Lithium composite oxide and production method thereof

A lithium composite oxide with controlled particle size distribution and zigzag layered structure improves electrical conductivity and capacity by optimizing particle size and crystal structure through controlled production processes.

JP2024151837APending Publication Date: 2024-10-25NAT UNIV CORP YOKOHAMA NAT UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023065577
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Lithium composite oxides like LiMnO2, used as positive electrode active materials for lithium secondary batteries, suffer from wide particle size distribution due to mechanical milling, which impedes the formation of conductive paths and reduces electrical conductivity.

Method used

A lithium composite oxide with a controlled particle size distribution, characterized by a specific span value (1.0 ≤ S ≤ 5.0) and a zigzag layered structure, is produced through a process involving slurry preparation, spray drying, and heat treatment in an inert gas, ensuring optimal particle sizes and crystal structure.

Benefits of technology

The solution enhances the electrical conductivity of the electrode, enabling rapid activation and high capacity without the need for an initial charge/discharge cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151837000004
    Figure 2024151837000004
  • Figure 2024151837000005
    Figure 2024151837000005
  • Figure 2024151837000006
    Figure 2024151837000006
Patent Text Reader

Abstract

To provide a lithium composite oxide and a production method thereof, which control the particle size distribution for the purpose of improving the electric conductivity of an electrode.SOLUTION: A lithium composite oxide has a composition of LixMnO2 (0.80≤x≤1.20), a zigzag layered structure as the mother structure, and a domain of α-NaFeO2 type layered structure, and a span value S obtained by the following formula (1) is between 1.0 and 5.0, and a production method relates to the lithium composite oxide. S is expressed by the formula 1(D90-D10) / D50) (In Formula (1), D10, D50, and D90 are the cumulative 10% particle diameter, cumulative 50% particle diameter, and cumulative 90% particle diameter, respectively, of the volume-based particle size distribution).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a lithium composite oxide and a method for producing the same, and more particularly to a lithium composite oxide having a controlled particle size distribution and a method for producing the same. [Background technology]

[0002] Lithium composite oxides are generally used as the positive electrode active material for lithium secondary batteries. Lithium composite oxides, specifically lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), etc., are widely used as the positive electrode active material for lithium secondary batteries distributed around the world. Active research is being conducted on these lithium composite oxides to improve their characteristics (higher capacity, higher output, cycle stability) and safety.

[0003] Regarding performance improvement through improvement of the characteristics of positive electrode active materials for lithium secondary batteries, for example, increasing capacity has been attracting attention, and a lithium composite oxide represented by LiMnO2, which has a crystal structure with a zigzag layered structure as a parent structure and has an α-NaFeO2 type layered structure domain (Patent Document 1) has been disclosed. Patent Document 2 and Patent Document 3 disclose a LiMnO2 type compound characterized by being composed of at least one of orthorhombic and monoclinic crystals, and the discharge capacity of a lithium ion secondary battery produced using the compound was low at about 170 mAh / g. Patent Document 1 discloses that the crystal structure was changed by a process of heat treatment after mechanical milling, and the discharge capacity was improved to 260 mAh / g. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6956039 [Patent Document 2] JP 2003-007297 A [Patent Document 3] JP 2002-145619 A Summary of the Invention [Problem to be solved by the invention]

[0005] Such LiMnO2-type compounds are high-capacity yet inexpensive positive electrode active materials for lithium secondary batteries. However, when mechanical milling is applied to LiMnO2-type compounds, the particle size distribution becomes broad, which hinders the formation of conductive paths and reduces the electrical conductivity of the electrode. The present disclosure aims to improve the electrical conductivity of an electrode and provides a lithium composite oxide with a controlled particle size distribution and a method for producing the same. [Means for solving the problem]

