Semiconductor device
By using a gate insulating layer with low hydrogen and high halogen content, the issue of excessive drain current in oxide semiconductor transistors is resolved, enhancing electrical performance and reducing manufacturing complexity.
Patent Information
- Application Number
- JP2024128719
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2010-07-01
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Transistors using oxide semiconductors face issues with significant drain current flow when the gate electrode potential equals the source electrode potential, due to hydrogen migration from the gate insulating layer to the oxide semiconductor layer, affecting electrical characteristics.
Incorporating a gate insulating layer with low hydrogen content and high halogen concentration, such as fluorine and chlorine, to suppress hydrogen movement and inactivate hydrogen present in the oxide semiconductor layer, thereby reducing hydrogen concentration to levels below 6×10^20 atoms/cm^3 and increasing halogen concentration to 1×10^19 atoms/cm^3 or more.
This configuration results in transistors with improved electrical characteristics, maintaining reliable operation below 0°C and reducing manufacturing costs by avoiding high-temperature processes.
Smart Images

Figure 2024150761000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor device including an oxide semiconductor and a manufacturing method thereof.
[0002] In this specification, a semiconductor device is a device that can function by utilizing semiconductor characteristics. Generally speaking, electro-optical devices, semiconductor circuits, and electronic devices are all semiconductor devices. [Background technology]
[0003] In recent years, in liquid crystal display devices and light-emitting display devices, such as flat panel displays, The transistors used in many of these devices are made of amorphous silicon or polycrystalline silicon on a glass substrate. It is made of silicon semiconductors such as crystalline silicon.
[0004] Recently, technology that uses oxide semiconductors in transistors instead of silicon semiconductors has been attracting attention. do.
[0005] For example, oxide semiconductors include zinc oxide, which is a single-component metal oxide, and There are In-Ga-Zn-O oxides, and transistors are made using them. Technologies for use in switching elements of device pixels have been disclosed (Patent Documents 1 and 2). (See Reference 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2006-165528 A [Patent Document 2] JP 2007-96055 A [Patent Document 3] JP 2007-123861 A Summary of the Invention [Problem to be solved by the invention]
[0007] A transistor that uses an oxide semiconductor for the channel region has a threshold voltage (V th ) but my When the potential of the gate electrode is the same as that of the source electrode (V gs =0 V), there is a problem that a certain amount of drain current flows.
[0008] In view of the above, one embodiment of the present invention disclosed in this specification is a semiconductor device having excellent electrical characteristics. An object of the present invention is to provide a semiconductor device. [Means for solving the problem]
[0009] In order to solve the above problem, a gate insulating film in contact with an oxide semiconductor layer in which a channel region is formed is The layer is an insulating layer having a low hydrogen content and containing halogen such as fluorine or chlorine. Therefore, the migration of hydrogen from the gate insulating layer to the oxide semiconductor layer is suppressed, and the oxide semiconductor In order to inactivate or release hydrogen present in the layer, a hydrogen-containing oxide semiconductor layer is The amount of can be reduced.
[0010] Specifically, when the hydrogen concentration is 6×10 20 atoms / cm 3 Less than 2 x 10 20 atoms / cm 3 Less than 5×10, more preferably 19 atoms / cm 3 Below is , and the halogen concentration is 1×10 19 atoms / cm 3 More than 1×10 2 0 atoms / cm 3The above gate insulating layer is used.
[0011] One embodiment of the present invention is a semiconductor device including a gate electrode layer, an oxide semiconductor layer in which a channel region is formed, and an oxide A source electrode layer and a drain electrode layer electrically connected to the oxide semiconductor layer, and a gate electrode layer and an oxide semiconductor layer a gate insulating layer disposed between the oxide semiconductor layer and the gate insulating layer via the oxide semiconductor layer; A semiconductor layer having a hydrogen concentration of 6×10 20 atoms / cm 3 less than , preferably 2 x 10 20 atoms / cm 3 Less than 5×10, more preferably 19 at oms / cm 3 The halogen concentration is less than 1×10 19 atoms / cm 3 That's all, Preferably 1 x 10 20 atoms / cm 3 The semiconductor device has the insulating layer described above. .
[0012] Another embodiment of the present invention is a semiconductor device comprising: an oxide semiconductor layer; Another embodiment of the present invention is a bottom-gate transistor in which a gate electrode The transistor has a top gate structure in which the oxide semiconductor layer is overlapped with the gate insulating layer. It is a ninja.
[0013] In another embodiment of the present invention, the gate insulating layer is formed using a material selected from the group consisting of silicon oxide, silicon oxynitride, and silicon nitride. an oxide insulating layer which is silicon oxide, hafnium oxide, aluminum oxide, or tantalum oxide; To do so.
[0014] The gate insulating layer includes a first gate insulating layer in contact with the gate electrode layer and an oxide semiconductor. and a second gate insulating layer in contact with the semiconductor layer. In this case, the second gate insulating layer is formed by a water By using a material that has a low halogen content and contains halogen, The transfer of hydrogen from the oxide semiconductor layer to the oxide semiconductor layer is suppressed, and the hydrogen present in the oxide semiconductor layer is prevented from being transferred to the oxide semiconductor layer. In order to inactivate or release hydrogen from the oxide semiconductor layer, the hydrogen content in the oxide semiconductor layer is reduced. This can be done.
[0015] In another aspect of the present invention, the gate insulating layer includes a first gate insulating layer in contact with a gate electrode layer; a second gate insulating layer in contact with the oxide semiconductor layer, Concentration is 6×10 20 atoms / cm 3 Less than 2 x 10 20 atoms / cm 3 Less than 5×10, more preferably 19 atoms / cm 3 The second gate insulator The concentration of halogen in the edge layer is 1×10 19 atoms / cm 3 More than 1x, preferably 10 20 atoms / cm 3 The semiconductor device is characterized as described above.
[0016] Furthermore, in other insulating layers constituting the above-mentioned semiconductor device and in contact with the oxide semiconductor layer, By using materials with low hydrogen content and containing halogens, the oxide semiconductor layer is prevented from The migration of hydrogen to the conductor layer is suppressed, and the hydrogen present in the oxide semiconductor layer is inactivated. Therefore, the hydrogen content in the oxide semiconductor layer can be reduced. .
[0017] In another embodiment of the present invention, the hydrogen concentration in an insulating layer in contact with an oxide semiconductor layer is 6×1020 at oms / cm 3 Less than 2 x 10 20 atoms / cm 3 The following is more preferable: is 5 x 10 19 atoms / cm 3 The halogen concentration is less than 1×10 20 ato ms / cm 3 More than 1×10 21 atoms / cm 3 The present invention is characterized by the above. It is a semiconductor device.
[0018] Another embodiment of the present invention is a semiconductor device having a gate insulating film, the gate insulating film being in contact with the oxide semiconductor layer and provided between the oxide semiconductor layer and a substrate. The hydrogen concentration in the insulating layer is 6×10 20 atoms / cm 3 Less than 2 x 10 20 a toms / cm 3 Less than 5×10, more preferably 19 atoms / cm 3 is as follows: The concentration of halogen is 1×10 20 atoms / cm 3 More than 1×10 21 at oms / cm 3 The thickness of the insulating layer is the thickness of the oxide semiconductor layer and the thickness of the gate insulating layer. A top-gate transistor and such a transistor are more than five times the sum of the thicknesses of the The semiconductor device has the following features.
[0019] Another embodiment of the present invention is a semiconductor device including an insulating layer provided over a substrate and an oxide semiconductor layer in contact with the insulating layer. a pair of conductive regions provided in contact with the oxide semiconductor layer; a gate electrode layer provided on the conductive region with an insulating film interposed therebetween, A top-gate transistor characterized in that it does not contact with The semiconductor device has the following features.
[0020] In another embodiment of the present invention, a semiconductor device is provided in which silicon tetrafluoride (SiF4), tetrafluoride (SiF4), tetrafluoride (Te) are in contact with an oxide semiconductor layer. It is obtained by using silicon halide such as silicon chloride (SiCl4) as a raw material gas. The semiconductor device is provided with an insulating film mainly made of silicon oxide. The insulating film to be used is one in which the ratio of silicon among elements other than oxygen in the insulating film is 70% or more, preferably is 90% or more. Effect of the Invention
[0021] According to one embodiment of the present invention, a semiconductor device having favorable electrical characteristics can be provided. [Brief description of the drawings]
[0022] [Figure 1] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device (transistor). [Diagram 2] FIG. 1 is a diagram showing a cluster model centered on a gallium atom. [Diagram 3] FIG. 1 is a diagram showing a reaction formula and an energy diagram for a hydrogen atom elimination reaction. [Figure 4] FIG. 1 is a diagram showing a model used for calculating binding energy. [Diagram 5] FIG. 1 is a diagram showing a reaction formula and an energy diagram for a hydrogen atom elimination reaction. [Figure 6] 1A to 1C are cross-sectional views illustrating a method for manufacturing a transistor. [Figure 7] 1A to 1C are cross-sectional views illustrating a method for manufacturing a transistor. [Figure 8] 1A to 1C are cross-sectional views illustrating a method for manufacturing a transistor. [Figure 9] 1A to 1C are cross-sectional views illustrating a method for manufacturing a transistor. [Figure 10] FIG. 4 is a diagram showing the hydrogen concentration and the fluorine concentration contained in a silicon oxide layer. [Figure 11] FIG. 1 is an external view showing an example of an electronic book. [Figure 12] FIG. 1 is an external view showing an example of a television device and a digital photo frame. [Figure 13] FIG. 1 is a perspective view showing an example of a portable computer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following description, and the embodiments and aspects of the present invention may be modified without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various modifications may be made to the details. The present invention should not be construed as being limited to the description of the following embodiment. In describing the configuration of the invention using the same reference numerals, the same elements are used in different drawings. In addition, when referring to similar items, the same hatch pattern will be used and no particular symbol will be attached. For convenience, the insulating layer may not be shown in the top view. The size, layer thickness, or area of each component shown in the figures may be exaggerated for clarity. Therefore, it is not necessarily limited to that scale.
