Gravure printing ink for surface printing, and printed matter using the same

The gravure printing ink composition, featuring a urethane resin with specific aliphatic dibasic acid content and a rosin resin with defined acid value, addresses adhesion and blocking resistance issues, delivering superior adhesiveness and printability on diverse packaging materials.

JP2024152344AActive Publication Date: 2024-10-25TOYO INK MFG CO LTD +1
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2023066476
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

Existing gravure printing inks face challenges in achieving excellent adhesiveness, blocking resistance to vinyl chloride sheets and antifogging films, and printability, which are crucial for high-quality surface printing on diverse packaging materials.

Method used

A gravure printing ink composition containing a urethane resin with a specific aliphatic dibasic acid content, a rosin resin with a defined acid value, a chelating agent, and optional additives like fatty acid amides and hydrocarbon wax, enhancing adhesion and blocking resistance through interactions and film cohesion.

Benefits of technology

The ink exhibits superior adhesiveness, blocking resistance to vinyl chloride sheets and antifogging films, and maintains high printability even under demanding conditions of high temperature and humidity, ensuring effective surface printing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152344000001
    Figure 2024152344000001
  • Figure 2024152344000002
    Figure 2024152344000002
  • Figure 2024152344000003
    Figure 2024152344000003
Patent Text Reader

Abstract

To provide gravure printing ink for surface printing which is excellent in adhesion, blocking resistance to a vinyl chloride sheet, blocking resistance to an antifogging film, and printability.SOLUTION: Gravure printing ink for surface printing contains an urethane resin (A), a rosin resin, a chelate agent and an organic solvent, wherein the urethane resin (A) contains a polyester-derived constitutional unit composed of aliphatic dibasic acid and diol, the aliphatic dibasic acid contains 80 mass% or more of aliphatic dibasic acid having 7 to 16 carbon atoms, and the acid value of the rosin resin is 50 to 250 mgKOH / g.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gravure printing ink for surface printing and a printed matter produced using the same. [Background technology]

[0002] In recent years, it has become common for product packages and other wrapping materials to be printed for decoration and surface protection. In addition, the quality of the print, such as the design, beauty, and luxury of the printed matter, can stimulate consumer purchasing motivation, and is of great industrial value.

[0003] On the other hand, food manufacturers, printing companies, and the like are demanding high quality and performance from printing inks for surface printing due to the diversification of packaging materials and the sophistication of packaging technology. Examples of printing inks for surface printing include flexographic inks, offset inks, gravure printing inks, and others, among which gravure printing inks are often used from the viewpoint of productivity due to their good printing speed.

[0004] The performance of gravure printing ink for front surface printing requires not only the quality of printing performance, but also various resistances such as adhesion, blocking resistance to prevent the ink from transferring to the back side of the substrate when it is printed and rolled up, and printability.

[0005] Examples of surface printing gravure printing inks that have excellent adhesion and various resistances include a surface printing gravure printing ink containing a binder resin in which a urethane resin and a cellulose derivative and / or a vinyl chloride-vinyl acetate copolymer are mixed in a specified ratio, a chelating agent, and a polyamide resin with a specific mass average molecular weight (Patent Document 1); a surface printing gravure printing ink composition in which the content ratio of a polyamide resin made from either tall oil fatty acid or rice bran fatty acid as a reaction raw material and a cellulose derivative and the content of each ink component are specified (Patent Document 2); a detachment printing ink composition containing a binder resin without an acid group and a rosin-based resin with a specified acid value and content (Patent Document 3); and an ink composition in which the dibasic acid contained in the urethane resin skeleton has 6 carbon atoms (Patent Document 4). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-025256 A [Patent Document 2] JP 2019-183112 A [Patent Document 3] JP 2022-080724 A [Patent Document 4] JP 2022-101885 A Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a gravure printing ink for surface printing which is excellent in adhesion, blocking resistance to vinyl chloride sheets, blocking resistance to anti-fog films, and printability. [Means for solving the problem]

[0008] As a result of extensive research into the above problems, the present inventors have found that the above problems can be solved by using the gravure printing ink for front printing described below, and have thus completed the present invention.

[0009] That is, the present invention provides a gravure printing ink for surface printing, which contains a urethane resin (A), a rosin resin, a chelating agent, and an organic solvent, The urethane resin (A) contains a structural unit derived from a polyester composed of an aliphatic dibasic acid and a diol, The aliphatic dibasic acid contains 80 mass% or more of an aliphatic dibasic acid having 7 to 16 carbon atoms, The present invention relates to a gravure printing ink for surface printing, wherein the rosin resin has an acid value of 50 to 250 mgKOH / g.

[0010] The present invention relates to the above gravure printing ink for surface printing, wherein the urethane resin (A) has an amine value of 1 to 20 mgKOH / g.

[0011] The present invention further relates to the above gravure printing ink for surface printing, which contains a vinyl chloride resin and / or a cellulose resin.

[0012] The present invention relates to the above gravure printing ink for surface printing, wherein the chelating agent comprises an acetylacetone-based titanium chelate and / or an alkyl acetoacetate-based titanium chelate.

[0013] The present invention further relates to the above gravure printing ink for surface printing, which contains a fatty acid amide and / or a polyamide resin.

[0014] The present invention relates to the above gravure printing ink for surface printing, wherein the fatty acid amide has a weight average molecular weight of 500 to 2,000.

[0015] The present invention relates to the above gravure printing ink for surface printing, wherein the polyamide resin has a weight average molecular weight of 1,000 to 20,000.

[0016] The present invention relates to the gravure printing ink for surface printing, wherein the fatty acid constituting the fatty acid amide contains an unsaturated fatty acid.

[0017] The present invention relates to the gravure printing ink for surface printing, wherein the fatty acid amide comprises a bisamide.

[0018] The present invention further relates to said gravure printing ink for surface printing, which contains hydrocarbon wax particles.

[0019] The present invention relates to a printed matter having a printed layer made of the above-mentioned gravure printing ink for surface printing on a substrate. Effect of the Invention

[0020] INDUSTRIAL APPLICABILITY The present invention makes it possible to provide a gravure printing ink for surface printing which is excellent in adhesion, blocking resistance to polyvinyl chloride sheets, blocking resistance to anti-fog films, and printability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The following describes in detail the embodiments of the present invention. However, the description of the components described below is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents as long as it does not go beyond the gist of the present invention.

[0022] In the following description, the term "gravure printing ink for surface printing" may be abbreviated to simply "gravure printing ink," "ink composition," or "ink." Furthermore, unless otherwise specified, "parts" refers to "parts by mass," and "%" refers to "% by mass."

