Method for producing granular carrier

The reverse-phase suspension polymerization of carboxyalkyl cellulose salt in a hydrophobic container addresses the issues of non-spherical and costly cellulose-based SAPs, producing high-yield, spherical, and transparent granular carriers with improved functionality and reduced environmental impact.

JP2024150221APending Publication Date: 2024-10-23S T CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023063532
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Existing cellulose-based superabsorbent polymers (SAPs) used in granular gel preparations for fragrance and deodorant compositions are non-spherical, non-uniform, and costly, leading to inefficient air flow, poor aesthetics, and high raw material loss, while polyacrylic acid-based SAPs pose environmental concerns due to non-biodegradability and high energy consumption.

Method used

A method involving reverse-phase suspension polymerization of carboxyalkyl cellulose salt in a low polar organic solvent using a hydrophobic container, controlling viscosity and crosslinking agent ratios to produce spherical, uniform, and transparent granular carriers with high water absorption and biodegradability.

Benefits of technology

The method enables the production of high-yield, spherical, and transparent granular carriers with excellent strength and uniform size, enhancing drug functionality and aesthetics, while reducing raw material loss and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150221000001_ABST
    Figure 2024150221000001_ABST
Patent Text Reader

Abstract

To provide a technology capable of easily producing a granular carrier that has both high water absorbency and biodegradability, and has a substantially spherical shape, a uniform particle size, and excellent strength and transparency while reducing raw material loss and improving yield.SOLUTION: There is provided a method for producing a granular carrier comprising gel particles containing a crosslinked body of a carboxyalkyl cellulose salt, the method including: dissolving a specific carboxyalkyl cellulose and / or a salt thereof in an aqueous alkali solution, preparing a carboxyalkyl cellulose salt aqueous solution, adding a crosslinking agent to the aqueous solution to obtain a mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent, mixing the mixture with a specific low-polarity organic solvent in a first container, and obtaining a suspension in which the mixture is dispersed in the low-polarity organic solvent; and allowing cross-linking polymerization to proceed in the suspension to form dispersed particles containing a cross-linked body of the carboxyalkyl cellulose salt, wherein the first container has a hydrophobic inner surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a granular carrier. [Background technology]

[0002] Superabsorbent polymers (SAP) absorb water upon contact with water and instantly become a transparent hydrated gel. This gel is one of the functional polymers that does not release water even when pressure is applied and retains water. Superabsorbent polymers have a wide range of uses, for example, in the field of sanitary products, they are used as highly absorbent substances in absorbent articles such as paper diapers and sanitary napkins for women. In addition, superabsorbent polymers are also used as carriers in gel preparations that absorb and support aqueous liquid compositions containing pharmaceuticals such as fragrances and deodorants. Gel preparations containing carriers made of such superabsorbent polymers are widely used in stationary air fresheners and deodorants because there is no risk of liquid spilling from the container and they have excellent design.

[0003] Currently, polyacrylic acid-based SAP is the mainstream of superabsorbent polymers (SAPs) from the viewpoints of ease of synthesis, cost, etc. However, because polyacrylic acid-based SAPs are made from petroleum, there is a problem that the production cost is affected by fluctuations and increases in crude oil prices, and the amount of CO emitted during production and disposal is also high. 2 In particular, when used for diapers, SAP is disposed of in a water-absorbed state, so incineration of acrylic acid-based SAP requires a large amount of energy and emits CO 2 In addition, when acrylic acid-based SAP is disposed of in landfills, problems such as soil contamination arise because it is not biodegradable.

[0004] The fact that polyacrylic acid-based SAPs are the mainstream of superabsorbent polymers (SAPs) may be a cause of environmental problems. As the demand for disposable diapers is expected to rapidly increase in emerging countries in the future, it is desirable to use biodegradable natural polymers as superabsorbent polymers. In this situation, superabsorbent polymers using plant-derived raw materials such as polysaccharides have been proposed.

[0005] For example, Patent Documents 1 to 3 propose a cellulose-based SAP consisting of a crosslinked polymer of carboxymethyl cellulose (CMC) or a CMC salt as a biodegradable, highly water-absorbent polymer to replace polyacrylic acid-based SAP. This CMC is a water-soluble cellulose derivative, and is synthesized by etherifying the hydroxyl groups of cellulose with chloroacetic acid or the like. Its aqueous solution exhibits anionic properties and has high viscosity and excellent dispersibility, and is therefore widely used as a thickener, dispersant, and stabilizer.

[0006] CMC is neither toxic nor allergenic, and is also used as a food additive and a pharmaceutical binder. Its physical properties depend strongly on the degree of substitution (DS), which is the average number of carboxymethyl groups substituted per glucose residue, and in one example, it is said to be water-soluble when DS>0.55. For example, Patent Document 1 uses CMC and CMC salts with a degree of substitution of 1.1 or more (see Claim 1, etc.), and Patent Document 2 uses CMC salts with a degree of substitution of 0.65 to 1.4 (see Claim 1, etc.). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-140534 A [Patent Document 2] International Publication No. 2012 / 147255 [Patent Document 3] JP 2008-285611 A Summary of the Invention [Problem to be solved by the invention]

[0008] Stationary products in which gel preparations such as fragrance compositions and deodorant compositions are filled in containers are on the market. Many of these products use granular gel preparations in which liquid compositions containing various chemicals are supported on gel carriers made of highly water-absorbent polymers. Many of these products are designed to have the surface of the granular gel preparation exposed to air to exert the functions of the various chemicals supported on the gel carriers. That is, when the chemical supported on the gel carrier is a volatile chemical such as a fragrance, the surface of the granular gel preparation is exposed to air to volatilize the volatile chemical. Also, when the chemical supported on the gel carrier is a non-volatile chemical, for example, a deodorant that uses a chemical reaction to deodorize, the surface of the granular gel preparation is exposed to air to bring the malodorous molecules into contact with the non-volatile deodorant, and the malodorous molecules are decomposed by a chemical reaction to deodorize.

[0009] For this reason, in order to allow the drug carried by the gel carrier in the granular gel preparation to function efficiently, it is desirable that air flow occurs easily when the granular gel preparation is filled in a container. In order to facilitate air flow, it is preferable that the gaps between the granular gel preparations are uniform and have a certain degree of size. For this reason, it is desirable that the granular gel preparations are uniform in size and nearly spherical in shape.

[0010] In addition, considering that granular gel preparations such as fragrance compositions and deodorant compositions are distributed as stationary products filled in containers, it is desirable for the granular gel preparation to have excellent gel strength. In addition, in such products, the granular gel preparation is often filled in a transparent or semitransparent container and can be seen from the outside. The granular gel preparation having a uniform size and a nearly spherical shape is preferable from the viewpoint of aesthetics, in addition to enabling the above-mentioned drugs to function efficiently. From the viewpoint of aesthetics, it is even more preferable that the granular gel preparation also has excellent transparency.

[0011] On the other hand, as a conventional method for producing cellulose-based SAP, a method of polymerizing CMC or a CMC salt in an aqueous solution using a crosslinking agent (hereinafter referred to as "aqueous solution polymerization") is known. For example, a crosslinking agent is added to a CMC salt aqueous solution in which CMC or a CMC salt is dissolved in a sodium hydroxide aqueous solution, and a crosslinking reaction is carried out to obtain a hydrogel in which the aqueous solution is uniformly gelled. The hydrogel is pulverized and undergoes a sorting process such as classification to form a cellulose-based SAP (for example, see paragraph 0035 of Patent Document 1, paragraph 0024 of Patent Document 2, and paragraph 0044 of Patent Document 3).

