatom or halogen atom, and specific examples thereof include a hydroxyl group, a carbonyl group, a carboxyl group, an amino group, a nitro group, an ammonium group, a cyano group, etc. Among these, a hydroxyl group, a carbonyl group, and a carboxyl group are preferred. Furthermore, the term "cleavable group that generates a polar group" refers to a group that generates the above-mentioned polar group upon cleavage, but in the present invention also includes a group that reacts with an oxygen molecule after radical cleavage to generate a polar group.

[0067] Examples of such cleavable photo-alignable polymers include the photo-alignable polymers described in paragraphs

[0014] to

[0049] of International Publication No. 2018 / 216812, the contents of which are incorporated herein by reference.

[0068] Other examples of photoalignable polymers containing a repeating unit having a fluorine atom or a silicon atom include copolymers (hereinafter also referred to as "specific copolymers") having a repeating unit having a fluorine atom or a silicon atom, represented by the following formula (1) or formula (2), and a repeating unit having a photoalignable group. The repeating unit having a fluorine atom or a silicon atom represented by the following formula (1) or formula (2) is a repeating unit containing a cleavable group that is decomposed by the action of at least one selected from the group consisting of light, heat, acid and base to generate a polar group.

[0069] <<Repeating unit having a fluorine atom or a silicon atom represented by formula (1) or formula (2)>>

[0070] [ka]

[0071] In the above formulas (1) and (2), r and s each independently represent an integer of 1 or more. Also, R B1 and R B2 each independently represents a hydrogen atom or a substituent. Also, Y 1 and Y 2 each independently represents -O- or -NR Z -, where R Z represents a hydrogen atom or a substituent. Also, L B1 represents a linking group having a valence of r+1. Also, L B2 represents a linking group having a valence of s+1. In addition, B1 represents a group represented by the following formula (B1): B1and when r is an integer of 2 or more, multiple B1's may be the same or different. In addition, B2 represents a group represented by the following formula (B2): B2 and when s is an integer of 2 or more, multiple B2's may be the same or different.

[0072] [ka]

[0073] In the above formulas (B1) and (B2), * represents a bonding position. Furthermore, n represents an integer of 1 or greater, provided that multiple n's may be the same or different. Additionally, m represents an integer of 2 or more. Also, R b1 represents a hydrogen atom or a substituent. Also, R b2 , R b3 , and R b4 Each independently represents a hydrogen atom or a substituent. b3 may be bonded to each other to form a ring, and multiple R b2 may be the same or different, and multiple R b3 may be the same or different, and multiple R b4 may be the same or different. Also, L b1 represents a n+1-valent linking group. b1 may be the same or different. Also, L b2 represents a linking group having a valence of m+1. Furthermore, Z represents an aliphatic hydrocarbon group having a fluorine atom or an organosiloxane group, provided that the aliphatic hydrocarbon group may have an oxygen atom, and multiple Z's may be the same or different.

[0074] In the above formula (1), R B1 Examples of the substituent represented by include known substituents. Among them, an alkyl group having 1 to 12 carbon atoms is preferable, and a methyl group is more preferable.

[0075] In the above formula (1), Y 1 each independently represents -O- or -NR Z - represents R Z represents a hydrogen atom or a substituent. Z The substituent of Y may be a known substituent, and is preferably a methyl group. 1 Preferably, —O— or —NH— is represented, and more preferably —O—.

[0076] In the above formula (1), L B1 represents a linking group having a valence of r+1. The r+1 valent linking group is preferably an r+1 valent hydrocarbon group having 1 to 24 carbon atoms which may have a substituent, in which some of the carbon atoms constituting the hydrocarbon group may be substituted with heteroatoms, and more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may contain an oxygen atom or a nitrogen atom. The r+1 valent linking group is preferably a divalent or trivalent linking group, and more preferably a divalent linking group.

[0077] In the above formula (1), r represents an integer of equal to or greater than 1. Among them, from the viewpoint of suitability for synthesis, an integer of 1 to 3 is preferable, an integer of 1 to 2 is more preferable, and 1 is even more preferable.

[0078] In the above formula (2), R B2 Examples of the substituent represented by include known substituents. Among them, an alkyl group having 1 to 12 carbon atoms is preferable, and a methyl group is more preferable.

[0079] In the above formula (2), Y 2 is -O- or -NR Z -, where R Z represents a hydrogen atom or a substituent. ZThe substituent of Y may be a known substituent, and is preferably a methyl group. 2 Preferably, —O— or —NH— is represented, and more preferably —O—.

[0080] In the above formula (2), L B2 represents a linking group having a valence of s+1. The s+1 valent linking group is preferably an s+1 valent hydrocarbon group having 1 to 24 carbon atoms which may have a substituent, in which some of the carbon atoms constituting the hydrocarbon group may be substituted with heteroatoms, and more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may contain an oxygen atom or a nitrogen atom. The s+1 valent linking group is preferably a divalent linking group.

[0081] In the above formula (2), s represents an integer of equal to or greater than 1. Among them, from the viewpoint of suitability for synthesis, an integer of 1 to 2 is preferable, and 1 is more preferable.

[0082] In the above formula (B1), R b1 The substituent represented by R is preferably an aliphatic hydrocarbon group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, and particularly preferably a methyl group. b1 is preferably a substituent.

[0083] In the above formula (B1), R b2 The substituent represented by R in the above formula (B1) may be a known substituent. b1 The substituents of R b2 preferably represents a hydrogen atom.

[0084] In the above formula (B1), L b1 represents an n+1 valent linking group, and the n+1 valent linking group is an n+1 valent hydrocarbon group having 1 to 24 carbon atoms which may have a substituent, preferably a hydrocarbon group in which some of the carbon atoms constituting the hydrocarbon group may be substituted with a heteroatom, and more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may contain an oxygen atom or a nitrogen atom.

[0085] The (n+1)-valent linking group is preferably a divalent to tetravalent linking group, more preferably a divalent to trivalent linking group, and even more preferably a divalent linking group.

[0086] In the above formula (B1), n ​​represents an integer of equal to or greater than 1. Among them, from the viewpoint of suitability for synthesis, an integer of 1 to 5 is preferable, an integer of 1 to 3 is more preferable, and 1 is even more preferable.

[0087] In the above formula (B1) and formula (B2), Z represents an aliphatic hydrocarbon group having a fluorine atom or an organosiloxane group, provided that the aliphatic hydrocarbon group may have an oxygen atom, and multiple Z may be the same or different. Examples of the aliphatic hydrocarbon group having a fluorine atom include a fluorine atom-containing alkyl group, a fluorine atom-containing alkyl group in which one or more of -CH2- constituting the fluorine atom are replaced with -O-, a fluorine atom-containing alkenyl group, etc. The number of carbon atoms in the fluorine atom-containing aliphatic hydrocarbon group is not particularly limited, and is preferably 1 to 30, more preferably 3 to 20, and further preferably 3 to 10. The number of fluorine atoms contained in the fluorine atom-containing aliphatic hydrocarbon group is not particularly limited, and is preferably 1-30, more preferably 5-25, and even more preferably 7-20.

[0088] In the above formula (B2), R b3 and R b4 The substituent represented by R in the above formula (B1) may be a known substituent. b1 The substituents represented by R b3 is two Rb 3 are preferably bonded to each other to form a ring, and two Rb 3 More preferably, R are bonded to each other to form a cyclohexane ring. b4 preferably represents a hydrogen atom.

[0089] In the above formula (B2), L b2 represents a linking group having a valence of m+1. The (m+1)-valent linking group is preferably an (m+1)-valent hydrocarbon group having 1 to 24 carbon atoms which may have a substituent, in which some of the carbon atoms constituting the hydrocarbon group may be substituted with a heteroatom, and more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may contain an oxygen atom or a nitrogen atom. The (m+1)-valent linking group is preferably a trivalent or tetravalent linking group, and more preferably a tetravalent linking group.

[0090] In the above formula (B2), m represents an integer of 2 or greater. Among them, from the viewpoint of synthesis suitability, an integer of 2 to 4 is preferred, and an integer of 2 to 3 is more preferred.

[0091] Specific examples of the repeating unit containing a group represented by formula (B1) above include repeating units represented by formulas B-1 to B-22 below, and specific examples of the repeating unit containing a group represented by formula (B2) above include repeating units represented by formulas B-23 to B-24 below.

[0092] [ka] JPEG2024149527000004.jpg38135 JPEG2024149527000005.jpg51141 JPEG2024149527000006.jpg38131 JPEG2024149527000007.jpg37137 JPEG2024149527000008.jpg4377 JPEG2024149527000009.jpg39109 JPEG2024149527000010.jpg4474

[0093] The content of the repeating units having a group represented by formula (1) or (2) in the photoalignment polymer is not particularly limited, and is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, particularly preferably 20% by mass or more, preferably 95% by mass or less, more preferably 80% by mass or less, even more preferably 70% by mass or less, particularly preferably 60% by mass or less, and most preferably 50% by mass or less, relative to the total repeating units of the photoalignment polymer, because this improves the liquid crystal alignment properties of the optically anisotropic layer formed in the upper layer.

