Manufacturing method of three-dimensional object, and three-dimensional object
The method enhances the adhesion and smoothness of three-dimensional structures by applying a film before full curing, addressing the inefficiencies of traditional polishing and coating adhesion issues in stereolithography.
Patent Information
- Application Number
- JP2023064182
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Three-dimensional objects manufactured by stereolithography have minute step-like modeling marks on their surfaces, which require polishing to achieve smoothness, a process that is time-consuming and inefficient, and applying coatings without sufficient adhesion can lead to peeling issues.
A method involving stereolithography to form a three-dimensional object with an uncured portion, followed by applying a film using a photocurable composition containing the same photopolymerizable component, and then curing the film before fully curing the object, which enhances adhesion and smoothness.
The method results in a three-dimensional structure with excellent surface adhesion and smoothness, eliminating the need for polishing and improving production efficiency by ensuring the coating adheres well to the surface.
Smart Images

Figure 2024151061000003 
Figure 2024151061000004 
Figure 2024151061000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a three-dimensional object and a three-dimensional object. [Background technology]
[0002] 2. Description of the Related Art In recent years, methods of using three-dimensional objects formed by stereolithography using a 3D printer as dental products such as dental prostheses and mouthpieces have been considered (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 4160311 Summary of the Invention [Problem to be solved by the invention]
[0004] Due to the nature of the manufacturing process, three-dimensional objects formed by stereolithography have tiny step-like modeling marks remaining on the surface. On the other hand, three-dimensional objects used as dental products are required to have a smooth surface (smoothness). Therefore, a process is carried out to polish three-dimensional objects formed by stereolithography to give the surface a smoothness.
[0005] The process of polishing a three-dimensional object requires a lot of time, which is a heavy burden in terms of production efficiency. As a method for smoothing the surface of a three-dimensional object other than polishing, a method of forming a coating on the surface of the three-dimensional object is considered. However, if the adhesion between the three-dimensional object and the coating is insufficient, problems such as peeling of the coating may occur. In view of the above circumstances, an object of one aspect of the present disclosure is to provide a method for producing a three-dimensional object having a coating with excellent adhesion on a surface thereof, and a three-dimensional object obtained by the method. [Means for solving the problem]
[0006] Specific means for solving the above problems are as follows. <1> A step 1 of obtaining a three-dimensional object including an uncured portion by a stereolithography method using the photocurable composition (a); A step 2 of forming a coating on a surface of the three-dimensional object; and step 3 of curing an uncured portion of the three-dimensional object having the coating. <2> The formation of the coating is carried out using a photocurable composition (b). <1> 13. A method for producing a three-dimensional object according to claim 12. <3> The photocurable composition (b) contains the same photopolymerizable component as the photopolymerizable component contained in the photocurable composition (a). <2> 13. A method for producing a three-dimensional object according to claim 12. <4> The method further includes a step 4 of cleaning the three-dimensional object. <1> or <2> 13. A method for producing a three-dimensional object according to claim 12. <5> Step 4 is carried out between steps 1 and 2; <4> 13. A method for producing a three-dimensional object according to claim 12. <6> The photolithography method is an SLA method or a DLP method, <1> ~ <5> 13. The method for producing a three-dimensional object according to claim 12 . <7> A method for producing a dental product, <1> ~ <6> 13. The method for producing a three-dimensional object according to claim 12 . <8> <1> ~ <6> 13. A three-dimensional object manufactured by the method for manufacturing a three-dimensional object according to any one of claims 1 to 12. Effect of the Invention
[0007] According to one aspect of the present disclosure, there is provided a method for producing a three-dimensional object having excellent adhesion of a coating formed on a surface thereof, and a three-dimensional object obtained by the method. [Brief description of the drawings]
[0008] [Figure 1A] FIG. 1 is a diagram showing the shape of a three-dimensional object produced in an example. [Figure 1B] FIG. 1 is a diagram showing the shape of a three-dimensional object produced in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, the term "(meth)acrylic monomer" refers to a concept that includes both acrylic monomers and methacrylic monomers, and the term "(meth)acryloyl" refers to a concept that includes both acryloyl and methacryloyl.