[0012] Crushed gel particles (crushed gel) finely granulated by crushing are typically fragmented with sharp edges, and most of them are irregularly shaped particles that are difficult to call spherical. When such cellulose-based SAP consisting of a collection of small, non-spherical, non-uniform gel fragments is filled in a container, the gel particles are in close contact with each other, making it difficult for air to flow. In addition, cellulose-based SAP consisting of a collection of such non-uniform small gel fragments is not preferable from the viewpoint of aesthetics.

[0013] In addition, since cellulosic SAP produced using CMC or a CMC salt is relatively expensive compared to polyacrylic acid-based SAP, it is desirable to develop a technology that can reduce raw material losses and increase yields.

[0014] The present invention aims to provide a technology for easily and efficiently producing a granular carrier that is both highly absorbent and biodegradable, has a roughly spherical shape, a uniform particle size, and excellent strength and transparency, while reducing raw material loss. [Means for solving the problem]

[0015] According to one aspect of the present invention, there is provided a method for producing a granular carrier comprising gel particles containing a crosslinked product of a carboxyalkyl cellulose salt, comprising the steps of: preparing a carboxyalkyl cellulose salt aqueous solution by dissolving a carboxyalkyl cellulose and / or a salt thereof having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1 mass% aqueous solution at 25°C in an alkaline aqueous solution; adding a crosslinking agent to the aqueous carboxyalkyl cellulose salt solution to obtain a mixture of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent; mixing the mixture with a low-polarity organic solvent in a first container to obtain a suspension in which the mixture is dispersed in the low-polarity organic solvent; and Crosslinking polymerization of the carboxyalkyl cellulose salt is allowed to proceed in the suspension to form dispersed particles containing a crosslinked body of the carboxyalkyl cellulose salt. The low-polarity organic solvent has a relative dielectric constant of 10 or less at 25° C. and a kinetic viscosity of 10 mm at 37.8° C. 2 / s or more, and the first vessel has a hydrophobic inner surface.

[0016] According to another aspect of the present invention, there is provided a manufacturing method according to the above aspect, wherein the inner surface of the first container is made of a material including at least one of tetrafluoroethylene resin, perfluoroalkoxyalkane, polypropylene, polystyrene, polymethylpentene, and polyethylene.

[0017] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the mixture of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent is prepared in the first container, and the mixture is mixed with the low-polarity organic solvent by adding the low-polarity organic solvent to the mixture contained in the first container.

[0018] According to yet another aspect of the present invention, there is provided the production method according to the above aspect, wherein the reaction is carried out in the first vessel until dispersed particles containing a crosslinked product of the carboxyalkyl cellulose salt are formed.

[0019] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the mixture of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent is prepared in a second container, and the mixture is mixed with the low-polarity organic solvent by adding the mixture to the low-polarity organic solvent contained in the first container.

[0020] According to yet another aspect of the present invention, there is provided the production method according to any of the above aspects, wherein the temperature of the low-polarity organic solvent when the low-polarity organic solvent is mixed with the mixture is within the range of 15°C to 43°C.

[0021] According to yet another aspect of the present invention, there is provided the production method according to any one of the above aspects, wherein the low-polarity organic solvent is liquid paraffin or silicone oil.

[0022] According to yet another aspect of the present invention, the low-polarity organic solvent has a kinetic viscosity of 10 mm at 37.8° C. 2 / s or more 100mm 2 / s or less.

[0023] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the viscosity of the carboxyalkyl cellulose and / or salt thereof is 5 mPa·s or more and 100 mPa·s or less.

[0024] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the mass ratio (X / Y) of the carboxyalkyl cellulose and / or salt thereof (X) to the crosslinking agent (Y) in the mixture is in the range of 10 / 2 to 10 / 5.

[0025] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the crosslinking agent is a compound having two or more epoxy groups in the molecule.

[0026] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the granular carrier is used for carrying a drug.

[0027] According to yet another aspect of the present invention there is provided a method according to any of the above aspects, in which the granular carrier is used as a water-absorbing material in an absorbent article. Effect of the Invention

[0028] According to the present invention, a technology is provided for easily and efficiently producing a granular carrier which is both highly absorbent and biodegradable, has an approximately spherical shape, a uniform particle size, and excellent strength and transparency, while reducing raw material loss. [Brief description of the drawings]

[0029] [Figure 1] FIG. 1 is a flow diagram showing an example of a method for producing a granular carrier according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flow diagram showing another example of a method for producing a granular carrier according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a photograph showing the water absorption state of the granular carrier obtained in Example 1. [Figure 4] FIG. 4 is a photograph of the pulverized gel particles in a dried state obtained in Comparative Example 2 (a) and the granular carrier in a dried state obtained in Reference Example 2 (b). [Diagram 5] FIG. 5 is a photograph showing the water absorption state of the pulverized gel particles (a) obtained in Comparative Example 2 and the water absorption state of the granular carrier (b) obtained in Reference Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. The preferred embodiments described below are embodiments in which any of the above aspects are more specifically embodied.

[0031] The granular carrier obtained by the manufacturing method according to this embodiment (hereinafter, also referred to as "the granular carrier according to this embodiment") is a gel particle containing a crosslinked body of a carboxyalkyl cellulose salt, and as described below, is a gel particle derived from a dispersed particle formed by suspension polymerization (i.e., reversed-phase suspension polymerization) in a suspension using a low-polarity organic solvent as a dispersion medium. The granular carrier derived from a dispersed particle obtained through the formation of a crosslinked body of a carboxyalkyl cellulose salt by this reversed-phase suspension polymerization has a substantially spherical shape, a uniform particle size, and excellent strength and transparency. According to the manufacturing method according to this embodiment, a granular carrier having such characteristics can be easily obtained without undergoing the steps of crushing the gel body, classifying, etc., in the conventional manufacturing method described above.

[0032] In this embodiment, the carboxyalkyl cellulose or its salt as the raw material is preferably a carboxyalkyl cellulose or its salt having an alkyl group having 1 to 3 carbon atoms, for example, from the viewpoint of production cost, etc., and specific examples thereof include carboxymethyl cellulose, carboxyethyl cellulose, carboxybutyl cellulose, or salts thereof. The carboxyalkyl cellulose and / or its salt may be used alone or in combination of two or more.

[0033] In this embodiment, it is important to select carboxyalkyl cellulose and / or its salt as the raw material, which has a viscosity of 1% by mass aqueous solution within a predetermined range. The longer the polymer chain of carboxyalkyl cellulose, the higher the viscosity when dissolved, and the worse the handling property when injected into the low-polarity organic solvent, which is the dispersion medium. As a result, there is a possibility that the uniformity of the particle shape and particle size of the obtained granular carrier may be adversely affected. On the other hand, the longer the polymer chain of carboxyalkyl cellulose, the higher the water absorption amount, which means that when the granular carrier according to this embodiment is used as a drug carrier, it can carry a large amount of drug. However, if the water absorption amount becomes too large, problems such as a decrease in gel strength and an increase in water separation may occur. From these points of view, in the embodiment of the present invention, carboxyalkyl cellulose and / or its salt is used, which has a viscosity of 1% by mass aqueous solution of 5 mPa·s to 300 mPa·s.

[0034] Here, the viscosity of a 1% by mass aqueous solution of carboxyalkyl cellulose and / or a salt thereof is the viscosity value measured by a B-type viscometer after preparing a 200 mL aqueous solution of carboxyalkyl cellulose so that the solid content is 1% by mass. Hereinafter, the viscosity of a 1% by mass aqueous solution of carboxyalkyl cellulose and / or a salt thereof measured under these conditions will be simply referred to as the "viscosity of carboxyalkyl cellulose." The viscosity of carboxyalkyl cellulose is preferably 10 mPa·s or more and 100 mPa·s or less, more preferably 20 mPa·s or more and 50 mPa·s or less.