[0024] In addition, when it is stated that A and B are connected, it means that A and B are electrically connected. This includes the case where A and B are directly connected to each other, and the case where A and B are directly connected to each other. The object is assumed to be an object (e.g., a device, an element, a circuit, a wiring, an electrode, a terminal, a conductive film, a layer, etc.). do.
[0025] In addition, the function of the "source" and "drain" in a transistor is to control the current in the circuit operation. For this reason, in this specification, The terms "source" and "drain" may be used interchangeably.
[0026] (Embodiment 1) In this embodiment, a semiconductor device according to one embodiment of the present invention will be described with reference to FIG. Although FIG. 1 shows a transistor as a semiconductor device, it may be a diode or other device. can also be implemented in the same way.
[0027] FIG. 1(A) is a top view of a transistor. FIG. 1(B) is a top view of a transistor shown in FIG. 1(A) along A1-B1. The transistor has a base insulating layer 102 and a gate electrode formed on a substrate 101. a gate insulating layer 104; and an oxide semiconductor layer 106 in which a channel region is to be formed. The source electrode layer 107a and the drain electrode layer 107b, the oxide semiconductor layer 106 and the source and an insulating layer 108 that covers the source electrode layer 107a and the drain electrode layer 107b.
[0028] In the transistor illustrated in FIG. 1, an oxide semiconductor layer 106 is connected to a gate insulating layer 104 via a gate insulating layer 104. The transistor has a bottom gate structure and is formed to overlap the top electrode layer 103. In the transistor shown in FIG. 1, the source electrode layer 107a and the drain electrode layer 107b are It is a top contact type formed in contact with a part of the upper surface of the compound semiconductor layer 106 .
[0029] In addition to the top-contact type, bottom-gate transistors also have a source electrode layer. and a drain electrode layer is formed in contact with a part of the lower surface of the semiconductor layer in which the channel region is formed. In this embodiment, a top contact type will be described. However, even if it is a bottom contact type, it can be implemented by referring to this embodiment mode.
[0030] The transistor shown in FIG. 1 has a portion of the upper surface of the gate insulating layer 104 and a portion of the lower surface of the oxide semiconductor layer 106. Therefore, in the process of manufacturing a transistor, the gate insulating layer 10 When a large amount of hydrogen is present in the oxide semiconductor layer 104, the hydrogen diffuses into the oxide semiconductor layer 106, and the oxide semiconductor layer 1 When the hydrogen content in the oxide semiconductor layer 106 increases, the hydrogen content in the oxide semiconductor layer 106 increases. The number of carriers in the compound semiconductor layer 106 increases. As a result, the threshold voltage ( V th ) changes in the negative direction, and the potential of the gate electrode becomes the same as the potential of the source electrode. In this case (V gs = 0V), drain current flows. Become a star.
[0031] In order to remove hydrogen diffused from the oxide semiconductor layer 106, the oxide semiconductor layer 106 is subjected to a heat treatment. However, this method requires additional manufacturing steps for the transistors, which is costly and requires a lot of labor. Heat treatment at about 400℃ is not effective enough. I also know that it isn't.
[0032] On the other hand, according to the findings of the present inventors, hydrogen in the gate insulating layer 104 in contact with the oxide semiconductor layer 106 Concentration 6×10 20 atoms / cm 3 Less than 2 x 10 20 atoms / cm 3 Less than 5×10, more preferably 19 atoms / cm 3 and the halogen concentration is Degrees 1×10 19 atoms / cm 3 More than 1×10 20 atoms / cm 3 In this case, the transfer of hydrogen from the gate insulating layer 104 to the oxide semiconductor layer 106 is suppressed. In addition, hydrogen present in the oxide semiconductor layer 106 can be inactivated or released. Since the above effect can be obtained, the hydrogen content in the oxide semiconductor layer 106 can be reduced. It became clear that...
[0033] That is, the gate insulating layer 104 in contact with the oxide semiconductor layer 106 is treated to have the above-mentioned hydrogen concentration and halide concentration. By using a gate insulating layer with a high concentration of fluorine, it is possible to obtain a good In particular, the maximum process temperature is set to 40 A transistor that can be operated at temperatures below 0°C, preferably below 350°C, while still having practical reliability and characteristics. Of course, the maximum process temperature is not a limitation in the practice of the present invention. The maximum temperature of the process may be 400° C. or higher.
[0034] In addition, the oxide semiconductor layer 106, the source electrode layer 107a, and the drain electrode layer 107b The insulating layer 108 covering the oxide semiconductor layer 106 is in contact with a part of the upper surface of the oxide semiconductor layer 106. The hydrogen concentration in layer 108 is 6×10 20 atoms / cm 3 Less than 2 x 10 20 a toms / cm 3 Less than 5×10, more preferably 19 atoms / cm 3 The following is Haroge The concentration of 19 atoms / cm 3 More than 1×10 20atoms / c m 3 In this manner, transfer of hydrogen from the insulating layer 108 to the oxide semiconductor layer 106 is suppressed. At the same time, hydrogen present in the oxide semiconductor layer 106 is inactivated or desorbed. Therefore, the hydrogen content in the oxide semiconductor layer 106 can be reduced. It is possible to provide a semiconductor device having excellent electrical characteristics.
[0035] There are no particular limitations on the substrate 101 as long as it can withstand the subsequent manufacturing steps. For example, The substrate 101 is a glass substrate, a ceramic substrate, a quartz substrate, or a sapphire substrate. Insulating substrates such as silicon, semiconductor substrates made of semiconductor materials such as metal or stainless steel A conductive substrate made of any conductor, or a semiconductor substrate or a conductive substrate with its surface covered with an insulating material A coated substrate or the like can be used. Plastic substrates can also be used as appropriate. Cut.
[0036] In addition, the glass substrate is heated to 600°C or higher during the transistor manufacturing process. If you do this, it is best to use a material with a strain point of 730°C or higher. For example, aluminosilicate Glass materials such as vitreous glass, aluminoborosilicate glass, and barium borosilicate glass are used. Used.
[0037] The base insulating layer 102 prevents the diffusion of impurity elements from the substrate 101 and also serves to This prevents the substrate from being etched during the etching process in the manufacturing process. Although there is no limitation on the thickness of the insulating layer 102, for the above reasons, the thickness of the base insulating layer 102 is set to 50 nm. It is preferable that the amount is equal to or more than that.
[0038] The base insulating layer 102 may be made of silicon oxide, silicon oxynitride, silicon nitride, silicon nitride oxide, or hafnium oxide. A single or double layer structure is used with an insulating layer of tantalum oxide, aluminum oxide, or tantalum oxide. The laminated structure described above is formed.
[0039] Here, silicon oxynitride refers to a material whose composition contains more oxygen than nitrogen. For example, oxygen is at least 50 atomic % to 70 atomic % and nitrogen is at least 0.5 atomic %. % or less, and silicon in the range of 25 atomic % or more and 35 atomic % or less. Silicon nitride oxide refers to a material whose composition contains more nitrogen than oxygen. For example, oxygen is 5 atomic % or more and 30 atomic % or less, and nitrogen is 20 atomic % or more and 55 atomic % or less. % or less, and silicon content in the range of 25 atomic % to 35 atomic %.
[0040] The above range is based on the Rutherford Backscattering Spectroscopy (RBS). tering spectrometry and Hydrogen Forward Scattering (HFS) The measurements were taken using 10-nm forward scattering (FSc). The total content of the constituent elements does not exceed 100 atomic %.
[0041] The gate electrode layer 103 is formed on the base insulating layer 102. The material of the gate electrode layer 103 is , molybdenum, titanium, chromium, tantalum, tungsten, platinum, palladium, osmium Metallic materials such as tungsten, alloy materials mainly composed of these metallic materials, or nitrides of these metals It is to be noted that the temperature of the heat treatment to be performed in the subsequent step can be set to 100° C. If the metal material can withstand high temperatures, aluminum or copper may be used. Aluminum or copper is a high melting point metal material to avoid heat resistance and corrosion problems. It is recommended to use it in combination with high melting point metal materials such as molybdenum, titanium, chromium, Tantalum, tungsten, neodymium, scandium, etc. can be used.
