Ballistic translation efficiency of high performance fibers
By aligning fibers uniformly through axial stretching in a compression device, the method addresses fiber breakage issues, improving tensile properties and reducing elongation, enhancing the efficiency and performance of composite materials.
Patent Information
- Application Number
- JP2024113800
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-07-12
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2039-07-19
AI Technical Summary
Existing methods for producing high-strength thermoplastic fibers face inefficiencies due to fiber breakage during drawing, leading to low product yields and unpredictable strength loss in composite materials, which increases weight, bulk, and cost.
The method involves limiting fiber elongation and enhancing strength through axial stretching in a compression device, such as an isobaric press, to align fibers uniformly and reduce elongation at break, thereby improving tensile properties without significant stretching.
This approach enhances fiber toughness by at least 1% and reduces elongation at break by at least 1%, resulting in higher tensile properties, lower elongation, greater shear strength, and lower coefficient of friction in composite materials.
Smart Images

Figure 2024150559000001_ABST
Abstract
Description
[Technical field]
[0001] The present technology relates to improvements in ballistic composite materials, and in particular to an efficient method for enhancing the tensile properties of fibrous composite materials. [Background technology]
[0002] High performance thermoplastic fibers, such as polyolefin fibers, are widely used in the manufacture of composite structures. Various methods for producing high strength thermoplastic fibers are known, for example, U.S. Pat. Nos. 4,413,110, 4,536,536, 4,551,296, 4,663,101, 5,032,338, 5,578,374, 5,736,244, 5,741,451, 5,958,582, 5,972,498, 6,441,451, and 6,572,597. Nos. 8,359, 6,746,975, 6,969,553, 7,078,099, 7,344,668, 7,846,363, 8,361,366, 8,444,898, 8,747,715, and 9,365,953, the disclosures of which are incorporated by reference herein to the extent consistent herewith.
[0003] Each of these patents describes a gel spinning technique for the production of high strength filaments, in which the filaments are drawn, i.e., stretched over a series of drawing rolls to improve their tensile strength properties. For example, U.S. Patents 4,413,110, 4,663,101 and 5,736,244 describe the stretching of formed polyethylene gel precursors and low porosity xerogels obtained from the polyethylene gel precursors to form high tenacity, high modulus fibers. U.S. Patents 5,578,374 and 5,741,451 describe the post-stretching of polyethylene fibers that have already been oriented by drawing at a specific temperature and drawing speed. U.S. Patent 6,746,975 describes high tenacity, high modulus multifilament yarns formed from a polyethylene solution via extrusion through a multi-orifice spinneret to form a fluid product. The fluid product is gelled, stretched and formed into a xerogel. The xerogel is then subjected to a two-stage stretch to form the desired multifilament yarn. U.S. Pat. No. 7,078,099 describes drawn gel-spun multifilament yarns with increased molecular structure extension. The yarns are produced by an improved manufacturing process and drawn under special conditions to obtain multifilament yarns with high molecular weight and crystalline order. U.S. Pat. No. 7,344,668 describes a process for drawing essentially diluent-free gel-spun polyethylene multifilament yarns in a forced convection air orb and the drawn yarns produced thereby. The process conditions of draw ratio, elongation, residence time, oven length and feed rate are selected in specific relationships to each other to achieve improved efficiency and productivity. U.S. Patent Nos. 7,846,363, 8,361,366, 8,444,898, 8,747,715, and 9,365,953 each teach improvements in methods known in the art for improving fiber tensile properties and thereby improving the ballistic properties of armor composites formed from the improved fiber tensile properties.
[0004] A common processing step required by all of the above referenced methods is fiber drawing, which is conventionally known to improve fiber strength and is important in the manufacture of highly effective composite armor. However, in the process of drawing filaments using any such drawing method, as the fiber approaches its elongation limit, the filaments may break. Broken filaments tend to wind around one of the drawing rolls, and as they wind around the drawing roll, they often interfere with adjacent unbroken filaments on the same drawing roll, breaking the adjacent filaments apart. The fibers may also break. Ultimately, this may lead to the breakage of the entire yarn. When a yarn breaks, other yarns that are simultaneously drawn by the same drawing device may also break, resulting in process failure and substantial product waste. In view of these issues, maximally drawing the fibers to maximize their toughness may be inefficient and result in relatively low product yields. Therefore, it would be beneficial in the art if there were an alternative means to improve fiber tensile properties without the need for significant fiber drawing after initial production to avoid such fiber breakage and waste.
[0005] Maximizing fiber tensile properties, as well as strength in the presence of a matrix (binder), is important for the production of effective composite armor, especially in the production of effective armor from nonwoven unidirectional fibrous composites where a binder is used to hold the fibers of the unidirectional tape together. However, the strength of a composite does not strictly follow the rules of mixture; that is, the strength of a composite is not simply a direct measure of the strength of the fiber and matrix components. In particular, during the processing of the individual components into a fabric, some loss of strength of the composite occurs relative to the strength of the raw material components, referred to in the art as conversion efficiency. This can occur for a variety of reasons, such as material degradation due to processing conditions or incomplete processing results during the conversion of the fiber to the composite (such as fiber misalignment, void formation, or uneven application of the coating). This presents two significant problems. First, the extent of strength loss is unpredictable, making the strength of the composite unpredictable. Second, to compensate for this inefficiency in strength conversion from fibers to composites, more layers of material are required to maintain a desired level of ballistic performance when converting the composite into an armor article, which undesirably increases the weight, bulk and cost of the armor. A solution is needed to address this problem.
[0006] The present technology has been unexpectedly found to solve both of the manufacturing inefficiencies discussed above, namely, reduced fiber yield due to lost manufactured product, and reduced efficiency of strength conversion from fiber to composite, by limiting fiber elongation and maximizing fiber strength through alternative processing. Summary of the Invention
[0007] In particular, it has been found that the efficiency of conversion of fiber and binder strength to composite strength is improved by first priming (i.e., lightly pressing under mild conditions such as wet lamination) a single-ply unidirectional prepreg web, multiple adjacent / stacked unidirectional prepreg webs, prepreg unidirectional tape (single individual prepreg ply), or multiple adjacent / stacked prepreg plies, and then passing the primed web, individual plies, or multiple plies / webs through an isostatic press (dual belt press). When multiple plies and / or webs are primed, the priming step bonds the plies / webs together to form a prepreg composite web / fabric that typically includes two, four, six, or eight or more plies (layers) (also referred to herein as a "multi-ply fabric" or "multi-ply prepreg fabric") or a prepreg composite web / fabric that includes two, four, six, or eight all unidirectional webs (also referred to herein as a "multi-ply web" or "multi-ply prepreg web"). Each individual web is a single web layer / web ply. A multi-ply prepreg fabric or multi-ply prepreg web can be processed through an isostatic press by itself, or with one or more other multi-ply prepreg fabrics, or unidirectional prepreg webs, or with a single prepreg unidirectional tape (single individual ply) not previously combined with or attached to another web / individual ply.
[0008] In each embodiment, the prepreg web(s) / unidirectional single individual prepreg webs A ply / multi-ply prepreg fabric comprises fibers coated with a polymeric binder or comprises fibrous tapes (with fibers) or non-fibrous tapes (without fibers) optionally coated with a polymeric binder. The coating with binder is performed before subjecting the web(s) / individual plies / fabric to axial stretching in a compression device (e.g., a compression conveyor). By priming the web(s) / individual plies / plies, the unidirectional alignment of the component fibers / tapes is made more uniform such that all component fibers / tapes are aligned straighter and more uniformly in the same axial direction, improving the uniformity of the binder coating on the fibers or tapes (if present). In this regard, the fibers / tapes may move slightly when they are coated with resin. Priming the layers helps in more ideal alignment of such fibers / tapes. This maximizes the fiber / tape coverage of the unidirectional fiber plies and also adjusts areas of excess binder concentration, thereby maximizing the engagement of protrusions with the fibers / tapes, but straightening the fibers / tapes in preparation for axial stretching. After priming, the primed unidirectional web(s) / individual plies / multi-ply fabric are then subjected to axial stretching stress(es) in the axial direction of each web / individual ply. By axially stretching the fibers / tapes in the compaction device rather than completing the fiber stretching by conventional stretching, the yield loss problem associated with maximum fiber stretching is avoided. In addition, axial stretching of the fibers / tapes in the compaction device under the conditions described herein avoids fiber / tape degradation and achieves improved conversion efficiency of the tensile properties of the fibers / tapes to the tensile properties of the final composite compared to conventional manufacturing methods such as consolidation under pressures of 5 psi or more in flatbed laminators, autoclaves, or molding devices.
[0009] More specifically, provided is a fibrous article comprising one or more unidirectional fiber plies, each unidirectional fiber ply comprising a plurality of unidirectionally oriented fibers coated with a polymeric binder, the composite fibrous article being primed, the composite fibers being axially stretched in a compression device, the composite fibers having an initial elongation to break value before being axially stretched and a reduced elongation to break value after being axially stretched, the composite initial elongation to break value being greater than the composite reduced elongation to break value, and the composite reduced elongation to break value being between about 2.0% and about 3.9%.