[0035] In this embodiment, the average degree of etherification (average degree of substitution, DS) of the raw carboxyalkyl cellulose may be, for example, 0.5 to 1.5. By using a carboxyalkyl cellulose having an average degree of etherification in this range, the water absorption and strength of the gel can be easily improved. The average degree of etherification (average degree of substitution) is the average of the degrees of substitution of hydroxyl groups at the 2-, 3-, and 6-positions of the glucose units constituting the cellulose.

[0036] The method for producing a granular carrier according to this embodiment includes dissolving carboxyalkyl cellulose and / or its salt in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution, adding a crosslinking agent to the carboxyalkyl cellulose salt aqueous solution to obtain a mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent, mixing the mixture with a low-polarity organic solvent in a first container to obtain a suspension in which the mixture is dispersed in the low-polarity organic solvent, and proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in the suspension to form dispersed particles containing a crosslinked body of the carboxyalkyl cellulose salt. In this embodiment, the first container used for mixing the mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent with the low-polarity organic solvent and in which the reversed-phase suspension polymerization is performed has a hydrophobic inner surface.

[0037] <First production method: One-pot reaction> Fig. 1 is a flow diagram showing an example of a method for producing a granular carrier according to the present embodiment. The production method shown in Fig. 1 includes steps S101 to S104. That is, the production method shown in Fig. 1 includes a step S101 of dissolving carboxyalkyl cellulose and / or its salt in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution, a step S102 of adding a crosslinking agent to the carboxyalkyl cellulose salt aqueous solution obtained in step S101 to prepare a mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent, a step S103 of adding a low-polarity organic solvent to the mixture obtained in step S102 to obtain a suspension (reverse phase suspension) in which the mixture is dispersed in the low-polarity organic solvent, and a step S103 of proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in this suspension to form dispersed particles containing a crosslinked body of the carboxyalkyl cellulose salt, and a step S104 of filtering, washing, and drying the dispersed particles formed in step S103 from the suspension.

[0038] As described above, the manufacturing method shown in Fig. 1 is an example. The manufacturing method according to this embodiment may further include other steps not shown in Fig. 1. Furthermore, step S104 is an optional step that is performed as necessary as described below, and the manufacturing method according to this embodiment may not include step S104. Each step will be described in detail below.

[0039] In step S101, carboxyalkyl cellulose and / or its salt are added to an aqueous alkali solution and completely dissolved under stirring at room temperature to prepare an aqueous carboxyalkyl cellulose salt solution. In step S101, the time required to prepare the aqueous carboxyalkyl cellulose salt solution can be appropriately set. In one example, this time can be set to 1 to 5 hours. After adding the carboxyalkyl cellulose to the aqueous alkali solution, a defoaming treatment can be performed by reducing pressure or by leaving the solution at normal pressure for a predetermined time, if necessary.

[0040] The carboxyalkyl cellulose and / or salt thereof used in step S101 may be one obtained by using cellulose such as pulp as a starting material and carboxyalkylating it in a conventional manner, or a commercially available carboxyalkyl cellulose and / or salt thereof may be used.

[0041] The carboxyalkylcellulose salt contained in the carboxyalkylcellulose salt aqueous solution obtained in step S101 may be, for example, an alkali metal salt or an alkaline earth metal salt of carboxyalkylcellulose. In this case, an alkali aqueous solution containing an alkali metal or an alkaline earth metal is used as the alkali aqueous solution to which carboxyalkylcellulose and / or its salt is added. Examples of carboxyalkylcellulose salts include sodium salts, potassium salts, and calcium salts. In this case, an aqueous solution of sodium hydroxide, potassium hydroxide, or calcium hydroxide is used as the alkali aqueous solution to which carboxyalkylcellulose is added. According to one example, sodium carboxymethylcellulose (CMC-Na) is used as the carboxyalkylcellulose and / or its salt, and an aqueous solution of sodium hydroxide is used as the alkali aqueous solution, and an aqueous CMC-Na solution is prepared in step S101.

[0042] In step S102, a crosslinking agent is added to the carboxyalkyl cellulose salt aqueous solution obtained in step S101 to prepare a mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent. Hereinafter, when the term "mixture" is used simply, this refers to the mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent prepared in step S102.

[0043] The mixing of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent is preferably performed in a temperature range of 15°C to 43°C, more preferably in a temperature range of 20°C to 35°C, using, for example, a static mixer. If the temperature is too low, the viscosity of the mixture increases, and the handling properties decrease. In addition, in step S102, the crosslinking reaction of the carboxyalkyl cellulose salt starts immediately after the crosslinking agent is added to the aqueous carboxyalkyl cellulose salt solution, and the viscosity begins to increase. By appropriately lowering the temperature during this mixing, the crosslinking reaction can be prevented from proceeding too quickly or excessively, and excellent handling properties can be achieved. After stirring, a degassing operation under reduced pressure may be performed as necessary.

[0044] The crosslinking agent used in the production method according to this embodiment is not particularly limited, and known compounds such as polyepoxy compounds, polyglycidyl compounds, polyaldehyde compounds, polycarboxylic acids, vinyl ether compounds, methylol compounds, polyisocyanates, polyoxazoline compounds, polyvinyl compounds, polyacrylate compounds, polymethacrylate compounds, polyhalogen compounds, methylene bisacrylamide, epichlorohydrin, polyacid anhydrides, citric acid, methylene bisacrylamide, and glycidyl methacrylate can be used.

[0045] Preferred specific examples of the crosslinking agent include (a) a compound having two or more hydroxyl groups in the molecule, (b) a compound having two or more polymerizable double bonds, and (c) a compound having two or more epoxy groups.

[0046] (a) Examples of compounds having two or more hydroxyl groups in the molecule include ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, glycerin, polyglycerin, propylene glycol, diethanolamine, polyoxypropylene, sorbitan fatty acid esters, trimethylolpropane, pentaerythritol, 1,3-propanediol, and sorbitol.

[0047] (b) Examples of compounds having two or more polymerizable double bonds in the molecule include bis(meth)acrylamide, allyl(meth)acrylamide, diethylene glycol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate, and ethoxylated trimethylolpropane triacrylate.

[0048] (c) Examples of compounds having two or more epoxy groups in the molecule include polyglycidyl ethers such as ethylene glycol diglycidyl ether (EGDE), polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin triglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, and hydrogenated bisphenol A diglycidyl ether.

[0049] Among these, from the viewpoints of reactivity and the water absorption performance of the resulting granular carrier, (b) a compound having two or more polymerizable double bonds in its molecule, and (c) a compound having two or more epoxy groups in its molecule are preferred, (c) a compound having two or more epoxy groups in its molecule is more preferred, polyglycidyl ether is even more preferred, and ethylene glycol diglycidyl ether (EGDE) is particularly preferred.

[0050] The blending mass ratio of the carboxyalkyl cellulose and / or its salt to the crosslinking agent can be appropriately set. From the viewpoint of the shape, transparency and strength of the granular carrier, the blending mass ratio (X / Y) of the carboxyalkyl cellulose and / or its salt (X) to the crosslinking agent (Y) is preferably in the range of 10 / 2≧X / Y≧10 / 5, more preferably in the range of 10 / 2>X / Y≧10 / 4.

[0051] In step S103, a low-polarity organic solvent is added (injected) to the mixture obtained in step S102 to obtain a suspension (reverse phase suspension) in which the mixture is dispersed in the low-polarity organic solvent. Crosslinking polymerization of the carboxyalkyl cellulose salt is allowed to proceed in this suspension to form dispersed particles containing crosslinked bodies of the carboxyalkyl cellulose salt.

