Three-dimensional lamination shaping device and method for controlling three-dimensional lamination shaping device
The apparatus uses electron detection to monitor and adjust powder spreading and melting in real-time, addressing throughput issues in conventional 3D additive manufacturing by ensuring consistent and efficient layer formation.
Patent Information
- Application Number
- JP2023063587
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-04-10
AI Technical Summary
Conventional 3D additive manufacturing apparatuses face issues with deteriorating throughput due to improper spreading of powder material, requiring frequent stops and re-spreading, which affects the efficiency of the modeling process.
A three-dimensional additive manufacturing apparatus and method that includes a detection unit to monitor backscattered electrons during the manufacturing process, allowing for real-time adjustments in powder supply and beam irradiation to correct spreading and melting issues without interrupting the process.
The solution enables continuous operation without reducing throughput by accurately controlling the amount of powder supplied and the melting conditions, ensuring proper layer formation and maintaining production efficiency.
Smart Images

Figure 2024150257000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a three-dimensional additive manufacturing apparatus and a method for controlling a three-dimensional additive manufacturing apparatus. [Background technology]
[0002] In recent years, 3D additive manufacturing technology, which creates objects by stacking thin layers of powder material one by one, has been attracting attention, and many types of 3D additive manufacturing technologies have been developed based on differences in powder materials and manufacturing methods.
[0003] In a conventional 3D additive manufacturing device, for example, a powder material is spread layer by layer on a base plate installed on the upper surface of a stage. Next, only the two-dimensional structure part corresponding to one cross section of the model is melted from the powder material spread on the base plate by a heating mechanism consisting of an electron beam or laser. Then, the layers of such powder material are stacked one by one in the height direction (Z direction) to form a model (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-138653 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in conventional 3D additive manufacturing devices, if the powder material was not properly spread during the modeling process, the modeling operation had to be temporarily stopped and the powder material had to be spread again, which resulted in a problem of poor throughput in the modeling operation.
[0006] In consideration of the above problems, an object of the present invention is to provide a three-dimensional additive manufacturing apparatus and a control method for a three-dimensional additive manufacturing apparatus that are capable of performing correction work without deteriorating throughput. [Means for solving the problem]
[0007] In order to solve the above problems and achieve the object of the present invention, the three-dimensional additive manufacturing apparatus of the present invention includes a modeling plate, a powder supplying device that supplies a powder material to the modeling plate to form a powder layer, and a beam irradiation device that irradiates the powder layer with an electron beam. The three-dimensional additive manufacturing apparatus also includes a detection unit that detects reflected electrons generated when the powder material is irradiated with the electron beam, and a control unit that controls the powder supplying device and the beam irradiation device. The control unit acquires a pre-main melting reflected electron signal, which is a reflected electron signal detected by the detection unit after the powder material is spread by the powder supplying device and before the powder material is main melted by the electron beam. The control unit also acquires a post-main melting reflected electron signal of the previous layer, which is a reflected electron signal detected by the detection unit after the powder material is main melted by the electron beam in the modeling process of the previous layer of the current layer. Then, the control unit sets the supply amount of powder material from the powder supplying device in the modeling process of the next layer based on the pre-main melting reflected electron signal and the post-main melting electron signal of the previous layer.
[0008] The three-dimensional additive manufacturing method of the present invention includes the following steps (1) to (5). (1) A process in which a powder feeder supplies powder material to a build plate to form a powder layer. (2) A process of acquiring a pre-main melting reflected electron signal, which is a reflected electron signal detected by the detection unit after the powder material has been spread out by the powder supplying device and before the powder material is main melted by the electron beam. (3) The main melting process involves using a beam irradiation device to irradiate the powder layer with an electron beam to melt the powder material. (4) A process of acquiring a reflected electron signal after main melting of the previous layer, which is a reflected electron signal detected by the detection unit after the powder material is main melted by the electron beam in the modeling process of the layer previous to the current layer. (5) A process of setting the amount of powder material to be supplied from a powder supplying device in the modeling process of the next layer based on the reflected electron signal before the main melting and the electron signal after the main melting of the previous layer. Effect of the Invention
[0009] According to the three-dimensional additive manufacturing apparatus and the control method for the three-dimensional additive manufacturing apparatus of the present invention, correction work can be performed without deteriorating the throughput. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic cross-sectional view showing a three-dimensional additive manufacturing apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a block diagram showing an example of the configuration of a control system of a three-dimensional additive manufacturing apparatus according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a plan view showing the position of a detection unit in a three-dimensional additive manufacturing apparatus according to an embodiment of the present invention. [Figure 4] 5 is a flowchart showing an example of operation of the three-dimensional additive manufacturing device according to the embodiment of the present invention. [Diagram 5] 1 shows an example of a reflected electron image acquired after powder heating. [Figure 6] A backscattered electron image taken after a powder heat shows an example of improperly packed powder material. [Figure 7] 1 is a backscattered electron image taken after full melting, showing an example of melted powder material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of a three-dimensional additive manufacturing apparatus and a control method for a three-dimensional additive manufacturing apparatus of the present invention will be described with reference to Fig. 1 to Fig. 7. In addition, the same reference numerals are used to designate common members in each drawing.