[0010] Also provided is a method for improving fiber tensile properties of a fibrous prepreg composite, the composite method comprising: a) providing at least one fibrous prepreg composite including one or more unidirectional fiber plies, each of the composite plies including a plurality of unidirectionally oriented fibers coated with a polymeric binder, the composite fibers having a toughness of 7 g / denier or greater and a tensile modulus of 150 g / denier or greater and an elongation to break of at least 2.0%, the composite fibers having a softening temperature and a melting temperature; b) heating the fibers of the composite material to a temperature greater than the softening temperature of the composite material fibers but less than the melting temperature of the composite material fibers; c) subjecting the composite to an axial elongation stress while the composite fibers are at a composite temperature greater than the softening temperature of the composite fibers but less than the melting temperature of the composite fibers, wherein the fibers in each fiber ply are elongated axially by the composite axial elongation stress, thereby increasing the toughness of each fiber in each ply by at least 1% and decreasing the elongation to break of each fiber by at least 1%.
[0011] Composites and ballistic articles formed according to the composite methods are also provided. [Brief description of the drawings]
[0012] [Figure 1]FIG. 1 is a top perspective view of the formation of a unidirectional fiber ply. [Diagram 2] FIG. 1 is a schematic perspective view of a unidirectional fiber array being coated with a binder resin by passing it through a dip coater, followed by bonding the coated array with a release film. [Diagram 3] FIG. 2 is a schematic cross-sectional view of an isostatic belt press and a composite material formed therein. [Figure 4] FIG. 1 is a schematic perspective view of the manufacture of a two-ply 0° / 90° web. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A method is provided for producing high performance composite articles from one or more unidirectional fiber plies, where each "unidirectional fiber ply" may be in the form of a continuous web of unidirectionally oriented (aligned) fibers, or in the form of a single, individual unidirectional ply / unidirectional tape having a length, as described below. Prior to pressing in a compaction device, the unidirectional fiber ply is also referred to herein as a prepreg. A prepreg (a single unidirectional prepreg web, a single individual prepreg unidirectional tape (single individual ply), or a multi-ply prepreg (i.e., comprising multiple unidirectional webs and / or multiple unidirectional tapes) is initially formed from unidirectionally aligned fibers / tapes that are not fully stretched, the fibers / tapes having an elongation to break of at least 2.0%, typically at least 2.1%, or at least 2.2%, or at least 2.3%, or at least 2.4%, or at least 2.5%, or at least 2.6%, or at least 2.7%, or at least 2.8%, or at least 2.9%, or at least 3.0%, up to about 4.0% or 5.0% or more. The fibers / tapes forming the prepreg are then subjected to an axial stress which reduces the elongation to break and increases the toughness of the fibers / tapes, thereby improving the properties of composites formed from said fibers / tapes.
[0014] As used herein, the terms "orient" and "draw" refer to the elongation of the fiber / yarn, and the terms are used interchangeably. When used in the context of "unidirectionally oriented fibers," the term "oriented" refers to the direction of alignment of the fibers, rather than the elongation of the fibers. As used herein, a "fiber" is a long strand of material, such as a strand of polymeric material, whose length dimension is much greater than the transverse dimensions of width and thickness. Fibers are preferred to be long, continuous (but of clearly defined length) strands, rather than short sections of strands referred to in the art as "staple" or "staple fibers." A "strand" by conventional definition is a single, thin, length, such as a thread or fiber. The cross-section of a fiber for use herein may vary widely and may be circular, elliptical, flat, or oval in cross-section. A strand may also be of irregular or regular multi-lobed cross-section, with one or more regular or irregular lobes protruding from the linear (axial) axis of the filament. Thus, the term "fiber" includes filaments, ribbons, strips, etc., having regular or irregular cross-sections. As used herein, the term "composite" refers to a combination of multiple fibers and / or tapes, typically with a polymeric binder material.
[0015] A single fiber may be formed from only one filament or from multiple filaments. Fibers formed from only one filament are referred to herein as either "single filament" fibers or "monofilament" fibers, and fibers formed from multiple filaments are referred to herein as "multifilament" fibers. As defined herein, multifilament fibers preferably include 2 to about 3000 filaments, more preferably 2 to 1000 filaments, even more preferably 30 to 500 filaments, even more preferably 40 to 500 filaments, even more preferably about 40 filaments to about 240 filaments, and most preferably about 120 to about 240 filaments. Multifilament fibers are also often referred to in the art as fiber bundles or bundles of filaments. As used herein, "yarn" refers to a "fiber bundle" or "filament bundle." The term "multifilament fiber" is defined as a single strand of multiple filaments and is used interchangeably with "multifilament fiber." As used herein, the term "tenacity" refers to the tensile stress, expressed as force (grams) per unit of linear density (denier), of an unstressed sample, as measured by ASTM D2256. The "initial modulus" of a fiber is the property of a material that describes its resistance to deformation. The term "tensile modulus" refers to the ratio of the change in tenacity, expressed in grams of gravity per denier (g / d), to the change in strain, expressed as a fraction of the original fiber length (in / in). The term "denier" is the unit of linear density, equal to the mass in grams per 9000 meters of the fiber / yarn. In this regard, the fibers of the present disclosure may be of any suitable denier. For example, the fibers may have a denier of about 50 to about 5000 denier, more preferably about 200 to about 5000 denier, even more preferably about 650 to about 3000 denier, and most preferably about 800 to about 1500 denier. The selection is governed by ballistic effectiveness and cost considerations. Finer fibers are more costly to manufacture and weave, but can produce greater ballistic effectiveness per unit weight. Like the fibers, the tapes may be of any suitable denier, preferably having a denier of about 50 to about 30,000 denier, more preferably about 200 to 10,000 denier, even more preferably about 650 to about 2000 denier, and most preferably about 800 to about 1500 denier.
[0016] Processes for producing ultra-high molecular weight polyethylene (UHMW PE) fibers are known from the prior art, such as commonly owned U.S. Patents 7,846,363, 8,361,366, 8,444,898, 8,747,715, and 9,365,953, each of which is incorporated herein by reference to the extent consistent herewith. For example, in the processes of U.S. Patents 8,747,715 and 9,365,953, gel-spun yarns are made from ultra-high molecular weight polyethylene by adding a slurry of UHMW PE and a spinning solvent to an extruder and forming a liquid mixture from the slurry in the extruder, which is then passed through a heated vessel to form a homogenous solution containing UHMW PE and a spinning solvent. The solution is then fed from a heated vessel to a spinneret to form a solution yarn, and the solution yarn from the spinneret is then drawn at a draw ratio of about 1.1:1 to about 30:1 to form a drawn solution yarn. The drawn solution yarn is then cooled to a temperature below the gel point of the UHMW PE polymer to form a gel yarn, and the gel yarn is then drawn one or more times in one or more stages. The spinning solvent is then removed from the gel yarn (by evaporation or extraction) to form a dry yarn, and the dry yarn is then drawn to form a partially oriented yarn, and then further drawn in a post-draw operation to form a highly oriented yarn. In the context of this disclosure, the fibers useful herein produced from the present process are either partially oriented fibers or highly oriented fibers. The breaking elongation values of the fibers vary depending on the degree of orientation, and generally range from 2.9% to 3.9% for highly oriented fibers and about 4.0% or greater for partially oriented fibers. For purposes of this disclosure, the required maximum or minimum thickness for the fibers (or tapes) forming the prepreg web / single discrete ply (UDT) / multi-ply fabric is There is no minimum elongation to break, however, the fibers forming each prepreg web / single discrete ply (UDT) / multi-ply fabric have a preferred elongation to break of about 2.0% to about 3.9% after axial stretching in the compaction device, and a single pass through the compaction device under the conditions described herein will reduce the elongation to break by at least about 1% to about 5% or more.
[0017] In accordance with the disclosed method for improving composite tensile properties, a nonwoven web of unidirectionally oriented fibers (or tapes) is formed by placing continuous fibers / tapes in a parallel, parallel arrangement, most typically followed by coating the fibers / tapes with a polymeric binder material (also referred to herein as a "resin" or polymeric "matrix") and drying the binder material so that the fibers / tapes are bonded together. This web of continuous, parallel bonded fibers is referred to herein as a "prepreg web." As used herein, "Array" describes an ordered arrangement of fibers or threads, and "parallel array" describes an ordered, side-by-side, planar oriented, parallel arrangement of fibers / tapes or threads. As used herein, the term "prepreg" more specifically refers to a combination of fibers or tapes connected to each other in the form of one or more fibrous plies or one or more fibrous webs, but not yet consolidated / compressed in an isostatic press, e.g., connected by adhesive. If the ply / web comprises fibers, the fibers are coated / impregnated with a polymeric binder (as produced in FIG. 1), and if the ply / web comprises tapes, the polymeric binder is optional. Tapes that are not coated with a polymeric binder are fused together under high heat and optionally pressure before being primed. Thus, "prepreg" is a precursor used as a component of a subsequently formed material / article, and thus for the purposes of this disclosure, and "prepreg web" refers to a continuous unidirectional web of nonwoven parallel fibers / tapes, coated with a binder / resin, as described above. A "prepreg unidirectional tape" is an individual single layer / ply of nonwoven parallel fibers cut from a prepreg web (and therefore having a fixed length) before being subjected to a compaction process in a compaction device (as in the process described in more detail below). Such individual single unidirectional nonwoven plies of parallel fibers / tapes having a fixed length are also referred to in the art as "unitapes", "UDs" or "UDTs", which are synonymous terms with "unidirectional tapes" and "unidirectional tape plies". In this regard, a "unidirectional tape" differs from the above-mentioned "tapes", in that a "tape" (fibrous or non-fibrous) is a fiber-like elongated body that can be grouped with other "tapes" in a parallel arrangement to form an individual ply of a "unidirectional tape" only as a plurality of fibers (or a combination of tapes and fibers) can be grouped in a parallel arrangement to form a "unidirectional tape".As mentioned above, a "multi-ply fabric" or "multi-ply prepreg fabric" is a combination of multiple individual nonwoven unidirectional tapes, each having a length (e.g., cut from a continuous prepreg unidirectional fiber web) and bonded together by priming, such as by bonding them together by wet lamination under low pressure. Typically, but not necessarily, such multi-ply prepreg fabrics have an even number of plies, e.g., two or four or six or eight plies, and each ply is preferably rotated so that the longitudinal / axial fiber direction of each ply is at an angle to the adjacent ply. In this regard, each individual unidirectional tape ply has both an outer upper surface and an outer lower surface. The plies are overlapped with each other such that the lower surface of one contacts the upper surface of the next individual ply, and the plies are rotated so that the longitudinal / axial fiber directions of adjacent plies are not equal. Such rotated unidirectional alignments are conventionally known in the art of ballistic composite armor and are described, for example, in U.S. Patent Nos. 4,457,985, 4,748,064, 4,916,000, 4,403,012, 4,623,574, and 4,737,402, all of which are incorporated herein by reference to the extent incompatible herewith. Most commonly, the unidirectional plies are orthogonally cross-plied so that the fibers of all adjacent layers are oriented at angles between 0° and 90° to one another, although adjacent plies can be aligned at virtually any angle between about 0° and about 90° to the longitudinal / axial fiber direction of another ply. Methods of forming such multi-ply nonwoven prepreg fabrics are well known in the art and may be accomplished manually or automated with conventional stacking or cross-plying equipment, for example, using a cross-plying device as taught in U.S. Patent No. 5,173,138, which is incorporated by reference to the extent consistent herewith, provided that the plies forming the multi-ply fabric are abutted under low pressure according to the priming conditions described herein, since it is the priming step that forms the multi-ply structure.