[0006] The present invention is as described in the claims, and the gist of the present disclosure is as follows. [1] Composition formula Li x A lithium composite oxide represented by the formula MnO2 (where 0.80≦x≦1.20), having a zigzag layered structure as a parent structure and an α-NaFeO2 type layered structure domain, and further having a span value S obtained by the following calculation formula (1) of 1.0 or more and 5.0 or less. S=(D 90 -D 10 ) / D 50 (1) (In formula (1), D 10 , D 50 and D. 90 indicate the cumulative 10% particle size, cumulative 50% particle size, and cumulative 90% particle size in the volume-based particle size distribution, respectively.) [2] D in the above formula (1) 50 The lithium composite oxide according to the above [1], wherein the average particle size is 5 μm or more and 15 μm or less. [3] The lithium composite oxide according to the above [1] or [2], wherein the intensity ratio (A / B) between the integrated intensity (A) of a diffraction peak observed at 2θ=15.3±1.0° and the integrated intensity (B) of a diffraction peak observed at 2θ=18.2±1.0° in a powder X-ray diffraction pattern is 0.5 or more. [4] A method for producing the lithium composite oxide according to any one of the above [1] to [3], comprising the steps of: mixing lithium hydroxide, manganese oxide or manganese oxyhydroxide, and water to prepare a slurry; evaporating the water from the obtained slurry to produce granular dry particles; and heat-treating the granular dry particles obtained in the above step in an inert gas. [5] The method for producing a lithium composite oxide according to the above [4], wherein water is evaporated by spray drying in the step of preparing the granular dry particles. [6] An electrode comprising the lithium composite oxide according to any one of the above [1] to [3] as a positive electrode active material. [7] A lithium secondary battery comprising the electrode described in [6] above. Effect of the Invention

[0007] By using the lithium composite oxide of the present disclosure as a positive electrode active material for a lithium secondary battery, it is possible to provide an electrode having higher electrical conductivity than conventional ones. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic diagram showing a zigzag layered structure. [Diagram 2] Schematic diagram showing a layered structure (2a) and a rock salt structure (2b). [Diagram 3] FIG. 2 is a diagram showing XRD patterns of the lithium composite oxides of Examples 1 to 3. [Figure 4] 1 is a graph showing particle size distributions of the lithium composite oxides of Examples 1 to 3. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment for carrying out the present disclosure (hereinafter referred to as the "present embodiment") will be described in detail by taking an example. The present embodiment is an example for explaining the present disclosure, and is not intended to limit the present disclosure to the following content. The present disclosure can be carried out by appropriately modifying it. In the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in a certain numerical range. In addition, in the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0010] The lithium composite oxide of the present embodiment has the composition formula Li x MnO2 (where 0.80≦x≦1.20). In the above composition formula, 0.90≦x≦1.10 is preferable, and 0.95≦x≦1.05 is more preferable.

[0011] The lithium composite oxide of the present embodiment has a zigzag layer structure as a base structure and an α-NaFeO2 type layer structure domain. By having such a structure, it is possible to exhibit high capacity from the initial cycle without requiring an initial activation charge-discharge cycle, which is advantageous over orthorhombic LiMnO2, which exhibits high capacity only after activation by performing several tens of charge-discharge cycles.

[0012] A schematic diagram of the zigzag layered structure is shown in Figure 1. Schematic diagrams of the layered structure and the rock salt type structure are shown in Figure 2 (2a) and (2b), respectively. As can be seen from Figures 1 and 2, the zigzag layered structure is a crystal structure in which the layers in the α-NaFeO2 type layered structure grow regularly, alternating up and down, to form a zigzag layered structure.

[0013] The lithium composite oxide of this embodiment has a span value S obtained by the following formula (1) of 1.0 or more and 5.0 or less. S=(D 90 -D 10 ) / D 50 (1) (In the formula, D 10 , D 50 and D. 90 indicate the cumulative 10% particle size, cumulative 50% particle size, and cumulative 90% particle size in the volume-based particle size distribution, respectively.)

