Floor slub and connection structure thereof, connection method of floor slub and connection structure thereof, precast floor slab, and connection part of floor slub
The use of continuous fiber reinforcement and short steel fibers in precast floor slabs addresses corrosion and workability issues, ensuring durable and efficient construction of floor slab connections.
Patent Information
- Application Number
- JP2023147897
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2023-09-12
- Publication Date
- 2024-10-23
AI Technical Summary
Existing floor slab connection structures face issues with corrosion of reinforcing bars and tendons, particularly in prestressed systems, leading to potential schedule delays and reduced workability due to the elongation of certain tendon materials like FRP under tensile load.
The use of precast floor slabs with continuous fiber reinforcement extending along the slab arrangement direction, terminating at connecting portions, and a filler material with short steel fibers to enhance adhesion and prevent corrosion, eliminating the need for prestressing and reducing the width of the connection portion.
This approach eliminates corrosion risks, improves workability by simplifying construction, and enhances the structural integrity and durability of the connection, while maintaining high tensile strength and reducing the likelihood of cracking.
Smart Images

Figure 2024150386000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a deck slab and its connection structure, a construction method for the deck slab and its connection structure, a precast deck slab, and a deck slab connection portion. [Background technology]
[0002] In recent years, many deck replacement works for bridges and the like have been carried out. Patent Document 1 discloses a deck and its connection structure in which decks are connected to each other with filler. The deck is a precast deck with built-in reinforcing bars, and the filler contains steel fiber or vinylon fiber. Prestress is sometimes applied to precast decks to control cracks. Patent Document 2 discloses a tensioning method for precast decks. As tensioning materials for applying prestress, in addition to PC steel wires, tensioning materials using carbon fiber or resin fiber are described. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-2250 A [Patent Document 2] JP 2022-165352 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the deck and its connection structure described in Patent Document 1, the deck reinforcement is made of reinforcing bars. The reinforcing bars protrude into the connection to form a joint structure. For this reason, the deck and its connection structure may have reinforcing bars corroded over a long period of use. When prestressing the deck, the tendons may also corrode. If tendons such as FRP are used as described in Patent Document 2, the problem of corrosion of tendons does not occur. However, in general, depending on the type of FRP, the amount of elongation when a tensile load is applied is large, making tensioning difficult. For this reason, there is an inherent risk of delays in the deck replacement work, which requires early use.
[0005] An object of the present invention is to provide a deck and its connection structure which eliminates the possibility of corrosion and is easy to install. [Means for solving the problem]
[0006] The deck and its connection structure of the present invention includes a pair of precast decks and a connection part for the pair of decks. The pair of decks and the connection part include steel short fibers, and each deck has a continuous fiber reinforcement. The continuous fiber reinforcement extends along the arrangement direction of the pair of decks and the connection part, protrudes from the end face facing the connection part of the decks, and terminates at the connection part. Effect of the Invention
[0007] According to the present invention, it is possible to provide a deck slab and its connection structure which eliminates the possibility of corrosion and has excellent workability. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a perspective view of a structure and a steel girder according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the structure shown in FIG. [Diagram 3] FIG. 2 is a cross-sectional view of the structure shown in FIG. [Figure 4] FIG. 11 is a cross-sectional view of a structure of a comparative example. [Diagram 5] FIG. 1 is a diagram showing the tensile softening properties of a deck slab in an embodiment and a comparative example. [Figure 6] FIG. 13 is a diagram showing the rate of change in length at a connection portion in an embodiment and a comparative example. [Figure 7] FIG. 1 is a diagram showing the tensile softening properties of a connection portion in an embodiment and a comparative example. [Figure 8] FIG. 1 is a diagram showing the shape of the deck used in the test. [Figure 9] FIG. 9 is a diagram showing the relationship between beam center displacement and load of the test specimen shown in FIG. [Figure 10] FIG. 9 is a diagram showing the state of cracks after destruction of the test specimen shown in FIG. [Figure 11] This figure shows the change in total crack width in the uniform bending section of Rn and G specimens. [Figure 12] FIG. 1 is a diagram showing the shape of a test specimen used in a test of a connection portion. [Figure 13] FIG. 13 is a diagram showing the relationship between beam center displacement and load of the test specimen shown in FIG. [Figure 14] FIG. 13 is a diagram showing the state of cracks after the test specimen shown in FIG. 12 is broken. [Figure 15] FIG. 13 is a diagram showing the load and the number of repetitions in a wheel load running test. [Figure 16] FIG. 1 is a diagram showing the shape of a test specimen used in a test for fatigue durability of a connection portion. [Figure 17] This figure shows the relationship between the number of loading cycles of the test specimen shown in Figure 16 and the deflection of the deck. [Figure 18] FIG. 17 is a diagram showing the distribution of deflection of the deck in the bridge axis direction of the test specimen shown in FIG. 16. [Figure 19] FIG. 17 is a diagram showing a cross section of the joint of the test specimen shown in FIG. 16. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the deck and its connection structure (hereinafter referred to as structure 1) of the present invention will be described with reference to the drawings. In the following description, the direction in which the steel girder 3 extends, i.e., the longitudinal direction of the steel girder 3, is referred to as the girder direction X, and the width direction of the steel girder 3 is referred to as the girder width direction Y. The girder direction X is parallel to the arrangement direction of the pair of decks 2A, 2B and the connection portion 4. The girder direction X and the girder width direction Y are approximately perpendicular to each other, and the girder direction X and the girder width direction Y are approximately perpendicular to the vertical direction Z. FIG. 1 is a perspective view of the structure 1 and the steel girder 3, and FIG. 2 is a partial cross-sectional view of the steel girder 3 and the structure 1 along the line AA in FIG. 1. FIG. 3(a) is a cross-sectional view of the steel girder 3 and the structure 1 along the line BB in FIG. 1, FIG. 3(b) is an enlarged view of FIG. 3(a) showing the pair of decks 2A, 2B and their connection portion 4, and FIG. 3(c) is a cross-sectional view (plan view) along the line CC in FIG. 3(b).
