Adhesive composition, adhesive film using the same, surface protective film, optical film with adhesive layer
The adhesive composition for surface protection films, using a specific blend of acrylic polymers and ionic compounds, addresses the challenges of balancing adhesive strength, stain resistance, and antistatic performance, ensuring effective peeling and reducing contamination on optical members.
Patent Information
- Application Number
- JP2024135221
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2038-11-12
AI Technical Summary
Existing adhesive layers for surface protection films in optical members like polarizing plates struggle to balance adhesive strength at low and high peeling speeds, provide stain resistance, and achieve excellent antistatic performance simultaneously, especially with diverse adherend materials and surface treatments.
An adhesive composition comprising an acrylic polymer, a crosslinking agent, and an ionic compound, with specific ratios of alkyl (meth)acrylates, monofunctional methacrylate monomers, and copolymerizable monomers, along with a trifunctional isocyanate crosslinking agent, is used to form an adhesive layer that maintains balanced adhesive strength, stain resistance, and antistatic properties.
The adhesive layer achieves a well-balanced adhesive force at low and high peeling speeds, effective stain resistance, and excellent antistatic performance, ensuring easy peeling and reducing static charge-induced contamination on optical members.
Smart Images

Figure 2024149779000001 
Figure 2024149779000002 
Figure 2024149779000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition that can be suitably used for a surface protection film such as a surface protection film for a polarizing plate, and a pressure-sensitive adhesive film and a surface protection film using the same. More specifically, the present invention relates to a pressure-sensitive adhesive composition that has a balanced adhesive strength at a low peeling speed and a high peeling speed, and is capable of achieving both antistatic performance and anti-staining performance, and a pressure-sensitive adhesive film and a surface protection film using the same. [Background technology]
[0002] Conventionally, in the manufacturing process of optical members such as polarizing plates, which are members constituting liquid crystal displays, a surface protection film is attached to temporarily protect the surface of the optical member. Such a surface protection film is used only in the process of manufacturing the optical member, and is peeled off and removed from the optical member when the optical member is assembled into a liquid crystal display. Since such a surface protection film for protecting the surface of the optical member is used only in the manufacturing process of the optical member, it is also generally called a process film.
[0003] The surface protection film used in the process of producing such an optical member has an adhesive layer formed on one side of an optically transparent polyethylene terephthalate (PET) resin film, and a release film that has been subjected to a release treatment is attached to the surface of the adhesive layer of the surface protection film in order to protect the adhesive layer until it is attached to the optical member. Then, optical members such as polarizing plates, with the surface protection film attached, undergo product inspections involving optical evaluation of the display ability, hue, contrast, inclusion of foreign matter, etc. of the liquid crystal display panel. For this reason, the performance required for the surface protection film is that the pressure-sensitive adhesive layer is free of air bubbles or foreign matter, and that the film is capable of reducing adhesion of low molecular weight components of the pressure-sensitive adhesive composition to the surface of the adherend, i.e., that the film has anti-staining performance. In addition, when peeling a surface protection film from an optical component such as a polarizing plate, there is a concern that the peeling charge generated by static electricity generated when the adhesive layer is peeled off from the adherend may affect the breakdown of the electric control circuit of the liquid crystal display, so the adhesive layer of the surface protection film is required to have excellent antistatic properties. Furthermore, in recent years, in addition to the conventionally used triacetyl cellulose (TAC), materials that are prone to peeling static electricity when the surface protective film of a polarizing plate is peeled off, such as acrylic resins such as polymethyl methacrylate (PMMA), polyester resins such as polyethylene terephthalate (PET), cyclic olefin polymers, polycarbonates, etc., are increasingly being used as protective layers (sometimes called protective films) for the polarizers of polarizing plates. For this reason, there is a demand for the pressure-sensitive adhesive layer for the surface protective film of a polarizing plate to have antistatic properties that are superior to conventional materials. Furthermore, when the surface protection film is finally peeled off from an optical member such as a polarizing plate, it is required that the film can be peeled off quickly, that is, the adhesive strength is required to change little depending on the peeling speed so that the film can be peeled off quickly even when peeled off at high speed.
[0004] Thus, in recent years, the adhesive layer constituting a surface protection film is required to have the following characteristics in terms of ease of use when using the surface protection film: (1) a balance of adhesive strength at both low and high peel speeds, (2) anti-soiling performance, and (3) excellent antistatic performance. However, while it is possible to satisfy each of the required performance items (1) to (3) individually for the pressure-sensitive adhesive layer constituting the surface protection film, it has been an extremely difficult task to simultaneously satisfy all of the required performance items (1) to (3) required for the pressure-sensitive adhesive layer of the surface protection film.
[0005] In order to solve these problems, for example, the following proposals are known with respect to (1) balancing the adhesive strength at low and high peeling speeds, (2) providing stain resistance, and (3) providing excellent antistatic performance.
[0006] (1) Regarding balancing the adhesive strength at low and high peeling speeds, an acrylic adhesive layer made of a copolymer of a (meth)acrylic acid alkyl ester having an alkyl group with 7 or less carbon atoms and a carboxyl group-containing copolymerizable compound, which is crosslinked with a crosslinking agent, has the problem that the adhesive transfers to the adherend when adhered for a long period of time, and the adhesive strength to the adherend increases significantly over time. To avoid this, an adhesive layer with a gel fraction of 60% or more, which uses a copolymer of a (meth)acrylic acid alkyl ester having an alkyl group with 8 to 10 carbon atoms and a copolymerizable compound having an alcoholic hydroxyl group, and which is crosslinked with a crosslinking agent, and a surface protection member provided with the adhesive layer are known (Patent Document 1). However, the pressure-sensitive adhesive layer described in Patent Document 1 has a problem in that it does not completely solve the problem of the adhesive strength to an adherend increasing over time. Also, a copolymer similar to the above is mixed with a small amount of a copolymer of an alkyl (meth)acrylate ester and a copolymerizable compound containing a carboxyl group, and a pressure-sensitive adhesive layer is formed by crosslinking the copolymer with a crosslinking agent. However, when these pressure-sensitive adhesive layers are used for surface protection of a plastic plate or the like having a low surface tension and a smooth surface, there are problems in that peeling phenomena such as lifting occur due to heating during processing or storage, and that the adhesive strength is large at high peeling speeds, which are the range of manual work, resulting in poor removability.
[0007] In order to solve these problems, a pressure-sensitive adhesive composition has been proposed in which a copolymer of a monomer mixture obtained by adding a) 100 parts by weight of a (meth)acrylic acid alkyl ester mainly composed of a (meth)acrylic acid alkyl ester having an alkyl group having 8 to 10 carbon atoms, b) 1 to 15 parts by weight of a carboxyl group-containing copolymerizable compound, and c) 3 to 100 parts by weight of a vinyl ester of an aliphatic carboxylic acid having 1 to 5 carbon atoms, is blended with a crosslinking agent in an amount equivalent to or greater than the amount of the carboxyl group in the above component b) (Patent Document 2). In the adhesive layer obtained by crosslinking the adhesive composition described in Patent Document 2, peeling phenomena such as lifting do not occur during processing or storage, and furthermore, the increase in adhesive strength over time is small, resulting in excellent removability; it can be peeled off with little force even after long-term storage, particularly long-term storage under a high-temperature atmosphere, without leaving any adhesive residue on the adherend, and it can be peeled off with little force even when peeled off at high speed. However, in the pressure-sensitive adhesive layer obtained by crosslinking the pressure-sensitive adhesive composition described in Patent Document 2, the gel fraction of the pressure-sensitive adhesive layer in Examples 1 to 3 was all 90%, and the adhesive strength at a low peeling speed was prone to be excessive, and unpolymerized monomers or oligomers were prone to elution from the pressure-sensitive adhesive layer. Furthermore, Patent Document 2 does not mention antistatic performance and anti-staining performance, and there was a problem that it was difficult to improve the pressure-sensitive adhesive layer to have excellent antistatic performance and anti-staining performance when a material that is prone to peeling static electricity was used as an adherend.
[0008] Regarding (2) the stain resistance, a pressure-sensitive adhesive composition has been disclosed that contains 100 parts by mass of a (meth)acrylic copolymer having a weight average molecular weight of 100,000 or more and less than 1,000,000, which is composed of 0 part by mass or more and less than 0.5 part by mass of a carboxyl group-containing monomer, 0.6 to 9 parts by mass of a hydroxyl group-containing (meth)acrylic monomer, and 99.4 to 90.5 parts by mass of a (meth)acrylic acid ester monomer; and 0.1 to 5 parts by mass of a carbodiimide crosslinking agent (Patent Document 3). The adhesive composition described in Patent Document 3 is characterized by using a carbodiimide-based crosslinking agent as a crosslinking agent for a (meth)acrylic copolymer of a specific composition. This makes it possible to provide an adhesive layer having a crosslinked structure that can follow shrinkage caused by pressure and temperature during autoclave treatment. For this reason, the adhesive layer formed using the adhesive composition described in Patent Document 3 is said to be able to suppress or prevent foaming even under high temperature and high pressure conditions (during autoclave treatment), to have excellent stain resistance, and to also have excellent transparency. However, in the pressure-sensitive adhesive layer obtained by crosslinking the pressure-sensitive adhesive composition described in Patent Document 3, although the stain resistance performance is improved, it has not been possible to simultaneously achieve antistatic performance and excellent adhesive performance by balancing the adhesive strength at both low and high peel speeds, and this remains as a problem to be solved.
