Thermoelectric material, manufacturing method thereof, and thermoelectric power generation element

A thermoelectric material with a specific composition of Mg, Sb, Bi, and Cu, optionally with Se or Te, addresses the performance limitations of existing materials by enhancing electrical conductivity and reducing thermal conductivity, making it suitable for efficient thermoelectric power generation at room temperature.

JP2024150770AActive Publication Date: 2024-10-23NAT INST FOR MATERIALS SCI
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024130036
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-09-10
Filing Date
2024-08-06
Publication Date
2024-10-23
Estimated Expiration
2041-08-25

AI Technical Summary

Technical Problem

Existing thermoelectric materials face challenges in achieving high performance at room temperature due to the rarity of tellurium (Te) and insufficient power factor and dimensionless figure of merit (ZT) for practical applications, particularly in IoT power generation.

Method used

A thermoelectric material composed of magnesium (Mg), antimony (Sb), bismuth (Bi), and copper (Cu), optionally with selenium (Se) or tellurium (Te), formulated as Mg a Sb 2-b-c Bi b M c Cu d, where a=3≦a≦3.5, 0≦b≦2, 0≦c≦0.06, 0

Benefits of technology

The material exhibits improved electrical conductivity and reduced thermal conductivity, achieving a high dimensionless figure of merit (ZT) suitable for thermoelectric power generation, especially at room temperature, suitable for IoT applications and waste heat recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150770000001_ABST
    Figure 2024150770000001_ABST
Patent Text Reader

Abstract

To provide a thermoelectric material having excellent thermoelectric properties at room temperature, a method for manufacturing the same, and a thermoelectric generating element thereof.SOLUTION: A thermoelectric material according to an embodiment of the present invention includes an inorganic compound containing magnesium (Mg), antimony (Sb) and / or bismuth (Bi), copper (Cu), and optionally M (M is at least one element selected from the group consisting of selenium (Se) and tellurium (Te)), and the inorganic compound is represented by MgaSb2-b-cBibMcCud, and parameters a, b, c, and d satisfy 3≤a≤3.5, 0≤b≤2, 0≤c≤0.06, 0<d≤0.1, and b+c≤2.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoelectric material, a manufacturing method thereof, and a thermoelectric generating element, and more particularly to a thermoelectric material comprising Mg 3 Bi 2 The present invention relates to a thermoelectric material containing the above-mentioned thermoelectric material, a method for producing the same, and a thermoelectric generating element. [Background technology]

[0002] Even in Japan, where energy conservation has progressed particularly well compared to other countries in the world, the current situation is that approximately three-quarters of the primary energy supply is discarded as thermal energy in waste heat recovery. Under these circumstances, thermoelectric power generation elements have attracted attention as solid-state elements that can recover thermal energy and directly convert it into electrical energy.

[0003] Thermoelectric power generation elements are elements that directly convert energy into electrical energy, and therefore have the advantages of easy maintenance due to the lack of moving parts, scalability, etc. For this reason, active material research is being conducted on thermoelectric semiconductors as a power source for IoT devices, etc.

[0004] For IoT power source applications, practical use at around room temperature is expected, but the thermoelectric material with the best performance at around room temperature is Bi. 2 Te 3 In the case of materials based on the ferrite alloy, the rarity of Te makes it difficult to put them to practical use on a wide scale. However, there are few materials other than these Te compounds that have relatively high performance at room temperature, which has been a problem. 3 Sb 2 Materials based on these compounds have been cited as one candidate (see, for example, Patent Documents 1 and 2 and Non-Patent Document 1).

[0005] Non-Patent Document 1 describes Mg 3.2 Sb 1.5 Bi 0.49 Te 0.01 In this study, we report a doped thermoelectric material in which the magnesium (Mg) site of the material is doped with Fe, Co, Hf, and Te (see, for example, Patent Document 1). 3 Sb2 As a system, Mg 3.2 Sb 1.5 Bi 0.5 Te 0.01 It is disclosed that by doping a small amount of the above-mentioned metal element into the Mg site of the thermoelectric material, the electrical conductivity and Seebeck coefficient of the thermoelectric material are increased, and the figure of merit is improved.

[0006] Patent Document 1 describes Mg 3+m A a B b D 2-e E e Here, the element A represents at least one selected from the group consisting of Ca, Sr, Ba, and Yb, the element B represents at least one selected from the group consisting of Mn and Zn, the value of m is -0.39 or more and 0.42 or less, the value of a is 0 or more and 0.12 or less, the value of b is 0 or more and 0.48 or less, the element D represents at least one selected from the group consisting of Sb and Bi, the element E represents at least one selected from the group consisting of Se and Te, and the value of e is 0.001 or more and 0.06 or less.

[0007] Patent Document 2 describes Mg 3+m-a A a B 2-c-e C c E e In the present invention, the element A represents at least one selected from the group consisting of Ca, Sr, Ba, Nb, Zn, and Al, the element B represents at least one selected from the group consisting of Sb and Bi, the element C represents at least one selected from the group consisting of Mn, Si, and Cr, the element E represents at least one selected from the group consisting of Se and Te, and the value of m is -0.1 or more and 0.4 or less, the value of a is 0 or more and 0.1 or less, the value of c is 0 or more and 0.1 or less, and the value of e is 0.01 or more and 0.06 or less.

[0008] Patent Documents 1 and 2 and Non-Patent Document 1 also disclose combinations of various materials, but the values ​​of the power factor and dimensionless figure of merit ZT at room temperature are particularly insufficient. Considering IoT power generation applications, -1 K -2 It is expected that thermoelectric materials with high power factors exceeding 0.1 and dimensionless figure of merit ZT exceeding 0.3 will be developed. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2017 / 072982 [Patent Document 2] JP 2018-190953 A [Non-patent literature]

[0010] [Non-Patent Document 1] Jun Mao et al., PNAS, 114(40), 10548-10553, 2017 Summary of the Invention [Problem to be solved by the invention]

[0011] In view of the above, an object of the present invention is to provide a thermoelectric material having excellent thermoelectric properties at room temperature, a method for producing the same, and a thermoelectric power generation element using the same. [Means for solving the problem]