[0094] <<Repeating units having photoalignment groups>> The structure of the main chain of the repeating unit having a photoalignable group is not particularly limited, and examples thereof include known structures, and for example, a skeleton selected from the group consisting of (meth)acrylic, styrene, siloxane, cycloolefin, methylpentene, amide, and aromatic ester structures is preferred. Among these, a skeleton selected from the group consisting of a (meth)acrylic, a siloxane, and a cycloolefin skeleton is more preferred, and a (meth)acrylic skeleton is even more preferred.

[0095] Specific examples of the repeating unit having a photoalignable group include the following.

[0096] [ka]

[0097] [ka]

[0098] [ka]

[0099] [ka]

[0100] [ka]

[0101] [ka]

[0102] The content of the repeating units having photoalignable groups in the photoalignable polymer is not particularly limited, and is preferably 5 to 60 mass %, more preferably 10 to 50 mass %, and even more preferably 15 to 40 mass %, of the total repeating units of the photoalignable polymer, because this improves the liquid crystal alignment of the optically anisotropic layer formed on the upper layer.

[0103] <<Repeating units having crosslinkable groups>> The specific copolymer may further have a repeating unit having a crosslinkable group in addition to the repeating unit having a group represented by the above formula (1) or (2) and the repeating unit having a photoalignable group. The type of crosslinkable group is not particularly limited, and examples thereof include known crosslinkable groups, such as an epoxy group, an epoxycyclohexyl group, an oxetanyl group, an acryloyl group, a methacryloyl group, a vinyl group, a styryl group, and an allyl group.

[0104] The structure of the main chain of the repeating unit having a crosslinkable group is not particularly limited, and examples thereof include known structures. For example, a skeleton selected from the group consisting of (meth)acrylic, styrene, siloxane, cycloolefin, methylpentene, amide, and aromatic ester skeletons is preferred. Among these, a skeleton selected from the group consisting of a (meth)acrylic, a siloxane, and a cycloolefin skeleton is more preferred, and a (meth)acrylic skeleton is even more preferred.

[0105] Specific examples of the repeating unit having a crosslinkable group include the following.

[0106] [ka]

[0107] The content of the repeating unit having a crosslinkable group in the specific copolymer is not particularly limited, but is preferably 10 to 60% by mass, more preferably 20 to 50% by mass, based on the total repeating units of the photoalignment polymer, because this improves the liquid crystal alignment properties of the optically anisotropic layer formed on the upper layer.

[0108] Examples of monomers (radical polymerizable monomers) that form other repeating units than those described above include acrylic acid ester compounds, methacrylic acid ester compounds, maleimide compounds, acrylamide compounds, acrylonitrile, maleic anhydride, styrene compounds, and vinyl compounds.

[0109] The method for synthesizing the photoalignable polymer of the present invention is not particularly limited, and the polymer can be synthesized, for example, by mixing a monomer that forms a repeating unit having a group represented by the above-mentioned formula (1) or (2), a monomer that forms a repeating unit having the above-mentioned photoreactive group, and a monomer that forms any other repeating unit, and polymerizing the mixture in an organic solvent using a radical polymerization initiator.

[0110] The weight average molecular weight (Mw) of the photoalignment polymer of the present invention is not particularly limited, but is preferably 25,000 or more, more preferably 25,000 to 500,000, even more preferably 25,000 to 300,000, and particularly preferably 30,000 to 150,000, in order to improve the liquid crystal alignment property of the optically anisotropic layer formed on the upper layer. Here, the weight average molecular weight of the photoalignable polymer and the surfactant described below is a value measured by gel permeation chromatography (GPC) under the following conditions. Solvent (eluent): THF (tetrahydrofuran) ·Device name: TOSOH HLC-8320GPC Column: TOSOH TSKgel Super HZM-H (4.6mm x 15cm ) for use with three connected Column temperature: 40℃ Sample concentration: 0.1% by mass ·Flow rate: 1.0ml / min Calibration curve: TOSOH TSK standard polystyrene Calibration curve using 7 samples with Mw = 2,800,000 to 1,050 (Mw / Mn = 1.03 to 1.06)

[0111] (substrate) As described later, when forming an optically anisotropic layer, it is preferable to form the optically anisotropic layer on a substrate. The substrate is a plate that supports the optically anisotropic layer. The substrate is preferably a transparent substrate. Note that the transparent substrate refers to a substrate having a visible light transmittance of 60% or more, preferably 80% or more, and more preferably 90% or more.

[0112] The retardation value (Rth(550)) in the thickness direction of the substrate at a wavelength of 550 nm is not particularly limited, but is preferably −110 to 110 nm, more preferably −80 to 80 nm. The in-plane retardation value (Re(550)) of the substrate at a wavelength of 550 nm is not particularly limited, but is preferably 0 to 50 nm, more preferably 0 to 30 nm, and further preferably 0 to 10 nm.

[0113] The material for forming the substrate is preferably a polymer having excellent optical properties such as transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy. Examples of polymer films that can be used as the substrate include cellulose acylate films (e.g., cellulose triacetate film (refractive index 1.48), cellulose diacetate film, cellulose acetate butyrate film, and cellulose acetate propionate film), polyolefin films such as polyethylene and polypropylene, polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyethersulfone films, polyacrylic films such as polymethyl methacrylate, polyurethane films, polycarbonate films, polysulfone films, polyether films, polymethylpentene films, polyether ketone films, (meth)acrylonitrile films, and films of polymers having an alicyclic structure (norbornene-based resins (Arton: product name, manufactured by JSR Corporation, and amorphous polyolefins (Zeonex: product name, manufactured by Zeon Corporation)). Among these, the material for the polymer film is preferably triacetyl cellulose, polyethylene terephthalate, or a polymer having an alicyclic structure, and more preferably triacetyl cellulose.

[0114] The substrate may contain various additives (for example, an optical anisotropy adjusting agent, a wavelength dispersion adjusting agent, fine particles, a plasticizer, an ultraviolet protection agent, a deterioration inhibitor, a release agent, etc.).

[0115] The thickness of the substrate is not particularly limited, but is preferably 10 to 200 μm, more preferably 10 to 100 μm, and even more preferably 20 to 90 μm. The substrate may be made of a laminate of multiple sheets. In order to improve adhesion with a layer provided thereon, the surface of the substrate may be subjected to a surface treatment (e.g., glow discharge treatment, corona discharge treatment, ultraviolet (UV) treatment, flame treatment). In addition, an adhesive layer (undercoat layer) may be provided on the substrate. In addition, in order to impart slipperiness to the substrate during the transport process and to prevent sticking between the front and back surfaces after winding, a polymer layer containing inorganic particles having an average particle size of about 10 to 100 nm at a solid content ratio of 5 to 40 mass % may be placed on one side of the substrate.

[0116] The substrate may be a so-called temporary support, that is, the substrate may be peeled off from the optically anisotropic layer after carrying out the production method of the present invention.

[0117] In addition, the surface of the substrate may be directly subjected to rubbing treatment. In other words, a substrate that has been subjected to rubbing treatment may be used. The direction of the rubbing treatment is not particularly limited, and an optimal direction is appropriately selected depending on the direction in which the liquid crystal compound is desired to be aligned. The rubbing treatment can be a treatment method that is widely used as a liquid crystal alignment treatment process for LCDs (liquid crystal displays), in which the surface of the substrate is rubbed in a certain direction with paper, gauze, felt, rubber, nylon fiber, polyester fiber, or the like to obtain alignment.

[0118] An alignment film may be disposed on the substrate. The alignment layer can be formed by such means as rubbing an organic compound (preferably a polymer), oblique deposition of an inorganic compound, formation of a layer with microgrooves, or deposition of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearate) by the Langmuir-Blodgett technique (LB film). Furthermore, an alignment film is also known that exhibits an alignment function when an electric field is applied, a magnetic field is applied, or light (preferably polarized light) is irradiated.

[0119] The procedure for forming the optically anisotropic layer is not particularly limited, and examples thereof include a method of applying a polymerizable liquid crystal composition containing the liquid crystal compound having the above-mentioned polymerizable group onto a substrate, and performing a drying treatment as necessary (hereinafter, also simply referred to as a "coating method"); and a method of forming an optically anisotropic layer separately and transferring it onto a substrate. Among them, the coating method is preferred from the viewpoint of productivity. The coating method will be described in detail below.

