Injection molding die, injection molding device, and manufacturing method of molded article

The multi-layer injection mold addresses CO2 emission and cycle time inefficiencies by maintaining high temperature during filling and rapid cooling, enhancing heat transfer and cooling efficiency for improved product quality and reduced energy consumption.

JP2024150285AInactive Publication Date: 2024-10-23PANASONIC HOLDINGS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023063630
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional injection molding processes face challenges in reducing CO2 emissions, particularly during mold temperature control operations, which are energy-intensive and limit cycle time efficiency due to uneven heat distribution and poor cooling efficiency, leading to defects and increased environmental burden.

Method used

An injection mold with a multi-layer structure comprising a base mold, a heat insulating layer, a lower layer with high thermal conductivity, and a surface layer with low thermal conductivity, designed to maintain high temperature during filling and rapid cooling post-filling, enhancing heat transfer and reducing cycle time.

Benefits of technology

The multi-layer mold structure improves heat transfer uniformity and cooling efficiency, allowing for shorter cycle times with improved product surface quality and reduced energy consumption, achieving low-temperature, short-time molding with minimal defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150285000001_ABST
    Figure 2024150285000001_ABST
Patent Text Reader

Abstract

To provide an injection molding die which can improve transferability from a mold surface to a resin and enable takeout of a product in a shorter molding cycle than heretofore.SOLUTION: An injection molding die includes a base mold, a heat insulation layer formed on the base mold and having a heat conductivity of 20 W / m K or under, an underside layer formed on the heat insulation layer and having a heat conductivity of 200 W / m K or over and 2000 W / m K or under, and a surface layer formed on the underside layer and having a heat conductivity of 15 W / m K or over and 2000 W / m K or under.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an injection molding die, an injection molding apparatus, a molding method, and a manufacturing apparatus that contribute to reducing CO2 emissions in an injection molding process.

[0002] As typified by the SDGs and carbon neutrality in recent years, environmentally friendly technological development is actively progressing. The applicant is also developing carbon neutral resin materials to reduce CO2 emissions. In light of the growing momentum of SDGs and carbon neutrality in the future, it is considered necessary to reduce CO2 emissions throughout the entire LCA (Life Cycle Assessment). For this reason, it is becoming important to develop an injection molding process that can reduce CO2 emissions not only from the resin materials used in products, but also from the manufacturing process of products that use those resin materials.

[0003] As a result of investigating the total CO2 emissions during one injection molding cycle, the highest amount of CO2 emissions (power consumption) was generated by the mold temperature control operation for warming the mold, followed by the injection and metering operations, material heating operation, and mold opening and closing operations. In order to reduce CO2 emissions, it is preferable to approach the mold temperature control operation, which accounts for a large proportion of CO2 emissions, or the injection and metering operations, but the approximate amount of CO2 emissions (power consumption) for the injection and metering operations is determined by the properties of the resin material being injected (mainly viscosity, etc.). For this reason, it is preferable to approach the mold temperature control operation, which is more versatile and likely to produce results, regardless of the properties of the resin material being injected.

[0004] The parameters that determine the amount of CO2 emissions (electricity consumption) during mold temperature control operation are (1) the control temperature and (2) the molding cycle time.

[0005] (1) Temperature control As the mold temperature increases, the amount of electricity required increases, so it is preferable to control the mold temperature at as low a temperature as possible. Although molding without temperature control is ultimately the most effective way to reduce CO2 emissions, the range of use is thought to be limited when various trade-offs (insufficient filling, poor appearance, etc.) are taken into account. In light of the above issues, this development aims to develop a molding process that is premised on mold temperature control.

[0006] (2) Molding cycle time Basically, the temperature control operation is always in operation during injection molding, and as the molding cycle time becomes longer, the amount of power consumption increases proportionally. Therefore, it is preferable to mold in as short a time as possible. Generally, shortening the cooling time is given as a method to shorten the molding cycle, but if the molded product is removed in an insufficiently cooled state, there is a tendency for the risk of mold release failure and secondary deformation to increase. Therefore, simply shortening the cooling time may lead to defects and reduced yields, which may actually increase the environmental burden. In this development, instead of the conventional approach of simply shortening the cooling time to determine the product removal temperature within a range where various trade-offs do not occur, we aim to develop a process that allows molding in a short time while maintaining the same product removal temperature as before by improving cooling efficiency. In view of the above, there is a demand for an injection molding process and molding apparatus that allows for short-time molding at low temperatures.