[0023] In the present invention, "surface printing" refers to a printing method in which, when printed on a plastic substrate or paper substrate, the printed pattern or design can be confirmed when viewed from the printed layer side. When made into a laminate or a packaging bag, the outermost surface becomes the printed layer. The layer obtained by printing with a gravure printing ink for surface printing may be referred to as a "printed layer," "ink layer," or "ink coating," but these terms are synonymous.

[0024] <Gravure printing ink for surface printing> The gravure printing ink for surface printing contains a urethane resin (A), a rosin resin, a chelating agent, and an organic solvent, wherein the urethane resin (A) contains structural units derived from a polyester composed of an aliphatic dibasic acid and a diol, the aliphatic dibasic acid contains 80 mass% or more of an aliphatic dibasic acid having 7 to 16 carbon atoms, and the rosin resin has an acid value of 50 to 250 mgKOH / g. (1) The urethane resin (A) contains a polyester-derived structural unit consisting of a dibasic acid containing 80% by mass or more of an aliphatic dibasic acid having 7 to 16 carbon atoms and a diol, thereby improving adhesion. In addition, (2) the chelating agent and the rosin resin having an acid value of 50 to 250 mgKOH / g are contained, and the chelating agent and the carboxyl group of the rosin resin interact with each other to improve the cohesive force of the coating film, and the carboxyl group of the rosin interacts with the colorant to improve dispersion stability. The effects of (1) and (2) above improve adhesion, blocking resistance to anti-fog films, blocking resistance to vinyl chloride sheets, and printability. Furthermore, (3) the amide group is oriented on the surface of the ink film by containing a fatty acid amide (particularly a bisamide) and / or a polyamide, thereby reducing the interaction between the ink film and the substrate in contact with the ink film. The effects of (1) to (3) further improve adhesion, blocking resistance to anti-fog films, and blocking resistance to vinyl chloride sheets.

[0025] <Urethane resin (A)> The urethane resin (A) used in the present invention contains a polyester-derived structural unit consisting of a dibasic acid containing 80% by mass or more of an aliphatic dibasic acid having 7 to 16 carbon atoms and a diol, and its manufacturing method can be synthesized by the method described in, for example, JP-A-2013-256551 or JP-A-2016-043600. In a preferred embodiment, the urethane resin (A) has a urethane bond obtained by reacting a polyol containing a polyester polyol containing the above structural unit with a polyisocyanate. In addition, if necessary, the chain may be extended via a urea bond generated by the remaining isocyanate and a polyamine. The urethane resin (A) contains structural units derived from a polyester composed of an aliphatic dibasic acid and a diol, and the aliphatic dibasic acid contains 80% by mass or more of an aliphatic dibasic acid having 7 to 16 carbon atoms, thereby imparting adhesiveness and blocking resistance to the anti-fog film and contributing to solving the problems of the present application. The aliphatic dibasic acid carbon preferably contains 90% by mass or more, and even more preferably 95% by mass or more, of an aliphatic dibasic acid having 7 to 16 carbon atoms.

[0026] In addition, urethane resins other than the above-mentioned "urethane resin (A) containing structural units derived from a polyester composed of a dibasic acid containing 80% by mass or more of an aliphatic dibasic acid having 7 to 16 carbon atoms and a diol" may be contained within a range that does not impair the functions and effects of the present invention, and known urethane resins can be used.

[0027] (Polyol) The polyol preferably has about 1.7 to 2.3 hydroxyl groups on average in one molecule, more preferably 2 on average. Examples of the polyol include polyester polyols, polyether polyols such as polymers or copolymers of ethylene oxide, propylene oxide, tetrahydrofuran, etc., polycarbonate polyols, polybutadiene glycols, polyols obtained by adding ethylene oxide or propylene oxide to bisphenol A, dimer diols, castor oil polyols, and hydrogenated castor oil polyols, and may be used alone or in combination of two or more kinds. Also, a compound or raw material derived from biomass (biomass raw material) may be included as a component of the polyol.

[0028] In the present invention, among polyols, polyester polyols are preferred from the viewpoint of adhesion to the polyester film or polyolefin film that serves as the substrate. When two or more polyols are used in combination, the polyester polyol is preferably contained in an amount of 40 to 100 mass % based on the total mass of the polyols, more preferably 60 to 100 mass %, and further preferably 80 to 100 mass %, from the viewpoint of adhesion and blocking resistance.

[0029] The polyester polyol constituting the urethane resin (A) must contain a polyester-derived structural unit consisting of a dibasic acid and a diol, including an aliphatic dibasic acid having 7 to 16 carbon atoms. Examples of the aliphatic dibasic acid having 7 to 16 carbon atoms include pimelic acid (7 carbon atoms), suberic acid (8 carbon atoms), azelaic acid (9 carbon atoms), sebacic acid (10 carbon atoms), dodecanedioic acid (12 carbon atoms), and tetradecanedioic acid (14 carbon atoms). The number of carbon atoms of the aliphatic dibasic acid is preferably 8 to 14, and more preferably 9 to 12. When the number is within the above range, the adhesion and anti-fog film blocking properties are improved. Examples of the diol include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, methylpentanediol, hexadiol, octanediol, nonanediol, methylnonanediol, diethylene glycol, triethylene glycol, and dipropylene glycol.

[0030] The number average molecular weight of the polyol is preferably 300 or more, more preferably 500 to 6,000, and even more preferably 1,000 to 3,000, in order to maintain the solubility of the urethane resin (A) and the blocking resistance to the anti-fogging substrate.

[0031] (Aliphatic diol) The polyol constituting the urethane resin (A) preferably contains an aliphatic diol. Examples of the aliphatic diol include linear diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, and 1,9-nonanediol, branched diols such as 1,2-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, butylethylpropanediol, and methylnonanediol, and alicyclic diols such as cyclohexanedimethanol and cyclohexanediol, and may be used in combination. Among them, an aliphatic diol having an alkyl group having 1 to 6 carbon atoms as a substituent is preferable because of its excellent adhesion to polyolefin substrates and printability. More specifically, aliphatic diols having a molecular weight of 180 or less, such as 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, butylethylpropanediol, 2-methyl-1,3-propanediol, and neopentyl glycol, are preferably used.

[0032] The structural units derived from an aliphatic diol having a molecular weight of 180 or less increase the urethane bond density and impart crystallinity and cohesive strength, while the structural units derived from a polyol contribute to flexibility and adhesiveness. As a result, blocking resistance and adhesiveness are improved. The content of the structural units derived from the aliphatic diol (excluding the structural units contained in the polyol) in the total amount of the structural units derived from the polyol is preferably 10 to 60 mass%, more preferably 20 to 40 mass%. When it is within the above range, the cohesive strength of the urethane bonds obtained by reaction with isocyanate is improved, and the anti-blocking resistance of the anti-fog film is excellent.

[0033] Examples of other polyol components include aromatic diols and aliphatic diols having a molecular weight of more than 180, and these may be used in combination.