[0010] <Method of manufacturing 3D objects> A method for producing a three-dimensional object according to the present disclosure includes: A step 1 of obtaining a three-dimensional object including an uncured portion by a stereolithography method using the photocurable composition (a); A step 2 of forming a coating on a surface of the three-dimensional object; and step 3 of curing an uncured portion of the three-dimensional object having the coating.
[0011] As will be shown in the examples described later, a three-dimensional object produced by a method according to the present disclosure has excellent adhesion of a coating provided on the surface.
[0012] In the method of the present disclosure, a three-dimensional object is manufactured by stereolithography. In stereolithography, a photocurable composition is generally irradiated with light to form a layer, and a new layer is formed on the formed layer, and the process is repeated to form a three-dimensional object. In this case, in order to ensure adhesion between the layers, each layer is formed under conditions in which the photocurable composition is not completely cured (for example, a curing rate of 65 to 85%). After the lamination step, the three-dimensional object including the formed uncured portion is further irradiated with light to further harden the three-dimensional object (e.g., to a hardening rate of 85% or more), thereby obtaining a three-dimensional object made of a hardened product of the photocurable composition.
[0013] In the method of the present disclosure, a coating is formed on the surface of a three-dimensional object including an uncured portion obtained by stereolithography before the object is further cured. This makes it possible to omit a step such as polishing to impart lubricity to the surface of the three-dimensional object after the object is further cured. This results in excellent production efficiency of three-dimensional objects. The method of the present disclosure is described in detail below.
[0014] (Process 1) In step 1, a three-dimensional object including an uncured portion is obtained using the photocurable composition (a). Hereinafter, step 1 is also referred to as a photolithography step. The method for carrying out step 1 is not particularly limited, and can be selected from various stereolithography methods.
[0015] Representative stereolithography methods include liquid tank type stereolithography methods such as the SLA (Stereo Lithography Apparatus) method and the DLP (Digital Light Processing) method, and the inkjet method. The SLA method includes a method in which a photocurable composition is irradiated with spot-shaped light, and layers formed are laminated to obtain a three-dimensional object. The DLP method includes a method in which a photocurable composition is irradiated with planar light to form layers, and then the layers are laminated to obtain a three-dimensional object. An example of the inkjet method is a method in which droplets of a photocurable composition are continuously discharged from an inkjet nozzle onto a substrate, and the droplets attached to the substrate are irradiated with light to obtain a three-dimensional object.
[0016] From the viewpoint of production efficiency of a three-dimensional object, the stereolithography method is preferably a liquid tank type stereolithography method, and more preferably an SLA method or a DLP method.
[0017] The conditions for irradiating light in step 1 are not particularly limited and can be selected depending on the type of photocurable composition (a) used, the size of the three-dimensional object, etc. For example, the cumulative light amount of light irradiation per layer is 0.1 J / cm 2 ~100J / cm 2The wavelength of the irradiated light may be selected within the range. In addition, the wavelength of the irradiated light may be appropriately selected in consideration of the excitation wavelength of the photopolymerization initiator contained in the photocurable composition (a), etc. For example, the irradiated light may have a wavelength range of 300 nm to 500 nm.
[0018] When layers formed from the photocurable composition (a) are laminated in step 1, the thickness of each layer (lamination width) is not particularly limited. From the viewpoint of production efficiency of a three-dimensional object, the thickness of each layer is preferably 10 μm or more, more preferably 25 μm or more, and even more preferably 50 μm or more. From the viewpoint of smoothness of the surface of the three-dimensional object, the thickness of each layer is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less.
[0019] The photocurable composition (a) used in step 1 is not particularly limited as long as it has the property of being cured when irradiated with light. Specific examples of the photocurable composition (a) include compositions containing a component (photopolymerizable component) that has the property of being polymerized when irradiated with light.
[0020] The photopolymerizable component contained in the photocurable composition (a) includes a compound containing an ethylenic double bond. Examples of the compound containing an ethylenic double bond include (meth)acrylic monomers, styrene, styrene derivatives, and (meth)acrylonitrile.
[0021] The photocurable composition (a) preferably contains at least one (meth)acrylic monomer as a photopolymerizable component.
