Nitrile rubber composition and rubber crosslinked product

A nitrile rubber composition with nitrile rubber, epoxidized natural rubber, and silica addresses dispersibility and mechanical strength issues, achieving high abrasion resistance and mechanical strength in crosslinked products without silane coupling agents, thereby lowering production costs.

JP2024150296AInactive Publication Date: 2024-10-23TOKYO MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023063648
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Nitrile rubber compositions containing silica as a filler face issues with poor dispersibility and reduced mechanical strength due to silica's hydrophilic surface, necessitating high-cost silane coupling agents that are easily removable.

Method used

A nitrile rubber composition comprising nitrile rubber, epoxidized natural rubber, and silica with an epoxy content of 1 to 20, which enhances dispersibility and mechanical strength without the need for silane coupling agents.

Benefits of technology

The composition achieves excellent abrasion resistance and mechanical strength in the crosslinked rubber product, reducing production costs and improving processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150296000001
    Figure 2024150296000001
  • Figure 2024150296000002
    Figure 2024150296000002
Patent Text Reader

Abstract

To provide a nitrile rubber composition which contains silica and can give a rubber crosslinked product excellent in wear resistance and mechanical strength.SOLUTION: The rubber composition contains a nitrile rubber, an epoxidized natural rubber, and silica and has an epoxy content in a rubber component of 1-20.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nitrile rubber composition and a cross-linked rubber product. [Background technology]

[0002] Nitrile rubber (acrylonitrile-butadiene rubber) with high abrasion resistance is known as a rubber used for spinning rolls. In the nitrile rubber for such spinning rolls, silica is preferably used as a filler from the viewpoint of preventing coloring of the fibers. For example, Patent Document 1 discloses a rubber composition containing acrylonitrile butadiene rubber, a polyether polymer, and silica.

[0003] However, since the surface of silica is highly hydrophilic, when silica is used as a filler, its dispersibility in rubber is extremely poor, and there is a risk that the mechanical strength of the obtained cross-linked rubber product will decrease. To address this problem, there are techniques for improving the dispersibility of silica, such as using a silane coupling agent or hydrophobizing silica, but both of these techniques require high processing costs, and a method for dispersing silica more easily is desired. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-115005 A Summary of the Invention [Problem to be solved by the invention]

[0005] The problem to be solved by the present invention is to provide a nitrile rubber composition which contains silica and is capable of giving a cross-linked rubber product having excellent abrasion resistance and mechanical strength. [Means for solving the problem]

[0006] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by containing nitrile rubber, epoxidized natural rubber, and silica and having an epoxy content of 1 to 20 in the rubber component, and have completed the present invention based on this finding.

[0007] [1] According to a first aspect of the present invention, there is provided a nitrile rubber composition comprising a nitrile rubber, an epoxidized natural rubber, and silica, and having an epoxy amount of 1 to 20 in the rubber component.

[0008] [2] According to a second aspect of the present invention, there is provided the nitrile rubber composition of the first aspect, wherein the content ratio of the nitrile rubber and the epoxidized natural rubber in the rubber component is 97:3 to 60:40 in terms of a weight ratio of "nitrile rubber:epoxidized natural rubber".

[0009] [3] According to a third aspect of the present invention, there is provided the nitrile rubber composition of the first or second aspect, which does not contain a silane coupling agent.

[0010] [4] According to a fourth aspect of the present invention, there is provided a cross-linked rubber product obtained by cross-linking the nitrile rubber composition according to any one of the first to third aspects.

[0011] [5] According to a fifth aspect of the present invention, there is provided a cross-linked rubber product obtained by cross-linking the nitrile rubber composition according to any one of the first to third aspects with sulfur.

[0012] [6] According to a sixth aspect of the present invention, there is provided a roll made using the cross-linked rubber product according to the fourth or fifth aspect. Effect of the Invention

[0013] According to the present invention, it is possible to provide a nitrile rubber composition which contains silica and is capable of giving a cross-linked rubber product having excellent abrasion resistance and mechanical strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] <Nitrile rubber composition> The rubber composition of the present invention is a rubber composition containing a nitrile rubber, an epoxidized natural rubber, and silica, and having an epoxy amount of 1-20 in the rubber component.