[0034] (Polyisocyanate) As the polyisocyanate, it is preferable to use a diisocyanate. For example, aromatic diisocyanates such as 1,5 naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, and tolylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, and 2,2,4 Examples of the diisocyanate include aliphatic diisocyanates such as 1-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, alicyclic diisocyanates such as 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, and m-tetramethylxylylene diisocyanate, and dimer diisocyanates in which the carboxyl groups of dimer acids are converted to isocyanate groups. Among these, isophorone diisocyanate and hexamethylene diisocyanate are preferred.

[0035] To obtain the urethane resin (A) used in the present invention, NCO derived from polyisocyanate is reacted with OH containing polyol and aliphatic diol so that the reaction molar ratio (NCO molar equivalent / OH molar equivalent) is 0.5 to 2, preferably 1.05 to 3, and then chain extension can be performed with polyamine as necessary. In addition, a reaction terminator can be further used to prevent overreaction.

[0036] The urethanization reaction may be carried out in an organic solvent or without a solvent. When using an organic solvent, it is advisable to select an appropriate solvent based on the reaction temperature, viscosity, and control of side reactions. When carrying out the urethanization reaction without a solvent, it is desirable to raise the temperature so that the viscosity is sufficient for stirring in order to obtain a uniform urethane resin (A). The urethanization reaction is desirably carried out for 10 minutes to 5 hours, and the end point of the reaction is determined by viscosity measurement, NCO-derived peak by IR measurement, NCO% measurement by titration, etc.

[0037] The polyamine used for chain extension is preferably an aliphatic diamine such as ethylenediamine, 1,4-butanediamine, isophoronediamine, aminoethylethanolamine, etc. Furthermore, as the chain extender, glycols such as ethylene glycol, propylene glycol, butylene glycol, diethylene glycol, triethylene glycol, etc. can also be used. Furthermore, as the reaction terminator, monoalcohols such as methanol and ethanol, alkylamines such as n-propylamine, n-butylamine, di-n-butylamine, etc., and alkanolamines such as monoethanolamine and diethanolamine can be mentioned.

[0038] The weight average molecular weight of the urethane resin (A) is preferably 8,000 to 80,000, more preferably 10,000 to 60,000, and even more preferably 20,000 to 50,000. The glass transition temperature is preferably 0°C or lower, more preferably -40°C to -5°C, and even more preferably -35 to -10°C. This is because the affinity with vinyl chloride resin or cellulose resin is good. The urethane resin (A) preferably has an amine value, and the amine value is more preferably 1 to 20 mgKOH / g, even more preferably 5 to 15 mgKOH / g, and particularly preferably 7 to 10 mgKOH / g. When it is within the above range, the adhesiveness is improved. The urethane bond concentration of the urethane resin (A) is preferably 0.5 to 4 mmol / g, more preferably 1.0 to 3.5 mmol / g, even more preferably 2 to 3 mmol / g, and particularly preferably 2.5 to 2.8 mmol / g. When it is within the above range, the adhesiveness, PVC blocking resistance, and anti-fog film blocking resistance are improved. The urea bond concentration of the urethane resin (A) is preferably 0.1 to 2.0 mmol / g, more preferably 0.4 to 1.7 mmol / g, and even more preferably 0.9 to 1.4 mmol / g. When it is within the above range, the adhesiveness, PVC blocking resistance, and anti-fog film blocking resistance are improved. The softening point of the urethane resin (A) is preferably 80 to 240°C, more preferably 110 to 210°C, and even more preferably 140 to 180°C. When it is within the above range, the PVC blocking resistance and anti-fog film blocking resistance are improved. The production method in the case where a urea bond is contained is not particularly limited, but it is preferable that the total number of amino groups in the chain extender and reaction terminator is within the range of 0.5 to 1.3 when the number of isocyanate groups in a prepolymer having an isocyanate group at its end obtained by reacting an aliphatic diol, a polyol, and a polyisocyanate is taken as 1.

[0039] (Urethane bond concentration) In the above, when (NCO molar equivalent / OH molar equivalent)>1, it is represented by the following formula (1). Formula (1) Urethane bond concentration (mmol / g) = total number of moles of hydroxyl groups (mmol) / total solid content (g) The total number of moles of hydroxyl groups refers to the total number of moles of hydroxyl groups contained in the polymer polyol, aliphatic diol, and other polyols used in the reaction to form the urethane, and the total solid content refers to the total mass of non-volatile components that become the urethane resin. In the above, when (NCO molar equivalent / OH molar equivalent)<1, it is represented by the following formula (2). Formula (2) Urethane bond concentration (mmol / g)=total number of moles of isocyanate groups (mmol) / total solid content (g) Here, the total number of moles of isocyanate groups refers to the total number of moles of isocyanate groups contained in the polyisocyanate used in the reaction to form urethane.

[0040] (urea bond concentration) When a prepolymer having a terminal isocyanate group is synthesized under the above condition of (NCO molar equivalent / OH molar equivalent)>1 and then chain-extended with polyamine to give a urethane resin having an amino group at its terminal, the product is represented by the following formula (3). Formula (3) Urea bond concentration (mmol / g) = [total number of moles of isocyanate groups (mmol) - total number of moles of hydroxyl groups (mmol)] / total solid content (g) When a prepolymer having a terminal isocyanate group is synthesized under the above condition of (NCO molar equivalent / OH molar equivalent)>1 and then chain-extended with polyamine to give a urethane resin having an isocyanate group at its terminal, the product is represented by the following formula (4). Formula (4) Urea binding concentration (mmol / g) = (total number of amino group moles (mmol)) / total solid content (g) The total number of moles of amino groups herein refers to the total number of moles of amino groups contained in the polyamine used to form urea bonds by reacting with a prepolymer having a terminal isocyanate group.

[0041] <Rosin resin> The rosin resin used in the present invention refers to one having a structural unit derived from rosin acid (abietic acid, neoabietic acid, palustric acid, pimaric acid, isopimaric acid, dehydroabietic acid, etc.) as the main component (50 mass% or more). The rosin acid or rosin resin may be hydrogenated. Examples of the rosin resin include rosin-modified phenolic resin, rosin-modified maleic acid resin, rosin ester, polymerized rosin resin, etc., and at least one rosin resin selected from these is preferable.

[0042] Rosin-modified maleic acid resin is a resin that has a structure derived from rosin and a structure derived from maleic acid and / or maleic anhydride. Rosin ester refers to a resin obtained by esterifying hydrogenated rosin with alcohol and then dehydrogenating the esterified product, or a resin obtained by esterifying hydrogenated rosin with alcohol in the presence of a dehydrogenation catalyst and dehydrogenating the esterified product.