[0022] The (meth)acrylic monomer contained in the photocurable composition (a) may be a monofunctional (meth)acrylic monomer (i.e., a monomer having one (meth)acryloyl group in the molecule), a difunctional (meth)acrylic monomer (i.e., a monomer having two (meth)acryloyl groups in the molecule), or a polyfunctional (meth)acrylic monomer (i.e., a monomer having three or more (meth)acryloyl groups in the molecule), or a combination thereof.
[0023] Specific examples of monofunctional (meth)acrylic monomers include cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, and cyclic trimethylolpropane formal (meth)acrylate. Examples of the acrylates include 4-(meth)acryloylmorpholine, lauryl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, 2-dodecyl-1-hexadecanyl (meth)acrylate, 2-(meth)acryloyloxyethyl-succinic acid, 2-[[(butylamino)carbonyl]oxy]ethyl (meth)acrylate, and 2-(2-ethoxyethoxy)ethyl (meth)acrylate.
[0024] Specific examples of bifunctional (meth)acrylic monomers include ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, glycerin di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, dioxane glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, acrylate, dipropylene glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, ethoxylated hydrogenated bisphenol A di(meth)acrylate, 2-hydroxy-3-acryloyloxypropyl (meth)acrylate, biscarbamate bis(2-(meth)acryloxyethyl)N,N'-1,9-nonylene ((meth)acrylic acid diurethane), polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and the like.
[0025] From the viewpoint of promoting the curing of the photocurable composition (a), the photocurable composition (a) preferably contains at least a difunctional (meth)acrylic monomer as a photopolymerizable component. In this case, the total amount of the bifunctional (meth)acrylic monomers contained in the photocurable composition (a) is preferably 60 mass % or more of the total photopolymerizable components, more preferably 80 mass % or more, and even more preferably 90 mass % or more.
[0026] The amount of the photopolymerizable component contained in the photocurable composition (a) is not particularly limited. The amount of the photopolymerizable component is, for example, preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, of the entire photocurable composition (a).
[0027] The photocurable composition (a) may contain a photopolymerization initiator in addition to the photopolymerizable component. Examples of the photopolymerization initiator include an alkylphenone compound, an acylphosphine oxide compound, a titanocene compound, an oxime ester compound, a benzoin compound, an acetophenone compound, a benzophenone compound, a thioxanthone compound, an α-acyloxime ester compound, a phenylglyoxylate compound, a benzyl compound, an azo compound, a diphenyl sulfide compound, an iron phthalocyanine compound, a benzoin ether compound, and an anthraquinone compound.
[0028] From the viewpoint of reactivity, the photopolymerization initiator is preferably an alkylphenone compound or an acylphosphine oxide compound.
[0029] The photocurable composition (a) may contain components other than the photopolymerizable component and the photopolymerization initiator, if necessary. For example, the photocurable composition (a) may contain inorganic fillers, modifiers, stabilizers, antioxidants, solvents, colorants, and the like.
[0030] The photocurable composition (a) preferably has a viscosity (hereinafter simply referred to as "viscosity") of 5 mPa·s to 50,000 mPa·s, as measured with an E-type viscometer at 25° C. and 5 rpm. Here, rpm means revolutions per minute. When the viscosity of the photocurable composition (a) is within the above range, the photocurable composition (a) has good handleability when a three-dimensional object is produced by stereolithography.
[0031] (Process 2) In step 2, a coating is formed on the surface of the three-dimensional object obtained in step 1. Hereinafter, step 2 is also referred to as a coating formation step.
[0032] In the method of the present disclosure, the uncured portion of the three-dimensional object obtained in step 1 is not cured (e.g., irradiated with light) before step 2. That is, the coating is formed when the three-dimensional object formed by stereolithography is in a state in which it is not completely cured. For this reason, the coating has better adhesion to the main body of the three-dimensional object than when the coating is formed on the surface of a more cured three-dimensional object.
[0033] From the viewpoint of controlling the smoothness of the surface of the three-dimensional object, it is preferable to form the coating using the photocurable composition (b). For example, by applying the photocurable composition (b) to the surface of a three-dimensional object to form a coating, the uneven shape resulting from the traces of modeling on the surface of the three-dimensional object is covered with the coating, resulting in a three-dimensional object with excellent surface smoothness. The method for applying the photocurable composition (b) to the surface of the three-dimensional object is not particularly limited, and specific examples of the application method include coating, spraying, immersion, and the like.
