Semiconductor device and manufacturing method thereof

By applying a thin, amorphous metal film to a ferroelectric film and crystallizing it through heat treatment, the stress is increased, improving the crystallinity and performance of ferroelectric memory cells, enabling faster and more efficient operation.

JP2024151890APending Publication Date: 2024-10-25RENESAS ELECTRONICS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023065681
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing ferroelectric memory cells require large stresses to achieve a ferroelectric phase, but the relationship between metal films and stress has not been sufficiently clarified, affecting the performance of semiconductor devices.

Method used

A semiconductor device with a thin, amorphous metal film applied to a ferroelectric film, where the metal film is crystallized through heat treatment to apply large stress, enhancing the crystallinity of the ferroelectric film and improving its performance.

Benefits of technology

The improved crystallinity of the ferroelectric film leads to enhanced performance of the memory cell, allowing for higher writing speed and lower voltage operation, reducing power consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151890000001_ABST
    Figure 2024151890000001_ABST
Patent Text Reader

Abstract

To improve the performance of a semiconductor device.SOLUTION: A gate insulating film GI is formed on a semiconductor substrate SUB. A gate electrode GE is formed on the gate insulating film GI. A ferroelectric film FE and a metal film MF are formed between the gate insulating film GI and the gate electrode GE. The thickness of the metal film MF is thinner than the thickness of the ferroelectric film FE. The metal film MF is amorphous.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device and a manufacturing method thereof, and more particularly to a semiconductor device including a ferroelectric film and a manufacturing method thereof. [Background technology]

[0002] In recent years, ferroelectric memory cells using a ferroelectric film have been developed as semiconductor memory elements that operate at low voltages. Ferroelectric memory cells are non-volatile memory cells that change the write and erase states of information by controlling the direction of polarization of the ferroelectric film.

[0003] Patent Document 1 discloses a ferroelectric memory cell including a ferroelectric film and a metal film formed on the ferroelectric film. The metal film is made of titanium nitride or the like and has a thickness of 10 nm or more. A crystallized ferroelectric film is obtained by performing a heat treatment while the metal film is in contact with the amorphous ferroelectric film. At this time, the crystal orientation of the ferroelectric film can be aligned by the stress from the metal film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-22602 Summary of the Invention [Problem to be solved by the invention]

[0005] Thermodynamically, it is known that a large stress is necessary to obtain the ferroelectric phase. Titanium nitride films or tungsten films are used as metal films formed on ferroelectric films. Generally, such metal films have a thickness of about 10 nm and are crystallized. Until now, the relationship between the properties of the metal film and the stress has not been fully elucidated.

[0006] The main object of the present application is to provide a metal film capable of applying a large stress to a ferroelectric film, thereby improving the performance of a ferroelectric memory cell and improving the performance of a semiconductor device. Other objects and novel features will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]

[0007] A brief outline of a representative embodiment of the present invention will be described below.

[0008] A semiconductor device according to one embodiment includes a gate insulating film formed on a semiconductor substrate, a gate electrode formed on the gate insulating film, and a ferroelectric film and a first metal film formed between the gate insulating film and the gate electrode. The thickness of the first metal film is thinner than the thickness of the ferroelectric film, and the first metal film is amorphous.

[0009] A method for manufacturing a semiconductor device according to one embodiment includes the steps of: (a) forming a gate insulating film on a semiconductor substrate; (b) forming a first amorphous film on the gate insulating film; (c) forming a first metal film on the gate insulating film; (d) performing a heat treatment after steps (b) and (c) while the first metal film is in contact with the first amorphous film to crystallize the first amorphous film to form a ferroelectric film having an orthorhombic crystal structure; and (e) forming a conductive film for a gate electrode on the ferroelectric film and the first metal film after step (d). The thickness of the first metal film is thinner than that of the ferroelectric film, and the first metal film is amorphous during step (d). Effect of the Invention