[0012] In an embodiment of the present invention, the thermoelectric material comprises an inorganic compound containing magnesium (Mg), antimony (Sb) and / or bismuth (Bi), copper (Cu), and optionally M, where M is at least one element selected from the group consisting of selenium (Se) and tellurium (Te), and the inorganic compound is Mg. a Sb 2-b-c Bi b M cCu d and the parameters a, b, c, and d are 3≦a≦3.5, 0≦b≦2, 0≦c≦0.06, 0 <d≦0.1、および、 b+c≦2 The above problem is solved. The parameter d is 0.005≦d≦0.05 may be satisfied. The parameters a, b, c and d are 3≦a≦3.5, 0.2≦b≦0.7, 0≦c≦0.06, and 0.005≦d≦0.05 may be satisfied. The inorganic compound is La 2 O 3 It may have the type structure and the symmetry of the space group P-3m1. The Cu is 2 O 3 It may be interstitially dissolved in the structure. The thermoelectric material may be n-type. The thermoelectric material may be in a form selected from the group consisting of a powder, a sintered body, and a thin film. The thermoelectric material may be in the form of a powder or a sintered body, and the inorganic compound may be composed of crystal grains having an average grain size in the range of 3.5 μm to 30 μm. The inorganic compound may be composed of crystal grains having an average grain size in the range of 4 μm to 20 μm. The thermoelectric material is in the form of a thin film, the inorganic compound is composed of crystal grains having an average grain size in the range of 3.5 μm to 30 μm, and may further contain an organic material. In an embodiment of the present invention, the method for producing the thermoelectric material may include mixing a raw material containing magnesium (Mg), a raw material containing antimony (Sb) and / or a raw material containing bismuth (Bi), a raw material containing copper (Cu), and optionally a raw material containing M (wherein M is at least one element selected from the group consisting of selenium (Se) and tellurium (Te)) to prepare a mixture, and sintering the mixture. The above problem is solved. The sintering may be spark plasma sintering. The spark plasma sintering may be performed at a temperature of 723 K or more and 1173 K or less, under a pressure of 30 MPa or more and 100 MPa or less, for a period of 1 minute or more and 10 minutes or less. The method may further include pulverizing the sintered body obtained by the sintering. The method may further include mixing the powder obtained by the pulverization with an organic material. The method may further include carrying out a physical vapor deposition method using the sintered body obtained by the sintering as a target. In an embodiment of the present invention, the thermoelectric generating element includes p-type thermoelectric materials and n-type thermoelectric materials alternately connected in series, and the n-type thermoelectric materials may be the above-mentioned thermoelectric materials. Effect of the Invention

[0013] In an embodiment of the present invention, the thermoelectric material comprises an inorganic compound containing magnesium (Mg), antimony (Sb) and / or bismuth (Bi), copper (Cu), and optionally M, where M is at least one element selected from the group consisting of selenium (Se) and tellurium (Te). a Sb 2-b-c Bi b M c Cu dIt is represented by 3 ≦ a ≦ 3.5, 0 ≦ b ≦ 2, 0 ≦ c ≦ 0.06, 0 < d ≦ 0.1, and b + c ≦ 2. Thus, by adding Cu to an inorganic compound having Mg, Sb and / or Bi, and M as a matrix phase, a thermoelectric material with improved electrical conductivity at room temperature, effectively reduced thermal conductivity, and improved performance index can be provided. Such a thermoelectric material is advantageous for thermoelectric power generation elements.

[0014] In an embodiment of the present invention, the method for manufacturing a thermoelectric material includes mixing a raw material containing magnesium (Mg), a raw material containing antimony (Sb), and / or a raw material containing bismuth (Bi), a raw material containing copper (Cu), and, if necessary, a raw material containing M (where M is an element selected from at least one of the group consisting of selenium (Se) and tellurium (Te)) to prepare a mixture, and sintering this mixture, so that the above-mentioned thermoelectric material can be obtained, which is excellent in versatility.

Brief Description of Drawings

[0015] [Figure 1A] Flowchart showing the steps of manufacturing a thermoelectric material in an embodiment of the present invention [Figure 1B] Diagram schematically showing Mg3(Sb,Bi)2-based crystals having a La2O3-type structure [Figure 2A] Schematic diagram showing a thermoelectric power generation element (π-shaped) using a thermoelectric material in an embodiment of the present invention [Figure 2B] Schematic diagram showing a thermoelectric power generation element (U-shaped) using a thermoelectric material in an embodiment of the present invention [Figure 2C] Schematic diagram showing thin film manufacturing using a thermoelectric material in an embodiment of the present invention [Figure 2D] Schematic diagram showing powder, a compacting machine, a sintering furnace, and a sintered body using a thermoelectric material in an embodiment of the present invention [Diagram 3] Diagram showing the appearance of the sample of Example 1 [Figure 4] Diagram showing SEM images and EDS mappings of the samples of Examples 1 to 5 [Diagram 5] Diagram showing the EBSD image of the sample of Example 2 [Figure 6] EBSD image of the sample in Example 5 [Figure 7] FIG. 1 shows XRD patterns of samples of Examples 1 to 5. [Figure 8] FIG. 1 shows the Cu addition dependence of the lattice constant of the samples of Examples 1 to 5. [Figure 9] FIG. 1 shows the temperature dependence of electrical conductivity of samples in Examples 1 to 5. [Figure 10] FIG. 1 shows the Cu doping dependence of carrier concentration and mobility of samples in Examples 1 to 5. [Figure 11] FIG. 1 shows the temperature dependence of the Seebeck coefficient of samples in Examples 1 to 5. [Figure 12] FIG. 1 shows the temperature dependence of the electrical output factor of samples in Examples 1 to 5. [Figure 13] FIG. 1 shows the temperature dependence of the total thermal conductivity of samples in Examples 1 to 5. [Figure 14] FIG. 1 shows the temperature dependence of lattice thermal conductivity of samples in Examples 1 to 5. [Figure 15] FIG. 1 shows the temperature dependence of the dimensionless figure of merit ZT of the samples of Examples 1 to 5. [Figure 16] FIG. 1 shows the temperature dependence of electrical conductivity of samples in Examples 6 and 7. [Figure 17] FIG. 1 shows the temperature dependence of the Seebeck coefficient of samples in Examples 6 and 7. [Figure 18] FIG. 1 shows the temperature dependence of the electrical output factor of samples in Examples 6 and 7. [Figure 19] FIG. 13 shows the temperature dependence of the total thermal conductivity of samples of Examples 6 to 7. [Figure 20] FIG. 1 shows the temperature dependence of lattice thermal conductivity of samples in Examples 6 and 7. [Figure 21] FIG. 13 shows the temperature dependence of the dimensionless figure of merit ZT of the samples of Examples 6 to 7. [Figure 22] FIG. 1 shows the temperature dependence of electrical conductivity of samples of Examples 8 to 10. [Figure 23] FIG. 1 shows the temperature dependence of the Seebeck coefficient of samples in Examples 8 to 10. [Figure 24] FIG. 13 shows the temperature dependence of the electrical output factor of samples of Examples 8 to 10. [Diagram 25]FIG. 13 shows the temperature dependence of the total thermal conductivity of samples of Examples 8 to 10. [Figure 26] FIG. 13 shows the temperature dependence of the lattice thermal conductivity of samples of Examples 8 to 10. [Figure 27] FIG. 13 shows the temperature dependence of the dimensionless figure of merit ZT of the samples of Examples 8 to 10. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that like elements are given like reference numerals and their description will be omitted.