[0052] The low-polarity organic solvent added to the mixture in step S103 and used as a dispersion medium is a low-polarity organic solvent having a relative dielectric constant of 10 or less at 25°C, and is less polar than the above mixture of dispersoids. Therefore, the suspension prepared in step S103 is a reversed-phase suspension, and the cross-linking polymerization of the carboxyalkyl cellulose salt is a reversed-phase suspension polymerization. Here, the relative dielectric constant is the relative dielectric constant at 25°C measured by a capacitance meter. According to one example, it is more preferable that the low-polarity organic solvent used as a dispersion medium has a relative dielectric constant of 3 or more and 6 or less.

[0053] Examples of low-polarity organic solvents having a relative dielectric constant of 10 or less include aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, liquid paraffin, silicone oil, etc., and these can be used alone or in combination of two or more.

[0054] The low polarity organic solvent used in step S103 has a kinetic viscosity of 10 mm at 37.8° C. 2 When the dispersion medium is a viscous fluid, the aggregation of the generated spherical gel particles can be suppressed, and the adhesion between the spherical gel particles can be suppressed, thereby suppressing the formation of clumps of the spherical gel particles. 2 / s or more is important in order to obtain high quality granular carriers which are spherical in shape and have a uniform particle size.

[0055] Here, the kinematic viscosity is the kinematic viscosity at 37.8° C. measured by a vibration viscometer. According to one example, the low polarity organic solvent used as the dispersion medium has a kinematic viscosity of 10 mm 2 / s or more 100mm 2 / s or less, and according to other examples, 15 mm 2 / s or more 80mm 2 / s or less, and according to another example, 20 mm 2 / s or more 50mm 2 / s or less.

[0056] Among the above-mentioned specific examples of low-polarity organic solvents having a relative dielectric constant of 10 or less, liquid paraffin and silicone oil are particularly preferable as the low-polarity organic solvent used in step S3 because they are viscous fluids.

[0057] The liquid paraffin is not particularly limited as long as it is a paraffin that is liquid at room temperature, and examples thereof include liquid saturated hydrocarbons having 12 to 50 carbon atoms, and may be any of n-paraffin, isoparaffin, and naphthene. In addition, examples of commercially available products that can be used include MORESCO (registered trademark) White, MORESCO Bioless, and Smoil (registered trademark) (all trade names, manufactured by MORESCO Corporation), Stanol, Krystoll, Esso White Oil, and Purelex (all trade names, manufactured by Esso Petroleum Co., Ltd.). These may be used alone, or two or more of them may be used in combination.

[0058] The silicone oil is not particularly limited as long as it has a siloxane structure that is liquid at room temperature, and examples thereof include polysiloxane oils such as dimethyl silicone oil, and modified silicone oils having functional groups such as hydroxyl groups, carboxyl groups, amino groups, epoxy groups, cyano groups, mercapto groups, trifluoropropyl groups, chlorophenyl groups, long-chain alkyl groups, and the like, or modified with polyethers, alcohols, etc. These may be used alone or in combination of two or more kinds.

[0059] In step S103, the above-mentioned crosslinking agent may be further added to the low-polarity organic solvent to perform surface crosslinking (secondary crosslinking) to provide a portion with high crosslink density on the surface layer of the gel particles. By performing surface crosslinking (secondary crosslinking), it is possible to improve the gel strength while maintaining the water absorption amount.

[0060] In step S103, the temperature of the low-polarity organic solvent added to the mixture obtained in step S102 is preferably within the range of 15°C to 43°C, more preferably within the range of 15°C to 30°C.

[0061] As described above, the crosslinking reaction of the carboxyalkyl cellulose salt starts immediately after the crosslinking agent is added to the aqueous carboxyalkyl cellulose salt solution. The time from mixing the aqueous carboxyalkyl cellulose salt solution with the crosslinking agent to adding the low-polarity organic solvent to this mixture is preferably within 30 minutes, for example.

[0062] Step S103 is carried out under stirring. Examples of the stirring device include a mechanical stirrer, and examples of the stirring blade include anchor type, propeller type, and paddle type, which can be appropriately selected and used. The rotation speed is appropriately set depending on the shape of the stirring blade and the size of the reaction vessel in which the suspension is contained.

[0063] In step S103, the time required for the cross-linking polymerization reaction of the carboxyalkyl cellulose salt can be appropriately set. According to one example, it can be set to 1 hour to 6 hours.

[0064] According to one example, in step S103, the cross-linking polymerization is carried out by carrying out a first step of stirring the suspension under first conditions and a second step of stirring the suspension under second conditions in this order.

[0065] First, in the first step, the mixture immediately before the addition of the low polarity organic solvent is adjusted to a moderately low temperature (T1), and after the addition of the mixture, the mixture is stirred at the temperature T1 for a predetermined time (t1). Specifically, the temperature T1 is preferably in the range of 15°C to 43°C, more preferably in the range of 15°C to 40°C. The stirring time t1 at the temperature T1 is preferably in the range of 5 minutes to 120 minutes, more preferably in the range of 10 minutes to 120 minutes, and even more preferably in the range of 20 minutes to 60 minutes. In the first step, stirring is continued for a sufficiently long time under temperature conditions in which cross-linking polymerization does not proceed rapidly. Therefore, in the first step, the particle size is uniformized by the coalescence and division of the dispersed particles. In addition, in the first step, since the cross-linking polymerization proceeds slowly, further coalescence and division of the dispersed particles are unlikely to occur as the particle size is uniformized. Therefore, the particle size of the dispersed particles is uniform at the time when the first step is completed.

[0066] In the second step, the mixture to which the low-polarity organic solvent has been added is heated to a higher temperature T2 and stirred for a predetermined time (t2). Specifically, the temperature T2 is preferably in the range of 46°C to 80°C, more preferably in the range of 46°C to 60°C. The stirring time t2 at the temperature T2 is preferably in the range of 120 minutes to 360 minutes, more preferably in the range of 240 minutes to 300 minutes. By carrying out the stirring at a higher temperature in the second step, the crosslinking polymerization proceeds sufficiently. Therefore, the step S103 can be completed in a sufficiently short time.

[0067] The above-mentioned production method shown in Fig. 1 can be carried out by a one-pot reaction. Here, the one-pot reaction means, in a broad sense, that at least the reactions included in step S102 and step S103 are continuously carried out in one reaction vessel, and in a narrow sense, that all the reactions included in steps S101 to S103 are continuously carried out in one reaction vessel.

[0068] The one-pot reaction in the broad sense specifically means that a mixture of an aqueous carboxyalkyl cellulose salt solution and a crosslinking agent is prepared in a first container (step S102), and then a low-polarity organic solvent is added to the mixture contained in the first container (step S103). The one-pot reaction in the narrow sense specifically means that an aqueous carboxyalkyl cellulose salt solution is prepared in a first container (step S101), and then a crosslinking agent is added thereto to prepare a mixture of an aqueous carboxyalkyl cellulose salt solution and a crosslinking agent in the first container (step S102), and then a low-polarity organic solvent is added thereto (step S103).

[0069] In contrast, in another example of the production method shown in Fig. 2 described later, a mixture of an aqueous carboxyalkyl cellulose salt solution and a crosslinking agent is prepared in a second container, and then the resulting mixture is mixed with a low-polarity organic solvent in a first container that is a container separate from the second container. Hereinafter, the example of the production method shown in Fig. 1 is referred to as the "first production method" or "one-pot reaction," and the other example of the production method shown in Fig. 2 is referred to as the "second production method" or "two-pot reaction."

[0070] The first production method (one-pot reaction) is simpler than the second production method (two-pot reaction) described later, and can further reduce raw material loss and improve yield. Moreover, the first production method (one-pot reaction) is more preferably a one-pot reaction in the narrow sense in which all reactions included in steps S101 to S103 are continuously performed in a first vessel.