[0010] As an example, the steel girder 3 is composed of four steel beams 31, and a large number of precast deck slabs 2 are arranged on top of the steel girder 3 in the girder direction X. Since the deck slabs 2 are attached one by one in order in the girder direction X, the deck slab that is installed on the steel girder 3 first is called the first deck slab 2A, and the deck slab 2 that is installed on the steel girder 3 immediately after the first deck slab 2A and adjacent to the first deck slab 2A is called the second deck slab 2B. Note that when there is no need to distinguish between the first deck slab 2A and the second deck slab 2B, they may simply be called deck slabs 2.
[0011] The deck 2 has a rectangular shape when viewed from above, and the arrangement direction of the pair of decks 2A, 2B and the connection parts 4 usually coincides with the girder direction X. However, the deck 2 installed on a curved road bridge may be curved to match the shape of the curve. Therefore, the girder direction X more generally means the direction along the arrangement direction of the pair of decks 2A, 2B and the connection parts 4.
[0012] The deck slabs 2 are precast decks made of concrete reinforced with continuous fiber reinforcement. The length of each deck slab 2 in the girder direction X is 2 to 3 m, and the length in the girder width direction Y is longer than the overall width of the steel girder 3. Connections 4 are provided between the deck slabs 2. The connection parts 4 are formed of filler material. The connection parts 4 are provided linearly in the girder width direction Y, and the width W of the connection parts 4 is constant in the girder width direction Y. The width W of the connection parts 4 (see Figures 3(b) and 3(c)) is about 180 mm, but can be appropriately selected from a width of about 140 to 250 mm. The composition of the deck slabs 2 and the connection parts 4 will be described later.
[0013] A wall parapet substructure 5 is provided on both ends of the deck slab 2 in the girder width direction Y, and a wall parapet superstructure (not shown) is installed above the substructure. The deck slab 2 has a flat plate-shaped main body 21 and a number of haunches 22 provided on the underside of the main body 21. The haunches 22 extend in the girder direction X and are provided in positions facing the steel beams 31. In other words, the deck slab 2 is fixed to the steel girder 3 at the positions of the haunches 22.
[0014] The deck 2 has continuous fiber reinforcement 6 extending in the girder direction X and tension members 7 extending in the girder width direction Y. Both the continuous fiber reinforcement 6 and tension members 7 have the shape of a long and thin rod. The continuous fiber reinforcement 6 is provided in multiple rows in the girder width direction Y and in two stages in the thickness direction (vertical direction Z) of the deck 2, but the arrangement and number of the continuous fiber reinforcement 6 and the number of stages in the thickness direction are not particularly limited. The continuous fiber reinforcement 6 extends linearly over its entire length in the girder direction X and penetrates the deck 2 in the girder direction X. The continuous fiber reinforcement 6 terminates at the connection parts 4 on both sides of the deck 2. That is, the continuous fiber reinforcement 6 starts from the connection part 4 on one side of the deck 2, penetrates the deck 2, and terminates at the connection part 4 on the other side of the deck 2. The continuous fiber reinforcement 6 protrudes from each end face (only end faces 8A and 8B are shown) facing the connection parts 4 on both sides of the deck 2. A rib is provided on the outer periphery of the continuous fiber reinforcement 6, but excluding this rib, the outer diameter of the continuous fiber reinforcement 6 is constant in the length direction. In other words, no enlarged diameter portion such as a mechanical fixing portion is provided at the tip of the continuous fiber reinforcement 6.
[0015] In addition, since the deck 2 and the connection parts 4 are installed alternately in the girder direction X in large numbers, the continuous fiber reinforcement 6 usually penetrates the deck 2. However, for the deck 2 at the end, i.e., for the deck 2 having the connection parts 4 only on one side, one end of the continuous fiber reinforcement 6 terminates inside the deck 2, and the other end protrudes from the end face 8A or 8B of the deck 2. In addition, for the deck 2 that is curved, the continuous fiber reinforcement 6 may be curved along the shape of the deck 2, but it is also possible to arrange multiple linear continuous fiber reinforcements 6 via lap joints. In this case, too, one end of the continuous fiber reinforcement 6 terminates inside the deck 2, and the other end protrudes from the end face of the deck 2.