[0017] (Embodiment 1) In an embodiment of the present invention, the thermoelectric material comprises an inorganic compound containing magnesium (Mg), antimony (Sb) and / or bismuth (Bi), copper (Cu), and optionally M, where M is at least one element selected from the group consisting of selenium (Se) and tellurium (Te).

[0018] Inorganic compounds include Mg a Sb 2-b-c Bi b M c Cu d The parameters a to d are expressed as follows: 3≦a≦3.5, 0≦b≦2, 0≦c≦0.06, 0 <d≦0.1、および、 b+c≦2 By making the composition as described above, the whole may be configured as an inorganic compound having a composition in which an inorganic compound consisting of Mg, Sb and / or Bi, and M is used as a parent phase, to which Cu is added. In this way, a thermoelectric material can be provided in which the electrical conductivity is improved, particularly at room temperature (temperature range of 273 K or more and 320 K or less), the thermal conductivity is effectively reduced, and the figure of merit is improved. In the embodiment of the present invention, by making the thermoelectric material satisfy the above-mentioned composition, it can function as an n-type thermoelectric material having electrons as carriers.

[0019] The inorganic compound matrix is ​​preferably Mg a Sb 2-b-c Bi b M c The matrix preferably comprises Mg 3 Sb 2 It is a La-based crystal. 2 O 3 It has a structure of the above formula (I) and belongs to the P-3m1 space group (164th in the International Tables for Crystallography). In the present specification, "-3" represents "3 with an overscore".

[0020] Mg 3 Sb 2 The system is composed of the above elements (e.g., Mg, Sb, Bi, Se, Te) and has the above crystal structure (e.g., La 2 O 3 The structure may be a tetracyclic structure (type structure) and a space group (for example, P-3m1 space group). Other than that, there are no particular limitations, but examples include Mg 3 Sb 2 , Mg 3.2 (Sb,Bi) 2 , Mg 3.2 ((Sb,Bi),M) 2 The term (Sb,Bi) indicates that Sb and Bi occupy the site where Sb and Bi occupy without distinction from each other, and the term ((Sb,Bi),M) indicates that Sb and / or Bi and M occupy the site where Sb and / or Bi occupy without distinction from each other. Here, M is at least one element selected from the group consisting of Se and Te. Mg 3.2 (Sb,Bi) 2 Exemplary compositions include Mg 3.2 Sb 1.5 Bi 0.5 There is. Mg 3.2 ((Sb,Bi),M) 2 Exemplary compositions include Mg 3.2 Sb 1.5 Bi 0.49 Te 0.01Any of these may have the above-mentioned crystal structure and space group, and the so-called excess components may constitute so-called defects in some crystal structures, and the inorganic compound as a whole may be endowed with properties such as n-type.

[0021] In the embodiment of the present invention, Mg 3 Sb 2 The crystals are La 2 O 3 It has a tetrahydrofuran-type structure and belongs to the P-3m1 space group. 3 Sb 2 The crystal structure of the Mg system is shown diagrammatically. 3 Sb 2 The components constituting the system crystal may be replaced by other elements, or may be dissolved as interstitial atoms (e.g., Cu). In such cases, the lattice constant may change, but it is considered that the atomic positions given by the crystal structure, the sites occupied by the atoms, and their coordinates will not change so much that the chemical bonds between the skeletal atoms are broken. In the examples of the present invention, if the lattice constants obtained by Rietveld analysis of the results of X-ray diffraction or neutron diffraction of the obtained inorganic compound in the space group P-3m1 are within ±5% of the theoretical values ​​(a=4.582 Å, b=4.582 Å, c=7.244 Å), it is determined that the compound is Mg. 3 Sb 2 It can be determined that the crystal is a crystalline form.

[0022] In the embodiment of the present invention, Mg a Sb 2-b-c Bi b M c The parent phase is Mg 3 Sb 2 The Sb and Bi may be completely substituted for each other. For example, Mg 3 Sb 2 The crystals are Mg 3 Bi 2It may include a crystal structure. For example, the parameter b may be 0 or more, and may be 0.2 or more. It may be 2 or less. It may be 0.7 or less. Also, c representing the component amount of M(Se and / or Te) may be 0 or more, and may be 0.06 or less. The addition of M is the Mg of the matrix phase 3 Sb 2 It may be imparted to an inorganic compound that has obtained some properties without causing destruction of the crystal structure of the system crystal. The parameter d representing the component amount of Cu is greater than 0. More preferably, it may be 0.001 or more, and may be 0.005 or more. The parameter d is 0.1 or less, but preferably may be 0.05 or less, 0.025 or less. Also, it may satisfy the range of 0 < d ≤ 0.1, and preferably may satisfy the range of 0.005 ≤ d ≤ 0.05. In such a range, the electrical conductivity at room temperature can be further improved, the thermal conductivity can be further reduced, and the performance index can be improved. The parameter d more preferably may satisfy the range of 0.005 ≤ d ≤ 0.025. In this range, the performance index at room temperature can be improved.

[0023] The parameters a to d preferably 3 ≤ a ≤ 3.5, 0.2 ≤ b ≤ 0.7, 0 ≤ c ≤ 0.06, and, 0.005 ≤ d ≤ 0.05 are satisfied. By having such a composition, the electrical conductivity at room temperature can be further improved, the thermal conductivity can be further reduced, and the performance index can be improved.