[0010] According to one embodiment, the performance of a semiconductor device can be improved. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view of a semiconductor device in a first embodiment. [Diagram 2] 1 is a table showing an example of conditions for applying voltages to each portion of a memory cell during "writing," "erasing," and "reading." [Diagram 3] 1 is a graph obtained through an experiment conducted by the inventor of the present application. [Figure 4] 1 is a graph obtained through an experiment conducted by the inventor of the present application. [Diagram 5] 1 is a graph obtained through an experiment conducted by the inventor of the present application. [Figure 6] 2A to 2C are cross-sectional views showing a manufacturing process of the semiconductor device in the first embodiment. [Figure 7] 7A to 7C are cross-sectional views showing the manufacturing process of the semiconductor device following FIG. 6. [Figure 8] 8 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 7. [Figure 9] 9 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 8. [Figure 10] 10 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. [Figure 11] 11 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 10. [Figure 12] 12 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 11. [Figure 13] FIG. 11 is a cross-sectional view of a semiconductor device according to a first modified example. [Figure 14] FIG. 11 is a cross-sectional view of a semiconductor device according to a second modified example. [Figure 15] FIG. 11 is a cross-sectional view of a semiconductor device according to a third modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments will be described in detail with reference to the drawings. In all the drawings for explaining the embodiments, the same reference numerals are used for the members having the same functions, and the repeated explanations are omitted. In the following embodiments, the explanations of the same or similar parts will not be repeated as a rule unless it is particularly necessary.

[0013] (Embodiment 1) <Structure of Semiconductor Device> A semiconductor device according to a first embodiment will be described below with reference to Figures 1 and 2. The semiconductor device includes a memory cell MC. The memory cell MC is a non-volatile memory cell and a ferroelectric memory cell.

[0014] As shown in FIG. 1, the memory cell MC includes a semiconductor substrate SUB, a gate insulating film GI, a ferroelectric film FE, a metal film MF, a gate electrode GE, a sidewall spacer SW, a well region PW, an extension region EX, and a diffusion region ND.

[0015] The semiconductor substrate SUB is made of p-type single crystal silicon. A p-type well region PW is formed in the semiconductor substrate SUB. A gate insulating film (paraelectric film) GI is formed on the semiconductor substrate SUB including the well region PW. The gate insulating film GI is, for example, a silicon oxide film, and has a thickness of, for example, 0.1 nm or more and 3 nm or less.

[0016] A gate electrode GE is formed on the gate insulating film GI. A ferroelectric film FE and a metal film MF are formed between the gate insulating film GI and the gate electrode GE. In the first embodiment, the ferroelectric film FE is formed on the gate insulating film GI, the metal film MF is formed on the ferroelectric film FE, and the gate electrode GE is formed on the metal film MF. The gate electrode GE is, for example, a polycrystalline silicon film into which an n-type impurity is introduced.

[0017] The ferroelectric film FE is an insulating film made of a material that generates dielectric polarization when an electric field is applied from the outside, and the polarization does not become zero even when the electric field is removed. In other words, the ferroelectric film FE is an insulating film made of a ferroelectric material. Even when no electric field is applied, a remnant polarization with a certain magnitude exists in the ferroelectric film FE.

[0018] The ferroelectric film FE must be an orthogonal crystal. In other words, a film mainly composed of crystals other than an orthogonal crystal is a paraelectric film. Therefore, in the memory cell MC, in order to increase the remanent polarization of the ferroelectric film FE, improve the performance as a ferroelectric, and reduce the driving power, it is necessary to form the crystals constituting the ferroelectric film FE as orthogonal as possible. The ferroelectric film FE in the first embodiment contains hafnium (Hf), oxygen (O), and zirconium (Zr). More specifically, the ferroelectric film FE is an orthogonal HfZrO2 film. The thickness of the ferroelectric film FE is, for example, 4 nm or more and 10 nm or less. In the following description, the HfZrO2 film is referred to as an HZO film.