[0009] As for (3) having excellent antistatic performance, a method of kneading an antistatic agent into a base film is known as a method for imparting antistatic properties to a surface protective film. Examples of the antistatic agent disclosed include (a) various cationic antistatic agents having cationic groups such as quaternary ammonium salts, pyridinium salts, and primary to tertiary amino groups, (b) anionic antistatic agents having anionic groups such as sulfonate groups, sulfate groups, phosphate groups, and phosphonate groups, (c) amphoteric antistatic agents such as amino acid-based and amino sulfate-based agents, (d) nonionic antistatic agents such as amino alcohol-based, glycerin-based, and polyethylene glycol-based agents, and (e) polymer-type antistatic agents obtained by increasing the molecular weight of the above-mentioned antistatic agents (Patent Document 4). However, although the surface protection film described in Patent Document 4 describes imparting antistatic performance related to the adhesion of dirt to the adherend, it does not describe a solution for achieving both excellent adhesive performance and contamination resistance, and this remains a problem to be solved.
[0010] In recent years, it has been proposed to directly incorporate an antistatic agent into the adhesive layer, rather than incorporating the antistatic agent into the substrate film or applying it to the surface of the substrate film.For example, an antistatic adhesive composition has been disclosed, which is characterized in that a salt having an anion having a fluoro group and a sulfonyl group is dissolved and dispersed in a polyetherester plasticizer containing a polyether group in the main chain (Patent Document 5). The adhesive composition described in Patent Document 5 discloses the use of a plasticizer consisting of an ester formed from a mono- or dicarboxylic acid having a saturated or unsaturated acyclic hydrocarbon group and an alcohol having a C1-20 acyclic hydrocarbon group, or an ester in which the unsaturated group in the unsaturated acyclic hydrocarbon group has been epoxidized. Such a mono- or dicarboxylic acid having a saturated or unsaturated acyclic hydrocarbon group has a carbon number close to that of the acrylic monomer constituting the acrylic copolymer used in the adhesive layer, and thus has good compatibility with the antistatic adhesive composition, and the plasticizer is suitably retained in the acrylic antistatic adhesive composition, thereby suppressing bleed-out. However, although Patent Document 5 discloses a technique for improving antistatic performance and bleed-out in a pressure-sensitive adhesive layer obtained by crosslinking the antistatic pressure-sensitive adhesive composition, it does not disclose that excellent adhesive performance can be obtained by balancing adhesive strength at low and high peel speeds, and the problem of obtaining a pressure-sensitive adhesive layer with excellent adhesive performance remains. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Publication No. 63-225677 [Patent Document 2] Japanese Patent Application Publication No. 11-256111 [Patent Document 3] JP 2011-122054 A [Patent Document 4] Japanese Patent Application Publication No. 11-070629 [Patent Document 5] JP 2014-118469 A Summary of the Invention [Problem to be solved by the invention]
[0012] As described above, there is no prior art that solves the problems of simultaneously achieving the required performance for the adhesive layer that constitutes a surface protection film: (1) balancing adhesive strength at low and high peel speeds, (2) having anti-soiling performance, and (3) having excellent antistatic performance. Furthermore, in the past, there has been a trade-off between the antistatic performance of a pressure-sensitive adhesive layer formed using a pressure-sensitive adhesive composition with antistatic properties, and the anti-contamination performance of an adherend, and it has been difficult to improve the anti-contamination performance while maintaining the antistatic performance, in a pressure-sensitive adhesive layer formed using the same and a surface protective film using the same. Furthermore, in recent years, the types of materials of the adherends to which the surface protection film is attached have increased, and the surface treatment conditions of the adherends have become more diverse, making it increasingly difficult for the adhesive layer that constitutes the surface protection film to balance the adhesive strength for all adherends, particularly at the above-mentioned (1) low and high peel speeds, and (2) to have contamination resistance.
[0013] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a pressure-sensitive adhesive composition that has balanced adhesive strength at both low and high peel speeds and is capable of achieving both antistatic performance and anti-soiling performance, and a pressure-sensitive adhesive film and a surface protection film using the same. [Means for solving the problem]
[0014] The inventors of the present invention have reconsidered the type of compound to be copolymerized with an acrylic polymer in an adhesive composition used in a surface protection film for polarizing plates, the adhesive composition containing an acrylic polymer, an antistatic agent, and a crosslinking agent, and have worked diligently to improve the above-mentioned problem of (1) achieving a balance in adhesive strength at both a low peel speed and a high peel speed, and (2) having stain resistance. As a result, it was found that the above problems (1) and (2) can be simultaneously solved by specifying the content ratio of 2-ethylhexyl acrylate and a monofunctional methacrylate monomer whose homopolymer has a glass transition temperature (Tg) of 0°C or higher within a specific range among (A) alkyl (meth)acrylates having an alkyl group with a carbon number of C1 to C10, and the present invention was completed by further forming a pressure-sensitive adhesive composition containing an antistatic agent.
[0015] In order to solve the above problems, the present invention provides a pressure-sensitive adhesive composition comprising a first acrylic polymer, a crosslinking agent, and an ionic compound, wherein the first acrylic polymer is a copolymer of (A) 100 parts by weight of at least two or more alkyl (meth)acrylates having an alkyl group carbon number of C1 to C10, (B) 1.0 to 6.0 parts by weight of at least one or more copolymerizable monomers containing a hydroxyl group, and (C) 0.01 to 0.6 parts by weight of at least one or more copolymerizable monomers containing a carboxyl group, and has an acid value of 0.1 to 1.0 and a weight average molecular weight of more than 300,000. The adhesive composition is an acrylic polymer consisting of a copolymer having a carbon number of more than 1 million, and contains 50 parts by weight or more of 2-ethylhexyl acrylate and 5 to 40 parts by weight of one or more monofunctional methacrylate monomers having a homopolymer Tg of 0°C or higher out of a total of 100 parts by weight of at least two or more alkyl (meth)acrylates (A) having a carbon number of C1 to C10 in the alkyl group, and the adhesive composition contains a trifunctional or higher isocyanate compound as the crosslinking agent, a crosslinking retarder, and a crosslinking catalyst other than a tin compound as the crosslinking catalyst.
[0016] A surface protection film obtained by laminating a 15 μm thick adhesive layer obtained by crosslinking the adhesive composition on one side of a 38 μm thick polyester film is attached to the surface of a polarizing plate, and then the surface protection film is peeled off from the polarizing plate. It is preferable that the adhesive strength at a low peeling speed of 0.3 m / min is 0.01 to 0.1 N / 25 mm and the adhesive strength at a high peeling speed of 30 m / min is 1.0 N / 25 mm or less.
[0017] The monofunctional methacrylate monomer having a homopolymer Tg of 0° C. or higher is preferably at least one selected from the group consisting of n-butyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, ethyl methacrylate, and methyl methacrylate.
[0018] It is preferable that the pressure-sensitive adhesive composition further contains a second acrylic polymer, the second acrylic polymer being a copolymer obtained by copolymerizing (a) at least one or more (meth)acrylic acid ester monomers having an alkyl group with a carbon number of C1 to C18, (b) at least one or more copolymerizable monomers having a hydroxyl group, and (c) at least one or more polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomers, and that the pressure-sensitive adhesive composition contains 0.1 to 5.0 parts by weight of the second acrylic polymer per 100 parts by weight of the total of the at least two or more (A) alkyl (meth)acrylates having an alkyl group with a carbon number of C1 to C10.
[0019] It is preferable that the pressure-sensitive adhesive composition is a pressure-sensitive adhesive composition for forming a pressure-sensitive adhesive layer used in a surface protection film for a polarizing plate, the protective layer of the polarizer of the polarizing plate is one type selected from the group consisting of a TAC-based film, a PMMA-based film, and a PET-based film, and the surface treatment applied to the surface of the protective layer of the polarizer of the polarizing plate is one type selected from the group consisting of untreated, AG treatment, LR treatment, AR treatment, AG-LR treatment, and AG-AR treatment.
[0020] It is preferable that the ionic compound is an ionic compound having a melting point of 25 to 80°C, the cation of the ionic compound is pyridinium, and the pressure-sensitive adhesive composition contains the ionic compound as an essential component in a ratio of 0.01 to 10 parts by weight per 100 parts by weight of the first acrylic polymer.
