Method for producing fired pellets for reduction
By formulating fired pellets with specific M.Fe and viscous slag components, the method addresses clustering in solid reduction furnaces, improving operational efficiency and reducing slag fusion without additional coatings.
Patent Information
- Application Number
- JP2024138920
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for preventing clustering in solid reduction furnaces are insufficient and require additional coating processes, increasing costs and needing specialized equipment, while failing to effectively address the issue of low-melting slag contact and fusion.
Producing fired pellets with a specific composition containing 4-24% M.Fe and a highly viscous slag component (Al2O3+MgO+SiO2) in a ratio of 0.07 to 0.12 relative to total iron (T.Fe), ensuring porosity of 20% or more, and using iron ores with an LOI of 5% or more to prevent slag fusion and clustering.
The method effectively reduces slag fusion and clustering in solid reduction furnaces by controlling the composition and porosity of the pellets, enhancing operational efficiency and reducing the need for additional coatings.
Smart Images

Figure 2024149831000001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a fired pellet for reduction effective for use in a solid reduction furnace and a method for producing the same.
Background Art
[0002] In recent years, various technological developments have been carried out to reduce the emissions of CO2 in order to avoid global warming caused by its increase.
[0003] Under such circumstances, in the field of the iron and steel industry, an iron-making method using a solid reduction furnace, which is a hydrogen-based reduction process, has been attracting attention, and research on the fired pellets used in this method has been advanced. By the way, in the solid reduction furnace, when the charged raw material (fired pellet) passes through the high-temperature region in the furnace, when the hematite phase in the fired pellet is reduced and changes to the magnetite phase, it is accompanied by volume expansion and causes a pulverization phenomenon. In addition to the contact and fusion of metallic irons, it is known that the contact and fusion of low-melting-point slags are caused. As a result, it is known that clustering occurs in the furnace, or a hanging phenomenon occurs in which the pellets in the furnace cannot move and cannot be taken out from the bottom of the furnace. In particular, in a solid reduction furnace that performs reduction based on hydrogen, this clustering is a very large problem to be solved.
[0004] Under such circumstances, several prior arts have been proposed for the purpose of preventing clustering observed in the above-mentioned solid reduction furnace. For example, Patent Document 1 proposes a method of coating the pellet surface with Ca(OH)2 or Mg(OH)2. Patent Document 2 proposes a method of preventing reduction pulverization by coating the surface of a fired lump ore (pellet) with a granular solid fuel, and a method of obtaining a fired pellet with less swelling. And Patent Document 3 aims to prevent the occurrence of clustering in a solid reduction furnace, reduce heat loss, and improve operation efficiency by coating the surface of a fired pellet with a cement-blended iron ore. Furthermore, Patent Document 4 proposes a technique of coating a substance containing a calcium iron compound composed of CaxFeyOz (1 < y / x ≦ 2; 1 ≦ z). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 59-10411 [Patent Document 2] Japanese Patent Application Publication No. 62-37325 [Patent Document 3] Japanese Patent Application Publication No. 63-262426 [Patent Document 4] JP 2017-119910 A Summary of the Invention [Problem to be solved by the invention]
[0006] Each of the above-mentioned conventional techniques (Patent Documents 1-4) is a method for reducing contact between metallic iron particles after reduction, which is a cause of clustering observed near the high temperature range (500 to 600°C) in a solid reduction furnace such as a shaft furnace, mainly by interposing a nonmetallic component. However, according to the research of the inventors, the above-mentioned conventional techniques for preventing clustering are insufficient, and there are problems such as the need to adopt a separate coating process for nonmetallic components, which increases costs, and the need to add dedicated equipment.