[0043] Hydrogenated rosin is obtained by partially or completely hydrogenating gum rosin, wood rosin, or tall oil rosin, which contains resin acids such as abietic acid, palustric acid, neoabietic acid, pimaric acid, isopimaric acid, and dehydroabietic acid as its main components, and then purifying the resulting product. Examples of the alcohol component include monohydric alcohols such as n-octyl alcohol, 2-ethylhexyl alcohol, decyl alcohol, and lauryl alcohol; dihydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, and neopentyl glycol; trihydric alcohols such as glycerin, trimethylolethane, trimethylolpropane, and cyclohexanedimethanol; and tetrahydric alcohols such as pentaerythritol and diglycerin. An esterification catalyst is not necessarily required for the reaction, but an acid catalyst such as acetic acid or paratoluenesulfonic acid, an alkali metal hydroxide such as calcium hydroxide, or a metal oxide such as calcium oxide or magnesium oxide can be used to shorten the reaction time.

[0044] The acid value of the rosin resin is 50 to 250 mgKOH / g, more preferably 100 to 250 mgKOH / g, further preferably 150 to 250 mgKOH / g, and particularly preferably 180 to 220 mgKOH / g. When it is within the above range, the interaction with the pigment is improved, resulting in good printability. In addition, by using a rosin resin having an acid value of 50 to 250 mgKOH / g in combination with a chelating agent, the cohesive force of the coating film is improved by the interaction between them, forming a strong ink coating and improving the blocking resistance to the vinyl chloride sheet. The rosin resin having an acid value of 50 to 250 mgKOH / g is preferably contained in an amount of 0.1 to 5 mass% of the total mass of the gravure printing ink, more preferably 0.5 to 4%. In addition, it is preferably contained in an amount of 5 to 40 mass% of the total mass of the resin, more preferably 15 to 25%. In the above case, the blocking resistance to the vinyl chloride sheet and the blocking resistance to the anti-fog film are improved. The solid content ratio of the urethane resin (A) to the rosin resin is preferably 5:5 to 9.5:0.5, and more preferably 7:3 to 9:1. In this case, blocking resistance to the vinyl chloride sheet, blocking resistance to the anti-fog film, and printability are improved.

[0045] The softening point of the rosin resin is preferably 100 to 200°C, and more preferably 130 to 180°C. When it is within the above range, the adhesiveness is improved. The softening point is a value measured by the ring and ball method. The softening point can be measured, for example, by the measurement method described in JIS K2207.

[0046] The gravure printing ink for surface printing preferably further contains a vinyl chloride resin and / or a cellulose resin.

[0047] <Vinyl chloride resin> The vinyl chloride resin used in the present invention is not particularly limited as long as it contains a structural unit derived from vinyl chloride and a structural unit derived from another monomer. Examples of the vinyl chloride-vinyl acetate copolymer resin include vinyl chloride-acrylic acid copolymer resin, and the like, with vinyl chloride-vinyl acetate copolymer resin being preferred.

[0048] (Vinyl chloride-vinyl acetate copolymer resin) The vinyl chloride-vinyl acetate copolymer resin is obtained by copolymerizing vinyl chloride monomer and vinyl acetate monomer. The molecular weight is preferably 5,000 to 100,000 in weight average molecular weight, more preferably 20,000 to 70,000. The structure derived from vinyl acetate monomer in 100% by mass of the solid content of the vinyl chloride-vinyl acetate copolymer resin is preferably 1 to 30% by mass, more preferably 1 to 20% by mass, and the structure derived from vinyl chloride monomer is preferably 70 to 99% by mass, more preferably 80 to 99% by mass. In this case, the solubility in organic solvents is improved, and the adhesiveness and physical properties of the ink layer are further improved. In addition, it is preferable that the resin has a hydroxyl group, and it is obtained by further using vinyl alcohol in the copolymerization or by saponifying a part of vinyl acetate. The monomer ratio of vinyl chloride, vinyl acetate and vinyl alcohol affects the properties of the resin coating and the resin dissolution behavior. For example, vinyl chloride imparts toughness and hardness to the resin coating, vinyl acetate imparts adhesion and flexibility, and vinyl alcohol imparts good solubility in polar solvents. The hydroxyl value of the vinyl chloride-vinyl acetate copolymer resin is preferably 50 to 180 mgKOH / g, more preferably 70 to 160 mgKOH / g. The glass transition temperature is preferably 50°C to 90°C, more preferably 60 to 80°C.

[0049] The combination of the urethane resin (A) and the vinyl chloride resin improves the blocking resistance of the anti-fog film. When other resins are used in combination, the total amount of the urethane resin (A) and the vinyl chloride resin is preferably 60 to 100 mass%, more preferably 80 to 100 mass%, of the total amount of the resin. This is because the adhesiveness is improved. Furthermore, the solid content mass ratio of the urethane resin (A) to the vinyl chloride resin (urethane resin / vinyl chloride resin) is preferably 95 / 5 to 50 / 50, more preferably 95 / 5 to 60 / 40, and even more preferably 95 / 5 to 70 / 30. With this blending ratio and combination, the adhesiveness, blocking resistance, and printability are excellent.

[0050] <Cellulose-based resin> Examples of the cellulose-based resin include cellulose acetate propionate, cellulose acetate butyrate and other cellulose ester resins, nitrocellulose, hydroxyalkylcellulose, carboxyalkylcellulose, etc. The cellulose ester resin preferably has an alkyl group, and examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a pentyl group, a hexyl group, etc., and the alkyl group may further have a substituent. Of the above, the cellulose-based resin is preferably cellulose acetate propionate, cellulose acetate butyrate, and nitrocellulose. Nitrocellulose is particularly preferred. The molecular weight is preferably 5,000 to 200,000 in weight average molecular weight, more preferably 10,000 to 50,000. The glass transition temperature is preferably 120°C to 180°C, more preferably 140°C to 180°C. This is because the ink film properties such as blocking resistance are further improved by using it in combination with the urethane resin (A).

[0051] (nitrocellulose) The nitrocellulose is preferably obtained as a nitric acid ester by reacting native cellulose with nitric acid to replace three hydroxyl groups in a six-membered ring of an anhydrous glucopyranose group in the native cellulose with nitric acid groups, and has an average degree of polymerization of 20 to 200, more preferably 30 to 150. When the average degree of polymerization is 20 or more, the strength of the ink layer is improved and the abrasion resistance is improved. When the average degree of polymerization is 200 or less, the solubility in the solvent, the low-temperature stability of the ink, and the compatibility with the co-used resin are improved. The molecular weight is preferably 5,000 to 200,000 in weight average molecular weight, more preferably 7,500 to 100,000, and even more preferably 10,000 to 50,000. In addition, the glass transition temperature is preferably 120°C to 180°C, more preferably 140 to 180°C, and the nitrogen content is preferably 10.5 to 12.5% ​​by mass. Preferred nitrocellulose resins include the TR series (manufactured by TNC INDUSTRIAL) and the DLX series (manufactured by Nobel Enterprises).