[0021] The pressure-sensitive adhesive layer obtained by crosslinking the pressure-sensitive adhesive composition has a surface resistivity of 1.0×10 +12 Ω / □ or less, the peeling electrification voltage of the pressure-sensitive adhesive layer relative to a low refractive index layer formed using a composition for forming a low refractive index layer containing a fluorine compound is within the range of +0.3 to −0.3 kV; It is preferable that the surface substrate is one selected from the group consisting of a TAC-based film, a PMMA-based film, and a PET-based film, and that the surface treatment applied to the surface of the surface substrate is one selected from the group consisting of untreated, AG treatment, LR treatment, AR treatment, AG-LR treatment, and AG-AR treatment, and then the film is laminated to a polarizing plate, left for two days in an atmosphere at a temperature of 60°C and a humidity of 90%, removed, and then peeled off after one day has passed, so that there is no contamination.
[0022] the (B) hydroxyl group-containing copolymerizable monomer is at least one selected from the group consisting of 8-hydroxyoctyl(meth)acrylate, 6-hydroxyhexyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxyethyl(meth)acrylate, N-hydroxy(meth)acrylamide, N-hydroxymethyl(meth)acrylamide, and N-hydroxyethyl(meth)acrylamide, The (C) carboxyl group-containing copolymerizable monomer is preferably at least one selected from the group consisting of (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl maleic acid, carboxypolycaprolactone mono(meth)acrylate, and 2-(meth)acryloyloxyethyl tetrahydrophthalic acid.
[0023] It is preferable that the crosslinking retarder is a keto-enol tautomer compound, and the crosslinking retarder is contained in a ratio of 0.1 to 300 parts by weight relative to 100 parts by weight of the first acrylic polymer, the crosslinking catalyst is at least one metal chelate compound selected from the group consisting of aluminum chelate compounds, titanium chelate compounds, and iron chelate compounds, and the crosslinking catalyst is contained in a ratio of 0.001 to 0.5 parts by weight relative to 100 parts by weight of the first acrylic polymer, and the weight ratio of the crosslinking retarder / the crosslinking catalyst is 80 to 1000.
[0024] The pressure-sensitive adhesive composition preferably contains 0.01 to 0.5 parts by weight of a polyether-modified siloxane compound having an HLB value of 6 to 12 and a weight average molecular weight of 10,000 or less, based on 100 parts by weight of the first acrylic polymer.
[0025] The second acrylic polymer is a copolymer having a weight average molecular weight of more than 300,000 and not more than 800,000, which is obtained by copolymerizing 2.0 to 12.0 parts by weight of at least one or more (b) copolymerizable monomers containing a hydroxyl group and 1 to 30 parts by weight of at least one or more (meth)acrylic acid ester monomers containing a polyalkylene glycol chain, with respect to a total of 100 parts by weight of at least one or more (a) (meth)acrylic acid ester monomers having a carbon number of an alkyl group of C1 to C18, and the ratio (b-1) / (B-1) of the total parts by weight of the at least one or more (B) copolymerizable monomers containing a hydroxyl group contained in the first acrylic polymer to the total of 100 parts by weight of the first acrylic polymer and the total parts by weight of the at least one or more (b) copolymerizable monomers containing a hydroxyl group contained in the second acrylic polymer to the total of 100 parts by weight of the second acrylic polymer is preferably within the range of 1.0 to 2.0.
[0026] It is preferable that the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer has an average repeat number of 3 to 14 for the alkylene oxide constituting the polyalkylene glycol chain, the diester content in the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer is 0.2% or less, and the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer contains at least one selected from the group consisting of polyalkylene glycol mono(meth)acrylate, methoxypolyalkylene glycol (meth)acrylate, and ethoxypolyalkylene glycol (meth)acrylate in an amount of 1 to 50 parts by weight per 100 parts by weight of the second acrylic polymer.
[0027] The present invention also provides a pressure-sensitive adhesive film, comprising a resin film and a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition on one side of the resin film.
[0028] The present invention also provides a surface protection film using the above-mentioned pressure-sensitive adhesive film.
[0029] The present invention also provides a surface protection film for a polarizing plate, which uses the above-mentioned pressure-sensitive adhesive film.
[0030] The present invention also provides an optical film with a pressure-sensitive adhesive layer, comprising an optical film and a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition, laminated on at least one surface of the optical film.
[0031] The present invention also provides a pressure-sensitive adhesive film, wherein one surface of the resin film opposite the surface on which the pressure-sensitive adhesive layer is formed is subjected to an antistatic treatment and an antifouling treatment. Effect of the Invention
[0032] In the pressure-sensitive adhesive composition according to the present invention, the first acrylic polymer contains 50 parts by weight or more of 2-ethylhexyl acrylate and 5 to 40 parts by weight of one or more monofunctional methacrylate monomers having a homopolymer Tg of 0° C. or higher out of a total of 100 parts by weight of at least two or more alkyl (meth)acrylates (A) whose alkyl group has carbon numbers of C1 to C10. This makes it possible to simultaneously achieve (1) a balance of adhesive strength at low and high peel speeds and (2) stain resistance, particularly in a surface protective film for polarizing plates using PMMA as a substrate. Incidentally, it is not clear why the inclusion of one or more monofunctional methacrylate monomers having a homopolymer Tg of 0° C. or higher in the pressure-sensitive adhesive composition of the present invention contributes to (1) balancing the adhesive strength at low and high peel speeds, and (2) providing stain resistance. Possible reasons for this are that these methacrylate monomers provide polymers with high Tg despite not having polar functional groups such as carboxyl groups or amide groups, or long-chain alkyl groups exceeding C10, thereby greatly improving adhesive performance in the crosslinked state, and that the affinity with methyl methacrylate, the main component of PMMA-based films, is improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Hereinafter, the present invention will be described based on preferred embodiments. The pressure-sensitive adhesive composition of the present embodiment is a pressure-sensitive adhesive composition containing an acrylic polymer, a crosslinking agent, and an ionic compound, wherein the acrylic polymer is (A) 100 parts by weight of a total of at least two or more alkyl (meth)acrylates having an alkyl group with a carbon number of C1 to C10, (B) 1.0 to 6.0 parts by weight of at least one copolymerizable monomer containing a hydroxyl group; (C) 0.01 to 0.6 parts by weight of at least one copolymerizable monomer containing a carboxyl group; and an acrylic polymer having an acid value of 0.1 to 1.0 and a weight average molecular weight of more than 300,000 and not more than 1,000,000. (A) contains 50 parts by weight or more of 2-ethylhexyl acrylate and 5 to 40 parts by weight or more of one or more monofunctional methacrylate monomers having a homopolymer Tg of 0° C. or higher out of a total of 100 parts by weight of at least two or more alkyl (meth)acrylates having an alkyl group with a carbon number of C1 to C10; The pressure-sensitive adhesive composition is characterized by comprising a tri- or higher functional isocyanate compound as the crosslinking agent, a crosslinking retarder, and a crosslinking catalyst other than a tin compound as the crosslinking catalyst.
[0034] The acrylic polymer used in the pressure-sensitive adhesive composition of the present embodiment is a main polymer of the pressure-sensitive adhesive composition, and may be referred to as a first acrylic polymer when distinguishing it from a second acrylic polymer described below. The first acrylic polymer is an acrylic polymer having a glass transition temperature (Tg) of 0° C. or lower. The first acrylic polymer is preferably a copolymer mainly composed of an alkyl (meth)acrylate in which the carbon number of the alkyl group (A) is C1 to C10.
[0035] (A) Examples of the alkyl (meth)acrylate having an alkyl group with a carbon number of C1 to C10 include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, cyclopentyl (meth)acrylate, and cyclohexyl (meth)acrylate. The alkyl group of these alkyl (meth)acrylates may be either acyclic (straight-chain or branched) or cyclic (monocyclic or polycyclic).
[0036] The first acrylic polymer preferably contains, out of a total of 100 parts by weight of (A), 50 parts by weight or more of 2-ethylhexyl acrylate and 5 to 40 parts by weight of a total of one or more monofunctional methacrylate monomers having a homopolymer Tg of 0°C or higher. In addition, 2-ethylhexyl acrylate is preferably contained in an amount of 50 parts by weight or more, more preferably 60 parts by weight or more, and particularly preferably 70 parts by weight or more, of a total of 100 parts by weight of (A). Furthermore, among (A) alkyl (meth)acrylates having an alkyl group with a carbon number of C1 to C10, examples of monofunctional methacrylate monomers having a Tg of 0°C or higher include one or more selected from the group consisting of n-butyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, ethyl methacrylate, methyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-hexyl methacrylate, isohexyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, and dicyclopentamethacrylate. Among these monofunctional methacrylate monomers having a Tg of 0°C or higher, methacrylate monomers in which the alkyl group has a carbon number of C1 to C6 are preferred, and methacrylate monomers in which the alkyl group has a carbon number of C1 to C4 are more preferred, and one or more selected from the group consisting of n-butyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, ethyl methacrylate, and methyl methacrylate are particularly preferred. The total amount of one or more monofunctional methacrylate monomers having a Tg of 0° C. or higher is preferably 5 to 40 parts by weight, more preferably 8 to 40 parts by weight, and particularly preferably 10 to 35 parts by weight, out of 100 parts by weight of the total of (A). In the following description, when the Tg of a monomer is simply mentioned, it may refer to the Tg of a homopolymer.