[0042] The gate electrode layer 103 may have a single-layer structure or may be a laminate of two or more films made of different materials. For example, the gate electrode layer 103 having a stacked structure may be formed by depositing a molybdenum film on an aluminum film. Two-layer structure with molybdenum film laminated on copper film, or two-layer structure with molybdenum film laminated on copper film, or copper A two-layer structure in which a titanium nitride film or a tantalum nitride film is laminated on the film, a titanium nitride film and a molybdenum film It is preferable that the gate electrode has a two-layer structure in which the gate electrode is laminated with a silicon film. The layer 103 may be an aluminum film, an alloy film of aluminum and silicon, or an alloy film of aluminum and titanium. The intermediate layer is a tungsten film, a nitride film, or an aluminum-neodymium alloy film. It is preferable to have a structure in which a tungsten film, a titanium nitride film or a titanium film is disposed above and below the above-mentioned film. I wish.
[0043] The gate electrode layer 103 may be formed of indium oxide, an alloy of indium oxide and tin oxide, or Zinc oxide, zinc aluminum oxide, zinc aluminum oxide nitride, The light-transmitting oxide conductor such as zinc gallium oxide or polycrystalline silicon can be used. can.
[0044] In addition, the gate electrode layer 103 is made of In-ON, In-Zn-ON, In-Ga-O- InN-based, In-Ga-Zn-ON-based oxynitrides, etc. may also be used. -Ga-Zn-ON oxynitrides are oxynitrides that contain at least In, Ga, and Zn. There is no particular limitation on the composition ratio. In addition, elements other than In, Ga, and Zn may be included. stomach.
[0045] The thickness of the gate electrode layer 103 is not particularly limited, and may be made of a metal material, an alloy material, or other chemical material. The time required for the manufacturing process and the electrical resistance of the conductive film made of the compound can be taken into consideration and the For example, it may be formed to a thickness of 10 nm to 500 nm.
[0046] A gate insulating layer 104 is provided over the gate electrode layer 103. As described above, the gate Since the insulating layer 104 is in contact with the oxide semiconductor layer 106, the hydrogen concentration of the gate insulating layer 104 is 6×10 20 atoms / cm 3 Less than 2 x 10 20 atoms / cm 3 below , and more preferably 5 × 10 19 atoms / cm 3 The fluorine concentration is 1×1 or less. 0 19 atoms / cm 3 More than 1×10 20 atoms / cm 3 That is all It is good.
[0047] This suppresses the transfer of hydrogen from the gate insulating layer 104 to the oxide semiconductor layer 106. At the same time, hydrogen present in the oxide semiconductor layer 106 is inactivated or desorbed. Therefore, the amount of hydrogen contained in the oxide semiconductor layer 106 can be reduced. The thickness of the edge layer 104 is appropriately determined taking into consideration the dielectric strength and the manufacturing process of the transistor. It is possible.
[0048] If the above hydrogen concentration and fluorine concentration are satisfied, the gate insulating layer 104 is Although the example shown in FIG. 02 can be used, in this embodiment, plasma CVD (Pl asma Enhanced Chemical Vapor Deposition) The silicon oxide layer formed by this method is described below.
[0049] The plasma CVD method is a method in which deposition gas is supplied as a raw material to a reaction chamber in a plasma CVD device. In the plasma CVD method, the following steps are performed: For example, a film with better step coverage can be formed compared to sputtering methods.
[0050] Plasma CVD equipment includes capacitively coupled high-frequency plasma CVD equipment that uses a high-frequency power source, and inductively coupled Inductively coupled high-frequency plasma CVD equipment, magnetron and dielectric as microwave sources A microwave plasma CVD apparatus (electron Cyclotron resonance plasma CVD equipment) and other helicon wave plasma CVD equipment. In the plasma CVD method described in this specification, glow discharge plasma is used for film formation. In addition, the plasma CVD method can be used by heating the substrate. This can be done.
[0051] As the deposition gas source, a gas that does not contain hydrogen in its composition formula is selected, and silicon oxide is In other words, fluorine (HF) is used as the deposition gas, not silane (SiH4). Silicon carbide (e.g., SiF4) or silicon chloride (e.g., SiCl4) is used. The gas used for oxidation is nitrous oxide (N2O), which has a reduced content of hydrogen and water. Or oxygen, with other gases such as argon added to stabilize the plasma. The gas used should also have a low hydrogen and water content.
[0052] Furthermore, when forming a silicon oxide layer by plasma CVD, After removing impurities such as hydrogen and water remaining in the reactor or adsorbed on the inner wall of the reactor, The deposition gas is preferably a gas having the above composition, while the inner wall of the reaction chamber is heated. When silicon fluoride is used, the hydrogen concentration of the gate insulating layer 104 is set to 6×10 20 atom s / cm 3 Less than 2 x 10 20 atoms / cm 3 Less than 5, more preferably ×10 19 atoms / cm 3 The fluorine concentration is 1×10 19 atoms / cm 3 End , preferably 1 x 10 20 atoms / cm 3 It can be more than that.
[0053] In addition, when a silicon oxide layer containing fluorine is formed on the gate electrode layer 103, The resulting fluorine may etch the gate electrode layer 103, but it may not etch the gate insulating layer. This can be prevented by forming the edge layer in two or more layers. The fluorine concentration of the first gate insulating layer is 1×10 19 atoms / cm 3 Less than is preferred It is.
[0054] The second gate insulating layer in contact with the oxide semiconductor layer 106 is made of the above-mentioned silicon tetrafluoride. The silicon oxide layer used has a fluorine concentration of 1×10 19 atoms / cm 3 Above, I prefer 1×10 20 atoms / cm3 The insulating layer must be at least 100%. The gate insulating layer is formed of silicon tetrafluoride or the like, and the second gate insulating layer is a silicon oxide layer. For example, the first gate insulating layer has a thickness that does not disappear when the first gate insulating layer is formed. The insulating layer exemplified as the ground insulating layer 102 can be used.
[0055] The oxide semiconductor layer 106 in which the channel region is formed is formed on and in contact with the gate insulating layer 104. The thickness of the oxide semiconductor layer 106 is 10 nm to 300 nm, preferably 20 nm to 100 nm.
[0056] The oxide semiconductor layer 106 is an In-Ga-Zn-O-based oxide containing In, Ga, and Zn. As the oxide semiconductor, a quaternary oxide such as In-Sn -Ga-Zn-O system, ternary oxides such as In-Sn-Zn-O system and In-Al-Zn -O system, Sn-Ga-Zn-O system, Al-Ga-Zn-O system, Sn-Al-Zn-O system, etc. , binary oxides such as In-Zn-O, In-Ga-O, Sn-Zn-O, and Al- Zn-O, Zn-Mg-O, Sn-Mg-O, In-Mg-O, and indium oxide The insulating layer can be formed of In-Ga, tin oxide, zinc oxide, or the like. The Zn-O oxide is an oxide containing at least In, Ga, and Zn. There is no particular limitation on the composition ratio. Furthermore, elements other than In, Ga, and Zn may be included.
[0057] The oxide semiconductor layer 106 is formed of a material having the chemical formula InMO3(ZnO). m (m>0) The oxide can be used to form the layer. Here, M is Ga, Al, Mn, or Co. For example, M is Ga, Ga, and Al, Ga and Mn, or Ga and Co, etc.
[0058] The source electrode layer 107a and the drain electrode layer 107b are formed by the gate insulating layer 104 and the oxide The source electrode layer 107a and the drain electrode layer 10 7 b may be of a similar material and thickness to the gate electrode layer 103 .
[0059] The insulating layer 108, which functions as a passivation film or an interlayer insulating film, is The drain electrode layer 107a, the drain electrode layer 107b, and the oxide semiconductor layer 106 are formed in contact with each other. The insulating layer 108 can be formed in the same manner as the gate insulating layer 104. Since the gate insulating layer 104 is in contact with a part of the upper surface of the gate insulating layer 106, a silicon oxide layer similar to the gate insulating layer 104 is used. The transfer of hydrogen from the insulating layer 108 to the oxide semiconductor layer 106 is suppressed, and the oxide semiconductor layer In order to inactivate or desorb hydrogen present in the oxide semiconductor layer 106, The hydrogen content in 06 can be reduced.
[0060] In the process of forming the insulating layer 108, the same process as that of the gate insulating layer 104 is performed. Similarly, the fluorine contained in the deposition gas causes the source electrode layer 107a and the drain electrode layer Therefore, the thickness of the insulating layer 108 may be reduced by It should be decided appropriately taking into consideration the above.
[0061] The insulating layer 108 may be formed by a method capable of reducing the hydrogen content. Silicon oxide is formed by a silicon target or a silicon oxide target. Preferably, a silicon oxide target is used, and more preferably, Preferably, the hydroxyl group concentration is 1000 ppm or less, or the hydrogen concentration is 3.5×10 1 9 atoms / cm 3 The silicon oxide target is as follows: The gases to be supplied are a rare gas such as argon and oxygen. The gas to be used should have impurities such as hydrogen, water, hydroxyl groups, or hydrides of 1 ppm or less, preferably 1 It is preferable to use a high-purity gas that has been removed to below ppb level.
[0062] The following describes how hydrogen present in the oxide semiconductor layer 106 is inactivated by fluorine. The effect of desorption is explained using quantum chemical calculations. The quantum chemical calculations shown below use Gaussian Density Functional Theory using the Gaussian Basis In density functional theory, the exchange-correlation interaction is expressed by the electron density. Since the calculation is approximated by a functional of the one-electron potential, the calculation is fast and highly accurate. In this embodiment, the mixed functional B3LYP is used to calculate the exchange and correlation energy. A weight for each parameter is specified.