[0024] The Cu atoms are preferably considered to be substitutionally solid-solved in the La 2 O 3 type structure. Generally, Mg 3 Sb 2It was thought that the elements added to the system crystals would replace some of the elements that make up the crystal structure. It was also thought that the elements would affect the crystal structure of the resulting inorganic compound. However, the inventors of the present application have found that adding Cu can promote grain growth and grain boundary modification of the material. Such grain growth and grain boundary modification contribute to the carrier scattering mechanism, and scattering is reduced at relatively low temperatures such as room temperature (500K or less), so that it is believed that electrical resistance at room temperature is reduced, electrical conductivity is improved, and thermoelectric performance is improved.

[0025] The presence of Cu atoms in the interstitial solid solution can be confirmed by measuring the change in the lattice constants of the a-axis and c-axis by powder X-ray diffraction of the resulting inorganic compound. 3 Sb 2 When the system crystal is identified and the lattice constants (e.g., a, c) obtained by Rietveld analysis are increased compared to the lattice constants of the corresponding inorganic compound without Cu, it may be possible to determine that Cu is interstitially dissolved.

[0026] In the embodiment of the present invention, the thermoelectric material may be in a form selected from the group consisting of powder, sintered body, and thin film, which can be applied to various thermoelectric generating elements exhibiting high thermoelectric performance at room temperature.

[0027] In the embodiment of the present invention, when the thermoelectric material is a powder or a sintered body, the inorganic compound may be made of crystal grains having an average grain size in the range of 3.5 μm to 30 μm. This can increase the scattering effect, improve the electrical conductivity at room temperature, and improve the thermoelectric performance. More preferably, the inorganic compound may be made of crystal grains having an average grain size in the range of 4 μm to 20 μm. This can further increase the scattering effect, improve the electrical conductivity at room temperature, and reduce the thermal conductivity despite the large grain size, thereby further improving the thermoelectric performance. Even more preferably, the inorganic compound may be made of crystal grains having an average grain size in the range of 4 μm to 10 μm.

[0028] In this specification, the average grain size of crystal grains is analyzed and calculated by image analysis software (HKL CHANNEL5, HKL Tango, ver.5.12.72.0, Oxford Instruments Co., Ltd.) attached to an electron backscatter diffraction (EBSD) measurement device.

[0029] In the embodiment of the present invention, the thermoelectric material may be in the form of a thin film, and the thin film may be a crystalline thin film formed by physical vapor deposition or the like, as described below, or may be a thin film containing the above-mentioned powder. Here, generally, the powder may include crushed fine particles or powder. A powder compact can be formed by pressing the powder with a press such as a powder compactor. Generally, a powder compact refers to a powder compressed into a predetermined shape. When heated at a temperature below the melting point of the powder components, the contact surfaces of the powder particles are bonded to each other, and the powder compact shrinks and densifies with increasing heating time. This phenomenon is called sintering, and the product obtained by sintering can also be called a sintered body. The thin film refers to a thin film, and may include a layer formed by condensing a gas phase on a solid surface.

[0030] In the embodiment of the present invention, when the thermoelectric material is a film containing powder of an inorganic compound, the powder is mixed with an organic material and processed into a film. In this case, the organic material can be at least one organic material selected from the group consisting of poly(3,4-ethylenedioxythiophene) polystyrene sulfonate (PEDOT:PSS), poly[2,5-bis(3-tetradecylthiophen-2-yl)thieno[3,2-b]thiophene] (PBTTT), polyaniline (PANI), tetrathiafulvalene (TTF), and benzodifurandione paraphenylene vinylidene (BDPPV). These organic materials can provide a flexible film-like thermoelectric material.

[0031] In this case, the powder content is not particularly limited as long as a film can be formed, but the powder may be preferably contained in the range of 4% by mass to 80% by mass, preferably 4% by mass to 50% by mass, more preferably 4% by mass to 10% by mass, and even more preferably 4% by mass to 7% by mass, based on the organic material. This allows the film to have flexibility and thermoelectric performance.

[0032] In the embodiment of the present invention, the thermoelectric material has improved electrical conductivity, particularly at room temperature, and effectively reduced thermal conductivity, improving the figure of merit. 3 Sb 2 The inherent excellent figure of merit of the materials was not compromised.

[0033] Next, an exemplary method for producing a thermoelectric material in accordance with such an embodiment of the present invention will be described. FIG. 1A is a flow chart illustrating a process for producing a thermoelectric material in accordance with an embodiment of the present invention.

[0034] Step S110: A raw material containing magnesium (Mg), a raw material containing antimony (Sb) and / or a raw material containing bismuth (Bi), a raw material containing copper (Cu), and, as necessary, a raw material containing M (wherein M is at least one element selected from the group consisting of selenium (Se) and tellurium (Te)) are mixed to prepare a mixture. Step S120: The mixture obtained in step S110 is fired.

[0035] In an embodiment of the present invention, the thermoelectric material is obtained by the above steps S110 and S120. Each step will be described in detail.

[0036] In step S110, the raw material containing Mg may be Mg metal alone, or may be a silicide, oxide, carbonate, nitride, oxynitride, chloride, fluoride, or oxyfluoride of Mg. The raw material containing Sb may be Sb metal alone, or may be a silicide, oxide, carbonate, nitride, oxynitride, chloride, fluoride, or oxyfluoride of Sb. The raw material containing Bi may be Bi metal alone, or may be a silicide, oxide, carbonate, nitride, oxynitride, chloride, fluoride, or oxyfluoride of Bi. The raw material containing Cu may be Cu metal alone, or may be a silicide, oxide, carbonate, nitride, oxynitride, chloride, fluoride, or oxyfluoride of Cu. The raw material containing M may be M metal alone, or may be a silicide, oxide, carbonate, nitride, oxynitride, chloride, fluoride, or oxyfluoride of M. From the viewpoint of mixability and handling, the raw materials are preferably in the form of powder, granules or small lumps.

[0037] In step S110, the metal element in the raw material is selected from the group consisting of Mg a Sb 2-b-c Bi b M c Cu d where the parameters a, b, c, and d are 3≦a≦3.5, 0≦b≦2, 0≦c≦0.06, 0 <d≦0.1、および、 b+c≦2 The preferable parameters are as described above, and therefore the description will be omitted.