[0016] The tendons 7 extend between both ends of the deck slab 2 in the girder width direction Y, and apply a compressive force in the girder width direction Y to the deck slab 2. The tendons 7 are provided in multiple rows in the girder row direction X, and in two rows in the thickness direction (vertical direction Z) of the deck slab 2, but the number of tendons 7, the number of rows, and the number of rows in the thickness direction are not particularly limited. The compressive force is applied in advance at a factory or the like. Ribs are provided on the outer periphery of the tendons 7, but excluding these ribs, the outer diameter of the tendons 7 is constant in the length direction.
[0017] The continuous fiber reinforcement 6 is preferably one that is resistant to corrosion, and in this embodiment is made of synthetic resin. In addition, for reasons that will be described later, it is preferable that the continuous fiber reinforcement 6 has a high adhesive strength. From this viewpoint, glass fiber reinforced plastic (GFRP) is particularly preferable, but aramid fiber, carbon fiber reinforced plastic (CFRP), etc. may also be used. The tension member 7 is also made of synthetic resin such as FRP.
[0018] The continuous fiber reinforcement 6 of the first deck 2A and the continuous fiber reinforcement 6 of the second deck 2B protrude into the connection portion 4, and are offset from each other in the girder width direction Y to avoid interference. In addition, the continuous fiber reinforcement 6 of the first deck 2A and the continuous fiber reinforcement 6 of the second deck 2B are overlapped in the girder direction X to form a lap joint 8. The joint length of the lap joint 8 is 5d to 10d, preferably 5d to 7d (d: diameter of the continuous fiber reinforcement 6). Since no tension member or reinforcing bar is placed in the connection portion 4, workability is improved. In addition, since the width W of the connection portion 4 is small as described above, the effort of filling the connection portion 4 with a filler is also reduced, further improving workability.
[0019] FIG. 4 shows a deck and its connection structure of a comparative example. The advantages of this embodiment will be further described by comparing this embodiment with the comparative example. The structure 101 shown in FIG. 4(a) has a deck 102 made of reinforced concrete and a connection part 104 equipped with a U-shaped loop reinforcing bar. The deck 102 has a reinforcing bar 106 built in, and the reinforcing bar 106 forms a loop shape at the connection part 104. The deck 102 is prestressed in the girder width direction Y by a PC steel material 107. The connection part 104 is provided with a reinforcing bar 108 extending in the girder width direction Y. This structure is unlikely to crack, but the reinforcing bar may corrode after long-term use. The structure 1 of this embodiment does not use iron members such as reinforcing bars and PC steel materials inside the deck 2, so there is no possibility of corrosion and it can withstand long-term use.
[0020] It is also possible to replace the steel members with FRP in the structure 101 shown in FIG. 4(a). However, the strength of FRP is easily reduced at the bent portion. This makes it necessary to increase the number of FRP reinforcements to compensate for the loss of strength at the U-shaped bent portion, which may lead to poor workability and economic efficiency. In this embodiment, the continuous fiber reinforcement 6 has a straight shape including the connection portion 4, so that it is easy to ensure the strength of the continuous fiber reinforcement 6.
[0021] The structure 201 shown in FIG. 4(b) has a concrete deck 202 reinforced with a general FRP reinforcement material 206, and a connection part 204 with a linear lap joint. The deck 202 is prestressed in the girder width direction Y by an FRP tendon 207. Synthetic fibers are mixed into the concrete of the connection part 204. In this configuration, the tensile softening property of the concrete is small, as described later, and bond splitting cracks are likely to occur in the concrete around the FRP reinforcement material 206. Since the bond strength of the FRP reinforcement material 206 is small, it is necessary to make the connection part 204 long in the girder direction X to ensure the anchorage length. In this embodiment, the material of the continuous fiber reinforcement material 6 and the composition of the connection part 4 are devised, as described later, to make it possible to shorten the connection part 4.
[0022] The structure 301 shown in FIG. 4(c) has a concrete deck 302 and a connection part 304 made of mortar. The deck 302 is prestressed in the girder width direction Y by the FRP tendons 307, and is also prestressed in the girder length direction X by the FRP tendons 308. The FRP tendons 308 are housed in a sheath 309 provided on the deck 302 and a sheath joint 310 provided on the connection part 304. In this configuration, the deck 302 is compressed in two directions, so cracks are less likely to occur. In addition, since a joint structure is not required for the connection part 304, the width of the connection part 304 is also reduced. On the other hand, the deck 302 is required to have a protruding structure for tensioning work, and the structure of the deck 302 is likely to become complicated. In particular, although the FRP tendons 308 are not likely to corrode, they elongate a lot when a tensile load is applied, and therefore, skilled workers are required for tensioning work. For this reason, there is a risk of delay in the process when it is difficult to secure workers. In this embodiment, the above problem does not occur because a highly durable deck joint structure is established without applying prestress in the girder direction X to the deck 2 and the connection portion 4. Note that in this embodiment and the comparative example shown in Figures 4(a) to (c), prestress is applied in the girder width direction Y of the deck, but this process can be performed in a factory, so the above problem does not occur.