[0015] The epoxy amount in the rubber component contained in the nitrile rubber composition is 1 to 20, preferably 2 to 15, and more preferably 3 to 10. The epoxy amount in the present invention is an amount calculated by multiplying the epoxidation rate (mol%) of the epoxidized natural rubber by the content ratio (weight%) of the epoxidized natural rubber in the rubber component, and dividing the result by 100. By setting the epoxy amount within the above range, the obtained cross-linked rubber product can be made excellent in abrasion resistance, mechanical strength, and compression set resistance.

[0016] <Nitrile rubber> Nitrile rubber contains α,β-ethylenically unsaturated nitrile monomer units and conjugated diene monomer units.

[0017] The α,β-ethylenically unsaturated nitrile monomer forming the α,β-ethylenically unsaturated nitrile monomer unit is not particularly limited, but an ethylenically unsaturated compound having a nitrile group and preferably having 3 to 18 carbon atoms can be used. Examples of such α,β-ethylenically unsaturated nitrile monomers include acrylonitrile; α-halogenoacrylonitrile such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkylacrylonitrile such as methacrylonitrile and ethacrylonitrile; and the like. Among these, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is particularly preferred. These α,β-ethylenically unsaturated nitrile monomers may be used alone or in combination of two or more.

[0018] The content of the α,β-ethylenically unsaturated nitrile monomer units in the nitrile rubber component is 15 to 48% by weight, preferably 20 to 45% by weight, more preferably 25 to 40% by weight, and particularly preferably 30 to 40% by weight, based on the total monomer units.

[0019] The conjugated diene monomer forming the conjugated diene monomer unit is not particularly limited, but is preferably a conjugated diene monomer having 4 to 6 carbon atoms such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, etc., more preferably 1,3-butadiene and isoprene, and even more preferably a combination of 1,3-butadiene or 1,3-butadiene and isoprene, and particularly preferably a combination of 1,3-butadiene and isoprene, since it is possible to obtain a nitrile rubber composition having even better shape retention. Note that these conjugated diene monomers may be used alone or in combination of two or more.

[0020] When 1,3-butadiene and isoprene are used in combination to form the conjugated diene monomer units, the weight ratio of the 1,3-butadiene units to the isoprene units (1,3-butadiene units / isoprene units) is preferably 50 / 50 to 90 / 10, more preferably 60 / 40 to 90 / 10, and particularly preferably 70 / 30 to 85 / 15.

[0021] The content of the conjugated diene monomer unit in the nitrile rubber component contained in the nitrile rubber composition is preferably 45 to 85% by weight, more preferably 55 to 80% by weight, and particularly preferably 60 to 75% by weight, based on the total monomer units. By setting the content of the conjugated diene monomer unit within the above range, the obtained cross-linked rubber product can be excellent in mechanical properties while maintaining good rubber elasticity.

[0022] The nitrile rubber component contained in the nitrile rubber composition may contain, in addition to the α,β-ethylenically unsaturated nitrile monomer units and the conjugated diene monomer units, units of other monomers copolymerizable with the monomers forming these monomer units.

[0023] Such other monomers include α-olefin monomers, non-conjugated diene monomers, aromatic vinyl monomers, α,β-ethylenically unsaturated monocarboxylic acids and their esters, α,β-ethylenically unsaturated polycarboxylic acids and their monoesters, polyesters and anhydrides, crosslinking monomers, fluorine-containing vinyl monomers, and copolymerizable antioxidants.

[0024] The α-olefin monomer preferably has 2 to 12 carbon atoms, and examples thereof include ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene.

[0025] The non-conjugated diene monomer preferably has 5 to 12 carbon atoms, and examples thereof include 1,4-pentadiene, 1,4-hexadiene, vinylnorbornene, and dicyclopentadiene.

[0026] Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, and vinylpyridine.