[0038] In step S120, sintering may be performed by any method such as spark plasma sintering (SPS), hot press sintering (HP), hot isostatic pressing (HIP), cold isostatic pressing (CIP), or Paltz current sintering, but is preferably performed by spark plasma sintering (SPS). This makes it possible to obtain a sintered body with suppressed grain growth in a short time without using a sintering aid.

[0039] SPS may be preferably performed at a temperature in the range of 723 K to 1173 K, under a pressure of 30 MPa to 100 MPa, for a time period of 1 minute to 10 minutes. In an embodiment of the present invention, under these conditions, the above-mentioned sintered thermoelectric material can be obtained with good yield.

[0040] Furthermore, the obtained sintered body may be pulverized by mechanical milling such as a ball mill, thereby obtaining a powdered thermoelectric material in the embodiment of the present invention.

[0041] In the embodiment of the present invention, the thus obtained powdered thermoelectric material can be mixed with an organic material to provide a flexible thermoelectric material. In this case, the organic material and the mixing ratio described above can be used.

[0042] Alternatively, the resulting sintered body may be used as a target to carry out physical vapor deposition, thereby providing a thin film of a thermoelectric material in an embodiment of the present invention.

[0043] (Embodiment 2) In the second embodiment, a thermoelectric generating element using the thermoelectric material explained in the first embodiment will be explained in an example of the present invention.

[0044] FIG. 2A is a schematic diagram showing a thermoelectric generating element (π-shaped) using a thermoelectric material in an embodiment of the present invention.

[0045] In an embodiment of the present invention, the thermoelectric generating element 200 includes a pair of n-type and p-type thermoelectric materials 210 and 220, and electrodes 230, 240 at their respective ends. The electrodes 230, 240 electrically connect the n-type and p-type thermoelectric materials 210 and 220 in series.

[0046] Here, the p-type thermoelectric material 210 is not particularly limited, but it is preferable that the material has high thermoelectric performance (for example, ZT is 0.4 to 1.6) at 500 K or less, particularly at room temperature. Illustrative p-type thermoelectric materials 210 include BiSbTe-based, MgAgSb-based, and AgSbSe-based materials. An exemplary composition of the BiSbTe-based material is, for example, Bi 0.5 Sb 1.5 Te 3 , Bi 0.4 Sb 1.6 Te 3 Exemplary compositions of the MgAgSb system include, for example, MgAgSb, MgAg 0.965 Ni 0.005 Sb 0.99 An exemplary composition of the AgSbSe system is, for example, AgSbSe 2 Please note that these are examples and are not limiting.

[0047] On the other hand, in the embodiment of the present invention, the n-type thermoelectric material 220 is the thermoelectric material described in embodiment 1. In the embodiment of the present invention, the thermoelectric material exhibits excellent thermoelectric properties, particularly at room temperature, and is therefore advantageous for waste heat recovery.

[0048] The electrodes 230, 240 can be any conventional electrode material, illustratively Fe, Ag, Al, Ni, Cu, or the like.

[0049] 2A shows a state in which a chip made of n-type thermoelectric material 210 is joined by solder or the like to an electrode 240 on the low-temperature side, and an opposite end of the chip of n-type thermoelectric material 210 is joined by solder or the like to an electrode 230 on the high-temperature side. Similarly, a chip made of p-type thermoelectric material 220 is joined by solder or the like to an electrode 230 on the high-temperature side, and an opposite end of the chip of p-type thermoelectric material 220 is joined by solder or the like to an electrode 240 on the low-temperature side.

[0050] In an embodiment of the present invention, when the thermoelectric generating element 200 is placed in an environment where the electrode 230 is at a high temperature and the electrode 240 is at a low temperature compared to the electrode 230, and the end electrodes are connected to an electric circuit or the like, a voltage is generated by the Seebeck effect, and a current flows in the order of the electrode 240, the n-type thermoelectric material 210, the electrode 230, and the p-type thermoelectric material 220, as shown by the arrows in Fig. 2A. In detail, the electrons in the n-type thermoelectric material 210 obtain thermal energy from the electrode 230 on the high temperature side, move to the electrode 240 on the low temperature side, and release the thermal energy there, and in response, the holes in the p-type thermoelectric material 220 obtain thermal energy from the electrode 230 on the high temperature side, move to the electrode 240 on the low temperature side, and release the thermal energy there. This is the principle by which a current flows.

[0051] In the embodiment of the present invention, the thermoelectric material described in the first embodiment is used as the n-type thermoelectric material 210, so that the thermoelectric generating element 200 that generates a large amount of electricity, especially at room temperature (275 K or more and 320 K or less), can be realized. 3 Sb 2 In the case where a powder made of an inorganic compound to which Cu atoms are added using a system as a parent phase, a film containing the powder, or a thin film obtained by using a sintered body made of the above-mentioned inorganic compound as a target as a thermoelectric material in the embodiment of the present invention, a flexible thermoelectric power generation module can be provided as an IoT power source. For example, FIG. 2C illustrates a state in which a sintered body made of the inorganic compound is used as a target 300, and particles 330 made of the inorganic compound are sputtered by argon 320 onto a substrate 310 to form a thin film 340. It goes without saying that this thin film 340 is peeled off from the substrate 310 by existing technology and formed into a single film. For example, FIG. 2D illustrates powder 350 made of the inorganic compound. If this powder 350 is compressed by a powder compression machine 370, a compact 360 is obtained, and if the compact 380 is placed in a sintering furnace 390 and sintered, a sintered body 400 is obtained.

[0052] In the embodiment of the present invention, if a thermoelectric material is used, a thermoelectric generating element 200 that generates a large amount of electricity at room temperature can be provided, but in the embodiment of the present invention, the thermoelectric generating element 200 is not limited to use in a temperature range higher than room temperature (for example, 573 K, etc.). Since the thermoelectric generating element 200 exhibits a high dimensionless figure of merit (ZT) even in a high temperature range, it goes without saying that a thermoelectric generating element that generates a large amount of electricity can be provided.

[0053] 2A has been described using a π-type thermoelectric generating element, but in an embodiment of the present invention, the thermoelectric material may be used in a U-shaped thermoelectric generating element (FIG. 2B). In this case, in an embodiment of the present invention, n-type thermoelectric material 210 and p-type thermoelectric material 220 made of thermoelectric materials are directly connected at junction 215 on the high temperature side. Low temperature side electrodes 240a and 240b may be electrically connected to low temperature side electrodes of separate U-shaped thermoelectric generating elements.