[0012] 1. Example of embodiment 1-1. Configuration of 3D additive manufacturing equipment First, a first embodiment of a three-dimensional additive manufacturing device according to an embodiment of the present invention (hereinafter, referred to as "this example") will be described with reference to FIG. Fig. 1 is a schematic cross-sectional view showing a three-dimensional additive manufacturing apparatus of this embodiment. In the following description, in order to clarify the shapes and positional relationships of the various parts of the three-dimensional additive manufacturing apparatus, the left-right direction in Fig. 1 is defined as the X direction, the depth direction in Fig. 1 is defined as the Y direction, and the up-down direction in Fig. 1 is defined as the Z direction. The X direction, Y direction, and Z direction are mutually orthogonal. Moreover, the X direction and Y direction are parallel to the horizontal direction, and the Z direction is parallel to the vertical direction.
[0013] The 3D additive manufacturing device 1 shown in FIG. 1 is a device that irradiates a powder material made of a metal powder such as titanium, aluminum, or iron with an electron beam to melt the powder material, and then stacks layers of the solidified powder material to form a three-dimensional object.
[0014] 1, the 3D additive manufacturing apparatus 1 includes a vacuum chamber 3, a beam irradiation device 2, a powder supplying device 16, a modeling table 18, a modeling box 20, and a collection box 21. The 3D additive manufacturing apparatus 1 also includes a modeling plate 22, an inner base 24, a plate moving device 26, a radiation shield cover 28, a mask cover 30, a camera 42, and a shutter 44. The 3D additive manufacturing apparatus 1 also includes a plurality of detection units 46 that detect reflected electrons.
[0015] The vacuum chamber 3 is a chamber for creating a vacuum state by evacuating the air inside the chamber with a vacuum pump (not shown).
[0016] The beam irradiation device 2 is a device that irradiates the electron beam 15 onto the shaping plate 22 or the shaping surface 32a of the powder layer formed by the powder material 32. The shaping surface 32a corresponds to the upper surface of the powder layer. The state of the powder layer changes as the 3D additive manufacturing process progresses. Although not shown, the beam irradiation device 2 has an electron gun that is a source of the electron beam 15, a focusing lens that focuses the electron beam generated by the electron gun, and a deflection lens that deflects the electron beam 15 focused by the focusing lens. The focusing lens is configured using a focusing coil and focuses the electron beam 15 by the magnetic field generated by the focusing coil. The deflection lens is configured using a deflection coil and deflects the electron beam 15 by the magnetic field generated by the deflection coil.
[0017] The powder supplying device 16 is a device that supplies a powder material 32, which is an example of a powder material that is a raw material of the molded object 38, onto the molding plate 22 to form a powder layer. The powder supplying device 16 has a hopper 16a, a powder dropper 16b, and a squeegee 16c. The hopper 16a is a container for storing metal powder. The powder dropper 16b is a device that drops the powder material 32 stored in the hopper 16a onto the molding table 18. The squeegee 16c is a long, elongated member that is long in the Y direction and has a blade 16d for spreading powder. The squeegee 16c spreads the powder material 32 dropped by the powder dropper 16b onto the molding table 18. The squeegee 16c is provided so as to be movable in the X direction in order to spread the powder material 32 over the entire surface of the molding table 18.
[0018] The modeling table 18 is arranged horizontally inside the vacuum chamber 3. The modeling table 18 is arranged below the powder supplying device 16. The center of the modeling table 18 is open. The shape of the opening of the modeling table 18 is circular or angular (for example, rectangular) when viewed from above.
[0019] The modeling box 20 is a box that forms a space for modeling. An upper end of the modeling box 20 is connected to an edge of the opening of the modeling table 18. A lower end of the modeling box 20 is connected to the bottom wall of the vacuum chamber 3.
[0020] The recovery box 21 is a box for recovering the powder material 32 that has been supplied onto the modeling table 18 by the powder supplying device 16 in an amount greater than necessary.
[0021] The shaping plate 22 is a plate for forming a shaped object 38 using the powder material 32. The shaped object 38 is formed by stacking on the shaping plate 22. The shaping plate 22 is formed to be circular or angular in plan view to match the opening shape of the shaping table 18. The shaping plate 22 is connected (grounded) to the inner base 24 by an earth wire 34 so as not to be in an electrically floating state. The inner base 24 is held at GND (ground) potential. The powder material 32 is spread over the shaping plate 22 and the inner base 24.
[0022] The inner base 24 is provided so as to be movable in the vertical direction (Z direction). The shaping plate 22 moves vertically together with the inner base 24. The inner base 24 has outer dimensions larger than those of the shaping plate 22. The inner base 24 slides vertically along the inner side surface of the shaping box 20. A sealing member 36 is attached to the outer periphery of the inner base 24. The sealing member 36 is a member that maintains slidability and airtightness between the outer periphery of the inner base 24 and the inner side surface of the shaping box 20. The sealing member 36 is made of a material that is heat-resistant and elastic.
[0023] The plate moving device 26 is a device that moves the shaping plate 22 and the inner base 24 in the up-down direction. The plate moving device 26 includes a shaft 26a and a drive mechanism unit 26b. The shaft 26a is connected to the lower surface of the inner base 24. The drive mechanism unit 26b includes a motor and a power transmission mechanism (not shown), and moves the shaping plate 22 and the inner base 24 together with the shaft 26a in the up-down direction by driving the power transmission mechanism using the motor as a drive source. The power transmission mechanism is, for example, configured by a rack-and-pinion mechanism, a ball screw mechanism, or the like.