[0037] The (B) hydroxyl group-containing copolymerizable monomer used in the first acrylic polymer is preferably at least one selected from the group consisting of 8-hydroxyoctyl(meth)acrylate, 6-hydroxyhexyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxyethyl(meth)acrylate, N-hydroxy(meth)acrylamide, N-hydroxymethyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and the like. The first acrylic polymer preferably contains at least one kind of copolymerizable monomer containing a hydroxyl group (B) in a ratio of 1.0 to 6.0 parts by weight, more preferably 2.0 to 6.0 parts by weight, and particularly preferably 2.5 to 5.5 parts by weight, per 100 parts by weight of the total of (A).
[0038] The (C) carboxyl group-containing copolymerizable monomer used in the first acrylic polymer is preferably at least one selected from the group consisting of (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl maleic acid, carboxypolycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethyl tetrahydrophthalic acid, and the like. The first acrylic polymer preferably contains at least one or more kinds of copolymerizable monomers containing a carboxyl group (C) in a ratio of 0.01 to 0.6 parts by weight, more preferably 0.01 to 0.5 parts by weight, and particularly preferably 0.01 to 0.4 parts by weight, per 100 parts by weight of the total of (A).
[0039] The method for producing the first acrylic polymer is not particularly limited, and any known polymerization method such as solution polymerization or emulsion polymerization can be used as appropriate. The first acrylic polymer preferably has a weight average molecular weight of more than 300,000 and not more than 1,000,000. The first acrylic polymer preferably has an acid value of 0.1 to 1.0. This can improve the stain resistance. Here, the "acid value" is an index representing the acid content, and is expressed as the number of milligrams of potassium hydroxide required to neutralize 1 g of a polymer containing a carboxyl group.
[0040] The pressure-sensitive adhesive composition according to the present embodiment contains an antistatic agent (G). The antistatic agent (G) according to the present embodiment is preferably an ionic compound having a melting point of 25 to 80° C. The ionic compound is preferably solid at room temperature. The room temperature is, for example, a temperature below 25° C., and specifically, the ionic compound is preferably solid at 23° C. The pressure-sensitive adhesive composition according to the present embodiment preferably contains the ionic compound as an essential component in a ratio of 0.01 to 10 parts by weight per 100 parts by weight of the first acrylic polymer.
[0041] The anion of the ionic compound is hexafluorophosphate (PF6 - ), thiocyanate (SCN - ), perchlorate (ClO4 - ), tetrafluoroborate (BF4 - ), inorganic anions such as carboxylates (RCOO - ), sulfonates (RSO3 - ), alkoxide or phenoxide salts (RO - ), organic imide salts (R - ), methide salt (R3C - ), organic borate salts (R4B - ) and other organic anions. R contained in each general formula of the organic anion is an organic group which may have a fluorine substitution. Examples of the organic group include at least one of an alkyl group, an alkoxy group, an aromatic group (aryl group, aralkyl group, etc.), an aliphatic or aromatic carbonyl group, and an aliphatic or aromatic sulfonyl group. The organic group contained in the anion may have some or all of the hydrogen atoms substituted with one or more halogen atoms such as a fluorine atom.
[0042] The cation of the ionic compound may be one selected from the group consisting of pyridinium, imidazolium, phosphonium, sulfonium, pyrrolidinium, guanidinium, ammonium, isouronium, thiouronium, piperidinium, pyrazolium, methylium, and morpholinium. The cation of the ionic compound is preferably pyridinium. The organic group contained in the cation may have some or all of the hydrogen atoms substituted with one or more halogen atoms such as fluorine atoms. When the anion and / or cation of an ionic compound contains an organic group such as an alkyl group, an ionic compound having a melting point of 25 to 80°C can be obtained by selecting the chain length of the alkyl group, the position and number of the substituents, etc.
[0043] Specific examples of the ionic compound include 1-octylpyridinium hexafluorophosphate, 1-nonylpyridinium hexafluorophosphate, 2-methyl-1-dodecylpyridinium hexafluorophosphate, 3-methyl-1-dodecylpyridinium hexafluorophosphate, 1-octylpyridinium dodecylbenzenesulfonate, 1-dodecylpyridinium thiocyanate, 1-dodecylpyridinium dodecylbenzenesulfonate, 4-methyl-1-octylpyridinium hexafluorophosphate, 1-nonylpyridinium 2-iodobenzenesulfonate, 4,5-diiodo-1-butyl-3-methylimidazolium hexafluorophosphate, 2-methyl-1-dodecylpyridinium 2-iodobenzenesulfonate, and 4,5-diiodo-1-butyl-3-methylimidazolium. 3-Iodobenzenesulfonate, 1-octyl-2-methylpyridinium trifluoromethanesulfonate salt, 1,2,3-trimethylimidazolium pentafluoroethanesulfonate salt, 1-butyl-2,3-dimethylimidazolium trifluoromethanesulfonate salt, 1-hexyl-4-methylpyridinium pentafluoroethanesulfonate salt, 1-octyl-3-methylpyridinium trifluoromethanesulfonate salt, n-octylpyridinium trifluoromethanesulfonate salt, 1-propyl-3-methylpyridinium nonafluorobutanesulfonate salt, 3-methyl-1-octylpyridinium nonafluorobutanesulfonate salt, methyltrioctylammonium tris(pentafluorobenzenesulfonyl)methide salt, 1-ethyl-3-methylimidazolium tetrakispentafluorophenylborate salt, 1-butyl-1-methylpiperidinium Examples thereof include bis(pentafluorobenzenesulfonyl)imide salts.
[0044] The pressure-sensitive adhesive composition according to the present embodiment further contains a trifunctional or higher isocyanate compound as a crosslinking agent (D). Examples of the trifunctional or higher isocyanate compound include biuret modified or isocyanurate modified diisocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, and xylylene diisocyanate, and adducts with trivalent or higher polyols such as trimethylolpropane and glycerin. The proportion of the trifunctional or higher isocyanate compound as the crosslinking agent (D) is preferably 0.1 to 10 parts by weight, more preferably 0.1 to 6 parts by weight, relative to 100 parts by weight of the first acrylic polymer.
[0045] The adhesive composition according to the present embodiment may contain a crosslinking retarder (E). Examples of the crosslinking retarder (E) include β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, octyl acetoacetate, oleyl acetoacetate, lauryl acetoacetate, and stearyl acetoacetate, and β-diketones such as acetylacetone, 2,4-hexanedione, and benzoylacetone. These are ketoenol tautomer compounds, and in an adhesive composition using a polyisocyanate compound as a crosslinking agent, blocking the isocyanate group of the crosslinking agent (D) can suppress excessive viscosity increase and gelation of the adhesive composition after the crosslinking agent is added, and the pot life of the adhesive composition can be extended. The crosslinking retarder (E) is preferably at least one selected from the group of compounds consisting of acetylacetone and ethyl acetoacetate. The crosslinking retarder (E) is preferably contained in an amount of 0.1 to 300 parts by weight per 100 parts by weight of the first acrylic polymer.
[0046] The pressure-sensitive adhesive composition according to this embodiment may contain a crosslinking catalyst other than a tin compound as the crosslinking catalyst (F). The crosslinking catalyst (F) may be any substance that functions as a catalyst for the reaction (crosslinking reaction) between the acrylic polymer and the crosslinking agent when a polyisocyanate compound is used as the crosslinking agent. The crosslinking catalyst (F) is preferably a metal chelate compound. The metal chelate compound is a compound in which one or more multidentate ligands L are bonded to a central metal atom M. The metal chelate compound may or may not have one or more monodentate ligands X bonded to the metal atom M. Specific examples of metal chelate compounds include iron tris(2,4-pentanedionato)(III), iron trisacetylacetonate, titanium trisacetylacetonate, ruthenium trisacetylacetonate, zinc bisacetylacetonate, aluminum trisacetylacetonate, zirconium tetrakisacetylacetonate, iron tris(2,4-hexanedionato)(III), zinc bis(2,4-hexanedionato), titanium tris(2,4-hexanedionato), aluminum tris(2,4-hexanedionato), and zirconium tetrakis(2,4-hexanedionato).
[0047] The crosslinking catalyst (F) is preferably at least one metal chelate compound selected from the group consisting of aluminum chelate compounds, titanium chelate compounds, and iron chelate compounds, and the crosslinking catalyst (F) is preferably contained in a ratio of 0.001 to 0.5 parts by weight based on 100 parts by weight of the first acrylic polymer.
[0048] Since the (E) crosslinking retarder has an effect of suppressing crosslinking in contrast to the (F) crosslinking catalyst, it is preferable to appropriately set the ratio of the (E) crosslinking retarder to the (F) crosslinking catalyst. In order to extend the pot life of the pressure-sensitive adhesive composition and improve its storage stability, the (E) / (F) weight parts ratio is preferably 80 to 1000, more preferably 80 to 700, and particularly preferably 80 to 300. Here, the (E) / (F) weight parts ratio is the quotient value obtained by dividing the parts by weight of (E) by the parts by weight of (F).