[0054] The present invention will now be described in detail with reference to specific examples, but it should be noted that the present invention is not limited to these examples. EXAMPLES

[0055] [Raw materials] In the following examples, Mg (powder, purity 99.99%, manufactured by Sigma-Aldrich Japan LLC), Sb (powder, purity 99.99%, manufactured by Sigma-Aldrich Japan LLC), Bi (powder, purity 99.99%, manufactured by Sigma-Aldrich Japan LLC), Te (powder, purity 99.99%, manufactured by Sigma-Aldrich Japan LLC), and Cu (powder, purity 99.99%, manufactured by Sigma-Aldrich Japan LLC) were used as necessary.

[0056] [Example 1 to Example 10] In Examples 1 to 5, the general formula Mg 3.2 Sb 1.5 Bi 0.49 Te 0.01 Cu d The raw materials were mixed so as to satisfy the following formula (d=0, 0.005, 0.01, 0.025, 0.05) to produce thermoelectric materials. 3.2 Sb0.5 Bi 1.498 Te 0.002 Cu 0.01 In Examples 8 to 10, the raw materials were mixed so as to satisfy the general formula Mg 3.2 Sb 0.5 Bi 1.495 Te 0.005 Cu 0.01 The raw materials were mixed so as to satisfy the above requirements, and a thermoelectric material was produced.

[0057] Each raw material powder was weighed to satisfy the composition in Table 1, filled into a stainless steel ball mill container in a glove box, and mixed with a ball mill for 5 hours. Then, it was sintered at 973K for 5 minutes in a spark plasma sintering apparatus (SPS, manufactured by SPS Syntex, Inc., SPS-1080 system). In detail, the mixture was filled into a graphite sintering die (inner diameter 10 mm, height 30 mm), and held at a sintering temperature of 973K for 5 minutes under a uniaxial stress of 60 MPa at a heating rate of 100K / min. In this way, a sintered body was obtained. The samples of Examples 1 to 5 satisfied the compositions of d=0.005, d=0.01, d=0.025, d=0.05, and d=0, respectively, and the samples of Examples 6 to 10 satisfied the compositions as described above.

[0058] The sintered bodies were observed. In addition, the surfaces were observed using a scanning electron microscope (SEM, JEOL Ltd., JSM-7800F) equipped with an electron backscatter diffraction detector (EBSD) and an energy dispersive X-ray spectrometer (EDS) to determine the average grain size. The average grain size was calculated using the image analysis software described above. These results are shown in Figures 3 to 6 and Table 2.

[0059] The obtained sintered body was wet-pulverized using ethanol in an agate mortar. The particles of the sintered body after pulverization were sieved through a mesh (45 μm mesh size), and only particles with a particle size of 45 μm or less that passed through the mesh were taken out. The particles were identified by powder X-ray diffraction (Rigaku Corporation, SmartLab3), and composition analysis was performed by fluorescent X-ray analysis (Horiba, Ltd., EMAX Evolution EX). The results of X-ray diffraction are shown in Figures 7 and 8.

[0060] The sintered body was processed into a rectangular parallelepiped of 1.5 mm × 1.5 mm × 9 mm by a high-speed cutter, and the electrical conductivity and thermoelectric property measurements were performed. The electrical conductivity was measured by a direct current four-terminal method. The Seebeck coefficient and thermal conductivity as thermoelectric properties were measured by a steady-state temperature difference method using a thermoelectric property measurement evaluation device (ZEM-3, manufactured by Advance Riko Co., Ltd.) and a thermal conductivity evaluation device (HyperflashXXX, manufactured by Netsch Co., Ltd.), respectively. The measurement conditions were a helium gas atmosphere, and the measurements were performed in a temperature range from room temperature to 800 K. The electrical output factor (power factor) was calculated from the thermoelectromotive force obtained from the electrical conductivity or electrical resistivity and the Seebeck coefficient, and the dimensionless figure of merit ZT was calculated from the Seebeck coefficient, electrical conductivity, and thermal conductivity. These results are shown in Figures 9 to 15 and Table 3, and will be described later.

[0061] For simplicity, the manufacturing conditions of the samples of Examples 1 to 10 are summarized in Table 1. All of the samples of Examples 1 to 10 were sintered at a stress of 60 MPa. Examples 1 to 5 were sintered at a sintering temperature of 973 K (700°C) for 5 minutes. Examples 6 and 8 were sintered at a sintering temperature of 973 K (700°C) for 10 minutes, Examples 7 and 9 were sintered at a sintering temperature of 1023 K (750°C) for 10 minutes, and Example 10 was sintered at a sintering temperature of 1073 K (800°C) for 10 minutes. The results are explained below.

[0062] [Table 1]

[0063] FIG. 3 is a diagram showing the appearance of the sample of Example 1.

[0064] As shown in Figure 3, the sample of Example 1 was a disk-shaped sintered body with a diameter of 10 mm and a thickness of 2 mm. Although not shown, the other samples had the same morphology.

[0065] FIG. 4 shows SEM images and EDS mapping of the samples of Examples 1 to 5.

[0066] Figures 4(A)-(E) show SEM images of the samples of Example 5, Example 1-Example 4, respectively, and Figure 4(F) shows EDS mapping of the sample of Example 2. Figures 4(A)-(E) show that the addition of Cu caused clear grain growth, and as the amount of Cu added increased, the grain size also increased. Figure 4(F) shows the results in gray scale, and it was confirmed that Mg, Bi, and Sb were uniformly located throughout the sample.

[0067] FIG. 5 shows an EBSD image of the sample of Example 2. FIG. 6 is a diagram showing an EBSD image of the sample of Example 5.

[0068] Figures 5 and 6 show grain mapping and grain size histograms along with inverse pole point (IPF) maps. According to Figures 5 and 6, the average grain size of the sample of Example 5, which did not contain Cu, was 3.24 μm, while that of the sample of Example 2, which contained Cu, was 4.57 μm. The EBSD and SEM images suggest that the samples of Examples 1, 3, and 4, which contained Cu, were composed of inorganic compounds having an average grain size of 4 μm or more and 6 μm or less. It was also found that the average grain size increased by 40% or more by adding Cu. Furthermore, the average grain size tended to increase as the amount of Cu added increased.

