Aqueous coating varnish and printed material

The aqueous coating varnish with zinc oxide and acrylic resin particles addresses the issue of insufficient water and alcohol abrasion resistance, achieving enhanced film-forming properties and abrasion resistance.

JP2024150990APending Publication Date: 2024-10-24SAKATA INX
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023064084
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing water-based coating varnishes lack sufficient water and alcohol abrasion resistance.

Method used

An aqueous coating varnish containing a zinc oxide crosslinking agent and acrylic resin particles with a specific glass transition temperature, along with optional wax and phosphoric acid ester, to enhance film-forming properties and abrasion resistance.

Benefits of technology

The varnish exhibits excellent water and alcohol abrasion resistance, with improved film-forming properties and blocking resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150990000001
    Figure 2024150990000001
Patent Text Reader

Abstract

To provide an aqueous coating varnish with superior water abrasion resistance and alcohol abrasion resistance.SOLUTION: An aqueous coating varnish contains a zinc oxide-based crosslinker and acrylic resin particles, where the acrylic resin particles have a glass transition temperature of -5°C or more and 30°C or less, and the zinc oxide-based crosslinker constitutes 0.05 mass% or more and 0.5 mass% or less of the aqueous coating varnish.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-based coating varnish and a printed matter. [Background technology]

[0002] An aqueous coating varnish that has excellent blocking resistance and abrasion resistance and is used for carton paper containers, wrapping paper, etc. is known (Patent Document 1). This aqueous coating varnish contains a specific amount of a zinc oxide-based crosslinking agent, specific amounts of polyolefin resin particles, and styrene or acrylic resin particles. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2022-116795 A Summary of the Invention [Problem to be solved by the invention]

[0004] On the other hand, there is a strong demand for water-based coating varnishes that are excellent in water- and alcohol-based abrasion resistance, but the water-based coating varnish specifically disclosed in Patent Document 1 is insufficient in these respects.

[0005] Therefore, the present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an aqueous coating varnish that has excellent water abrasion resistance and alcohol abrasion resistance.

[0006] Another object of the present invention is to provide a printed matter obtained by printing the above-mentioned aqueous coating varnish. [Means for solving the problem]

[0007] That is, the present invention relates to an aqueous coating varnish containing a zinc oxide-based crosslinking agent and acrylic resin particles, wherein the acrylic resin particles have a glass transition temperature of -5°C or more and 30°C or less, and the zinc oxide-based crosslinking agent is present in an amount of 0.05% by mass or more and 0.5% by mass or less in the aqueous coating varnish.

[0008] The aqueous coating varnish of the present invention preferably contains wax particles.

[0009] In the aqueous coating varnish of the present invention, the acrylic resin particles preferably account for 20% by mass or more and 40% by mass or less in the aqueous coating varnish.

[0010] The present invention also relates to a printed matter obtained by printing the above-mentioned aqueous coating varnish. Effect of the Invention

[0011] The aqueous coating varnish of the present invention contains a zinc oxide-based crosslinking agent and acrylic resin particles, the acrylic resin particles having a glass transition temperature of -5°C or more and 30°C or less, and the zinc oxide-based crosslinking agent is present in an amount of 0.05% by mass or more and 0.5% by mass or less in the aqueous coating varnish. The aqueous coating varnish of the present invention has excellent film-forming properties because the acrylic resin particles have a glass transition temperature of -5°C or more and 30°C or less, and also has excellent water abrasion resistance and alcohol abrasion resistance because it contains a specific amount of zinc oxide-based crosslinking agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <Water-based coating varnish> The aqueous coating varnish of the present invention contains a zinc oxide-based crosslinking agent and acrylic resin particles, the acrylic resin particles having a glass transition temperature of -5°C or more and 30°C or less, and the zinc oxide-based crosslinking agent is present in an amount of 0.05% by mass or more and 0.5% by mass or less in the aqueous coating varnish.