[0027] Preferred examples of the α,β-ethylenically unsaturated monocarboxylic acid include acrylic acid, methacrylic acid, crotonic acid, and cinnamic acid. Examples of the α,β-ethylenically unsaturated monocarboxylic acid esters include (meth)acrylic acid esters having an alkyl group having 1 to 18 carbon atoms, such as methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, n-dodecyl acrylate, methyl methacrylate, and ethyl methacrylate (abbreviation for "methacrylic acid esters and acrylic acid esters"; the same applies below); methoxymethyl acrylate, methoxyethyl acrylate, ethoxypropyl acrylate, methoxybutyl acrylate, ethoxydodecyl acrylate, methoxyethyl methacrylate, methoxybutyl methacrylate, and ethoxypentyl methacrylate. (meth)acrylic acid esters having an alkoxyalkyl group having 2 to 18 carbon atoms; (meth)acrylic acid esters having a cyanoalkyl group having 2 to 12 carbon atoms, such as α-cyanoethyl acrylate, α-cyanoethyl methacrylate, and cyanobutyl methacrylate; (meth)acrylic acid esters having a hydroxyalkyl group having 1 to 12 carbon atoms, such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 2-hydroxyethyl methacrylate; and (meth)acrylic acid esters having a fluoroalkyl group having 1 to 12 carbon atoms, such as trifluoroethyl acrylate and tetrafluoropropyl methacrylate.

[0028] Examples of the α,β-ethylenically unsaturated polycarboxylic acid include maleic acid, fumaric acid, and itaconic acid. Examples of the α,β-ethylenically unsaturated polyvalent carboxylic acid monoester include monoalkyl maleates such as monomethyl maleate, monoethyl maleate, monopropyl maleate, and mono-n-butyl maleate; monocycloalkyl maleates such as monocyclopentyl maleate, monocyclohexyl maleate, and monocycloheptyl maleate; monoalkylcycloalkyl maleates such as monomethylcyclopentyl maleate and monoethylcyclohexyl maleate; monoalkyl fumarate esters such as monomethyl fumarate, monoethyl fumarate, monopropyl fumarate, and mono-n-butyl fumarate; monocycloalkyl fumarate esters such as monocyclopentyl fumarate, monocyclohexyl fumarate, and monocycloheptyl fumarate; and monoalkylcycloalkyl fumarate esters such as monomethylcyclopentyl fumarate and monoethylcyclohexyl fumarate. monoalkyl esters of citraconic acid such as monomethyl citraconic acid, monoethyl citraconic acid, monopropyl citraconic acid, and mono-n-butyl citraconic acid; monocycloalkyl esters of citraconic acid such as monocyclopentyl citraconic acid, monocyclohexyl citraconic acid, and monocycloheptyl citraconic acid; monoalkyl cycloalkyl esters of citraconic acid such as monomethylcyclopentyl citraconic acid and monoethylcyclohexyl citraconic acid; monoalkyl esters of itaconic acid such as monomethyl itaconic acid, monoethyl itaconic acid, monopropyl itaconic acid, and mono-n-butyl itaconic acid; monocycloalkyl esters of itaconic acid such as monocyclopentyl itaconic acid, monocyclohexyl itaconic acid, and monocycloheptyl itaconic acid; monoalkyl cycloalkyl esters of itaconic acid such as monomethylcyclopentyl itaconic acid and monoethylcyclohexyl itaconate; and the like. Examples of the α,β-ethylenically unsaturated polycarboxylic acid polyester include dimethyl maleate, di-n-butyl maleate, dimethyl fumarate, di-n-butyl fumarate, dimethyl itaconate, and di-n-butyl itaconate. Examples of the α,β-ethylenically unsaturated polycarboxylic acid anhydride include maleic anhydride and itaconic anhydride.

[0029] Examples of the crosslinkable monomer include polyfunctional ethylenically unsaturated monomers such as divinyl compounds such as divinylbenzene; di(meth)acrylic acid esters such as ethylene di(meth)acrylate, diethylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; and trimethacrylic acid esters such as trimethylolpropane tri(meth)acrylate; as well as self-crosslinkable monomers such as N-methylol(meth)acrylamide and N,N'-dimethylol(meth)acrylamide.