[0063] In addition, the basis functions applied to all atoms are three contraction functions for each valence orbital. The basis function of the triple split valence basis set is 6-311G. With this basis function, the 1s to 3s orbitals are taken into account for hydrogen atoms, and If present, the 1s-4s and 2p-4p orbitals are taken into account. Furthermore, to improve the accuracy of the calculation, As a polarization basis set, p-functions are added to hydrogen atoms, and d-functions are added to non-hydrogen atoms. Then, The quantum chemistry calculation program used was Gaussian 09 from Comflex Corporation. There are.
[0064] In this embodiment, hydrogen atoms present in the oxide semiconductor layer 106 are substituted with oxygen atoms or metal atoms. Since the hydrogen atom is bonded to the oxide semiconductor layer 106, the structure containing hydrogen is represented by the following structural formula (α- 1) and structural formula (α-2). The following structural formula (α-1) and structural formula In (α-2), coordinate bonds are not taken into consideration, and only ionic bonds are taken into consideration. The oxide semiconductor layer 106 in the above embodiment is made of In (indium) or Ga (gallium). and Zn (zinc), and the following structural formula (α-1) and structural formula (α-2) The metal atom represented by (α-2) is Ga (gallium).
[0065] [ka]
[0066] The process in which fluorine atoms react with hydrogen in the oxide semiconductor layer 106 is as shown in (Formula 1). There are the reactions shown in (Equation 2) and (Equation 2).
[0067] Ga-OH + F →HF + Ga-O (Eq. 1)
[0068] Ga-H + F →HF + Ga (Eq. 2)
[0069] In formula 1, fluorine radicals react with hydrogen atoms of hydroxyl groups to produce HF (hydrogen fluoride) molecules. In formula 2, the fluorine radical reacts with the hydrogen atom bonded to the gallium atom to form a molecule. The reaction forms HF (hydrogen fluoride) molecules. " represents a radical.
[0070] In this quantum chemical calculation, in the above structural formula (α-1) and structural formula (α-2), A simple cluster model was used to calculate the activation energy for the above reaction. and evaluates the likelihood of a reaction occurring.
[0071] Quantum chemical calculations were performed on the reaction of (Equation 1), and the reaction path and energy diagram were analyzed. The ram is shown in Figure 3.
[0072] In Figure 3, in the initial state (1), the hydroxyl group and the fluorine radical are assumed to be infinitely far apart. In the energy diagram, the energy of the initial state (1) is used as the reference. Intermediate (2) In the case of fluorine radicals, the Ga-O bond is broken and a hydroxyl radical is generated. This reaction produces a Ga-F bond. The energy is -1.67 eV.
[0073] In intermediate (3), the hydrogen atom of the hydroxyl radical combines with a fluorine atom to produce an HF molecule. The activation energy, which is the potential energy difference between intermediates (2) and (3), is The energy is calculated to be 0.61 eV. In intermediate (4), oxygen radicals and HF molecules react with each other. In the final state (5), the oxygen radical and the HF molecule are infinitely far apart.
[0074] In reality, HF may be desorbed from the oxide semiconductor layer 106 or may remain there for some reason. Even if HF remains in the oxide semiconductor layer 106, the water in the HF molecule may be Since the silicon is not bonded to the oxide semiconductor (i.e., it is inactivated), It does not serve as a carrier source for the conductor.
[0075] In intermediate (2), the fluorine radical approaches the gallium atom, forming a Ga-O bond. The fact that the Ga-O bond is broken and a Ga-F bond is formed means that the bond energy of the Ga-O bond is 4.37 This is due to the fact that the bond energy of the Ga-F bond is 5.31 eV.
[0076] The bond energy of the Ga-O bond here is the state in which a hydroxyl group is bonded to a gallium atom. (See Figure 4(A)) and the hydroxyl radical are infinitely far apart. This is the calculated value of the potential energy difference between the two states (see FIG. 4(B)). The bond energy of the Ga-F bond is the state in which fluorine is bonded to a gallium atom (Figure 4( C)) and the potential energy of the fluorine radicals in the state where they are infinitely far apart ( This is the calculated value of the potential energy difference between the two (see Figure 4(D)).
[0077] The reaction of hydrogen and fluorine in the oxide semiconductor layer 106 shown in formula 1 occurs in the initial state (1 The energy difference between the initial state (1) and the final state (5) indicates that this reaction is exothermic. It can be said that the reaction proceeds easily.
[0078] Next, quantum chemical calculations were performed on the reaction of (Equation 2), and the reaction path and energy diagram were analyzed. The agram is shown in Figure 5.
[0079] In FIG. 5, in the initial state (1), the hydrogen atom and the fluorine radical are infinitely far apart. In the energy diagram, the energy of the initial state (1) is used as the reference. In (2), the fluorine radical approaches the gallium atom, breaking the Ga-H bond and forming a hydrogen bond. This reaction produces a Ga-F bond. The peak energy is -1.99 eV.
[0080] In intermediate (3), a hydrogen radical combines with a fluorine atom to form an HF molecule. The activation energy, which is the difference in potential energy between (2) and intermediate (3), is 0. In intermediate (4), the oxygen atom bonded to the gallium atom and the HF The molecules are interacting, and in the final state (5), the HF molecules are infinitely far apart.
[0081] As in (Equation 1), in intermediate (2), when a fluorine radical approaches a gallium atom, G The a-H bond is broken and the Ga-F bond is formed for the same reason as explained in (Equation 1). In particular, the Ga-F bond is more stable than the Ga-H bond in terms of bond energy. This is due to the following.
[0082] In the reaction of desorbing hydrogen from the oxide semiconductor layer 106 shown in Formula 2, the initial state ( The energy difference between (1) and the final state (5) indicates that this is an exothermic reaction. Therefore, hydrogen It can be said that the reaction of removing the
[0083] As described above, hydrogen present in the oxide semiconductor layer 106 is inactivated by fluorine, or It can be detached.
[0084] Next, a method for manufacturing the semiconductor device shown in FIG. 1 will be described with reference to FIG.
[0085] An underlying insulating layer 102 is formed on a substrate 101. The substrate 101 and the underlying insulating layer 102 are In this embodiment, a glass substrate is used as the substrate 101. The insulating base layer 102 can also be formed by a plasma CVD method. In the manufacturing method of the device, the target is silicon oxide, and the gas supplied during formation is argon, etc. A silicon oxide layer of 200 nm is formed by RF sputtering using rare gas and oxygen. .
[0086] Next, a conductive film that functions as a gate electrode layer 103 is formed. The device was fabricated using a DC sputtering method with a titanium target, with a thickness of 150 nm. A titanium film having a thickness of 1.0 m is then formed. Then, a first photolithography step and an etching step are performed. Thus, a gate electrode layer 103 having a thickness of 150 nm is formed.
[0087] The conductive film may be etched by either wet etching or dry etching. From the viewpoint of miniaturization of elements, it is preferable to use dry etching. The etching gas and etching solution must be selected appropriately depending on the material to be etched. can.
[0088] Note that the side surface of the gate electrode layer 103 is preferably tapered. On the top of 3, a conductive film that will become an oxide semiconductor film, a source electrode layer, and a drain electrode layer in a later process is provided. Therefore, if the side surface of the gate electrode layer 103 is tapered, the alignment at the step portion is not performed. This is effective in preventing disconnection of the line. To do this, etching may be performed while the resist mask is being recessed.
[0089] Next, the gate insulating layer 104 is formed by the plasma CVD method. The inner wall of the reaction chamber is heated to release impurities from the inner wall of the reaction chamber. The impurities that are released from the inner wall of the reaction chamber are removed by fluoride such as nitrogen trifluoride (NF3). The fluorine compound is used for plasma cleaning. A capacitively coupled plasma CVD apparatus using a power supply is used.
[0090] The temperature to which the inner wall of the reaction chamber in the plasma CVD device is heated is set to 100°C or higher and 350°C or lower. The temperature is preferably 100° C. or higher and 125° C. or lower, and the heating time is preferably at least 30 minutes or longer. It is preferable to carry out the heating process for 60 minutes or more. In addition, this heating process should be carried out while exhausting air. It is also possible.
[0091] There is no particular limitation on the method of plasma cleaning. A method of generating plasma and cleaning in a reaction chamber where cleaning is performed. The example shown here is a plasma generated in advance outside the reaction chamber where cleaning is performed. The generated plasma is supplied to a reaction chamber to perform cleaning. It may also be training.
[0092] The plasma cleaning in the present semiconductor device manufacturing method includes a plasma processing step and an exhaust step. The specific plasma cleaning conditions are: nitrogen trifluoride at 400sccm The pressure in the reaction chamber is kept at 10 Pa to 200 Pa. The electrode spacing is adjusted to 15mm to 60mm, and the frequency range is 13.56MHz to 60MHz. High frequency power supply: 500W to 2000W (power per unit electrode area (power density) As for the power consumption, it is 1W / cm 2 ~4W / cm 2 ) to generate plasma, and the The more preferable plasma cleaning conditions are nitrogen trifluoride and The pressure in the reaction chamber was set to about 70 Pa. The pole spacing was adjusted to 50 mm, and the output was 900 W (converted to power density) at a high frequency power source of 60 MHz. Approximately 1.8 W / cm 2 ) for 7 minutes.
