Resin composition and method for producing the same
A resin composition with a thermoplastic resin, elastomer, and acid-modified elastomer, processed via a multi-screw extruder, addresses the balance of embrittlement temperature and rigidity in lignocellulose fiber-reinforced resins, ensuring mechanical strength and low-temperature resistance.
Patent Information
- Application Number
- JP2023064962
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
AI Technical Summary
Lignocellulose fibers, when used as reinforcing materials for resins, face challenges in achieving a balance between embrittlement temperature and rigidity, particularly at low temperatures, and existing resin compositions do not adequately address this issue.
A resin composition is developed containing a thermoplastic resin with an elastomer, lignocellulose fibers, and an acid-modified elastomer, processed using a multi-screw extruder to maintain mechanical properties while lowering embrittlement temperature, with specific mass percentages and processing conditions to ensure compatibility and rigidity.
The resin composition achieves excellent mechanical properties and low-temperature embrittlement resistance, maintaining rigidity and preventing excessive embrittlement, suitable for applications requiring both.
Smart Images

Figure 2024151536000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and a method for producing the same. [Background technology]
[0002] Lignocellulosic resources derived from wood and non-wood plants accumulate carbon dioxide during the plant growth process and are recognized as carbon-neutral materials that do not emit excess carbon dioxide during their use or disposal. Lignocellulosic resources obtained from wood and non-wood plants are composed of lignocellulosic fibers. Lignocellulosic fibers can be obtained by mechanically, thermomechanically, chemically, chemomechanically, or chemothermo-mechanically treating lignocellulosic resources to soften or destroy the intermediate layer that adhesively binds the fibers, and to disentangle or refine the fibers. The lignocellulosic fibers obtained in this manner are mainly used as pulp, a raw material for paper, or as fibers, a raw material for fiberboard. This is because lignocellulosic fibers are lightweight, high-strength, highly elastic, renewable, and low-cost.
[0003] In order to solve recent environmental problems such as global warming, the use of lignocellulosic fibers is expected to replace talc, glass fiber, carbon fiber, synthetic resin fiber, mineral fiber, and metal fiber, which have traditionally been used as reinforcing materials for resins. By replacing traditional non-renewable materials with lignocellulosic fibers, advantages such as lighter weight of materials, improved LCA (Life Cycle Assessment), and cost reduction can be obtained, and for this reason the use of lignocellulosic fibers has attracted attention in the transportation equipment manufacturing industry, especially the automobile manufacturing industry.
[0004] Among resin materials, those used outdoors are exposed to environments below 0°C during the cold season, and for example, crystalline polypropylene becomes brittle at low temperatures and is not suitable for practical use. To improve this, elastomers are added or other components are copolymerized during the resin polymerization to create a block copolymer structure (copolymer structure). However, when such elastomer-blended resins or copolymer resins are used, although brittleness is improved, the opposing property of rigidity is reduced, and sufficient mechanical properties cannot be obtained.
[0005] For this reason, talc has conventionally been added to resins containing elastomers or block copolymer resins to compensate for the lack of rigidity. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2-124956 [Patent Document 2] Japanese Patent Application Publication No. 7-18151 [Patent Document 3] Japanese Patent Application Publication No. 11-60828 [Patent Document 4] JP 2001-172466 A [Patent Document 5] JP 2002-97337 A [Patent Document 6] JP 2020-158606 A [Patent Document 7] JP 2016-166365 A [Patent Document 8] JP 2022-156073 A Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, it is expected that lignocellulose fibers will be used as a resin reinforcing material instead of talc, which has been conventionally used, but the present inventors have found that reinforcing resin with lignocellulose fibers is more effective at imparting rigidity than reinforcing resin with a filler such as talc, but that it also exhibits brittleness, particularly at low temperatures. In other words, the present inventors' research has revealed that when lignocellulose fibers are used as a resin reinforcing material, there is a problem in that it is difficult to achieve a desired balance between brittleness temperature and rigidity.
[0008] In order to solve the above problems, it is desirable to develop a resin composition that contains lignocellulose fibers, has excellent resistance to low-temperature embrittlement, and at the same time has a certain level of mechanical properties, while using lignocellulose fibers as a raw material and generally used resin processing equipment. Patent Documents 1 to 8 are known as techniques for improving the mechanical properties of resin materials. Patent Document 1 discloses a low-temperature impact-resistant resin composition comprising a polypropylene resin and polyester long fibers. However, the low-temperature impact-resistant resin composition in this document is not a resin composition containing lignocellulose fibers, and the document does not mention the brittle temperature. Patent Document 2 discloses a low-temperature impact-resistant resin composition consisting of a polypropylene block copolymer resin, EBR (ethylene butene copolymer elastomer), and talc, but this is not a resin composition containing lignocellulose fibers, and there is no mention of the brittle temperature. Patent Document 3 discloses a low-temperature impact-resistant resin composition consisting of polypropylene resin, long glass fibers, and talc, but this is not a resin composition containing lignocellulose fibers, and there is no mention of the brittle temperature.
[0009] Patent Document 4 discloses a low-temperature impact-resistant resin composition consisting of a polypropylene block copolymer resin, EPR (ethylene propylene copolymer elastomer), and talc, but this is not a resin composition containing lignocellulose fibers, and no mention is made of the brittleness temperature. Patent Document 5 discloses a low-temperature impact-resistant resin composition that is composed of polypropylene resin, polypropylene block copolymer resin, and talc and has excellent moldability. However, this is not a resin composition that contains lignocellulose fibers, and there is no mention of the brittleness temperature. Patent Document 6 discloses an impact-resistant resin composition having excellent mechanical strength, which is composed of a polypropylene resin, a polyethylene resin, wood powder, and a compatibilizer for an acid-modified polyethylene resin. However, this does not mention the effects on low-temperature impact properties or brittle temperature, nor does it suggest the use of a modified elastomer.
[0010] Patent Document 7 discloses an impact-resistant resin composition with excellent mechanical strength, which is composed of polyamide resin, polypropylene resin, and an EPR (ethylene propylene copolymer elastomer) modified compatibilizer, but this is a polymer alloy that makes use of the relatively superior mechanical properties of polyamide compared to polypropylene, and the means of solving the problem are different. In addition, there is no mention of the effects on impact properties and brittle temperature at low temperatures, and furthermore, it is not a resin composition containing lignocellulose fibers, and the use of an acid-modified resin compatibilizer is also negative.
[0011] Patent Document 8 discloses a resin composition with excellent strength and impact resistance, which contains cellulose, an acid-modified elastomer, and high-density polyethylene as essential components in a copolymerized polypropylene resin. The technology in this document differs from the present invention in that it contains high-density polyethylene as an essential component, requires a sufficient amount of acid-modified elastomer relative to the cellulose, the cellulose is limited to high-purity cellulose, and the object of the invention is to rebalance the strength of the resin by increasing the impact resistance.