[0024] The radiation shield cover 28 is disposed between the shaping plate 22 and the beam irradiation device 2 in the Z direction. The radiation shield cover 28 is made of a metal such as stainless steel. The radiation shield cover 28 shields radiant heat generated when the powder material 32 is irradiated with the electron beam 15 by the beam irradiation device 2. When the powder material 32 is irradiated with the electron beam 15 in order to perform the main sintering of the powder material 32, the powder material 32 melts. At this time, if the heat radiated from the shaping surface 32a of the powder layer, i.e., the radiant heat, is widely diffused within the vacuum chamber 3, the thermal efficiency is deteriorated. In contrast, when the radiation shield cover 28 is disposed above the shaping plate 22, the heat radiated from the shaping surface 32a is shielded by the radiation shield cover 28, and the shielded heat is reflected by the radiation shield cover 28 and returned to the shaping plate 22 side. Therefore, the heat generated by the irradiation of the electron beam 15 can be efficiently utilized.
[0025] In addition, the radiation shield cover 28 functions to prevent evaporated material generated when the powder material 32 is irradiated with the electron beam 15 from adhering (evaporating) onto the inner wall of the vacuum chamber 3. When the powder material 32 is irradiated with the electron beam 15, part of the molten metal becomes a mist of evaporated material and rises from the printing surface 32a. The radiation shield cover 28 is disposed to cover the space above the printing surface 32a to prevent the evaporated material from diffusing inside the vacuum chamber 3.
[0026] The mask cover 30 has an opening 30a and a mask portion 30b. When forming the shaped object 38, the mask cover 30 is placed over the upper surface of the powder material 32, i.e., the shaping surface 32a. At this time, the opening 30a exposes the powder material 32 spread on the shaping plate 22, and the mask portion 30b shields the powder material 32 located outside the opening 30a. The shape of the opening 30a is set according to the shape of the shaping plate 22. For example, if the shaping plate 22 is circular in plan view, the shape of the opening 30a in plan view is set to be circular accordingly, and if the shaping plate 22 is angular in plan view, the shape of the opening 30a in plan view is set to be angular accordingly.
[0027] The mask cover 30 is disposed below the radiation shield cover 28. The opening 30a and the mask portion 30b of the mask cover 30 are disposed between the modeling plate 22 and the radiation shield cover 28 in the Z direction. The mask cover 30 has an enclosure portion 30c. The enclosure portion 30c is disposed so as to surround the space above the opening 30a. A part (upper portion) of the enclosure portion 30c overlaps with the radiation shield cover 28 in the Z direction. The enclosure portion 30c serves to shield radiant heat generated from the modeling surface 32a and to suppress the diffusion of evaporated substances generated from the modeling surface 32a. In other words, the enclosure portion 30c serves the same function as the radiation shield cover 28.
[0028] The mask cover 30 is made of a metal having a higher melting point than the powder material 32 used as the raw material of the molded object 38. The mask cover 30 is made of a material having low reactivity with the powder material 32. Titanium can be given as an example of a material for the mask cover 30. The mask cover 30 may be made of the same metal material as the powder material 32 used. The mask cover 30 is electrically grounded to GND. The mask cover 30 serves as an electrical shield when the powder material 32 is pre-sintered by irradiation with the electron beam 15 in a pre-heating step before the main sintering step described later, thereby minimizing the occurrence of powder scattering.
[0029] The camera 42 is a camera capable of photographing the modeling surface 32a of the powder layer. The camera 42 is disposed at a position shifted in the Y direction from the beam irradiation device 2 so as not to interfere with the position of the camera 42 and the beam irradiation device 2. The camera 42 is preferably configured by a visible light camera such as a digital video camera. The camera 42 photographs the modeling surface 32a of the powder layer to generate an image (image data) of the powder layer. Therefore, the image generated by the camera 42 is an image showing the state of the modeling surface 32a of the powder layer. The photographing by the camera 42 is performed in a state where the modeling surface 32a of the powder layer is irradiated with illumination light emitted by an illumination light source (not shown) provided in the 3D additive manufacturing apparatus 1.
[0030] The shutter 44 protects the camera 42 and the observation window so that evaporated substances generated from the forming surface 32a do not adhere to the camera 42 or the observation window when the powder material 32 is melted by irradiation with the electron beam 15. The camera 42 photographs the forming surface 32a with the shutter 44 open. Moreover, in a process in which evaporated substances are likely to be generated or a process in which a large amount of evaporated substances are generated, that is, when the powder material 32 is melted by the electron beam 15, the shutter 44 is closed.
[0031] A plurality of detectors 46 for detecting reflected electrons are disposed below the beam irradiation device 2. Specifically, the detectors 46 are disposed between the beam irradiation device 2 and the printing surface 32a of the object 38 formed on the printing plate 22.
[0032] FIG. 3 is a plan view showing the position of the detection unit 46. As shown in FIG. As shown in FIG. 3, the multiple detection units 46a, 46b, 46c, and 46d are arranged so as to surround the periphery of the object 38. The first detection unit 46a is arranged on one side of the object 38 in the X direction, and the second detection unit 46b is arranged on the other side of the object 38 in the X direction. The first detection unit 46a and the second detection unit 46b face each other with the object 38 in between. The third detection unit 46c is arranged on one side of the object 38 in the Y direction, and the fourth detection unit 46d is arranged on the other side of the object 38 in the Y direction. The third detection unit 46c and the fourth detection unit 46d face each other with the object 38 in between.