[0019] The metal film MF is a cap film provided to apply stress to the ferroelectric film FE and control the crystal orientation of the ferroelectric film FE. The metal film MF in the first embodiment also functions as a part of the gate electrode GE. The metal film MF is amorphous, for example, an amorphous titanium nitride film. The thickness of the metal film MF is thinner than the thickness of the ferroelectric film FE, for example, 1 nm or more and 4 nm or less, and preferably 2 nm or less.

[0020] The main feature of the first embodiment is that the metal film MF is extremely thin and amorphous, and this feature will be described in detail later.

[0021] A sidewall spacer SW is formed on the side surface of the gate electrode GE. The sidewall spacer SW is made of, for example, a laminated film of a silicon oxide film and a silicon nitride film.

[0022] In the well region PW below the sidewall spacer SW, an extension region EX, which is a low-concentration n-type impurity region, is formed. In addition, in the well region PW at a position aligned with the sidewall spacer SW, a diffusion region ND, which is a higher-concentration n-type impurity region than the extension region EX, is formed. The extension region EX and the diffusion region ND are connected to each other and are respectively a part of the source region or a part of the drain region of the memory cell MC. The well region PW located directly below the gate electrode GE and sandwiched between the two extension regions EX becomes the channel region of the memory cell MC.

[0023] <Operation of memory cell MC> An example of the operation of the memory cell MC will be described with reference to FIG. 2. Voltage Vg shown in FIG. 2 is the voltage applied to the gate electrode GE. Voltage Vd is the voltage applied to the drain region (one of the diffusion regions ND). Voltage Vs is the voltage applied to the source region (the other diffusion region ND). Voltage Vb is the voltage applied to the well region PW. Note that the magnitude of each voltage is not limited to that shown in FIG. 2, and can be changed in various ways as necessary.

[0024] In a write operation, the polarization of the ferroelectric film FE is directed upward by applying a voltage as shown in "write" in Fig. 2, and the threshold voltage of the memory cell MC is brought into a relatively high state. In an erase operation, the polarization of the ferroelectric film FE is directed downward by applying a voltage as shown in "erase" in Fig. 2, and the threshold voltage of the memory cell MC is brought into a relatively low state.

[0025] In a read operation, a voltage as shown in "Read" in FIG. 2 is applied. The voltage applied to the gate electrode GE during a read operation is set to be smaller than the threshold voltage of the memory cell MC in the written state and larger than the threshold voltage of the memory cell MC in the erased state. In a memory cell MC in the written state, no current flows, or even if a current flows, the amount is very small. In a memory cell MC in the erased state, a large amount of current flows. In this way, the state of the memory cell MC can be determined based on the amount of current flowing through the memory cell MC.

[0026] <Features of Metal Film MF> The metal film MF in the first embodiment will be described below with reference to FIGS.

[0027] The present inventors focused on the stress of the metal film MF and investigated in detail the effect of this stress on the crystallinity of the ferroelectric film FE. A titanium nitride film (TiN film) was used as the metal film MF, and an HZO film was used as the ferroelectric film FE. After the TiN film was formed, a heat treatment was performed to crystallize the ferroelectric film FE. It was revealed for the first time that the greater the stress change (residual stress) applied to the HZO film before and after this heat treatment, the more improved the crystallinity of the HZO film. The amorphous TiN film formed at an extremely low rate showed the highest stress change, with a thickness of 2 nm or less.

[0028] 3 is a graph showing the relationship between the diffraction angle in X-ray diffraction and the X-ray diffraction intensity of a TiN film. As shown in FIG. 3, the TiN film in the first embodiment does not have a crystal orientation. The TiN film is formed as a TiN film with weak orientation (crystallinity) by setting the film forming conditions to predetermined conditions. Here, weak orientation means, for example, that no significant peak is observed in X-ray diffraction, and refers to a state in which the fine crystals constituting the film have little regular periodicity and symmetry. In addition, weak orientation also includes a state in which the arrangement of the fine crystals constituting the film is disordered, so-called "non-oriented" state.