[0012] An object of the present invention is to provide a resin composition which is excellent in mechanical properties and has resistance to low-temperature embrittlement. [Means for solving the problem]
[0013] For example, polypropylene is a crystalline resin with a relatively high brittle temperature. In order to lower the brittle temperature of polypropylene to less than 0°C, the problem of high brittle temperature can be solved to a certain extent by blending an elastomer into the polypropylene resin or using a block copolymer polypropylene resin copolymerized with an elastomer as the matrix resin. However, the rigidity of such a resin containing an elastomer decreases. Therefore, the present inventors noticed that blending lignocellulose fibers to compensate for the rigidity tends to raise the brittle temperature above the desired brittle temperature.
[0014] As a result of intensive research to solve this problem, the inventors have discovered that by using the simple method of changing the acid-modified polyolefin, which is usually used as a compatibilizer for lignocellulosic fibers and thermoplastic resins, to a modified elastomer, it is possible to achieve a resin composition that has excellent low-temperature embrittlement resistance and mechanical properties by compensating for rigidity while purposefully suppressing the increase in brittleness temperature. The present invention was completed based on the above findings and through further investigation.
[0015] The present invention provides a resin composition for fiber-reinforced resin, comprising the following components (A) to (C), in which the total mass proportion of an elastomer component contained in the following component (A) and the following component (C) is 0.1% or more and 30% or less, the mass proportion of the following component (B) is 1% or more and 80% or less, and the mass proportion of a thermoplastic resin contained in the following component (A) is 10% or more and 95% or less. (A) Thermoplastic resin containing elastomer (B) Lignocellulosic fibers (C) Acid-modified elastomer
[0016] The present invention also provides a method for producing a resin composition, comprising the steps of: producing the resin composition according to any one of claims 1 to 5 using a multi-screw extruder having two or more screws; and the multi-screw extruder is provided with a cylinder having a kneading space in which the screws are arranged inside; and a heating device including a heating section arranged on the outer periphery of the cylinder along the axial direction of the cylinder. The method includes a step of melting a thermoplastic resin containing an elastomer at a temperature equal to or higher than the melting point of the thermoplastic resin; and a step of kneading the molten thermoplastic resin containing an elastomer, lignocellulose fibers, and an acid-modified elastomer while maintaining the set temperature of the heating section below the melting point of the thermoplastic resin; or a step of melting a thermoplastic resin at a temperature equal to or higher than the melting point of the thermoplastic resin; and a step of kneading the molten thermoplastic resin, elastomer, lignocellulose fibers, and acid-modified elastomer while maintaining the set temperature of the heating section below the melting point of the thermoplastic resin. The present invention provides a method for producing a resin composition for fiber-reinforced resin. Effect of the Invention
[0017] According to the present invention, it is possible to provide a resin composition having excellent mechanical properties and resistance to low-temperature embrittlement. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic diagram showing a twin-screw extruder, which is an example of a multi-screw extruder used in the production of a resin composition having resistance to low-temperature embrittlement of the present invention. [Diagram 2] FIG. 2 is a perspective plan view of two screws arranged parallel to each other, viewed from above with the cylinder omitted. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will now be described in detail based on preferred embodiments thereof. First, the resin composition for fiber reinforced resin of the present invention will be described. The resin composition of the present invention contains the following components (A) to (C). (A) Thermoplastic resin containing elastomer (B) Lignocellulosic fibers (C) Acid-modified elastomer
[0020] The resin composition of the present invention, which contains the above-mentioned components (A) to (C), is able to achieve both mechanical properties and resistance to low-temperature embrittlement. This point will be described in detail below.
[0021] [Component (A): Thermoplastic resin containing elastomer] Examples of the thermoplastic resin containing an elastomer, which is component (A), include (i) a copolymer of an elastomer and a thermoplastic resin, (ii) a mixture of an elastomer and a thermoplastic resin, and (iii) a mixture of the above (i) with an elastomer and / or a thermoplastic resin. In terms of production and cost, the above (i) or (iii) is particularly preferred. (1)Thermoplastic resin The thermoplastic resin used in the present invention preferably has a melting point of 260° C. or lower. The thermoplastic resin used in the present invention must have a certain degree of heat resistance, and preferably has a melting point of 100° C. or higher. The melting point of the thermoplastic resin here means the melting point of the thermoplastic resin in (i), (ii) or (iii) above. The thermoplastic resin may be one or more selected from the group consisting of polyethylene, polypropylene, polyvinyl alcohol, polyvinyl acetate, polyvinyl chloride, polystyrene, polylactic acid, polyacetal, polyamides, polyhydroxyalkanoic acids, acrylonitrile-butadiene-styrene copolymer resin (ABS), modified resins thereof, copolymer resins, polymer alloys, etc. Among these, polyolefin resins that are widely used are preferred, and polypropylene is more preferred. Taking polypropylene resin as a representative example, the polypropylene resin may be a homopolymer, a block copolymer, or a random copolymer.
[0022] When a homopolymer is used, an elastomer described later or a block copolymer described later can be blended during kneading. Block copolymers (also called block copolymers) are made by blending various comonomers (mainly ethylene propylene copolymer elastomers (EPR), etc.) during the polymerization of polypropylene resin, and have a significant reduction in the brittle temperature. If necessary, elastomers or homopolymers (described below) can also be added during kneading. Random copolymers are made by blending various comonomers (mainly ethylene, etc.) during the polymerization of polypropylene resin, and the reduction in the brittle temperature is not significant. If necessary, elastomers or block copolymers, which will be described later, can be further blended during kneading. Therefore, whether it is a homopolymer or a copolymer, it is composed of, for example, a propylene homopolymer portion and a propylene-ethylene copolymer portion, which do not necessarily need to be bonded together, and may be in a mixed state or in a state including both a mixed state and a bonded state. In recent years, not only polypropylene produced by conventional Ziegler catalysts but also polypropylene produced by metallocene catalysts, which is characterized by excellent flexibility, have been put on the market. Either or any type of polypropylene can be suitably used as long as it meets the objectives of the present invention.