[0071] In the method for producing a granular carrier according to the present embodiment, a reaction vessel having a hydrophobic inner surface that comes into contact with the raw material is used as the first vessel. The reaction vessel having a hydrophobic inner surface has a low surface energy compared to a reaction vessel having an inner surface made of glass or metal that has not been subjected to hydrophobic treatment, and therefore monomers and polymers are not fixed to the side wall of the reaction vessel during or after the polymerization reaction. This allows for a uniform reaction, not only improving the yield but also facilitating the recovery of the product. The reaction vessel having a hydrophobic inner surface may be one whose inner surface is made of a material having hydrophobicity, or may be one whose inner surface has been subjected to a chemical or physical treatment (hydrophobic treatment) that imparts hydrophobicity to the inner surface. The hydrophobic material that can be used for the first vessel is not particularly limited as long as it is a material having hydrophobicity, and known materials can be used. Examples of such materials include fluororesins having fluoroalkyl groups (e.g., tetrafluoroethylene resin, perfluoroalkoxyalkane), polyolefin resins having saturated alkyl groups (e.g., polypropylene, polystyrene, polymethylpentene, polyethylene), and the like.

[0072] The method for producing a granular carrier according to this embodiment usually includes step S104 as shown in FIG. 1. That is, the dispersed particles containing the crosslinked body of the carboxyalkyl cellulose salt formed in the suspension in step S103 of this embodiment are usually taken out of the suspension by filtration, and further washed and dried as necessary. The washing after filtration is, for example, washing the low polarity organic solvent attached to the surface of the gel particles with a detergent aqueous solution such as a surfactant, and / or immersing the gel particles in ethanol to dehydrate and dealkalize them, and the drying can be performed, for example, by air drying. When a solvent with a low boiling point such as n-hexane is used as the low polarity organic solvent, the solvent on the surface of the gel particles can be volatilized / removed without washing by using a method such as reduced pressure distillation.

[0073] However, in the manufacturing method of the granular carrier according to the present embodiment, step S104 is an optional step, and the dispersed particles may be distributed as a product in a dispersed state in the suspension without being taken out of the suspension. That is, the granular carrier according to the present embodiment may be in the form of dispersed particles present in the suspension, gel particles derived from dispersed particles that have been subjected to reverse phase suspension polymerization in the suspension formed in step S103, and may be in the form of, for example, dispersed particles present in the suspension, gel particles in a water-absorbed state (water-absorbed gel particles) that have been taken out of the suspension and not dried, or gel particles in a dry state (dry gel particles) that have been taken out of the suspension and dried.

[0074] The particle diameter of the granular carrier according to the present embodiment is not particularly limited, but there is a preferred particle diameter depending on the purpose of use.For example, when the granular carrier according to the present embodiment is used for carrying medicine, the average particle diameter of the gel particles in the water-absorbed state may be 2 mm or more and 30 mm or less in one example, and 2 mm or more and 20 mm or less in another example.Here, the average particle diameter means the one measured by measuring the major axis of 30 randomly selected particles using a caliper and averaging them.

[0075] In addition, when the granular carrier according to the present embodiment is used for carrying drugs, the average particle size of the gel particles in a dry state may be, for example, 0.2 mm to 6 mm, and in another example, 0.5 mm to 4 mm. Here, the average particle size refers to the value measured by measuring the major axis of 30 randomly selected particles using a vernier caliper and averaging the measurements.

[0076] According to one example, the granular carrier of this embodiment can be used in a dry state as a highly absorbent material in absorbent articles such as disposable diapers, sanitary products (napkins, tampons, etc.), pads (sweat pads, breast milk pads, incontinence pads, etc.), and pet toilets.

[0077] In another example, the granular carrier according to the present embodiment is used as a drug carrier. That is, a liquid composition containing at least one drug selected from drugs having, for example, aromatic, deodorant, deodorizing, insect repellent, insecticidal, or antifungal properties is absorbed and carried by the granular carrier made of the dry gel particles according to the present embodiment. This makes it possible to provide gel formulations such as granular drug compositions, such as granular aromatic composition, granular deodorant composition, granular deodorant composition, granular insect repellent composition, granular insecticide composition, and granular antifungal composition.

[0078] In a gel preparation consisting of such a granular pharmaceutical composition, various commonly used drugs can be used as the pharmaceutical component contained in the liquid composition that is absorbed and carried by the granular carrier, depending on the purpose. Specific examples of aromatic drugs include animal fragrances such as musk, spirit cat fragrance, and dragon jasmine fragrance, and vegetable fragrances such as abies oil, acorn oil, almond oil, angelica root oil, page oil, bergamot oil, perch oil, boa bur rose oil, kayabuchi oil, gananga oil, capsicum oil, caraway oil, cardamom oil, cassia oil, celery oil, cinnamon oil, citronella oil, cognac oil, coriander oil, cumin oil, camphor oil, basil oil, estugoran oil, eucalyptus oil, fennel oil, garlic oil, ginger oil, grapefruit oil, hop oil, lemon oil, lemongrass oil, nutmeg oil, mandarin oil, peppermint oil, orange oil, sage oil, star anise oil, turpentine oil, rosemary oil, eucalyptus oil, anise oil, lavender oil, cumin oil, cinnamon oil, and hiba oil. In addition, artificial fragrances such as synthetic fragrances or extracted fragrances can also be used. Specific examples include hydrocarbon fragrances such as pinene and limonene, alcohol fragrances such as linalool, geraniol, citronellol, menthol, borneol, benzyl alcohol, anise alcohol, and β-phenethyl alcohol, phenol fragrances such as anethole and eugenol, aldehyde fragrances such as n-butyl aldehyde, isobutyraldehyde, hexyl aldehyde, citral, citronellal, benzaldehyde, and cinnamic aldehyde, ketone fragrances such as carvone, menthone, camphor, acetophenone, and ionone, lactone fragrances such as γ-butyrolactone, coumarin, and cineol, and ester fragrances such as octyl acetate, benzyl acetate, cinnamyl acetate, butyl propionate, and methyl benzoate. These may be used alone or in any combination of two or more.

[0079] The deodorizing agent may be either a volatile agent or a non-volatile agent, and specific examples include metal oxides such as titanium oxide and zinc oxide, flavonoid compounds, plant extracts such as catechin and polyphenol or derivatives thereof, cyclodextrin or derivatives thereof, amine compounds, etc. These may be used alone or in any combination of two or more.

[0080] Specific examples of deodorizing agents include activated carbon such as coconut shell activated carbon, charcoal such as binchotan charcoal, and other carbon-based adsorbents, as well as silica-based adsorbents such as zeolite, silica gel, and layered zinc aluminosilicate, etc. These may be used alone or in any combination of two or more.

[0081] Specific examples of agents having insect repellent or insecticidal properties include pyrethroid insecticidal components such as empenthrin, transfluthrin, allethrin, fenothrin, eminence, and profluthrin, and volatile insect repellent and insecticidal components such as paradichlorobenzene, naphthalene, camphor, 2-phenoxyethanol, hinokitiol, and allyl isothiocyanate. These can be used alone or in any combination of two or more.

[0082] In addition to the above-mentioned drugs, various additives can be used in the liquid composition, such as surfactants, colorants, preservatives, and pH adjusters.

[0083] The granular pharmaceutical composition according to this embodiment can be produced, for example, by impregnating dry gel particles into a liquid pharmaceutical composition.