[0029] A method for manufacturing such a TiN film will be described. The TiN film is formed by a film formation process using a sputtering method. This film formation process uses a target made of titanium, and is performed under the conditions of a power for plasma generation of 1000 W or less, a pressure of 0.025 Pa or less, a nitrogen flow rate of 12 sccm or less, and an argon flow rate of 15 sccm or less. Plasma is discharged at a low power of 1000 W or less, and titanium and nitrogen are chemically reacted to form the film. The film formation rate of the TiN film in this film formation process is 0.01 nm / sec or more and 0.05 nm / sec or less, for example, 0.02 nm / sec.

[0030] As shown in Fig. 3, this film formation process can suppress the formation of the preferred orientations of TiN(111), TiN(200), and TiN(220). Usually, when the film reaches a certain thickness, these crystal planes are naturally formed, but the TiN film in the first embodiment is amorphous because it is about 2 nm thick.

[0031] After forming an amorphous HZO film and then forming a TiN film on it, a heat treatment is performed using, for example, the RTA (Rapid Thermal Annealing) method. The temperature of this heat treatment is, for example, 500 degrees Celsius or higher and 600 degrees Celsius or lower. This heat treatment generates a large stress in the TiN film. Then, the stress of the TiN film is transmitted to the HZO film, and the amorphous HZO film undergoes a phase transition (structural phase transition), forming a rectangular HZO film with high orientation (crystallinity).

[0032] Fig. 4 is a graph showing the relationship between the residual stress in the HZO film and the amount of crystals having a (111) orientation in the HZO film. The measurement points of "TiN amorphous" in Fig. 4 were measured using the metal film MF of the first embodiment. The measurement points included in "TiN crystal" in Fig. 4 each have a different thickness, and each measurement was performed using a crystallized TiN film.

[0033] As shown in Fig. 4, when an amorphous TiN film was used, a larger residual stress was obtained than when a crystallized TiN film was used. The reason why a large stress occurs in the TiN film in the first embodiment is presumably because the TiN film with weak orientation has a large linear expansion coefficient, and therefore the stress increases when the film is subjected to heat treatment.

[0034] Figure 5 is a graph showing the results of measurements made by the inventors of the present invention on the various characteristics required for memory cells MC. Here, measurements were made on the memory window, local variations within the wafer surface, and retention. As shown in Figure 5, improvements were observed in each characteristic due to the improvement in the crystallinity of the HZO film. Furthermore, the improvement in the crystallinity of the HZO film makes it possible to increase the write speed and erase speed at low voltage, thereby enabling the memory cells MC to operate at lower voltages and consume less power.

[0035] As described above, in the first embodiment, it is possible to provide the metal film MF that can apply a large stress to the ferroelectric film FE. By applying this metal film MF, it is possible to improve the performance of the memory cell MC, and therefore the performance of the semiconductor device.

[0036] <Method of Manufacturing Semiconductor Device> Each manufacturing process included in the method for manufacturing the semiconductor device in the first embodiment will be described below with reference to FIGS.

[0037] 6, first, a semiconductor substrate SUB made of, for example, p-type single crystal silicon is prepared. Next, a p-type well region PW is selectively formed in the semiconductor substrate SUB by using photolithography and ion implantation.

[0038] As shown in FIG. 7, a gate insulating film GI is formed on a semiconductor substrate SUB by, for example, thermal oxidation processing.

[0039] As shown in FIG. 8, an amorphous film AM is formed on the gate insulating film GI by, for example, ALD (Atomic Layer Deposition). The amorphous film AM has a thickness of, for example, 4 nm or more and 10 nm or less. The amorphous film AM contains hafnium (Hf), oxygen (O) and zirconium (Zr). More specifically, the amorphous film AM is a HfZrO2 film (HZO film).

[0040] As shown in Fig. 9, an amorphous metal film MF is formed on the gate insulating film GI by a film formation process using, for example, a sputtering method. The metal film MF is, for example, an amorphous titanium nitride film (TiN film). The thickness of the metal film MF is thinner than the thickness of the amorphous film AM, for example, 1 nm or more and 4 nm or less, and preferably 2 nm or less. The conditions of the film formation process of the metal film MF are the same as those described in Fig. 3.