[0023] (2) Elastomer In the present invention, the elastomer effectively acts to lower the brittle temperature. The elastomer used in the present invention is a material that has the property of softening and becoming fluid when heated and returning to a rubber-like state when cooled, and examples of such elastomers include ethylene-based elastomers and styrene-based elastomers. Examples of ethylene-based elastomers include ethylene-propylene copolymer elastomers (EPR), ethylene-butene copolymer elastomers (EBR), ethylene-octene copolymer elastomers (EOR), and ethylene-propylene-diene copolymer elastomers (EPDM). Examples of styrene-based elastomers include styrene-butadiene-styrene copolymer elastomers (SBS), styrene-isoprene-styrene copolymer elastomers (SIS), styrene-ethylene-propylene-styrene copolymer elastomers (SEPS), and hydrogenated styrene-butadiene-styrene block elastomers (SEBS). Since each of these elastomers exhibits unique physical and chemical properties, they can be appropriately blended according to the desired physical properties. Such elastomers may be used alone or in combination of two or more. (3) The copolymer of the above (i) elastomer and thermoplastic resin The copolymer may be a block copolymer of polypropylene, typically a copolymer of polypropylene and an elastomer such as EPR. When producing the resin composition of the present invention, it is convenient to use a copolymer of an elastomer and a thermoplastic resin as component (A) in advance. The method for producing the resin composition of the present invention will be described later.
[0024] [Component (B): Lignocellulosic fiber] The lignocellulosic fibers used in the present invention are obtained by mechanically, thermomechanically, chemically, chemomechanically, or chemothermo-mechanically treating lignocellulosic materials derived from wood or non-wood plants to soften, destroy, disentangle, or refine the middle layer that adhesively binds the fibers. Note that lignocellulosic fibers is a general term, and even plant fibrous materials that have been subjected to physical, chemical, or biological treatments (e.g., delignification treatment in wood pulping, or retting treatment in herbs) so as to be free of lignin, hemicellulose, etc., are included in the lignocellulosic fibers. This is because the presence of lignin and hemicellulose has a limited effect on the effects of the present invention, and the physical and chemical properties of the cellulose fibrous material affect the brittleness temperature.
[0025] Such materials can be used as lignocellulosic fibers without any particular restrictions. Wood may be either coniferous or broad-leaved. Examples of non-wood plant-derived lignocellulosic fibers include straw pulp, bagasse pulp, reed pulp, kenaf pulp, linen pulp, ramie pulp, hemp pulp, flax pulp, bamboo pulp, and the like. Furthermore, the meaning of fiber or pulp includes fibrous materials that appear to be in a powder form, such as wood flour, finely ground materials, sawdust, paper, waste paper, cut pieces of nonwoven fabric, and powder. As the lignocellulose fiber used in the present invention, for example, lignocellulose powder, kraft pulp, semi-chemical pulp, chemi-ground pulp, refiner ground pulp, thermomechanical pulp, ground wood pulp, dissolving pulp, mechanical pulp, or fiberboard fibers can be preferably used.
[0026] Fibers for fiberboards are thermomechanical pulp in a broad sense, and relatively coarse fibers in a narrow sense. As an example of the physical form of the fiber, thermomechanical pulp can be exemplified by a diameter of 30 μm and a length of about 2 to 3 mm. In addition, nanocellulose fibers (also called nano lignocellulose fibers) finely divided into nano-sized fibers in the length and width directions, microcellulose fibers (also called micro lignocellulose fibers) in which nano-sized or micro-sized fibers are mixed in the length and width directions, or even fine powder of wood, so-called wood flour, have an aspect ratio due to the difference in the size of the length and width, and can be exemplified as a type of lignocellulose fiber. Such lignocellulose fibers may be used alone or in combination of two or more types.
[0027] As a method for converting lignocellulosic materials into lignocellulosic fibers, any known method can be used without any particular restrictions. For example, a conventional method for producing pulp, a conventional method for producing fibers for fiberboard, or a mill for powdering chips, etc. can be appropriately used. One example of a method for converting lignocellulosic material into lignocellulosic fibers is to crush the lignocellulosic material into chips, then steam it using a preheater or presteamer under pressure of about 1 to 10 Bar to soften the lignin and hemicellulose that are components of the lignocellulosic material, and then defibrate it into fibers or fiber bundles using a disc-type blade while applying pressure in a pressurized refiner to produce the desired fibers.
[0028] The lignocellulose fibers used in the present invention preferably have a width of 1 μm to 100 μm, more preferably 10 μm to 50 μm, and a length of 0.1 mm to 50 mm, more preferably 1 mm to 5 mm. The length and width of such fibers can be appropriately adjusted to the desired length and width by adjusting operating conditions such as the spacing between the refiner disks. When it is desired to obtain lignocellulosic fibers while maintaining a large aspect ratio, it is efficient to manufacture them through a hydrothermal process as described above, and the resulting fibers are less damaged. On the other hand, when a powder with a low aspect ratio such as wood flour is acceptable, a grinding device or mill can be used. The GHG assessment of the material differs depending on the type of electricity and thermal energy used, so it can be selected according to the purpose.
[0029] Nano- or microcellulose fibers can be those that have been refined by any known method, such as a method of mechanically refining the fibers to the desired size, a method of chemically modifying the fibers and then refining them by applying an external force in water or in a resin, or a combination of these methods. In many cases, lignocellulosic fibers are dried for the purpose of improving transportation, preservation, storage, and handling. As a method for drying lignocellulosic fibers, any known method can be used without particular limitation. For example, as used in the paper and pulp industry, wet lignocellulosic fibers are discharged onto a roller or wire, dehydrated by suction or pressure, and then thermally dried, and as used in the manufacture of fibers for fiberboard, wet lignocellulosic fibers are thermally dried under air flow in a pipe through which hot air flows. The drying of lignocellulosic fibers is preferably performed at a temperature of 60°C or higher and 200°C or lower, more preferably 80°C or higher and 160°C or lower, and even more preferably 100°C or higher and 140°C or lower. In recent years, methods of producing defibration and fiber under dry conditions without using hydrothermal conditions have also become widespread. In some cases, fibers not produced under hydrothermal conditions are acceptable from the standpoint of cost and quality, and in such cases, fibers produced under dry conditions are also acceptable.
[0030] [Component (C): Acid-modified elastomer] In the present invention, the acid-modified elastomer is used to suppress the increase in the brittle temperature as much as possible even when lignocellulose fibers are used, and also to function as a compatibilizer. The acid-modified elastomer is not only used for the purpose of improving the compatibility and affinity between lignocellulose fibers and thermoplastic resins, which have different polarities, but also has an effect on the determination of the brittle temperature in particular. In this specification, "compatibility between lignocellulose fibers and thermoplastic resins" refers to a dispersion state in which lignocellulose fibers and thermoplastic resins, which have different polarities, are mediated by a compatibilizer, which is a compound having both polarities. Thermoplastic resins that are compatible with lignocellulose fibers by the acid-modified elastomer include the following (a) to (d). (a) a thermoplastic resin which is a part of the copolymer (i) (b) The thermoplastic resin in (ii) above (c) a thermoplastic resin other than the thermoplastic resin which is a part of the copolymer (i) in (iii) (d) When the resin composition of the present invention is mixed with another thermoplastic resin to obtain a fiber-reinforced resin material, the other thermoplastic resin The fiber reinforced resin material will be described later.