[0084] As described above, the granular carrier according to the present embodiment, which is a gel particle derived from a dispersed particle formed by reversed-phase suspension polymerization using a low-polarity organic solvent as a dispersion medium, has a substantially spherical shape and a uniform particle size. Therefore, the granular drug composition obtained by carrying a liquid drug composition on the granular carrier according to the present embodiment is likely to cause air flow when filled in a container, and the drug carried on the granular carrier can function efficiently. In addition, the granular drug composition according to the present embodiment is also excellent in strength and transparency. Therefore, the granular carrier according to the present embodiment is suitably used for carrying a drug in a granular gel preparation filled in a container in stationary products such as air fresheners and deodorants.

[0085] <Second production method: Two-pot reaction> The granular carrier according to this embodiment can also be obtained by a second production method, which is another example of the production method according to this embodiment, shown in FIG.

[0086] Fig. 2 is a flow diagram showing an example of the second production method. The second production method shown in Fig. 2 includes a step S1 of dissolving carboxyalkyl cellulose and / or its salt in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution, a step S2 of preparing a mixture of the carboxyalkyl cellulose salt aqueous solution obtained in step S1 and a crosslinking agent, a step S3 of adding (injecting) and dispersing the mixture obtained in step S2 into a low-polarity organic solvent to form a suspension (reverse phase suspension), a step S4 of forming dispersed particles containing a crosslinked body of the carboxyalkyl cellulose salt by proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in this suspension, and a step S4 of filtering, washing, and drying the dispersed particles formed in step S3.

[0087] The second manufacturing method includes steps S1 and S2 which are similar to steps S101 and S102, respectively, described in the first manufacturing method, except that step S3 differs from step S103 in the first manufacturing method.

[0088] In step S3, the mixture obtained in step S2 is mixed with a low-polarity organic solvent as a dispersion solvent to form a suspension (reverse phase suspension), and dispersed particles containing a crosslinked body of carboxyalkyl cellulose salt are formed by crosslinking polymerization in this suspension. In this respect, step S3 is similar to step S103 in the first production method. However, the first production method is a one-pot reaction in which a mixture is prepared in a first container in step S102, and a low-polarity organic solvent is added to the mixture present in the first container in the subsequent step S103. In contrast, the second production method is a two-pot reaction in which a mixture of an aqueous carboxyalkyl cellulose salt solution and a crosslinker is prepared in a second container in step S2, and then, in step S3, the mixture prepared in step S2 is added under stirring to a low-polarity organic solvent present in a first container that is a container different from the second container.

[0089] The low-polarity organic solvent used as the dispersion medium in step S3 is the same as the low-polarity organic solvent used in step S103 of the first production method.

[0090] In the second production method, the first vessel used to mix the mixture with the low-polarity organic solvent is the same as the first vessel used in the first production method, and the inner surface in contact with the raw material is hydrophobic. This allows for a uniform reaction and improves the yield. In addition, the product can be easily recovered, reducing raw material loss.

[0091] In the second production method, the material of the second container used for mixing the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent is not particularly limited. The second container may be a container whose inner surface in contact with the raw material is hydrophobic, like the first container, or may be a container that is not hydrophobic. Examples of hydrophobic substances that can be used for the second container are the same as those for the first container. Examples of containers made of non-hydrophobic materials include glass containers. From the viewpoint of further reducing raw material loss, it is preferable that the second container is a container similar to the first container, that is, a container whose inner surface in contact with the raw material is hydrophobic.

[0092] In step S3, the stirring device used for stirring the low-polarity organic solvent may be, for example, a mechanical stirrer, and the stirring blade may be, for example, an anchor type, a propeller type, a paddle type, etc., and may be appropriately selected and used. In one example, in step S3, the low-polarity organic solvent is stirred at a rotation speed of 50 to 500 rpm, in another example, at a rotation speed of 200 to 500 rpm, and in yet another example, at a rotation speed of 250 to 400 rpm.

[0093] In step S3, the mixture obtained in step S2 is added (injected) into the low-polarity organic solvent, for example, by dripping the mixture drop by drop from the liquid surface of the low-polarity organic solvent using a pipette (hereinafter, sometimes referred to as the "drop injection method"). Another example is by continuously injecting the mixture while immersing a pipette in the low-polarity organic solvent (hereinafter, sometimes referred to as the "continuous injection method"). The drop injection method is preferred because it makes it easier to obtain uniform particle sizes for the dispersed particles. The continuous injection method is preferred because it can be easily performed in a short time.

[0094] In step S3, the time required for the cross-linking polymerization reaction of the carboxyalkyl cellulose salt can be appropriately set. According to one example, it can be set to 1 hour to 6 hours.

[0095] In step S3, the low-polarity organic solvent is at room temperature or in a heated state immediately before the mixture obtained in step S2 is added. According to one example, in step S3, the cross-linking polymerization is carried out by carrying out a third step of stirring the suspension under a first condition and a fourth step of stirring the suspension under a second condition in this order.

[0096] First, in the third step, the low polarity organic solvent is adjusted to a moderately low temperature (T3) just before the mixture is added, and after the mixture is added, the mixture is stirred at the temperature T3 for a predetermined time (t3). Specifically, the temperature T3 is preferably in the range of 15°C to 43°C, more preferably in the range of 15°C to 40°C. The stirring time t3 at the temperature T3 is preferably in the range of 5 minutes to 120 minutes, more preferably in the range of 10 minutes to 120 minutes, and even more preferably in the range of 20 minutes to 60 minutes. In the third step, stirring is continued for a sufficiently long time under temperature conditions in which cross-linking polymerization does not proceed rapidly. Therefore, in the third step, the particle size is uniformized by the coalescence and division of the dispersed particles. In addition, in the third step, the cross-linking polymerization proceeds slowly, so that when the particle size is uniformized, further coalescence and division of the dispersed particles are unlikely to occur. Therefore, the particle size of the dispersed particles is uniform at the time when the third step is completed.

[0097] In the fourth step, the low polarity organic solvent is heated to a higher temperature T4 and stirred for a predetermined time (t4). Specifically, the temperature T4 is preferably in the range of 46°C to 80°C, more preferably in the range of 46°C to 60°C. The stirring time t4 at the temperature T4 is preferably in the range of 120 minutes to 360 minutes, more preferably in the range of 240 minutes to 300 minutes. By carrying out the stirring at a higher temperature in the fourth step, the crosslinking polymerization proceeds sufficiently. Therefore, the step S3 can be completed in a sufficiently short time.

[0098] The second manufacturing method typically includes step S4 as shown in Fig. 2. Step S4 is similar to step S104 described in the first manufacturing method. EXAMPLES

[0099] The results of tests carried out in relation to the present invention are described below. (1) Production of granular carriers (1.1) Example 1 (One-pot reaction, first vessel: PP) Sodium carboxymethylcellulose (CMC-Na) (Daicel 1120, Daicel Miraize Co., Ltd.) with a viscosity in the range of 20 to 50 mPa s was used as a raw material to produce a granular carrier by the first production method (one-pot reaction) described below. The viscosity here is the viscosity of a 1% by mass aqueous solution of CMC-Na at 25°C measured by the method described above.

[0100] A 500 mL beaker made of polypropylene (PP) was prepared as the first container. 150 g of ion-exchanged water was poured into this container, and 3 g of sodium hydroxide was added to obtain a 0.5 M aqueous sodium hydroxide solution. 15 g of the above CMC-Na (Daicel 1120) was added to this aqueous sodium hydroxide solution, and it was completely dissolved while stirring at room temperature. Then, it was left to stand overnight to defoam. Next, 6 g of ethylene glycol diglycidyl ether (EGDE) (Denacol (registered trademark) EX-810, Nagase ChemteX Corporation) was dropped into this aqueous CMC-Na solution as a crosslinking agent, and it was stirred at a stirring speed of 250 rpm for 30 minutes. As a result, a mixture of the aqueous CMC-Na solution and EGDE was obtained. In this example, the blending mass ratio of CMC-Na to the crosslinking agent EGDE (CMC-Na / EGDE) was 10 / 4.