[0033] Although an example in which a plurality of detectors 46 are arranged has been described, the present invention is not limited to this, and the number of detectors 46 may be one, three or less, or five or more.
[0034] The detector 46 is not limited to a semiconductor detector, but may be a Ti electrode having a low secondary electron emission rate due to electronic excitation. The detector 46 may detect the reflected electrons incident on the electrode as a current using a current detection amplifier, and detect the increase or decrease of the current.
[0035] FIG. 2 is a block diagram showing an example of the configuration of a control system of the three-dimensional additive manufacturing apparatus 1 of this embodiment. As shown in Figure 2, the 3D additive manufacturing device 1 has a polarization amplifier control circuit 101 which is an electron beam control unit, an analog-to-digital conversion circuit (ADC) 102, a preamplifier (Pre-AMP) 103, a personal computer (PC) 104 which is an example of a control unit, and a display unit 105.
[0036] The polarization amplifier control circuit 101 is connected to the beam irradiation device 2 and the PC 104. The polarization amplifier control circuit 101 controls the beam irradiation device 2 based on the set beam scanning information. As a result, the beam irradiation device 2 irradiates a predetermined position with the electron beam 15. The polarization amplifier control circuit 101 also transmits beam irradiation position information indicating the irradiation position of the electron beam 15 to the PC 104.
[0037] The Pre-AMP 103 is connected to the detection unit 46 and the ADC 102. The Pre-AMP 103 converts the reflected electron current detected by the detection unit 46 from a current signal to a voltage signal. The voltage signal converted by the Pre-AMP 103 is transmitted to the ADC 102. The ADC 102 converts the reflected electron signal, which has become a voltage signal, from an analog signal to a digital signal and transmits it to the PC 104.
[0038] PC 104 has an image processing unit and a storage unit (not shown). The image processing unit of PC 104 captures an image generated by camera 42 and performs a predetermined image processing on the captured image. PC 104 outputs the camera image that has been subjected to image processing by the image processing unit to display unit 105.
[0039] The storage unit stores the camera images generated by the image processing unit. Furthermore, the storage unit stores beam irradiation position information transmitted from the polarization amplifier control circuit 101. The storage unit also stores a plurality of arithmetic expressions for performing arithmetic processing on the reflected electron signals obtained from the plurality of detection units 46a, 46b, 46c, and 46d.
[0040] The PC 104 selects a predetermined arithmetic expression from a plurality of arithmetic expressions according to the modeling process. Then, the PC 104 performs arithmetic processing on the reflected electron signal using the selected arithmetic expression to calculate an arithmetic signal. Then, the image processing unit visualizes the arithmetic signal to obtain a reflected electron image (BSE image). The PC 104 outputs the obtained reflected electron image (BSE image) to the display unit 105. In addition, the reflected electron image (BSE image) is stored in the storage unit.
[0041] The display unit 105 is configured with a display such as a liquid crystal display (LCD) or an organic ELD (Electro Luminescence Display), etc. The display unit 105 displays the BSE image and the camera image output from the PC 104 on a display screen 106 (see FIG. 4, etc.).
[0042] 1-2. Example of operation of 3D additive manufacturing device Next, an example of the operation of the three-dimensional additive manufacturing apparatus 1 having the above-mentioned configuration will be described with reference to FIG. FIG. 4 is a flowchart showing an example of the operation of the three-dimensional additive manufacturing apparatus 1.
[0043] 4, the beam irradiation device 2 operates based on a control command given from the PC 104 to heat the shaping plate 22 (step S1). In step S1, the beam irradiation device 2 irradiates the shaping plate 22 with the electron beam 15 through the opening 30a of the mask cover 30, and scans the shaping plate 22 with the electron beam 15. As a result, the shaping plate 22 is heated to a temperature at which the powder material 32 is provisionally sintered.
[0044] Next, the powder material 32 is spread on the shaping plate 22 (step S2). In step S2, the plate moving device 26 operates based on a control command given from the PC 104 to lower the shaping plate 22 by a predetermined amount. The plate moving device 26 lowers the inner base 24 by a predetermined amount so that the upper surface of the shaping plate 22 is slightly lower than the upper surface of the powder material 32 spread on the shaping table 18. At this time, the shaping plate 22 is lowered by the predetermined amount together with the inner base 24.
[0045] Then, the powder supplying device 16 drops the powder material 32 supplied from the hopper 16a to the powder dropper 16b onto the modeling table 18 by the powder dropper 16b, and then moves the squeegee 16c from one end side to the other end side in the X direction to spread the powder material 32 on the inner base 24. At this time, the powder material 32 is spread on the modeling table 18 to a thickness equivalent to ΔZ. In addition, excess powder material 32 is collected in the collection box 21. At this time, the powder material 32 set in the process of step S8 of the previous layer is spread. For example, if the PC 104 determines that the powder material 32 was not properly spread in step S8 of the previous layer, two layers of powder material 32 are spread.