[0007] In response to the above-mentioned problems, an injection molding process has been developed using a mold having multiple layers, as shown in, for example, Patent Document 1. Fig. 1 is a schematic cross-sectional view showing the layer structure of a cross section of the molding mold described in Patent Document 1.

[0008] In Fig. 1, the molding die 10 is a die for injection molding a member (resin molded product) having a microstructure made of a resin material, and is preferably used for transfer molding of resin molded products such as microchips and optical elements having fine flow paths with a width of 1 to 1000 µm. The molding die 10 has a die body 12 (base die) having a roughly rectangular parallelepiped appearance and made of a metal material such as steel, and on the die body 12, a surface layer 13, a lower surface layer 14, and a heat insulating layer 15 are formed in this order from the transfer surface side.

[0009] The surface layer 13 is a layer for substantially forming the shape of the microchannel, and is formed by a transfer process described later. The surface layer 13 is formed on the mold body 2 via the lower surface layer 14 and the heat insulating layer 15, and is formed on the lower surface layer 14 with a thickness t1 in the range of 0.03 to 1.0 mm (preferably 0.1 to 0.5 mm). The surface layer 13 is made of a material having a thermal conductivity of 10 W / m·K or less, such as nickel composite alloy plating such as nickel-phosphorus, nickel-cobalt-phosphorus alloy plating, nickel-PTFE plating, and nickel boron plating, and a convex portion 13a is formed on the surface layer 13 (transfer surface side).

[0010] The protruding portion 13a as the transfer portion corresponds to the recessed portion (groove) of the microstructure formed in the resin molded product, and has a micro shape with a width W and a height H in the range of 0.1 to 1 mm. In particular, the protruding portion 13a may have a micro flow passage shape with a width W and a height H of 1 to 1000 μm, in which case a micro flow passage with a width and depth of 1 to 1000 μm can be formed in the resin molded product such as a microchip molded from the molding die 10. Preferably, the width W is 100 μm or less.

[0011] The lower layer 14 has the function of allowing the heat of the resin injected onto the surface of the surface layer 13 to spread quickly over the entire transfer surface. The lower layer 14 is sandwiched between the surface layer 13 and the heat insulating layer 15, and is provided with a thickness t2 in the range of 0.1 to 2.0 mm. The lower layer 14 has a higher thermal conductivity than the surface layer 13, and is specifically made of a material with a thermal conductivity of 60 W / m K or more, such as Ni plating, Cu plating, Cr plating, or Ni-Co plating.

[0012] The heat insulating layer 15 has a function of preventing the heat of the resin injected onto the surface of the surface layer 13 from spreading throughout the entire mold body 12, and is adapted to retain the heat in the area where the resin is injected and its vicinity. The heat insulating layer 15 is made of a material such as a ceramic material, a titanium alloy, or glass (zirconia in this example), and has a lower thermal conductivity than the lower surface layer 14, specifically, a thermal conductivity of 30 W / m·K or less (preferably 10 W / m·K or less). The heat insulating layer 15 is formed by a thermal spraying method described later, and has a thickness of 0.1 to 3.0 mm. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Patent No. 6124023 Summary of the Invention [Problem to be solved by the invention]

[0014] The present disclosure is an injection molding mold that solves the above-mentioned conventional problems, and aims to provide an injection molding mold that improves transferability from the mold surface to resin and enables the product to be removed in a molding cycle time shorter than conventional times. [Means for solving the problem]

[0015] In order to achieve the above-mentioned object, the injection molding die of the present disclosure has a base die, an insulating layer formed on the base die and having a thermal conductivity of 20 W / m·K or less, a lower surface layer formed on the insulating layer and having a thermal conductivity of 200 W / m·K or more and 2000 W / m·K or less, and a surface layer formed on the lower surface layer and having a thermal conductivity of 10 W / m·K or more and 2000 W / m·K or less. Effect of the Invention