[0030] Examples of the fluorine-containing vinyl monomer include fluoroethyl vinyl ether, fluoropropyl vinyl ether, o-trifluoromethylstyrene, vinyl pentafluorobenzoate, difluoroethylene, and tetrafluoroethylene.

[0031] Examples of the copolymerizable antioxidant include N-(4-anilinophenyl)acrylamide, N-(4-anilinophenyl)methacrylamide, N-(4-anilinophenyl)cinnamamide, N-(4-anilinophenyl)crotonamide, N-phenyl-4-(3-vinylbenzyloxy)aniline, and N-phenyl-4-(4-vinylbenzyloxy)aniline.

[0032] A plurality of types of these copolymerizable other monomers may be used in combination. The content of the units of the other monomers in the nitrile rubber component is preferably 20% by weight or less, more preferably 10% by weight or less, and particularly preferably 5% by weight or less, based on the total monomer units.

[0033] The Mooney viscosity (ML1+4, 100°C) of the nitrile rubber is preferably 10 to 100, more preferably 20 to 90, and further preferably 30 to 85. By setting the Mooney viscosity of the nitrile rubber within the above range, the processability of the nitrile rubber composition can be improved, and the mechanical strength of the cross-linked rubber obtained from the nitrile rubber composition can be further improved.

[0034] The content of the nitrile rubber in the rubber component contained in the nitrile rubber composition is preferably 60 to 97% by weight, more preferably 76 to 92% by weight, and further preferably 86 to 92% by weight, based on 100% by weight of the rubber component. By setting the content of the nitrile rubber in the rubber component within the above range, the cross-linked rubber obtained from the nitrile rubber composition can be excellent in abrasion resistance, mechanical strength, and compression set resistance.

[0035] <Epoxidized natural rubber> The nitrile rubber composition contains epoxidized natural rubber as a rubber component in addition to nitrile rubber. The nitrile rubber composition of the present invention contains epoxidized natural rubber, which can improve the dispersibility of silica in the rubber composition, and therefore can improve the abrasion resistance, mechanical strength, and compression set resistance of the cross-linked rubber.

[0036] The epoxidized natural rubber preferably has an epoxidation rate of 5 to 60 mol%, more preferably 10 to 60 mol%, and even more preferably 20 to 60 mol%. The epoxidation rate is the ratio (mol%) of the number of epoxidized double bonds to the total number of double bonds in the rubber before epoxidation. The epoxidation rate can be determined as the ratio of the integrated value of the double bond portion to the aliphatic portion by subjecting the epoxidized natural rubber to nuclear magnetic resonance spectroscopy (NMR). By setting the epoxidization rate of the epoxidized natural rubber within the above range, the cross-linked rubber obtained from the nitrile rubber composition of the present invention can be made to have excellent abrasion resistance, mechanical strength, and compression set resistance.

[0037] The Mooney viscosity (ML1+4, 100°C) of the epoxidized natural rubber is preferably from 20 to 110, more preferably from 30 to 100, and further preferably from 40 to 90. By setting the Mooney viscosity of the epoxidized natural rubber within the above range, the processability of the nitrile rubber composition can be improved.

[0038] The content ratio of the nitrile rubber and the epoxidized natural rubber in the rubber component contained in the nitrile rubber composition is preferably 97:3 to 60:40, more preferably 92:8 to 76:24, and even more preferably 92:8 to 86:14, in terms of the weight ratio of "nitrile rubber:epoxidized natural rubber". By setting the content ratio of the nitrile rubber and the epoxidized natural rubber within the above range, the cross-linked rubber obtained from the nitrile rubber composition of the present invention can be made excellent in abrasion resistance, mechanical strength, and compression set resistance. The content ratio of the epoxidized natural rubber in the rubber component is preferably 3 to 40% by weight, more preferably 8 to 24% by weight, and even more preferably 8 to 14% by weight.

[0039] <Silica> The nitrile rubber composition of the present invention contains silica. The silica is not particularly limited, but for example, dry process white carbon, wet process white carbon, colloidal silica, precipitated silica, etc. can be used.