[0034] When a coating is formed using the photocurable composition (b), the components contained in the photocurable composition (b) are not particularly limited. From the viewpoint of adhesion of the coating to the surface of the three-dimensional object, it is preferable that the photocurable composition (b) contains the same photopolymerizable component as the photopolymerizable component contained in the photocurable composition (a).
[0035] A method for forming a coating using the photocurable composition (b) includes a method in which the photocurable composition (b) is applied to the surface of a three-dimensional object, and then irradiated with light as necessary to cure the photocurable composition (b). The conditions for irradiating light can be appropriately selected from conditions under which the photocurable composition (b) can be cured, taking into consideration the performance of an irradiation device (such as an LED light irradiator). For example, an integrated light dose of 1.0 J / cm 2 ~10J / cm 2The wavelength of the irradiation light may be selected within the range, and irradiation may be performed multiple times. The wavelength of the irradiation light may be appropriately selected in consideration of the excitation wavelength of the photopolymerization initiator contained in the photocurable composition (b). For example, the irradiation light may include a wavelength range of 300 nm to 500 nm. When the photocurable composition (b) is cured, the photocurable composition (b) may or may not be completely cured.
[0036] The thickness of the coating formed in step 2 (if the thickness is not constant, the minimum thickness) is not particularly limited. From the viewpoint of smoothness of the surface of the three-dimensional object, the thickness of the coating is preferably 2 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. From the standpoint of coating uniformity, the thickness of the coating may preferably be 500 μm or less, more preferably be 250 μm or less, and even more preferably be 200 μm or less.
[0037] The coating may be formed on the entire surface of the three-dimensional object, or may be formed only on a portion of the surface of the three-dimensional object. The coating may be in a state that can be distinguished from the main body of the three-dimensional object, or in a state that cannot be distinguished from the main body of the three-dimensional object.
[0038] (Step 3) In step 3, the uncured portion of the three-dimensional object having the coating is cured. Hereinafter, step 3 is also referred to as a main curing step.
[0039] There is no particular limitation on the method for carrying out step 3. For example, step 3 may be carried out by irradiating the surface of the three-dimensional object with light using an LED lamp or the like.
[0040] The conditions for irradiating light in step 3 are not particularly limited and are selected depending on the type of photocurable composition used, the size of the three-dimensional object, etc. For example, 2 ~100J / cm 2The wavelength of the irradiation light may be selected within the range of 100 nm to 500 nm, and irradiation may be performed several times. The wavelength of the irradiation light may be appropriately selected in consideration of the excitation wavelength of the photopolymerization initiator contained in the photocurable composition. For example, the irradiation light may have a wavelength range of 300 nm to 500 nm.
[0041] (Step 4) In the method of the present disclosure, step 4 may be carried out to clean the surface of the three-dimensional object. Hereinafter, step 4 may also be referred to as a cleaning step.
[0042] The method for carrying out step 4 is not particularly limited. For example, the surface of the three-dimensional object may be washed using an organic solvent. The type of organic solvent is not particularly limited, and examples thereof include isopropanol (IPA), ethanol, and tripropylene glycol monomethyl ether.
[0043] Step 4 may be performed between steps 1 and 2, or after step 3. By carrying out step 4 between step 1 and step 2, the uncured portion can be exposed on the surface of the three-dimensional object, and the adhesion of the coating tends to improve. By carrying out step 4 after step 3, the uncured photocurable composition remaining on the surface can be removed. It is preferable that step 4 is carried out at least between step 1 and step 2, and it is more preferable that step 4 is carried out between step 1 and step 2 and after step 3, respectively.
[0044] <3D object> The three-dimensional object according to the present disclosure is manufactured by the manufacturing method of a three-dimensional object according to the present disclosure described above. The three-dimensional object according to the present disclosure can be used for various purposes. The three-dimensional object according to the present disclosure can be suitably used, for example, as a dental product.
[0045] The type of dental product is not particularly limited. Specific examples include instruments to be placed in the oral cavity, dental models (such as models for dental surgery), and dental materials (such as dental restorative materials). Specific examples of devices that are worn in the oral cavity include dentures, lining materials, mouthpieces, mouthguards, splints, etc.