[0046] Next, the beam irradiation device 2 operates based on control commands given from the polarization amplifier control circuit 101 and the PC 104 to preheat the powder layer on the modeling plate 22, so-called powder heat (PH) (step S3). In this step S3, the powder layer is preheated to pre-sinter the powder material 32. Pre-sintering the powder material 32 can impart electrical conductivity to the powder material 32. This can suppress powder scattering in the main sintering step that is performed after the pre-heating step.
[0047] In step S3, the beam irradiation device 2 irradiates the powder material 32 on the printing plate 22 with the electron beam 15. The beam irradiation device 2 also scans the electron beam 15 over an area wider than the area for forming the model 38 (hereinafter also referred to as the "printing area"). As a result, the powder material 32 present in the printing area and the powder material 32 present around the printing area are both pre-sintered.
[0048] If the PC 104 determines that the powder material 32 was not properly spread in step S8 of the previous layer, two layers of powder material are spread in step S2. Therefore, the powder heat time in step S3 is made longer than normal. This allows the powder material 32 for two layers to be completely pre-sintered.
[0049] Next, a backscattered electron image (BSE image) before the main melting is acquired (step S4). In step S4, first, the beam irradiation device 2 operates based on control commands given from the polarization amplifier control circuit 101 and the PC 104 to scan the electron beam 15 on the pre-sintered region where the pre-sintered powder material 32 exists. At this time, the beam irradiation device 2 reduces the electron beam current of the electron beam 15 as much as possible and irradiates the electron beam 15 while focusing it on the manufacturing surface 32a. Then, the detection unit 46 detects the backscattered electrons generated by the electron beam 15.
[0050] Furthermore, the detection unit 46 outputs the detected reflected electron signal to the PC 104 via the Pre-AMP 103 and the ADC 102. Then, the image processing unit of the PC 104 performs arithmetic processing on the reflected electron signal (reflected electron information) acquired from the detection unit 46 to acquire a reflected electron image (BSE image). Furthermore, the image processing unit stores the acquired BSE image before main melting (before melting) in the storage unit.
[0051] Next, the PC 104 judges the BSE image after melting of the previous layer and sets the melting conditions to be performed in step S6 described later (step S5). The melting conditions are the control conditions of the beam irradiation device 2 in the main melting process in step S6 described later. In step S5, the PC 104 acquires the BSE image acquired in step S7 when the previous layer is formed from the storage unit (hereinafter, referred to as the BSE image after melting of the previous layer). Then, the judgment of the BSE image after melting of the previous layer may use, for example, an unevenness analysis of the modeling surface 32a. That is, the frequency of the unevenness is detected, and if the frequency is higher than a threshold value, it is judged as not melted, and if the frequency is lower than the threshold value, it is judged as overmelted. Then, the PC 104 sets the melting conditions such as the irradiation spot diameter and scanning speed of the electron beam 15, the heat energy value supplied by the electron beam 15, etc. according to the melting degree of the powder material 32.
[0052] Furthermore, if the PC 104 determines that the powder material 32 was not properly spread in step S8 of the previous layer, two layers of the powder material 32 are spread in step S2. Therefore, the PC 104 sets the melting conditions so that the powder material 32 for two layers can be melted.
[0053] The melting condition setting process in step S5 may be performed between the acquisition of a post-melt BSE image in step S7 described below during the modeling operation of the previous layer and the main melting process in step S6 during the modeling operation of the current layer.
[0054] Next, the beam irradiation device 2 operates based on the melting conditions set in step S5 to melt and solidify the powder material 32 to perform final sintering (melt) (step S6). In step S6, the powder material 32 provisionally sintered as described above is irradiated with the electron beam 15 to melt and solidify, thereby performing final sintering of the powder material 32 as a provisionally sintered body.
[0055] In step S6, the beam irradiation device 2 specifies a printing region based on two-dimensional data obtained by slicing the three-dimensional CAD data of the target object 38 at a certain thickness (a thickness corresponding to ΔZ), and selectively melts the powder material 32 on the printing plate 22 by scanning the electron beam 15 on this printing region. The powder material 32 melted by irradiation with the electron beam 15 solidifies after the electron beam 15 has passed. This forms the first layer of the object.
[0056] After the process of step S6 is completed, a backscattered electron image (BSE image) after the main melting, i.e., a post-melt BSE image, is acquired (step S7). In step S7, first, the beam irradiation device 2 operates based on control commands given from the polarization amplifier control circuit 101 and the PC 104 to scan the electron beam 15 on the pre-sintered region where the pre-sintered powder material 32 exists. At this time, the beam irradiation device 2 reduces the electron beam current of the electron beam 15 as much as possible and irradiates the electron beam 15 while focusing it on the modeling surface 32a. Then, the detection unit 46 detects the backscattered electrons generated by the electron beam 15.
[0057] The detection unit 46 also outputs the detected reflected electron signal to the PC 104 via the Pre-AMP 103 and the ADC 102. The detection unit 46 also outputs the detected reflected electron signal to the PC 104 via the Pre-AMP 103 and the ADC 102. The image processing unit of the PC 104 then performs arithmetic processing on the reflected electron signal acquired from the detection unit 46 to acquire a reflected electron image (BSE image).
[0058] Next, PC 104 compares the post-melt BSE image of the previous layer with the current pre-melt BSE image, and sets the supply amount of powder material 32 from powder supply device 16 for the next layer (step S8). In step S8, PC 104 acquires from the memory unit the BSE image acquired in step S7 when the previous layer was formed (hereinafter referred to as the post-melt BSE image of the previous layer). Furthermore, PC 104 acquires from the memory unit the pre-melt BSE image acquired in step S4 when the current layer was formed. Then, PC 104 compares the two BSE images, determines the degree of spreading of powder material 32, and sets the powder supply amount in step 2 for forming the next layer.