[0052] The combination of the urethane resin (A) and the cellulose-based resin improves the blocking resistance of the anti-fog film. The solid content mass ratio of the urethane resin (A) to the cellulose-based resin is preferably 95 / 5 to 40 / 60, more preferably 95 / 5 to 50 / 50, and even more preferably 95 / 5 to 60 / 40. This is because, with this combination and blending ratio, various resistances of the printing ink layer, such as adhesion and blocking resistance, become good.

[0053] <Chelating agent> The gravure printing ink for front printing of the present invention contains a chelating agent. By containing a chelating agent, the cohesive force in the ink coating is improved, and the adhesion to the substrate is improved. Examples of the chelating agent include organic titanium compounds and organic zirconium compounds, and titanium chelates having a Ti-OC type bond in one molecule are preferred. Although titanium chelates generally require heating to complete the crosslinking reaction, they are less likely to hydrolyze at room temperature and have excellent stability, making them suitable for use in inks and suitable for use. Specifically, titanium chelates include titanium alkoxides such as tetraisopropyl titanate, tetra-normal-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate, tetramethyl titanate, and tetrastearyl titanate, and titanium chelates such as triethanolamine titanate, titanium acetylacetonate, titanium ethyl acetoacetate, titanium lactate, octylene glycol titanate, and titanium tetraacetylacetonate. An example of a zirconium chelate having a Zr-OC type bond in one molecule is zirconium ethylacetoacetate.

[0054] Among them, it is preferable to use acetylacetone-based titanium chelate and / or alkyl acetoacetate-based titanium chelate, more preferable to use acetylacetone-based titanium chelate having alkoxy group and / or alkyl acetoacetate-based titanium chelate having alkoxy group, and more preferable to use acetylacetone-based titanium chelate having alkoxy group and alkyl acetoacetate-based titanium chelate having alkoxy group in combination. In the above case, adhesion, anti-blocking property of anti-fog film, and printability are improved. Furthermore, by using the rosin resin and the acetylacetone-based titanium chelate and / or the alkyl acetoacetate-based titanium chelate, the PVC blocking resistance is further improved. In order to achieve both adhesion to the substrate and PVC blocking resistance, the mass ratio of the rosin resin to the acetylacetone-based titanium chelate and / or the alkyl acetoacetate-based titanium chelate is preferably 10:90 to 90:10, more preferably 15:85 to 60:40, and particularly preferably 20:80 to 40:60.

[0055] The chelating agent is preferably contained in an amount of 0.1 to 5 mass % based on the total mass of the gravure printing ink, and more preferably 0.3 to 3 mass %. When the amount is 0.1 mass % or more, the adhesion and blocking resistance are improved. When the amount is 5 mass % or less, the storage stability and printability of the ink are improved.

[0056] <Fatty acid amide, polyamide resin> In the gravure printing ink for front printing of the present invention, it is preferable to further use a fatty acid amide and / or a polyamide resin. In this application, fatty acid amide refers to a compound having a fatty acid residue and an amide group or an amide bond, and includes monoamides in which the total number of amide groups and amide bonds is 1, and bisamides in which the total number of amide groups and amide bonds is 2, and polyamide resin refers to a resin having an amide group or amide bond, and the total number of amide groups and amide bonds is 3 or more. Among them, polyamide resins and bisamides are preferable, and bisamides are more preferable. Bisamides have more amide groups per molecule than monoamides, and have a relatively lower weight average molecular weight than polyamide resins, which have more amide groups per molecule. Therefore, in the case of bisamides, there are more amide groups oriented on the surface of the ink film compared to monoamides and polyamides, and it is thought that blocking resistance is further improved by the effect of reducing the interaction between the ink film and the substrate in contact with it.

[0057] The fatty acid constituting the fatty acid amide may be a saturated fatty acid and / or an unsaturated fatty acid, with an unsaturated fatty acid being preferred. The saturated fatty acid is preferably a saturated fatty acid having 10 to 22 carbon atoms, more preferably a saturated fatty acid having 12 to 18 carbon atoms. The unsaturated fatty acid is preferably an unsaturated fatty acid having 16 to 25 carbon atoms, more preferably an unsaturated fatty acid having 18 to 22 carbon atoms. Examples of saturated fatty acids include lauric acid, palmitic acid, stearic acid, behenic acid, and hydroxystearic acid, and examples of unsaturated fatty acids include oleic acid and erucic acid. Bisamides made of unsaturated fatty acids are particularly preferred from the standpoints of anti-fog film blocking resistance, solubility in organic solvents and printability.

[0058] (monoamide) The monoamide is represented by the following general formula (5) or general formula (6). General formula (5) R 1 -CONH General formula (6) R 2 -CONH-R 3 (In the formula, R 1 , R 2、 and R 3 represents an aliphatic hydrocarbon group having 10 to 25 carbon atoms, and may be the same or different.)

[0059] Examples of monoamides include lauric acid amide, palmitic acid amide, stearic acid amide, hydroxystearic acid amide, behenic acid amide, oleic acid amide, erucic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, N-stearyl erucic acid amide, N-oleyl palmitic acid amide, N-oleyl oleic acid amide, and the like. Palmitic acid amide, oleic acid amide, and erucic acid amide are preferred, and oleic acid amide and erucic acid amide are more preferred.

[0060] (Bisamide) The bisamide is represented by the following general formula (7) or general formula (8). General formula (7) R 4 -CONH-R 5 -HNCO-R 6 General formula (8) R 7 -NHCO-R 8 -CONH-R 9 (In the formula, R 4 , R 6 , R 7 , and R 9 represents an aliphatic hydrocarbon group having 10 to 25 carbon atoms, which may be the same or different, R 5 and R 8 represents an alkylene group or an arylene group.

[0061] In addition, bisamides other than those represented by the above general formula (7) or (8) may be contained within the scope of the invention without impairing the functions and effects thereof, and known bisamides can be used.

[0062] Examples of bisamides include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene bishydroxystearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, and hexamethylene bisoleic acid amide. , N,N'-distearyl adipamide, N,N'-distearyl sebacic acid amide, N,N'-dioleyl adipamide, N,N'-dioleyl sebacic acid amide, etc. are included, of which ethylene bisstearic acid amide, ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, and N,N'-dioleyl adipamide are preferred, and ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, and N,N'-dioleyl adipamide are more preferred.

[0063] The weight average molecular weight of the fatty acid amide is preferably 500 to 2,000, more preferably 550 to 1,750, and even more preferably 600 to 1,500. When the weight average molecular weight is 500 or more, blocking resistance is improved. When the molecular weight is 5,000 or less, the fatty acid amide is easily oriented on the surface of the ink film after printing, and the fatty acid amide exhibits slip properties and good blocking resistance. The content of the fatty acid amide in the ink composition is preferably 0.1 to 5% by mass, and more preferably 0.2 to 4% by mass. When the content is 0.1% by mass or more, blocking resistance is improved, and when the content is 5% by mass or less, printability is improved.