[0046] The three-dimensional object according to the present disclosure has excellent surface smoothness. Therefore, it is comfortable to wear in the oral cavity and is safe because it is unlikely to damage the oral cavity. Furthermore, the surface coating has excellent adhesion and durability. EXAMPLES
[0047] Hereinafter, the embodiments of the present disclosure will be specifically described based on examples, but the present disclosure is not limited to these examples.
[0048] <Preparation of test pieces for tensile tests> Test pieces for tensile testing were prepared by stereolithography under the following conditions. Using Solidworks 2022 (made by Solidworks Japan), data for a three-dimensional object with the shape shown in Figures 1A and 1B was created. Fig. 1A is a diagram of the three-dimensional object observed from the main surface (33.65 mm × 9.9 mm) side, and Fig. 1B is a diagram of the three-dimensional object observed from the side (33.65 mm × 3.3 mm) side. As shown in Fig. 1B, the three-dimensional object has an inclined surface X that is inclined at an angle of 45°. Based on the data obtained, specimens 1A, 1B, and 1C of three-dimensional objects including uncured parts were produced under the following conditions. The ink layer width was set to 100 μm.
[0049] Printer A: Pro95 (Spirntray) Ink A: die and model2 grey (Spirntray) Washing and drying method A: Wash with IPA twice using Pro Wash (Sprintray) (first wash: 3 minutes, second wash: 3 minutes), and dry for 5 minutes. Curing device A: ProCure (manufactured by Sprintray)
[0050] Printer B: Form3B+ (Formlabs) Ink B: Dental LT Clear (Formlabs) Cleaning and drying method B: Wash with IPA twice using Form Wash (Formlabs) (first time: 10 minutes, second time: 5 minutes), then use compressed air to blow off any remaining IPA on the surface and dry it. Curing device B: Formcure (manufactured by Formlabs)
[0051] Printer C: Cara4.0Pro (Kulzer) Ink C: dima Print Digital Denture Original Pink (Kulzer) Cleaning and drying method C: Perform IPA ultrasonic cleaning twice (first time: 3 minutes, second time: 3 minutes) using an ultrasonic cleaner (Branson), then use compressed air to blow off any IPA remaining on the surface and dry. Main curing device C: Hi Lite 3D (manufactured by Kulzer)
[0052] Example 1A Ink A was applied to the inclined surface X of one of the two test pieces 1A prepared using printer A, ink A, and cleaning and drying method A, and the inclined surface X of the other test piece 1A was brought into close contact with the ink. In this state, a VALO cordless (Ultradent) was used to irradiate the sample with light in extra mode for three seconds twice (accumulated amount per irradiation: 3.1 J / cm2). 2 ) to bond the two test pieces together. The bonded test specimens were cured with the main curing device A at 88 mJ / cm per minute. 2 for 8 minutes (accumulated light intensity: 0.7 J / cm 2 ) to completely cure the composition. After curing, the test piece was washed with IPA to obtain a test piece according to Example 1A.
[0053] Comparative Example 1A Two test pieces 1A were prepared using printer A, ink A, and cleaning and drying method A. The test pieces were then cured with this curing device A at a rate of 88 mJ / cm per minute. 2 for 8 minutes (accumulated light intensity: 0.7 J / cm2 ) to completely cure it. After that, ink A was applied to one of the inclined surfaces X of the test piece 1A, and the inclined surface X of the other test piece 1A was brought into close contact with it. In this state, a VALO cordless (manufactured by Ultradent) was used to apply light twice for 3 seconds in extra mode (accumulated amount per time: 3.1 J / cm 2 ) to bond the two test pieces together. The bonded test body was washed with IPA to obtain a test piece according to Comparative Example 1A.
[0054] Example 1B Ink B was applied to the inclined surface X of one of the two test specimens 1B prepared using printer B, ink B, and cleaning and drying method B, and the inclined surface X of the other test specimen 1B was brought into close contact with the ink B. In this state, a VALO cordless (Ultradent) was used to irradiate the specimen with light in extra mode for 3 seconds twice (accumulated amount per irradiation: 3.1 J / cm 2 ) to bond the two test pieces together. The bonded specimens were cured with the main curing device B at 3740 mJ / cm per minute. 2 for 15 minutes (accumulated light intensity: 56.1 J / cm 2 ) to completely cure the composition. After curing, the test piece was washed with IPA to obtain a test piece according to Example 1B.