[0007] Therefore, the object of the present invention is to propose a method for producing sintered pellets for use in a solid reduction furnace, which contains a predetermined amount of M.Fe and also contains a highly viscous slag component, thereby reducing the chance of contact between low-melting-point slags and preventing fusion, thereby effectively preventing clustering. [Means for solving the problem]
[0008] The present invention is a technology developed to solve the above-mentioned problems of the conventional technology and to achieve the above-mentioned object, and proposes a method for producing sintered pellets for reduction, in which the ratio of highly viscous slag components (Al2O3+MgO+SiO2) to total Fe (T.Fe) satisfies the following formula (1), by using a mixed raw material containing M.Fe in an amount of 4 mass% or more and 24 mass% or less, and granulating and sintering the mixed raw material. Note (Al2O3+MgO+SiO2) / T.Fe≧0.07 ···(1) Where Al2O3: Concentration of Al2O3 in the fired pellet (mass%) MgO: MgO concentration in the fired pellets (mass%) SiO2: SiO2 concentration in the fired pellets (mass%) T.Fe: T.Fe concentration in the fired pellets (mass%)
[0009] In the present invention, the method for producing the sintered pellets for reduction is as follows: (a) The ratio of high-viscosity slag components (Al2O3+MgO+SiO2) to total Fe (T.Fe) satisfies the following formula (2); Note (Al2O3+MgO+SiO2) / T.Fe≧0.12 ···(2) Where Al2O3: Concentration of Al2O3 in the fired pellet (mass%) MgO: MgO concentration in the fired pellets (mass%) SiO2: SiO2 concentration in the fired pellets (mass%) T.Fe: T.Fe concentration in the fired pellets (mass%) (b) having a porosity of 20% or more; (e) the mixed raw material is reduced iron having a particle size of 3 mm or less that has been reduced in a solid reduction furnace; (f) the reduced iron contains 78 mass % or more of M.Fe; It is believed that this provides a more preferred embodiment. Effect of the Invention
[0010] According to the manufacturing method of the sintered pellets for reduction of the present invention having the above-mentioned configuration, by containing M.Fe and containing a relatively large amount of high viscosity slag components (Al2O3, MgO, SiO2) with respect to the total iron, it is possible to reduce the generation of low melting point slag due to FeO and its fluidity during reduction in a solid reduction furnace. As a result, it is possible to prevent contact and fusion between pellets due to the presence of such slag, and thus it is possible to effectively prevent the above-mentioned clustering in the reduction furnace, which is a problem. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a diagram showing the relationship between (Al2O3+MgO+SiO2) / T.Fe and LOI for Australian iron ore, which is an iron-containing raw material to be blended. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The solid reduction furnace used in the present invention is a furnace that uses hydrogen gas or the like as a reducing gas, charges sintered pellets for reduction into the furnace, and reduces the pellets to a reduction ratio of 90% or more. In the operation of this solid reduction furnace, the properties of the raw material charged into the furnace, i.e., the sintered pellets, are important.
[0013] For the fired pellets, it is most important to prevent clustering caused by contact and mutual fusion of pellets in the high temperature region (500-800°C) in the solid reduction furnace. In response to such a demand, in the present invention, the relationship between iron-containing raw materials such as iron oxides such as iron ore, iron sulfide, and iron-making dust, as well as metallic iron (M.Fe), and highly viscous slag components was examined. As a result, it was found that it is preferable to properly manage the relationship between the raw materials and the highly viscous slag components, from the viewpoint of the fluidity of the raw materials in the furnace. In other words, by always producing highly viscous slag in the furnace, undesirable flow in the high temperature region can be suppressed, and therefore, the fusion of slag can be prevented, and clustering can be prevented.
[0014] As described above, in the present invention, it has been found to be effective to make the iron-containing raw material and the auxiliary raw materials to be mixed contain a certain proportion of a highly viscous slag component.
[0015] Focusing on Al2O3, MgO, and SiO2 as components that can become highly viscous slag, when the total amount of these components is maintained at a specific ratio to the total iron (T·Fe), it becomes possible to effectively prevent the slag generated in the furnace from melting together.
[0016] This means that the composition of the sintered pellets for reduction must contain a certain ratio of the highly viscous slag components (Al2O3+MgO+SiO2) relative to the total iron (T·Fe) in the iron-containing raw materials; in other words, the sintered pellets must satisfy the relationship in formula (1) below. Note (Al2O3+MgO+SiO2) / T.Fe≧0.07 ···(1)
[0017] In the above formula (1), Al2O3 is the component concentration (mass%) of Al2O3 in the sintered pellets for reduction, MgO is the component concentration (mass%) of MgO in the sintered pellets for reduction, SiO2 is the component concentration (mass%) of MgO in the sintered pellets for reduction, and T.Fe is the total Fe concentration (mass%) in the sintered pellets for reduction.
[0018] In the present invention, from the viewpoint of preventing contact and fusion between slags in the high temperature region in the furnace, a more preferable relationship between the above-mentioned high viscous slag components (Al2O3+MgO+SiO2) and total iron (T.Fe) is as shown in the following formula (2), in which the amount of high viscous slag components is greater. Note (Al2O3+MgO+SiO2) / T.Fe≧0.12 ···(2)
[0019] In the above formula (2), Al2O3 is the component concentration (mass%) of Al2O3 in the sintered pellets for reduction, MgO is the component concentration (mass%) of MgO in the sintered pellets for reduction, SiO2 is the component concentration (mass%) of MgO in the sintered pellets for reduction, and T.Fe is the total Fe concentration (mass%) in the sintered pellets for reduction.
[0020] In the present invention, the total Fe (T.Fe) in the iron-containing raw material is the total value of the iron concentration consisting of metallic iron (M.Fe) and iron compounds (iron oxide, iron sulfide, calcium ferrite, etc.), while the highly viscous slag component is the total value of the Al2O3 concentration, MgO concentration, and SiO2 concentration contained in the iron-containing raw materials such as iron ore and steelmaking dust, auxiliary raw materials (limestone, quicklime, dolomite, etc.), and binders (bentonite, etc.).