[0016] The injection molding die according to the present disclosure makes it possible to efficiently conduct heat in the in-plane direction while preventing the heat from being lost to the die by the injected resin, and allows the die surface to be transferred uniformly and efficiently to the molded product surface, resulting in a good product surface. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a layer structure in a cross section of a molding die described in Patent Document 1. [Diagram 2] FIG. 1(a) is a diagram showing the temperature change on the surface of a product and at the center of the product thickness formed from resin in contact with the mold surface from the start of filling the resin into a mold having a layer structure described in embodiment 1 of Patent Document 1 to the completion of filling, and FIG. 1(b) is a diagram showing the temperature change on the surface of a product and at the center of the product thickness formed from resin in contact with the mold surface from the start of filling the resin into the product part in the mold to the removal of the product. [Diagram 3] 1 is a diagram showing schematic diagrams of resin cooling profiles in the injection molding die according to the first embodiment, a normal die, and the die described in Patent Document 1. FIG. [Figure 4] 1 is a table 1 showing a comparison between the layer structure on the surface of the injection molding die according to the first embodiment and the layer structure on the surface of the die described in Patent Document 1. [Diagram 5] 1 shows a layer structure of an injection molding die according to embodiment 1. [Figure 6] Table 2 shows a list of the thermal properties of each material. [Figure 7A]Table 3-1 shows the temperature cooling profile of the resin in a mold using surface layers of each material as Example 1 of the injection molding mold according to the first embodiment. [Figure 7B] Table 3-2 shows the temperature cooling profiles of the resins in Comparative Example 1, where the mold of Patent Document 1 shown in FIG. 3 was used, and in Comparative Example 2, where a normal mold was used. [Figure 8] 13 is Table 4 showing layer structure conditions and resin temperature cooling profiles for Example 2 which is an example of the injection molding die according to the second embodiment, and Comparative Examples 1 and 2. [Figure 9] 13 is Table 5 showing the appearance and cycle time of a molded product molded using the optimum layer configuration mold according to the third embodiment and a molded product molded using a normal mold. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] <About the process leading to the injection mold disclosed herein> The inventors of the present invention have found that in the conventional structure, the heat capacity per volume of the Ni-based alloy plating set in the surface layer is 3680 to 3740 kJ / (m 3 ·K), and the thermal conductivity is 10 W / m·K or less. Generally, the injected molten resin is cooled and solidified before being removed, so the relationship is resin temperature > mold temperature. It was previously thought that if the specific heat per unit mass was low, the energy required to raise the temperature by 1 K could be kept low.

[0019] However, the surface layer needs to have a certain thickness, and therefore a certain volume, and the inventors have found that, even if the specific heat per unit mass is low, if a certain volume is required for a metal with a high density as in the conventional configuration, the energy required to raise the temperature by 1K becomes relatively large.

[0020] In the above case, when the mold surface is heated by the resin heat, the energy per unit volume required to raise the temperature by 1K is high, so the heat of the resin is rapidly taken away and the mold surface is heated. Furthermore, in the above case, since the material is poorly conductive, a temperature difference occurs between the gate side and the flow end side of the product shape, and the temperature distribution on the mold surface becomes uneven, which may cause differences in the surface normality of the molded product. In addition, since the various platings set on the lower surface layer are all made of materials with a relatively high heat capacity per unit volume, the heat of the resin continues to be taken away even after heat transfer from the surface layer to the lower surface layer. In addition, there are various issues such as low heat transfer performance and reduced cooling efficiency due to the low thermal conductivity of the surface layer. Below, the temperature profile of the product surface and the center of the product thickness during injection molding is derived by analysis.

[0021] 2 is a diagram showing a temperature profile of a resin filled in a mold having a layer structure described in the embodiment 1 of Patent Document 1. In addition, various molding conditions were set as follows when deriving the temperature profile. In addition, Abaqus, which is a proprietary software for performing finite element analysis, was used for the heat transfer analysis. <Analysis conditions> Injection resin: Polypropylene, resin temperature 190℃, mold temperature 30℃, injection speed 100mm / sec, product thickness 4mm

[0022] FIG. 2(a) is a diagram showing the temperature transition of the surface of the product formed from the resin in contact with the mold surface and the center of the product thickness from the start of filling the resin into the product part in the mold to the completion of filling. It can be seen that the product surface drops by about 63°C from 138.5°C to 75.5°C in about 0.1 seconds immediately after the resin comes into contact with the mold surface. On the other hand, the center of the product thickness maintains its temperature from the start of filling to the completion of filling. FIG. 2(b) is a diagram showing the temperature transition of the surface of the product formed from the resin in contact with the mold surface and the center of the product thickness from the start of filling the resin into the product part in the mold to the removal of the product. In FIG. 2(b), the temperature of the product surface at the time of product removal is 39.6°C, and the temperature of the center of the product thickness is 65.2°C, both of which are low temperatures and can be expected to be effective in shortening the cycle time. However, the cooling efficiency from 5 seconds to 30 seconds after the start of filling is low, remaining at about 0.346°C / sec, and about 91% of the total cooling to the product removal temperature is completed within 5 seconds from the start of filling.