[0120] The coating method is not particularly limited, and examples thereof include wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, and die coating. If necessary, after the application of the composition, a treatment for drying the coating film applied onto the substrate may be carried out. By carrying out the drying treatment, the solvent can be removed from the coating film.

[0121] The thickness of the coating film is not particularly limited, but is preferably 0.1 to 20 μm, more preferably 0.2 to 15 μm, and even more preferably 0.5 to 10 μm.

[0122] Next, the formed coating film is subjected to an alignment treatment to align the polymerizable liquid crystal compound in the coating film. The alignment treatment can be carried out by drying the coating film at room temperature or by heating the coating film. In the case of a thermotropic liquid crystal compound, the liquid crystal phase formed by the alignment treatment can generally be transitioned by a change in temperature or pressure. In the case of a lyotropic liquid crystal compound, the transition can also be caused by a composition ratio such as the amount of solvent. The conditions for heating the coating are not particularly limited, but the heating temperature is preferably 50 to 250° C., more preferably 50 to 150° C., and the heating time is preferably 10 seconds to 10 minutes. After heating the coating film, the coating film may be cooled, if necessary, before the curing treatment (light irradiation treatment) described below. The cooling temperature is preferably 20 to 200°C, and more preferably 30 to 150°C.

[0123] Next, the coating film in which the polymerizable liquid crystal compound is aligned is subjected to a curing treatment. The method of hardening treatment performed on the coating film in which the polymerizable liquid crystal compound is oriented is not particularly limited, and examples thereof include light irradiation treatment and heat treatment. Among them, from the viewpoint of manufacturability, light irradiation treatment is preferred, and ultraviolet irradiation treatment is more preferred. The irradiation conditions for the light irradiation treatment are not particularly limited, but are preferably 50 to 1000 mJ / cm 2 is preferred. The atmosphere during the light irradiation treatment is not particularly limited, but a nitrogen atmosphere is preferred.

[0124] In addition, when the optically anisotropic layer (C) contains the above-mentioned photo-alignable polymer, it is preferable to subject the surface of the optically anisotropic layer (C) that comes into contact with the optically anisotropic layer (A) or the optically anisotropic layer (B) to a photo-alignment treatment before coming into contact with the optically anisotropic layer (A) or the optically anisotropic layer (B) in order to impart alignment control ability. Examples of photoalignment treatment include a method in which a coating film of the polymerizable liquid crystal composition (including a cured film that has been subjected to a curing treatment) is irradiated with polarized light, or a method in which the coating film surface is irradiated with unpolarized light from an oblique direction.

[0125] In the photo-alignment treatment, the polarized light to be irradiated is not particularly limited. For example, linearly polarized light, circularly polarized light, and elliptically polarized light are included, with linearly polarized light being preferred. Furthermore, the "oblique direction" in which unpolarized light is irradiated is not particularly limited as long as it is a direction inclined at a polar angle θ (0<θ<90°) with respect to the normal direction to the coating surface, and can be appropriately selected depending on the purpose, with θ being preferably from 20 to 80°.

[0126] The wavelength of the polarized or unpolarized light is not particularly limited as long as it is light to which the photo-alignable group is sensitive, and examples thereof include ultraviolet light, near ultraviolet light, and visible light, with near ultraviolet light of 250 to 450 nm being preferred. Examples of light sources for irradiating polarized or non-polarized light include xenon lamps, high-pressure mercury lamps, extra-high-pressure mercury lamps, and metal halide lamps. By using an interference filter or a color filter on the ultraviolet or visible light obtained from such light sources, the wavelength range of the light to be irradiated can be limited. By using a polarizing filter or a polarizing prism on the light from these light sources, linearly polarized light can be obtained.

[0127] The integrated amount of polarized or unpolarized light is not particularly limited and may be 1 to 300 mJ / cm2 is preferable, and 5 to 100 mJ / cm 2 is more preferred. The illuminance of polarized or unpolarized light is not particularly limited and may be 0.1 to 300 mW / cm 2 is preferable, and 1 to 100 mW / cm 2 is more preferred.

[0128] Furthermore, with regard to the optically anisotropic layer (C), when the photoalignable polymer contained in the polymerizable liquid crystal composition is the above-mentioned cleavage-type photoalignable polymer, it is preferable to carry out a light irradiation treatment before carrying out the above-mentioned photoalignment treatment, from the viewpoint of proceeding with cleavage at the cleavage group and eliminating the group containing a fluorine atom or a silicon atom. The light irradiation treatment may be any treatment to which the photoacid generator is photosensitive, and may be, for example, a method of irradiating ultraviolet light. As a light source, a lamp that emits ultraviolet light, such as a high-pressure mercury lamp or a metal halide lamp, may be used. The irradiation dose is 10 mJ / cm. 2 ~50J / cm 2 is preferred, and 20 mJ / cm 2 ~5J / cm 2 More preferably, 30 mJ / cm 2 ~3J / cm 2 More preferably, 50 to 1000 mJ / cm 2 is particularly preferred. The light irradiation treatment may be carried out after the above-mentioned curing treatment, or may be carried out simultaneously with the above-mentioned curing treatment.

[0129] [Circular polarizing plate] The circular polarizing plate of the present invention has the above-mentioned optical film of the present invention and a polarizer, and the polarizer is disposed adjacent to the optically anisotropic layer (A) of the optical film. In other words, the circular polarizing plate of the present invention is a circular polarizing plate in which the optically anisotropic layer (A) is disposed closer to the polarizer than the optically anisotropic layer (B) and the optically anisotropic layer (C). As one embodiment of the circular polarizing plate, as shown in Fig. 3, a circular polarizing plate 30 of the present invention includes a polarizer 3 and an optical film 10. The polarizer 3 is disposed on the side of the optical film 10 opposite to the optically anisotropic layer 1c side. As a different embodiment, as shown in Fig. 4, a circular polarizing plate 40 of the present invention includes a polarizer 3 and an optical film 20. The polarizer 3 is disposed on the side of the optical film 20 opposite to the optically anisotropic layer 2b side. The absorption axis of the polarizer is preferably parallel to the longitudinal direction of the long optical film, that is, the angle between the absorption axis of the polarizer and the longitudinal direction of the long optical film is preferably 0 to 10°. In the first embodiment, the angle between the in-plane slow axis of the optically anisotropic layer (A) and the absorption axis of the polarizer is preferably 40 to 85°, more preferably 50 to 85°, and even more preferably 65 to 85°. In the second embodiment, the angle between the in-plane slow axis of the optically anisotropic layer (A) and the absorption axis of the polarizer is preferably 5 to 50°, more preferably 5 to 40°, and even more preferably 5 to 25°. As described above, the absorption axis of the polarizer is usually likely to be located in the longitudinal direction, and therefore, when the polarizer and the long optical film are laminated together so that the absorption axis of the polarizer and the longitudinal direction of the long optical film are parallel to each other, the polarizer and the long optical film are laminated together continuously by roll-to-roll lamination so that the longitudinal directions of the polarizer and the long optical film are aligned, thereby making it possible to produce a desired circularly polarizing plate.

[0130] The polarizer may be any member capable of converting natural light into a specific linearly polarized light, and an example of the polarizer is an absorptive polarizer. The type of polarizer is not particularly limited, and any commonly used polarizer can be used, such as an iodine-based polarizer, a dye-based polarizer using a dichroic dye, and a polyene-based polarizer. Iodine-based polarizers and dye-based polarizers are generally produced by adsorbing iodine or a dichroic dye to polyvinyl alcohol and stretching it. A protective film may be disposed on one or both sides of the polarizer.

[0131] In addition, as described in WO 2019 / 131943 and JP 2017-83843 A, a coating-type polarizer produced by coating a liquid crystal compound and a dichroic organic dye (for example, a dichroic azo dye used in the light-absorbing anisotropic film described in WO 2017 / 195833 A) without using polyvinyl alcohol as a binder may be used as the polarizer. In other words, the polarizer may be a polarizer formed using a composition containing a polymerizable liquid crystal compound. This coating type polarizer is a technology that utilizes the orientation of a liquid crystal compound to orient a dichroic organic dye. As described in JP 2012-83734 A, it is preferable for the polymerizable liquid crystal compound to exhibit smectic properties in terms of increasing the degree of orientation. Alternatively, as described in WO 2018 / 186503 A, it is also preferable to crystallize the dye in terms of increasing the degree of orientation. WO 2019 / 131943 A describes a structure of a polymer liquid crystal that is preferable for increasing the degree of orientation.