[0014] In the volume-based particle size distribution, the cumulative 10% particle size, the cumulative 50% particle size, and the cumulative 90% particle size are particle sizes at which the cumulative values ​​from the small particle side are 10 volume%, 50 volume%, and 90 volume%, respectively. In this embodiment, the volumetric particle size distribution may be measured using a slurry in which a sample is placed in pure water, using a general laser diffraction / scattering particle size distribution measuring device (e.g., MT3000II series, manufactured by MicrotracBEL) under the following conditions. [Measurement conditions] Calculation mode: HRA Measurement time: 30 seconds Solvent refractive index: 1.33 Refractive index of powder sample: 2.46

[0015] The above span value S is an index showing the spread of the particle size distribution of the lithium composite oxide, and the lower the value, the smaller the variation in particle size of the lithium composite oxide. In the lithium composite oxide of this embodiment, the calculation formula (D 90 -D 10 ) / D 50 The span value S, expressed as:

[0016] By keeping the span value S within the above range, a lithium composite oxide with a controlled particle size distribution can be obtained, and the electrical conductivity of the resulting electrode can be improved without impeding the formation of a conductive path. If the span value S is outside this range, coarse particles are included. Since electrical conduction within the particles is slower than that of the conductive material, the electrical conductivity of the electrode decreases when coarse particles are included. On the other hand, when fine particles are present, the amount of active material that cannot participate in charge and discharge increases, and the electrical conductivity of the electrode decreases. The span value S is preferably in the range of 1.0 or more and 3.0 or less, and more preferably in the range of 1.0 or more and 2.5 or less.

[0017] D in formula (1) 50 is preferably 5 μm or more and 15 μm or less, and more preferably 8 μm or more and 12 μm or less. D in formula (1) 50When D is equal to or less than the upper limit of the above range, the electrical conductivity of the active material particles is increased, and the conductivity of the electrode is improved. 50 When the surface area of ​​the active material particles is increased by being equal to or larger than the lower limit of the above range, good conductive paths connecting the active material particles to each other are easily formed.

[0018] D in formula (1) 90 is preferably 50 μm or less, more preferably 10 μm or more and 50 μm or less, and further preferably 15 μm or more and 30 μm or less. D in formula (1) 90 When the content is within the above range, the generation of coarse secondary particles is suppressed, and the electrical conductivity is likely to be high.

[0019] D in formula (1) 10 is preferably 1 μm or more, more preferably 1 μm or more and 10 μm or less, and further preferably 1 μm or more and 5 μm or less. D in formula (1) 10 When the amount of fine particles is small, the amount of active material not involved in charge and discharge, i.e., the active material not connected to the conductive path, can be reduced, and the electrical conductivity of the electrode can be more easily improved.

[0020] In the lithium composite oxide of the present embodiment, it is preferable that the intensity ratio (A / B) between the integrated intensity (A) of the diffraction peak observed at 2θ=15.3±1.0° and the integrated intensity (B) of the diffraction peak observed at 2θ=18.2±1.0° in powder X-ray diffraction under the following measurement conditions is 0.5 or more.

[0021] [Measurement conditions] ·X-ray source: CuKα ray = 1.5418Å Output: 1.6kW (40mA-40kV) Divergence slit: 1° Vertical limit divergence slit: 10mm Scattering slit: open Receiving slit: open Scan width: 0.04°(2θ / θ) Scan speed: 4° / min Measurement range: 10~90°(2θ / θ)

[0022] If the intensity ratio (A / B) is 0.5 or more, the main phase has a zigzag layer structure as a base structure and an α-NaFeO2 type layer structure coexists, so that activation is fast and a high capacity can be obtained. The intensity ratio (A / B) is more preferably 1.0 to 150.0, and even more preferably 2.0 to 50.0. When the intensity ratio (A / B) is within the above range, a crystal structure in which a zigzag layer structure and an α-NaFeO2 type layer structure coexist is adopted, which is preferable because it allows for a lithium composite oxide with rapid activation and high capacity to be obtained.

[0023] The BET specific surface area of ​​the lithium composite oxide of this embodiment is 2.0 m 2 / g or more 20.0m 2 / g or less, and 3.0m 2 / g or more 10.0m 2 It is more preferable that the molecular weight is not more than 1 / g. If the BET specific surface area is within the above range, the lithium composite oxide slurry has a good viscosity, which is preferable in terms of handling. In addition, when the lithium composite oxide is used as a positive electrode active material for a lithium secondary battery, it is possible to obtain excellent charge / discharge characteristics at high temperatures and excellent output characteristics. In the lithium composite oxide of this embodiment, the specific surface area is an important factor for achieving high capacity without undergoing a long-term activation cycle. By setting the BET specific surface area value to the lower limit of the above range or more, a lithium composite oxide with a high capacity can be obtained.