[0031] Typically, a compatibilizer used for the purpose of improving compatibility or affinity is an acid-modified resin that has high affinity with the matrix resin. For example, for polyolefin resins, acid-modified polyolefin resins, particularly maleic anhydride-modified polyolefin resins, are preferably used. However, as a result of the inventors' investigations, it was found that when lignocellulose fibers and maleic anhydride modified polyolefin resin as a compatibilizer are added to a polyolefin resin whose brittle temperature has been lowered by containing an elastomer, the rigidity is improved compared to a case in which the lignocellulose fibers are not contained, but the brittle temperature becomes higher than desired, making it difficult to balance the physical properties and the brittle temperature.
[0032] This is thought to be because the combined use of lignocellulose fibers and acid-modified polyolefin resin makes the interface between the lignocellulose fibers and the matrix resin relatively rigid, and the stress applied to the test specimen during the brittle temperature test is easily transmitted to the resin, resulting in concentrated cracks in the resin, or because the acid-modified polyolefin resin compatibilizer itself present at the interface between the lignocellulose fibers and the matrix resin may also become brittle at low temperatures. Therefore, in order to reduce the phenomenon in which the impact stress propagating through the fibers is efficiently transmitted to the resin, or to suppress the effect of embrittlement of the acid-modified polyolefin resin compatibilizer, the whole or part of the acid-modified polyolefin resin was replaced with an acid-modified elastomer, which effectively cancels the stress transmitted from the fibers to the matrix resin, does not raise the brittle temperature more than desired, and at the same time, maintains the rigidity within a desired range, making it possible to suitably design a balance between the conflicting properties of mechanical properties and brittle temperature. According to the present invention, by including an acid-modified elastomer (component (C)) in addition to a thermoplastic resin containing an elastomer (component (A)) and lignocellulose fibers (component (B)), it is possible to achieve both mechanical properties and resistance to low-temperature embrittlement.
[0033] The acid-modified elastomer used in the present invention may be an acid-modified product of various elastomers, such as an ethylene propylene copolymer elastomer (EPR), an ethylene butene copolymer elastomer (EBR), an ethylene octene copolymer elastomer (EOR), an ethylene propylene diene copolymer elastomer (EPDM), or a hydrogenated styrene butadiene styrene block elastomer (SEBS). These may be used alone or in combination of two or more. As the acid-modified elastomer, it is preferable to use a maleic anhydride-modified product. The acid used for the acid modification may be other than maleic anhydride, and any acid compound capable of imparting a polar group may be used without any particular limitation, and examples thereof include acrylic acid and glycidyl methacrylate.
[0034] In the resin composition of the present invention, the effect of achieving both mechanical properties and low-temperature embrittlement resistance can be reliably achieved by setting the total mass ratio of the elastomer component contained in component (A) and component (C) to 0.1% or more and 30% or less, the mass ratio of component (B) to 1% or more and 80% or less, and the mass ratio of the thermoplastic resin contained in component (A) to 10% or more and 95% or less, and this allows the design of physical properties of a wide range of materials according to the desires. Here, the mass ratio means the mass ratio relative to the mass of the resin composition of the present invention.
[0035] The total mass ratio of the elastomer component contained in component (A) and component (C) is preferably 1% or more, more preferably 5% or more, from the viewpoint of lowering the brittle temperature of the resin composition of the present invention. The total mass ratio of the elastomer component contained in component (A) and component (C) is preferably 30% or less, more preferably 27.5% or less, and even more preferably 25% or less, from the viewpoint of preventing the rigidity of the resin composition of the present invention from decreasing. In the present invention, the total mass ratio of the elastomer component contained in component (A) and component (C) is, in other words, the total mass ratio of the acid-modified elastomer and the non-acid-modified elastomer.
[0036] The total mass proportion of the elastomer component contained in component (A) and component (C) can be measured by the following method. <Method for measuring the total mass proportion of the elastomer component contained in component (A) and component (C)> Any known method can be used as the measurement method, but an example of the method is the CEF-TGIC method (Molding and Processing, Vol. 32, No. 2, 2020, pp. 33-37; Industrial Materials, Vol. 65, No. 5, 2017, pp. 31-36).
[0037] In the resin composition of the present invention, the lignocellulose fiber of component (B) plays a role of imparting a desired rigidity to the thermoplastic resin. Therefore, in order to make the resin composition of the present invention have a desired rigidity, the mass ratio of component (B) can be arbitrarily determined according to the rigidity of the thermoplastic resin contained in the resin composition. Thus, the mass ratio of component (B) can be arbitrarily determined, and examples of the mass ratio of component (B) are shown below. The mass ratio of component (B) is preferably 5% or more, more preferably 10% or more, from the viewpoint of improving the rigidity of the resin composition of the present invention, and is preferably 80% or less, more preferably 70% or less, from the viewpoint of preventing an increase in the brittle temperature of the resin composition of the present invention.
[0038] The mass proportion of component (B) can be measured by the following method. <Method for measuring the mass proportion of component (B)> Any known method can be used as the measurement method. Examples of the method include a method in which the resin component is dissolved in a hot solvent such as dichloromethane or xylene, and the residue after filtering is used as the lignocellulose fiber component, a method in which the specific gravity of the resin or elastomer is known and the specific gravity is calculated from the overall specific gravity, and a thermal analysis method such as DSC.
[0039] The mass proportion of the thermoplastic resin contained in component (A) varies depending on the mass proportions and types of other elastomer components coexisting during blending, but from the viewpoint of ensuring the desired rigidity, it is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more. Also, from the viewpoint of ensuring the desired brittle temperature, the mass proportion of the thermoplastic resin contained in component (A) is preferably 95% or less, more preferably 92.5% or less, and even more preferably 90% or less.
[0040] The mass proportion of the thermoplastic resin contained in component (A) can be measured by the following method. <Method for measuring the mass proportion of thermoplastic resin contained in component (A)> As the above measurement method, any known method can be used. Examples of the method include a method in which the resin component is dissolved in a hot solvent such as dichloromethane or xylene, and the mass of the filtered solution is used as the mass ratio, a method in which the CEF-TGIC method is applied in addition to the hot solvent dissolution method, a method in which the mass ratio is calculated from the total specific gravity, and a method in which the mass ratio is measured using a thermal analysis method such as DSC.