[0018] When manufacturing prepregs, ideal fiber spreading is when the individual fibers, or even individual filaments, are positioned next to each other in a single fiber plane with a minimal amount, if any, of the fibers overlapping each other to form a substantially unidirectional array of parallel fibers. Typically, a prepreg web or single prepreg unidirectional tape will contain about 3 to 55 fiber ends per inch (about 1.18 to about 21.65 ends per cm), more preferably about 5 to about 45 ends per inch (about 1.97 to about 17.72 ends per cm), even more preferably about 5 to about 20 ends per inch (about 1.97 to about 7.87 ends per cm), and most preferably about 6 to about 16 ends per inch (about 2.36 to about 6.30 ends per cm), with a typical fiber bundle (yarn) having about 30 to about 2000 individual filaments depending on the fiber type, and the preferred polyethylene fiber bundles most typically having about 120 to about 240 individual filaments.
[0019] As mentioned above, the exemplary prepreg manufacturing process described above is illustrated in FIG. 1. As illustrated, multifilament fiber bundles are fed from a clair and directed through a collimating comb / heddle to align the fibers in the proper parallel arrangement coated with a binder material / resin and pressed through a pair of spreader bars / rolls to spread the filaments of the fiber bundle and spread the binder. The binder is then dried or cured to complete the manufacturing of the prepreg, which can then be rolled onto a storage roll for later use or cut into individual layers of a certain length. This method is merely exemplary and may be modified as desired. For example, the binder may actually be applied at any point in the manufacturing process, including any time before or after the multiple fiber bundles are arranged in a parallel arrangement. In such an alternative process, the fibers may instead be coated with the binder after passing through the spreader bar. In another alternative embodiment illustrated in Figure 2, an array of uncoated fibers (formed from fiber bundles aligned via heddles / combs as described above) is coated with a polymer binder such as in a conventional dip and squeeze coater, excess binder is squeezed out, and the fibers are further spread by passing through additional rolls. The coated array is then combined with a release film / paper (e.g., silicone release paper), optionally dried, and sent for further processing, e.g., into a unidirectional tape of a desired length.
[0020] Following formation of the prepreg web(s) and optional cutting of the web(s) into one or more individual unidirectional prepreg plies of desired length, the web(s) and / or one or more single unidirectional tape(s) are then primed. In the most preferred embodiment, multiple continuous fibrous webs or multiple single plies of unidirectional tape are laminated (lightly bonded) together and primed to be bonded to each other. "Priming" refers to lightly pressing the web or unidirectional tape ply / plies with very low pressure between two platens with or without heat (e.g., via a conventional flatbed laminator set at very low pressure) or by passing through the nip of a pair of laminating rolls by techniques well known in the art. Such priming steps include, among other things, wet laminating the plies together, and may optionally be performed in-line on a coater assembly (such as with the combined rollers illustrated in FIG. 2), as well as combinations of wet lamination and dual platens / nip of a flatbed laminator / roll. Such priming also includes pressing a single individual ply or a single unidirectional web, where such a single individual ply or web is not attached to another individual ply or web. Regardless of the priming method, the pressure applied to the prepreg web or individual prepreg unidirectional tape ply(s) during priming is preferably less than 5 psi (0.0345 MPa), preferably from about 0.01 psi (68.9 Pa) to 2.0 psi (0.0138 MPa), more preferably from 0.01 psi (68.9 Pa) to 1.0 psi (0.00689 MPa), and most preferably from 0.1 psi (689 Pa) to 0.5 psi (0.00345 MPa). When priming is performed by heat, the heat is usually very low, i.e., in the range of just above room temperature (20-22° C.) to about 50° C., preferably from about 20° C. to about 50° C., more preferably from about 25° C. to about 50° C., and most preferably from about 25° C. to about 40° C. It may be carried out at elevated temperatures, for example, from about 90° C. to about 100° C. The prepreg web / unitape ply (or a combination of web / unitape plies not yet bonded to one another that will become a multi-ply structure upon priming) is subjected to priming conditions for a short duration of from about 0.01 seconds to about 30 seconds, thereby pressing the fibers into a more ideal alignment.
[0021] Priming may also be performed using the same cross-ply apparatus used in the prior art to consolidate multiple plies, such as the apparatus of U.S. Patent No. 5,173,138. The apparatus of U.S. Patent No. 5,173,138 includes means for laminating stacked plies, which is set at low temperatures and pressures, and may be employed to prime the prepregs provided by the present disclosure. Priming may also be accomplished using any other conventional lamination apparatus, where the web / UDT / web stack and / or UDT plies are treated according to the mild conditions described above.
[0022] Once primed, the web, single UDT ply, or multiple bonded webs and / or multiple bonded UDT plies (multi-ply prepreg web / fabric) are then heated and compressed in a suitable compression device under a pressure great enough to apply an axial extensional stress to each of the fibers forming the web or each UDT ply, whereby each of the fibers / tapes forming the web or each UDT ply are stretched axially, i.e., axially elongated by being subjected to an axial compressive stress in the axial direction. If the prepreg is a multi-ply prepreg fabric or web, the multi-ply prepreg fabric / web will be multiaxially stretched (e.g., a two-ply fabric will be biaxially stretched) since the fibers / tapes of each web / UDT ply will be axially stretched in the axial direction of each respective cross-plied fiber / tape forming the individual component webs / UDT plies. Depending on the pressure, the axial extension stress is sufficient to increase the toughness of the component fibers by about 1% or more, preferably by about 1% to about 5%, such that the elongation to break of each fiber is also reduced by at least about 1%, or by about 1% to about 5%, resulting in greater axial extension.
[0023] The temperature to which the single prepreg UDT ply, multi-ply fabric, and / or web(s) are heated will vary depending on the fiber type and polymer binder type (if present) that forms the prepreg. In this regard, suitable fibers are synthetic thermoplastic fibers having an axial (linear) thermal conductivity, when measured at 23° C. (room temperature), of at least 0.1 W / (m·K) to about 300 W / (m·K), more preferably about 0.1 W / (m·K) to about 125 W / (m·K), even more preferably about 0.1 W / (m·K) to about 105 W / (m·K), even more preferably about 50 W / (m·K) to about 105 W / (m·K), and most preferably about 80 W / (m·K) to about 105 W / (m·K), when measured by conventional known methods such as the guarded hot plate method according to ASTM C-177 (measuring up to 100 W / (m·K)) or the guarded heat flow sensor method according to ASTM C518 (measuring values greater than 100 W / (m·K)). These polymer types have both a softening temperature (Vicat softening temperature as determined by ASTM D1525 / ISO306) and a melting temperature. Suitable synthetic thermoplastic polymers include, non-exclusively, polyolefin fibers such as extended chain polyethylene and extended chain polypropylene fibers, polyester fibers including polyethylene terephthalate fibers, nylon fibers, polyvinyl acetate fibers, and polyacrylonitrile fibers. The melting points of all thermoplastic fiber types other than UHMW PE can be determined by ASTM D7138. UHMW PE has such a high molecular weight that it is a different method to determine its melting point according to ASTM F2625. For example, UHMW PE fibers with a c-axis orientation function of at least 0.96 and an intrinsic viscosity of about 7 dl / g to 40 dl / g when measured in decalin at 135°C by ASTM D1601-99 have a Vicat softening temperature of 80°C and a melting temperature of about 136°C as measured by ASTM F2625. Therefore, the UHMW PE fibers are heated to a temperature of about 80° C. to about 136° C. after priming and in preparation for compression, preferably to a temperature of about 90° C. to about 200° C. The polyethylene fibers are heated to a temperature of 0°C to about 136°C, or from about 115°C to about 136°C. Polyethylene fibers having lower molecular weights will have lower softening and melting temperatures that can be readily determined by one skilled in the art. Fiber types having axial (linear) thermal conductivities of less than 0.1 W / (m·K), such as aramid fibers, graphite (carbon) fibers, glass fibers, quartz fibers, basalt fibers, etc., will not exhibit improved toughness but may still benefit from similar processing. For example, composite types including any primed fiber and binder types will benefit from the improved compaction and reduced air voids within the composite caused by the composite passing through a compaction conveyor.