[0023] The structure 1 described above is constructed in the following procedure. First, the first deck 2A, which has been prestressed in the girder width direction Y, is installed on the steel girder 3. Next, the second deck 2B, which has been prestressed in the girder width direction Y, is installed on the steel girder 3. At this time, the second deck 2B is placed in the girder direction X with a gap between them with respect to the first deck 2A. In other words, the pair of decks 2A and 2B are placed so that the continuous fiber reinforcement 6 penetrates each of the decks 2A and 2B and terminates at the gap. The position and range of the gap coincide with the connection 4 shown in FIG. 2. Next, the gap is filled with a filler to create the connection 4 of the pair of decks 2A and 2B.
[0024] According to this procedure, there is no need to apply prestress to the first deck 2A and the second deck 2B in the girder direction X, so not only is tensioning unnecessary, but it also becomes easier to align the decks in advance. Also, since the width W of the connection 4 is about 180 mm as described above, construction of the connection 4 can be completed in a very short time. Furthermore, since no reinforcing bars or PC steel materials are used, there is no risk of corrosion. Thus, the structure 1 of this embodiment has many advantages over conventional structures in terms of long-term reliability and ease of construction.
[0025] However, despite the above advantages, the structure 1 of this embodiment may be disadvantageous in terms of the reliability of the lap joints 8, particularly the adhesion strength of the continuous fiber reinforcement 6. In addition, because no prestress is applied, cracks due to shrinkage are likely to develop in the deck 2 and the joints 4. Therefore, in this embodiment, the composition of the deck 2 and the joints 4 is mainly devised to prevent such potential problems from becoming apparent. Table 1 shows the composition (mixture example) of the concrete of the deck 2, and Table 2 shows the composition (mixture example) of the concrete of the joints 4.
[0026] [Table 1]
[0027] [Table 2]
[0028] The deck 2 includes steel short fibers. The steel short fibers have, for example, an outer diameter of 0.2 to 0.62 mm and a fiber length of 15 to 30 mm, and are distributed almost evenly in the deck 2 and are independent of each other. The mixing rate of the steel short fibers used in each embodiment is 0.5 to 1.5%, and by ensuring this mixing rate, the required performance can be imparted. Note that the embodiments shown in Table 1 are merely illustrative, and the mixing rate of the steel short fibers is not intended to be limited to the embodiments. The steel short fibers in the deck 2 have the effect of making the deck 2 structurally viable without applying prestress to the deck 2. Therefore, the only member that extends in the arrangement direction (beam direction X) of the pair of decks 2A and 2B and the connection part 4 of the deck 2 is the continuous fiber reinforcement material 6. As will be described later, this effect cannot be obtained sufficiently with synthetic fibers. Conventionally, the occurrence and progression of cracks were suppressed by applying compressive force through prestress. In this embodiment, the steel short fibers are used as an alternative to prestressing, so the progression of cracks is suppressed. As described above, the deck 2 does not contain reinforcing bars or PC steel, so even if cracks occur and moisture penetrates into the deck 2, damage such as concrete spalling due to corrosion and expansion of the steel will not occur. Furthermore, even if the waterproof layer (not shown) of the deck 2 is damaged, the steel short fibers suppress cracks and reduce water infiltration into the deck 2, so fatigue deterioration of the deck 2 is suppressed and the long-term reliability of the deck 2 can be improved.
[0029] The connection part 4 includes short steel fibers. The short steel fibers in the connection part 4 are the same as the short steel fibers in the deck 2, but may be different. The mixing ratio of the short steel fibers used in each embodiment is 1.0 to 2.0%. The short steel fibers are almost evenly distributed in the connection part 4 and are independent of each other. The short steel fibers in the connection part 4 improve the anchorage performance of the continuous fiber reinforcement 6 by increasing the adhesion strength. Since the adhesion strength is generally proportional to the adhesion length, it is necessary to ensure a long anchorage length when using a reinforcement material with low adhesion performance. In particular, the continuous fiber reinforcement 6 using a synthetic resin such as FRP may have low adhesion performance, and an anchorage length of 35 to 50d (d is the outer diameter of the continuous fiber reinforcement 6) may be required. However, in this embodiment, the anchorage length can be significantly reduced by using the continuous fiber reinforcement 6 with high adhesion performance and mixing the short steel fibers in the connection part 4. In addition, the continuous fiber reinforcement 6 with high adhesion performance can be anchored even in concrete that does not have a very high compressive strength, so the autogenous shrinkage of the concrete does not become excessively large. In this embodiment, by using the continuous fiber reinforcement 6 made of GFRP, the width W of the connection part 4 can be suppressed to about 180 mm (minimum 140 mm). Also, even if a material other than GFRP is used, the width W of the connection part 4 may increase, but a significant increase in the anchorage length can be suppressed.