[0093] Then, silicon tetrafluoride is used as a deposition gas, and suboxide is used as an oxidation gas. Nitrogen chloride and argon as an additive gas are supplied to the reaction chamber, and plasma energy is assisted to In addition, when the gate insulating layer 104 is formed as a two-layer structure, a silicon oxide film is formed to a thickness of 200 nm. The first gate insulating layer in contact with the gate electrode layer 103 is treated with an oxidizing gas using silane as a deposition gas. A silicon film is formed to a thickness of 150 nm, and deposited on the second gate insulating layer in contact with the oxide semiconductor layer 105. A silicon oxide film of 50 nm thickness is formed by using silicon tetrafluoride as the reactive gas. The structure obtained in this process is shown in FIG. 6(A).
[0094] Next, a 50 nm thick oxide semiconductor film is formed by DC sputtering. Since the conductor film is formed in contact with the gate insulating layer 104, the conductive film is formed by the gate insulating layer 104. The fluorine in the oxide semiconductor film inactivates or releases hydrogen present in the oxide semiconductor film. Furthermore, oxygen is supplied from the gate insulating layer 104 to defects in the oxide semiconductor film. In the form of, DC sputtering method is used, but vacuum deposition method, pulsed laser deposition method, CV It may be formed by using the D method or the like.
[0095] In the method for manufacturing a semiconductor device, In (indium), Ga (gallium), and Zn (zinc ) containing oxide semiconductor target (molar ratio of In2O3:Ga2O3:ZnO=1:1 :1, or In2O3:Ga2O3:ZnO=1:1:2) The semiconductor device uses an In-Ga-Zn-O-based oxide semiconductor film obtained by the above method. The fabrication method used was DC sputtering, with an argon flow rate of 30 sccm and an oxygen The flow rate of the raw material is set to 15 sccm.
[0096] Note that before the oxide semiconductor film is formed by a sputtering method, argon gas is introduced. It is preferable to perform reverse sputtering to generate plasma. In the experiment, a voltage was applied to the substrate side using an RF power source in an atmosphere of argon, nitrogen, helium, etc. This is a method of forming plasma near the substrate by using oxygen, nitrous oxide, etc. It may be performed in an atmosphere containing chlorine (Cl2), carbon tetrafluoride (CF4), etc. It may be carried out in a comfortable atmosphere.
[0097] When the oxide semiconductor film is formed, the substrate temperature is set to 100° C. or higher and lower than 550° C., preferably 2 The substrate is heated to 00°C or higher and 400°C or lower. Then, the moisture in the processing chamber is removed. Then, a sputtering gas from which hydrogen, water, etc. have been removed is introduced, and the oxide semiconductor target is The oxide semiconductor film is formed by heating the substrate. In this way, moisture contained in the oxide semiconductor film can be further reduced. This can reduce damage caused by the gun.
[0098] In order to remove moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. For example, a cryopump, an ion pump, a titanium sublimation pump, etc. can be used. Alternatively, a turbo pump with a cold trap may be used. Hydrogen and water can be removed from the processing chamber by evacuating it using a pump, etc. Therefore, the concentrations of these elements in the oxide semiconductor film can be reduced.
[0099] Thereafter, a second photolithography step and an etching step are performed to form an island-shaped An oxide semiconductor layer 105 is formed. A structure obtained through the steps up to this point is shown in FIG 6B.
[0100] Then, place the sample in an inert gas atmosphere (nitrogen, helium, neon, argon, etc.) or in a room with a dew point of 100°C. The oxide semiconductor layer 1 is grown in a dry air atmosphere with a low moisture content, for example, at a temperature of 60° C. or less. For example, heat treatment may be performed at 100°C to 400°C for 10 minutes or more. This can be done by heat treatment.
[0101] Heat treatment is carried out using an electric furnace, a GRTA (Gas Rap) method using heated gas, etc. id Thermal Anneal (LRTA) method or lamp light Rapid Thermal Annealing (RTA) and other instantaneous heating methods can be used. For example, when heat treatment is performed using an electric furnace, the temperature rise rate can be set to 0.1℃ / min. Temperature drop rate should be 0.1℃ / min to 15℃ / min. is preferred.
[0102] In the method for manufacturing the semiconductor device, the oxide semiconductor layer 105 is subjected to heat treatment to remove moisture, water, and other The oxide semiconductor layer 106 is formed from which the atoms are desorbed. The fluorine contained in 4 inactivates or deactivates hydrogen present in the oxide semiconductor film. Furthermore, oxygen is supplied from the gate insulating layer 104 to the defects in the oxide semiconductor layer 106. will be done.
[0103] In addition, under an inert gas atmosphere (nitrogen, helium, neon, argon, etc.), 00℃ to 750℃ (or a temperature below the distortion point of the glass substrate) for 1 minute to 10 minutes RTA (Rapid Threshold Annealing) is preferably performed at 600°C for 3 to 6 minutes. The RTA method can be used to perform thermal annealing in a short time. Since dehydration or dehydrogenation can be performed quickly, processing can be performed even at temperatures exceeding the distortion point of the glass substrate. can be done.
[0104] In the heat treatment, an inert gas (nitrogen, helium, neon, argon, etc.) is used. It is preferable that the rare gas does not contain moisture, hydrogen, etc. The purity of nitrogen or rare gases such as helium, neon, and argon is 6N (99.999). 9%) or more, preferably 7N (99.99999%) or more (i.e., impurity concentration of 1 ppm It is preferable to set the concentration to 0.1 ppm or less.
[0105] Note that the heat treatment can be performed after the island-shaped oxide semiconductor layer 105 is formed. The heat treatment may be performed on the oxide semiconductor film before the formation of the oxide layer 105. After the heat treatment, the oxide semiconductor layer 106 may be partly crystallized. .
[0106] Here, the exposed surface of the oxide semiconductor layer 106 is oxidized with oxygen, ozone, or nitrous oxide. Plasma treatment may be performed. By performing the plasma treatment, defects in the oxide semiconductor layer 106 can be eliminated. The structure obtained by the above steps is shown in Figure 6(C).
[0107] Next, a conductive film is formed, and a third photolithography step and an etching step are performed; The source electrode layer 107a and the drain electrode layer 107b are formed. In the method for manufacturing a semiconductor device, the titanium target A titanium film with a thickness of 150 nm was formed by DC sputtering using a photolithography machine. The source electrode layer 107a and the drain electrode layer 107b are formed by a lithography process and an etching process. Form 07b.
[0108] Then, the insulating layer 108 is formed. Using the same gas and method, a silicon oxide layer having a thickness of 50 nm is formed. After forming the insulating film 08, a heat treatment may be performed. The heat treatment may be performed in an inert gas atmosphere (nitrogen, The heating is preferably performed under a temperature of 200°C or higher and 40°C or lower. It is recommended to carry out the treatment at 0°C or below. Alternatively, you can carry out the RTA treatment described above. The structure obtained through the process is shown in FIG. 6(D).
[0109] The structure described in this embodiment prevents diffusion of hydrogen into the oxide semiconductor layer 106. In addition, hydrogen present in the oxide semiconductor layer 106 can be inactivated or desorbed, and thus the oxide semiconductor layer 106 can be favorably deactivated. A semiconductor device having favorable electrical characteristics can be obtained. can be appropriately combined with the configurations shown in other embodiments of this specification.
[0110] (Embodiment 2) In this embodiment, the deposition gas contains silicon tetrafluoride, and the gas for oxidizing the silicon tetrafluoride is a suboxide. Nitrogen was used as the gas for generating stable plasma, and argon was used as the gas for plasma generation. Silicon oxide with low hydrogen concentration obtained by the Zuma CVD method is used as the base insulation for top-gate transistors. An example of use as an edge layer will be described with reference to FIG.
[0111] A base insulating layer 202 containing silicon oxide as a main component is formed on a substrate 201. As mentioned above, 2 is formed by plasma CVD using silicon tetrafluoride. The method for forming the gate insulating layer 104 in the first embodiment can be referred to. Five times or more the sum of the thicknesses of the oxide semiconductor layer and the gate insulating layer that are subsequently formed It would be good if that were the case.
[0112] At such a thickness, the amount of fluorine that diffuses from the insulating underlayer is sufficient to form an oxide Hydrogen present in the semiconductor layer and the gate insulating layer is inactivated, or the oxide semiconductor layer The thickness of the base insulating layer is larger than that of the oxide semiconductor layer and the gate insulating layer. If the thickness is less than twice the sum of the thicknesses of the edge layers, the amount of fluorine is insufficient to prevent such No effect is obtained.
[0113] Then, an In-Ga-Zn-O oxide film having a thickness of 10 to 30 nm is formed as an oxide semiconductor film. A film of oxide is formed by sputtering. This is then etched to form island-shaped oxide films. A semiconductor layer 203 is obtained. The oxide semiconductor layer 203 is subjected to heat treatment in order to reduce the hydrogen concentration. This state may be achieved. The state up to this point is shown in FIG.