[0064] The softening point of the fatty acid amide is preferably 80 to 160°C, more preferably 90 to 130°C. In the above range, the ink film is strong. When the softening point is 80°C or higher, the surface tack of the ink film on the printed matter is easily removed, preventing blocking. When the softening point is 140°C or lower, the ink film becomes flexible and the adhesion is improved.

[0065] (Polyamide resin) The polyamide resin used in the present invention is not limited to the following, but is preferably a thermoplastic polyamide soluble in an organic solvent that can be obtained by polycondensation of a polybasic acid and a polyamine. In particular, it is more preferable that the polyamide resin contains a reaction product of an acid component containing a polymerized fatty acid and / or a dimer acid with an aliphatic and / or aromatic polyamine, and further preferably that the polyamide resin contains a portion of a primary and secondary monoamine.

[0066] Examples of polybasic acids used as raw materials for polyamide resins include, but are not limited to, adipic acid, sebacic acid, azelaic acid, phthalic anhydride, isophthalic acid, suberic acid, glutaric acid, fumaric acid, pimelic acid, oxalic acid, malonic acid, succinic acid, maleic acid, terephthalic acid, 1,4-cyclohexyldicarboxylic acid, trimellitic acid, dimer acid, hydrogenated dimer acid, and polymerized fatty acid. Among these, polyamide resins containing a structure derived from dimer acid or polymerized fatty acid (50% by mass or more in the polyamide resin) are preferred. Here, polymerized fatty acid is obtained by cyclization reaction of unsaturated fatty acid, and includes monobasic fatty acid, dimerized polymerized fatty acid (dimer acid), trimerized polymerized fatty acid, and the like. In addition, fatty acids constituting polymerized fatty acid or dimer acid can be preferably derived from natural oils such as soybean oil, palm oil, and rice bran oil, and those obtained from oleic acid and linoleic acid are preferred. The polybasic acid may be used in combination with a monocarboxylic acid, such as acetic acid, propionic acid, lauric acid, palmitic acid, benzoic acid, or cyclohexane carboxylic acid.

[0067] Examples of polyamines used as raw materials for polyamide resins include polyamines and primary or secondary monoamines. Examples of polyamines include aliphatic diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, and methylaminopropylamine; aliphatic polyamines such as diethylenetriamine and triethylenetetramine; alicyclic polyamines such as cyclohexylenediamine and isophoronediamine; aromatic aliphatic polyamines such as xylylenediamine; and aromatic polyamines such as phenylenediamine and diaminodiphenylmethane. Further, primary and secondary monoamines include n-butylamine, octylamine, diethylamine, monoethanolamine, monopropanolamine, diethanolamine, dipropanolamine, and the like.

[0068] The weight-average molecular weight of the polyamide resin is preferably 1,000 to 20,000, more preferably 3,000 to 14,000, and even more preferably 6,000 to 10,000. When the weight-average molecular weight is 500 or more, blocking resistance is improved. When the molecular weight is 20,000 or less, the polyamide resin is easily oriented on the surface of the ink film after printing, and the ink exhibits slip properties, resulting in good blocking resistance. The polyamide resin is preferably contained in the ink composition in an amount of 0.1 to 5% by mass, more preferably 0.2 to 4% by mass. When the content is 0.1% by mass or more, blocking resistance is improved, and when the content is 5% by mass or less, printability is improved.

[0069] The softening point of the polyamide resin is preferably 80 to 150°C, more preferably 90 to 130°C. Within the above range, the ink film is strong. When the softening point is 80°C or higher, the surface tack of the ink film on the printed matter is easily removed, preventing blocking. When the softening point is 140°C or lower, the ink film becomes flexible and the adhesion is improved.

[0070] <Hydrocarbon wax particles> The gravure printing ink for front printing of the present invention preferably further contains hydrocarbon wax particles. Examples of the hydrocarbon wax include polyolefin wax and paraffin wax, and the content of the wax in the ink composition is preferably 0.1 to 3 mass %, more preferably 0.3 to 2.5 mass %. The blocking resistance is further improved by using the wax in combination with the binder resin of the present invention.

[0071] The hardness (penetration) of the hydrocarbon wax at 25°C as specified by JISK2207 is preferably 12 or less, more preferably 0.5 to 10, and even more preferably 1 to 8. When it is within the above range, blocking resistance is good. The density of the hydrocarbon wax at 23°C as specified by JISK7112 (Method B) is 900 to 990 kg / m 3 It is preferable that the viscosity is 925 to 990 kg / m 3It is more preferable that the melting point is within the above range. When it is within the above range, the blocking resistance is good. The melting point of the hydrocarbon wax in DSC measurement is preferably 90 to 150°C, and more preferably 100 to 125°C. When it is within the above range, the blocking resistance is good. The melting point of the hydrocarbon wax refers to the melting point of the peak top (minimum value) of the endothermic peak in the DSC temperature rise curve. The average particle size of the hydrocarbon wax is preferably 0.5 to 12 μm, more preferably 1 to 10 μm, and even more preferably 1.5 to 4 μm. The average particle size of the hydrocarbon wax refers to the D50 value measured by dynamic light scattering.

[0072] <Colorants, pigments> The gravure printing ink for surface printing of the present invention may contain a colorant. Examples of the colorant include pigments. The pigments that can be used in the present invention are not particularly limited, and various inorganic pigments and organic pigments that can be used in general printing inks and paints can be suitably used. Examples of inorganic pigments include colored pigments such as titanium oxide, red iron oxide, Prussian blue, ultramarine blue, carbon black, and graphite, and extender pigments such as calcium carbonate, kaolin, clay, barium sulfate, aluminum hydroxide, and talc. Examples of organic pigments include soluble azo pigments, insoluble azo pigments, azo lake pigments, condensed azo pigments, copper phthalocyanine pigments, and condensed polycyclic pigments. However, the pigments are not limited to these, and those listed by generic names in the Color Index can be used as appropriate. The content of these pigments is preferably 0.5 to 50% by mass in the total amount of ink.

[0073] <Additives> Various additives may be used in the gravure printing ink for front printing of the present invention, if necessary. Examples include pigment dispersants, extender pigments, inorganic fine particles, leveling agents, and adhesion aids. Specific examples include various additives such as pigment dispersants for improving the dispersibility of pigments, extender pigments for improving drying properties and coating film hiding properties, inorganic fine particles for imparting anti-slip properties, leveling agents for improving leveling properties, antifoaming agents for imparting antifoaming properties, and adhesion aids for improving adhesion to substrates.