[0030] Next, the effect of suppressing shrinkage cracks in the interfacial packing material of the joint 4 will be described. The joint 4 is prone to so-called restraint cracks. There are two main causes of restraint cracks. One is slippage between the interfacial packing material and the continuous fiber reinforcement 6. The joint 4 is subjected to shear loads due to vehicle travel, etc., and this shear load may cause minute slippage at the interface between the continuous fiber reinforcement 6 and the interfacial packing material. In this embodiment, the short steel fibers of the joint 4, combined with the use of the continuous fiber reinforcement 6 with high adhesion performance, increase the adhesion strength and suppress slippage between the interfacial packing material and the continuous fiber reinforcement 6. This makes it difficult for cracks in the joint 4 to progress. The other is the phenomenon in which the first and second decks 2 and 2 restrain the joint 4. Since the first and second decks 2 and 2 are sufficiently solidified at the time of installation at the site, the interfacial packing material of the joint 4 tries to shrink while being restrained by the first and second decks 2 and 2. This causes cracks to occur in the joints 4. However, by using continuous fiber reinforcement 6 with high adhesion properties in the joints 4, there is no need to make the compressive strength of the filler extremely high. Generally, the higher the compressive strength, the greater the autogenous shrinkage of concrete and the more likely it is that cracks will occur, but in this embodiment, a material that does not cause excessive autogenous shrinkage can be used for the filler (see Figure 6). This makes it possible to suppress the phenomenon in which the first and second decks 2 and 2 restrain the joints 4. Furthermore, by mixing short steel fibers, cracks in the joints 4 are less likely to progress.
[0031] As described above, it is necessary to improve the adhesion performance in the connection part 4. For this reason, it is preferable that the mixing rate of the short steel fibers in the connection part 4 is equal to or higher than the mixing rate of the short steel fibers in the pair of decks 2A, 2B. If the mixing rate of the short steel fibers in the connection part 4 is reduced, the adhesion strength decreases accordingly, and this may increase the width W of the connection part 4 and the amount of work at the site. From this viewpoint, it is preferable to add the short steel fibers to the connection part 4 at a mixing rate equal to or higher than that of the deck 2.
[0032] The mixing ratio of the steel short fibers contained in the connection part 4 is preferably adjusted to 0.5% or more and 2.5%. However, increasing the mixing ratio of the steel short fibers not only increases the cost but also reduces the fluidity when fresh, so it is preferable to set it to a maximum of 2.0%, more preferably 0.9 to 1.5%, and even more preferably 0.9 to 1.1%. On the other hand, the mixing ratio of the steel short fibers contained in the pair of deck slabs 2A, 2B can be selected from a smaller value, for example, a range of 0.5% to 1.0%, which is economically preferable because the structure can be established. Note that the examples shown in Table 2 are merely illustrative and are not intended to limit the mixing ratio of the steel short fibers to the examples.
[0033] The compressive strength of the concrete in the connection portion 4 is, for example, 120 MPa or more, more preferably about 140 MPa or more, and the compressive strength of the concrete in the deck 2 is, for example, about 80 MPa or more. Since the compressive strength of a deck is generally about 50 MPa, the structure 1 in this embodiment has sufficient strength. The connection portion 4, which requires high strength, has a compressive strength greater than that of the pair of decks 2A and 2B. As described above, the higher the compressive strength, the greater the autogenous shrinkage of the concrete and the greater the tendency for cracks to occur, but in this embodiment, excessive autogenous shrinkage is suppressed by not increasing the compressive strength excessively, and the combined use of a shrinkage reducing agent and an expansive material further suppresses shrinkage.
[0034] The possibility of corrosion of the steel short fibers cannot be denied. However, in this embodiment, as described later, the water-binder ratio of the concrete constituting the deck 2 and the connection parts 4 is reduced to increase density, which makes it difficult for water and oxygen necessary for corrosion reactions to penetrate. Also, unlike the reinforcing bars arranged near the surface of the deck 2, the steel short fibers are almost evenly distributed in the deck 2 and the connection parts 4 and are independent of each other, so even if some of the steel short fibers present at the very surface corrode, the corrosion of the steel short fibers is unlikely to cause significant cracking in the deck 2 and the connection parts 4.
[0035] FIG. 5 shows an example of the tensile softening properties of concrete (Example 1-1) mixed with steel short fibers of this embodiment and concrete (Comparative Example 1) mixed with polyvinyl alcohol (PVA) fibers. The tensile softening properties are the relationship between crack width and tensile stress, and indicate the tensile stress that can be borne when a certain crack width occurs. It can be said that the tensile softening properties of Example 1-1 and Comparative Example 1 are roughly the same in terms of the overall shape. However, since Example 1-1 uses steel short fibers, the tensile stress is large in the range where the crack width is small. That is, for deck slabs 2 and joints 4 used on expressways, the idea of suppressing the crack width to 0.2 mm or less is generally adopted, and the tensile stress of Example 1-1 is larger in this range than that of Comparative Example 1. Example 1-1 using steel short fibers has a higher tensile stress required to generate a certain crack width, i.e., a higher resistance to cracking, compared to Comparative Example 1 using PVA fibers, and the cracks are less likely to progress.