[0055] (Comparative example 1B) Two test pieces 1B were prepared using printer B, ink B, and cleaning and drying method B. The test pieces 1B were then cured with this curing device B at 3740 mJ / cm per minute. 2 for 15 minutes (accumulated light intensity: 56.1 J / cm 2 ) to completely cure it. After that, ink B was applied to one of the inclined surfaces X of test piece 1B, and the inclined surface X of the other test piece 1B was brought into close contact with it. In this state, a VALO cordless (manufactured by Ultradent) was used to apply light twice for 3 seconds in extra mode (accumulated amount per time: 3.1 J / cm 2 ) to bond the two test pieces together. The bonded test body was washed with IPA to obtain a test piece according to Comparative Example 1B.
[0056] Example 1C Two specimens 1C were prepared using printer C, ink C, and cleaning and drying method C. Ink C was applied to the inclined surface X of one of the specimens, and the inclined surface X of the other specimen 1C was brought into close contact with the specimen. In this state, a VALO cordless (Ultradent) was used to irradiate the specimen with light in extra mode for three seconds twice (accumulated amount per irradiation: 3.1 J / cm2). 2 ) to bond the two test pieces together. The bonded test specimens were cured with the main curing device C at 364 mJ / cm per minute. 2 for 15 minutes (accumulated light intensity: 5.5 J / cm 2 ) to completely cure the composition. After curing, the test piece was washed with IPA to obtain a test piece according to Example 1C.
[0057] (Comparative example 1C) Two test pieces 1C were prepared using printer C, ink C, and cleaning and drying method C. The test pieces 1C were then cured with this curing device C at a rate of 364 mJ / cm per minute. 2 for 15 minutes (accumulated light intensity: 5.5 J / cm 2 ) to completely cure it. After that, ink C was applied to one of the inclined surfaces X of test piece 1C, and the inclined surface X of the other test piece 1C was brought into close contact with it. In this state, a VALO cordless (Ultradent) was used to apply light twice for 3 seconds in extra mode (accumulated amount per exposure: 3.1 J / cm2). 2 ) to bond the two test pieces together. The bonded test body was washed with IPA to obtain a test piece according to Comparative Example 1C.
[0058] (Tensile test) Tensile tests were carried out on the test pieces prepared in the examples and comparative examples. Specifically, the tensile strength (N) was measured at a speed of 60 mm / s using a force gauge ZTS-1000N, an electric test stand EMX-1000N, and a pantograph chuck PGC-0510 (all manufactured by Imada). The results are shown in Table 1 below.
[0059] [Table 1]
[0060] As shown in Table 1, the test pieces of Examples 1A, 1B, and 1C, in which ink was applied to the test piece before the final curing, had greater tensile strength than the test pieces of Comparative Examples 1A, 1B, and 1C, in which ink was applied to the test piece after the final curing. From the above results, it is evident that the coating formed on the surface of the three-dimensional object before full curing has superior adhesiveness compared to the coating formed on the surface of the three-dimensional object after full curing.
[0061] <Preparation of test pieces for cross-cut tests> Test pieces for tensile testing were prepared by stereolithography under the following conditions. Using Solidworks 2022 (made by Solidworks Japan), data for a 3D object measuring 64 mm in length, 20 mm in width, and 3.3 mm in thickness was created. Based on the data, specimens 2A, 2B, and 2C were created, including uncured portions, under the conditions described above for the preparation of test pieces for tensile tests. The ink layer width was 100 μm.
[0062] Example 2A Ink A was applied to one side of the 64 mm × 20 mm surface of test piece 2A, and then VALO Cordless (Ultradent) was used to irradiate the ink six times for three seconds in extra mode (accumulated amount per irradiation: 3.1 J / cm 2 ) was performed to form a coating. The test specimen with the coating was then subjected to a curing device A at 88 mJ / cm per minute. 2 for 8 minutes (accumulated light intensity: 0.7 J / cm 2 ) to completely cure the composition. After curing, the test piece was washed with IPA to obtain a test piece according to Example 2A.