[0101] Next, to the resulting mixture, liquid paraffin (Sumoil P-100, manufactured by Matsumura Oil Co., Ltd.; kinetic viscosity 20.5 mm) at room temperature (24°C) was added under stirring (stirring speed 250 rpm). 2 With stirring continued, the liquid temperature was kept at room temperature for 5 minutes after the completion of injection of the liquid paraffin, and then heating was started. When the liquid temperature exceeded 50°C, stirring was continued for an additional 4 hours to allow the reaction to proceed.

[0102] After the reaction, the gel particles formed were filtered off. Next, the liquid paraffin adhering to the surface of the gel particles was washed off with an appropriate amount of surfactant aqueous solution. Furthermore, the gel particles were immersed in ethanol to dehydrate and remove alkali, and then dried under reduced pressure. This resulted in a dry granular carrier.

[0103] (1.2) Example 2 (two-pot reaction, first vessel: PP) The above CMC-Na (Daicel 1120, manufactured by Daicel Miraize Co., Ltd.) was used as a raw material, and a granular carrier was produced by the second production method (two-pot reaction) described below.

[0104] 2 g of sodium hydroxide was dissolved in 100 g of ion-exchanged water poured into a 200 mL glass beaker to obtain a 0.5 M aqueous sodium hydroxide solution. 10 g of the above CMC-Na (Daicel 1120) was dissolved in this aqueous sodium hydroxide solution, and the solution was left to stand overnight to defoam. 4 g of the above EGDE (Denacol EX-810) was dropped into this aqueous solution as a crosslinking agent, and the solution was stirred at a stirring speed of 250 rpm for 30 minutes. This resulted in a mixture of the aqueous CMC-Na solution and EGDE. In this example, the blending mass ratio of CMC-Na to the crosslinking agent EGDE (CMC-Na / EGDE) was 10 / 4.

[0105] A 500 mL beaker made of polypropylene (PP) was prepared as the first container. 300 g of liquid paraffin (Sumoil P-100) at room temperature (24°C) was poured into this container. The mixture obtained above was poured into the container while stirring at a stirring speed of 250 rpm. The mixture was poured using a high viscosity pipette with the tip of the pipette immersed in the liquid paraffin. With stirring continued, the liquid temperature was kept at the above room temperature for 5 minutes after the mixture had been poured, and then heating was started. Once the liquid temperature exceeded 50°C, stirring was continued for an additional 4 hours to allow the reaction to occur.

[0106] After the reaction, the gel particles formed were filtered, and the liquid paraffin adhering to the surface of the gel particles was washed off with an appropriate amount of surfactant aqueous solution. The gel particles were then immersed in ethanol for dehydration and dealkalization. The gel particles were then dried at room temperature and then dried under reduced pressure to obtain a dry granular carrier.

[0107] (1.3) Reference Example 1 (Two-pot reaction, first vessel: glass)

[0108] A dry granular carrier was obtained in the same manner as in Example 2, except that a 500 mL glass beaker was used as the first container instead of the 500 mL polypropylene (PP) beaker.

[0109] (1.4) Reference Example 2 (Two-pot reaction, first vessel: glass) The above CMC-Na (Daicel 1120) was used as a raw material to produce a granular carrier by the second production method (two-pot reaction) described below.

[0110] 10.0 g of the above CMC-Na (Daicel 1120) was dissolved in 100 mL of 0.5 mol / L aqueous sodium hydroxide solution. 4.0 g of the above EGDE (Denacol EX-810) was added dropwise to this aqueous solution as a crosslinking agent, and the solution was stirred for 20 minutes, after which a degassing operation was performed for 5 minutes under reduced pressure. This resulted in a mixture of the CMC-Na aqueous solution and EGDE. In this example, the blending mass ratio of CMC-Na to the crosslinking agent EGDE (CMC-Na / EGDE) was 10 / 4.

[0111] The mixture was then poured into a 500 mL glass beaker containing liquid paraffin (Sumoil P-100, Matsumura Oil Co., Ltd.; kinetic viscosity 20.5 mm) that had been heated to 60° C. and stirred at a stirring speed of 250 rpm. 2 The mixture was injected into a liquid paraffin (100 ml / s). A high-viscosity pipette was used to inject the mixture, and the tip of the pipette was immersed in the liquid paraffin while it was being injected. The mixture was allowed to react in the liquid paraffin for 4 hours. After the reaction, the gel particles that had formed were filtered off, and the liquid paraffin adhering to the gel particle surfaces was washed off with an appropriate amount of aqueous surfactant solution. The gel particles were then immersed in ethanol to dehydrate and dealkalize them, and then air-dried to obtain a dry granular carrier.

[0112] (1.5) Comparative Example 1 (Two-pot reaction, first vessel: glass) A granular carrier was produced in the same manner as in Reference Example 2, except that CMC-Na (Daicel 1120, viscosity 20 to 50 mPa·s) was changed to CMC-Na (Daicel 1190, viscosity 1300 to 2000 mPa·s).

[0113] (1.6) Comparative Example 2 (Aqueous Solution Polymerization) 2 g of sodium hydroxide was dissolved in 100 g of ion-exchanged water to obtain a 0.5 M aqueous sodium hydroxide solution. 10 g of the above CMC-Na (Daicel 1120, Daicel Miraize Co., Ltd.) was dissolved in this aqueous sodium hydroxide solution. 4 g of EGDE (Denacol EX-810, Nagase ChemteX Co., Ltd.) was added dropwise to the mixture and stirred for 20 minutes. After degassing for 5 minutes under reduced pressure, the mixture was reacted for 4 hours in a thermostatic bath at 60°C. After the reaction, the gel-like material formed was removed from the beaker and roughly crushed using a mixer. The crushed gel obtained was immersed in ethanol to dehydrate and remove alkali, and then air-dried to obtain a solid (crushed gel).

[0114] (2) Evaluation (2.1) Dried gel shape The shape of each of the resulting granular carriers (dried gels) was visually evaluated according to the following criteria. The results are summarized in Table 1. A: Spherical dry gels make up almost the entire sample, and dry gels of other shapes are hardly observed. B: Mostly spherical dry gel. Flat or thread-like dry gel is mixed in, but not noticeable. C: Non-spherical dry gel accounts for the majority, and spherical dry gel is scarce.

[0115] (2.2) Transparency Each of the obtained granular carriers (dried gels) was immersed in ion-exchanged water to absorb the maximum amount of water that it could absorb, and the transparency of the water-absorbed gel particles was evaluated visually according to the following criteria. The results are summarized in Table 1. A: There is no or almost no cloudiness, and the transparency is high overall. B: Some parts are cloudy, but more than 80% is transparent, and the overall appearance is transparent. C: Many parts are cloudy or the whole is cloudy, with low transparency overall.

[0116] (2.3) Strength 1 g of each of the obtained granular carriers (dried gel particles) was filled into a 200 mL beaker, 150 mL of ion-exchanged water was added, and the mixture was left to stand overnight to obtain water-absorbed gel particles carrying the maximum amount of water that they could absorb. After filtering the water-absorbed gel particles to remove excess water, the water-absorbed gel particles were filled into a 200 mL beaker again. At this time, the inside of the container was piled up with approximately six layers of particles from the bottom to the top. These were used as evaluation samples, and the strength was evaluated according to the following criteria. The results are summarized in Table 1.

[0117] A: The strength at which a particle located at the bottom of a container and bearing a weight approximately six times its own weight maintains its spherical shape and uniformly sized gaps form between particles throughout the packed structure. B: A strength at which at least some of the particles located at the bottom of the container and subjected to a weight approximately six times its own weight are unable to maintain their spherical shape, resulting in some areas where no gaps exist between the particles at the bottom. C: A strength at which the particles are unable to maintain their spherical shape even under their own weight.