[0024] The BET specific surface area of ​​the lithium composite oxide can be determined by a method, which is known as the BET method, in which an adsorption isotherm determined from physical gas adsorption based on JIS Z 8830 is converted into a BET plot, the amount of gas adsorption Vm of a monolayer is determined based on the BET isotherm, and the specific surface area is calculated based on the molecular size of the gas used for physical adsorption.

[0025] The lithium composite oxide of the present embodiment can be produced by carrying out a step of mixing lithium hydroxide, manganese oxide or manganese oxyhydroxide, and water to prepare a slurry, a step of evaporating water from the obtained slurry to produce granular dry particles, and a step of heat-treating the granular dry particles obtained in the above step in an inert gas.

[0026] The type of lithium hydroxide used in the step of preparing the slurry is not particularly limited, but examples include hydrates such as lithium hydroxide monohydrate (LiOH·H2O) and anhydrous forms such as anhydrous lithium hydroxide (LiOH). Among these, lithium hydroxide monohydrate is preferred from the viewpoints of being able to be handled under air and reducing errors due to water contamination during synthesis. The type of manganese oxide used in the step of preparing the slurry is not particularly limited, and examples thereof include one or more selected from the group consisting of MnO2, Mn2O3, MnO2, Mn3O4, and Mn2O7. Among these, Mn2O3 is preferred from the viewpoint of preventing a change in valence in the subsequent firing step.

[0027] After the step of preparing the slurry, pulverization and mixing may be performed. The pulverizer used in the pulverization and mixing may be at least one selected from the group consisting of a wet medium stirring mill, a ball mill, a vibration mill, a jet mill, and a planetary mill.

[0028] In the process of producing granular dry particles, spray drying is preferably carried out as a method for evaporating water. Spray drying can be performed using a spray dryer that sprays the slurry and dries the droplets with hot air. As a granulation method, methods other than spray drying, such as at least one of a submerged granulation method and a tumbling granulation method, can be used, but spray drying is the most industrially advantageous.

[0029] The treatment temperature and treatment time in the step of heat treatment in an inert gas are not particularly limited, but are preferably performed at 500°C or higher and 900°C or lower for 30 minutes to 6 hours, and more preferably at 600°C or higher and 800°C or lower for 1 hour to 4 hours. The inert gas used may be, for example, at least one of nitrogen and argon.

[0030] The electrode (positive electrode) of this embodiment only needs to contain the lithium composite oxide of this embodiment as a positive electrode active material, and preferably further contains a conductive material, a binder, and a current collector in addition to the lithium composite oxide.

[0031] The conductive material is added to improve the conductivity of the electrode. The conductive material is not particularly limited, but examples thereof include at least one carbon black such as acetylene black and ketjen black. It is preferable in terms of improving the output characteristics of the battery that the conductive material is uniformly distributed around the positive electrode active material to form a network through which electrons flow.

[0032] The content of the conductive material relative to the lithium composite oxide in the electrode of this embodiment is not particularly limited, but is preferably 1% by mass or more and 10% by mass or less.

[0033] The binder may be any binder that can be used in electrodes for lithium secondary batteries, and examples thereof include one or more selected from the group consisting of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl fluoride (PVF), polyvinyl chloride (PVC), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR), but are not particularly limited thereto.

[0034] The content of the binder in the electrode of the present embodiment is not particularly limited, but is preferably, for example, from 1% by mass to 10% by mass. The current collector may be any conductor whose surface in contact with the positive electrode composite layer exhibits electrical conductivity, and may be one or more selected from the group consisting of copper, gold, aluminum, titanium, nickel, stainless steel, and alloys thereof, indium oxide, tin oxide, and conductive carbon. There is no particular limitation on the shape of the current collector, and examples of such shapes include foil, film, sheet, net, expanded metal, and punched metal. There is also no particular limitation on the thickness of the current collector, and examples of such shapes include 1 to 100 μm.