[0114] Next, a conductive film is formed to cover the base insulating layer 202 and the oxide semiconductor layer 203. For example, a multi-layer film of titanium and aluminum may be formed by sputtering. Then, this is etched to form a source electrode layer 204a and a drain electrode layer 204b. At that time, the relationship between the etching rate of the conductive film and the etching rate of the oxide semiconductor layer 203 is Therefore, the surface of the oxide semiconductor layer 203 may also be etched.
[0115] Here, fluorine and fluorine are used as the material for the bottom surface of the source electrode layer 204a and the drain electrode layer 204b. Reactive metallic materials (e.g. titanium, tungsten, molybdenum, aluminum or When a nitride of these is used, the source electrode layer 204a and the drain electrode layer 204b are However, it is preferable that the insulating base layer 202 is not in contact with the insulating base layer 202 .
[0116] The source electrode layer 204a and the drain electrode layer 204b made of these materials are formed on the base insulating layer 2 When the source electrode layer 204a and the drain electrode layer 202 come into contact with each other, a chemical reaction occurs at the interface. Therefore, as shown in FIG. 7B, the source electrode layer 204a The drain electrode layer 204b is preferably provided only over the oxide semiconductor layer 203.
[0117] The bottom surfaces of the source electrode layer 204a and the drain electrode layer 204b are made of a material such as an oxide conductor. If the material is used, the above-mentioned problems do not occur.
[0118] Further, a base insulating layer 202, an oxide semiconductor layer 203, a source electrode layer 204a, a drain electrode layer 204b, and a The electrode layer 204b is covered with a silicon oxynitride film having a thickness of 10 to 30 nm by a plasma CVD method. A gate insulating layer 205 is formed by using a plasma CVD method. Therefore, a gate insulating film with excellent electrical conductivity can be obtained.
[0119] It is preferable that the gas used does not contain fluorine or chlorine. When a gas having such a property is used, the source electrode layer 204a and the drain electrode layer 204b are etched during deposition. This is because there is a risk that the information may be compromised.
[0120] Therefore, it is preferable to use silane and ammonia as the deposition gas. The silicon oxynitride obtained by the above method contains a large amount of hydrogen. However, as mentioned above, These hydrogen atoms are inactivated because fluorine is provided by the insulating underlayer 202 having a sufficient thickness. The state up to this point is shown in FIG 7(B).
[0121] Next, a conductive film is formed covering the gate insulating layer 205, and then etched to form a gate electrode. A gate electrode layer 206 is formed. A gate insulating layer 205 and a conductive film for forming a gate electrode layer are deposited. It is desirable to carry out the deposition continuously without exposing it to the atmosphere.
[0122] Then, a 100 to 300 nm thick insulating layer of silicon oxide is formed by plasma CVD. Then, an insulating layer 207 is deposited on the insulating film 208, which has a flat surface, using an organic resin or the like. The deposition of the layer 207 is also carried out in a deposition manner in order to avoid etching of the gate electrode layer 206 during deposition. The reactive gas is silane or TEOS (tetraethoxysilane, Si(OC2H5 )4) is recommended.
[0123] Although a large amount of hydrogen is contained in the insulating layer 207, the insulating layer 207 and the channel region of the transistor are The regions are separated by the gate electrode layer 206 and therefore are less likely to cause reliability problems. In order to improve reliability and prevent etching of the gate electrode layer 206, an insulating layer 207 is a multi-layered first insulating layer having a thickness of 20 to 100 nm that contacts the gate electrode layer 206. The first insulating layer is formed using the above-mentioned silane or TEOS, and the second insulating layer on top is formed using fluoride. It may also be formed using silicon (for example, silicon tetrafluoride).
[0124] Finally, the source electrode layer 204a, the source electrode layer 204b, the gate insulating layer 205, the insulating layer 207, and the insulating layer 208 are formed. A contact hole reaching the drain electrode layer 204b is provided, and the electrodes 209a and 209b are The state up to this point is shown in Figure 7(C).
[0125] By the above steps, a top-gate transistor can be manufactured. Although an example in which silicon fluoride is used as the deposition gas for the edge layer 202 has been shown, silicon chloride may also be used. It goes without saying that this embodiment can be combined with other embodiments.
[0126] (Embodiment 3) In this embodiment, a silicon oxide film having a low hydrogen concentration obtained by using silicon tetrafluoride as a deposition gas is used. An example of using this as a base insulating layer for a top-gate transistor is explained with reference to FIG. do.
[0127] A base insulating layer 302 containing silicon oxide as a main component is formed on a substrate 301. As mentioned above, 2 is formed by plasma CVD using silicon tetrafluoride. The method for forming the gate insulating layer 104 in the first embodiment can be referred to. Five times or more the sum of the thicknesses of the oxide semiconductor layer and the gate insulating layer that are subsequently formed It would be good if that were the case.
[0128] Then, as the oxide semiconductor film 303, an In-Ga-Zn-O based A conductive film 3 is formed by sputtering to cover the oxide semiconductor film 303. As the conductive film, for example, a tungsten film is formed by a sputtering method. That's good.
[0129] Further, a resist is applied onto the conductive film 304, and photolithography is performed using a multi-tone mask. A resist mask 305 having at least two portions with different thicknesses formed by a patterning method. The state up to this point is shown in Figure 8(A).
[0130] Then, a first etching is performed using this resist mask 305. The conductive film 304 and the portion not covered with the resist mask are removed by isotropic dry etching. The first etching is performed on the oxide semiconductor film 303. The first etching is performed on the oxide semiconductor film 303. A conductive layer 303a and a conductive layer 304a having approximately the same shape as the conductive layer 303a are obtained (see FIG. 8(B)).
[0131] In the dry etching, the resist mask 305 is also etched, resulting in the formation of the resist mask 305 shown in FIG. As shown in FIG. 1, the resist mask 305 is divided into two resist masks 305a and 305b. On the other hand, etching of the resist mask 305 does not occur in wet etching. In addition, even in dry etching, depending on the conditions, the resist mask 305 is almost completely etched. In some cases, the etching process is not completed. In such cases, a separate ashing process is performed. The resist mask 305 is etched to have a shape as shown in FIG. 8(B).
[0132] Next, a second etch is performed using the two resist masks 305a and 305b. This etching is required to selectively etch the conductive layer 304a. In addition, a method is adopted in which the side surface of the conductive layer 304a after etching is tapered. In this manner, the source electrode layer 304b and the drain electrode layer 304c are obtained. (See FIG. 8(C)).
[0133] From the above-mentioned formation of the base insulating layer 302, a source electrode layer 304b and a drain electrode layer 304c are obtained. In the process up to this stage, a multi-tone mask is used, so the In contrast, in the second embodiment, the source electrode layer 204a and the drain electrode layer 2 Two photolithography steps are required to obtain 04b.
[0134] In the second embodiment, in order to form the oxide semiconductor layer 203, In the conventional method, it was necessary to apply a resist onto the oxide semiconductor film 3. Alternatively, no resist is applied onto the oxide semiconductor layer 303a, and the oxide semiconductor The surface of the layer 303a can be kept clean.
[0135] As is clear from the above process, the source electrode layer 304b and the drain electrode layer 304c Since the insulating film 303 is formed only on the oxide semiconductor layer 303a, it is not in contact with the base insulating layer 302. do not have.
[0136] Further, a base insulating layer 302, an oxide semiconductor layer 303a, a source electrode layer 304b, a drain electrode layer 304b, and a The electrode layer 304c is covered with a silicon oxynitride film having a thickness of 10 to 30 nm by a plasma CVD method. A gate insulating layer 306 made of the above is formed. The state up to this point is shown in FIG.
[0137] Next, a conductive film is formed covering the gate insulating layer 306, and then etched to form a gate electrode. Then, a pole layer 307 is formed by sputtering to a thickness of 100 to 300 nm. An insulating layer 308 made of silicon oxide is deposited, and then an insulating layer with a flat surface is formed by using an organic resin or the like. Then, a solenoid is formed on the gate insulating layer 306, the insulating layer 308 and the insulating layer 309. Contact holes are provided to reach the source electrode layer 304b and the drain electrode layer 304c, and the electrode 31 The state up to this point is shown in FIG.
[0138] By the above steps, a top-gate transistor can be manufactured. Although silicon fluoride is used as the deposition gas for the edge layer 302, silicon chloride may also be used. It goes without saying that this embodiment can be combined with other embodiments.
[0139] (Embodiment 4) In this embodiment, a silicon oxide film having a low hydrogen concentration obtained by using silicon tetrafluoride as a deposition gas is used. An example of using the above-mentioned as an insulating base layer for a top-gate type transistor provided on a multilayer wiring circuit This will be described with reference to FIG.
[0140] Wiring 402a and wiring 402b are provided on substrate 401. 402b is not limited to a simple wiring, but may be a gate voltage of a transistor provided on the substrate 401. The electrode layer, source electrode, drain electrode, or wiring extending from them may be used. That is, even if a transistor using a semiconductor material such as silicon is provided on the substrate 401, good.