[0049] The pressure-sensitive adhesive composition according to the present embodiment may contain, as an optional component, a polyether-modified siloxane compound (H). The polyether-modified siloxane compound (H) is a siloxane compound having a polyether group, and has a general siloxane unit [-SiR 1 2-O-], as well as siloxane units with polyether groups [-SiR 1 (R 2 O(R 3 O) n R 4 )-O-], where R 1 is one or more alkyl or aryl groups, R 2 and R 3 is one or more alkylene groups, R 4 indicates one or more alkyl or acyl groups (terminal groups). The polyether group is a polyoxyethylene group [(C2H4O) n 〕 and polyoxypropylene group〔(C3H6O) n In the siloxane unit having a polyether group, the terminal of the polyether group is an OH group (R 4 =H).
[0050] The polyether-modified siloxane compound (H) is preferably a polyether-modified siloxane compound having an HLB value of 6 to 12. The polyether-modified siloxane compound (H) is preferably contained in a ratio of 0.01 to 0.5 parts by weight, more preferably in a ratio of 0.02 to 0.35 parts by weight, and particularly preferably in a ratio of 0.02 to 0.25 parts by weight, relative to 100 parts by weight of the first acrylic polymer. The HLB value is, for example, the hydrophilic-lipophilic balance (hydrophilic-lipophilic ratio) as defined in JIS K3211 (surfactant terminology) or the like. Polyether-modified siloxane compounds can be obtained, for example, by grafting an organic compound having an unsaturated bond and a polyoxyalkylene group onto a polyorganosiloxane main chain having a silicon hydride group by a hydrosilylation reaction.Specific examples include dimethylsiloxane-methyl(polyoxyethylene)siloxane copolymer, dimethylsiloxane-methyl(polyoxyethylene)siloxane-methyl(polyoxypropylene)siloxane copolymer, and dimethylsiloxane-methyl(polyoxypropylene)siloxane polymer.
[0051] By blending the (H) polyether-modified siloxane compound in the pressure-sensitive adhesive composition, the adhesive strength and rework performance of the pressure-sensitive adhesive layer can be improved. The weight-average molecular weight of the (H) polyether-modified siloxane compound is preferably 10,000 or less. From the viewpoint of compatibility with acrylic polymers, the lower the HLB value and the lower the molecular weight, the better the compatibility. However, if the polyether-modified siloxane compound has a low molecular weight, it can obtain excellent antistatic properties even if it has a relatively high HLB value and somewhat low compatibility with the polymer.
[0052] The adhesive composition according to the present embodiment may contain a second acrylic polymer as an optional component. The adhesive composition further contains a second acrylic polymer obtained by copolymerizing a polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer, thereby improving the compatibility between the ionic compound and the acrylic polymer, and further improving the antistatic performance and the stain resistance. The second acrylic polymer may be a copolymer obtained by copolymerizing (a) at least one or more (meth)acrylic acid ester monomers having an alkyl group with a carbon number of C1 to C18, (b) at least one or more copolymerizable monomers containing a hydroxyl group, and (c) at least one or more polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomers.
[0053] Examples of the (a) (meth)acrylic acid ester monomer having an alkyl group with a carbon number of C1 to C18 used in the second acrylic polymer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, and isooctyl. Examples of the alkyl group include ethylhexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, cyclopentyl (meth)acrylate, and cyclohexyl (meth)acrylate. The alkyl group in (a) may be either acyclic (straight-chain or branched) or cyclic (monocyclic or polycyclic). It is also possible to select a compound or ratio in which (a) the (meth)acrylic acid ester monomer having an alkyl group with a carbon number of C1 to C18 used in the second acrylic polymer is the same as (A) the alkyl (meth)acrylate having an alkyl group with a carbon number of C1 to C10 used in the first acrylic polymer. Alternatively, (a) may contain a compound different from (A). Even if the monomers are the same compound, the ratio in (a) may be different from the ratio in (A). For example, the second acrylic polymer may be a copolymer in which alkyl methacrylate is not copolymerized. The second acrylic polymer may be a copolymer in which a (meth)acrylic acid ester monomer having an alkyl group with a carbon number of C11 to C18 is not copolymerized, or the second acrylic polymer may contain a (meth)acrylic acid ester monomer having an alkyl group with a carbon number of C11 to C18.
[0054] The (b) hydroxyl group-containing copolymerizable monomer used in the second acrylic polymer is preferably at least one selected from the group consisting of 8-hydroxyoctyl(meth)acrylate, 6-hydroxyhexyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxyethyl(meth)acrylate, N-hydroxy(meth)acrylamide, N-hydroxymethyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and the like. The second acrylic polymer preferably contains 2.0 to 12.0 parts by weight, more preferably 3.0 to 12.0 parts by weight, and particularly preferably 4.0 to 12.0 parts by weight of at least one copolymerizable monomer containing a hydroxyl group, per 100 parts by weight of the at least one (meth)acrylic acid ester monomer having a carbon number of C1 to C18 in the alkyl group (a). It is also possible to select the same compound or ratio of the (b) hydroxyl group-containing copolymerizable monomer used in the second acrylic polymer as the (B) hydroxyl group-containing copolymerizable monomer used in the first acrylic polymer. Alternatively, (b) may contain a compound different from (B). Even if the monomers are the same compound, the ratio in (b) may be different from the ratio in (B).
[0055] The second acrylic polymer used in the pressure-sensitive adhesive composition of the present embodiment contains (c) a polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer. In the pressure-sensitive adhesive composition of the present embodiment, the second acrylic polymer containing (c) a polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer functions as an antistatic auxiliary. The first acrylic polymer may be a copolymer in which no polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer is copolymerized, or it is also possible to copolymerize a polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer similar to that of the second acrylic polymer. The second acrylic polymer is preferably contained in a proportion of 0.1 to 5.0 parts by weight, more preferably 0.1 to 3.5 parts by weight, and particularly preferably 0.1 to 2.5 parts by weight, relative to 100 parts by weight in total of the at least two or more kinds of alkyl (meth)acrylates (A) whose alkyl group has carbon numbers of C1 to C10 used in the first acrylic polymer.
[0056] The (c) polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer may be a compound in which one of the multiple hydroxyl groups of a polyalkylene glycol is esterified as a (meth)acrylic acid ester. Since the (meth)acrylic acid ester group is a polymerizable group, it can be copolymerized with a second acrylic polymer. It may be a polyalkylene glycol mono(meth)acrylate in which the other hydroxyl group remains OH, or an alkoxy polyalkylene glycol mono(meth)acrylate in which the other hydroxyl group is converted to an alkyl ether. Since polyalkylene glycol mono(meth)acrylate corresponds to (c), it is not classified as (B) or (b) even if it contains a hydroxyl group.
[0057] The polyalkylene glycol constituting the polyalkylene glycol chain may be any glycol compound having one or more alkylene groups, and examples thereof include polyethylene glycol, polypropylene glycol, polybutylene glycol, polyethylene glycol-polypropylene glycol, polyethylene glycol-polybutylene glycol, polypropylene glycol-polybutylene glycol, and polyethylene glycol-polypropylene glycol-polybutylene glycol.
[0058] It is preferable that (c) the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer has an average repeat number of alkylene oxide constituting the polyalkylene glycol chain of 3 to 14. The "average repeat number of alkylene oxide" refers to the average number of repeating alkylene oxide units in the "polyalkylene glycol chain" portion contained in the molecular structure of (c) the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer. The diester content in the (c) polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer is preferably 0.2% or less. The "diester content in the monomer" refers to the content (wt%) of polyalkylene glycol di(meth)acrylic acid ester contained in the (c) polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer.
[0059] The (c) polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer is preferably at least one selected from the group consisting of polyalkylene glycol mono(meth)acrylate, methoxypolyalkylene glycol (meth)acrylate, and ethoxypolyalkylene glycol (meth)acrylate. The second acrylic polymer preferably contains 1 to 30 parts by weight, more preferably 2 to 30 parts by weight, and particularly preferably 5 to 25 parts by weight of (c) a polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer, relative to 100 parts by weight in total of (a) the at least one or more (meth)acrylic acid ester monomers having an alkyl group with a carbon number of C1 to C18.
[0060] The method for producing the second acrylic polymer is not particularly limited, and a known polymerization method such as a solution polymerization method or an emulsion polymerization method can be used as appropriate. The second acrylic polymer is preferably a copolymer having a weight average molecular weight of more than 300,000 and not more than 800,000. The weight average molecular weight of the second acrylic polymer may be approximately the same as the weight average molecular weight of the first acrylic polymer, or may be larger or smaller than the weight average molecular weight of the first acrylic polymer. The second acrylic polymer may have a functional group capable of reacting with the (D) crosslinking agent. The second acrylic polymer may be a copolymer in which no copolymerizable monomer containing a carboxyl group is copolymerized, or may be a copolymer in which a copolymerizable monomer containing a carboxyl group similar to that of the first acrylic polymer is copolymerized. The (D) crosslinking agent may participate in crosslinking between the first acrylic polymer and the second acrylic polymer.