[0035] The electrode (positive electrode) of this embodiment can be produced by a known method. For example, The material, conductive material, and binder are mixed uniformly, and the resulting positive electrode mixture ink is applied to the surface of a current collector, followed by drying.

[0036] The lithium secondary battery of this embodiment has, in addition to the above-mentioned positive electrode, a negative electrode, an electrolyte, a separator, and the like. The negative electrode is made of a material that reversibly absorbs and releases Li, such as a carbon-based material, a tin oxide-based material, a silicon oxide-based material, or Li4Ti5O 12 , and one or more materials that form an alloy with Li can be mentioned.

[0037] Examples of the electrolyte include an organic electrolyte solution in which Li salts or various additives are dissolved in an organic solvent, an ionic liquid, a Li-ion conductive solid electrolyte, and a combination of these. The organic solvent of the electrolyte is not particularly limited, but may be one or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), and diethyl carbonate (DEC). The electrolyte may be tetrafluoroborate (BF4 - ), hexafluorophosphate (PF6 - ), fluoromethanesulfonylimide (FSI - ), trifluoromethanesulfonylimide (TFSI - ) and trifluoromethanesulfonate (CF3SO3 - ) group, but there is no particular limitation.

[0038] There is no particular limitation on the separator, and known ones can be used. For example, a sheet of polyethylene, polypropylene, or a composite material thereof can be mentioned.

Examples

[0039] Hereinafter, the examples of the present disclosure will be given and described in more detail, but the present disclosure is not to be construed as being limited to these examples. Example 1 and Example 2 are examples, and Example 3 is a comparative example.

[0040] <Identification of crystal structure> Powder X-ray diffraction (hereinafter also referred to as "powder XRD") was performed using a powder X-ray diffractometer (trade name: UltimaIV, manufactured by Rigaku Corporation) to identify the crystal structure of the lithium composite oxide. The measurement conditions in powder XRD were as follows. · X-ray source: CuKα ray = 1.5418 Å · Output: 1.6 kW (40 mA - 40 kV) · Divergence slit: 1° · Divergence vertical limit slit: 10 mm · Scattering slit: Open · Receiving slit: Open · Scan speed: 4° / min · Scan width: 0.04° (2θ / θ) · Measurement range: 10 to 90° (2θ / θ)

[0041] <Composition analysis> After the sample was heated and dissolved in a hydrochloric acid - hydrogen peroxide mixed aqueous solution, the composition of the lithium composite oxide sample was analyzed using an inductively coupled plasma optical emission spectrometer (trade name: OPTIMA5300DV, manufactured by PerkinElmer Japan).

[0042] <Measurement of BET specific surface area> 0.3 g of the sample was placed in a glass cell for BET specific surface area measurement, and dehydration treatment was performed at 150°C for 30 minutes under a nitrogen stream to remove the moisture adhering to the powder particles. The treated sample was then placed in a B The BET specific surface area was measured by the BET flow method (one-point method) based on JIS Z 8830 using an ET measurement device (product name: MiCROMETRICS DesorbIII, manufactured by Shimadzu Corporation) and a mixed gas of 30% nitrogen and 70% helium as the adsorption gas.

[0043] <Measurement of particle size distribution> A particle size distribution based on volume was obtained using a particle size distribution analyzer (product name: MT3000II series, manufactured by MicrotracBEL Co., Ltd.) The particle size distribution was measured after adding an appropriate amount of pure water to the powder sample and subjecting it to ultrasonic dispersion for 5 minutes. The sample was dispersed using the sample circulator attached to the instrument and measurements were performed under the following conditions. Particle size was calculated using the software attached to the instrument. [Measurement conditions] Calculation mode: HRA Measurement time: 30 seconds Solvent refractive index: 1.33 Refractive index of powder sample: 2.46 The span value is known as an index that indicates the spread of particle size distribution. The span value is calculated using the following formula: (D 90 -D 10 ) / D 50 However, D 10 , D 50 and D. 90 are the cumulative 10% particle size, the cumulative 50% particle size, and the cumulative 90% particle size in the volume-based particle size distribution, respectively.