[0023] Before describing the embodiments, differences between the features of the injection molding die according to the present disclosure and those of Patent Document 1 will be described.

[0024] FIG. 3 is a diagram that shows a schematic view of a resin cooling profile in each of the injection molding die according to the present disclosure, a normal die, and the die of Patent Document 1.

[0025] In FIG. 3, the injection mold according to the present disclosure is intended to maintain a high temperature at the time of completion of filling, not at the time of contact with the resin, and is selected and configured to have a surface layer and a lower layer with a smaller heat capacity than the normal mold and the mold of Prior Document 1, and to prevent heat from being easily taken away by the mold side. In addition, the high temperature retention time is controlled by the thickness of the insulating layer (low thermal conductivity). In order to improve the appearance quality when shortening the cycle time, which is one of the problems to be solved in the present disclosure, it is considered that the transferability will be improved if the temperature at the time of completion of filling is higher than the temperature at the time of contact with the resin. With these configurations, the temperature at the time of contact with the resin tends to be lower than that of the normal mold and the mold of Prior Document 1, but the concept is that the temperature at the time of completion of filling is higher than that of the normal mold and the mold of Patent Document 1. In addition, the aim is to shorten the cycle time by rapidly cooling after the completion of filling, and the material selection and structure are such that the heat capacity and thickness per unit volume of the insulating layer are reduced to efficiently transmit the heat or cold of the base mold to which the cooling pipe is actually set.

[0026] Fig. 4 is Table 1 comparing the mold layer configuration of the present disclosure with the mold configuration of Patent Document 1. Fig. 6 is Table 2 showing a list of thermal properties of each material listed in Table 1 of Fig. 4. The inventors have found that a material with a small heat capacity per unit volume is preferable in order to realize the concept of the present disclosure of maintaining a high temperature until the completion of filling. The heat capacity per unit volume defined in the present disclosure is a characteristic expressed by the density of the material times the specific heat (heat capacity per unit mass). The smaller the density and specific heat of a material, the smaller the heat capacity per unit volume, and when the material comes into contact with the resin, it will warm up instantly without absorbing much of the resin heat. Conversely, if the heat capacity is high, it will warm up by absorbing a lot of the resin heat. Conventionally, metals with a small specific heat, which is the heat capacity per unit mass, have been used as metals that do not absorb the resin heat. However, when a certain thickness is required and a certain volume is to be provided, it is better to have a small heat capacity per unit volume. Specifically, as shown in FIG. 6, even a nickel alloy with a low specific heat per unit mass has a high density, so that the heat capacity per unit volume is 3738 kJ / m 3·K. On the other hand, aluminum alloys and graphite have high specific heat but low density, and the heat capacity per unit volume is 2700 kJ / m 3 K, 1896 kJ / m 3 ·K becomes relatively small.

[0027] In order to realize the concept of the present disclosure, a material with high thermal conductivity and low heat capacity per unit volume, such as graphite, is preferable for the surface layer, and three layers, including the surface layer, the heat insulating layer, and the base mold, are preferable from the viewpoint of mold cost. However, due to the hard and brittle characteristics of graphite, it is subject to rapid wear due to various pressures and the like generated in the injection molding process, and there are concerns about durability. Therefore, an injection molding mold having a laminated structure according to the present disclosure has been developed that is as close as possible to the characteristics of graphite and has a four-layer structure in total, in which a metal layer is provided on the surface layer and graphite is used as the bottom layer to play a role of durable protection, thereby making the most of the thermal properties of graphite.

[0028] Based on the concept explained in Fig. 3, the major difference between this disclosure and Patent Document 1 is the setting of the thermal conductivity and heat capacity per unit volume of the surface layer. Due to the difference in the thermal conductivity and heat capacity of the surface layer, the temperature profile from contact with the resin to the completion of filling changes, which is thought to improve the transferability of the mold surface to the product surface.

[0029] The laminated structure of the injection molding die according to the present disclosure reduces the amount of heat lost to the surface layer the moment the resin comes into contact with the surface layer, and the high thermal conductivity facilitates heat propagation in the in-plane direction, resulting in a uniform temperature on the surface of the die formed using this structure. In addition, the high thermal conductivity and small heat capacity per volume allow the product to be cooled uniformly and quickly over the entire surface.