[0132] A polarizer in which a dichroic organic dye is oriented by utilizing the orientation of liquid crystals without stretching has the following characteristics: It has many advantages, such as the ability to make the layer extremely thin, at around 0.1 μm to 5 μm, the fact that cracks are unlikely to occur when the layer is bent and thermal deformation is small, as described in JP 2019-194685 A, and the fact that polarizers with high transmittance exceeding 50% have excellent durability, even in such polarizing plates, as described in JP 6483486 A. Taking advantage of these advantages, the film can be used in applications requiring high brightness, small size and light weight, fine optical systems, molding onto curved surfaces, and flexible surfaces. Of course, the film can also be used by peeling off the support and transferring the polarizer thereto.

[0133] From the viewpoint of power saving, the transmittance of the polarizer is preferably a luminosity-corrected single transmittance of 40% or more, more preferably 44% or more, and even more preferably 50% or more. In the present invention, the luminosity-corrected single transmittance of the polarizer is measured using an automatic polarizing film measuring device: VAP-7070 (manufactured by JASCO Corporation). The luminosity-corrected single transmittance can be measured as follows. A sample (5 cm x 5 cm) is prepared by attaching a polarizer to glass via an adhesive. At this time, a polarizing plate protective film is attached to the polarizer so that it is on the side opposite the glass (air interface). The glass side of this sample is set facing the light source and measured.

[0134] The method for producing the circularly polarizing plate is not particularly limited, and any known method can be used. For example, the optical film and the polarizer may be bonded to each other via an adhesive layer.

[0135] [Organic EL display device] The organic EL display device of the present invention has the above-mentioned optical film (or circular polarizer). Usually, the circular polarizer is provided on an organic EL display panel of the organic EL display device. That is, the organic EL display device of the present invention has an organic EL display panel and the above-mentioned circular polarizer. An example of an organic EL display device includes an organic EL display panel, an optical film, and a polarizer in this order.

[0136] An organic EL display panel is a member in which a light-emitting layer or a plurality of organic compound thin films including a light-emitting layer are formed between a pair of electrodes, an anode and a cathode, and may have a hole injection layer, a hole transport layer, an electron injection layer, an electron transport layer, a protective layer, etc. in addition to the light-emitting layer, and each of these layers may have other functions. Various materials can be used to form each layer.

[0137] [Application] The above-mentioned optical film can be used as a polarizing element (polarizing plate) in various articles having a curved surface. For example, it can be used in rollable displays, in-vehicle displays, sunglasses lenses, goggle lenses for image display devices, etc. having a curved surface. The optical film or circular polarizing plate in this embodiment can be attached to a curved surface or integrally molded with a resin, which contributes to improving design. It is also preferable to use the optical system for in-vehicle displays such as head-up displays, optical systems such as AR (augmented reality) glasses and VR (virtual reality) glasses, and optical sensors such as LiDAR (Light Detection and Ranging), face recognition systems, and polarization imaging for the purpose of suppressing stray light. EXAMPLES

[0138] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts, ratios, processing contents, and processing procedures shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0139] [Example 1] <Preparation of cellulose acylate film (substrate)> The following composition was put into a mixing tank, stirred, and heated at 90°C for 10 minutes. The obtained composition was then filtered through a filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a dope. The solid content concentration of the dope was 23.5% by mass, the amount of the plasticizer added was the ratio relative to the cellulose acylate, and the solvent of the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (mass ratio).

[0140] ------------------------------------------------------------------ Cellulose Acylate Dope ------------------------------------------------------------------ Cellulose acylate (acetyl substitution degree 2.86, viscosity average polymerization degree 310) 100 parts by mass Sugar ester compound 1 (shown in the following formula (S4)) 6.0 parts by mass Sugar ester compound 2 (shown in the following formula (S5)) 2.0 parts by mass Silica particle dispersion (AEROSIL R972, Nippon Aerosil Co., Ltd.) 0.1 part by mass Solvent (methylene chloride / methanol / butanol) ------------------------------------------------------------------

[0141] [ka]

[0142] [ka]

[0143] The dope prepared above was cast using a drum film-forming machine. The dope was cast from a die onto a metal support cooled to 0° C., and then the obtained web (film) was peeled off. The drum was made of SUS.

[0144] The web (film) obtained by casting was peeled off from the drum, and then dried for 20 minutes in a tenter apparatus, which clips both ends of the web with clips and transports the web at 30 to 40°C during film transport. The web was then post-dried by zone heating while being transported by rolls. The obtained web was knurled and then wound up. The obtained cellulose acylate film had a thickness of 40 μm, an in-plane retardation Re(550) at a wavelength of 550 nm of 1 nm, and a retardation in the thickness direction Rth(550) at a wavelength of 550 nm of 26 nm. (Alkaline saponification treatment) The above-mentioned cellulose acylate film was passed through a dielectric heating roll at a temperature of 60°C to raise the film surface temperature to 40°C, and then an alkaline solution having the composition shown below was applied to the band surface of the film using a bar coater in an amount of 14 ml / m 2 The plate was then conveyed for 10 seconds under a steam-type far-infrared heater manufactured by Noritake Co., Ltd., which had been heated to 110°C. Next, pure water was applied at a rate of 3 ml / m using the same bar coater. 2 Next, the film was washed with water using a fountain coater and then dried with an air knife three times, and then conveyed to a drying zone at 70° C. for 10 seconds to prepare an alkali saponified cellulose acylate film.

[0145] ---------------------------------------------------------------------------------- Alkaline solution ---------------------------------------------------------------------------------- Potassium hydroxide 4.7 parts by mass Water 15.8 parts by mass Isopropanol 63.7 parts by weight Surfactant: C 14 H 29 O(CH2CH2O) 20 H 1.0 parts by mass Propylene glycol 14.8 parts by weight ----------------------------------------------------------------------------------

[0146] <Formation of alignment film> An alignment layer coating solution having the following composition was continuously coated on the alkaline saponified surface of the cellulose acylate film using a wire bar #14, and then dried with hot air at 60° C. for 60 seconds and then with hot air at 100° C. for 120 seconds.

[0147] ---------------------------------------------------------------------------------- Alignment film coating solution ---------------------------------------------------------------------------------- 10 parts by weight of the following polyvinyl alcohol Water 371 parts by mass Methanol 119 parts by weight Glutaraldehyde (crosslinking agent) 0.5 parts by weight Citric acid ester (manufactured by Sankyo Chemical Co., Ltd.) 0.175 parts by mass ----------------------------------------------------------------------------------

[0148] Polyvinyl alcohol [ka]

[0149] <Formation of Optically Anisotropic Layer (A)> The above-prepared alignment film was subjected to continuous rubbing treatment. At this time, the longitudinal direction of the long film was parallel to the transport direction, and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was 76°. The longitudinal direction of the film (transport direction) was set to 90°, and when observed from the film side, the film width direction was taken as the reference (0°) and the clockwise direction was expressed as a positive value, so the rotation axis of the rubbing roller was at -14°. In other words, the position of the rotation axis of the rubbing roller was rotated 76° clockwise with the longitudinal direction of the film as the reference.

[0150] On the above-mentioned rubbed alignment film, an optically anisotropic layer coating solution (1a) containing a discotic liquid crystal compound of the following composition was applied using a Giesser coater to form a composition layer. The obtained composition layer was then heated with hot air at 110°C for 2 minutes to dry the solvent and ripen the alignment of the discotic liquid crystal compound. The obtained composition layer was then irradiated with UV light (500 mJ / cm2) at 80°C. 2 ) was carried out to fix the alignment of the liquid crystal compound, thereby forming an optically anisotropic layer (1a) corresponding to the optically anisotropic layer (A). The thickness of the optically anisotropic layer (1a) was 1.1 μm. The retardation at 550 nm was 168 nm. The average inclination angle of the discotic surface of the discotic liquid crystal compound with respect to the film surface was 90°, and it was confirmed that the compound was aligned perpendicular to the film surface. The angle of the slow axis of the optically anisotropic layer (1a) was parallel to the rotation axis of the rubbing roller, and the slow axis was -14° when viewed from the optically anisotropic layer (1a) side, assuming that the width direction of the film is 0° (the longitudinal direction is 90° counterclockwise and -90° clockwise).