[0044] <Preparation of electrodes> The lithium composite oxide obtained in Examples 1 to 3, the conductive material (Denka black, manufactured by Denka Co., Ltd.), and the binder (10 wt% PvdF / N-Methyl-2-Pyrrolidone solution) were mixed and homogenized using a mixer (AR-100, manufactured by Thinky Co., Ltd.) at a mass ratio of lithium composite oxide:conductive material:binder = 80:10:10 to prepare a positive electrode composite ink. The obtained positive electrode composite ink was applied to an aluminum foil serving as a current collector to a thickness of 125 μm, dried at 80 °C for 30 minutes, further dried under reduced pressure at 150 °C for 1 hour or more, and then cut into a circle with a diameter of 15.956 mm. The circular electrode after cutting was uniaxially pressed at 3 ton / cm 2 and dried under reduced pressure at 150 °C for 2 hours to fabricate an electrode.

[0045] <Measurement of Electrode Electrical Conductivity> The electrode electrical conductivity was evaluated by the alternating current impedance method. The circular electrode was sandwiched between an SH2-Z type four-terminal sample holder (manufactured by Toyo Technica), and alternating current impedance measurement was performed using a potentiostat (product name: SI1287, manufactured by Solartron) and a frequency response analyzer (product name: SI1260, manufactured by Solartron). The alternating current impedance was measured under the conditions of a sweep frequency of 100000 Hz to 1 Hz and an amplitude of 5 mV, and the resistance value was obtained.

[0046] From this resistance value, the thickness, and the area of the circular electrode, the electrical conductivity of the electrode was calculated by the following formula. σ = L / (R·A) σ: Conductivity [S / cm] L: Electrode thickness [cm] (value obtained by subtracting the thickness of the aluminum foil from the actually measured electrode thickness) R: Resistance [Ω] A: Electrode area [cm2]

[0047] <Fabrication of Li Counter Electrode Battery> Using the electrode fabricated by the above method as the positive electrode, a solution in which LiPF6 was dissolved at a concentration of 1.0 M in a solution obtained by mixing EC and DMC at a volume ratio of 1:2 was used as the electrolyte, a polypropylene sheet (product name: Celgard 2400, manufactured by Celgard) was used as the separator, and a lithium foil ( A CR2032-type coin cell (Li counter electrode battery) was fabricated using a 16.16 mm diameter, 200 μm thickness, manufactured by Honjo Metals Co., Ltd., as the negative electrode.

[0048] <Initial capacity measurement> The initial capacity of the Li counter electrode battery prepared by the above method was measured at 25°C using a charge / discharge device (product name: BTS2004W, manufactured by NAGANO). First, a two-cycle charge / discharge test was performed at a voltage range of 2.0V-4.5V and a current density of 6mA / g, and then a one-cycle charge / discharge test was performed at a voltage range of 2.0V-4.5V and a current density of 0.3C to evaluate the initial capacity. The C rate was calculated by taking the discharge capacity when charged and discharged at a current density of 6mA / g as the practical discharge amount of 1C and the current density of 0.3C.

[0049] (Example 1) 800g of electrolytic manganese dioxide (MnO2) was calcined at 600°C for 12 hours to obtain 726g of manganese dioxide (Mn2O3). 338g of lithium hydroxide monohydrate (LiOH·H2O) and 662g of the manganese dioxide obtained above were mixed with 4000mL of pure water to prepare 5kg of slurry, which was then pulverized for 2 hours using a pulverizer (product name: Dyno Mill Multi-Lab model, manufactured by Shinmaru Enterprises). The average particle diameter (D 50 ) was measured using a particle size distribution analyzer (product name: MT3000II series, manufactured by MicrotracBEL) and found to be 0.6 μm. The obtained slurry was spray-dried using a spray dryer (product name: SB39, manufactured by PRIS) under conditions of a 90-type nozzle spray pressure of 0.2 MPa and a solution rate of 3 kg / h to produce spherical granular dried particles. Spray drying was performed at a hot air inlet temperature of 220°C.