[0041] Also, as in other embodiments described later, there are cases where the metal film MF is formed on the gate insulating film GI before the amorphous film AM, but in the first embodiment, the metal film MF is formed on the gate insulating film GI after the amorphous film AM. Therefore, in the first embodiment, the metal film MF is formed on the amorphous film AM so that the metal film MF is in contact with the amorphous film AM.

[0042] As shown in Fig. 10, a heat treatment is performed while the metal film MF is in contact with the amorphous film AM, thereby crystallizing the amorphous film AM to form a rectangular ferroelectric film FE. This heat treatment is called RTA (Rapid Thermal Annealing), and is performed, for example, for a period of 1 second to 3 minutes at a temperature of 500 degrees Celsius to 600 degrees Celsius. Even after this heat treatment, the metal film MF maintains an amorphous state.

[0043] This heat treatment generates a large stress in the metal film MF. The stress in the metal film MF is then transmitted to the amorphous film AM, which undergoes a phase transition to form a highly oriented orthorhombic ferroelectric film FE. As described in FIG. 4, the metal film MF being amorphous allows the stress change applied to the ferroelectric film FE to be larger than when the metal film MF is crystalline.

[0044] 11, after the heat treatment of FIG. 10 is performed, a conductive film CF1 for the gate electrode GE is formed on the metal film MF by, for example, a CVD (Chemical Vapor Deposition) method. The conductive film CF1 is made of, for example, polycrystalline silicon doped with n-type impurities.

[0045] 12, first, the conductive film CF1, the metal film MF, the ferroelectric film FE, and the gate insulating film GI are patterned in sequence by photolithography and anisotropic etching. The patterned conductive film CF1 becomes the gate electrode GE.

[0046] Next, by photolithography and ion implantation, an extension region EX, which is an n-type impurity region, is formed in the well region PW exposed from the gate electrode GE.

[0047] Thereafter, the following manufacturing steps are performed to obtain the memory cell MC shown in FIG.

[0048] First, a laminated film of, for example, a silicon oxide film and a silicon nitride film is formed by, for example, a CVD method so as to cover the gate electrode GE. Next, the laminated film is processed by anisotropic etching to form a sidewall spacer SW made of the laminated film on the side surface of the gate electrode GE.

[0049] Next, a diffusion region ND, which is an n-type impurity region, is formed in the well region PW exposed from the sidewall spacer SW and the gate electrode GE by photolithography and ion implantation. The diffusion region ND has a higher impurity concentration than the extension region EX. The diffusion region ND and the extension region EX function as a part of the source region or a part of the drain region of the memory cell MC, respectively.

[0050] (Variation 1) A semiconductor device according to Modification 1 of the first embodiment will be described below with reference to Fig. 13. In the following description, differences from the first embodiment will be mainly described, and descriptions of points that overlap with the first embodiment will be omitted.

[0051] In the first embodiment, the metal film MF is a single amorphous film. In the first modification, the metal film MF is a laminated film including a plurality of amorphous films.

[0052] As shown in Fig. 13, the metal film MF in the first modification includes an amorphous film MFa and an amorphous film MFb. Each of the amorphous films MFa and MFb is formed by a film formation process under the same conditions as those described in Fig. 3, as in the first embodiment. Each of the amorphous films MFa and MFb is, for example, an amorphous titanium nitride film. The thickness of each of the amorphous films MFa and MFb is thinner than the thickness of the ferroelectric film FE, for example, 1 nm or more and 4 nm or less, and preferably 2 nm or less.

[0053] 9, the metal film MF of Modification 1 can be formed by sequentially stacking an amorphous film MFa and an amorphous film MFb by a film formation process similar to the conditions described in Fig. 3. Also in Modification 1, the entire metal film MF is amorphous, so that the stress change applied to the ferroelectric film FE can be increased.

[0054] In the first modification, by stacking a plurality of amorphous films such as the amorphous film MFa and the amorphous film MFb, it is possible to finely adjust the work function of the metal film MF as a whole. Therefore, by adjusting the thickness of each of the plurality of amorphous films and the number of stacked layers of the plurality of amorphous films, it is possible to finely adjust the threshold voltage of the memory cell MC.