[0151] ---------------------------------------------------------------------------------- Composition for forming optically anisotropic layer (1a) ---------------------------------------------------------------------------------- 80 parts by weight of the following discotic liquid crystal compound 1 20 parts by weight of the following discotic liquid crystal compound 2 0.55 parts by weight of the following alignment film interface alignment agent 1 0.1 parts by mass of the following fluorine-containing compound A 0.05 parts by mass of the following fluorine-containing compound B 0.21 parts by mass of the following fluorine-containing compound C Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 10 parts by mass Photopolymerization initiator (Irgacure 907, manufactured by BASF) 3.0 parts by mass Methyl ethyl ketone 200 parts by mass ----------------------------------------------------------------------------------

[0152] Discotic Liquid Crystal Compound 1 [ka]

[0153] Discotic Liquid Crystal Compound 2 [ka]

[0154] Alignment film interface alignment agent 1 [ka]

[0155] Fluorine-containing compound A (in the following formula, a and b represent the content (mass%) of each repeating unit relative to all repeating units, where a represents 90 mass% and b represents 10 mass%). [ka]

[0156] Fluorine-containing compound B (the numerical value in each repeating unit indicates the content (mass%) relative to all repeating units, the content of the repeating unit on the left side was 32.5 mass%, and the content of the repeating unit on the right side was 67.5 mass%). [ka]

[0157] Fluorine-containing compound C (the numerical value in each repeating unit indicates the content (mass%) relative to all repeating units, the content of the repeating unit on the left was 25 mass%, the content of the repeating unit in the middle was 25 mass%, and the content of the repeating unit on the right was 50 mass%). [ka]

[0158] <Formation of a laminate of the optically anisotropic layer (C) and the optically anisotropic layer (B)> (Formation of Optically Anisotropic Layer (1c)) On the cellulose acylate film prepared above, the optically anisotropic layer coating solution (1c) containing the rod-shaped liquid crystal compound of the following composition was applied using a Giesser coater to form a composition layer. Then, both ends of the film were held, a cooling plate (9°C) was placed on the side of the film on which the coating film was formed so as to be 5 mm away from the film, and a heater (75°C) was placed on the side opposite to the side on which the coating film was formed so as to be 5 mm away from the film, and the film was dried for 2 minutes. Next, the sample was heated to 60°C for 1 minute with hot air, and then irradiated with a 365 nm UV-LED at a dose of 100 mJ / cm while purging with nitrogen to keep the oxygen concentration in the atmosphere at 100 ppm or less. 2 After that, it was annealed with hot air at 120°C for 1 minute to form a precursor layer. The obtained precursor layer was irradiated with UV light (ultra-high pressure mercury lamp; UL750; manufactured by HOYA) at room temperature through a wire grid polarizer at 7.9 mJ / cm. 2 By irradiating the film with light (wavelength: 313 nm), a composition layer having an alignment control ability was formed on the surface. The thickness of the composition layer formed was 0.5 μm. The in-plane retardation Re at a wavelength of 550 nm was 0 nm, and the retardation Rth in the thickness direction at a wavelength of 550 nm was −68 nm. The average tilt angle of the long axis direction of the rod-like liquid crystal compound with respect to the film surface was 90°, and it was confirmed that the compound was aligned perpendicular to the film surface. In this manner, an optically anisotropic layer (1c) corresponding to the optically anisotropic layer (C) was formed.

[0159] ---------------------------------------------------------------------------------- Composition for forming optically anisotropic layer (1c) ---------------------------------------------------------------------------------- 100 parts by weight of the following rod-shaped liquid crystal compound (A) Polymerizable monomer (A-400, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4.0 parts by mass 5.0 parts by mass of the following polymerization initiator S-1 (oxime type) 3.0 parts by weight of the following photoacid generator D-1 2.0 parts by weight of the following polymer M-1 2.0 parts by weight of the vertical alignment agent S01 listed below 2.0 parts by mass of the photo-alignable polymer A-1 shown below 0.2 parts by weight of the following surfactant B-1 Methyl ethyl ketone 42.3 parts by mass Methyl isobutyl ketone 627.5 parts by mass ----------------------------------------------------------------------------------

[0160] Rod-shaped liquid crystal compound (A) (hereinafter, a mixture of compounds) [ka]

[0161] Polymerization initiator S-1 [ka]

[0162] Photoacid generator D-1 [ka]

[0163] Polymer M-1 [ka]

[0164] Vertical alignment agent S01 [ka]

[0165] Photoalignable polymer A-1 (the numerical value in each repeating unit indicates the content (mass%) of each repeating unit relative to the total repeating units, and the repeating units from the left were 43 mass%, 27 mass%, and 30 mass%. The weight average molecular weight was 69,800.) [ka]

[0166] Surfactant B-1 (weight average molecular weight was 2200) [ka]

[0167] (Formation of Optically Anisotropic Layer (1b)) Next, the optically anisotropic layer coating solution (1b) containing a rod-shaped liquid crystal compound having the following composition was applied onto the optically anisotropic layer (1c) prepared above using a Giesser coater, and heated with hot air at 80°C for 60 seconds. Next, the obtained composition layer was irradiated with UV light (500 mJ / cm2) at 80°C. 2 ) was carried out to fix the alignment of the liquid crystal compound, thereby forming an optically anisotropic layer (1b) corresponding to the optically anisotropic layer (B). The optically anisotropic layer (1b) had a thickness of 1.2 μm, a Δnd at a wavelength of 550 nm of 164 nm, and a twist angle of the liquid crystal compound of 81°. When viewed from the optically anisotropic layer (1b) side, assuming that the width direction of the film is 0° (the longitudinal direction is 90°), the alignment axis angle of the liquid crystal compound was 14° on the air side and 95° on the side in contact with the optically anisotropic layer (1c). The alignment axis angle of the liquid crystal compound contained in the optically anisotropic layer is expressed as negative when clockwise (right-handed) and positive when counterclockwise (left-handed), with the width direction of the substrate being taken as the reference 0°, when observing the substrate from the surface side of the optically anisotropic layer. In addition, the twist angle of the liquid crystal compound is expressed by observing the substrate from the surface side of the optically anisotropic layer, and taking the orientation axis direction of the liquid crystal compound on the surface side (front side) as the reference, when the orientation axis direction of the liquid crystal compound on the substrate side (rear side) is clockwise (right-handed), it is negative, and when it is counterclockwise (left-handed), it is positive.

[0168] ---------------------------------------------------------------------------------- Composition for forming optically anisotropic layer (1b) ---------------------------------------------------------------------------------- The above rod-shaped liquid crystal compound (A) 100 parts by mass Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by weight 0.60 parts by mass of the following left-twisted chiral agent (L1) 0.08 parts by mass of the above fluorine-containing compound C Methyl ethyl ketone 156 parts by mass ----------------------------------------------------------------------------------

[0169] Left-twisted chiral agent (L1) [ka]

[0170] By the above procedure, a laminate (1c-1b) was prepared in which the optically anisotropic layer (1c) and the optically anisotropic layer (1b) were directly laminated on a long cellulose acylate film. When the surface of the optically anisotropic layer (1c) in contact with the optically anisotropic layer (1b) was confirmed by the above method, the presence of a photoalignable polymer was confirmed.

[0171] <Formation of a laminate of optically anisotropic layer (A), optically anisotropic layer (B) and optically anisotropic layer (C)> The surface side of the optically anisotropic layer (1a) formed on the long-length cellulose acylate film prepared above and the surface side of the optically anisotropic layer (1b) of the laminate (1c-1b) formed on the long-length cellulose acylate film prepared above were bonded to a continuous machine using an ultraviolet-curing adhesive. Then, the cellulose acylate film on the optically anisotropic layer (1a) side was peeled off to expose the surface of the optically anisotropic layer (1a) that had been in contact with the cellulose acylate film. In this manner, an optical film (1c-1b-1a) was obtained in which the optically anisotropic layer (1c), the optically anisotropic layer (1b), and the optically anisotropic layer (1a) were laminated in this order on the long cellulose acylate film.

[0172] <Preparation of Linear Polarizing Plate 1> The surface of the support of cellulose triacetate film TJ25 (manufactured by Fujifilm Corporation: thickness 25 μm) was subjected to an alkali saponification treatment. Specifically, the support was immersed in a 1.5N sodium hydroxide aqueous solution at 55° C. for 2 minutes, then washed in a water washing bath at room temperature, and further neutralized with 0.1N sulfuric acid at 30° C. After neutralization, the support was washed in a water washing bath at room temperature, and further dried with hot air at 100° C. to obtain a polarizer protective film. A rolled polyvinyl alcohol (PVA) film with a thickness of 60 μm was continuously stretched in the longitudinal direction in an iodine aqueous solution and dried to obtain a polarizer with a thickness of 13 μm. The luminous efficiency corrected single transmittance of the polarizer was 43%. At this time, the absorption axis direction of the polarizer coincided with the longitudinal direction. The above polarizer protective film was attached to one surface of the above polarizer using the following PVA adhesive to prepare a linear polarizing plate 1.

[0173] (Preparation of PVA adhesive) A PVA adhesive was prepared by dissolving 100 parts by mass of a polyvinyl alcohol resin having acetoacetyl groups (average degree of polymerization: 1200, degree of saponification: 98.5 mol%, degree of acetoacetylation: 5 mol%) and 20 parts by mass of methylol melamine in pure water at a temperature of 30°C to prepare an aqueous solution with a solids concentration of 3.7% by mass.