[0021] The Al2O3 concentration, MgO concentration, and SiO2 concentration can be determined by measuring the Al concentration, Mg concentration, and Si concentration by elemental analysis such as fluorescent X-rays, and multiplying the concentration by the molecular weight / atomic weight, respectively. Specifically, for example, the Al2O3 concentration can be determined by multiplying the Al concentration measured by elemental analysis such as fluorescent X-rays by Al2O3 molecular weight / Al atomic weight = 101.96 / 26.98 = 3.779.
[0022] Next, for the reduction firing pellets according to the present invention, it is also important to control the porosity of the pellets. That is, by making the reduction firing pellets porous (20% or more, preferably 30% or more), the number of contact points between the pellets can be reduced, which reduces contact between the metallic iron particles and prevents them from fusing together, which in turn contributes to preventing the above-mentioned clustering. In this regard, a porosity of less than 20% is not effective in preventing fusing. The upper limit is about 60% from the viewpoint of strength.
[0023] Next, a method for producing the fired pellets according to the present invention will be described. In producing the fired pellets for reduction according to the present invention, in order to realize the above-mentioned relationship between the highly viscous slag components (Al2O3+MgO+SiO2) and the total iron (T.Fe) in the resulting fired pellets, for example, it is possible to use a blend of one or more types of iron ore having the above-mentioned component composition, and to select and use two or more types of iron ore that show the above-mentioned relationship. For example, one or more types of iron ore (brands) shown in Figure 1 are blended from Australian iron ores, and binders and auxiliary materials such as bentonite and quicklime are added as necessary, and then granulated.
[0024] When the above-mentioned fired pellets are charged into a solid reduction furnace and reduced, it is desirable that the pellets have properties that do not cause the clustering in the high-temperature reducing atmosphere in the furnace. For example, by selecting and blending some of the iron ores (A to Z) shown in Fig. 1 so that the LOI (Loss on Ignition) value is 5% or more, clustering can be more effectively reduced. The reason for this is that when the LOI is dissociated and vaporized during the pellet firing process and dissipates outside the pellet, the volume of the mineral phase remaining in the pellet shrinks, causing voids between the mineral phases.
[0025] In the manufacturing method according to the present invention, in order to realize the LOI of the iron-containing raw material of ≧5%, it is preferable to make the iron ore used have an LOI of ≦2% by performing a pretreatment such as a crystal water removal treatment in advance. The reason for this is that many iron-containing raw materials such as raw iron ore contain a lot of crystal water, and the pellets often burst due to the water vapor generated due to the crystal water during granulation, so that it is necessary to raise the temperature slowly.
[0026] In addition, in the pretreatment for removing the water of crystallization, it is desirable to manage the evaluation of the LOI using a measured value at the exit side (discharge position) of a granulator such as a rotary kiln.
[0027] (Example) Example 1: This example (including comparative examples) clarifies how the relationship between the T.Fe of the firing pellets for reduction and the highly viscous slag components (Al2O3+MgO+SiO2) affects clustering in a solid reduction furnace.
[0028] The iron-containing raw materials used in the experiment, i.e., iron ore, were mainly one or more of the Australian iron ores (A to Z) shown in Figure 1, and auxiliary raw materials and reagents (commercially available Al2O3 reagents, etc.) were used as needed. An example of the blend is shown in Table 1.
[0029] All raw materials, including one or more of the Australian raw materials mentioned above (examples shown in Figure 1) (A to Z), were pulverized in a ball mill, then granulated into pellets of 9 to 16 mm in size using a pelletizer while adding moisture. The resulting pellets were placed in a dryer and dried at 110°C for 24 hours, then placed in an electric furnace, heated at 7°C / min, held at 1250°C for 10 hours, and then cooled at a rate of 7°C / min. The resulting fired pellets shown in Table 1 were evaluated using porosity and clustering index.
[0030] (Clustering evaluation test) 500 g of sample was placed in a 100φ vertical cylindrical furnace and heated to 1000°C in a N2 atmosphere. When the temperature reached 1000°C, the reducing gas was added at 24 L / min, H2:N2 = 20:80 (vol%), and a load of 1 kg / cm was applied. 2 The pellets were then held at 400° C. for 3 hours and cooled in a N2 atmosphere to produce reduced iron. The pellets were then sieved through a 16 mm sieve, the maximum size of which is 16 mm, and their weight was measured (Wa(g)). The sieved pellets were placed in a type I testing machine (cylindrical container (132 mmφ×700 mL)) and rotated at 30 rpm for 5 minutes, after which the amount of the pellets sieved through the 16 mm sieve, Wb(g), was evaluated.