[0141] The wiring 402a and the wiring 402b are covered with a silicon oxynitride film by a plasma CVD method. A base film 403 is formed. The silicon nitride oxide film 403 preferably contains an appropriate amount of hydrogen. The silicon oxynitride film 403 is formed on the wiring 402a, the wiring 402b and the substrate 401. By covering the transistor, hydrogen can be supplied to the transistor. If the transistor is made of silicon or germanium, hydrogen can damage the semiconductors. Dangling bonds in conductor materials can be terminated, improving transistor characteristics. It can be done as follows.
[0142] The thickness of the silicon oxynitride film 403 is preferably determined in consideration of several factors. First, it must be determined taking into consideration the effect of hydrogenation. Thus, the silicon oxynitride film 403 also serves as an etching stopper in the planarization process. Thirdly, in the etching process after planarization, Since the insulating layer (formed on the silicon oxynitride film 403) is etched together with the insulating layer, The difference in etching rate between the insulating layer and the silicon oxynitride film 403 does not impair flatness. It is necessary that the degree of
[0143] From the above first and second requirements, it is desirable that the silicon oxynitride film 403 be thick. Considering these factors, the thickness of the silicon oxynitride film 403 is The thickness may be, for example, 50 to 200 nm.
[0144] Next, a base insulating layer 404 containing silicon oxide as a main component is formed. As shown in the figure, it is formed by using silicon tetrafluoride with the plasma CVD method. This allows the side surfaces of the wiring 402a and the wiring 402b to be formed with good step coverage. The thickness of the edge layer 404 is set to be equal to the thickness of the subsequently formed oxide semiconductor layer and gate insulating layer. The thickness of the base insulating layer 404 is preferably 5 times or more the sum of the thicknesses of the layers 402 and 403. It is advisable to make the plate thicker in anticipation of this. As shown in.
[0145] Thereafter, the insulating base layer 404 is planarized by a known chemical mechanical polishing (CMP) method. This process can be stopped when the silicon oxynitride film 403 is exposed. Silicon oxide has a smaller etching rate in the CMP method than silicon oxide, This is to function as a topper. The state up to this point is shown in FIG. 9(B). 4 is divided by the silicon nitride oxide film 403 (underlying insulating layer 404a). In addition, the surface is almost flat.
[0146] Thereafter, the silicon oxynitride film 403 and the base insulating layer 404a are roughly removed by dry etching. The same thickness is etched to obtain a flat surface. At this stage, the etching process is stopped when the surface of the insulating base layer 404a is exposed. The state is changed to that shown by 404b in FIG. 9(C).
[0147] Thereafter, a top-gate transistor is manufactured in the same manner as in the second and third embodiments. That is, an In-Ga-Zn-O-based film having a thickness of 10 to 20 nm is used, and the oxide is formed. A semiconductor layer 405 is formed, and a source electrode layer 406a and a drain electrode layer 406b are formed thereon. Furthermore, a gate insulating layer 407 is formed (see FIG. 9C).
[0148] Here, the oxide semiconductor layer 405 is in contact with the wiring 402a and the source electrode layer 406a. The source electrode layer 402a and the source electrode layer 406a overlap with each other with the oxide semiconductor layer 405 interposed therebetween. When an oxide semiconductor and a conductor are in ohmic contact, the oxide semiconductor In the region up to a depth of about 10 nm, the carrier concentration is 1×10 19 / cm 3 The degree or Since the thickness is more than 100 nm, the wiring 402 is substantially the same as the wiring 402 although the oxide semiconductor layer 405 is present therebetween. a and the source electrode layer 406a can be regarded as being electrically connected.
[0149] In order to achieve ohmic contact, the wiring 402a and the source electrode layer 406a are made of an oxide semiconductor. It is necessary to make an ohmic contact at the interface with the conductive layer 405. The work function of the source electrode layer 406a is It is preferable to use a material having an electron affinity smaller than that of the oxide semiconductor layer 405. For example, In the case of In-Ga-Zn-O oxide semiconductors, the electron affinity is about 4.3 eV. Therefore, titanium or titanium nitride is preferably used. The same applies to 6b.
[0150] Next, a conductive film is formed covering the gate insulating layer 407, and then etched to form a gate electrode. Then, an insulating layer 409 made of silicon nitride and a surface layer made of organic resin or the like are formed. A flat insulating layer 410 is formed. Then, the gate insulating layer 407 and the insulating layer 409 are insulated. Contact holes are formed in the layer 410, which reach the source electrode layer 406a and the drain electrode layer 406b. Electrodes 411a and 411b are formed by providing a conductive layer 411b on the insulating layer 411. The state up to this point is shown in FIG.
[0151] Through the above steps, a top-gate transistor can be manufactured. It can be combined with the embodiments.
[0152] (Embodiment 5) The transistor described in the above embodiment is manufactured, and the transistor is used in a pixel portion and a driving By using the semiconductor device in the operating circuit, a semiconductor device having a display function (also called a display device) can be manufactured. In addition, a part or the whole of a driver circuit using transistors may be formed on the same substrate as the pixel portion. In addition, the above-described embodiment can be used to form a system on panel. A semiconductor device including a memory cell is manufactured using a transistor using an oxide semiconductor material. It is also possible.
[0153] The display device includes a display element. The display element may be a liquid crystal element (also called a liquid crystal display element), a light-emitting A light-emitting element (also called a light-emitting display element) can be used. A light-emitting element is a light-emitting element that emits light by applying a current or a voltage. This category includes elements whose brightness is controlled by a specific factor, such as inorganic EL (Electroluminescent) devices. Also, electronic inks and other electronic devices A display medium in which the contrast changes due to thermal effects can also be applied.
[0154] The display device includes a panel in which a display element is sealed, and a controller for the panel. and a module in which an IC or the like including the above is mounted. In the process, the element substrate corresponds to one form before the display element is completed, and the element substrate is The element substrate is provided with a means for supplying a current to the display element in each of the plurality of pixels. The display element may be in a state where only the pixel electrodes of the display element are formed, or a conductive film that becomes the pixel electrodes may be formed. may be formed after etching and before forming the pixel electrode, All forms apply.
[0155] In this specification, the term "display device" refers to an image display device, a display device, or an optical Also refers to connectors, such as FPC (Flexible Printed Circuit). inted circuit) or TAB (Tape Automated Bon ding tape or TCP (Tape Carrier Package) is used. Modules with printed wiring boards attached to the ends of TAB tape or TCP or the display element is mounted with an IC (integrated circuit) by the COG (Chip On Glass) method. The display device also includes all modules in which a display circuit (or other circuit) is directly mounted.
[0156] (Embodiment 6) A display including a transistor manufactured by the manufacturing method of the transistor described in the above embodiment. The device can be applied to electronic paper that displays images by driving electronic ink. The LCD can be used in any electronic device that displays information. For example, electronic paper can be used for electronic books, posters, digital signs, etc. Nage, PID (Public Information Display), trains, etc. This can be applied to in-vehicle advertisements, displays on various cards such as credit cards, etc. An example of an electronic device is shown in Figure 11.
[0157] An electronic book 501 in FIG. 11 is composed of two cases, a case 502 and a case 503. The housing 502 and the housing 503 are integrated by a shaft portion 508. This structure allows the book to move like a paper book. It becomes possible to perform work.
[0158] A display unit 504 and a photoelectric conversion device 505 are incorporated in the housing 502, and a display The display unit 504 and the display unit 506 are incorporated. The screen may be configured to display one continuous screen, or may be configured to display different screens. By configuring the display to display different screens, for example, the display on the right side (display unit 504 in FIG. 11) ) and an image can be displayed on the left display section (display section 506 in FIG. 11). Cut.
[0159] FIG. 11 shows an example in which the housing 502 is provided with an operation unit and the like. For example, the housing 50 2, a power switch 509, operation keys 510, a speaker 511, etc. are provided. The user can turn pages by using the operation keys 510. The configuration may include a keyboard, a pointing device, etc. , external connection terminals (earphone terminal, USB terminal, or AC adapter and USB cable) A configuration including a terminal that can be connected to various cables such as a recording medium insertion section, etc. Furthermore, the electronic book 501 may be configured to have a function as an electronic dictionary. .
[0160] The electronic book 501 may be configured to transmit and receive information wirelessly. It is also possible to purchase and download desired book data from the child book server. It is possible.
[0161] (Embodiment 7) The semiconductor device disclosed in this specification can be applied to various electronic devices (including game machines). The electronic device can be, for example, a television device (television or television receivers), computer monitors, digital cameras and digital video cameras digital photo frames, mobile phones (also called mobile phones or mobile phone devices), ), portable game machines, personal digital assistants, audio playback devices, pachinko machines and other large game machines, etc. There is.
[0162] A television set 512 in FIG. 12A has a display unit 514 built in a housing 513. The display unit 514 can display images. A configuration in which a housing 513 is supported by 515 is shown.
[0163] The television device 512 can be operated using an operation switch provided on the housing 513 or a separate remote control. This can be done by the operation unit 518. 7, the channel and volume can be operated, and the image displayed on the display unit 514 can be The image can be operated by a remote control 518. A display unit 516 for displaying information output from the
[0164] The television device 512 is configured to include a receiver, a modem, and the like. It can receive general television broadcasts and can also receive wired or wireless signals via a modem. By connecting to a network, communication can be one-way (sender to receiver) or two-way It is also possible to communicate information in both directions (between sender and receiver, or between receivers). be.