[0174] <Preparation of circular polarizing plate> The surface of the optically anisotropic layer (1a) of the long optical film (1c-1b-1a) prepared above and the surface of the polarizer of the long linear polarizing plate prepared above (the surface opposite to the polarizer protective film) were continuously bonded together using an ultraviolet-curing adhesive. Then, the cellulose acylate film on the optically anisotropic layer (1c) side was peeled off to expose the surface of the optically anisotropic layer (1c) that had been in contact with the cellulose acylate film. In this way, a circular polarizing plate (P1) consisting of the optical film (1c-1b-1a) and the linear polarizing plate was produced. At this time, the polarizer protective film, the polarizer, the optically anisotropic layer (1a), the optically anisotropic layer (1b) and the optically anisotropic layer (1c) were laminated in this order, and the angle between the absorption axis of the polarizer and the slow axis of the optically anisotropic layer (1a) was 76°. In addition, the alignment axis angle of the liquid crystal compound on the optically anisotropic layer (1a) side of the optically anisotropic layer (1b) was 14°, which coincided with the slow axis direction of the optically anisotropic layer (1a), with the width direction being taken as 0° as the reference.

[0175] [Example 2] <Formation of alignment film> The photoalignment film-forming material described in Example 1 of WO2016 / 002722 was applied onto the long cellulose acylate film prepared above. The coating was then heated to 125° C. with hot air to harden it. Then, it was irradiated with polarized ultraviolet light of 313 nm.

[0176] <Formation of Optically Anisotropic Layer (B)> On the photo-alignment film prepared above, the optically anisotropic layer coating solution (1b) containing the rod-shaped liquid crystal compound having the above composition was applied using a Giesser coater, and heated with hot air at 80° C. for 60 seconds. Subsequently, the obtained composition layer was irradiated with UV (500 mJ / cm 2 ) at 80° C. 2 ) was carried out to fix the alignment of the liquid crystal compound, thereby forming an optically anisotropic layer (2b) corresponding to the optically anisotropic layer (B). The optically anisotropic layer (2b) had a thickness of 1.2 μm, a Δnd at a wavelength of 550 nm of 164 nm, and a twist angle of the liquid crystal compound of 81°. When viewed from the optically anisotropic layer (2b) side, assuming that the width direction of the film is 0° (the longitudinal direction is 90°), the alignment axis angle of the liquid crystal compound was −76° on the air side and 5° on the side in contact with the cellulose acylate film. The alignment axis angle of the liquid crystal compound contained in the optically anisotropic layer is expressed as negative when clockwise (right-handed) and positive when counterclockwise (left-handed), with the width direction of the substrate being taken as the reference 0°, when observing the substrate from the surface side of the optically anisotropic layer. In addition, the twist angle of the liquid crystal compound is expressed by observing the substrate from the surface side of the optically anisotropic layer, and taking the orientation axis direction of the liquid crystal compound on the surface side (front side) as the reference, when the orientation axis direction of the liquid crystal compound on the substrate side (rear side) is clockwise (right-handed), it is negative, and when it is counterclockwise (left-handed), it is positive.

[0177] <Formation of Laminate of Optically Anisotropic Layer (C) and Optically Anisotropic Layer (A)> (Formation of Optically Anisotropic Layer (2c)) A composition layer having an alignment control ability on its surface was formed in the same manner as in the formation of the optically anisotropic layer (1c) of Example 1, except that the thickness of the composition layer was changed. The film thickness of the composition layer formed was 0.7 μm. The in-plane retardation Re at a wavelength of 550 nm was 0 nm, and the retardation Rth in the thickness direction at a wavelength of 550 nm was −96 nm. The average tilt angle of the long axis direction of the rod-like liquid crystal compound with respect to the film surface was 90°, and it was confirmed that the compound was aligned perpendicular to the film surface. In this manner, an optically anisotropic layer (2c) corresponding to the optically anisotropic layer (C) was formed.

[0178] (Formation of Optically Anisotropic Layer (2a)) Next, the optically anisotropic layer coating solution (2a) containing a rod-shaped liquid crystal compound having the following composition was applied onto the optically anisotropic layer (2c) prepared above using a Giesser coater, and heated with hot air at 80°C for 60 seconds. Next, the obtained composition layer was irradiated with UV light (500 mJ / cm2) at 80°C. 2 ) was carried out to fix the alignment of the liquid crystal compound, thereby forming an optically anisotropic layer (2a) corresponding to the optically anisotropic layer (A). The thickness of the optically anisotropic layer (2a) was 1.2 μm. The retardation at 550 nm was 168 nm. The average tilt angle of the long axis direction of the rod-like liquid crystal compound with respect to the film surface was 0°, and it was confirmed that the compound was aligned horizontally with respect to the film surface. When the width direction of the film was 0° (the longitudinal direction was 90°), the slow axis was −76° when viewed from the optically anisotropic layer (2a) side.

[0179] ---------------------------------------------------------------------------------- Composition for forming optically anisotropic layer (2a) ---------------------------------------------------------------------------------- The above rod-shaped liquid crystal compound (A) 100 parts by mass Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by weight 0.08 parts by mass of the above fluorine-containing compound C Methyl ethyl ketone 156 parts by mass ----------------------------------------------------------------------------------

[0180] By the above procedure, a laminate (2c-2a) was prepared in which the optically anisotropic layer (2c) and the optically anisotropic layer (2a) were directly laminated on a long cellulose acylate film. When the surface of the optically anisotropic layer (2c) in contact with the optically anisotropic layer (2a) was confirmed by the above method, the presence of a photoalignable polymer was confirmed.

[0181] <Formation of a Laminate of Optically Anisotropic Layer (A), Optically Anisotropic Layer (C) and Optically Anisotropic Layer (B), and Preparation of a Circularly Polarizing Plate> The surface of the optically anisotropic layer (2a) of the laminate (2c-2a) formed on the long cellulose acylate film prepared above and the surface of the polarizer of the long linear polarizing plate prepared above (the surface opposite to the polarizer protective film) were continuously bonded together using an ultraviolet-curing adhesive. Then, the cellulose acylate film on the optically anisotropic layer (2c) side was peeled off to expose the surface of the optically anisotropic layer (2c) that had been in contact with the cellulose acylate film. The exposed surface of the optically anisotropic layer (2c) and the surface of the optically anisotropic layer (2b) formed on the long cellulose acylate film prepared above were attached to a continuous machine using an ultraviolet-curing adhesive. Then, the cellulose acylate film on the optically anisotropic layer (2b) side was peeled off to expose the surface of the optically anisotropic layer (2b) that had been in contact with the cellulose acylate film. In this way, a circular polarizing plate (P2) consisting of the optical film (2b-2c-2a) and the linear polarizing plate was produced. At this time, the polarizer protective film, the polarizer, the optically anisotropic layer (2a), the optically anisotropic layer (2c) and the optically anisotropic layer (2b) were laminated in this order, and the angle between the absorption axis of the polarizer and the slow axis of the optically anisotropic layer (2a) was 14°. In addition, the alignment axis angle of the liquid crystal compound on the optically anisotropic layer (2c) side of the optically anisotropic layer (2b) was -76°, which coincided with the slow axis direction of the optically anisotropic layer (2a), with the width direction being taken as 0° as the reference.

[0182] [Comparative Example 1] In a manner similar to that described in Example 1 of Japanese Patent No. 5,960,743, an optical film was prepared in which an optically anisotropic layer (ha) consisting of vertically oriented discotic liquid crystals and an optically anisotropic layer (hb) consisting of twistedly oriented discotic liquid crystals were laminated directly in that order on a long cellulose acylate film. In this case, the retardation of the optically anisotropic layer (ha) at a wavelength of 550 nm was 181 nm, and when the width direction of the film was 0° (longitudinal direction was 90°), the slow axis was -13° when viewed from the optically anisotropic layer (ha) side. Also, Δnd of the optically anisotropic layer (hb) at a wavelength of 550 nm was 172 nm, the twist angle of the liquid crystal compound was 81°, and when the width direction of the film was 0° (longitudinal direction was 90°), the alignment axis angle of the liquid crystal compound was -94° on the air side and -13° on the side in contact with the cellulose acylate film when viewed from the optically anisotropic layer (hb) side. The surface of the cellulose acylate film of the laminate (ha-hb) formed on the long cellulose acylate film prepared above and the surface of the polarizer of the long linear polarizing plate prepared above (opposite side of the polarizer protective film) are continuously bonded together using an ultraviolet curing adhesive. In this way, a circular polarizing plate (PH) is prepared.