[0013] <Zinc oxide-based crosslinking agent> The zinc oxide crosslinking agent is a crosslinking agent that reacts with an acid such as a carboxylic acid. The zinc oxide crosslinking agent is preferably used in a state of being dissolved in a basic aqueous solution, and can be used in the form of an aqueous solution in which a complex is formed using, for example, aqueous ammonia. The zinc oxide crosslinking agents can be used alone or in combination of two or more kinds.

[0014] The zinc oxide-based crosslinking agent is present in the aqueous coating varnish at a content of 0.05% by mass or more and 0.5% by mass or less. From the viewpoint of improving alcohol abrasion resistance, the zinc oxide-based crosslinking agent is preferably present in the aqueous coating varnish at a content of 0.1% by mass or more, and from the viewpoint of improving water abrasion resistance, the zinc oxide-based crosslinking agent is preferably present in the aqueous coating varnish at a content of 0.45% by mass or less.

[0015] <Acrylic resin particles> The acrylic resin particles are particles in which an acrylic resin is dispersed in water, and the glass transition temperature of the resin is −5° C. or more and 30° C. or less. Examples of the acrylic resin particles include acrylic resin particles (made only of acrylic monomers), as well as styrene-acrylic resin particles containing a styrene monomer component, acrylic-maleic acid resin particles containing a maleic acid monomer component, and styrene-acrylic-maleic acid resin particles containing a styrene monomer component and a maleic acid monomer component. The acrylic resin particles can be used alone or in combination of two or more kinds.

[0016] From the viewpoint of improving water abrasion resistance and alcohol abrasion resistance, the acrylic resin particles preferably have a glass transition temperature of 0° C. or higher, and from the viewpoint of improving water abrasion resistance and alcohol abrasion resistance, the glass transition temperature is preferably 20° C. or lower, and more preferably 15° C. or lower. Regarding the glass transition temperature, the values ​​in the manufacturer's catalogue can be used as a reference, but in the case of acrylic resins, the theoretical glass transition temperature calculated by the following Wood's formula can be used. Wood's formula: 1 / Tg=W1 / Tg1+W2 / Tg2+W3 / Tg3+····+Wx / Tgx [In the formula, Tg1 to Tgx represent the glass transition temperatures of the respective homopolymers of monomers 1, 2, 3...x constituting the resin, W1 to Wx represent the respective polymerization fractions of monomers 1, 2, 3...x, and Tg represents the theoretical glass transition temperature. However, the glass transition temperature in Wood's formula is an absolute temperature.]

[0017] From the viewpoint of efficient crosslinking with a zinc oxide-based crosslinking agent, the acrylic resin particles preferably contain a carboxyl group, and the acid value is preferably 30 mgKOH / g or more and 90 mgKOH / g or less, and more preferably 40 mgKOH / g or more and 80 mgKOH / g or less.

[0018] The acrylic resin particles are contained in the aqueous coating varnish at a content of preferably 20% by mass or more and 40% by mass or less, more preferably 25% by mass or more and 40% by mass or less, and even more preferably 30% by mass or more and 40% by mass or less, from the viewpoint of improving alcohol abrasion resistance in the aqueous coating varnish.

[0019] The aqueous coating varnish preferably contains wax particles from the viewpoint of improving water resistance, abrasion resistance and alcohol resistance. Examples of the wax particles include polyolefins such as polyethylene, polyethylene oxide, polypropylene, and polypropylene oxide, which are simply dispersed in water together with a surfactant or other emulsions, or which are made into emulsion dispersions. The wax particles can be used alone or in combination of two or more kinds. The wax particles are preferably 0.1% by mass or more and 2.0% by mass or less, more preferably 0.3% by mass or more and 1.5% by mass or less in the aqueous coating varnish.

[0020] The aqueous coating varnish may contain a phosphate ester from the viewpoint of imparting blocking resistance, and the content of the phosphate ester in the aqueous coating varnish is preferably 0.1% by mass or more and 1.5% by mass or less, and more preferably 0.3% by mass or more and 1.2% by mass or less.

[0021] The water content of the aqueous coating varnish is preferably 60% by mass or more and 75% by mass or less, and more preferably 60% by mass or more and 70% by mass or less.