[0041] The mass proportion of component (C) is preferably 0.05% or more, more preferably 0.1% or more, and even more preferably 0.5% or more from the viewpoint of lowering the brittle temperature of the resin composition of the present invention, depending on the mass proportion and type of the elastomer component contained in component A. Also, the mass proportion of component (C) is 20% or less, more preferably 15% or less, and even more preferably 10% or less from the viewpoint of preventing a decrease in the rigidity of the resin composition of the present invention.
[0042] The mass proportion of component (C) can be measured by the following measurement method. <Method for measuring the mass proportion of component (C)> As the above measurement method, any known method can be used, and an example of the method is the CEF-TGIC method.
[0043] The resin composition of the present invention has low-temperature embrittlement resistance, and the embrittlement temperature of the resin composition of the present invention is preferably −15° C. or lower, more preferably −20° C. or lower, and even more preferably −25° C. or lower. The lower limit of the embrittlement temperature is not particularly limited, but can be, for example, −15° C. The embrittlement temperature can be measured, for example, in accordance with JIS K 7216 “Testing method for embrittlement temperature of plastics”.
[0044] The resin composition of the present invention has excellent mechanical properties, and the tensile modulus of the resin composition of the present invention is preferably 1.5 GPa or more, more preferably 1.75 GPa or more, and even more preferably 2.0 GPa or more. The lower limit of the tensile modulus is not particularly limited, but can be, for example, 1.5 GPa. <Method for measuring tensile modulus> As the above measurement method, any known method can be adopted, for example, JIS K7113 "Tensile test method for plastics" or JIS K7161 "Plastics - Test method for tensile properties" can be used.
[0045] The resin composition of the present invention may contain other components in addition to the components (A) to (C). Examples of the other components include acid-modified polyolefin resins, glass fibers, talc, calcium carbonate, basalt fibers, carbon fibers, polyester fibers, and aramid fibers. The acid-modified polyolefin resins will be described later. The specific gravity of the resin composition of the present invention is not particularly limited and varies depending on the blending ratio of components (A) to (C) and the presence or absence of other components. For example, the specific gravity of the resin composition of the present invention is preferably 0.7 to 1.7, more preferably 0.8 to 1.6, and even more preferably 0.9 to 1.5.
[0046] The bulk density of the resin composition of the present invention is not particularly limited and varies depending on the blending ratio of components (A) to (C) and the presence or absence of other components. For example, the bulk density of the resin composition of the present invention is preferably 100 kg / m 3 More than 800kg / m 3 Less than or equal to 150 kg / m 3 More than 700kg / m 3 More preferably, 200 kg / m or less 3 More than 600kg / m 3 The following is the result.
[0047] The bulk density can be measured by the following method. <Method of measuring bulk density> Any known method can be used to measure the bulk density, but it can also be calculated by putting the object to be measured into a container with a known volume, leveling the top surface, and calculating the bulk density from the volume of the container. For example, JIS K7365 "Plastics - How to determine the apparent density of materials that can be poured from a specified funnel" can be used.
[0048] The resin composition of the present invention may contain water. For example, the moisture content of the resin composition of the present invention at the time of trade is preferably 0% or more and 20% or less, more preferably 0% or more and 15% or less, and even more preferably 0% or more and 10% or less. Here, the moisture content at the time of trade means the state at the time of inspection before shipment from the manufacturing factory. The moisture content can be calculated by the following formula (1). Moisture content (%)={(mass of water contained in the resin composition of the present invention) / (total mass of the resin composition of the present invention)}×100 (1) The mass of water contained in the resin composition of the present invention can be measured by known methods such as a method in which the weight loss due to drying or the like is regarded as the water content, or a commercially available moisture meter (for example, a Karl Fischer moisture meter, etc.).
[0049] [Component (D): Acid-modified polyolefin resin] As described above, the resin composition of the present invention may further contain an acid-modified polyolefin resin (component (D)) in addition to the components (A) to (C). The acid-modified polyolefin resin is used as a compatibilizer, similar to the acid-modified elastomer. As the acid-modified polyolefin resin, preferably, maleic anhydride-modified polyolefin resin, more preferably, maleic anhydride-modified polyethylene resin or maleic anhydride-modified polypropylene resin can be mentioned, but the amount of acid groups is not particularly limited. In the present invention, these acid-modified polyolefin resins may be used alone or in combination of two or more.
[0050] As described above, when only an acidic polyolefin resin is used as a compatibilizer in a composition of lignocellulose fibers and a thermoplastic resin, the rigidity is improved, but the brittle temperature becomes higher than desired, making it difficult to balance the physical properties and the brittle temperature. However, as a result of intensive research by the present inventors, it was found that the increase in the brittle temperature can be suppressed by using an acid-modified elastomer and an acid-modified polyolefin resin in combination as a compatibilizer. In other words, by including an acid-modified polyolefin resin in addition to an acid-modified elastomer, the resin composition of the present invention can further increase the rigidity of the resin composition and suppress an excessive increase in the brittle temperature.
[0051] The mass proportion of component (D) is preferably 5% or less, more preferably 2.5% or less, and even more preferably 1% or less, from the viewpoint of ensuring that the effect of suppressing an increase in the brittle temperature is reliably achieved. Also, the mass proportion of component (D) is preferably 0.05% or more, more preferably 0.1% or more, and even more preferably 0.2% or more, from the viewpoint of ensuring that the effect of further increasing the rigidity of the resin composition is reliably achieved.
[0052] [Method for producing resin composition] Next, a method for producing the resin composition of the present invention will be described. The resin composition of the present invention is obtained by kneading a thermoplastic resin containing an elastomer (component (A)), a lignocellulose fiber (component (B)), and an acid-modified elastomer (component (C)). The kneading can be performed by a kneading device such as a multi-screw extruder, a high-pressure kneader, a Banbury mixer, a Henschel mixer, or a roll mill. The components (A) to (C) may be mixed in advance before being fed into the kneading device, or the components (A) to (C) may be fed from the same or different feed ports for the purpose of being mixed in the kneading device. For example, the component (A) may be fed into the kneading device first, and the thermoplastic resin contained in the component (A) may be melted, and then the components (B) and (C) may be fed into the kneading device one by one, or the components (A) to (C) may be fed into the kneading device simultaneously, and the components (A) to (C) may be kneaded while melting the thermoplastic resin contained in the component (A).
[0053] When component (A) is a mixture of an elastomer and a thermoplastic resin, in the method for producing a resin composition of the present invention, the elastomer and the thermoplastic resin may be charged from the same or different charging ports in order to be mixed in the kneading device. For example, the thermoplastic resin may be charged first into the kneading device, and after the thermoplastic resin is melted, the elastomer, component (B), and component (C) may be successively charged into the kneading device.