[0059] Here, if the difference between the two BSE images is minute, the PC 104 determines that the powder material 32 was not properly spread in this step 2. Then, in step S2 for the next layer, the powder supply amount for two layers is set.
[0060] The step of setting the powder supply amount shown in step S8 may be performed after the step of acquiring the current pre-melt BSE image in step S4. In this case, if the powder is not properly spread, it is possible to minimize the effect on the model 38 by reducing the melt current used in the immediately following melt.
[0061] Next, in preparation for spreading the powder material 32, afterheating (AH) is performed to heat the printing surface 32a (step S9). In step S9, the beam irradiation device 2 operates under the control of the polarization amplifier control circuit 101 and the PC 104 to irradiate the electron beam 15 onto the printing surface 32a through the opening 30a of the mask cover 30. At this time, the polarization amplifier control circuit 101 defocuses the electron beam 15 using an objective lens or the like provided in the beam irradiation device 2. This defocusing is a state in which the focal position of the electron beam 15 is shifted downward from the printing surface 32a, that is, an underfocus state.
[0062] Furthermore, the polarization amplifier control circuit 101 and the PC 104 control the beam irradiation device 2 to scan the electron beam 15 over a wider area than the opening 30a of the mask cover 30. As a result, the electron beam 15 is irradiated onto the entire surface 32a to be molded that is exposed to the opening 30a. The surface 32a to be molded is heated to a temperature at which the powder material 32 is provisionally sintered. When the surface 32a to be molded is heated to a predetermined temperature, the beam irradiation device 2 stops irradiating the electron beam 15.
[0063] Furthermore, if it is determined in step S8 that the powder material 32 has not been properly laid, two layers of powder material will be laid in the next layer. Therefore, the after-heat time in step S9 is made longer than normal to increase the temperature of the printing surface 32a. This makes it possible to prevent the temperature of the printing surface 32a from dropping too much even if two layers of powder material 32 are laid in step S2 of the next layer.
[0064] Next, the shaping plate 22 is lowered by a predetermined amount (ΔZ) (step S10). In step S10, the plate moving device 26 lowers the inner base 24 by ΔZ so that the shaping surface 32a is slightly lower than the upper surface of the powder material 32 spread on the shaping table 18.
[0065] Thereafter, the above steps S2 to S11 are repeated until the modeling is completed up to the final layer in step S11, that is, until the modeling of the modeled object 38 is completed. The modeling of the modeled object 38 is completed at the stage where the powder material 32 has been melted and solidified for the number of layers required to form the modeled object 38. In this way, the desired modeled object 38 is obtained.
[0066] Thus, according to the operation example of the 3D additive manufacturing apparatus 1 of this embodiment, the degree of spreading of the powder material 32 and the degree of melting of the model 38 are judged in steps S5 and S8 before and after the main melting in step S6. Then, the supply amount of the powder material 32 and the melting conditions in the next layer are set and corrected as necessary. This makes it possible to reduce the number of times the modeling of the model 38 fails.
[0067] Furthermore, when the powder material 32 is not properly laid or melted, the correction of the molding process is performed not on the layer where the problem occurred but on the next layer. Furthermore, the correction is performed by changing the supply amount of the powder material 32 in the next layer and the melting conditions of the melting process. This allows the throughput of the molding operation to be always performed at the same timing, and correction can be performed without deteriorating the throughput.
[0068] In addition, by carrying out the correction work on the next layer, it becomes unnecessary to carry out a heating process to promote the preliminary sintering after the preliminary sintering on the same layer. This makes it possible to prevent the preliminary sintered body from becoming harder than necessary, and makes it easy to carry out the blasting process that is carried out after the 3D modeling operation. In addition, it is possible to prevent the mechanical properties of the model 38 that has been subjected to the correction work from being different from those of the model 38 that has been produced without the correction work.
[0069] Although an example in which a BSE image is used to perform the determinations in steps S5 and S8 has been described, the present invention is not limited to this. For example, the determinations in steps S5 and S8 may be performed using the reflected electron signal without performing image conversion processing on the reflected electron signal (reflected electron information) detected by the detection unit 46.
[0070] 2. Example of backscattered electron image Next, examples of the backscattered electron images (BSE images) acquired in steps S4 and S7 will be described with reference to FIGS. FIG. 5 shows an example of a backscattered electron image acquired after powder heating.
[0071] The image processing unit performs arithmetic processing on the reflected electron signals acquired from the multiple detection units 46a, 46b, 46c, and 46d to generate a reflected electron image. Here, in the reflected electron image acquired after the powder heating in step S4, the image processing unit adds the first reflected electron signal A of the first detection unit 46a and the second reflected electron signal B of the second detection unit 46b, which are arranged opposite to each other. That is, the arithmetic expression is A+B. The third reflected electron signal C of the third detection unit 46c and the fourth reflected electron signal D of the fourth detection unit 46d, which are arranged opposite to each other, may be added (C+D). By using such an arithmetic expression, it is possible to acquire a reflected electron image in which the contour of the model 38 is emphasized. As a result, it becomes easier to check whether the powder material 32 has been properly spread, and in the process of step S8, the PC 104 can accurately perform the process of determining whether the powder material 32 has been properly spread.