[0030] Each aspect of the present disclosure will be described below.

[0031] The injection molding die according to the first aspect has a base die, an insulating layer formed on the base die and having a thermal conductivity of 1.0 W / m·K or less, a lower layer formed on the insulating layer and having a thermal conductivity of 200 W / m·K or more and 2000 W / m·K or less, and a surface layer formed on the lower layer and having a thermal conductivity of 10 W / m·K or more and 2000 W / m·K or less.

[0032] The injection molding die according to the second aspect is the die according to the first aspect, wherein the heat insulating layer has a heat capacity per unit volume of 1500 kJ / m 3 ·K or less, and the lower layer has a heat capacity per unit volume of 1900 kJ / m 3 ·K or less, and the surface layer has a heat capacity per unit volume of 3650 kJ / m 3 ·K or less is also acceptable.

[0033] The injection molding die according to a third aspect is the die according to the first or second aspect, wherein the lower surface layer is made of a carbon-based material.

[0034] The injection molding die according to a fourth aspect is the die according to the first or second aspect, wherein the heat insulating layer may be made of a resin-based material.

[0035] An injection molding apparatus according to a fifth aspect has the injection mold according to the first or second aspect.

[0036] A method for manufacturing a molded product according to the sixth aspect includes the steps of clamping a cavity mold and a core mold of an injection molding die according to the first or second aspect, injecting a resin into a cavity defined between the cavity mold and the core mold while the cavity mold and the core mold are clamped, and, after the resin has hardened, opening the cavity mold and the core mold and removing the molded product.

[0037] Hereinafter, an injection molding die according to an embodiment of the present disclosure will be described with reference to the accompanying drawings.

[0038] (Embodiment 1) FIG. 5 is a schematic cross-sectional view showing the layer structure of the cross section of the injection mold according to the first embodiment. FIG. 7A is Table 3-1 showing the resin temperature cooling profile of each material in the layer structure shown in Table 1 of FIG. 4 in the first embodiment. FIG. 7B is Table 3-2 showing the resin temperature cooling profile of Comparative Example 1 in which the mold of Patent Document 1 shown in FIG. 3 is used, and Comparative Example 2 in which a normal mold is used. Note that Table 3 in FIG. 7A shows the analysis result of the configuration of the first embodiment of Patent Document 1 as Comparative Example 1, and the analysis result of a mold manufactured from a single stainless steel as a general normal mold as Comparative Example 2. Abaqus, which is one of the proprietary software for performing finite element analysis, was used for the analysis. Note that the analysis is not limited to the above.

[0039] The analysis conditions for the three types of the present embodiment 1 and Comparative Example 1 were the same as those in Fig. 3, with the injection resin being polypropylene, the resin temperature being 190°C, the mold temperature being 30°C, the injection speed being 100mm / sec, and the product plate thickness being 4mm.On the other hand, only Comparative Example 2 was set as a general molding using a normal mold, with the injection resin being polypropylene, the resin temperature being 190°C, the mold temperature being 60°C, the injection speed being 100mm / sec, and the product plate thickness being 4mm.

[0040] The injection molding die 400 according to the first embodiment has a base die 404, a heat insulating layer 403 formed on the base die 404, a lower surface layer 402 formed on the heat insulating layer 403, and a surface layer 401 formed on the lower surface layer 402. The heat insulating layer 403 has a thermal conductivity of 20 W / m·K or less. The lower surface layer 402 has a thermal conductivity of 200 W / m·K or more and 2000 W / m·K or less. The surface layer 401 has a thermal conductivity of 10 W / m·K or more and 2000 W / m·K or less. According to this injection molding die 400, the thermal conductivity of the surface layer 401 and the lower surface layer 402 is equal to or higher than a predetermined value, so that it is possible to achieve both a shortened molding cycle time and improved transferability from the die to the resin.

[0041] Each of the members constituting this injection molding die 400 will be described.

[0042] <Surface layer> As shown in Table 1 of FIG. 4, the surface layer 401 is made of, for example, stainless steel (thermal conductivity: about 15 W / m K, heat capacity per unit volume: 3630 kJ / (m 3 ·K) or less), aluminum alloy (thermal conductivity: about 190W / m·K, heat capacity per unit volume: 2700kJ / (m 3 ·K) or less), beryllium copper (thermal conductivity: about 245W / m·K, heat capacity per unit volume: 3470kJ / (m 3 The surface layer 401 is not limited to the above, and may have a thermal conductivity of 10 W / m K or more and 2000 W / m K or less. In addition, the heat capacity per unit volume may be set to 3650 kJ / m 3 ·K or less is also acceptable. The thickness of the surface layer 401 may be in the range of, for example, 0.15 mm to 2.5 mm.