[0074] <Organic solvent> The solvents used in the ink composition of the present invention include mainly alcohol-based organic solvents such as methanol, ethanol, n-propanol, isopropanol, and butanol, ketone-based organic solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ester-based organic solvents such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate, aliphatic hydrocarbon-based organic solvents such as n-hexane, n-heptane, and n-octane, and alicyclic hydrocarbon-based organic solvents such as cyclohexane, methylcyclohexane, ethylcyclohexane, cycloheptane, and cyclooctane. Taking into consideration the solubility and drying properties of the binder resin, it is preferable to use them in a mixed state. The amount of these organic solvents used is preferably 20% by mass or more in the total amount of ink. In addition, in order to deal with odors during printing and environmental issues, it is preferable that the organic solvent is mainly composed of a mixed solvent of an ester-based organic solvent and an alcohol-based organic solvent, and the mass ratio (ester-based organic solvent:alcohol-based organic solvent) is preferably 50:50 to 90:10.

[0075] <Manufacture of gravure printing ink for surface printing> The method for producing the gravure printing ink for front printing of the present invention includes a method in which a composition containing a pigment, a binder resin such as a urethane resin (A), a chelating agent, an organic solvent, and, if necessary, a fatty acid amide and / or polyamide resin, hydrocarbon wax particles, and other additives is first uniformly stirred and mixed using a bladed stirrer, and then dispersed using various mills such as a bead mill, ball mill, sand mill, attritor, roll mill, pearl mill, etc., and then other resins, additives, etc. are mixed in. Among these, it is preferable to knead and disperse the composition containing the pigment using a bead mill.

[0076] <Base material> The printing ink of the present invention is printed on a substrate to produce a printed matter. The substrate is not particularly limited, but is preferably a film substrate, and examples thereof include polyolefin substrates such as polyethylene and polypropylene, polyester substrates such as polyethylene terephthalate, polycarbonate, and polylactic acid, polystyrene-based substrates such as polystyrene, AS resin, and ABS resin, nylon substrates, polyamide substrates, polyvinyl chloride substrates, polyvinylidene chloride substrates, and cellophane substrates, as well as film substrates made of composite materials thereof. The substrate may be vapor-deposited with a metal or metal oxide such as silica, alumina, or aluminum, and the vapor-deposited surface may be coated with a paint such as polyvinyl alcohol. Generally, the substrate surface to be printed is often subjected to a surface treatment such as corona treatment. Furthermore, the substrate may be a film that has been previously coated or kneaded with an anti-fogging agent, or surface coated or kneaded with a matting agent. The substrate may be a single layer, or may be a laminate (substrate layer) in which two or more substrates are laminated. The substrates constituting the substrate layer may be the same or different. Among these, polyolefin substrates are preferred. The polyolefin substrate may or may not be surface-treated.

[0077] <Printed material> A printed matter is formed by printing a gravure printing ink for surface printing on a substrate. After printing on a substrate using the gravure printing ink for surface printing of the present invention, an ink layer is formed by removing volatile components, and a printed matter can be obtained. The printing method is a gravure printing method, and for example, the ink is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing, and is supplied to each printing unit alone or in a mixture and printed. Then, the ink layer is fixed by drying in an oven to obtain the printed matter. EXAMPLES

[0078] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the present invention, parts and % represent parts by mass and % by mass unless otherwise noted.

[0079] <Weight average molecular weight and number average molecular weight> The weight average molecular weight (Mw) and number average molecular weight (Mn) were determined by GPC (gel permeation chromatography). The molecular weight distribution was measured using "Shodex GPC-104" manufactured by Showa Denko K.K., and the polystyrene equivalent molecular weight was determined. The measurement conditions are as follows. Column: The following multiple columns are connected in series. Showa Denko Shodex LF-404 x 2 Showa Denko Shodex LF-G Detector: RI (differential refractometer), Column temperature: 40°C, Eluent: Tetrahydrofuran Flow rate: 0.3mL / min

[0080] <Acid value> The acid value is the number of milligrams of potassium hydroxide required to neutralize the free fatty acids, resin acids, etc. contained in 1 g of a sample, and was measured by the method described in JIS K 0070.

[0081] <Amine value> The amine value was measured according to the following method in accordance with JIS K0070 (1992). -Method for measuring amine value Accurately weigh out 0.5 to 2 g of sample (sample amount: Sg). Add 30 mL of neutral ethanol (BDG neutral) to the weighed sample to dissolve it. Titrate the resulting solution using 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The endpoint is when the color of the solution changes from green to yellow. Using the titration amount (A mL) at this point, calculate the amine value using the following (Equation 9). (Equation 9) Amine value = (A x f x 0.2 x 56.108) / S

[0082] <Softening point> The softening point was measured using an automatic ring and ball softening point tester OSK-40DP-81PV0144 (manufactured by Ogawa Seiki Co., Ltd.) according to the ring and ball softening point test method in accordance with Japanese Industrial Standards JIS K 6863-1944.

[0083] <Synthesis Example 1> <Preparation of urethane resin (A) solution PU1> A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser and a nitrogen gas inlet tube was charged with 103.2 parts of polyester polyol, which is a condensate of 3-methyl-1,5-pentanediol with a number average molecular weight of 2000 and sebacic acid, 35.2 parts of neopentyl glycol, 121.4 parts of isophorone diisocyanate, 0.03 parts of stannous 2-ethylhexyl acid and 65.1 parts of ethyl acetate, and reacted for 2 hours at 90°C under a nitrogen stream, and 165.3 parts of ethyl acetate was added and cooled to obtain 490.2 parts of a solvent solution of terminal isocyanate prepolymer. Next, 490.2 parts of the obtained terminal isocyanate prepolymer was gradually added at room temperature to a mixture of 33.6 parts of isophorone diamine, 1.2 parts of di-n-butylamine, 237.5 parts of ethyl acetate and 200.6 parts of isopropyl alcohol, and then reacted at 50°C for 1 hour. Thereafter, 5.3 parts of isophorone diisocyanate was added to adjust the viscosity, and then the solid content was adjusted to 30% with a solvent obtained by mixing ethyl acetate and isopropyl alcohol in a mass ratio of 2 / 1 to obtain a urethane resin (A) solution PU1 having a content of aliphatic dibasic acids having 7 to 16 carbon atoms of 100 mass%, a softening point of 161°C, a urethane bond concentration of 2.6 mmol / g, a urea bond concentration of 1.2 mmol / g, an amine value of 8.2 mgKOH / g, and a weight average molecular weight of 40,000.