[0055] In the first modification, the metal film MF has been exemplified as having a two-layer structure made up of the amorphous film MFa and the amorphous film MFb, but the metal film MF may be an amorphous film having two or more layers.

[0056] Moreover, the metal film MF having the laminated structure of the first modification can also be applied to all of the metal films MF disclosed in the second and third modifications described below.

[0057] (Variation 2) The semiconductor device in Modification 2 will be described below with reference to Fig. 14. In the following description, differences from the first embodiment will be mainly described, and descriptions of points that overlap with the first embodiment will be omitted.

[0058] In the first embodiment, the metal film MF is formed between the ferroelectric film FE and the gate electrode GE. As shown in Fig. 14, in the second modification, the metal film MF is formed between the gate insulating film GI and the ferroelectric film FE.

[0059] In order to obtain such a structure of Modification 2, a metal film MF may be formed first on the gate insulating film GI, and then an amorphous film AM may be formed on the metal film MF. The metal film MF in Modification 2 may be formed by a film formation process similar to the conditions described in FIG.

[0060] Also in the second modification, by performing the heat treatment of Fig. 10 in a state where the metal film MF is in contact with the amorphous film AM, the stress change applied to the ferroelectric film FE can be increased, and a ferroelectric film FE having an orthorhombic crystal structure can be obtained. In the second modification, the conductive film CF1 for the gate electrode GE is formed on the ferroelectric film FE.

[0061] (Variation 3) The semiconductor device in Modification 3 will be described below with reference to Fig. 15. In the following description, differences from the first embodiment will be mainly described, and descriptions of points that overlap with the first embodiment will be omitted.

[0062] As shown in FIG. 15, in the third modification, a metal film MF similar to that in the first embodiment is formed between the ferroelectric film FE and the gate electrode GE, and a metal film MF similar to that in the second modification is formed between the gate insulating film GI and the ferroelectric film FE.

[0063] To obtain such a structure of Modification 3, first, a metal film MF is formed on the gate insulating film GI. Next, an amorphous film AM is formed on the metal film MF. Next, a metal film MF is formed on the amorphous film AM. Note that the two metal films MF in Modification 3 can be formed by a film formation process similar to the conditions described in FIG. 3.

[0064] 10 in a state where the two metal films MF are in contact with the amorphous film AM, the stress change applied to the ferroelectric film FE can be increased, and a ferroelectric film FE having an orthorhombic crystal structure can be obtained. Since the heat treatment is performed in a state where the amorphous film AM is sandwiched between the two metal films MF from above and below, a larger stress change can be generated than in the first embodiment or the second modification.

[0065] Although the present invention has been specifically described above based on the above embodiment, the present invention is not limited to the above embodiment and can be modified in various ways without departing from the spirit of the present invention. [Explanation of symbols]

[0066] AM amorphous film CF1 conductive film EX Extension Area FE Ferroelectric film GE gate electrode GI Gate Insulator MC memory cell MF metal film MFa, MFb amorphous film ND Diffusion Area PW Well Region SUB Semiconductor Substrate SW Sidewall spacer

Claims

1. a gate insulating film formed on a semiconductor substrate; a gate electrode formed on the gate insulating film; a ferroelectric film and a first metal film formed between the gate insulating film and the gate electrode; Equipped with the thickness of the first metal film is smaller than the thickness of the ferroelectric film; The semiconductor device, wherein the first metal film is amorphous.

2. 2. The semiconductor device according to claim 1, A semiconductor device, wherein the first metal film has a thickness of 1 nm or more and 4 nm or less.

3. 3. The semiconductor device according to claim 2, A semiconductor device, wherein the first metal film has a thickness of 2 nm or less.

4. 3. The semiconductor device according to claim 2, The first metal film is made of amorphous titanium nitride.

5. 5. The semiconductor device according to claim 4, The semiconductor device, wherein the ferroelectric film contains hafnium, oxygen and zirconium.