[0024] Methods for heating a single UDT, multi-ply prepreg fabric(s) / web(s) are conventional in the art and include passing the prepreg web or cut unidirectional plies through one or more ovens, preferably forced air convection ovens as described in U.S. Patent No. 7,344,668, with oven residence times selected within the skill of one in the art and similarly heated with heated platens. Alternatively, the prepreg may be heated by the compaction equipment, if the compaction equipment has heating capabilities, which is most preferred.
[0025] Once heated to an appropriate temperature (provided it is preheated), the primed prepreg web(s) / individual plies / multi-ply fabric (each of which is also referred to herein as the "material" or "priming material" passing through the compaction device) is compacted in a compaction device capable of applying significant uniform pressure to the prepreg material, preferably also conveying the composite through the compaction device. Additionally, if a thicker material is desired depending on the desired end use, multiple of the above lightly bonded primed laminates of unidirectional tapes may be co-extensively combined and compacted together in the same compaction device. It is specifically contemplated that the compaction device is a compaction conveyor, most specifically a double belt press, or a steel belt press. Most preferably, the double belt press is an isobaric double belt press, or an isobaric steel belt press, when the belt comprises steel. The double belt press is a type of compaction conveyor that includes two pressure-applying elements, typically the steel belts just mentioned. The material is compressed between pressure applying elements whereby the pressure simultaneously subjects the composite to an axial tensile stress while the composite is simultaneously conveyed through a compression device.
[0026] Suitable double belt presses are commercially available from, for example, Hymmen International Inc. (Grand Rapids, Michigan), Dieffenbacher GmbH & Co. (Eppingen, Germany), Held Technologie GmbH (Trossingen, Germany), Sandvik Process Systems LLC (Totowa, New Jersey), and Siempelkamp LP (Marietta, Georgia), among others.
[0027] An exemplary isobaric double belt press 2 is shown in Figure 3. Referring to Figure 3, such a suitable double belt press 2 is shown and includes a first belt 10, a second belt 12, a first plurality of rollers 4 supporting the first belt 10, a second plurality of rollers 6 supporting the second belt 12, and a temperature unit 8. As shown, the first plurality of rollers 4 rotate in a clockwise direction and are positioned above the second plurality of rollers 6. Conversely, the second plurality of rollers 6 rotate in a counterclockwise direction and, in combination with the clockwise rotation of the first plurality of rollers 4, advance the primed material 14 through the press 2.
[0028] As the primed material 14 enters the isostatic press 2, the first belt 10 and the second belt 12 are The belt 12 is configured to apply a continuous pressure of about 45 bar (about 600 psi) to about 80 bar (1100 psi) to the primed material 14 as it advances through the isostatic press 2. The continuous high pressure is applied uniformly to the primed material 14, subjecting the fibers to an axial extensional stress. The axial extensional stress axially stretches or elongates each of the fibers in their respective axial fiber directions (i.e., the length direction in which the fibers / tapes are oriented / stretched into each component unidirectional web / UDT ply). This biaxial stretching increases the properties of the material as a whole in both directions. As discussed above, if the pressed primed material is only a single individual UDT ply or unidirectional web, the extensional stress is uniaxial. If the material being primed is a bonded combination of multiple cross-plied UDT plies or cross-plied multi-web prepregs, the extensional stress is biaxial or multiaxial, with the axial stress applied to the axial fiber direction of each web / UDT ply individually. The residence time of the primed material in the press is continued for a time sufficient to increase the tenacity of each fiber by at least about 1%, preferably 1% to about 5%, and the elongation to break of each fiber is reduced by at least 1%, preferably 1% to about 5%, achieved under the press conditions described herein.
[0029] In addition to being pressed by the first belt 10 and the second belt 12, the material 14 passes through a temperature unit 8, which includes a heating section 8a and a cooling section 8b. Thus, the material 14 is subjected to continuous high pressure from the first belt 10 and the second belt 12, while being heated (first) and then cooled (second). By this active cooling of the fibers while the material is under pressure in the press, rather than allowing the fibers to cool naturally to room temperature as they exit the press, the stretched fiber structure is maintained, whereas when the fabric is allowed to cool naturally, the warm fibers exhibit some contraction, reversing some of the fiber stretching, thereby at least partially reversing the improved fiber properties. Importantly, the pressure exerted by the press on the material restrains the fibers, thereby preventing the fiber contraction that would normally occur, which would be accompanied by a restoration of the fiber molecular structure to a more disordered state, reducing the tensile properties of the fiber / fibrous material.
[0030] This combination of intense pressure with both heating and cooling results in a high degree of compaction and reduction of air voids within the pressed material, as well as elimination of other voids within the material, thereby providing a smooth, substantially uniform surface that is more resistant to corrosive and degrading conditions, including resistance to environmental conditions such as gasoline, salt water, humidity, etc. These are believed to reduce the material properties of such fibrous composites compared to pressed materials that are simply cooled naturally to room temperature rather than being actively cooled in a cooling zone.
[0031] In a preferred embodiment, the material passing through the press is maintained under continuous and constant axial tension by a tensioning device, which may be a storage roll (not shown) on which the pressed material is wound, which is actively rotated to apply tension to the material as it passes through the press. In this embodiment, the primed material is typically a single web or a multi-ply web. Rear tension may also be applied by providing a roll of material to the press from a feed roll (i.e., a roll that stores the rolled-up primed material to be fed to the press, not shown) that is actively rolled (thereby unwinding the primed material to pass through the press) at a slower speed than the storage roll, or by limiting the roll speed of said feed roll to a speed lower than the speed at which the material passes through the press, with or without the presence of a storage roll, such as by equipping the feed roll with a brake or another type of tensioner, such as a disk type tensioner, a pin type tensioner, a dancer arm tensioner, etc., as determined by one skilled in the art. Again, the primed material is typically a single web or a multi-ply web. Typically, the overall axial tension in each fiber is about 10% as the material passes through the press. It is desirable for the tension to be in the range of 0 to about 1000 grams, more preferably in the range of about 200 to about 800 grams. It is preferable for the tension to be continuous and constant, particularly when the material passing through the compression conveyor is in the form of a continuous web of material, whether or not the web is compressed to contain a single unidirectional array of continuous fibers, or is a continuous multi-ply web formed from multiple primed fiber plies.
[0032] In another embodiment, where the material passing through the press comprises two or more individual fiber plies, such as one or more two-ply prepreg fabrics, simultaneous axial and transverse axial tension can be exerted on the material by mounting it on an axial or biaxial tension frame such as disclosed in U.S. Pat. No. 3,153,812, which is incorporated by reference to the extent consistent herewith.
[0033] With respect to residence time in the press, in a typical isostatic belt press having a 1.5 meter heating zone immediately followed by a 1.0 meter cooling zone directly adjacent thereto, the material moves through the press at a speed of about 2 meters / minute to about 10 meters / minute, most preferably at a speed of about 4 meters / minute to about 8 meters / minute. In an exemplary process in which the material passes through the press at about 6 meters / minute, the residence time in the heating zone is about 15 seconds and the residence time in the cooling zone is about 10 seconds. When the material passes through the press at these speeds, and at an applied pressure of about 45 bar (about 600 psi) to about 80 bar (1100 psi), and other processing conditions described herein include subsequent cooling to room temperature under a continuous, maintained constant pressure as described herein, the tenacity of each fiber will increase by at least about 1% and the elongation to break of each fiber will decrease by at least 1%. Additionally, the primed and compressed material exhibits higher shear strength properties and a lower coefficient of friction as compared to a comparative material that was not processed through the isopressure double belt press.
[0034] In a most preferred embodiment, the primed material is subjected to an axial elongational stress having a magnitude of at least about 1 pound per lineal inch (PLI) to about 30-PLI at a temperature of about 90° C. to about 125° C. It is expected that passing through at a sufficient speed will result in an increase in tensile properties of at least 5% for fibrous webs containing at least ultra high molecular weight polyethylene fibers.
[0035] When the primed material being conveyed through the press is in the form of a continuous single-ply or multi-ply web, the web is preferably provided in roll form from a first storage roll as shown in Figures 1 and 4, and the web is preferably wound onto a second storage roll as well after exiting the press. During conveyance through the press from such first storage roll to such second storage roll, the storage roll may be actively rotated to apply tension to the web as it is conveyed through the press. Mechanisms and methods for rotating such storage rolls are known in the art and would be readily deployed by one of ordinary skill in the art. When such tension is applied to the web, the tension is preferably in the range of about 2 Newtons / cm to about 50 Newtons / cm, or about 5 Newtons / cm to about 50 Newtons / cm, with a tension of 2 N / cm to about 25 N / cm being more preferred, and a tension of 2 N / cm to about 13 N / cm being most preferred.