[0050] Average particle size of dry granules (D 50 ) was measured using a particle size distribution analyzer (product name: MT3000II series, manufactured by MicrotracBEL) and found to be 12 μm. The dried granular particles are heated to 700°C in a nitrogen atmosphere for 2 hours, then cooled to room temperature for heat treatment. 50 A lithium composite oxide having a diameter of 10.3 μm, a main phase having a rectangular zigzag layer structure, and a domain having a monoclinic α-NaFeO2 type layer structure was obtained. In the above heat treatment, the heating rate was 10° C. / min and the cooling rate was 5° C. / min. The composition of the obtained lithium composite oxide was analyzed according to the above <Composition Analysis>. The composition was Li 1.01 It was MnO2.

[0051] (Example 2) A lithium composite oxide was obtained in the same manner as in Example 1, except that 338 g of lithium hydroxide monohydrate and 662 g of manganese trioxide were mixed with 2600 mL of pure water to prepare 3.6 kg of slurry. 50 ) is 0.6 μm, and the average particle size of the granular dry particles (D 50 ) was 10 μm. In addition, the D 50 The composition of the obtained lithium composite oxide was Li 1.05 It was MnO2.

[0052] (Example 3) 10g of manganese carbonate (MnCO3) was calcined in air at 850℃ for 12 hours to produce 6.8g of manganese dioxide (Mn2O3). 2g of manganese dioxide and 0.92g of commercially available lithium carbonate were dry mixed in a mortar for 20 minutes so that the Li / Mn molar ratio was 1.0. The resulting mixed powder was heated in a nitrogen atmosphere at 900℃ for 12 hours, and then cooled to room temperature, resulting in a heat treatment to obtain LiMnO2 with a zigzag layer structure. In the above heat treatment, the heating rate was 10℃ / min and the cooling rate was 5℃ / min. The obtained LiMnO2 was subjected to mechanical milling at 600 rpm for 36 hours in a sealed container in an argon atmosphere to obtain rock salt type LiMnO2. A zirconia container and balls were used for mechanical milling, and 1.5 g of LiMnO2 with a zigzag layered structure, three 10 mm diameter balls, ten 5 mm diameter balls, and 2 g of 1 mm diameter balls were placed in the container and balls. The ball mill used was a planetary ball mill P-7 Classic Line (manufactured by FRITSCH).

[0053] Next, the obtained rock-salt LiMnO2 was heat-treated by heating in a nitrogen atmosphere at 700℃ for 2 hours, and then cooling to room temperature to obtain a lithium composite oxide having a crystal structure in which the main phase has an orthorhombic zigzag layer structure and domains of a monoclinic α-NaFeO2 layer structure. In the above heat treatment, the heating rate was 10℃ / min and the cooling rate was 5℃ / min. The composition of the obtained lithium composite oxide was analyzed according to the above <Composition Analysis>. The composition was Li 0.97 It was MnO2.

[0054] Powder XRD was carried out on the lithium composite oxides of Examples 1 to 3 according to the above <Identification of Crystal Structure>, and the XRD patterns from 10 to 90° were confirmed. The results are shown in FIG. It was found that the XRD patterns of the lithium composite oxides of Examples 1 to 3 had strong peaks on the orthorhombic (010), (011), (200), and (021) planes and a weak peak on the monoclinic (001) plane. In other words, it was confirmed that the crystal structure of the lithium composite oxide prepared in the present invention has a zigzag layered structure as a parent structure and has domains of an α-NaFeO2 type layered structure.

[0055] For the lithium composite oxides of Examples 1 to 3, the intensity ratio (A / B) between the diffraction peak integrated intensity (A) observed at 2θ=15.3±1.0° and the diffraction peak integrated intensity (B) observed at 2θ=18.2±1.0° by powder XRD was calculated according to the above measurement conditions. The results are shown in Table 1. For the lithium composite oxides of Examples 1 to 3, the BET specific surface area was measured according to the above <Measurement of BET Specific Surface Area>, and the results are shown in Table 1. For the lithium composite oxides of Examples 1 to 3, the initial capacity of the Li counter electrode battery was measured according to the above <Measurement of Initial Capacity>, and the results are shown in Table 1.