[0069] FIG. 7 is a diagram showing XRD patterns of the samples of Examples 1 to 5. FIG. 8 is a diagram showing the Cu addition amount dependence of the lattice constants of the samples of Examples 1 to 5. In FIG.

[0070] According to FIG. 7, the diffraction peaks in the XRD patterns of the samples of Examples 1 to 5 are all Mg 2 Sb 3 The samples of Examples 1 to 5 correspond to those of the La phase. 2 O 3It was found that the compound has a symmetric structure and a P-3m1 space group. The composition analysis confirmed that the composition of each sample was consistent with the composition of the starting material. According to Figure 8, the a-axis and c-axis both increased with the addition of Cu. In general, the atomic diameter of Cu is not large compared to that of Mg and Sb. Therefore, it was shown that Cu is an interstitial solid solution, not a substitutional solid solution.

[0071] Therefore, the samples of Examples 1 to 4 are La containing Mg, Sb, Bi and Te. 2 O 3 It was shown that the parent crystal has a crystalline structure and contains an inorganic compound to which Cu has been added.

[0072] [Table 2]

[0073] Fig. 9 is a graph showing the temperature dependence of the electrical conductivity of the samples of Examples 1 to 5. Fig. 16 is a graph showing the temperature dependence of the electrical conductivity of the samples of Examples 6 to 7, and Fig. 22 is a graph showing the temperature dependence of the electrical conductivity of the samples of Examples 8 to 10.

[0074] According to FIG. 9, the electrical conductivity of the samples of Examples 1 to 4, in which Cu was added, was higher than that of the sample of Example 5, in which Cu was not added, and was particularly remarkably increased near room temperature. The samples of Examples 1 to 4 had electrical conductivity (electrical resistivity) that was usable as a thermoelectric material, and had temperature dependence. In addition, when focusing on electrical conductivity at room temperature, it was found that the electrical conductivity at room temperature could be increased to about 5×10 by controlling the amount of Cu added. 4 (Ωm) -1 16 to 27, the sintering temperature is shown in Celsius, with 700 in Figs. 16 to 21 being Example 6 and 750 being Example 7, and 700 in Figs. 22 to 27 being Example 8, 750 being Example 9, and 800 being Example 10. According to Fig. 16, the higher the sintering temperature, the higher the electrical conductivity, and similarly according to Fig. 22, the higher the sintering temperature, the higher the electrical conductivity.

[0075] FIG. 10 is a diagram showing the Cu additive amount dependence of carrier concentration and mobility of the samples of Examples 1 to 5. In FIG.

[0076] According to FIG. 10, as the amount of Cu added increases, the carrier concentration and mobility also tend to increase. In particular, when we look at the mobility, the addition of Cu increases the carrier concentration from 100 cm 2 V -1 s -1 This is believed to be due to the advantageous carrier scattering mechanism caused by the interstitial solid solution of Cu.

[0077] 11, 17, and 23 are diagrams showing the temperature dependence of the Seebeck coefficient of the samples of Examples 1 to 5, Examples 6 to 7, and Examples 8 to 10. In FIG.

[0078] According to FIG. 11, it was confirmed that all the samples had n-type conductivity with a large Seebeck coefficient of 170 μV / K or more. Surprisingly, the addition of Cu did not impair the magnitude of the Seebeck coefficient, even though the electrical conductivity was improved. According to FIG. 17, it was confirmed that all the samples had n-type conductivity with a large Seebeck coefficient of 220 μV / K or more. According to FIG. 23, it was confirmed that all the samples had n-type conductivity with a large Seebeck coefficient of 160 μV / K or more.

[0079] Fig. 12 is a graph showing the temperature dependence of the electric output factor of the samples of Examples 1 to 5. Fig. 18 is a graph showing the temperature dependence of the electric output factor of the samples of Examples 6 to 7. Fig. 24 is a graph showing the temperature dependence of the electric output factor of the samples of Examples 8 to 10.

[0080] According to FIG. 12, it was found that the electric power factor of the samples of Example 1 to Example 4, in which Cu was added, was dramatically increased in the low temperature range of 300 K to 400 K compared to that of the sample of Example 5, in which Cu was not added. For example, the electric power factor of the sample of Example 2 at room temperature (300 K) (21.03 μW cm -1 K -2) and that of the sample of Example 5 (7.16 μW cm -1 K -2 ), the increase was about three times. This means that the thermoelectric power generation element is suitable for various thermoelectric cooling applications and for recovering waste heat as a power source for IoT operation, and can provide a thermoelectric power generation element for consumer use. According to Fig. 18 and Fig. 24, the same results as those of Examples 1 to 4 were obtained.

[0081] Fig. 13 is a graph showing the temperature dependence of the total thermal conductivity of samples of Examples 1 to 5. Fig. 19 is a graph showing the temperature dependence of the total thermal conductivity of samples of Examples 6 to 7. Fig. 25 is a graph showing the temperature dependence of the total thermal conductivity of samples of Examples 8 to 10. Fig. 14 is a graph showing the temperature dependence of the lattice thermal conductivity of samples of Examples 1 to 5. Fig. 20 is a graph showing the temperature dependence of the lattice thermal conductivity of samples of Examples 6 to 7. Fig. 26 is a graph showing the temperature dependence of the lattice thermal conductivity of samples of Examples 8 to 10.

[0082] According to FIG. 13, the total thermal conductivity was slightly decreased by adding Cu. The Lorentz number L was calculated, and the electronic thermal conductivity was subtracted from the total thermal conductivity to obtain the lattice thermal conductivity. As shown in FIG. 14, in the relatively low temperature range below 400K, the lattice thermal conductivity of the samples of Example 1 to Example 4 in which Cu was added was significantly lower than that of the sample of Example 5 in which Cu was not added. For example, when comparing the lattice thermal conductivity of the sample of Example 2 with that of the sample of Example 5 in the entire temperature range measured, the lattice thermal conductivity of the sample of Example 2 was reduced by 20 to 30%. According to FIG. 19 and FIG. 25 and FIG. 20 and FIG. 26, the same results as those of Examples 1 to 4 were obtained.