[0040] The silica preferably has a nitrogen adsorption specific surface area of ​​50 to 400 m as measured by the BET method. 2 / g, more preferably 140 to 250 m 2 / g, more preferably 180 to 240m 2 / g. When the specific surface area is in this range, the abrasion resistance, hardness, and tensile strength of the obtained cross-linked rubber product can be further improved. The pH of the silica is preferably less than 7, and more preferably 5 to 6.9. The nitrogen adsorption specific surface area can be measured by the BET method in accordance with ASTM D3037-81.

[0041] The amount of silica blended in the nitrile rubber composition of the present invention is preferably 5 to 200 parts by weight, more preferably 10 to 150 parts by weight, further preferably 20 to 100 parts by weight, and particularly preferably 30 to 70 parts by weight, relative to 100 parts by weight of the rubber component. By making the amount of silica blended within the above range, the dispersion of silica during production can be improved, and the abrasion resistance, mechanical strength, and compression set resistance of the obtained cross-linked rubber can be more appropriately improved.

[0042] <Other ingredients> The nitrile rubber composition preferably contains a crosslinking agent. Examples of the crosslinking agent include sulfur, halogenated sulfur, organic peroxides, quinone dioximes, organic polyamine compounds, and alkylphenol resins having a methylol group. Among these, sulfur is preferably used. The amount of the crosslinking agent is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition for heavy-duty tires.

[0043] The nitrile rubber composition may further contain a phenolic resin. By including the phenolic resin, the processability of the nitrile rubber composition can be improved, the hardness of the vulcanizate can be increased, and the abrasion resistance can be improved. As the phenolic resin, any of the general-purpose phenolic resins obtained by condensing phenols and aldehydes under an acidic catalyst or a basic catalyst can be used. As the phenols used in the preparation of the phenolic resin, carbolic acid, m-cresol, p-cresol, o-cresol, p-alkylphenol, etc. can be preferably used, and mixtures thereof can also be used. As the aldehydes used in the preparation of the phenolic resin, formaldehyde, acetaldehyde, etc. can be preferably used, and mixtures thereof can also be used.

[0044] As the phenolic resin, either a resol type phenolic resin or a novolac type phenolic resin can be used, and further, various modified phenolic resins can be used, and these may be blended together. Furthermore, the phenolic resin to be used may be selected according to the purpose, such as the degree of condensation of phenols with aldehydes, the molecular weight, the residual rate of residual monomers, etc., and since various grades with different physical properties are commercially available, such commercially available products may be used as appropriate.

[0045] The phenolic resin referred to here includes so-called phenolic resin precursors before three-dimensional crosslinking to become cured phenolic resins. In addition, examples of modified phenolic resins include resol-type phenolic resins modified with various thermoplastic polymers, and novolac-type phenolic resins. Thermoplastic polymers used for modifying modified phenolic resins are not particularly limited, and examples thereof include elastomers such as nitrile rubber, hydrogenated nitrile rubber, isoprene rubber, polybutadiene rubber, acrylic rubber, and ethylene acrylic rubber, polyamide resins, phenoxy resins, polyvinyl butyral resins, polyethylene terephthalate, polyurethane, methyl methacrylate copolymers, polyester resins, cellulose acetate polymers, and polyvinyl alcohol.

[0046] When the nitrile rubber composition contains a phenolic resin, the content of the phenolic resin in the nitrile rubber composition is preferably 1.5 to 30 parts by weight, and more preferably 3 to 20 parts by weight, based on 100 parts by weight of the rubber component.

[0047] In addition to the above-mentioned components, the nitrile rubber composition of the present invention may contain, in accordance with a conventional method, a required amount of each of compounding agents such as a crosslinking accelerator, a crosslinking activator, an antiaging agent, a filler (excluding the above-mentioned silica), an activator, a process oil, a plasticizer, a lubricant, a tackifier, a compatibilizer, a surfactant, and an antistatic agent.