[0054] [Multi-screw extruder] In order to obtain the resin composition of the present invention, it is preferable to use a multi-screw extruder equipped with two or more screws. Multi-screw extruders that can be used to produce the resin composition of the present invention include twin-screw extruders equipped with two screws and multi-screw extruders equipped with three or more screws.
[0055] FIG. 1 shows a twin-screw extruder 1, which is an example of a multi-screw extruder that can be used to produce the resin composition of the present invention. The twin-screw extruder 1 includes a kneading screw 3, a cylinder 2, a heating device 8, a nozzle section 7 having an extrusion port 71, a material input section 6, and a degassing section (not shown) that vacuum-degassss the gas generated during kneading. The cylinder 2 has a kneading space in which the screw 3 is disposed. As shown in FIGS. 1 and 2, the twin-screw extruder 1 has two screws 3 rotatably arranged in parallel in the kneading space of the cylinder 2 with their screw shafts 31, which are the rotation shafts, being parallel to each other. As shown in FIG. 2, each of the screw shafts 31 is provided with screw blades 32 that mesh with each other. The heating device 8 includes a heating section 81 arranged in a plurality of parts along the axial direction of the cylinder 2 on the outer periphery of the cylinder 2. A plurality of heating sections 81 are installed along the axial direction of the cylinder 2 from the material input section 6 to the nozzle section 7. As the heating section 81, for example, a heater equipped with an electric heating wire, a heater through which a high-temperature heat medium flows, or the like can be used. The twin-screw extruder 1 is equipped with, for example, an electric motor as a drive source 4 for the two screws 3, and power is transmitted from the drive source 4 to the screw shafts 31 of the two screws 3 via a power transmission system 5 such as a gear mechanism, causing each of the two screw shafts 31 to rotate.
[0056] The twin-screw extruder 1 has a heating region Rh that can be heated by a heating device 8. The heating region Rh extends along the axial direction of the cylinder 2. In the twin-screw extruder 1 shown in FIG. 1, a heating section 81 of the heating device 8 is arranged in the heating region Rh. The heating region Rh can be divided into a plurality of sections S1 to S11 along the axial direction of the cylinder 2. Here, a section means a region in which the temperature can be set independently. The twin-screw extruder 1 shown in FIG. 1 is divided into eleven sections S1 to S11, and when the heating region Rh is viewed along the axial direction of the cylinder 2, one heating section 81 is arranged in each section. The number of heating sections 81 arranged in one section is not limited to one, and multiple heating sections 81 may be arranged in one section. In the twin-screw extruder 1, a heating section 81 is arranged in each section, so that the temperature can be set according to each stage of kneading and transporting the material. The number of sections is not limited to 11, and may be 1, or may be 2 to 10, or may be 12 or more.
[0057] A preferred embodiment of the method for producing a resin composition of the present invention will be described below by taking as an example a method for producing a resin composition using the above-mentioned twin-screw extruder 1. In the production method of this embodiment, a copolymer of an elastomer and a thermoplastic resin (hereinafter, simply referred to as "copolymer") is used as component (A). The copolymer may be in the form of a compression molded product, powder or granules, or fiber, but is preferably in the form of pellets. In the manufacturing method of this embodiment, the resin composition is manufactured by kneading the copolymer, the lignocellulose fibers, and the acid-modified elastomer, so that the mass ratio of the copolymer, the lignocellulose fibers, and the acid-modified elastomer used in the manufacturing process is the mass ratio of the copolymer, the lignocellulose fibers, and the acid-modified elastomer in the manufactured resin composition. Therefore, by setting the mass ratios of the copolymer, the lignocellulose fibers, and the acid-modified elastomer used in the manufacturing of the resin composition to predetermined values, the mass ratios of the copolymer, the lignocellulose fibers, and the acid-modified elastomer in the manufactured resin composition can be set to predetermined values.
[0058] The manufacturing method of this embodiment includes a kneading step, in which the copolymer A, the lignocellulose fibers B, and the acid-modified elastomer C are forcibly transferred by the rotation of the screw 3 toward the downstream side where the nozzle portion 7 is located. The kneading step of this embodiment includes a melting step and a low-temperature kneading step. The melting step is carried out in at least one section. In this embodiment, the melting step is carried out in the section S1. In the melting step, the set temperature of the heating section 81 is maintained at or above the melting point of the thermoplastic resin contained in the component (A), i.e., the melting point of the copolymer A, to melt the copolymer A and obtain a mixture of the molten copolymer A, the lignocellulose fiber B, and the acid-modified elastomer C. The number of sections in which the high-temperature kneading step is carried out may be one or more. In the melting step, after only the copolymer A is melted alone, the molten copolymer A, the lignocellulose fiber B, and the acid-modified elastomer C may be mixed. Also, after the copolymer A containing the lignocellulose fiber B is melted, the molten copolymer A, the lignocellulose fiber B, and the acid-modified elastomer C may be mixed. Also, after the copolymer A containing the acid-modified elastomer C is melted, the molten copolymer A, the lignocellulose fiber B, and the acid-modified elastomer C may be mixed. Also, after the copolymer A containing the acid-modified elastomer C is melted, the molten copolymer A, the lignocellulose fiber B, and the acid-modified elastomer C may be mixed. The copolymer A containing the lignocellulose fibers B and the acid-modified elastomer C may be melted, and then the molten copolymer A, the lignocellulose fibers B, and the acid-modified elastomer C may be mixed together.
[0059] The low-temperature kneading step is carried out after the melting step. The melting step is carried out in at least one section. In this embodiment, the low-temperature kneading step is carried out in sections S2 to S11. In the low-temperature kneading step, the mixture obtained in the melting step is kneaded while maintaining the set temperature of the heating section 81 at a temperature lower than the melting point of the copolymer A. In this embodiment, after the low-temperature kneading step, the mixture is discharged from the extrusion port 71 to obtain a resin composition E. The number of sections in which the low-temperature kneading step is carried out may be one or more.
[0060] In this embodiment, it is preferable to provide a pelletizing step in which the mixture is discharged from the extrusion port 71 after the kneading step, and then the discharged resin composition E is cut in the length direction and pelletized. By providing the pelletizing step, it becomes possible to use the resin composition E efficiently. In the pelletizing step, the resin composition E can be cut by known methods such as hot cutting in which the resin composition E is cut without being cooled in a water tank, a method in which the resin composition E is air-cooled or water-cooled and then cut, a method in which the resin composition E is discharged into water and then cut in water, etc. The discharged resin composition E can be cut to a desired length.