[0183] [Durability evaluation] In the above-mentioned preparation of the circular polarizing plate, instead of bonding the linear polarizing plate and the optically anisotropic layer with an ultraviolet-curing adhesive, the optically anisotropic layer cut into a 40 mm square was bonded to a glass plate using a pressure-sensitive adhesive. That is, the optical film (1c-1b-1a) or the optical film (2b-2c-2a) was formed on the glass plate. At this time, the optically anisotropic layer (1a) or the optically anisotropic layer (2a) was on the glass plate side. The optical film with the glass plate was placed on a screw-cap bottle containing a 2 mol% / L methanol solution of ammonia, and exposed to ammonia for 60 minutes. At this time, it was placed so that the exposed surface was the optically anisotropic layer (1c) or the optically anisotropic layer (2b). The in-plane retardations Re(450), Re(550) and Re(650) at wavelengths of 450 nm, 550 nm and 650 nm were measured using an Axoscan manufactured by Axometrics. When H=Re(450) / Re(550), H before exposure to ammonia was H0, H after exposure to ammonia was H1, and ΔH(%)=|H1-H0| / H0×100 was used as an index and the evaluation was performed as follows. The results are shown in Table 1. A: ΔH is less than 1% B: ΔH is 1% or more and less than 2% C: ΔH is 2% or more

[0184] <Fabrication of organic EL display device> (Mounting to a display device) A Samsung GALAXY S4 equipped with an organic EL panel was disassembled, the circular polarizing plate was peeled off, and the above-prepared circular polarizing plate was attached to the display device using a pressure-sensitive adhesive so that the polarizer protective film was placed on the outside.

[0185] [Evaluation of display performance] (Front direction) The organic EL display device thus produced was made to display black, and was observed from the front under bright light, and the coloring was evaluated according to the following criteria. The results are shown in Table 1 below. A: No visible coloring or only slight coloring (acceptable). B: Coloring is visible, but the reflected light is small and does not pose a problem in use. (Acceptable) C: Coloring is visible and the reflected light is large, which is unacceptable.

[0186] (Diagonal) The organic EL display device thus fabricated was made to display black, and a fluorescent lamp was projected onto it at a polar angle of 45° under bright light, and the reflected light was observed from all directions. The azimuth angle dependency of the color change was evaluated according to the following criteria. The results are shown in Table 1 below. A: The color difference is not visible at all, or is visible but very slight (acceptable). B: The color difference is visible, but the reflected light is small and does not pose a problem in use. (Acceptable) C: Color difference is visible and reflected light is large, unacceptable.

[0187] [Table 1]

[0188] From the results shown in Table 1, it was confirmed that the optical film of the present invention can suppress black coloring in the front direction and oblique directions when used as a circular polarizer in an organic EL display device. On the other hand, the optical film of the comparative example was inferior in suppressing black coloring in the oblique direction when used as a circular polarizer in an organic EL display device.

[0189] [Example 3] In the same manner as in Example 1, an optical film (1c-1b-1a) was obtained in which an optically anisotropic layer (1c), an optically anisotropic layer (1b) and an optically anisotropic layer (1a) were laminated in this order on a long cellulose acylate film. Next, a polarizing plate SHC-215U manufactured by Polatechno Co., Ltd., in which a polyvinyl alcohol film was dyed with a dichroic organic dye, was prepared as the linear polarizing plate 2. The luminous efficiency corrected single transmittance of the polarizer was 44%. The surface of the optically anisotropic layer (1a) of the long optical film (1c-1b-1a) and the surface of the long linear polarizing plate 2, which had been corona-treated on one side, were continuously bonded together using an ultraviolet-curing adhesive. Then, the cellulose acylate film of the optically anisotropic layer (1c) was peeled off to expose the surface of the optically anisotropic layer (1c) that had been in contact with the cellulose acylate film. In this way, a circular polarizing plate (P3) was produced.

[0190] [Example 4] In the same manner as in Example 1, an optical film (1c-1b-1a) was obtained in which an optically anisotropic layer (1c), an optically anisotropic layer (1b) and an optically anisotropic layer (1a) were laminated in this order on a long cellulose acylate film. Next, as polarizing film 4B, a polarizer using a dichroic organic dye and a polymerizable liquid crystal was prepared by the following procedure. The coating solution PA1 for forming an alignment layer, which will be described later, was continuously applied onto a cellulose triacetate film TJ40 (manufactured by Fujifilm; thickness 40 μm) using a wire bar. The support on which the coating film was formed was dried with hot air at 140° C. for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2 A photo-alignment layer PA1 was formed by irradiating the TAC film with the photo-alignment layer PA1. The thickness of the photo-alignment layer PA1 was 0.3 μm.

[0191] ---------------------------------------------------------------------------------- Coating solution for forming alignment layer PA1 ---------------------------------------------------------------------------------- The following polymer PA-1: 100.00 parts by weight Acid generator PAG-1 (listed below) 5.00 parts by weight 0.005 parts by weight of the acid generator CPI-110TF Xylene 1220.00 parts by mass Methyl isobutyl ketone 122.00 parts by mass ----------------------------------------------------------------------------------

[0192] Polymer PA-1 [ka]

[0193] Acid generator PAG-1 [ka]

[0194] Acid generator CPI-110F [ka]

[0195] On the obtained photoalignment layer PA1, the following composition for forming an optically absorptive anisotropic layer P2 was continuously applied with a wire bar to form a coating film P2. Next, the coating film P2 was heated at 140° C. for 30 seconds, after which the coating film P2 was cooled to room temperature (23° C.). The resulting coating film P2 was then heated at 90° C. for 60 seconds and cooled again to room temperature. Then, an LED (light emitting diode) lamp (center wavelength 365 nm) was used to illuminate the specimen at an intensity of 200 mW / cm 2 An optically absorptive anisotropic layer P2 was formed on the photo-alignment layer PA1 by irradiating the layer for 2 seconds under the irradiation conditions of: The molar content of the radical polymerizable group was 1.17 mmol / g. The optically absorptive anisotropic layer P2 had a thickness of 1.0 μm.

[0196] ---------------------------------------------------------------------------------- Optically absorptive anisotropic layer forming composition P2 ---------------------------------------------------------------------------------- 0.25 parts by weight of the following dichroic dye D-4 0.36 parts by weight of the following dichroic dye D-5 0.59 parts by weight of the following dichroic dye D-6 2.21 parts by weight of the following polymer liquid crystal compound P-1 1.36 parts by weight of the following low molecular weight liquid crystal compound M-1 Polymerization initiator IRGACUREOXE-02 (BASF) 0.150 parts by mass 0.026 parts by weight of the following surfactant F-1 Cyclopentanone 46.00 parts by mass Tetrahydrofuran 46.00 parts by weight Benzyl alcohol 3.00 parts by weight ----------------------------------------------------------------------------------

[0197] Dichroic dye D-4 [ka]

[0198] Dichroic dye D-5 [ka]

[0199] Dichroic dye D-6 [ka]

[0200] Polymer liquid crystal compound P-1 [ka]

[0201] Low molecular liquid crystal compound M-1 [ka]

[0202] Surfactant F-1 [ka]

[0203] Onto the obtained light absorption anisotropic layer P2, the following composition for forming a cured layer K1 was continuously applied with a wire bar to form a coating film. The coating was then dried at room temperature and then irradiated with a high-pressure mercury lamp at an illumination intensity of 28 mW / cm 2 By irradiating for 15 seconds under the irradiation conditions above, a hardened layer K1 was formed on the light absorption anisotropic layer P2. The thickness of the hardened layer K1 was 0.05 μm. ---------------------------------------------------------------------------------- Composition K1 for forming hardened layer ---------------------------------------------------------------------------------- 2.61 parts by weight of the mixture L1 of the following rod-shaped liquid crystal compounds 0.11 parts by weight of the following modified trimethylolpropane triacrylate 0.05 parts by weight of the following photopolymerization initiator I-1 0.21 parts by weight of the following surfactant F-3 Methyl isobutyl ketone 297 parts by weight ----------------------------------------------------------------------------------

[0204] Mixture L1 of rod-shaped liquid crystal compounds (the numerical values ​​in the formula below represent mass %, and R represents a group bonded via an oxygen atom). [ka]

[0205] Modified Trimethylolpropane Triacrylate [ka]

[0206] Photopolymerization initiator I-1 [ka]

[0207] Surfactant F-3 [ka]

[0208] The following oxygen barrier layer-forming composition B2 was continuously applied onto the cured layer K1 with a wire bar, and then dried for 2 minutes with hot air at 100°C to form an oxygen barrier layer B2 with a thickness of 1.0 μm on the cured layer K1, thereby producing a polarizing film 4B including a light absorption anisotropic layer P2. The luminous efficiency corrected single transmittance of polarizing film 4B was 44%. ---------------------------------------------------------------------------------- Composition B2 for forming oxygen barrier layer ---------------------------------------------------------------------------------- 3.80 parts by weight of the following modified polyvinyl alcohol Initiator Irg2959 0.20 parts by weight ·Water 70 parts by mass Methanol 30 parts by weight ----------------------------------------------------------------------------------

[0209] Modified Polyvinyl Alcohol [ka]

[0210] The oxygen barrier layer B2 side of the polarizing film 4B and the polarizing plate protective film were attached using an adhesive sheet. Then, only TJ40 of the polarizing film 4B was peeled off, and the peeled surface was continuously attached to the surface of the optically anisotropic layer (1a) of the long optical film (1c-1b-1a) using an ultraviolet-curing adhesive. Then, the cellulose acylate film of the optically anisotropic layer (1c) was peeled off, and the surface of the optically anisotropic layer (1c) that had been in contact with the cellulose acylate film was exposed. In this way, a circular polarizing plate (P4) was produced.