[0043] <Bottom layer> The lower layer 402 is made of, for example, graphite (thermal conductivity: about 200 W / m K, heat capacity per unit volume: 1900 kJ / (m 3 The thermal conductivity of the lower layer 402 is not limited to the above, and it is sufficient if the thermal conductivity is 200 W / m K or more and 2000 W / m K or less. By having the thermal conductivity within the above range, the heat of the resin can be quickly transferred to the base mold after filling is completed, thereby improving the cooling efficiency and shortening the cycle time. In addition, it is preferable that the thermal capacity per unit volume is 1900 kJ / m 3 ·K or less. The lower layer 402 may be made of a carbon-based material such as graphite or carbon nanotubes. The heat capacity per unit volume may be 1900 kJ / m 3 When the temperature is small, at .K or less, the resin heats up instantly without absorbing much of it when it comes into contact with the mold, and the drop in temperature of the resin from the start of resin filling to the end of filling can be suppressed. By effectively utilizing the resin heat in this way, the temperature of the resin can be kept high until the end of filling, improving the transferability from the mold surface to the resin. Furthermore, the thickness of the lower surface layer 402 may be in the range of, for example, 0.3 mm to 2.5 mm. By setting the thickness of the lower surface layer 402 in the above range, the overall volume of the lower surface layer 402 can be reduced, and the heat capacity of the entire lower surface layer 402 can be reduced. As a result, the heat that the lower surface layer 402 takes from the resin can be reduced, and the temperature at the completion of filling can be maintained higher than before.

[0044] <Cross section layer> Furthermore, the heat insulating layer 403 is made of, for example, epoxy resin (thermal conductivity: about 0.4 W / m K, heat capacity per unit volume: 1320 kJ / (m 3 The heat insulating layer 403 is not limited to the above, and may have a thermal conductivity of 20 W / m K or less. Also, the heat capacity per unit volume may be set to about 1500 kJ / m 3 The heat insulating layer 403 may be made of a resin-based material. Furthermore, the thickness of the heat insulating layer 403 may be in the range of, for example, 0.1 to 3.0 mm. By setting the thickness of the heat insulating layer 403 in the above range, it is possible to control the time for heat to propagate from the heat insulating layer 403 to the base mold 404, and it is also possible to control the time for which the temperature of the resin can be maintained high until the completion of filling.

[0045] <Base mold> The base mold 404 serving as a foundation is, for example, stainless steel. Note that the base mold 404 is not limited to the above. In addition, the surface temperature may be kept constant by, for example, passing cooling water through the inside of the base mold 404. The surface temperature of the base mold 404 is set to, for example, 30° C. in Example 1 of FIG. 7A and Comparative Example 1 of FIG. 7B, but is not limited thereto and may be set to 60° C. as shown in Comparative Example 2 of FIG. 7B. For example, by setting the temperature to 30° C., the cycle time can be shortened.

[0046] Furthermore, if this injection molding die is constructed entirely from a material with a small heat capacity per unit volume, less energy is required for temperature change, making it possible to lower the controlled temperature of the resin, improving the cooling efficiency after the resin is filled, and enabling molding to be completed in a short molding cycle time. In the example shown in Figs. 7A and 7B, the thickness of each layer is the same as that of the first embodiment of Patent Document 1, that is, the surface layer is 0.15 mm, the lower layer is 0.15 mm, and the heat insulating layer is 1.0 mm.