[0061] The manufacturing method of this embodiment has a low-temperature kneading step, which can reduce the thermal history of the lignocellulose fibers B. By reducing the thermal history of the lignocellulose fibers B, it is possible to suppress embrittlement of the lignocellulose fibers B themselves due to thermal oxidation and thermal denaturation. In addition, since the temperature of the strand of resin composition E discharged from the kneading device 1 can be reduced, it is possible to suppress the phenomenon that thermoplastic resins containing elastomers become soft and easily cut, and it is also possible to suppress the degradation of the molecular weight of the thermoplastic resin due to thermal decomposition and the associated deterioration in mechanical properties. As described above, according to the manufacturing method of this embodiment, a resin composition having excellent mechanical properties and low-temperature embrittlement resistance can be efficiently manufactured.
[0062] In the manufacturing method of this embodiment, the ratio of the number of sections performing the low-temperature kneading process to the number of sections performing the process after the melting process (hereinafter also referred to as the section ratio) is preferably 15% or more and 100% or less, more preferably 20% or more and 100% or less, and even more preferably 25% or more and 100% or less. By setting the section ratio within the above range, the effect of efficiently and easily obtaining the resin composition of the present invention can be more significantly achieved. The section ratio can be calculated by the following formula (2). Compartment ratio (%) = {(number of compartments performing the low-temperature kneading process) ÷ (number of compartments performing processes after the melting process)} × 100 (2)
[0063] In the manufacturing method of this embodiment, the ratio of the time required for passing through the section in which the low-temperature kneading step is performed to the time required for passing through the section in which the steps subsequent to the melting step are performed is preferably 10% or more and 100% or less, more preferably 15% or more and 100% or less, and even more preferably 20% or more and 100% or less. By setting the ratio of the time within the above range, the effect of being able to efficiently and easily obtain the resin composition of the present invention can be more significantly achieved. The ratio of the time can be calculated by the following formula (3). The ratio of the time (%) = {(time required to pass through the section where the low-temperature kneading process is performed) ÷ (time required to pass through the section where the process after the melting process is performed)} × 100 (3)
[0064] It is known that when exposed to high temperatures, lignocellulosic materials lose their flexible affinity between molecules due to oxidation or modification of functional groups, and become more brittle. Therefore, by setting the partition ratio and the time ratio within the above-mentioned ranges, it is possible to suppress the embrittlement of the fibers due to the oxidation or modification of the lignocellulosic fibers, and as a result, it is possible to more effectively suppress an undesirable increase in the embrittlement temperature. In addition, since thermoplastic resins containing elastomers are easily cut by heat, the resin composition E is easily cut when discharged from the kneading device 1, but by setting the partition ratio and the time ratio within the above-mentioned ranges, it is possible to suppress an increase in the resin temperature, and therefore it is possible to maintain high kneading workability.
[0065] In the manufacturing method of this embodiment, a copolymer of an elastomer and a thermoplastic resin is used as component (A), but a mixture of an elastomer and a thermoplastic resin may be used as component (A). In addition, in the melting step, the thermoplastic resin may be melted in a state of being a mixture of the elastomer and the thermoplastic resin, and then the molten resin composition, the elastomer, the lignocellulose fiber B, and the acid-modified elastomer C may be mixed. In the melting step, the thermoplastic resin may be melted alone, and then the molten thermoplastic resin, the elastomer, the lignocellulose fiber B, and the acid-modified elastomer C may be mixed.
[0066] When a mixture of an elastomer and a thermoplastic resin is used as component (A), the form of the thermoplastic resin may be a compression molded product, powder, granules, or fiber, but is preferably pelletized, and the form of the elastomer may be powder or pelletized. In addition, when a resin composition containing components other than the components (A) to (C) is produced, the other components can be added at any timing in the kneading step of the production method of this embodiment. For example, the other components may be added in the melting step or the low-temperature kneading step, or the components (A) to (C) and the other components may be mixed in advance before being charged into the kneading apparatus 1.
[0067] [Fiber reinforced resin material] The resin composition of the present invention contains lignocellulosic fibers that are renewable, lightweight, highly elastic, and have excellent LCA evaluation, and thus when used as a fiber-reinforced resin material, it exhibits excellent weight reduction effects, reinforcement effects, and LCA improvement effects, making it possible to obtain a high-performance fiber-reinforced resin material. Therefore, the resin composition of the present invention can be suitably used in the transportation industrial equipment sector, particularly in the automobile industry sector. In addition, the resin composition of the present invention can be used as a fiber-reinforced resin material for various applications other than industrial transportation and mobile equipment such as automobiles, trucks, aircraft, ships, drones, etc., such as industrial and household electrical appliances, construction and civil engineering products, store and office furniture and fixtures, stationery, and household goods.
[0068] The entire fiber-reinforced resin material constituting the final product may be the resin composition of the present invention, or a part of the fiber-reinforced resin material constituting the final product may be the resin composition of the present invention. For example, in the final product, only the part that should have both mechanical properties and low-temperature embrittlement resistance may be formed from the resin composition of the present invention. In addition, when the final product is composed of multiple components, one or more of the multiple components may be made of the resin composition of the present invention.
[0069] To the fiber-reinforced resin material containing the resin composition of the present invention, various additives such as preservatives, insect repellents, mildew inhibitors, water repellents, ultraviolet absorbers, flame retardants, fillers, coupling agents (organic silanate coupling agents, organic titanate coupling agents), rubbers, elastomers, defoamers, foaming agents, lubricants, pigments, dyes, waxes, release agents, flow improvers, strand strengtheners, antioxidants, adsorbents, deodorants, odor eliminators, and VOC reducers can be added within a range that does not impair the effects of the present invention. These may be used alone or in combination of two or more.
[0070] It goes without saying that the fiber-reinforced resin material includes not only the final product, but also the raw materials used to manufacture the product, such as a composition of lignocellulose fibers and resin, an intermediate in the process of manufacturing a composition of lignocellulose fibers, resin, elastomer, and compatibilizer, and a mixture of these. The resin composition of the present invention may be sold as a composition, an intermediate such as a master batch for dilution, a final molded product, or an aggregate or combination including a molded product, including, for example, a case where a block copolymer polypropylene and a homopolypropylene are mixed to design the desired physical properties. The mass ratio of the resin composition of the present invention in the fiber reinforced resin material is preferably 5% or more, more preferably 7.5% or more, and even more preferably 10% or more. By setting the mass ratio of the resin composition of the present invention in the fiber reinforced resin material within the above range, the effect of achieving both mechanical properties and low-temperature embrittlement resistance in the fiber reinforced resin material can be more reliably achieved.