[0036] When one or more multi-ply fabrics (e.g., multiple 2-ply fabrics) or one or more multi-ply webs (e.g., multiple 2-ply webs) pass through a press, the significant pressure of the press completely consolidates the fabrics / webs into a unitary composite, a monolithic layer or a single, monolithic web in which the component layers / webs are no longer separable from one another (at least without destroying the material being removed). They are converted into a single, consolidated, monolithic, multi-ply structure. The total number of unidirectional tapes or webs incorporated is then multiplied by 100 to produce a composite. The number of plies also depends on the end use of the composite armor and will be readily determined by one of ordinary skill in the art. For example, in armor applications, a composite armor article may include from 2 to about 100 2-ply UDTs, more preferably from about 2 to about 85 2-ply UDTs, and most preferably from about 2 to about 65 2-ply UDTs. In the context of the present disclosure, these multi-ply materials are preferably formed by cutting multiple individual lengths from a multi-ply web compressed in a compression device of the present disclosure, followed by another consolidation step, such as sewing or traditional fibrous composite molding techniques. The greater the total number of plies, the greater the ballistic resistance, but the greater the weight. The minimum level of ballistic resistance for body armor for military use is classified by the National Institute of Justice (NIJ) Threat Levels, as is well known in the art. For example, The two-ply fabric (also referred to herein as the "fibrous layer") has a fiber density of about 60 g / m 2 ~Approx. 130g / m 2 and has an areal density of 1.0 lb / ft 2 (psf)(4.88kg / m 2 To produce an armor article having an areal density of about 100 kSm (ksm), a total of about 38 to about 81 two-ply fabrics must be combined in the press.
[0037] The areal density of a single web ply or a single UDT ply, or multiple UDT / multi-web materials passing through an isostatic press is not intended to be strictly limited, however, each single unidirectional web ply or single unidirectional tape ply will generally have an areal density of about 10 g / m 2 ~about 95g / m 2 , or about 15 g / m 2 ~about 95g / m 2 Or about 30g / m 2 ~about 95g / m 2The multi-unit or multi-web laminate passed through the press preferably contains 2 to 8 total plies (webs and / or unitapes), each ply containing fibers coated with a polymeric binder / matrix that is preferably a very flexible, low modulus polymer, such as an elastomeric and / or thermoplastic polymeric binder having an initial tensile modulus of less than 6,000 psi, more preferably 4,000 psi or less, and most preferably 2,000 psi or less.
[0038] As mentioned above, the preferred fiber types herein are synthetic thermoplastic fibers that are thermally conductive and have a thermal conductivity of at least 0.1 W / (m·K). Such fibers typically exhibit both a softening temperature (Vicat softening temperature as determined by ASTM D1525 / ISO306) and a melting temperature. These include polyolefin fibers such as extended chain polyethylene and extended chain polypropylene fibers, polyester fibers including polyethylene terephthalate fibers, nylon fibers, fiber types such as polyvinyl acetate fibers, and polyacrylonitrile fibers. Also, melt spun polyethylene fibers such as those taught in U.S. Pat. No. 7,935,283, which is incorporated herein by reference to the extent consistent herewith. Also useful are polyethylene tapes, for example, as described in commonly owned U.S. Pat. No. 8,263,119. Nos. 8,697,220, 8,685,519, 8,852,714, 8,906,485, 9,138,961, and 9,291,440 are also useful, each of which is incorporated herein by reference to the extent consistent with the present specification. In this regard, the term "tape" refers to a flat, narrow, monolithic strip of material having a length greater than its width and an average cross-sectional aspect ratio, i.e., the ratio of the maximum dimension to the minimum dimension of the average cross-section over the length of the tape article, of at least about 3:1. Tapes may be fibrous or non-fibrous materials, with fibrous materials including one or more filaments, such as those described in the patents referenced above. Non-fibrous tape materials may be formed, for example, from strips of polymer formed by slicing a polymer film. Tapes are distinguished from fibers having a flat or rectangular cross section in that the fibers have an aspect ratio of less than 3:1, and typically have an aspect ratio of 1:1 to 2:1.
[0039] Aramid fibers, M5® fibers, graphite ( Fiber types such as carbon fiber, glass fiber, quartz fiber, basalt fiber, etc. may similarly benefit from similar processing, but will not see the same toughness enhancement as other fiber / tape types, i.e., they will experience little or no elongation when passed through the press, and thus will not achieve at least a 5% increase in toughness and at least a 5% decrease in elongation at break, but may benefit from improved compaction as discussed above.
[0040] In the case of polyethylene, the preferred fibers are extended chain polyethylene having a weight average molecular weight of at least 300,000, preferably at least 5,000,000, more preferably at least 1 million, and even more preferably 2 to 5 million. Those having a weight average molecular weight of at least 1,000,000 are generally referred to as ultra-high molecular weight polyethylene. Such extended chain polyethylene (ECPE) fibers are The fibers may be grown by a solution spinning process such as described in U.S. Pat. Nos. 4,137,394 or 4,356,138, which are incorporated herein by reference, or may be grown by a solution spinning process such as described in U.S. Pat. Nos. 4,413,110, 4,536,536, 4,551,296, 4,663,101, 5,006,390, 5,032,338, 5,578,374, 5,736,244, 5,741,451, 5,958, They may also be spun from solution to form gel structures, such as those described in Honeywell et al., 582, 5,972,498, 6,448,359, 6,746,975, 6,969,553, 7,078,099, 7,344,668, 7,846,363, 8,361,366, 8,444,898, 8,747,715, and 9,365,953, all of which are incorporated herein by reference. A particularly preferred fiber type is the Honeywell 1000 series. The polyethylene fibers may be any of those sold under the trademark SPECTRA® by International Inc. SPECTRA® fibers are well known in the art. Other useful polyethylene fiber types also include DYNEEMA® UHMW PE yarns available from Royal DSM NV Corporation, Heerlen, The Netherlands. The UHMW PE manufacturing methods of U.S. Patents 8,747,715 and 9,365,953, described in more detail above, are merely exemplary.
[0041] Particularly preferred methods for forming UHMW PE fibers are processes capable of producing UHMW PE fibers having a tenacity of at least 35 g / denier, most preferably the fibers being multifilament fibers. Most preferred processes include those described in commonly owned U.S. Patent Nos. 7,846,363, 8,361,366, 8,444,898, 8,747,715, and 9,365,953, the disclosures of which are incorporated herein by reference to the extent consistent herewith. These processes are capable of producing UHMW PE fibers of very high tenacity. Such processes are referred to as "gel spinning" processes, also referred to as "solution spinning", in which a solution of ultra-high molecular weight polyethylene and a solvent are formed, followed by extrusion of the solution through a multi-orifice spinneret to form solution filaments, cooling the solution filaments into gel filaments, and extracting the solvent to form dry filaments. These dry filaments are then gathered into bundles, referred to in the art as either fibers or yarns. The fiber / yarn can then be stretched (drawn) to its maximum elongation limit to increase toughness. As the fiber is drawn, the breaking elongation decreases. This means that when it is drawn, the degree to which it can be stretched further is essentially reduced.
[0042] Other suitable fiber types as well as methods for forming suitable polyethylene tapes are well known in the art. The stretching of all fibers / tapes useful herein should be limited to a point where their elongation to break is still at least 2.0%, but stretching should be limited to a minimum tenacity of at least 7 g / denier, with a preferred tenacity of at least about 150 g / denier. The strength of the fibers should be limited to a point sufficient to achieve a fiber having a tensile modulus, preferably an energy to break of at least about 8 J / g, each as measured by ASTM D2256. However, the composites of the present disclosure are intended for high performance applications such as ballistic materials or impact resistant textiles, and therefore it is desirable for the fibers forming each unidirectional fibrous ply (web and UDT) to be substantially greater than 7 g / denier. In this regard, it is preferred that each of the fibers forming the fibrous ply has a tenacity of greater than 25 g / denier, more preferably about 28 g / denier to about 50 g / denier, even more preferably about 33 g / denier to about 50 g / denier, even more preferably 39 g / denier or more, even more preferably at least 39 g / denier to about 50 g / denier, even more preferably 40 g / denier or more, even more preferably 43 g / denier or more, or at least 43.5 g / denier, even more preferably about 45 g / denier to about 50 g / denier, even more preferably at least 45 g / denier, before being subjected to an axial tensile stress (e.g., a double belt press). After being subjected to an axial tensile stress (e.g., a double belt press), the fibers will have a tenacity that is at least 1%, preferably at least 2%, more preferably at least 5%, even more preferably 10% or more, and most preferably at least 15% higher than the tenacity of the original fibers before being subjected to the axial tensile stress. These axially stretched fibers of the final compressed composite will have a tenacity of greater than about 27 g / denier, more preferably from about 28 g / denier to about 60 g / denier, even more preferably from about 33 g / denier to about 60 g / denier, even more preferably 39 g / denier or greater, even more preferably at least 39 g / denier to about 60 g / denier, even more preferably 40 g / denier or greater, even more preferably 43 g / denier or greater, or at least 43.5 g / denier, even more preferably from about 45 g / denier to about 60 g / denier, even more preferably at least 45 g / denier, at least about 48 g / denier, at least about 50 g / denier, at least about 55 g / denier, or at least about 60 g / denier, with similar tenacity ranges for the fibrous tapes.Fibers having these tenacity ranges can be achieved by conventional drawing without subjecting the fiber to axial stretching in a compaction device, however, greater results are achieved when the peak tenacity of the fiber / tape is achieved by a combination of drawing and compressive stretching (i.e., axial stretching in a compaction device) rather than by drawing alone for the reasons discussed above.