[0118] Among the evaluations shown in Table 1, the evaluations of Example 2 and Reference Example 1, which are related to a two-pot reaction, are estimated from the evaluation results of Reference Example 2, which is also related to a two-pot reaction. That is, in Example 2, in which the first container is changed from a glass beaker to a polypropylene beaker, it can be estimated that the shape, transparency, and strength of the dried gel are similar to those of Reference Example 2. In addition, in Reference Example 1, in which the temperature of the liquid paraffin immediately before the mixture is added is changed, it can be estimated that the shape, transparency, and strength of the dried gel are similar to those of Reference Example 2.

[0119] [Table 1]

[0120] The following can be seen from Table 1, Fig. 3, Fig. 4 and Fig. 5. Here, Fig. 3 is a photograph showing the water absorption state (water-absorbed gel) of the granular carrier obtained in Example 1. Fig. 4(a) is a photograph of the dried crushed gel particles (crushed gel) produced in Comparative Example 2, and Fig. 5(a) is a photograph of the water absorption state. Fig. 4(b) is a photograph of the dry granular carrier (dried gel particles) produced in Reference Example 2, and Fig. 5(b) is a photograph of the water absorption state.

[0121] That is, from Table 1 and Examples 1, 2, Reference Examples 1 and 2 shown in the above drawings, it is seen that the granular carrier derived from the dispersed particles formed by reverse phase suspension polymerization according to the first production method (one-pot reaction) or the second production method (two-pot reaction) has a substantially spherical shape, a uniform particle size, and excellent transparency and strength. On the other hand, it is seen that in Comparative Example 1, in which CMC with high viscosity was used, it is difficult to produce spherical gel particles by reverse phase suspension polymerization.

[0122] Furthermore, by comparing Example 1, Example 2, Reference Example 1, and Reference Example 2 with Comparative Example 2, it is clear that the particle shapes of the granular carrier derived from the dispersed particles formed by reversed-phase suspension polymerization and the crushed gel particles are completely different. That is, from FIG. 4(a) and FIG. 5(a), it can be seen that the crushed gel particles of Comparative Example 2 obtained by the conventional method of crushing the hydrogel formed by aqueous solution polymerization are in the form of fragments with sharp edges, and most of the particles have a distorted shape that is difficult to call spherical. On the other hand, from Table 1 and FIG. 4(b) and FIG. 5(b), the gel particles derived from the dispersed particles formed by reversed-phase suspension polymerization are spherical in shape and have a uniform particle size. It can be seen that the manufacturing method according to the embodiment of the present invention can easily obtain high-quality gel particles in this way.

[0123] (4) Yield of granular carrier For Example 1 (one-pot reaction, PP), Example 2 (two-pot reaction, PP) and Reference Example 1 (two-pot reaction, glass), the yield of the granular support was measured by the following method.

[0124] ·yield In Examples 1, 2 and Reference Example 1, the yield (%) of the finally obtained dry granular carrier was calculated according to the following formula (1). Yield(%)=[M2 / M1]×100 (1) In the formula, M1 represents the total mass (g) of the raw materials a to c shown in Table 2 below, and M2 represents the mass (g) of the finally obtained granular carrier in a dry state. The results are shown in Table 2.

[0125] [Table 2]

[0126] The following can be seen from Table 2. That is, a comparison of Examples 1 and 2 with Reference Example 1 shows that the use of a vessel having an inner surface that comes into contact with the sample made of a hydrophobic material as the first vessel for performing reversed-phase suspension polymerization can suppress raw material loss and improve the yield. Also, a comparison of Examples 1 and 2 shows that the above-mentioned effect of using a vessel made of the above-mentioned hydrophobic material as the first vessel is greater in a one-pot reaction than in a two-pot reaction.

[0127] The present invention is not limited to the above-mentioned embodiment, and can be modified in various ways without departing from the gist of the present invention. The embodiments may be combined as appropriate, and in that case, the combined effect can be obtained. Furthermore, the above-mentioned embodiment includes various inventions, and various inventions can be extracted by combinations selected from the multiple components disclosed. For example, if the problem can be solved and the effect can be obtained even if some components are deleted from all the components shown in the embodiment, the configuration from which the components are deleted can be extracted as an invention.

Claims

1. A method for producing a granular carrier comprising gel particles containing a crosslinked body of a carboxyalkyl cellulose salt, comprising the steps of: A carboxyalkyl cellulose and / or a salt thereof having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1% by mass aqueous solution at 25°C is dissolved in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution; adding a crosslinking agent to the aqueous carboxyalkyl cellulose salt solution to obtain a mixture of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent; mixing the mixture with a low-polarity organic solvent in a first container to obtain a suspension in which the mixture is dispersed in the low-polarity organic solvent; and Crosslinking polymerization of the carboxyalkyl cellulose salt is allowed to proceed in the suspension to form dispersed particles containing a crosslinked body of the carboxyalkyl cellulose salt. Including, The low-polarity organic solvent has a relative dielectric constant of 10 or less at 25° C. and a kinetic viscosity of 10 mm at 37.8° C. 2 / s or more, and the first vessel has a hydrophobic inner surface.

2. 2. The method according to claim 1, wherein the inner surface of the first container is made of a material containing at least one of tetrafluoroethylene resin, perfluoroalkoxyalkane, polypropylene, polystyrene, polymethylpentene, and polyethylene.

3. 3. The method according to claim 1, wherein the mixture of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent is prepared in the first container, and the mixture is mixed with the low-polarity organic solvent by adding the low-polarity organic solvent to the mixture contained in the first container.

4. The method according to claim 3, wherein the reaction is carried out in the first vessel until dispersed particles containing a crosslinked product of the carboxyalkyl cellulose salt are formed.

5. 3. The method according to claim 1, wherein the mixture of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent is prepared in a second container, and the mixture is mixed with the low-polarity organic solvent by adding the mixture to the low-polarity organic solvent contained in the first container.

6. 3. The method according to claim 1, wherein the temperature of the low-polarity organic solvent when the low-polarity organic solvent is mixed with the mixture is within the range of 15°C to 43°C.

7. 3. The method according to claim 1, wherein the low-polarity organic solvent is liquid paraffin or silicone oil.

8. The kinetic viscosity of the low polarity organic solvent at 37.8° C. is 10 mm 2 / s or more 100mm 2 The method according to claim 1 or 2, wherein the solubility is 1 / s or less.

9. The method according to claim 1 or 2, wherein the viscosity of the carboxyalkyl cellulose and / or salt thereof is 5 mPa·s or more and 100 mPa·s or less.

10. The method according to claim 1 or 2, wherein the mass ratio (X / Y) of the carboxyalkyl cellulose and / or its salt (X) to the crosslinking agent (Y) in the mixture is in the range of 10 / 2 to 10 / 5.

11. 3. The method according to claim 1, wherein the crosslinking agent is a compound having two or more epoxy groups in the molecule.

12. The method according to claim 1 or 2, wherein the granular carrier is used for carrying a drug.

13. The method according to claim 1 or 2, wherein the granular carrier is used as a water-absorbent material in an absorbent article.

Citation Information

Patent Citations

  • Spherical granule of chlorprenaline-hydrochloric acid and its production

    JP1992077422A

  • Microstirring granulator

    JP2011098259A

  • Granular carrier, granular agent composition and absorbent article containing the same, and method of producing granular carrier

    JP2023057864A

  • Process for producing crosslinked gel and its crosslinked gel

    JP2008285611A

  • High water-absorbing polymer

    JP2011140534A