[0083] Fig. 15 is a graph showing the temperature dependence of the dimensionless figure of merit ZT of the samples of Examples 1 to 5. Fig. 21 is a graph showing the temperature dependence of the dimensionless figure of merit ZT of the samples of Examples 6 to 7. Fig. 27 is a graph showing the temperature dependence of the dimensionless figure of merit ZT of the samples of Examples 8 to 10.

[0084] According to FIG. 15, it was found that the ZT of the samples of Example 1 to Example 4, in which Cu was added, was higher than that of the sample of Example 5, in which Cu was not added. In particular, this tendency was remarkable in the relatively low temperature range of 400 K or less for the samples of Example 1 to Example 4, in which Cu was added, and it was found that a high value of 0.4 or more was achieved at room temperature. In the high temperature range exceeding 400 K, the addition of Cu did not reduce the ZT of Mg 3 Sb 2 It was confirmed that the original ZT was substantially maintained. According to Fig. 21 and Fig. 27, the same results as in Examples 1 to 4 were obtained.

[0085] The above thermoelectric properties are summarized in Table 3. In Table 3, "E" represents a power of 10.

[0086] [Table 3]

[0087] According to Table 3, it was found that the samples of Example 1 to Example 4 to which Cu was added had a large electrical conductivity at room temperature and the figure of merit was improved. It was also shown that the amount of Cu added (d value) is preferably in the range of 0.005≦d≦0.05, and in particular, 0.005≦d≦0.025. It was also shown that the power factor at room temperature formed by the Seebeck coefficient and electrical conductivity in Examples 6 to 10 was larger and enhanced than in Examples 1 to 5. This is because in Examples 6 to 10, the composition ratio of Bi was made larger than that of Sb (see Table 1), so that the band gap became smaller and a particularly high electrical conductivity was obtained without significantly impairing the Seebeck coefficient at room temperature. In addition, although the total thermal conductivity was high, the lattice thermal conductivity was relatively low. It is generally said that there are two types of thermal conduction: thermal conduction due to the movement of heat accompanying the movement of charged particles such as electrons, and thermal conduction due to the transmission of lattice vibrations without the movement of such particles. It is said that in a thermoelectric element that generates a voltage based on a temperature difference, it is preferable that the thermal conductivity is low and the electrical conductivity is high. That is, it is considered that such a preferable state was obtained in Examples 6 to 10. For example, in consideration of the power factor, it is preferable to increase the composition ratio of Bi to Sb, and b>1 is more preferable, b≧1.2 is even more preferable, and b≧1.4 is even more preferable. [Industrial Applicability]

[0088] In the embodiment of the present invention, the thermoelectric material has excellent thermoelectric performance, particularly at around room temperature, and is made of Bi. 2 Te 3 It can function as an alternative material to the thermoelectric system and can be used in thermoelectric cooling devices and power generation devices used in various electrical devices. In particular, if it can be made into a thin film, it can provide a flexible thermoelectric generation element as a power source for IoT. [Explanation of symbols]

[0089] 200 Thermoelectric generation element 210 n-type thermoelectric materials 220 p type thermoelectric material 230, 240 electrode

Claims

1. an inorganic compound containing magnesium (Mg), antimony (Sb), bismuth (Bi), copper (Cu), and tellurium (Te); The inorganic compound is Mg a Sb 2-b-c Bi b Te c Cu d It is expressed as The parameters a, b, c and d are 3≦a≦3.5, 0.2≦b≦2, 0.002≦c≦0.06, 0.001<d≦0.1, and b + c≦2 Fulfilling The inorganic compound is La 2 O 3 It has a structure of the type 1 and has the symmetry of the space group P-3m1, Cu is the above-mentioned La 2 O 3 A thermoelectric material that is an n-type interstitial solid solution in the n-type structure.

2. The parameter d is 0.005≦d≦0.05 The thermoelectric material according to claim 1 ,

3. The parameters a, b, c and d are 3≦a≦3.5, 0.2≦b≦0.7, 0.002≦c≦0.06, and 0.005≦d≦0.05 The thermoelectric material according to claim 1 or 2, which satisfies the above.

4. The thermoelectric material according to any one of claims 1 to 3, wherein the thermoelectric material is in a form selected from the group consisting of a powder, a sintered body, and a thin film.

5. the thermoelectric material is in the form of a powder or a sintered body; The thermoelectric material according to claim 4 , wherein the inorganic compound is composed of crystal grains having an average grain size in the range of 3.5 μm to 30 μm.

6. The thermoelectric material according to claim 5 , wherein the inorganic compound is composed of crystal grains having an average grain size in the range of 4 μm to 20 μm.

7. the thermoelectric material is in the form of a thin film; The inorganic compound is composed of crystal grains having an average grain size in the range of 3.5 μm to 30 μm, The thermoelectric material of claim 4 further comprising an organic material.

8. mixing a raw material containing magnesium (Mg), a raw material containing antimony (Sb) and / or a raw material containing bismuth (Bi), a raw material containing copper (Cu), and a raw material containing tellurium (Te) to prepare a mixture; sintering the mixture; and A method for producing the thermoelectric material according to any one of claims 1 to 7, comprising:

9. The method of claim 8 , wherein the sintering comprises spark plasma sintering.

10. The method according to claim 9, wherein the spark plasma sintering is performed at a temperature range of 723 K to 1173 K, under a pressure of 30 MPa to 100 MPa, for a time period of 1 minute to 10 minutes.

11. The method according to any one of claims 8 to 10, further comprising pulverizing the sintered body obtained by sintering.

12. The method of claim 11, further comprising mixing the powder obtained by grinding with an organic material.

13. The method according to any one of claims 8 to 10, further comprising carrying out a physical vapor deposition method using the sintered body obtained by sintering as a target.

14. A thermoelectric power generation element comprising a p-type thermoelectric material and an n-type thermoelectric material alternately connected in series, the n-type thermoelectric material being the thermoelectric material according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Waste heat recovery system having thermoelectric conversion system

    JP2009087955A

  • Thermoelectric material system

    US6225550B1

  • Thermoelectric material, thermoelectric conversion module using thermoelectric material, method for manufacturing same, and peltier element

    WO2019017170A1

  • Thermoelectric conversion element and thermoelectric conversion module

    WO2020003554A1

  • Magnesium-antimony-based thermoelectric element, preparation method therefor, and application thereof

    WO2020168531A1