[0043] The fibers of the present disclosure have a higher denier before the compression axial stretching compared to after the compression axial stretching. In this regard, the pre-compression stretched fibers preferably have a denier of 2.0 to 10.0, more preferably about 2.0 dpf to about 9.0 dpf, even more preferably about 2.0 dpf to about 8.0 dpf, and most preferably about 2.0 dpf to about 7.0 dpf. The post-compression stretched fibers have a denier per filament reduced by at least 1.0, thereby having a dpf (depending on the starting dpf) of about 1.0 to about 9.0 dpf, more preferably about 1.0 dpf to about 8.0 dpf, even more preferably about 1.0 dpf to about 7.0 dpf, even more preferably about 1.0 dpf to about 6.0 dpf, even more preferably about 1.0 dpf to about 5.0 dpf, and most preferably about 1.0 dpf to about 4.0 dpf.
[0044] The polymeric binder material, as mentioned above, is referred to in the art as a polymeric "matrix" material or "resin" and is a material that bonds to the fibers (and tapes, if present) either by its inherent adhesive properties or after being subjected to well-known heat and / or pressure conditions. As used herein, "polymeric" binder or matrix materials are preferably, but not necessarily thermoplastic, and include resins and rubbers. If present, the polymeric binder / matrix material partially or substantially coats the individual fibers / tapes, and preferably substantially coats each of the individual filaments / fibers / tapes to form the prepreg.
[0045] Suitable polymeric binder materials include both low tensile modulus, i.e., elastomeric materials, and high tensile modulus, rigid materials. As used throughout this specification, the term tensile modulus refers to the coefficient of elasticity of the polymeric binder material as measured by ASTM D638. Low or high modulus binders may include a variety of polymeric and non-polymeric materials. For purposes of this disclosure, a low modulus elastomeric material has a tensile modulus measured at about 6,000 psi (41.4 MPa) or less according to the ASTM D638 test procedure. A low modulus polymer is preferably an elastomer having a tensile modulus of about 4,000 psi (27.6 MPa) or less, more preferably about 2400 psi (16.5 MPa) or less, even more preferably 1200 psi (8.23 MPa) or less, and most preferably about 500 psi (3.45 MPa) or less. The glass transition temperature (T g ) is preferably less than about 0° C., more preferably less than about −40° C., and most preferably less than about −50° C. The low modulus elastomeric materials also have a preferred elongation at break of at least about 50%, more preferably at least about 100%, and most preferably at least about 300%. Whether low or high modulus materials, the polymeric binder may also contain fillers such as carbon black or silica, may be oil extended, or may be vulcanized with sulfur, peroxide, metal oxide, or radiation curing systems as are well known in the art.
[0046] A wide variety of materials and formulations may be utilized as low modulus polymeric binders. Representative examples include polybutadiene, polyisoprene, natural rubber, ethylene-propylene copolymers, ethylene-propylene-diene terpolymers, polysulfide polymers, polyurethane elastomers, chlorosulfonated polyethylene, polychloroprene, plasticized polyvinyl chloride, butadiene acrylonitrile elastomers, poly(isobutylene-co-isoprene), polyacrylates, polyesters, polyethers, fluoroelastomers, silicone elastomers, copolymers of ethylene, polyamides (useful for use with some fiber types), acrylonitrile butadiene styrene, polycarbonates, and combinations thereof, as well as other low modulus polymers and copolymers that can be cured below the melting point of the fibers. Also useful are blends of different elastomeric materials, or blends of one or more thermoplastics with elastomeric materials.
[0047] Particularly useful are block copolymers of conjugated dienes and vinyl aromatic monomers. Butadiene and isoprene are the preferred conjugated diene elastomers. Styrene, vinyl toluene, and t-butyl styrene are the preferred conjugated aromatic monomers. Block copolymers incorporating polyisoprene may be hydrogenated to produce thermoplastic elastomers with segments of saturated hydrocarbon elastomers. Polymers include simple triblock copolymers of type ABA, type (AB) n (n=2~10) multi-block copolymer, or type R-(BA) x(x=3-150) radially structured copolymers, where A is a block from polyvinyl aromatic monomers and B is a block from conjugated diene elastomers. Many of these polymers are commercially manufactured by Kraton Polymers, Houston, Texas, and are described in the report "Kraton Thermoplastic Rubber", SC-68-81. Also useful are resin dispersions of styrene-isoprene-styrene (SIS) block copolymers, available under the trademark PRINLIN® from Henkel Technologies, based in Dusseldorf, Germany. Traditional low modulus polymeric binder polymers employed in ballistic composites include polystyrene-polyisoprene-polystyrene block copolymers, commercially manufactured by Kraton Polymers and sold under the trademark KRATON®.
[0048] A low modulus polymeric binder material is preferred for forming a flexible impact resistant material, whereas a high modulus High modulus polymeric binder materials are preferred for forming rigid impact resistant articles. High modulus rigid materials generally have an initial tensile modulus greater than 6,000 psi. Useful high modulus rigid polymeric binder materials include polyurethanes (both ether and ester based), epoxies, polyacrylates, phenolic / polyvinyl butyral (P Examples of suitable rigid polymeric binder materials include mixtures of polymers such as vinyl ester and diallyl phthalate, or phenol formaldehyde and polyvinyl butyral, as well as mixtures of such polymers. Particularly useful rigid polymeric binder materials are thermosetting polymers that are soluble in carbon-carbon saturated solvents such as methyl ethyl ketone and have a molecular weight of at least about 1×10 as measured by ASTM D638. 6It has a high tensile modulus upon cure at 100 psi (6895 MPa).Particularly useful rigid polymeric binder materials are those described in U.S. Patent No. 6,642,159, which is incorporated herein by reference.
[0049] Most specifically preferred herein are polar resins or polar polymers, especially polyurethanes in the range of both soft and hard materials, with tensile modulus in the range of about 2,000 psi (13.79 Mpa) to about 8,000 psi (55.16 Mpa). Preferred polyurethanes are applied as aqueous polyurethane dispersions, most preferably, but not necessarily, co-solvent-free. These include aqueous anionic polyurethane dispersions, aqueous cationic polyurethane dispersions, and aqueous non-ionic polyurethane dispersions. Particularly preferred are aqueous anionic polyurethane dispersions, aliphatic polyurethane water dispersions, and most preferred are aqueous anionic, aliphatic polyurethane water dispersions, all of which are preferably co-solvent-free dispersions. These include aqueous anionic polyester-based polyurethane dispersions, aqueous aliphatic polyester-based polyurethane dispersions, and aqueous anionic, aliphatic polyester-based polyurethane dispersions, all of which are preferably co-solvent-free dispersions. These also include aqueous anionic polyether polyurethane dispersions, aqueous aliphatic polyether-based polyurethane dispersions, and aqueous anionic, aliphatic polyether-based polyurethane dispersions, all of which are preferably co-solvent-free dispersions. Also preferred are all corresponding variants of aqueous cationic and aqueous non-ionic dispersions (polyester-based, aliphatic polyester-based, polyether-based, aliphatic polyether-based, etc.). Most preferred are aliphatic polyurethane dispersions having a modulus at 100% elongation of about 700 psi or more, with a particularly preferred range of 700 psi to about 3000 psi. More preferred are aliphatic polyurethane dispersions having a modulus at 100% elongation of about 1000 psi or more, even more preferably about 1100 psi or more. Most preferred are aliphatic polyether-based anionic polyurethane dispersions having a modulus at 100% elongation of 1000 psi or more, more preferably 1100 psi or more.
[0050] The total weight of the binder forming the prepreg / composite of the present disclosure is preferably about 2% to about 50% by weight, more preferably about 5% to about 30% by weight, more preferably about 7% to about 20% by weight, and most preferably about 13% to about 16% by weight of the fibers plus the weight of the binder. The most preferred amount of binder varies depending on the end use requirements. The amount of binder also depends on whether the component plies are formed from fibers or tapes. A smaller amount of binder is generally used when the plies are formed from tapes because the binder stays on the surface. Typically, when bonding two plies formed from tapes, the binder content is less than 10% by weight of the combined plies, most typically about 4% to about 8% by weight of the combined plies, and optionally, adjacent tapes are fused together and no binder is present between the tapes.
[0051] Methods for applying polymeric binder materials to fibers to form binder-impregnated prepregs are well known and readily determined by those skilled in the art. The term "impregnated" is used herein to mean that the polymeric coating is "embedded," "coated," or "bonded" to the fibers. is considered synonymous with differently applied (the binder material is dispersed in the web / UDT ply and not merely present on the web / UDT ply surface). Any suitable application method may be used to apply the polymeric binder material, and the specific use of terms such as "coated" is not intended to limit the manner in which the filaments / fibers / tapes are applied. Useful methods include, for example, spraying, extruding, or roll coating the polymer or polymer solution onto the fibers / tapes, as well as conveying the fibers / tapes through a molten polymer or polymer solution. The most preferred method is one in which the polymeric binder material substantially coats or encapsulates each individual fiber / tape, covering the entire or substantially the entire surface area of the fibers / tapes.
[0052] After a composite article is produced by passing through a compression device (e.g., a compression conveyor / press), or alternatively, before one or more webs and / or one or more unidirectional tape plies pass through the compression device, one or more thermoplastic polymer films may be attached to the top surface of the webs / plies of the material (pre-press) or the compressed composite (post-press). When attached to the webs / plies before compression, the film is simply placed on the outer surface of the outermost web / ply, and the film is fused to the web / ply as the combination passes through the press, as described in the examples below. When attached after the web(s) / UDT ply(s) / UDT plies are compressed in the press, the film can be laminated onto the compressed composite according to conventional heat lamination conditions in the art. Typically, lamination is performed by positioning the individual layers on top of each other under sufficient heat and pressure to bond the layers into an integral structure. Lamination may be performed at a pressure of about 5 psig (0.034 MPa) to about 100 psig (0.69 MPa) at a temperature ranging from about 95° C. to about 175° C., preferably from about 105° C. to about 175° C., for a period of about 5 seconds to about 36 hours, preferably from about 30 seconds to about 24 hours. Alternatively, such thermoplastic films may be bonded to the composite surface with hot glue or hot melt fibers, as will be appreciated by those skilled in the art.