[0022] The aqueous coating varnish may further contain additives such as a leveling agent, a surfactant, a thickener, an antioxidant, and a defoamer, if necessary.

[0023] The total amount of the zinc oxide crosslinking agent, acrylic resin particles, and water in the aqueous coating varnish is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When wax particles or a phosphate ester is used, the total amount of the zinc oxide crosslinking agent, acrylic resin particles, wax particles, phosphate ester, and water in the aqueous coating varnish is preferably 75% by mass or more, more preferably 85% by mass or more, and even more preferably 95% by mass or more.

[0024] <Preparation method of water-based coating varnish> The method for preparing the aqueous coating varnish is not particularly limited, and for example, the above-mentioned components may be added in order or simultaneously, and the aqueous coating varnish may be prepared using a roll mill, kneader, high-speed mixer, bead mill, ball mill, sand mill, ultrasonic disperser, high-pressure disperser, or the like.

[0025] The aqueous coating varnish can be applied to a recording medium by, for example, offset inline coating printing or flexographic printing to produce a printed matter. In addition, as the recording medium, a recording medium having a coating layer such as coated paper or coated board can be suitably used. In addition, the aqueous coating varnish can be applied to a recording medium on which characters or images are printed. EXAMPLES

[0026] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0027] <Examples 1-7, Comparative Examples 1-7> <Preparation of Water-Based Coating Varnish> Each water-based coating varnish was prepared by mixing the materials according to the composition shown in Table 1. The values ​​shown in each table are the parts by mass of the active ingredient.

[0028] The following evaluations were carried out using each of the aqueous coating varnishes obtained above. The results are shown in Table 1.

[0029] <Water and abrasion resistance> Sakata Inks' Ecoplata indigo ink was applied to bleached kraft paper (OK bleached kraft paper, Oji Paper Co., Ltd.) using a 200-line hand proofer, and the water-based coating varnishes of the Examples and Comparative Examples were applied on top of it using a 200-line hand proofer, and the applied surface was dried with a dryer. Evaluation was performed under the following conditions using a Gakushin-type rub fastness tester (Toyo Seiki Seisakusho Co., Ltd.). A or B is acceptable, and A is preferable. Evaluation conditions: 200g x 2 times, paper: 5 drops of water on Kanakin cloth A: The ink adhesion area on the paper is less than 10%. B: The area of ​​ink adhering to the paper is 10% or more but less than 20%. C: The area of ​​ink adhering to the paper is 20% or more but less than 50%. D: The ink adhesion area on the paper is 50% or more.

[0030] <Abrasion resistance to ethanol (concentration 80%)> Sakata Inks' Ecoplata indigo ink was applied to bleached kraft paper (OK bleached kraft paper, Oji Paper Co., Ltd.) using a 200-line hand proofer, and the water-based coating varnishes of the Examples and Comparative Examples were applied on top of it using a 200-line hand proofer, and the applied surface was dried with a dryer. Evaluation was performed under the following conditions using a Gakushin-type rub fastness tester (Toyo Seiki Seisakusho Co., Ltd.). A or B is acceptable, and A is preferable. Evaluation conditions: 200g x 2 times, paper: 5 drops of 80% ethanol solution on Kanakin cloth A: The ink adhesion area on the paper is less than 20%. B: The area of ​​ink adhering to the paper is 20% or more but less than 40%. C: The ink adhesion area on the paper is 40% or more but less than 60%. D: The ink adhesion area on the paper is 60% or more.

[0031] <Abrasion resistance to ethanol (concentration 60%)> Sakata Inks' Ecoplata indigo ink was applied to bleached kraft paper (OK bleached kraft paper, Oji Paper Co., Ltd.) using a 200-line hand proofer, and the water-based coating varnishes of the Examples and Comparative Examples were applied on top of it using a 200-line hand proofer, and the applied surface was dried with a dryer. Evaluation was performed under the following conditions using a Gakushin-type rub fastness tester (Toyo Seiki Seisakusho Co., Ltd.). A or B is acceptable, and A is preferable. Evaluation conditions: 200g x 2 times, paper: 5 drops of 60% ethanol solution on Kanakin cloth A: The ink adhesion area on the paper is less than 10%. B: The area of ​​ink adhering to the paper is 10% or more but less than 30%. C: The ink adhesion area on the paper is 30% or more but less than 60%. D: The ink adhesion area on the paper is 60% or more.