[0031] (Porosity) The porosity of the sintered pellets was evaluated by measuring the apparent density and then the true density. It was confirmed that in Examples 1 to 5 in which (Al2O3+MgO+SiO2) / T.Fe was 0.07 or more, the clustering index was less than 7 and the sintered pellets had good properties.
[0032] [Table 1]
[0033] The following Table 2 shows the component compositions of the fired pellets obtained in Examples 1 and 2 of Table 1.
[0034] [Table 2]
[0035] Example 2: Next, a test was carried out to evaluate whether the sample of Example 5 shown in Table 1 could be granulated and fired without being damaged by subjecting the sample to a pretreatment for removing water of crystallization. The temperature rise rate was 200° C. / min.
[0036] As a result, it was found that whether or not the water of crystallization is removed by the dewatering treatment determines whether or not the water of crystallization is removed. For example, if a large number of pores remain in the dewatered-crystallization ore, it may burst. On the other hand, if the water of crystallization is sufficiently removed, the ore will not burst. Furthermore, it was found that if the LOI of the ore before the treatment is sufficiently high, it is possible to produce a product of good quality even if the LOI of the ore after the dewatering-crystallization treatment is low.
[0037] [Table 3]
[0038] Example 3: The reduced iron (sample at the time of measuring Wa) obtained by the same method as in Comparative Example 2 of Example 1 (clustering evaluation test) was pulverized to a particle size of 3 mm or less, mixed with the raw material before firing of Comparative Example 2, and fired pellets were produced by the method of Example 1 using the pulverized pellets. The pellet (crushing) strength of the produced fired pellets was measured. The results are shown in Table 4. Note that "M.Fe" in Table 4 is derived from M.Fe contained in the reduced iron, and Examples 10 to 12 used reduced iron with M.Fe=78 mass%, and Example 13 used reduced iron with M.Fe=80 mass%. As a result, it was found that the pellet strength was improved by mixing M.Fe into the raw material. Clustering is promoted by increasing the amount of powder, so clustering can be suppressed by improving the strength of the fired pellets. In addition, it is considered that the strength of the fired pellets is improved by blending M.Fe into the raw material because the reduced iron powder is oxidized and heat is generated during firing of the fired pellets, which promotes adhesion between adjacent particles. In addition, in Example 13, reduced iron (sample at the time of measuring Wa) obtained by the same method as in Example 1 of Example 1 (clustering evaluation test) was pulverized to a particle size of 3 mm or less, mixed with the raw material of Example 1 before sintering, and sintered pellets were manufactured by the method of Example 1 using this, and high strength was obtained.
[0039] [Table 4] [Industrial Applicability]
[0040] The method for producing solid reduced sintered pellets according to the present invention is a technology developed primarily for application to hydrogen-based direct reduction processes, but it can also be used as a raw material for blast furnaces and the like.
Claims
1. Highly viscous slag components (Al 2 O 3 + MgO + SiO 2 A method for producing sintered pellets for reduction, comprising the steps of: using a mixed raw material containing 4 mass% or more and 24 mass% or less of M.Fe in the production of sintered pellets for reduction, the mixed raw material being granulated and sintered ... Note (Al 2 O 3 +MgO+SiO 2 ) / T.Fe≧0.07 ・・・(1) However, Al 2 O 3 : Al in fired pellets 2 O 3 Concentration of components (mass%) MgO: MgO component concentration (mass%) in the fired pellet SiO 2 : SiO in the fired pellets 2 Concentration of components (mass%) T.Fe: Component concentration (mass%) of T.Fe in fired pellets
2. Highly viscous slag components (Al 2 O 3 + MgO + SiO 2 2. The method for producing sintered pellets for reduction according to claim 1, characterized in that the ratio of the above-mentioned components satisfies the following formula (2): Note (Al 2 O 3 +MgO+SiO 2 ) / T.Fe≧0.12 ・・・(2) However, Al 2 O 3 : Al in fired pellets 2 O 3 Concentration of components (mass%) MgO: MgO component concentration (mass%) in the fired pellet SiO 2 : SiO in the fired pellets 2 Concentration of components (mass%) T.Fe: Component concentration (mass%) of T.Fe in fired pellets
3. 3. The method for producing sintered pellets for reduction according to claim 1, wherein the mixed raw material is reduced iron having a particle size of 3 mm or less that has been reduced in a solid reduction furnace.
4. 4. The method for producing sintered pellets for reduction according to claim 3, wherein the reduced iron contains 78 mass % or more of M.Fe.
Citation Information
Patent Citations
Fired pellet for reduction and method for producing the same
JP2023002956A
Controlling device of wall thickness in mandrel mill
JP1984010411A
Calcined lump ore and its production
JP1987037325A
Raw material for iron manufacture
JP1988262426A
Reduction raw material, and method for producing reduction raw material
JP2017119910A