[0047] In Table 3-1 of Fig. 7A and Table 3-2 of Fig. 7B, the temperature T1 of the product surface when in contact with the resin is low in all mold configurations in which the surface layer 401 is made of stainless steel, aluminum alloy, or beryllium copper. For example, the temperature T1 of the product surface when in contact with the resin was 134°C for stainless steel (compared to Patent Document 1: -4.5°C, compared to a normal mold: -0.6°C), 128°C for aluminum alloy (compared to Patent Document 1: -10.5°C, compared to a normal mold: -6.6°C), and 125°C for beryllium copper (compared to Patent Document 1: -13.5°C, compared to a normal mold: -9.6°C). On the other hand, the temperature T2 of the product surface at 0.54 seconds from the start of filling (completion of filling) was high, which means that a high temperature could be maintained. Specifically, the product surface temperature T2 at the completion of filling was 111.1°C for stainless steel (compared to Patent Document 1: +35.6°C, compared to a normal mold: +34°C), 116°C for aluminum alloy (compared to Patent Document 1: +40.5°C, compared to a normal mold: +38.9°C), and 111.6°C for beryllium copper (compared to Patent Document 1: +36.1°C, compared to a normal mold: +34.5°C). With the same thickness as each layer in the embodiment 1 of Patent Document 1, the material configuration of the embodiment 1 can maintain a high temperature at the timing of the completion of filling (switching to pressure holding operation), which determines the transferability of the mold surface on the product surface. Therefore, it was confirmed that the injection molding die according to the embodiment 1 can improve the transferability of the mold surface on the product surface compared to Patent Document 1 and general molding using a normal die.

[0048] On the other hand, the product surface temperature T3 and the product thickness center temperature T4 at 30 seconds after the start of filling are lower in the configuration of Patent Document 1, and the product thickness center temperature T4, which is particularly likely to contribute to defects such as deformation and sink marks when released from the mold, is slightly higher by about 17.7 to 18.1°C in the product surface temperature T3 for all of the stainless steel, aluminum alloy, and beryllium copper in this embodiment 1. This is about 4.5 to 4.7°C higher than general molding using a normal mold made of stainless steel alone. From the above, when the injection molding mold according to embodiment 1 is used, it is slightly inferior to Patent Document 1 in terms of cycle time, but it has been confirmed that it is superior in terms of the transferability of the mold surface to the product surface. Also, compared to general molding using a normal mold,

[0049] In addition, in the injection molding die according to the first embodiment, when the results of the three types of surface layers, stainless steel, aluminum alloy, and beryllium copper, were compared, the product surface temperature T1 was highest for stainless steel, which has the highest heat capacity per unit volume, and the product surface temperature T2 was highest for aluminum alloy, which has the lowest heat capacity per unit volume. On the other hand, there was not much difference between the product surface temperature T3 and the product thickness center temperature T4 30 seconds after the start of filling, and the cycle shortening effect was smaller than in Patent Document 1, so it is considered necessary to optimize the thermal conductivity and thickness of the lower layer and the thermal conductivity and thickness of the heat insulating layer.

[0050] <Injection molding equipment> The injection molding apparatus according to the first embodiment has the above-mentioned injection mold. The injection mold may have, for example, a cavity mold and a core mold.

[0051] <Method of manufacturing molded products> The method for producing a molded article may include, for example, the following steps. (1) The cavity mold and the core mold of the injection molding die are clamped together. (2) With the cavity mold and the core mold clamped together, resin is injected into the cavity defined between the cavity mold and the core mold. (3) After the resin has hardened, the cavity mold and the core mold are opened and the molded product is removed. In this manner, a molded product can be obtained.

[0052] (Embodiment 2) In the present embodiment 2, taking into consideration the results and knowledge obtained in the present embodiment 1, the surface layer 401 is set to an aluminum alloy, and the thermal conductivity and thickness of the entire layer structure, including the lower surface layer 402 and the heat insulating layer 403, are optimized through analysis. Fig. 8 is Table 4 showing the resin temperature cooling profile in the injection molding die having the optimized layer structure in the present embodiment 2.

[0053] In Table 4 of FIG. 8, the surface layer 401 is made of an aluminum alloy (thermal conductivity: about 190 W / m K, heat capacity per unit volume: 2700 kJ / (m 3 The thickness of the graphite layer 402 is set to 0.3 mm, and the lower layer 403 is set to 0.3 mm. The lower layer 402 is set to 0.3 mm. The lower layer 402 is set to 0.3 mm. The lower layer 402 is set to 0.3 mm. 3 The heat insulating layer 403 is made of epoxy resin (thermal conductivity: about 0.4 W / m K, heat capacity per unit volume: 1320 kJ / (m 3 7B, Comparative Example 1 shows a resin temperature cooling profile in a general molding using a mold having the layer structure of the first embodiment of Patent Document 1, and Comparative Example 2 shows a resin temperature cooling profile in a general molding using a normal mold. In the second embodiment, the selection was made in consideration of the thermal properties, processing properties, and durability of materials available on the market so as to maximize the effect while considering the feasibility as a mold.