[0056] [Table 1]

[0057] From FIG. 3 and Table 1, it was confirmed that the lithium composite oxide prepared in the present disclosure has a structure having a zigzag layered structure as a mother structure and domains of an α-NaFeO2 type layered structure. Further, by controlling the BET specific surface area, it was confirmed that the initial capacity when applied to a lithium ion secondary battery was exhibited.

[0058] In the lithium composite oxides of Examples 1 to 3, the particle size distribution was measured according to the above <Measurement of Particle Size Distribution>, and the obtained particle size distribution diagram is shown in FIG. 4. As shown in FIG. 4, in Example 3, the particle size distribution is wide, whereas in Examples 1 and 2, the particle size distribution has a single peak, and the average particle diameter D 50 is within a preferable range for handling as a powder of a positive electrode material for a lithium secondary battery.

[0059] Based on the particle size distribution obtained by the above measurement method, D 10 , D 50 , D 90 and span [(D 90 -D 10 ) / D 50 of the lithium composite oxides of Examples 1 to 3 were calculated, and the results are shown in Table 2.

[0060] [Table 2]

[0061] For the lithium composite oxides of Examples 1 to 3, the electrical conductivity of the electrodes was calculated according to <Measurement of electrode electrical conductivity>, and the results are shown in Table 3.

[0062] [Table 3] Table 3 shows that the electrode electrical conductivity of Examples 1 and 2, which are working examples, is higher than the electrode electrical conductivity of Example 3, which is a comparative example. [Industrial Applicability]

[0063] The lithium composite oxide of the present disclosure, when used as a positive electrode active material for lithium secondary batteries, has higher electrical conductivity than conventional materials, and is therefore expected to be used in the field of positive electrode active materials for lithium secondary batteries.

Claims

1. Composition formula Li x MnO 2 (where 0.80≦x≦1.20), the matrix structure is a zigzag layer structure, and the structure is α-NaFeO 2 A lithium composite oxide having a domain of a layered structure, and having a span value S obtained by the following calculation formula (1) of 1.0 or more and 5.0 or less. S=(D 90 -D 10 ) / D 50 (1) (In formula (1), D 10 , D 50 and D. 90 indicate the cumulative 10% particle size, the cumulative 50% particle size, and the cumulative 90% particle size, respectively, in the volume-based particle size distribution.)

2. D in the formula (1) 50 The lithium composite oxide according to claim 1, wherein the average particle size is 5 μm or more and 15 μm or less.

3. 3. The lithium composite oxide according to claim 1, wherein the intensity ratio (A / B) of an integrated intensity (A) of a diffraction peak observed at 2θ = 15.3 ± 1.0° in a powder X-ray pattern diffraction to an integrated intensity (B) of a diffraction peak observed at 2θ = 18.2 ± 1.0° is 0.5 or more.

4. 3. A method for producing a lithium composite oxide according to claim 1, comprising the steps of: mixing lithium hydroxide, manganese oxide or manganese oxyhydroxide, and water to prepare a slurry; evaporating water from the obtained slurry to produce granular dry particles; and heat-treating the granular dry particles obtained in the above step in an inert gas.

5. The method for producing a lithium composite oxide according to claim 4, wherein water is evaporated by spray drying in the step of producing the granular dry particles.

6. An electrode comprising the lithium composite oxide according to claim 1 or 2 as a positive electrode active material.

7. A lithium secondary battery comprising the electrode according to claim 6.

Citation Information

Patent Citations

  • Lithium manganese multiple oxide, positive electrode material for lithium secondary cell, positive electrode for lithium secondary cell and manufacturing method of lithium secondary cell and lithium manganese multiple oxide

    JP2002145619A

  • Positive electrode active material for nonaqueous electrolyte secondary battery

    JP2003007297A

  • Positive electrode active material for lithium ion battery, method for manufacturing positive electrode active material for lithium ion battery, positive electrode for lithium ion battery, and lithium ion battery

    JP6956039B2