[0063] (Comparative example 2A) A test piece according to Comparative Example 2A was obtained in the same manner as in Example 2A, except that the order of light irradiation using the VALO Cordless and main curing was reversed.
[0064] Example 2B Ink B was applied to one side of the 64 mm × 20 mm surface of test specimen 2B, and then VALO Cordless (Ultradent) was used to irradiate the ink six times for three seconds in extra mode (accumulated amount per irradiation: 3.1 J / cm 2 ) was performed to form a coating. The test specimen with the coating was then subjected to a curing device B at 3740 mJ / cm per minute. 2 for 15 minutes (accumulated light intensity: 56.1 J / cm 2 ) to completely cure the composition. After curing, the test piece was washed with IPA to obtain a test piece according to Example 2B.
[0065] (Comparative Example 2B) A test piece according to Comparative Example 2B was obtained in the same manner as in Example 2B, except that the order of light irradiation using the VALO Cordless and main curing was reversed.
[0066] Example 2C Ink C was applied to one side of the 64 mm × 20 mm surface of test specimen 2C, and then VALO Cordless (Ultradent) was used to irradiate the ink six times for three seconds in extra mode (accumulated amount per irradiation: 3.1 J / cm 2 ) was performed to form a coating. The test specimen with the coating was then subjected to a curing device C at 364 mJ / cm per minute. 2 for 15 minutes (accumulated light intensity: 5.5 J / cm 2 ) to completely cure the composition. After curing, the test piece was washed with IPA to obtain a test piece according to Example 2C.
[0067] (Comparative Example 2C) A test piece according to Comparative Example 2C was obtained in the same manner as in Example 2C, except that the order of light irradiation using the VALO Cordless and main curing was reversed.
[0068] (Cross-cut test) A cross-cut test was carried out on the test pieces prepared in the examples and comparative examples. Specifically, a cross-cut test (JIS-K5600) was performed at 2 mm intervals on the surface of the test piece on which the coating was formed, and the results were classified into a scale of 0 to 5. The results are shown in Table 2 below. The smaller the number in the cross-cut classification shown in Table 2, the higher the adhesion of the coating.
[0069] [Table 2]
[0070] As shown in Table 2, the test pieces of Examples 2A, 2B, and 2C, in which ink was applied to the test piece before main curing, had lower crosscut classification numbers than the test pieces of Comparative Examples 2A, 2B, and 2C, in which ink was applied to the test piece after main curing. From the above results, it is evident that the coating formed on the surface of the three-dimensional object before full curing has superior adhesiveness compared to the coating formed on the surface of the three-dimensional object after full curing.
Claims
1. Step 1 of obtaining a three-dimensional object including an uncured portion by a stereolithography method using a photocurable composition (a); A step 2 of forming a coating on a surface of the three-dimensional object; and step 3 of curing an uncured portion of the three-dimensional object having the coating.
2. The method for producing a three-dimensional object according to claim 1 , wherein the coating is formed using a photocurable composition (b).
3. The method for producing a three-dimensional object according to claim 2 , wherein the photocurable composition (b) contains the same photopolymerizable component as the photopolymerizable component contained in the photocurable composition (a).
4. The method for manufacturing a three-dimensional object according to claim 1 , further comprising a step 4 of cleaning the three-dimensional object.
5. The method for producing a three-dimensional object according to claim 4 , wherein step 4 is carried out between step 1 and step 2 .
6. The method for producing a three-dimensional object according to claim 1 , wherein the stereolithography is an SLA method or a DLP method.
7. The method for producing a three-dimensional object according to claim 1, which is a method for producing a dental product.
8. A three-dimensional object manufactured by the method for manufacturing a three-dimensional object according to any one of claims 1 to 7.
Citation Information
Patent Citations
Post-treating method for stereo lithographic matter and forming mold
JP2000318048A
Mold for photo fabrication
JP2001079855A
Device for holding optically molded article and apparatus for post processing optically molded article
JP2008168596A
Polymer-based mold and method of making same
JP2016509968A
How to create physical objects through additive manufacturing
JP2020528841A