[0072] FIG. 7 shows an example of a backscattered electron image acquired after the main melting. In the reflected electron image acquired after the main melting in step S7, the image processing unit subtracts the first reflected electron signal A from the second reflected electron signal B, or subtracts the third reflected electron signal C from the fourth reflected electron signal D. This makes it possible to acquire a reflected electron image in which the unevenness of the printing surface 32a of the object 38 is emphasized.
[0073] The arithmetic formula may be (AB) / (A+B) or (CD) / (C+D). That is, by dividing the subtraction signal of two reflected electron images by the addition signal of two reflected electron images, it is possible to suppress the influence of fluctuations in the electron beam current and noise. As a result, as shown in FIG. 7, it is possible to obtain a reflected electron image in which the unevenness of the printing surface 32a of the model 38 is emphasized. As a result, it becomes easier to check whether the powder material 32 has been properly melted, and the process of determining the degree of melting of the powder material 32 by the PC 104 can be accurately performed in the process of step S5.
[0074] 3. Example of powder material spreading condition evaluation Next, an example of determining the degree of spreading of the powder material 32 performed in step S8 will be described with reference to FIGS. Fig. 6 is a backscattered electron image acquired after powder heating, showing an example in which the powder material 32 was not properly spread. Note that the backscattered electron image shown in Fig. 6 is a backscattered electron image acquired by the calculation formula A+B.
[0075] If the powder material is properly laid, the reflected electron image will be a nearly completely black image (see FIG. 5). If no powder material is laid at all, the entire melted area in the previous layer will be white, and the other areas will be black, as shown in FIG. 6. If only a portion of the powder material is laid, a part of the melted area in the previous layer (the area where the powder material was laid) will be black, the remaining melted area (the area where the powder material 32 was not laid) will be white, and the remaining powder material 32 will be black.
[0076] Here, consider the three-dimensional coordinate system of xyz. Then, the data of the post-melt BSE image of the previous layer and the pre-melt BSE image of the current layer are digitized in the form of (x,y,z) for all pixel counts to create three-dimensional data of xyz. In other words, the position of the BSE image as the x coordinate, the position of the BSE image as the Y coordinate, and the brightness values of the BSE image corresponding to the X and Y coordinates are set. At this time, the whiter the image, the higher the brightness value, and the darker the image, the lower the value.
[0077] Then, 3D data is derived by taking the difference between the z coordinate values (brightness values of the BSE image corresponding to the X and Y coordinates) that correspond to the same x and y coordinates of the two 3D data. If no powder material is laid, the 3D data obtained by taking the difference between the post-melt BSE image of the previous layer and the pre-melt BSE image of the current layer will have z coordinate values (brightness values) that are nearly the same for all x and y coordinates. Therefore, it is expected that the z coordinate value will be close to 0 for all x and y coordinates.
[0078] On the other hand, if the powder material 32 is properly spread, the part of the model that was white in the previous layer will become black, so that the z-coordinate value in the xy coordinate indicating the position of the model in the three-dimensional data from which the difference is taken will be a brightness value indicating the difference between white and black (it will definitely be a value greater than 0). Therefore, two values are noted. The first value is the z-coordinate of the three-dimensional data from which the difference data is taken (the difference between the brightness and darkness of the two BSE images). A threshold value is then set for this value. The second value is the total number of pixels that exceed the threshold value of the z-coordinate of the three-dimensional data from which the difference data is taken (the difference between the brightness and darkness of the two BSE images), divided by the total number of pixels in the part where the BSE image has become white due to the presence of the model in the previous layer (hereinafter referred to as the powder spreading ratio). A threshold value can also be set for this powder spreading ratio, and if the value of the powder spreading ratio is smaller than this threshold, it is determined that the powder has not been spread properly. This makes it possible to determine the degree of spreading of the powder material 32 in step S8.
[0079] 4. Example of determining the degree of melting of powder materials Next, an example of the determination of the melting degree of the powder material 32 performed in step S5 will be described with reference to FIG. Figure 7 shows a backscattered electron image acquired after the main melting. Figure 7 shows an example including both a portion (i) where the powder material was relatively properly melted and portions (j) to (q) where the powder material was not properly melted. The backscattered electron image shown in Figure 7 is acquired using the formula (AB) / (A+B).
[0080] When the powder material 32 is properly melted, the top surface of the surface 32a to be molded becomes flat as shown in part (i) of FIG. 7. When the powder material 32 is not properly melted, the top surface of the surface 32a to be molded becomes very uneven as shown in parts (j) to (q) of FIG. 7. Here, the unevenness of the top surface can be regarded as a three-dimensional wave. Then, the maximum amplitude and maximum period of this three-dimensional wave are obtained. In addition, the unevenness of the top surface can be quantified in the form of three-dimensional coordinates (x, y, z) of xyz with all the number of pixels, and can be made into three-dimensional data of xyz. That is, the brightness value of the BSE image corresponding to the position as the X coordinate of the BSE image and the position X coordinate and Y coordinate of the BSE image are set.
[0081] Then, the maximum amplitude and maximum period are obtained from the three-dimensional data. Threshold values are set for the amplitude and period, and when either or both of the threshold values are exceeded, it is determined that the powder material 32 is not properly melted. This makes it possible to determine the degree of melting of the powder material 32, which is performed in step S5.