[0036] FIG. 6 shows the relationship between the number of days from water injection and the rate of change in length for Examples 2-1 to 2-10 and Comparative Example 2 (see Table 2). FIG. 7 shows the tensile stress (tensile softening properties) on the 28th day after water injection for Examples 2-1 to 2-10 and Comparative Example 2 (see Table 2). As shown in FIG. 6, the rate of change in length (shrinkage) is suppressed for Examples 2-1 to 2-10 compared to Comparative Example 2. Note that FIG. 6 shows only data up to 7 days of material age for Examples 2-2, 2-4, 2-7, and 2-8. As shown in FIG. 7, the tensile stress for Examples 2-1 to 2-10 is similar to that of Comparative Example 2. In other words, Examples 2-1 to 2-10 have suppressed shrinkage while maintaining mechanical properties similar to those of Comparative Example 2.
[0037] The composition of deck slab 2 is summarized below. The water-binder ratio is preferably 30% or less, more preferably 22-30%, and even more preferably around 25%. It is preferable to replace part of the Portland cement as a binder with ground granulated blast furnace slag or silica fume. Although not shown in Table 1, the maximum size of the coarse aggregate is 20 mm or less, and the unit absolute volume of the coarse aggregate is 0.225 m 3 / m3 The unit water content is preferably 175 to 185 kg / m 3 The volume ratio of fine aggregate in mortar is preferably 40% to 60%.
[0038] The composition of the connection part 4 will be summarized. The water-to-powder volume ratio is preferably 40-60%, more preferably 55%. It is preferable to replace part of the Portland cement as a binder with ground granulated blast furnace slag, fly ash, silica fume, etc. It is preferable to use a shrinkage reducing agent (an internally added high performance water reducing agent is acceptable). It is preferable to use an expansion material to suppress shrinkage of the joint 4. It is also preferable to use air-ground ferro-nickel slag (FNS) as fine aggregate. Although not shown in Table 2, the maximum size of the coarse aggregate is 13 to 15 mm, and the unit absolute volume of the coarse aggregate is 0.175 to 0.200 m 3 / m 3 The unit water content is preferably 135 to 175 kg / m 3 The volume ratio of fine aggregate in mortar is preferably 21% to 42%.
[0039] (Test Example) A test specimen for deck 2 was produced and several tests were carried out. The concrete used for deck 2 is steel fiber reinforced concrete with a design standard strength of 80MPa. The bridge axis direction (X direction) is an RC structure using GFRP, and deck 2 is joined together with gap lap joints. This eliminates the need for vertical tightening tension work in the bridge axis direction on-site. The direction perpendicular to the bridge axis (Y direction) is a PC structure using AFRP (aramid fiber FRP rods) as tensioning materials. Deck 2 is designed as a flat plate structure without ribs, making it easier to design and construct.
[0040] (1) Structural performance of decks using GFRP as reinforcement (a) Experimental overview Bending tests were conducted on beams using GFRP as reinforcement, and their crack properties and load-bearing behavior were compared. The test specimen, simulating a deck slab, had a wide cross-section of 200 mm thick and 400 mm wide, with three reinforcements placed on the top and bottom. The shape and dimensions of the test specimen are shown in Figure 8. Figure 8(a) shows the cross-section as seen from the side, while Figures 8(b) and 8(c) show the cross-sections of the plane perpendicular to the longitudinal direction of the beam. The shear span ratio was set to 4.5, and the uniform bending section was set to 600 mm, and the widths of all cracks that occurred in this section were measured.
[0041] The concrete used high-early-strength cement and ground granulated blast furnace slag as binders, with a water-binder ratio of 25%. Steel fibers with a diameter of 0.2 mm and a length of 15 mm were mixed in at 0.5% by volume. Assuming production in a factory, the mix was designed to achieve a compressive strength of 60 MPa after one day of steam curing. At 28 days of age, this reached 90-120 MPa. The compressive strength during loading tests (at ages of 14-21 days) was 90-94 MPa both with and without fibers.
[0042] A list of test specimens is shown in Table 3. Comparisons were made between rebar and GFRP with and without steel fibers mixed into the concrete. The rebar used was D19 (SD345), and the GFRP used was 18 mm nominal diameter with roughly the same cross-sectional area as D19, with ribs 1 mm high set at approximately 10 mm pitches on the surface. The guaranteed tensile strength of the GFRP was 1000 MPa, and Young's modulus was 60 GPa.
[0043] [Table 3]
[0044] (b) Experimental results Figure 9 shows the relationship between the beam center displacement and the load, and Figure 10 shows the crack characteristics after failure of each specimen. In all beams reinforced with steel bars, the concrete at the upper edge of the beam collapsed in compression after yielding. The addition of steel fiber increased the yield load and maximum load of the rebar by about 10%. No effect of steel fiber was observed on the number or spacing of cracks. In the G specimen, which is a GFRP-reinforced beam with steel fiber, the first bending crack occurred at a load of about 50kN, after which the load increased at a constant gradient and the concrete at the upper edge collapsed in compression when the load exceeded 300kN. The residual displacement after unloading was restored to about 20mm, indicating that the GFRP was sound. On the other hand, in the Gn specimen without steel fiber, the first crack occurred at about 50kN, and then as the load increased, diagonal cracks progressed to the load vicinity, and shear compression failure occurred at about 200kN. This is thought to be due to the fact that, as will be described later, GFRP has larger crack widths than reinforcing bars, which reduces the interlocking effect of coarse aggregate on diagonal crack surfaces, and the dowel effect of GFRP itself is small. It was found that these problems could be greatly improved by mixing in steel fibers.