[0048] When sulfur or a sulfur-containing compound is used as the crosslinking agent, it is preferable to use a crosslinking accelerator and a crosslinking activator in combination. Examples of the crosslinking accelerator include sulfenamide crosslinking accelerators, guanidine crosslinking accelerators, thiourea crosslinking accelerators, thiazole crosslinking accelerators, thiuram crosslinking accelerators, dithiocarbamic acid crosslinking accelerators, and xanthogenic acid crosslinking accelerators. Among these, those containing sulfenamide crosslinking accelerators are preferable. These crosslinking accelerators are used alone or in combination of two or more. The amount of the crosslinking accelerator is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, and particularly preferably 1 to 4 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition for heavy-duty tires.

[0049] Examples of the crosslinking activator include higher fatty acids such as stearic acid, zinc oxide, diethylene glycol, etc. These crosslinking activators may be used alone or in combination of two or more. The amount of the crosslinking activator is preferably 0.05 to 20 parts by weight, particularly preferably 0.5 to 15 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition for heavy load tires.

[0050] Examples of fillers other than silica include carbon black, calcium silicate, aluminum silicate, calcium carbonate, talc, aluminum hydroxide, alumina, clay, and mica. Among these, carbon black is preferred from the viewpoint of further improving the abrasion resistance of the resulting cross-linked rubber. These can be used alone or in combination of two or more. The amount of fillers other than silica is not particularly limited as long as it is within a range that does not impair the effects of the present invention.

[0051] Examples of carbon black include furnace black, acetylene black, thermal black, channel black, and graphite. Examples of channel black include EPC, MPC, and CC. Examples of furnace carbon black include SAF, ISAF, HAF, MAF, FEF, SRF, GPF, APF, FF, CF, SCF, and ECF. Examples of thermal black include FT and MT. Carbon black can be used alone or in combination of two or more kinds.

[0052] The ratio of the silica content to the total content of the fillers in the nitrile rubber composition (the total content of silica and fillers other than silica) is not particularly limited, but is preferably 30 to 100% by weight, more preferably 50 to 100% by weight, and even more preferably 80 to 100% by weight.

[0053] The nitrile rubber composition may contain other rubbers in addition to the nitrile rubber and the epoxidized natural rubber. Examples of the other rubbers include polyisoprene, emulsion-polymerized styrene-butadiene copolymer rubber, solution-polymerized styrene-butadiene copolymer rubber, styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, styrene-isoprene-butadiene copolymer rubber, acrylonitrile-styrene-butadiene copolymer rubber, cyclic olefin ring-opening polymer, and hydrogenated conjugated diene polymer. These rubbers may be used alone or in combination of two or more.

[0054] The content of rubbers other than the nitrile rubber and the epoxidized natural rubber in the rubber component contained in the nitrile rubber composition is preferably 10% by weight or less, more preferably 5% by weight or less, and further preferably 3% by weight or less, based on 100% by weight of the rubber component. Although not particularly limited, it is preferable that the nitrile rubber composition does not contain any rubber other than the nitrile rubber and the epoxidized natural rubber.

[0055] <Method of producing nitrile rubber composition> The nitrile rubber composition of the present invention can be produced by kneading the nitrile rubber, the epoxidized natural rubber, and the silica, as well as other components used as necessary, according to a conventional method. For example, the nitrile rubber, the epoxidized natural rubber, and other rubbers are put into a roll and kneaded, and further compounding agents such as silica are put into the roll and kneaded to obtain a nitrile rubber composition. The temperature during roll kneading is not particularly specified, but it is preferable to heat the roll surface temperature to 40°C to 50°C in advance. Other than the roll kneader, a closed type kneader such as a Banbury mixer, a pressure kneader, or an intermix can be used.

[0056] <Rubber cross-linked products> The cross-linked rubber product of the present invention is obtained by cross-linking the above-mentioned nitrile rubber composition. The cross-linking method of the nitrile rubber composition is not particularly limited, and may be selected according to the shape, size, etc. of the cross-linked rubber product. For example, the nitrile rubber composition may be filled in a mold and heated to cross-link simultaneously with molding, or a nitrile rubber composition that has been molded in advance may be heated to cross-link. The cross-linking temperature is preferably 100 to 200°C, more preferably 130 to 190°C, and the cross-linking time is preferably 1 minute to 24 hours, more preferably 2 minutes to 1 hour.