[0053] Suitable polymers for the thermoplastic polymer layer include, but are not limited to, polyolefins, polyamides, polyesters (especially polyethylene terephthalate (PET) and PET copolymers), polyurethanes, vinyl polymers, ethylene vinyl alcohol copolymers, ethylene octane copolymers, acrylonitrile copolymers, acrylic polymers, vinyl polymers, polycarbonates, polystyrenes, fluoropolymers, and the like, as well as copolymers including ethylene vinyl acetate (EVA) and ethylene acrylic acid, and mixtures thereof. Also useful are polymers of natural and synthetic rubber. Of these, polyolefin and polyamide layers are preferred. A preferred polyolefin is polyethylene. Non-limiting examples of useful polyethylenes include low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), linear low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), linear low density polyethylene (LDPE), linear low density polyethylene (LDPE), medium ... Polyethylene (medium density polyethylene, MDPE), linear medium density polyethylene (LMDPE), linear very-low density polyethylene (VLDPE), linear ultra-low density polyethylene (ULDPE), high density polyethylene (HDPE), and copolymers and mixtures thereof. Also useful are Examples include SPUNFAB® polyamide webs (registered trademark of Keuchel Associates, Inc.) available from Spunfab, Ltd, Cuyahoga Falls, Ohio, and THERMOPLAST® and HELIOPLAST® webs, netting, and films available from Protechnic SA, Cernay, France.
[0054] The optional thermoplastic polymer layer is preferably very thin, about 1 μm to about 250 μm, more preferably Preferably, the layer has a preferred thickness of about 5 μm to about 25 μm, and most preferably about 5 μm to about 9 μm. Discontinuous webs, such as SPUNFAB® nonwoven webs, preferably have a thickness of 6 g / m 2 It is understood that while such thickness is preferred, other thicknesses may be manufactured to meet particular needs, but are within the scope of this disclosure.
[0055] Finally, a particular advantage is achieved in that the fibers / tapes forming the prepreg web / UDT ply / multi-ply fabric are those having an initial breaking elongation of 3.0% or more, or more preferably, 4.0% or more before being subjected to said axial extension stress, and 2.0% to 3.9% after said axial extension stress. For example, UHMW PE fibers useful herein can be produced according to the method of US Pat. No. 9,365,953, but the post-drawing of the fiber(s) is limited to maintain a breaking elongation of more than 4.0%, and drawing of these fibers is carried out in a post-drawing operation (i.e., a drawing operation after the spinning solvent has been removed / evaporated and the fibers have been dried, as defined in US Pat. No. 9,365,953) while the breaking elongation of the fibers is greater than 4.0%. After the end of the post-drawing, the fibers are further axially stretched in a compression device (e.g., a double belt press) as described herein, whereby the breaking elongation is further reduced by at least 1%. The final breaking elongation depends on the starting breaking elongation before passing through the compression device. The preferred fibers have a final breaking elongation of 2.0% to 3.9%, preferably 2.9% to 3.9%, by being axially stretched in the compression device, and the breaking elongation of each fiber is reduced by at least 1% by passing through the compression device under the above conditions. If the post-stretching of the fibers forming the prepreg web / UDT ply / multi-ply fabric is terminated early and their breaking elongation remains above 4.0% when entering the compression device, a good minimization of the yield loss problem associated with maximum fiber stretching should be achieved (e.g., according to the method described in U.S. Pat. No. 9,365,953, or other methods of forming high tenacity UHMW PE fibers). However, fibers / tapes having any breaking elongation may be compressed and axially stretched according to the process of the present disclosure, and the breaking elongation of each fiber is reduced by at least 1%, regardless of its breaking elongation / elongation upon entry into the compression device.
[0056] Although the present technology has been shown and described with particular reference to preferred embodiments, it will be readily understood by those skilled in the art that various changes and modifications may be made without departing from the spirit and scope of the present disclosure. The claims are intended to be interpreted to cover the disclosed embodiments, their alternatives as described above, and all equivalents thereof. For example, instead of attaching two unidirectional squares / rectangles to each other by priming (e.g., each cut from a unidirectional fiber web and then coextensively laminated between surfaces followed by priming, etc.) before passing through a press, an alternative method may be used in which a two-ply web is first formed, such as a two-ply 0° / 90° web, by priming two unidirectional webs together as shown in FIG. 4. In this embodiment, a first unidirectional prepreg web of 0° axially oriented fibers (e.g., as described in more detail above, such as in the method illustrated in FIG. 1) is formed (step 1), followed by converting the web of axially oriented fibers to a web of fibers oriented at 90° (or any other angle, e.g., ±45°) by cutting the 0° web into sections, rotating the cut sections so that the fibers are oriented at the desired angles, and then taping the cut sections together to form a new web as shown in FIG. 4 (step 2). This new web, e.g., a 90° web as shown in FIG. 4, can then be adjacent to another 0° unidirectional prepreg web (step 3), such as by wet lamination, optionally with intermediate and / or surface polymer films, as well as existing resin / binder coatings on the fibers, or an optional polymer film that acts as an adhesive to help adhere the webs to each other. Thereafter, a two-ply web or multiple two-ply webs (e.g., multiple two-ply, 0° webs) can be formed. 4). The laminate (having wide webs and coextensive adjacent surfaces) is passed through a compression device as described above (step not shown in FIG. 4).
[0057] The following non-limiting examples serve to illustrate preferred embodiments of the present disclosure.
[0058] Comparative Examples 1 to 13 A continuous four-ply composite web was made from SPECTRA® ultra-high molecular weight polyethylene filament bundles / fibers (1332 denier unidirectional filament bundles; 5.5 denier per filament (dpf); tenacity of approximately 36.6 grams per denier (g / d), Honeywell International Inc.). In each web ply, the fibers were coated with PRINLIN® B7137HV binder (commercially available from Henkel Technologies, Düsseldorf, Germany), which is a water-based dispersion of styrene-isoprene-styrene resin block copolymer (KRATON® D1107), with the combined structure containing 15 weight percent PRINLIN® B7137HV binder (based on the total weight of the two-ply web).
[0059] To form a multi-ply composite web, a first 64 inch (162.5 cm) wide continuous nonwoven unidirectional (axial) web of unidirectional filament bundles was formed from a parallel array of fiber / filament bundles including 380 of the 1332 denier fiber / filament bundles. The array was formed from a process as shown in FIG. 1, in which each bundle was unwound from a spool mounted on a clair, followed by placing the bundles in a parallel array by passing the bundles through a collimating comb / heddle. The balanced array of bundles was then passed through an aqueous adhesive bath as shown in FIG. 2 of PRINLIN® B7137HV dispersion to coat the filament bundles (typically each of the individual filaments forming the bundle) with an adhesive. The coated array of filament bundles was then passed through a spreader bar as shown in FIG. 2 to achieve some partial filament spreading. The coated partially spread filaments were then passed through a nip to remove excess binder composition coating, after which the coated fiber array was coated onto one side of a silicone release paper (shown as an option in FIG. 2) and dried (e.g., by heating the web to about 100° C. to evaporate the water from the aqueous binder composition). The dried web was then cut into a plurality of 64 inch by 64 inch squares. The squares were then rotated such that the component filaments were oriented 90° relative to their original axial orientation when the web was produced (as shown in FIG. 4). A plurality of these squares were placed flush alongside one another and taped together with no spacing between the placed plies, thereby forming a continuous crosswise web (a continuous web of 90° oriented filaments).
[0060] A second 64 inch wide continuous nonwoven unidirectional (axial) web was then produced in the same manner as the first web, with the same 1332 denier, 36.6 g / d UHMW PE filament bundles / fibers formed into another arrangement and then coated with the same aqueous PRINLIN® B7137HV dispersion according to the coating method as shown in FIG. 2. This web was not cut, but remained as an axial web. Its component filaments are oriented in the same longitudinal direction, i.e., 0° direction, as when the filament bundles were first provided by the clair and passed through the collimating comb. At this point, rather than combining the coated axial arrangement with a silicone release paper as shown in FIG. 2, it was combined with the already produced transverse web, and the two webs were combined while the binder composition coating on the 0° axial web was still wet. During this process (priming by wet lamination), pressure of about 1 psi was applied to the web as it passed through the combining rollers, and heat was applied to the combined web (to a temperature of about 100° C.) to coat the aqueous binder composition. of water was allowed to evaporate, thereby forming a dry two-ply web with the filament directions of the plies orthogonally oriented at 0° / 90°.
[0061] A second two-ply web was then formed, manufactured exactly as described immediately above. The two two-ply webs were then coextensively adjacent (placed one above the other with full coverage of each other) while maintaining the 0° / 90° / 0° / 90° orientation of the filament webs. The two two-ply webs were then lightly adjacent, one on each outer surface of the combined web, to a continuous film / sheet of continuous low density polyethylene (LLDPE) (each film having a thickness of about 0.35 mil (8.9 μm)).