[0061] The ratio (b-1) / (B-1) of the total parts by weight of at least one or more kinds of (B) copolymerizable monomers containing a hydroxyl group contained in the first acrylic polymer relative to 100 parts by weight of the first acrylic polymer to the total parts by weight of at least one or more kinds of (b) copolymerizable monomers containing a hydroxyl group contained in the second acrylic polymer relative to 100 parts by weight of the second acrylic polymer is preferably within a range of 1.0 to 2.0.
[0062] The adhesive composition of the present embodiment may contain, as appropriate, known additives such as surfactants, curing accelerators, plasticizers, fillers, curing retarders, processing aids, antioxidants, antioxidants, etc. These may be used alone or in combination of two or more kinds.
[0063] The pressure-sensitive adhesive composition of the present embodiment is suitable as a pressure-sensitive adhesive composition for forming a pressure-sensitive adhesive layer used in a surface protection film for a polarizing plate. The pressure-sensitive adhesive layer of the surface protection film may be attached to a protective layer of a polarizer of a polarizing plate. Here, the protective layer of the polarizer of the polarizing plate may be at least one selected from the group consisting of a TAC-based film, a PMMA-based film, and a PET-based film. Here, TAC is an abbreviation for triacetyl cellulose, PMMA is an abbreviation for polymethyl methacrylate, and PET is an abbreviation for polyethylene terephthalate. The surface treatment applied to the protective layer of the polarizer of the polarizing plate may be at least one selected from the group consisting of untreated, AG treatment, LR treatment, AR treatment, AG-LR treatment, and AG-AR treatment, where AG stands for anti-glare, LR stands for low reflection, and AR stands for anti-reflection.
[0064] The pressure-sensitive adhesive layer obtained by crosslinking the pressure-sensitive adhesive composition of the present embodiment has a surface resistivity of 1.0×10 +12 It is preferable that the resistance is 5.0×10 +11 It is more preferable that the resistance is 1.0×10 +11 It is particularly preferable that the surface resistivity is Ω / □ or less. If the surface resistivity is high, the performance of dissipating static electricity generated when peeling the adhesive layer from the adherend is poor. Therefore, by making the surface resistivity sufficiently small, the peeling electrification voltage caused by static electricity generated when peeling the adhesive layer from the adherend is reduced, and the influence on the adherend can be suppressed.
[0065] The adhesive layer crosslinked with the adhesive composition of the present embodiment preferably has a peeling electrification voltage within the range of +0.3 to -0.3 kV with respect to a low refractive index layer formed using a composition for forming a low refractive index layer containing a fluorine compound. Examples of the fluorine compound used in the composition for forming a low refractive index layer include fluorine-containing copolymers which are polymers of one or more of fluorinated olefins, fluorinated vinyl ethers, fluorinated alkyl (meth)acrylates, etc., and condensates of fluorinated alkyl group-containing silane compounds. The fluorine-containing copolymer may be copolymerized with non-fluorinated monomers such as olefins, vinyl ethers, and (meth)acrylates in addition to fluorinated monomers. The low refractive index layer may be combined with a high refractive index layer or the like to form an antireflection layer.
[0066] When measuring the peeling electrification voltage for the low refractive index layer, examples of the substrate for forming the low refractive index layer on the surface include a PMMA substrate and a TAC substrate. In addition, the pressure-sensitive adhesive layer crosslinked with the pressure-sensitive adhesive composition of the present embodiment preferably has a peeling electrification voltage in the range of +0.3 to -0.3 kV for a plain layer that is not treated on the surface of the PMMA substrate or the TAC substrate.
[0067] It is preferable that the pressure-sensitive adhesive layer is not contaminated when it is attached to an adherend such as a polarizing plate, left in an atmosphere of 60°C and 90%RH for 2 days (48 hr), removed from the atmosphere, and peeled off after 1 day. An example of the adherend is a polarizing plate in which a protective layer is laminated on a polarizer, and the surface of the protective layer is subjected to a low-reflection surface treatment with a composition containing a fluorine compound. The composition containing a fluorine compound used for the low-reflection surface treatment may be the same as or different from the resin composition for forming the low refractive index layer containing the above-mentioned fluorine compound. Examples of the protective layer and surface treatment include the protective layer of the above-mentioned polarizer and the surface treatment applied to the surface thereof.
[0068] A surface protection film obtained by laminating a 15 μm thick adhesive layer crosslinked with the adhesive composition of the present embodiment on one side of a 38 μm thick polyester film is attached to the surface of a polarizing plate, and then the surface protection film is peeled off from the polarizing plate. The adhesive strength at a low peeling speed of 0.3 m / min is preferably 0.01 to 0.1 N / 25 mm, and the adhesive strength at a high peeling speed of 30 m / min is preferably 1.0 N / 25 mm or less, and the adhesive strength at a high peeling speed of 30 m / min is more preferably 0.2 to 1.6 N / 25 mm. This provides performance in which the adhesive strength changes little depending on the peeling speed, and allows for rapid peeling even at high-speed peeling. In addition, when the surface protection film is peeled off once for re-adhesion, excessive force is not required, and it is easy to peel off from the adherend.
[0069] The gel fraction of the pressure-sensitive adhesive layer obtained by crosslinking the pressure-sensitive adhesive composition of the present embodiment is preferably 95 to 100%, more preferably 97 to 100%. Such a high gel fraction of the pressure-sensitive adhesive layer prevents excessive adhesive strength at low peel speeds, reduces elution of unpolymerized monomers or oligomers from the copolymer, improves reworkability and durability at high temperatures and high humidity, and suppresses contamination of the adherend.
[0070] The adhesive film of this embodiment is formed by forming an adhesive layer formed by crosslinking the adhesive composition of this embodiment on one side or both sides of a resin film. Also, the surface protection film of this embodiment is a surface protection film formed by forming an adhesive layer formed by crosslinking the adhesive composition of this embodiment on one side of a resin film. The adhesive composition of this embodiment has excellent antistatic performance, has an excellent balance of adhesive strength at low and high peeling speeds, and also has anti-staining performance. Therefore, it can be suitably used as a surface protection film for a polarizing plate.
[0071] As the base film of the pressure-sensitive adhesive layer and the release film (separator) that protects the adhesive surface, a resin film such as a polyester film can be used. One side of the resin film may be subjected to antistatic treatment and antifouling treatment on the side opposite to the side on which the pressure-sensitive adhesive layer is formed. Antistatic treatment may include coating or kneading of an antistatic agent. Antifouling treatment may include treatment with a silicone-based or fluorine-based release agent or coating agent, silica fine particles, etc. The release film may be subjected to release treatment with a silicone-based, fluorine-based, or long-chain alkyl-based release agent on the side that is to be joined to the adhesive surface of the pressure-sensitive adhesive layer.
[0072] In addition, an optical film with a pressure-sensitive adhesive layer can be obtained by laminating a pressure-sensitive adhesive layer obtained by crosslinking the pressure-sensitive adhesive composition of the present embodiment on at least one surface of an optical film. Examples of optical films include polarizing films, retardation films, anti-reflection films, anti-glare films, ultraviolet absorbing films, infrared absorbing films, optical compensation films, and brightness enhancing films. Examples of devices to which optical members are applied include liquid crystal panels, organic EL panels, and touch panels. In the case of optical surface protection films such as surface protection films for polarizing plates and pressure-sensitive adhesive films, the base film and pressure-sensitive adhesive layer preferably have sufficient transparency. EXAMPLES
[0073] The present invention will now be described in detail with reference to examples.
[0074] <Production of First Acrylic Polymer> [Example 1] Nitrogen gas was introduced into a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, and the air in the reactor was replaced with nitrogen gas. Then, 70 parts by weight of 2-ethylhexyl acrylate, 30 parts by weight of n-butyl methacrylate, 5.5 parts by weight of 8-hydroxyoctyl acrylate, 0.2 parts by weight of acrylic acid, and a solvent (ethyl acetate) were added to the reactor. Then, 0.1 parts by weight of azobisisobutyronitrile was dropped as a polymerization initiator over 2 hours, and the mixture was reacted at 65°C for 6 hours to obtain a first acrylic polymer used in Example 1. [Examples 2 to 6 and Comparative Examples 1 to 4] The first acrylic polymer solutions used in Examples 2 to 6 and Comparative Examples 1 to 4 were obtained in the same manner as the first acrylic polymer solution used in Example 1 above, except that the monomer compositions were set as shown in Table 1 (A), (B), and (C), respectively. The first acrylic polymer used in Examples 1 to 6 and Comparative Examples 1 to 4 was a copolymer having a weight average molecular weight of more than 300,000 and not more than 1,000,000.