[0057] If the cross-linking is not sufficient to the inside in one step due to the shape, size, etc. of the cross-linked rubber product, secondary cross-linking may be performed by further heating. As the heating method, a general method used for cross-linking rubber, such as press heating, steam heating, oven heating, or hot air heating, can be appropriately selected.

[0058] The cross-linked rubber of the present invention is obtained by cross-linking the above-mentioned nitrile rubber composition, and is excellent in abrasion resistance, mechanical strength, and compression set resistance. In addition, since the nitrile rubber composition of the present invention does not contain a silane coupling agent, it can be produced at a lower cost. Due to these excellent properties, the cross-linked rubber of the present invention can be particularly suitably used as a spinning roll or a hulling roll. In addition, the cross-linked rubber of the present invention can be used for various purposes such as materials for various tire parts such as cap tread, base tread, carcass, sidewall, and bead parts in tires; materials for hoses, belts, mats, anti-vibration rubber, and various other industrial products; impact resistance improvers for resins; resin film cushioning agents; shoe soles; rubber shoes; golf balls; toys; and the like, making use of its excellent properties. EXAMPLES

[0059] The present invention will be described below in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" are by weight unless otherwise specified. In addition, various tests and evaluations were performed according to the following methods.

[0060] <Normal physical properties (tensile strength, elongation at break, tensile stress, hardness)> The nitrile rubber composition was placed in a mold measuring 15 cm in length, 15 cm in width, and 0.2 cm in depth, and press molded at 160°C for 15 minutes while applying a pressure of 10 MPa to obtain a sheet-shaped cross-linked rubber product. The obtained sheet-shaped cross-linked rubber product was punched out with a JIS No. 3 dumbbell to prepare a test piece. The obtained test piece was used to measure the tensile strength, elongation at break, and tensile stress (300% tensile stress) of the cross-linked rubber product according to JIS K6251, and the hardness of the cross-linked rubber product was measured using a durometer hardness tester (type A) according to JIS K6253-3.

[0061] <Compression set test> The nitrile rubber composition was pressed at a temperature of 160 °C for 20 minutes while applying pressure using a mold to obtain a cylindrical rubber crosslinked product with a diameter of 29 mm and a height of 12.5 mm. Then, using the obtained rubber crosslinked product, in accordance with JIS K6262, after placing it in an environment of 100 °C for 70 hours in a state where the rubber crosslinked product was compressed by 25%, the compression set was measured. The smaller this value, the better the compression set resistance.

[0062] <Taber Abrasion Test> A rubber crosslinked product sheet was prepared by press crosslinking the nitrile rubber composition at 160 °C for 15 minutes. Using the rubber crosslinked product sheet, in accordance with JIS K 6264-2, the abrasion loss (mg) was measured with a Taber abrasion tester under the conditions of a load of 9.8 N, an abrasion wheel H22, and a rotational speed of 60 rpm. Also, the abrasion index (%) was determined with the rubber crosslinked product sheet of Comparative Example 1 as the reference sample (index 100).

[0063] <DIN Abrasion Test> Rubber crosslinked product sheets were prepared by press crosslinking the nitrile rubber compositions prepared in the examples and comparative examples at 160 °C for 20 minutes. Using the rubber crosslinked product sheets, the DIN abrasion test defined in JIS K 6264-2:2005 was conducted to determine the abrasion loss (cc). The smaller the abrasion loss, the better the abrasion resistance. Also, the abrasion index (%) was determined with the rubber crosslinked product sheet of Comparative Example 3 as the reference sample (index 100).