[0045] Figures 11(a) and 11(b) show the transition of the total crack width in the equal bending section of the Rn and G specimens. Here, in the RC calculation ignoring the tensile resistance of the concrete, the load at which the stress of the reinforcing bars and GFRP reaches 140 MPa (corresponding to the limit value of the reinforcing bars when controlling the crack width in a general reinforced concrete structure) is 45 kN. Comparing at this load level, the crack width of the Rn specimen, which is a general reinforced concrete structure, was about 0.1 to 0.2 mm. In contrast, the G specimen with steel fiber did not crack at 45 kN, but the crack width when the crack that occurred at the smallest load was balanced with the load was about 0.2 mm. From the above, it was found that in a structure combining fiber reinforced concrete and GFRP, the crack width can be similarly controlled by controlling the stress of the reinforcing material to the same level as the reinforcing bars.
[0046] (2) Consideration of connection part 4 (a) Experimental overview A gapped lap joint was used for the joint 4. By increasing the concrete compressive strength and steel fiber mixing rate of the joint 4, the width of the joint 4 can be reduced, which is expected to improve workability. The fill concrete used here contains 1.0% steel fiber and uses silica fume premixed cement, with a mix that results in an actual compressive strength of 160 MPa or more at 28 days old. In addition, because shrinkage cracks are an issue at joint 4, an expansive material and shrinkage reducing agent are used to keep the amount of shrinkage as low as possible.
[0047] The determination of whether a gapped lap joint using GFRP is viable was made based on whether deformation such as bond splitting or cracking would occur until the tensile stress of the GFRP reached 345MPa. This assumes that the limit value of the stress of the GFRP during service will be the same as that of reinforcing bars, and takes into consideration that the bending strength of the deck will also be the same. A small double-pull test was carried out in advance, and it was confirmed that if the length of the joint 4 is five times the diameter of the GFRP, it can resist a tensile force of 345MPa or more, which is the GFRP tensile stress.
[0048] Figure 12 shows the shape and dimensions of the test specimens. The width of the test specimen was 825 mm, and the GFRP was arranged at a pitch of 150 mm. A shear key was provided on the joint surface of the connection part 4. The joint surface was coated with a retarder and roughened with a high washer. Three test specimens were used, with the joint lengths of the GFRP at the connection part 4 set at 5d, 6d, and 7d.
[0049] (b) Experimental results Figure 13 shows the relationship between the beam center displacement and the load, and Figure 14 shows the cracking condition after destruction. Figures 14(a) and 14(c) show the cracking condition on both sides, and Figure 14(b) shows the cracking condition on the front. In all test specimens, after the bending cracks occurred, the load increased at a certain rigidity, and then bond splitting cracks occurred in the GFRP at the joint, and the load decreased. The load at which bond splitting cracks occurred tended to increase as the length of the connection became longer. The maximum load was calculated without taking into account the tensile resistance of the concrete, and it was confirmed that all test specimens could withstand a load greater than the load at which the GFRP stress level was 345 MPa. The test results showed that the required strength could be achieved if the length of the connection was 5d or more, but in an actual structure, it is preferable to adopt 7d, taking into account the variation in material quality and construction errors.
[0050] (3) Confirmation of fatigue durability (a) Experimental overview A wheel load running test was conducted to confirm the fatigue durability of the deck joint. As shown in Figure 15, the load and number of repetitions were 250kN, which is equivalent to 100 years of traffic volume on the Tomei Expressway, 100,000 times, after which water was poured onto the deck surface and 250kN was applied again 100,000 times. The load was then increased by 50kN at a time and 40,000 repetitions were applied each time to confirm the damage condition. Figure 16 shows the dimensions of the test specimen. Figure 16(a) shows the plan view, Figure 16(b) shows the cross section, and Figure 16(b) shows the side view. The total length was 4.5m and the width was 2.8m, in accordance with NEXCO test method 442-2019. The deck span is a simply supported slab with a span of 2.5m. A trial design was made for a continuous slab with a span of 3.0m, and a prestress of about 2.0MPa was introduced with AFRP in the deck span direction so that the bending crack strength would be less than the design load.
[0051] The GFRP was placed at intervals of 150 mm, and the diameter was determined so that the stress generated under the design load would be 140 MPa or less. The test specimen was manufactured using the same procedures as those assumed for an actual bridge. After manufacturing two deck panels with a length of 2.15 m, they were lined up on a platform so that the length of the connection was 7d (connection part 4 width 200 mm), and concrete was poured into the joints to join them. As the test specimen was short at 4.5 m in total length, an elastic FEM analysis was conducted to ensure that the deformation would be equivalent to that in the case where the deck was continuous, and elastic support beams of H-shaped steel (300H) were attached to the ends of the test specimen.