[0211] [Example 5] A circularly polarizing plate (P5) was produced in the same direction as in Example 4, except that the thickness of the light absorptive anisotropic layer P2 in Example 4 was 0.8 μm. The luminous efficiency corrected single transmittance of the polarizer was 45%.

[0212] [Durability evaluation] The circularly polarizing plates of Examples 1 and 3 to 5 were evaluated for durability under a humid and hot environment. In the preparation of the circularly polarizing plate described above, a glass plate and an optically anisotropic layer cut into a 40 mm square were bonded together using a pressure-sensitive adhesive. That is, an optical film (1c-1b-1a) was formed on the glass plate. At this time, the optically anisotropic layer (1a) was on the glass plate side. The optical film with the glass plate was placed on a screw-cap bottle containing an aqueous ammonia solution of 0.05 mol% / L, and exposed to ammonia for 24 hours. At this time, it was placed so that the exposed surface was the optically anisotropic layer (1c). The difference in effective reflectance before and after the humidity and heat durability test was evaluated according to the following criteria using a spectrophotometer (Konica Minolta) to create a reflective substrate by attaching aluminum foil to a 100μm thick PET film using an adhesive sheet. AA: Reflectance difference is 0.2% or less A: The reflectance difference is greater than 0.2% and less than 0.5%. B: The reflectance difference is greater than 0.5% and less than or equal to 2.0%. C: The reflectance difference is greater than 2.0%

[0213] [Table 2]

[0214] It was also confirmed that when the circularly polarizing plates of Examples 3 to 5 were used as anti-reflection films in organic EL display devices, they exhibited initial performance equivalent to that of Example 1 while also reducing the change in display performance before and after humidity and heat durability. Furthermore, it was confirmed that the circular polarizing plates of Examples 3 and 5 exhibited an increase in transmittance during white display, and were able to achieve power saving in the organic EL element. [Explanation of symbols]

[0215] 10, 20, 101, 102, 201, 202 Optical films 30, 40 Circular polarizer 1a, 2a, 11a, 12a, 21a, 22a optically anisotropic layer (A) 1b, 2b, 11b, 12b, 21b, 22b Optical anisotropic layer (B) 1c, 2c, 11c, 12c, 21c, 22c optically anisotropic layer (C) 3 Polarizer 111a, 112a, 111b, 112b, 121a, 122a, 121b, 122b, 211a, 212a, 211b, 212b, 221a, 222a, 221b, 222b, Surface

Claims

1. A long optical film having an optically anisotropic layer (A), an optically anisotropic layer (B), and an optically anisotropic layer (C) in this order, the optically anisotropic layer (A) is a negative A plate having an in-plane retardation of 140 to 220 nm at a wavelength of 550 nm; the optically anisotropic layer (B) is a layer in which rod-like liquid crystal compounds are fixed and twisted and aligned with a helical axis in the thickness direction, and a product Δnd of a refractive index anisotropy Δn of the optically anisotropic layer (B) measured at a wavelength of 550 nm and a thickness d of the optically anisotropic layer (B) is 140 to 220 nm; the optically anisotropic layer (C) is a layer in which vertically aligned rod-like liquid crystal compounds are fixed, the in-plane retardation of the optically anisotropic layer (C) at a wavelength of 550 nm is 0 to 10 nm, and the retardation in the thickness direction of the optically anisotropic layer (C) at a wavelength of 550 nm is −120 to −20 nm, an in-plane slow axis of the optically anisotropic layer (A) is parallel to an in-plane slow axis of the optically anisotropic layer (B) on the surface thereof facing the optically anisotropic layer (A); When observed from the optically anisotropic layer (C) side toward the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) rotates clockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the optically anisotropic layer (B) on the surface facing the optically anisotropic layer (A) rotates counterclockwise with respect to the in-plane slow axis of the optically anisotropic layer (B) on the surface facing the optically anisotropic layer (A), When observed from the optically anisotropic layer (C) side toward the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (A) side rotates clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (A) side.

2. the angle between the longitudinal direction of the long optical film and the in-plane slow axis of the optically anisotropic layer (A) is 40 to 85°, the twist angle of the twisted liquid crystal compound in the optically anisotropic layer (B) is 90±30°, When observed from the optically anisotropic layer (C) side toward the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) is rotated clockwise by 40 to 85° with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the optically anisotropic layer (B) on the surface on the optically anisotropic layer (A) side is rotated counterclockwise with respect to the in-plane slow axis of the optically anisotropic layer (B) on the optically anisotropic layer (A) side, 2. The optical film according to claim 1, wherein, when observed from the optically anisotropic layer (C) side toward the optically anisotropic layer (A) side, the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise by 40 to 85° with respect to the longitudinal direction of the long optical film, and the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (A) side rotates clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (A) side.

3. A long optical film having an optically anisotropic layer (A), an optically anisotropic layer (C), and an optically anisotropic layer (B) in this order, the optically anisotropic layer (A) is a positive A plate having an in-plane retardation of 140 to 220 nm at a wavelength of 550 nm; the optically anisotropic layer (C) is a layer formed by fixing a vertically aligned rod-like liquid crystal compound, the in-plane retardation of the optically anisotropic layer (C) at a wavelength of 550 nm is 0 to 10 nm, and the retardation in the thickness direction of the optically anisotropic layer (C) at a wavelength of 550 nm is −150 to −50 nm, the optically anisotropic layer (B) is a layer in which rod-like liquid crystal compounds are fixed and twisted and aligned with a helical axis in the thickness direction, and a product Δnd of a refractive index anisotropy Δn of the optically anisotropic layer (B) measured at a wavelength of 550 nm and a thickness d of the optically anisotropic layer (B) is 140 to 220 nm; an in-plane slow axis of the optically anisotropic layer (A) is parallel to an in-plane slow axis of the optically anisotropic layer (B) on the surface facing the optically anisotropic layer (C); When observed from the optically anisotropic layer (B) side toward the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) rotates clockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (C) side rotates clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (C) side, When observed from the optically anisotropic layer (B) side toward the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (C) side rotates counterclockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (C) side.

4. an angle between a longitudinal direction of the long optical film and an in-plane slow axis of the optically anisotropic layer (A) is 5 to 50°; the twist angle of the twisted liquid crystal compound in the optically anisotropic layer (B) is 90±30°, When observed from the optically anisotropic layer (B) side toward the optically anisotropic layer (A) side, when the in-plane slow axis of the optically anisotropic layer (A) is rotated clockwise by 5 to 50° with respect to the longitudinal direction of the long optical film, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (C) side is rotated clockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (C) side, 4. The optical film according to claim 3, wherein, when observed from the optically anisotropic layer (B) side toward the optically anisotropic layer (A) side, with respect to the longitudinal direction of the long optical film, when the in-plane slow axis of the optically anisotropic layer (A) rotates counterclockwise by 5 to 50°, with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (C) side, the in-plane slow axis of the surface of the optically anisotropic layer (B) opposite to the optically anisotropic layer (C) side rotates counterclockwise with respect to the in-plane slow axis of the surface of the optically anisotropic layer (B) on the optically anisotropic layer (C) side.

5. The optical film according to any one of claims 1 to 4 and a polarizer, The circularly polarizing plate comprises the polarizer disposed adjacent to the optically anisotropic layer (A) of the optical film.

6. 6. The circular polarizing plate according to claim 5, wherein the polarizer has a luminous efficiency-corrected single transmittance of 44% or more.

7. The circular polarizing plate according to claim 5 , wherein the polarizer is formed using a composition containing a polymerizable liquid crystal compound.

8. An organic electroluminescence display device comprising the optical film according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Optical element consisting of liquid crystal layer and liquid crystal display device using the same

    JP2004258623A

  • Retardation plate for circularly polarizing plate, circularly polarizing plate, and organic el (electroluminescence) display device

    JP2014209220A

  • Optical film, transfer film, image display device, method for manufacturing optical film, and method for manufacturing transfer film

    JP2016206217A

  • Optical rotatory film

    JP2017102259A

  • Retardation plate for circular polarizer, circular polarizer, organic EL display device

    JP5960743B2