[0064] <Example 1> Using a roll, 95 parts of nitrile rubber (trade name "Nipol DN3350", manufactured by Zeon Corporation, acrylonitrile unit content: 33% by weight, Mooney viscosity (ML1+4, 100 °C): 50) and 5 parts of epoxidized natural rubber (trade name "FGV ENR 50", manufactured by FGV, epoxidation rate: 50 mol%, Mooney viscosity (ML1+4, 100 °C): 75) were kneaded on a roll to obtain a uniform blend. Then, 1 part of stearic acid, silica (trade name "Nipsil VN3", manufactured by Tosoh Silica Corporation, BET specific surface area: 200 m 240 parts of 100% cellulose acetate / g) and 10 parts of plasticizer (trade name "Adeka Cizer RS-107", manufactured by ADEKA Corporation) were added to disperse silica. Next, 2 parts of antioxidant (trade name "Nocrac CD", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.5 parts of antioxidant (trade name "Nocrac MBZ", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 5 parts of zinc oxide, 0.5 parts of powdered sulfur (325 mesh), 0.5 parts of vulcanization accelerator (trade name "Noccela TT", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.8 parts of vulcanization accelerator (trade name "Noccela TET", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), and 1.5 parts of vulcanization accelerator (trade name "Noccela CZ", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added and kneaded to obtain a nitrile rubber composition. Since the epoxidation rate of the epoxidized natural rubber was 50 mol%, and the content of the epoxidized natural rubber in the rubber component was 5 weight %, the epoxy content of the nitrile rubber composition was 50 x 5 / 100 = 2.5. The obtained nitrile rubber composition was evaluated according to the above-mentioned method. The results are shown in Table 1.

[0065] <Examples 2 to 4> A nitrile rubber composition was obtained and evaluated in the same manner as in Example 1, except that the amounts of the nitrile rubber and the epoxidized natural rubber used were changed to those shown in Table 1. The results are shown in Table 1.

[0066] <Example 5> Nitrile rubber and epoxidized natural rubber were mixed in the same manner as in Example 1. Next, 2 parts of stearic acid, 65 parts of silica (trade name "Nipsil VN3", manufactured by Tosoh Silica Corporation), 3 parts of titanium oxide, and 1 part of diethylene glycol were dispersed, and then 10 parts of phenolic resin (trade name "PR-12687", manufactured by Sumitomo Bakelite Co., Ltd.), 10 parts of zinc oxide, 3 parts of powdered sulfur (325 mesh), 1 part of vulcanization accelerator (trade name "Noccela DM", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), and 0.2 parts of vulcanization accelerator (trade name "Noccela D", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added and kneaded with a roll to obtain a nitrile rubber composition. The obtained nitrile rubber composition was evaluated according to the above-mentioned method. The results are shown in Table 2.

[0067] <Comparative Example 1> A nitrile rubber composition was obtained in the same manner as in Example 1, except that the amount of nitrile rubber used was 100 parts and no epoxidized natural rubber was used, and evaluations were performed in the same manner. The results are shown in Table 1.

[0068] <Comparative Example 2> A nitrile rubber composition was obtained and evaluated in the same manner as in Example 1, except that the amounts of the nitrile rubber and the epoxidized natural rubber used were changed to those shown in Table 1. The results are shown in Table 1.

[0069] <Comparative Example 3> A nitrile rubber composition was obtained and evaluated in the same manner as in Example 5, except that the amounts of the nitrile rubber and the epoxidized natural rubber used were changed to those shown in Table 1. The results are shown in Table 2.

[0070] [Table 1]

[0071] [Table 2]

[0072] As shown in Tables 1 and 2, the nitrile rubber composition containing nitrile rubber, epoxidized natural rubber, and silica, and having an epoxy content of 1 to 20 in the rubber component, allowed the obtained cross-linked rubber to have excellent abrasion resistance and mechanical properties.

Claims

1. Contains nitrile rubber, epoxidized natural rubber, and silica, A nitrile rubber composition having an epoxy content of 1 to 20 in the rubber component.

2. The nitrile rubber composition according to claim 1, wherein the content ratio of said nitrile rubber and said epoxidized natural rubber in the rubber component is 97:3 to 60:40 in terms of a weight ratio of "nitrile rubber:epoxidized natural rubber".

3. The nitrile rubber composition according to claim 1 or 2, which does not contain a silane coupling agent.

4. A cross-linked rubber product obtained by cross-linking the nitrile rubber composition according to claim 1 or 2.

5. A cross-linked rubber product obtained by cross-linking the nitrile rubber composition according to claim 1 or 2 with sulfur.

6. A roll made using the cross-linked rubber product according to claim 4.

Citation Information

Patent Citations

  • Rubber composition for roll and rubber roll comprising the same

    JP2001115005A