[0082] The present invention is not limited to the embodiment described above and shown in the drawings, and various modifications can be made without departing from the spirit of the invention described in the claims.
[0083] For example, in the above-mentioned embodiment, an example was described in which metal powder such as titanium, aluminum, iron, etc. was used as the powder material, but the present invention is not limited thereto, and resin, etc., may be used as the powder material. Also, an example was described in which an electron gun that irradiates an electron beam was used as a heating mechanism for preheating or melting the powder material, but the present invention is not limited thereto. For example, a laser irradiation unit that irradiates a laser may be used as the heating mechanism.
[0084] In the above-described embodiment, the detection unit 46 is disposed inside the radiation shield cover 28, but the present invention is not limited to this. The detection unit 46 may be disposed outside the radiation shield cover 28.
[0085] Although the example in which the PC 104 is applied as the control unit has been described, the present invention is not limited to this. As the control unit, a control unit having various kinds of calculation functions, such as an electron beam control unit that controls the beam irradiation device 2, can be applied.
[0086] In addition, the above-mentioned components, functions, processing units, etc. may be realized in part or in whole in hardware, for example, by designing an integrated circuit. In addition, the above-mentioned components, functions, etc. may be realized in software by a processor interpreting and executing a program that realizes each function. Information such as the program, table, file, etc. that realizes each function can be stored in a recording device such as a memory, a hard disk, or an SSD (Solid State Drive), or in a recording medium such as an IC card, an SD card, or a DVD.
[0087] In this specification, the words "parallel" and "orthogonal" are used, but these do not mean only "parallel" and "orthogonal" in the strict sense, but may also mean a "substantially parallel" or "substantially orthogonal" state that includes "parallel" and "orthogonal" and is within a range in which the respective functions can be exerted. [Explanation of symbols]
[0088] 1...3D additive manufacturing device, 2...beam irradiation device, 3...vacuum chamber, 15...electron beam, 16...powder supply device, 16a...hopper, 16b...powder dropper, 16c...squeegee, 16d...blade, 18...modeling table, 20...modeling box, 21...collection box, 22...modeling plate, 24...inner base, 26...plate moving device, 32...powder material, 32a...modeling surface, 38...modeled object, 42...camera, 44...shutter, 46...detection unit, 101...polarization amplifier control circuit, 102...digital conversion circuit (ADC), 103...preamplifier (Pre-AMP) 104...personal computer (PC, control unit), 105...display unit, 106...display screen
Claims
1. A molding plate, a powder supplying device for supplying a powder material to the build plate to form a powder layer; a beam irradiation device that irradiates the powder layer with an electron beam; a detection unit that detects reflected electrons generated when the electron beam is irradiated onto the powder material; a control unit for controlling the powder supplying device and the beam irradiation device, The control unit is acquiring a pre-main-melting reflected electron signal, which is a reflected electron signal detected by the detection unit after the powder material is spread by the powder supplying device and before the powder material is main-melted by the electron beam; In a modeling process of a layer previous to the current layer, a reflected electron signal after main melting of the previous layer is obtained, which is a reflected electron signal detected by the detection unit after the powder material is main melted by the electron beam; A supply amount of the powder material from the powder supplying device in the modeling process of the next layer is set based on the reflected electron signal before the main melting and the electron signal after the main melting of the previous layer. 3D additive manufacturing device.
2. The control unit sets a control condition of the beam irradiation device for a main melting step in the modeling process of the current layer based on the electronic signal after main melting of the previous layer. The three-dimensional additive manufacturing apparatus according to claim 1 .
3. The control unit has an image processing unit that generates a reflected electron image based on a pre-main-melting reflected electron signal and a post-main-melting electron signal of the front layer. The three-dimensional additive manufacturing apparatus according to claim 1 .
4. The detection unit is provided in plurality, The control unit performs arithmetic processing on a plurality of reflected electron signals detected by the plurality of detection units. The three-dimensional additive manufacturing apparatus according to claim 1 .
5. supplying powder material to a build plate by a powder supplying device to form a powder layer; acquiring a reflected electron signal before actual melting, which is a reflected electron signal detected by a detection unit after the powder material is spread by the powder supplying device and before the powder material is actually melted by an electron beam; a main melting step of irradiating the powder layer with the electron beam using a beam irradiation device to melt the powder material; acquiring a reflected electron signal after main melting of a previous layer, the reflected electron signal being detected by a detection unit after the powder material is main melted by the electron beam in a modeling process of a previous layer of a current layer; setting a supply amount of the powder material from the powder supplying device in a modeling process of a next layer based on the pre-main-melting reflected electron signal and the post-main-melting electron signal of the previous layer; A control method for a three-dimensional additive manufacturing apparatus comprising:
6. The method further includes a step of setting a control condition of the beam irradiation device for the main melting step in the modeling step of the current layer based on the electronic signal after the main melting of the previous layer. A method for controlling the three-dimensional additive manufacturing apparatus according to claim 5.
Citation Information
Patent Citations
Three-dimensional lamination molding method and three-dimensional lamination molding device
JP2021042410A
Method of manufacturing a component
US20150037599A1
Three-dimensional laminate molding apparatus and three-dimensional laminate molding method
JP2022138653A