[0071] Although the preferred embodiments of the present invention have been shown and described above, the inventions are not limited to the above-described embodiments and can be modified as appropriate. EXAMPLES
[0072] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way. [Production of a composition containing an elastomer-containing resin, lignocellulose fibers, and an acid-modified elastomer] Wood fiber (called thermomechanical pulp or fiber for MDF) mainly made of radiata pine, elastomer, thermoplastic resin, acid-modified elastomer, etc. were appropriately mixed, and pellets made of the resin composition of Examples 1 to 11 and Comparative Example 1 were produced by the manufacturing method of the above-mentioned embodiment. The composition of the materials used in the production of each pellet is as shown in Table 1. In Examples 1 to 10 and Comparative Example 1, a copolymer of polypropylene and EPR, lignocellulose fiber, acid-modified elastomer, acid-modified polyolefin resin, and other components were kneaded, and in Example 11, polypropylene (homo) and EPDM, lignocellulose fiber, acid-modified elastomer, acid-modified polyolefin resin, and other components were kneaded. In Examples 1 to 3, 5, and 7, EPDM or SEBS was also mixed in addition to the copolymer.
[0073] [Table 1]
[0074] In the pelletizing step, the resin composition was cut by cooling it with water and then cutting it. The set temperatures of each section when producing the compositions of Examples 1 to 11 and Comparative Example 1 are as shown in Table 2. In Table 2, section S11 is the nozzle. The set temperatures of sections before section S1, where no temperature was set, are omitted from Table 2. The screw rotation speed when producing the resin compositions of Examples 1 to 11 and Comparative Example 1 was set to 250 rpm.
[0075] [Table 2]
[0076] [Test specimen] The pellets of Examples 1 to 11 and Comparative Example 1 were molded by an injection molding machine into a flat plate shape of 2 mm thick × 100 mm long × 100 mm wide or a dumbbell shape conforming to the following standards to produce test specimens. The produced test specimens were either used as is or cut into the size to be used for each test, and the following mechanical property tests and brittle temperature tests were carried out.
[0077] [Mechanical property testing] The tensile test was performed in accordance with JIS K7161, and the bending test was performed in accordance with JIS K7171. [Brittleness temperature test] The brittle temperature test was carried out in accordance with JIS K7216.
[0078] 〔result〕 The results of the mechanical property tests and the brittle temperature tests are shown in Table 3. In Examples 1 to 11, the tensile modulus was 1.5 GPa (1500 MPa) or more and the brittle temperature was -15°C or less, and in Examples 1 to 11, a resin composition with an excellent balance between mechanical properties and brittle temperature was realized using wood fibers. In addition, in Example 7, in addition to the acid-modified elastomer, an acid-modified polypropylene resin is blended. In Example 7 as well, it is possible to successfully improve the bending strength while maintaining the brittle temperature at or below a desired temperature (e.g., -15°C). In addition, in Example 11, an elastomer is added to the homopolypropylene during kneading, and a resin composition having an excellent balance between mechanical properties and brittle temperature is realized using wood fibers, similar to the block copolymer polypropylenes in Examples 1 to 10. Furthermore, in Comparative Example 1, although an acid-modified polypropylene resin is used, no acid-modified elastomer is blended, and therefore, although the mechanical properties are excellent, the brittle temperature is higher than the desired temperature (e.g., -15°C). Therefore, it is understood that the resin composition of the present invention has an excellent balance between mechanical properties and brittle temperature.
[0079] [Table 3] [Explanation of symbols]
[0080] 1 Twin screw extruder 2 Cylinder 3 Screw 31 Screw shaft 32 Screw blade 4. Power Source 5 Power transmission system 6 Material input section 7 Nozzle section 71 Extrusion port 8 Heating device 81 Heating section A Copolymer of elastomer and thermoplastic resin B. Lignocellulosic fibers C Acid-modified elastomer E. Resin composition
Claims
1. Contains the following components (A) to (C): the total mass ratio of the elastomer component contained in the following component (A) and the following component (C) is 0.1% or more and 30% or less, The mass ratio of the following component (B) is 1% or more and 80% or less, A resin composition for fiber reinforced resin, comprising the following component (A): a thermoplastic resin having a mass ratio of 10% or more and 95% or less. (A) Thermoplastic resin containing elastomer (B) Lignocellulosic fibers (C) Acid-modified elastomer
2. The resin composition according to claim 1, wherein the thermoplastic resin in the component (A) is one or more selected from the group consisting of polypropylene, modified resins thereof, and copolymer resins thereof.
3. 2. The resin composition according to claim 1, wherein the elastomer in the component (A) is one or more selected from the group consisting of ethylene propylene copolymer elastomers, ethylene butene copolymer elastomers, ethylene octene copolymer elastomers, ethylene propylene diene copolymer elastomers, and hydrogenated styrene butadiene styrene block elastomers.
4. The resin composition according to claim 1, wherein the component (C) is one or more acid-modified compounds selected from the group consisting of ethylene-propylene copolymer elastomers, ethylene-butene copolymer elastomers, ethylene-octene copolymer elastomers, ethylene-propylene-diene copolymer elastomers, and hydrogenated styrene-butadiene-styrene block elastomers.
5. The resin composition according to claim 1, further comprising the following component (D): (D) Acid-modified polyolefin resin
6. The resin composition according to claim 1, having a brittle temperature of -15°C or lower and a tensile modulus of elasticity of 1.5 GPa or higher.
7. A method for producing a resin composition, comprising the steps of: producing the resin composition according to any one of claims 1 to 6 using a multi-screw extruder having two or more screws; The multi-screw extruder includes a cylinder having a kneading space therein in which the screws are disposed, and a heating device including a plurality of heating sections disposed on the outer periphery of the cylinder along the axial direction of the cylinder, The method includes a step of melting the component (A) at a temperature equal to or higher than the melting point of the thermoplastic resin contained in the component (A), and a step of kneading the component (A) containing the melted thermoplastic resin, the component (B), and the component (C) while maintaining the set temperature of the heating section below the melting point of the thermoplastic resin, or A method for producing a resin composition for fiber-reinforced resin, comprising: a step of melting a thermoplastic resin at a temperature equal to or higher than the melting point of the thermoplastic resin; and a step of kneading the molten thermoplastic resin, an elastomer, the component (B), and the component (C) while maintaining the set temperature of the heating section below the melting point of the thermoplastic resin.
8. A pellet comprising the resin composition according to any one of claims 1 to 6.
9. A fiber-reinforced resin material comprising the resin composition according to any one of claims 1 to 6.
10. A molded article made of the resin composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Polyolefin-based resin composition and wood meal to be used therein
JP1999286583A
Thermoplastic resin composition, method for producing it, and molded product of the same
JP2010001442A
High-toughness polyamide-cellulose resin composition
JP2020029488A
Highly tough polyamide-cellulose resin composition
JP2022007985A
Cellulose fiber-reinforced polyolefin-based resin composition and resin molded article
JP2022156073A