[0165] A digital photo frame 519 in FIG. 12B has a display unit 521 built into a housing 520. The display unit 521 is capable of displaying various images, for example, a digital camera. By displaying image data taken with a camera or other device, it can function like a normal photo frame. This can be done.
[0166] The digital photo frame 519 includes an operation unit, an external connection terminal (USB terminal, USB A configuration including a terminal that can be connected to various cables such as a cable, a recording medium insertion section, etc. These components may be incorporated on the same surface as the display unit, but may also be provided on the side or back. For example, the recording medium of a digital photo frame is A memory that stores image data taken with a digital camera is inserted into the insertion section. The captured image data can be displayed on the display unit 521.
[0167] Furthermore, the digital photo frame 519 may be configured to be capable of wirelessly transmitting and receiving information. It is also possible to configure the device so that desired image data is wirelessly acquired and displayed.
[0168] FIG. 13 is a perspective view showing an example of a portable computer. The hinge unit connecting the upper housing 522 and the lower housing 523 is shown in a closed state. An upper housing 522 having a keyboard 524 and a lower housing 523 having a keyboard 525 are stacked together. The keyboard can be easily carried and can be easily operated by the user. In this case, the hinge unit is opened and the input operation is performed while looking at the display unit 524. It is possible.
[0169] In addition to the keyboard 525, the lower housing 523 also includes a pointing device for inputting data. If the display unit 524 is a touch input panel, a part of the display unit Input operations can be performed by touching the screen. The lower housing 523 also contains the CPU and hardware. The lower housing 523 has a computing function section such as a disk. It has an external connection port 526 into which a communication cable conforming to the communication standard is inserted.
[0170] The upper housing 522 further includes a display unit 528 that can be slid into the upper housing 522 and stored therein. It has a large display screen. The orientation of the screen can be adjusted by the user. In addition, the retractable display unit 528 can be used as a touch input panel. This allows input operations to be performed by touching part of the retractable display unit.
[0171] The display unit 524 or the retractable display unit 528 may be a liquid crystal display panel, an organic light emitting device, or an infrared ray detector. A video display device such as a light-emitting display panel having a light-emitting element is used.
[0172] The portable computer shown in FIG. 13 is equipped with a receiver and the like, and can receive television broadcasts. The image can be displayed on the display unit 524 or the display unit 528. The hinge unit connecting the main body 522 and the lower housing 523 is closed, and the display unit 52 is opened. Slide the 8 to expose the entire screen, and adjust the screen angle to watch TV broadcasts. It is also possible to open the hinge unit to turn off the display unit 524 and to turn on the TV. Since it only activates the circuitry required to display the broadcast, it consumes minimal power. This is useful in portable computers where battery capacity is limited. EXAMPLES
[0173] The gate insulating layer 104, the gate insulating layer 205, and the gate insulating layer 3 described in the above embodiment 06, the gate insulating layer 407, the insulating layer 108, the base insulating layer 202, the base insulating layer 302, and A silicon oxide film (sample A) that can be used as the insulating base layer 404 was prepared. The results of evaluation of the hydrogen and fluorine concentrations are shown in FIG.
[0174] The method for fabricating sample A will be explained. Sample A was fabricated using the plasma CVD method. The inner wall temperature of the reaction chamber of the Zuma CVD device was heated to 115°C for 60 minutes. The gas containing impurities remaining or adsorbed in the gas was released.
[0175] Next, nitrogen trifluoride (NF3) was supplied into the reaction chamber at a flow rate of 600 sccm. The pressure was set to about 70 Pa, the gap was adjusted to 50 mm, and a high frequency power source of 60 MHz was used. A power of 900 W was output for 7 minutes, and the inner wall of the reaction chamber was heated to 115°C. Cleaning was performed to remove gases containing impurities. The electrode area in the VD device is 490 cm 2 It is.
[0176] After plasma cleaning, the inner wall temperature of the reaction chamber was heated to 115°C while removing silicon oxide. A film was formed on the wafer with a target thickness of 200 nm. Silicon fluoride was used at a flow rate of 6 sccm, and nitrous oxide was used as an additive gas at a flow rate of 1000 sccm. Argon was supplied as an inert gas into the reaction chamber at a flow rate of 1000 sccm. The pressure is adjusted to 133 Pa, the gap is adjusted to 10 mm, and a silicon oxide film is formed. The temperature of the silicon wafer was adjusted to 400°C, and the wafer was heated to 800W with a 60MHz high-frequency power supply. A silicon oxide film was formed.
[0177] Next, the measurement results of sample A by SIMS are shown in FIG. 10. In FIG. 10, the vertical axis is The horizontal axis represents the hydrogen concentration or fluorine concentration contained in sample A, and the horizontal axis represents the surface of the silicon oxide film of sample A. The hydrogen concentration profile of sample A is shown by a solid line. The fluorine concentration profile of sample A is shown by the dashed line. The quantitative range is 20 nm, and the horizontal axis of 200 nm or more represents silicon wafers.
[0178] From Figure 10, the hydrogen concentration of sample A is 3.4×10 19 atoms / c m 3 The fluorine concentration of sample A is 9.2 × 10 or less in the quantitative range. 20 atom s / cm 3 It was confirmed that this was the case.
[0179] Hydrogen release is suppressed, and hydrogen present in the oxide semiconductor layer is inactivated or desorbed. It has been found that the silicon oxide film that can be formed has the above hydrogen concentration and fluorine concentration. Ta.
[0180] The silicon oxide film shown in this embodiment is used as the gate insulating layer 104, the gate insulating layer 205, and the gate insulating layer 206. layer 306, gate insulating layer 407, insulating layer 108, under-insulating layer 202, under-insulating layer 302, By using the same for the base insulating layer 404, a semiconductor device having favorable electrical characteristics can be manufactured. It is possible. [Explanation of symbols]
[0181] 101 Substrate 102 Undercoat insulation layer 103 Gate electrode layer 104 Gate insulation layer 105 Oxide semiconductor layer 106 Oxide semiconductor layer 107a Source electrode layer 107b Drain electrode layer 108 Insulating layer 201 Substrate 202 Undercoat insulation layer 203 Oxide semiconductor layer 204a Source electrode layer 204b Drain electrode layer 205 Gate Insulation Layer 206 Gate electrode layer 207 Insulating Layer 208 Insulating layer 209a electrode 209b Electrode 301 Substrate 302 Undercoat insulation layer 303 Oxide Semiconductor Film 303a Oxide semiconductor layer 304 Conductive film 304a conductive layer 304b Source electrode layer 304c Drain electrode layer 305 Resist Mask 305a Resist mask 305b Resist mask 306 Gate Insulation Layer 307 Gate electrode layer 308 Insulating layer 309 Insulating layer 310a electrode 310b electrode 401 Substrate 402a Wiring 402b Wiring 403 Silicon oxynitride film 404 Undercoat insulation layer 404a Undercoat insulation layer 404b Undercoat insulation layer 405 Oxide semiconductor layer 406a Source electrode layer 406b Drain electrode layer 407 Gate Insulation Layer 408 Gate electrode layer 409 Insulating Layer 410 Insulating layer 411a electrode 411b Electrode 501 e-books 502 Case 503 Case 504 Display section 505 Photoelectric conversion device 506 Display section 507 Photoelectric conversion device 508 Shaft 509 Power Switch 510 Operation Key 511 Speaker 512 Television Equipment 513 Case 514 Display section 515 Stand 516 Display section 517 Operation Key 518 Remote control device 519 Digital Photo Frame 520 Case 521 Display section 522 Upper case 523 Lower housing 524 Display section 525 Keyboard 526 External connection port 527 Pointing Device 528 Display section
Claims
1. A first insulating layer; an oxide semiconductor layer having a channel formation region; a gate electrode overlapping the channel formation region; the oxide semiconductor layer contains indium oxide, the first insulating layer has a region overlapping the gate electrode, an upper surface of the first insulating layer has a region in contact with the oxide semiconductor layer; The first insulating layer has a halogen element concentration of 1×10 19 atoms / cm 3 A semiconductor device having the above-mentioned region.
2. A first insulating layer; an oxide semiconductor layer having a channel formation region; a gate electrode overlapping the channel formation region; the oxide semiconductor layer includes zinc oxide, the first insulating layer has a region overlapping the gate electrode, an upper surface of the first insulating layer has a region in contact with the oxide semiconductor layer; The first insulating layer has a halogen element concentration of 1×10 19 atoms / cm 3 A semiconductor device having the above-mentioned region.
3. A first insulating layer; an oxide semiconductor layer having a channel formation region; a gate electrode overlapping the channel formation region; the oxide semiconductor layer has an oxide containing In, Ga, and Zn; the first insulating layer has a region overlapping the gate electrode, an upper surface of the first insulating layer has a region in contact with the oxide semiconductor layer; The first insulating layer has a halogen element concentration of 1×10 19 atoms / cm 3 A semiconductor device having the above-mentioned region.
Citation Information
Patent Citations
Semiconductor device and manufacturing method thereof
JP2007134687A
Semiconductor device and manufacturing method thereof
JP2010056539A
Thin film transistor, display device, and electronic apparatus
JP2011119355A
Thin film transistor array substrate having improved electrical characteristics and method of manufacturing the same
US20090184315A1
Image display
JP2006165528A