6. 2. The semiconductor device according to claim 1, the first metal film is a laminated film including a plurality of amorphous films, The semiconductor device, wherein each of the plurality of amorphous films has a thickness of 2 nm or less.

7. 2. The semiconductor device according to claim 1, The first metal film is formed between the ferroelectric film and the gate electrode.

8. 8. The semiconductor device according to claim 7, a second metal film formed between the gate insulating film and the ferroelectric film; the thickness of the second metal film is smaller than the thickness of the ferroelectric film; The second metal film is amorphous.

9. 2. The semiconductor device according to claim 1, The first metal film is formed between the gate insulating film and the ferroelectric film.

10. (a) forming a gate insulating film on a semiconductor substrate; (b) forming a first amorphous film on the gate insulating film; (c) forming a first metal film on the gate insulating film; (d) after the steps (b) and (c), performing a heat treatment in a state in which the first metal film is in contact with the first amorphous film, thereby crystallizing the first amorphous film to form a ferroelectric film having an orthorhombic crystal structure; (e) after the step (d), forming a conductive film for a gate electrode on the ferroelectric film and the first metal film; Equipped with the thickness of the first metal film is smaller than the thickness of the first amorphous film; The method for manufacturing a semiconductor device, wherein the first metal film is amorphous in the step (d).

11. 11. The method of manufacturing a semiconductor device according to claim 10, A method for manufacturing a semiconductor device, wherein the first metal film has a thickness of 1 nm or more and 4 nm or less.

12. 12. The method of manufacturing a semiconductor device according to claim 11, A method for manufacturing a semiconductor device, wherein the first metal film has a thickness of 2 nm or less.

13. 12. The method of manufacturing a semiconductor device according to claim 11, In the step (c), the first metal film is formed by a film formation process using a sputtering method, A method for manufacturing a semiconductor device, wherein a deposition rate of the first metal film in the deposition process is not less than 0.01 nm / sec and not more than 0.05 nm / sec.

14. 14. The method of manufacturing a semiconductor device according to claim 13, The film formation process is performed using a target made of titanium under conditions of a power for plasma generation of 1000 W or less, a pressure of 0.025 Pa or less, a nitrogen flow rate of 12 sccm or less, and an argon flow rate of 15 sccm or less.

15. 15. The method of manufacturing a semiconductor device according to claim 14, The method for manufacturing a semiconductor device, wherein the ferroelectric film contains hafnium, oxygen and zirconium.

16. 11. The method of manufacturing a semiconductor device according to claim 10, In the step (c), the first metal film is formed by sequentially stacking a plurality of amorphous films; The method for manufacturing a semiconductor device, wherein each of the plurality of amorphous films has a thickness of 2 nm or less.

17. 11. The method of manufacturing a semiconductor device according to claim 10, The step (c) is carried out after the step (b); In the step (c), the first metal film is formed on the first amorphous film; In the step (e), the conductive film is formed on the first metal film.

18. 18. The method of manufacturing a semiconductor device according to claim 17, (f) forming a second metal film on the gate insulating film between the steps (a) and (b); Further comprising: In the step (b), the first amorphous film is formed on the second metal film; In the step (d), the heat treatment is performed in a state in which the first metal film and the second metal film are in contact with the first amorphous film; the second metal film has a thickness smaller than the thickness of the first amorphous film; The method for manufacturing a semiconductor device, wherein the second metal film is amorphous in the step (d).

19. 11. The method of manufacturing a semiconductor device according to claim 10, The step (c) is carried out before the step (b); In the step (b), the first amorphous film is formed on the first metal film; In the step (e), the conductive film is formed on the ferroelectric film.

Citation Information

Patent Citations

  • Bottom-electrode interface structure for memory

    US20220328508A1

  • Interface film to mitigate size effect of memory device

    US20220367493A1

  • Interfacial layer with high texture uniformity for ferroelectric layer enhancement

    US20230017020A1

  • Semiconductor device and manufacturing method thereof

    JP2021022602A