[0054] From the results in Table 4 in Figure 8, it was found that in the optimal layer configuration using aluminum alloy, the product surface temperature T2 was maintained at a high temperature of 102.3°C, while the product surface temperature T3 at 30 seconds after the start of filling was 43.1°C, and the product thickness center temperature T4 was 74.8°C, enabling efficient cooling. In addition, it was found that compared to general molding using a normal mold, the mold surface transferability to the product surface was improved, while a cycle time reduction of approximately 6.4 seconds was achieved (based on calculations).

[0055] (Embodiment 3) In this third embodiment, a mold was actually created with the optimal layer configuration obtained in the second embodiment, and the extent to which the appearance quality (mold surface transferability) and cycle time were improved and advanced compared to general molding using a normal mold made of only stainless steel was evaluated. In the third embodiment, in order to make it easier to evaluate the appearance quality, a cellulose fiber composite resin was used in which 55% by weight of cellulose fiber with an average fiber diameter of about 50 μm and an aspect ratio (fiber length / fiber diameter) of about 5 was composited as a filler in the resin. In general, resins composited with fillers can cause a phenomenon called fiber floating, in which the filler appears to float on the surface of the molded product, depending on the resin cooling and solidification process, and this phenomenon is generally considered to be a poor appearance.

[0056] In order to improve fiber floating, it is necessary to raise the temperature of the resin and the mold and create an environment in which the injected resin can maintain a molten state from the completion of filling until the application of dwell pressure. The reason for using cellulose-based fibers as a filler is that they have a very small fiber diameter and a high aspect ratio compared to other fillers. This increases the contact area between the cellulose-based fibers in the resin and the resin, which increases the flow resistance during injection, intentionally creating a situation in which fiber floating is likely to occur, and the effect of suppressing fiber floating can be confirmed more significantly.

[0057] Fig. 9 is Table 5 showing the appearance and cycle time of the molded product molded with the mold having the optimal layer configuration in the present embodiment 3 and with a normal mold. The molded product appearance in Table 5 in Fig. 9 is a schematic diagram, and the fiber floating is shown by a curved line. The fiber floating occurs at the leading edge in the direction of the resin flow. As shown in Table 5 of FIG. 9, the sample molded using the mold with the optimal layer configuration according to embodiment 3 had a cycle time 10 seconds shorter than that of the sample molded using a normal mold, and a molded product with a high-quality appearance and a low rate of fiber lifting was obtained. [Industrial Applicability]

[0058] The injection molding die according to the present disclosure is capable of shortening the molding cycle time while providing products with appearance quality equal to or better than those obtained by general injection molding using conventional normal dies. Furthermore, molding with low energy consumption can be achieved because the mold temperature control temperature can be lowered. These effects make it possible to obtain high-quality, high-yield molded products at low cost. [Explanation of symbols]

[0059] 10 Molding mold 12 Mold body (base mold) 13 Surface layer 13a Convex part 14 Bottom layer 15 Thermal insulation layer 400 Injection mold 401 Surface layer 402 Bottom layer 403 Cross section layer 404 Base Mold 501 Surface layer 502 Bottom layer 503 Insulation Layer 504 Base mold

Claims

1. An injection mold comprising: A base mold; A heat insulating layer having a thermal conductivity of 20 W / m K or less formed on the base mold; A lower layer having a thermal conductivity of 200 W / m·K or more and 2000 W / m·K or less formed on the heat insulating layer; a surface layer having a thermal conductivity of 10 W / m·K or more and 2000 W / m·K or less formed on the lower surface layer; An injection molding die having

2. In the injection mold The heat insulating layer has a heat capacity per unit volume of 1500 kJ / m 3 ・K or less, The lower layer has a heat capacity per unit volume of 1900 kJ / m 3 ・K or less, The surface layer has a heat capacity per unit volume of 3650 kJ / m 3 ・K or less, 2. The injection mold according to claim 1.

3. 3. The injection mold according to claim 1, wherein the lower surface layer is made of a graphite-based material.

4. The injection molding die according to claim 1 or 2, wherein the heat insulating layer is made of a resin-based material.

5. An injection molding apparatus comprising the injection mold according to claim 1 or 2.

6. A step of clamping the cavity mold and the core mold of the injection molding die according to claim 1 or 2; a step of injecting a resin into a cavity defined between the cavity mold and the core mold while the cavity mold and the core mold are clamped together; After the resin is cured, the cavity mold and the core mold are opened to remove the molded product. A method for producing a molded article, comprising:

Citation Information

Patent Citations

  • Manufacture of magnetic recording medium

    JP1986024023A