[0062] The stack of two consecutive 2-ply webs, along with the two outer LLDPE films on the webs, was then transferred to a flat laminator and consolidated under heat and pressure by wet lamination to create a 4-ply composite web. The lamination temperature was 110°C with a continuous pressure of about 200 pounds per square inch applied to the adjacent webs. The resulting structure was a one-piece, monolithic, 4 fibrous ply composite web comprising (film / 0° web / 90° web / 0° web / 90° web / film). Multiple square / rectangular test specimens were then cut from this 4-ply composite web and tested for their tensile, shear, and friction properties.
[0063] Comparative Examples 1 to 5 Tensile Property Testing Tensile properties were obtained following ASTM D3019 and ASTM D5034 / 5035 guidelines on a standard Instron 1332 load frame machine using MTS647.10A hydraulic grips. Test specimens were attached directly to the grips and tension was applied by pulling the specimen away from the grips until failure. All tests were performed at room temperature (72°F) with a tensile loading rate of 0.1 in / min. Displacement and strain data were obtained using DIC (digital image correlation) equipment to capture digital images, which were analyzed using VIC3D software from Correlated System Inc. Tension specimens were tested until failure.
[0064] [Table 1] Table 1
[0065] Comparative Examples 6 to 9 Shear Property Test The ASTM D8067 test method was used to obtain the shear properties. Rather than mounting the test specimens directly in hydraulic grips as in Comparative Examples 1-5, the test specimens were mounted on a rectangular picture frame type fixture held in a standard Instron 1332 load frame machine. The rectangular frame was then gripped using the same MTS647.10A hydraulic grips as in Comparative Examples 1-5. The shear properties of the materials are tested under quasi-static, extremely small loads (shear strains) with the load applied at two diagonal corners according to the ASTM D8067 method. The shear strain rate for the test was 0.1 in / min, and the specimens were then subjected to a tensile test at their respective shear strain rates. The load was applied until buckling. Displacement and strain data were acquired using a DIC instrument and analyzed using VIC3D software from Correlated Systems Inc., as described above for Comparative Examples 1-5.
[0066] [Table 2] Table 2
[0067] Comparative Examples 10 to 13 Friction Coefficient Test The samples were also tested to determine their coefficient of friction, with friction properties measured according to the ASTM G115 method. Friction testing was performed on a GCTS biaxial test frame (International Test Equipment, Tempe, AZ) with a shear actuator moving the sample and a normal actuator applying a normal force to the sample at a constant displacement. Friction data was obtained from the system using two load cells: a vertical normal actuator and a shear actuator.
[0068] [Table 3] Table 3
[0069] Examples 14 to 26 A novel continuous 4-ply fibrous composite web (film / 0° web / 90° web / 0° web / 90° web / film) was produced from the same materials (same fibers, binders and film type) using two 2-ply 0° / 90° continuous webs in exactly the same manner as described above in Comparative Examples 1-13. However, instead of consolidating the two 2-ply continuous webs and the LLDPE film together at high pressure in a flatbed laminator, the two 2-ply webs and film were consolidated in an equal pressure steel belt press (double steel belt press) as shown in Figure 3. In this regard, the two 2-ply fibrous webs and the two outer LLDPE films were abutted and then fed together one at a time into the equal pressure steel belt press and the combination was run through the press at a speed of 4 meters per minute. The press had a heating zone set to 110°C and was set to apply a pressure of 80 bar (1160 psi) to the laminated web and film passing through the press heating zone, subjecting it to an axial extensional stress while simultaneously heating it. After passing through the heating zone, the material (i.e., the combined web and film) was then cooled to below 50°C in a cooling zone of the press set to a temperature of approximately 40°C while maintaining the same 80 bar pressure on the material as in the heating zone. The material was then cooled at 30° C. for 10 min at 30° C. This continuously compresses / contracts the material by subjecting it to an axial extensional stress such that it is maintained under a continuous and constant pressure. After the 4-ply material had passed the full length of the press, it was cooled to room temperature (about 72° C.) while still being held under the same pressure. The compressed material was then removed from the press at or about room temperature. The resulting structure was a one-piece, monolithic, 4-fibrous ply composite web comprising (film / 0° web / 90° web / 0° web / 90° web / film). Multiple square / rectangular test specimens were then cut from this 4-ply composite web and tested for their tensile, shear, and friction properties.
[0070] Examples 14 to 18 Tensile Property Testing Tensile properties were obtained following ASTM D3019 and ASTM D5034 / 5035 guidelines on a standard Instron 1332 load frame machine using MTS647.10A hydraulic grips. Test specimens were attached directly to the grips and tension was applied by pulling the specimen away from the grips until failure. All tests were performed at room temperature (72°F) with a tensile loading rate of 0.1 in / min. Displacement and strain data were obtained using DIC (digital image correlation) equipment to capture digital images, which were analyzed using VIC3D software from Correlated Systems Inc. Tension specimens were tested until failure.
[0071] [Table 4] Table 4
[0072] Examples 19 to 22 Shear Property Test The shear properties were obtained using the ASTM D8067 test method. Rather than mounting the test specimens directly in hydraulic grips as in Comparative Examples 1-5, the test specimens were mounted on a rectangular picture frame type fixture held on a standard Instron 1332 load frame machine. The rectangular frame was then gripped using the same MTS647.10A hydraulic grips as in Comparative Examples 1-5. The shear properties of the materials are tested under quasi-static, extremely small loads (shear strains) with the load applied at two diagonal corners according to the ASTM D8067 method. The shear strain rate for the tests was 0.1 in / min, and the specimens were loaded until they buckled. Displacement and strain data were obtained using DIC equipment and analyzed using VIC3D software from Correlated Systems Inc. as described above for Comparative Examples 1-5.
[0073] [Table 5] Table 5
[0074] Examples 23 to 26 Friction Coefficient Test The samples were also tested to determine their coefficient of friction, with friction properties measured according to the ASTM G115 method. Friction testing was performed on a GCTS biaxial test frame (International Test Equipment, Tempe, AZ) with a shear actuator moving the sample and a normal actuator applying a normal force to the sample at a constant displacement. Friction data was obtained from the system using two load cells: a vertical normal actuator and a shear actuator.
[0075] [Table 6] Table 6
[0076] Conclusion: The fibers of each fiber ply were stretched axially as a result of the axial elongation stress applied to the fibers in the press. The tenacity of each fiber in each ply increased by at least 1% and the elongation to break of each fiber decreased by at least 1%, the reduced elongation to break value being from about 2.0% to about 3.9%. In addition, the new materials of the present disclosure exhibited higher tensile properties, lower elongation, greater shear strength, and lower coefficient of friction compared to comparative materials that were not processed by the press.
Claims
1. 1. A fibrous article comprising one or more unidirectional fiber plies, each unidirectional fiber ply comprising a plurality of unidirectionally oriented fibers coated with a polymeric binder, the fibrous article having been primed and the fibers having been axially stretched in a compression device, the fibers having an initial elongation to break value before being axially stretched and a reduced elongation to break value after being axially stretched, the initial elongation to break value being greater than the reduced elongation to break value, the reduced elongation to break value being from about 2.0% to about 3.9%.
2. The fibrous article of claim 1 , wherein the initial elongation at break value is 3.0% or greater.
3. The fibrous article of claim 1 , wherein the initial elongation at break value is 4.0% or greater.
4. 1. A method for improving fiber tensile properties of a fibrous prepreg composite, the method comprising: a) providing at least one fibrous prepreg composite including one or more unidirectional fiber plies, each of said plies including a plurality of unidirectionally oriented fibers coated with a polymeric binder, said fibers having a toughness of 7 g / denier or greater, a tensile modulus of 150 g / denier or greater, and an elongation to break of at least 2.0%, said fibers having a softening temperature and a melting temperature; b) heating the fibers of the composite to a temperature greater than the softening temperature of the fibers but less than the melting temperature of the fibers; c) subjecting the composite to an axial elongational stress while the fibers are at a temperature above the softening temperature of the fibers but below the melting temperature of the fibers, wherein the fibers in each fiber ply are elongated axially by the axial elongational stress, thereby increasing the toughness of each fiber in each ply by at least 1% and decreasing the elongation to break of each fiber by at least 1%.
5. 5. The method of claim 4, wherein the composite is subjected to the axial tensile stress while passing through a compression conveyor, the axial tensile stress being at least about 0.25 kilograms force (2.45 Newtons).
6. 6. The method of claim 5, wherein the compression conveyor includes two pressure application elements, the composite being compressed between the pressure application elements, whereby the pressure application elements simultaneously subject the composite to an axial tensile stress while simultaneously transporting the composite through the compression conveyor.
7. 7. The method of claim 6, wherein the composite passes over the compression conveyor as a continuous web, the web being maintained under continuous and constant axial tension.
8. 6. The method of claim 5, wherein each composite comprises two cross-plied unidirectional fiber plies consolidated together, and the composite is subjected to multiaxial tensile stresses while passing through a compression conveyor.
9. 6. The method of claim 5, wherein each composite comprises two cross-plied unidirectional fiber plies consolidated together, and the composite is subjected to multiaxial tensile stresses while passing through a compression conveyor.
10. A plurality of the composite materials are inserted into the compaction conveyor, and the composite materials are compressed by the compaction conveyor.
10. The method of claim 9, wherein the wires are not attached to each other upon insertion into the wire.
Citation Information
Patent Citations
Manufacture of reinforced plastic ribbon
JP1978058574A
High-strength, ultra-high molecular weight polyethylene tape articles
JP2013501653A
Method for manufacturing multilayer material sheets, multilayer material sheets and their uses
JP2013514206A
Polymer fibers with improved ballistic performance
JP2013529282A
Fiber-reinforced composite material
JP2014024969A