[0052] (b) Test results (i) Changes in deck deflection Figure 17 shows the relationship between the number of loading cycles and the deflection of the deck. In all steps, the deflection was standardized to the value for a loading load of 250 kN. Up until STEP 3, there was almost no change in either the residual displacement or the live load deflection, and it is believed that the impact of fatigue is very small. In STEP 4, there was a slight increase in the residual displacement, but no change was observed in the live load deflection, and it is believed that there is almost no impact on the structural performance. From STEP 5 to 7, the residual deflection increases as the load increases, but the increase in the live load deflection is not that great, confirming that the decline in structural performance is limited. The running test was terminated in STEP 7 (load of 490 kN) when the stroke of the test equipment reached its limit after approximately 17,000 cycles.
[0053] Figure 18 shows the deflection distribution of the deck in the bridge axis direction. The deflection increased with an increase in the number of loadings and the load, but the increase was small up to STEP 5, and it is believed that no sudden deterioration in performance occurred. Even in STEP 7 (when the test in Figure 18 was completed), the deflection distribution maintained continuity at the joints, confirming that the bridge possessed supporting performance and sufficient fatigue resistance.
[0054] (ii) Cracks on the underside and cut surface of the deck When the cracks on the underside of the specimen were checked, some of the undersides were found to have been buoyed, but the surface concrete did not spall off even after STEP 7. This is thought to be the effect of short fibers. In addition, from STEP 2 onwards, loading was performed with water on the top surface of the deck, but in STEP 4, water leakage from the joints on the supports was observed, and in STEPs 6 and 7, water seepage was also observed in the joints in the centre of the deck span. Looking at the cross section of the deck span direction, horizontal cracks were found at the upper GFRP position, and punching shear cracks occurred. The shear key installed on the joint surface had a crack in the middle on the convex side, but no displacement occurred. Figure 19 shows the cut surface of the joint. No pull-out or adhesion breakage of the GFRP was observed, and unlike static loading, destruction did not occur due to the pull-out of the GFRP. [Explanation of symbols]
[0055] 1 Structure (deck and its connecting structure) 2 Floor slab 4 Connection 6 Continuous fiber reinforcement
Claims
1. A pair of precast decks and a connection portion of the pair of decks, The pair of decks and the connection portion include steel short fibers, Each deck has continuous fiber reinforcement, A deck and its connection structure, wherein the continuous fiber reinforcement extends along the arrangement direction of the pair of decks and the connection portion, protrudes from the end face of the deck facing the connection portion, and terminates at the connection portion.
2. The deck and its connection structure described in claim 1, wherein the continuous fiber reinforcement of one deck and the continuous fiber reinforcement of the other deck constitute a connection portion 4, and the length of the connection portion 4 is 5d or more and 10d or less (d is the diameter of the continuous fiber reinforcement).
3. 2. The deck and its connection structure according to claim 1, wherein the continuous fiber reinforcement is made of glass fiber reinforced plastic.
4. 2. The deck and its connection structure according to claim 1, wherein the mixing ratio of the steel short fibers contained in the pair of decks is 0.5% to 2.5%.
5. 2. The deck and its connection structure according to claim 1, wherein the mixing ratio of the steel short fibers contained in the connection portion is 0.5% to 2.5%.
6. 6. The deck and its connection structure according to claim 4, wherein the mixing ratio of the steel short fibers contained in the connection portion is equal to or greater than the mixing ratio of the steel short fibers contained in the pair of decks.
7. The deck and its connection structure according to any one of claims 1 to 3, wherein the compressive strength of the connection portion is greater than 120 MPa.
8. 4. The deck and its connection structure according to claim 1, wherein the continuous fiber reinforcement is the only member extending through the pair of decks in the arrangement direction.
9. A precast deck connected to another precast deck via a joint, It has short steel fibre and continuous fibre reinforcement. A precast deck, in which the continuous fiber reinforcement extends along the arrangement direction of the deck and the other deck and the connection portion, and protrudes from the end face of the deck facing the connection portion.
10. A connection part connecting a pair of precast decks, Steel staple fibers; A connection portion comprising the pair of deck slabs and a portion of continuous fiber reinforcement extending through each deck slab along the arrangement direction of the connection portion, the portion of the continuous fiber reinforcement protruding from an end face facing the connection portion of the deck slabs and terminating at the connection portion.
11. A method for constructing a pair of precast decks and their connection structure, comprising: The pair of floor slabs are arranged with a gap therebetween; Filling the gap with a filler to create a connection between the pair of deck slabs; The pair of decks and the filler include steel short fibers, Each deck has continuous fiber reinforcement, The continuous fiber reinforcement extends linearly in the arrangement direction of the pair of decks and the connection portion, A construction method for a pair of deck slabs and their connection structure, wherein the pair of deck slabs are arranged so that the continuous fiber reinforcement penetrates the deck slabs and terminates in the gap portion.
Citation Information
Patent Citations
Precast concrete floor slab connection structure and connection method
JP2019002250A
Tensioning method for precast PC member
JP2022165352A