[0075] <Production of Pressure-Sensitive Adhesive Composition and Surface Protective Film> [Example 1] To the first acrylic polymer solution of Example 1 produced as described above, 2.0 parts by weight of a crosslinking agent (Coronate HX), 9 parts by weight of acetylacetone, 0.1 parts by weight of a crosslinking catalyst (titanium trisacetylacetonate), 0.9 parts by weight of an antistatic agent (3-methyl-1-octylpyridinium nonafluorobutanesulfonate salt), 0.05 parts by weight of a polyether-modified siloxane compound (HLB=7), 0.2 parts by weight of a copolymer having a weight average molecular weight (Mw) of 600,000, which was copolymerized with 2-ethylhexyl acrylate, 8-hydroxyoctyl acrylate, and methoxypolyethylene glycol acrylate (n=8) in a weight ratio of 100:8:15, were added and mixed by stirring to obtain a pressure-sensitive adhesive composition of Example 1. This pressure-sensitive adhesive composition was applied onto a release film (a silicone resin-coated PET film), and the solvent was removed by drying at 90°C to obtain a pressure-sensitive adhesive layer having a thickness of 20 μm. Thereafter, the adhesive layer with a release film was transferred to the side of the base film (a PET film with one side treated for antistatic and antifouling) opposite the side treated for antistatic and antifouling, thereby obtaining the surface protection film of Example 1 having a laminate structure of "base film / adhesive layer / release film". [Examples 2 to 6 and Comparative Examples 1 to 4] The surface protection films of Examples 2 to 6 and Comparative Examples 1 to 4 were obtained in the same manner as the surface protection film of Example 1 above, except that the compositions of the additives were as shown in Tables 1 to 2, (D) to (H), and (J), respectively. In the surface protection films of Examples 1 to 6 and Comparative Examples 1 to 4, the gel fraction of the pressure-sensitive adhesive layer was in the range of 95 to 100%.
[0076] [Table 1]
[0077] [Table 2]
[0078] In Tables 1 and 2, the parts by weight of each component were calculated relative to 100 parts by weight of the total of (A) alkyl (meth)acrylates having an alkyl group with carbon numbers of C1 to C10. In Tables 1 and 2, in each of columns (B) to (H) and (J), the content (parts by weight) of each component is shown as a numerical value in parentheses ( ), with the acrylic polymer being 100 parts by weight. The compound names of the abbreviations of the components (A) to (H) used in Tables 1 and 2 are shown in Table 3. Coronate (registered trademark) HX, HL, and L are product names of Tosoh Corporation, and Takenate (registered trademark) D-140N, D-127N, and D-110N are product names of Mitsui Chemicals, Inc.
[0079] [Table 3]
[0080] Among the (G) antistatic agents, G-1 to G-4 are ionic compounds having a melting point of 25° C. or more and 80° C. or less, which are solid at room temperature. G-5 is an ionic compound having a melting point of more than 80° C., which is solid at room temperature. Among the (H) polyether-modified siloxane compounds, H-1 to H-6 have a weight average molecular weight of 10,000 or less.
[0081] The composition and molecular weight (Mw) of the monomer constituting the second acrylic polymer shown in column (J) of Table 2 are shown in Table 4. The compound name of the abbreviation of each component used in Table 4 is shown in Table 5. In Table 4, the parts by weight of each component was calculated with the total of (a) being 100 parts by weight. Furthermore, in each of columns (b) to (c), the content ratio (parts by weight) calculated with the total of the second acrylic polymer being 100 parts by weight is shown in parentheses ( ).
[0082] [Table 4]
[0083] [Table 5]
[0084] (c) Among the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomers, I-1 to I-3 are monomers having a diester content of 0.2 wt% or less, and I-4 is a monomer having a diester content of 0.8 wt%. The value of n indicates the average repeat number of alkylene oxide.
[0085] <Test methods and evaluation> The surface protection films of Examples 1 to 6 and Comparative Examples 1 to 4 were each aged for 7 days in an atmosphere at a temperature of 23° C. and a humidity of 50% RH, and then evaluated by the following test method.
[0086] <Adhesive strength test method> The release film was peeled off to expose the adhesive layer, and the surface protection film was attached to the surface of a polarizing plate via the adhesive layer, and after leaving it for one day, it was autoclaved at 50°C and 5 atm for 20 minutes and left at room temperature for another 12 hours to prepare a sample for measuring adhesive strength. The obtained sample was peeled off in the 180° direction at a low speed (0.3 m / min) or a high speed (30 m / min) using a tensile tester, and the peel strength was measured and used as the adhesive strength. Here, the protective layer of the polarizer of the polarizing plate is polymethyl methacrylate (PMMA) having an AG-LR treatment layer.
[0087] <Surface resistivity test method> After aging the surface protection film and before bonding to a polarizing plate, the release film was peeled off to expose the adhesive layer, and the surface resistivity of the adhesive layer was measured using a resistivity meter Hiresta UP-HT450 (manufactured by Mitsubishi Chemical Analytech).
[0088] <Test method for peeling electrification voltage> The release film was peeled off to expose the pressure-sensitive adhesive layer, and the surface protection film was attached to a polarizing plate having a low refractive index layer formed on the adhesion surface using a composition for forming a low refractive index layer containing a fluorine compound. When the surface protection film was peeled off at 180° at a pulling speed of 30 m / min, the voltage (charged voltage) generated by the adhesion was measured using high-precision static electricity sensors SK-035 and SK-200 (manufactured by Keyence Corporation), and the maximum measured value was taken as the peeling charged voltage.
[0089] <Test method for stain resistance> A polarizing plate that had been subjected to low reflection (LR) surface treatment was attached to one side of a glass plate via an adhesive layer (double-sided adhesive tape) using a laminator. Then, a surface protective film was attached to the surface of the polarizing plate using a laminator. After attachment to the adherend, the plate was left in an atmosphere of 60°C temperature and 90% RH humidity for 2 days (48 hrs), and after removing it from the atmosphere, the surface protective film was peeled off after 1 day had passed, and the contamination state of the polarizing plate surface was visually observed. The criteria for judging the contamination resistance performance were as follows: no contamination on the surface of the polarizing plate was evaluated as "○", slight contamination was evaluated as "△", and contamination was evaluated as "×".
[0090] Table 6 shows the evaluation results for the surface protection films in Examples 1 to 6 and Comparative Examples 1 to 4. "Surface resistivity" is expressed as "m×10 +n " is expressed as "mE+n" (where m is any real value and n is a positive integer). The "Anti-soiling performance" column indicates the material (TAC, PMMA, PET) and surface treatment (untreated, AG treatment, LR treatment, AR treatment, AG-LR treatment) of the protective layer of the polarizer of the polarizing plate used in the test. "Plain" in "surface treatment" means untreated.
[0091] [Table 6]
[0092] The surface protection films of Examples 1 to 6 had an adhesive strength of 0.01 to 0.1 N / 25 mm at a low peel speed of 0.3 m / min to the adherend (polarizing plate), and an adhesive strength of 1.0 N / 25 mm or less at a high peel speed of 30 m / min, demonstrating excellent adhesive performance by achieving a balance between adhesive strength at low and high peel speeds. In addition, the surface protective films of Examples 1 to 6 had a surface resistivity of the pressure-sensitive adhesive layer of 1.0×10 +12 The peeling charge voltage of the adhesive layer against a low refractive index layer formed using a composition for forming a low refractive index layer containing a fluorine compound was in the range of +0.3 to -0.3 kV, indicating excellent antistatic performance. Furthermore, the surface protection films of Examples 1 to 6 were attached to an adherend, and then left in an atmosphere of 60°C and 90% RH for 48 hours. Even after being removed from the atmosphere and left for one day, there was no contamination of the adherend, i.e., various polarizing plates, and the films also had excellent contamination resistance. That is, the evaluation results shown in Table 6 demonstrate that the surface protection films of Examples 1 to 6 were able to solve the problems of the present invention.
[0093] The surface protection film of Comparative Example 1 (wherein the Tg of the monofunctional methacrylate monomer copolymerized with the first acrylic polymer was less than 0° C.) had poor stain resistance to adherends other than TAC. Furthermore, the surface protection film of Comparative Example 2 (containing an excess of hydroxyl-containing monomer copolymerized with the first acrylic polymer) had a large adhesive strength at a low peel speed and poor stain resistance to PMMA. In addition, the surface protection film of Comparative Example 3 (in which the first acrylic polymer did not contain a methacrylate monomer with a Tg of 0°C or higher, the proportion of carboxyl group-containing monomer was excessive, and the melting point of the antistatic agent exceeded 80°C) had high adhesive strength at a high peel speed, high peel charging voltage, and poor contamination resistance. Furthermore, the surface protection film of Comparative Example 4 (in Tables 1 and 2, the components (B) to (H) and (J) are the same as those of Example 3, except that the component (A) of Comparative Example 4 does not contain a methacrylate monomer with a Tg of 0°C or higher) had greater adhesive strength at a high peel speed, a higher peel electrification voltage, and poorer stain resistance against PMMA than the surface protection film of Example 3. From the comparison of the performance of the surface protection film of Comparative Example 4 with that of Example 3, it became clear that the inclusion of one or more monofunctional methacrylate monomers having a homopolymer Tg of 0°C or higher in the pressure-sensitive adhesive composition of the present invention contributes to achieving both (1) a balance of adhesive strength at low and high peel speeds, and (2) stain resistance. Further, in this way, the surface protection films of Comparative Examples 1 to 4 could not solve the problems of the present invention.