[0032] <Abrasion resistance to ethanol (concentration 40%)> Sakata Inks' Ecoplata indigo ink was applied to bleached kraft paper (OK bleached kraft paper, Oji Paper Co., Ltd.) using a 200-line hand proofer, and the water-based coating varnishes of the Examples and Comparative Examples were applied on top of it using a 200-line hand proofer, and the applied surface was dried with a dryer. Evaluation was performed under the following conditions using a Gakushin-type rub fastness tester (Toyo Seiki Seisakusho Co., Ltd.). A or B is acceptable, and A is preferable. Evaluation conditions: 200g x 2 times, paper: 5 drops of 40% ethanol solution on Kanakin cloth A: The ink adhesion area on the paper is less than 10%. B: The area of ​​ink adhering to the paper is 10% or more but less than 20%. C: The area of ​​ink adhering to the paper is 20% or more but less than 50%. D: The ink adhesion area on the paper is 50% or more.

[0033] [Table 1]

[0034] In Table 1, Saibinol EK-55 (Tg = 3°C) is an acrylic resin particle (acid value: 58 mg KOH / g, manufactured by Saiden Chemical Industry Co., Ltd.); Joncryl PDX-7341 (Tg = 16°C) is an acrylic resin particle (acid value: 51 mg KOH / g, manufactured by BASF); Joncryl PDX-7677 (Tg = 32°C) is an acrylic resin particle (acid value: 70 mg KOH / g, manufactured by BASF); Joncryl PDX-7789 (Tg = 60°C) is an acrylic resin particle (acid value: 60 mg KOH / g, manufactured by BASF); Nipol SX1706A (Tg = -6°C) is an acrylic resin particle (acid value: 0 mg KOH / g, manufactured by Zeon Corporation); Zinc Oxide Solution #1 (zinc oxide) is a zinc oxide-based crosslinker (manufactured by BASF); Zircosol AC-7 ((NH4)2ZrO(CO3)2) is a zirconium-based cross-linking agent (manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.); Orgatix TC-300 (titanium lactate ammonium salt) is a titanium-based cross-linking agent (manufactured by Matsumoto Fine Chemical Co., Ltd.); SN Deformer 777 is a defoamer (manufactured by San Nopco); Chemipearl W400 is a water dispersion of polyolefin (Mitsui Chemicals); Surfynol 104DEG is a surfactant (manufactured by Nissin Chemical Industry Co., Ltd.); Plysurf DB-01 is a phosphate ester compound (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.);

Claims

1. An aqueous coating varnish containing a zinc oxide-based crosslinking agent and acrylic resin particles, The acrylic resin particles have a glass transition temperature of −5° C. or more and 30° C. or less, The aqueous coating varnish is characterized in that the zinc oxide-based crosslinking agent is contained in an amount of 0.05% by mass or more and 0.5% by mass or less in the aqueous coating varnish.

2. 2. The aqueous coating varnish according to claim 1, further comprising wax particles.

3. 3. The aqueous coating varnish according to claim 1, wherein the acrylic resin particles are contained in an amount of from 20% by mass to 40% by mass in the aqueous coating varnish.

4. A printed matter obtained by printing the aqueous coating varnish according to claim 1 or 2.

Citation Information

Patent Citations

  • Aqueous resin composition for moistureproof coating for paper

    JP1998292290A

  • Emulsion composition for drying by heating, coating for drying by heating and coating film

    JP2015196740A

  • Aqueous coating varnish and printed material

    JP2022116795A

  • Food packaging paper

    WO2013008938A1

  • Aqueous flexographic printing ink composition

    WO2019117231A1