Claims
1. A pressure-sensitive adhesive composition comprising a first acrylic polymer, a crosslinking agent, and an ionic compound, The first acrylic polymer is (A) 100 parts by weight of a total of at least two or more alkyl (meth)acrylates having an alkyl group with a carbon number of C1 to C10, (B) 1.0 to 6.0 parts by weight of at least one copolymerizable monomer containing a hydroxyl group; (C) 0.01 to 0.6 parts by weight of at least one copolymerizable monomer containing a carboxyl group; an acrylic polymer comprising a copolymer having an acid value of 0.1 to 1.0 and a weight average molecular weight of more than 300,000 and not more than 1,000,000, The ionic compound has a melting point of 25 to 80° C. the pressure-sensitive adhesive composition contains a trifunctional or higher isocyanate compound as the crosslinking agent, A surface protection film obtained by laminating a 15 μm thick adhesive layer obtained by crosslinking the adhesive composition on one side of a 38 μm thick polyester film is attached to the surface of a polarizing plate, and then the surface protection film is peeled off from the polarizing plate, the adhesive composition having an adhesive strength of 0.01 to 0.1 N / 25 mm at a low peeling speed of 0.3 m / min and an adhesive strength of 1.0 N / 25 mm or less at a high peeling speed of 30 m / min.
2. (A) contains 50 parts by weight or more of 2-ethylhexyl acrylate and 5 to 40 parts by weight of one or more monofunctional methacrylate monomers having a homopolymer Tg of 0° C. or higher out of a total of 100 parts by weight of at least two or more alkyl (meth)acrylates having an alkyl group with a carbon number of C1 to C10; The pressure-sensitive adhesive composition according to claim 1, wherein the monofunctional methacrylate monomer having a homopolymer Tg of 0° C. or higher is at least one selected from the group consisting of n-butyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, ethyl methacrylate, and methyl methacrylate.
3. the pressure-sensitive adhesive composition further comprises a second acrylic polymer, The second acrylic polymer is (a) at least one (meth)acrylic acid ester monomer having an alkyl group with a carbon number of 1 to 18; (b) at least one copolymerizable monomer containing a hydroxyl group; (c) at least one polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer; The pressure-sensitive adhesive composition according to claim 1 or 2, characterized in that the pressure-sensitive adhesive composition contains 0.1 to 5.0 parts by weight of the second acrylic polymer per 100 parts by weight in total of the at least two or more kinds of alkyl (meth)acrylates (A) having a carbon number of C1 to C10 in the alkyl group.
4. The pressure-sensitive adhesive composition is a pressure-sensitive adhesive composition for forming a pressure-sensitive adhesive layer used in a surface protection film for a polarizing plate, The pressure-sensitive adhesive composition according to any one of claims 1 to 3, characterized in that the protective layer of the polarizer of the polarizing plate is one selected from the group consisting of a TAC-based film, a PMMA-based film, and a PET-based film, and the surface treatment applied to the surface of the protective layer of the polarizer of the polarizing plate is one selected from the group consisting of an untreated film, an AG treatment, a LR treatment, an AR treatment, an AG-LR treatment, and an AG-AR treatment.
5. The pressure-sensitive adhesive composition according to any one of claims 1 to 4, characterized in that a cation of the ionic compound is pyridinium, and the pressure-sensitive adhesive composition contains the ionic compound as an essential component in a ratio of 0.01 to 10 parts by weight per 100 parts by weight of the first acrylic polymer.
6. The pressure-sensitive adhesive layer obtained by crosslinking the pressure-sensitive adhesive composition has a surface resistivity of 1.0×10 +12 Ω / □ or less, the peeling electrification voltage of the pressure-sensitive adhesive layer relative to a low refractive index layer formed using a composition for forming a low refractive index layer containing a fluorine compound is within the range of +0.3 to −0.3 kV; The pressure-sensitive adhesive composition according to any one of claims 1 to 5, characterized in that the pressure-sensitive adhesive composition is free from contamination when it is attached to a polarizing plate in which the surface substrate is one selected from the group consisting of a TAC-based film, a PMMA-based film, and a PET-based film, and the surface treatment applied to the surface of the surface substrate is one selected from the group consisting of an untreated film, an AG treatment, a LR treatment, an AR treatment, an AG-LR treatment, and an AG-AR treatment, the polarizing plate is left for two days in an atmosphere having a temperature of 60°C and a humidity of 90%, taken out, and then peeled off after one day has passed.
7. the (B) hydroxyl group-containing copolymerizable monomer is at least one selected from the group consisting of 8-hydroxyoctyl(meth)acrylate, 6-hydroxyhexyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxyethyl(meth)acrylate, N-hydroxy(meth)acrylamide, N-hydroxymethyl(meth)acrylamide, and N-hydroxyethyl(meth)acrylamide, The pressure-sensitive adhesive composition according to any one of claims 1 to 6, wherein the (C) carboxyl group-containing copolymerizable monomer is at least one selected from the group consisting of (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl maleic acid, carboxypolycaprolactone mono(meth)acrylate, and 2-(meth)acryloyloxyethyl tetrahydrophthalic acid.
8. the pressure-sensitive adhesive composition contains a crosslinking retarder and a crosslinking catalyst other than a tin compound; The crosslinking retarder is a keto-enol tautomer compound, The crosslinking retarder is contained in an amount of 0.1 to 300 parts by weight based on 100 parts by weight of the first acrylic polymer, the crosslinking catalyst is at least one metal chelate compound selected from the group consisting of an aluminum chelate compound, a titanium chelate compound, and an iron chelate compound; The crosslinking catalyst is contained in an amount of 0.001 to 0.5 parts by weight based on 100 parts by weight of the first acrylic polymer, 8. The pressure-sensitive adhesive composition according to claim 1, wherein a ratio of the crosslinking retarder to the crosslinking catalyst is 80 to 1,000 parts by weight.
9. The pressure-sensitive adhesive composition according to any one of claims 1 to 8, characterized in that the pressure-sensitive adhesive composition contains 0.01 to 0.5 parts by weight of a polyether-modified siloxane compound having an HLB value of 6 to 12 and a weight average molecular weight of 10,000 or less, relative to 100 parts by weight of the first acrylic polymer.
10. The second acrylic polymer is (a) for a total of 100 parts by weight of at least one (meth)acrylic acid ester monomer having an alkyl group carbon number of C1 to C18, (b) 2.0 to 12.0 parts by weight of at least one copolymerizable monomer containing a hydroxyl group; (c) a copolymer having a weight average molecular weight of more than 300,000 and not more than 800,000, obtained by copolymerizing 1 to 30 parts by weight of at least one polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer; The pressure-sensitive adhesive composition according to claim 3, wherein a ratio (b-1) / (B-1) of a total part by weight of the at least one or more kinds of (B) copolymerizable monomers containing a hydroxyl group contained in the first acrylic polymer relative to a total of 100 parts by weight of the first acrylic polymer to a total part by weight of the at least one or more kinds of (b) copolymerizable monomers containing a hydroxyl group contained in the second acrylic polymer relative to a total of 100 parts by weight of the second acrylic polymer is within a range of 1.0 to 2.
0.
11. the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer has an average repeat number of alkylene oxides constituting the polyalkylene glycol chain of 3 to 14; the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer has a diester content of 0.2% or less, The pressure-sensitive adhesive composition according to claim 3 or 10, characterized in that the polyalkylene glycol chain-containing mono(meth)acrylic acid ester monomer is at least one selected from the group consisting of polyalkylene glycol mono(meth)acrylate, methoxypolyalkylene glycol (meth)acrylate, and ethoxypolyalkylene glycol (meth)acrylate, in an amount of 1 to 50 parts by weight per 100 parts by weight of the second acrylic polymer.
12. 12. A pressure-sensitive adhesive film comprising a resin film and a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition according to claim 1 on one side of the resin film.
13. A surface protection film using the pressure-sensitive adhesive film according to claim 12.
14. A surface protection film for a polarizing plate, comprising the pressure-sensitive adhesive film according to claim 12.
15. 12. An optical film with a pressure-sensitive adhesive layer, comprising an optical film and a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition according to claim 1 laminated on at least one surface of the optical film.
16. The pressure-sensitive adhesive film according to claim 12 , wherein one surface of the resin film opposite to the surface on which the pressure-sensitive adhesive layer is formed is subjected to an antistatic treatment and an antifouling treatment.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition for heat-resistant adhesive film, pressure-sensitive adhesive for heat-resistant adhesive film obtained by crosslinking the same, heat-resistant adhesive film for masking and method for using the heat-resistant adhesive film
JP2013177568A
Adhesive composition and optical member surface protective film
JP2015160908A
Surface protective film and optical member
JP2018154838A
Antistatic surface protective film
JP2018165370A
Adhesive composition, and adhesive film and surface protective film using the same
JP2020079333A