[0084] <Synthesis Examples 2 to 7> (Synthesis of Urethane Resins (A) PU2 to PU7) Urethane resins (A) (PU2) to (PU7) were synthesized in the same manner as in Synthesis Example 1, except that the compositions and raw materials were used as shown in Table 1. The abbreviations in Table 1 are as follows. MPD: 3-methyl-1,5-pentanediol SeA: Sebacic acid AdA: adipic acid NPG: Neopentyl glycol IPA: Isopropyl alcohol MPD / SeA: A polyester polyol with a number average molecular weight of 2,000, which is a dehydration condensation product of MPD and SeA. MPD / AdA·SeA: A polyester polyol with a number average molecular weight of 2,000, which is a dehydration condensation product of MPD and AdA·SeA.

[0085] [Table 1]

[0086] <Preparation of vinyl chloride-vinyl acetate copolymer resin solution> 20 parts of vinyl chloride-vinyl acetate copolymer resin (hydroxyl value: 154 mgKOH / g, weight average molecular weight: 28,000, glass transition temperature: 78°C) was mixed and dissolved in 80 parts of ethyl acetate to obtain a vinyl chloride-vinyl acetate copolymer resin solution with a solid content of 20%. <Preparation of vinyl chloride-acrylic acid copolymer resin solution> 20 parts of vinyl chloride-acrylic acid copolymer resin (hydroxyl value: 59 mgKOH / g, weight average molecular weight: 45,000, glass transition temperature: 69°C) was mixed and dissolved in 80 parts of ethyl acetate to obtain a vinyl chloride-acrylic acid copolymer resin solution with a solid content of 20%.

[0087] <Preparation of nitrocellulose solution> 20 parts of isopropyl alcohol-wet nitrocellulose (product name NC TR2, manufactured by TNC INDUSTRIAL) was dissolved in 80 parts of a mixed solvent consisting of n-propyl acetate: ethyl acetate: isopropyl alcohol: methylcyclohexane = 20:20:20:40 (weight ratio) to obtain a nitrocellulose solution with a solid content of 20%. <Preparation of Cellulose Acetate Butyrate Solution> 20 parts of cellulose acetate butyrate (manufactured by EASTMAN CHEMICAL, product name CAB553-0.4, glass transition temperature: 136°C, weight average molecular weight: 20,000) was mixed and dissolved in 80 parts of a mixed solvent consisting of ethyl acetate:isopropyl alcohol:=50:50 (weight ratio) to obtain a cellulose acetate butyrate solution with a solid content of 20%.

[0088] <Rosin resin> Rosin resin (1) Acid value 200, softening point 160°C (Harima Chemicals, Harimax AS-5) Rosin resin (2): acid value 100, softening point 175°C (Arakawa Chemical Industries, Marquid 3002) Rosin resin (3): acid value 20, softening point 145°C (Arakawa Chemical Industries, Marquid 5) Rosin resin (4): acid value 300, softening point 150°C (Arakawa Chemical Industries, Marquid 33) 50 parts of each rosin resin was mixed and dissolved in 50 parts of a mixed solvent consisting of ethyl acetate:isopropyl alcohol=50:50 (weight ratio) to obtain a rosin resin solution with a solid content of 50%.

[0089] <Chelating agent> Titanium chelate (1): Titanium diisopropoxybis(acetylacetonate) (ingredients concentration 75%, isopropyl alcohol 25%) Titanium chelate (2): Titanium diisopropoxybis(ethyl acetoacetate) (ingredients concentration 75%, isopropyl alcohol 25%) Zirconium chelate: Zirconium ethyl acetoacetate (ingredients concentration 75%, butyl alcohol 25%)

[0090] <Fatty acid amide and polyamide resins> Bisamide (1): Hexamethylene bisoleic acid amide (Mw) 650 Bisamide (2): Ethylene bis oleamide (Mw) 590 Bisamide (3): Ethylene bisstearic acid amide (Mw) 590 Monoamide: Oleic acid amide (Mw) 280 Polyamide (1): (Mw) 8,000 (Harima Chemicals, product name: Newmide 838) Polyamide (2): (Mw) 15,000 (manufactured by Sanyo Chemical Industries, product name Polyamide S-1962)

[0091] <Hydrocarbon wax> Polyethylene wax (Mitsui Chemicals, product name Hiwax 320MP, molecular weight: 3,000, density: 930, melting point 107°C, softening point 114°C, hardness (penetration): 7)

[0092] <Example 1> A gravure printing ink for surface printing (ink S1) was prepared by kneading 10 parts of a phthalocyanine blue pigment (Leonol Blue FG-7400G (CI Pigment Blue 15:4) manufactured by Toyo Color Co., Ltd.), 34 parts of a urethane resin (A) (PU1), 6 parts of a vinyl chloride-vinyl acetate copolymer resin solution, 5 parts of a rosin resin solution, 1 part of a bisamide (1), 0.5 parts of a titanium chelate (1), 1.3 parts of a titanium chelate (2), 1 part of a polyethylene wax, and 41.2 parts of a mixed solvent consisting of n-propyl acetate: ethyl acetate: isopropyl alcohol: methylcyclohexane = 35: 30: 20: 15 (weight ratio) with a sand mill (Eiger mill).

[0093] <Examples 2 to 22> Gravure printing ink compositions for surface printing (inks S2 to S22) were obtained in the same manner as in Example 1, except that the raw materials and compounding ratios shown in Table 2 were used.

[0094] <Comparative Examples 1 to 6> Gravure printing ink compositions for surface printing (inks T1 to T6) were obtained in the same manner as in Example 1, except that the raw materials and compounding ratios shown in Table 3 were used.

[0095] <Production of gravure printed materials for surface printing (printing)> The gravure printing ink for front printing obtained in Example 1 was diluted with a dilution solvent (n-propyl acetate: ethyl acetate: isopropyl alcohol: mesylcyclohexane = 35:30:20:15 (weight ratio)) and adjusted to 15 seconds using a Zahn cup No. 3 to prepare diluted ink for printing. Next, a corona discharge weakly treated polypropylene film (D-SHNY01, 28 μm, manufactured by DIC Corporation) or an anti-fog film (AF-642S 25 μm, manufactured by Futamura Chemical Co., Ltd.) was printed with a etched plate with a plate depth of 30 microns using a gravure proofing press (drying temperature 50° C., printing speed 50 m / min) to obtain a print.

[0096] Polypropylene film prints and anti-fog film prints were obtained in the same manner as above, except that the gravure printing inks for surface printing obtained in Examples 2 to 22 were used.

[0097] Polypropylene film prints and anti-fog film prints were obtained in the same manner as above, except that the gravure printing inks for surface printing obtained in Comparative Examples 1 to 6 were used.

[0098] The gravure printing inks for surface printing and their printed matter obtained in Examples 1 to 22 and Comparative Examples 1 to 6 were used to carry out the evaluations described below. The results are shown in Tables 2 and 3.

[0099] <Adhesiveness> Adhesive tape (product name: cellophane tape) was applied to the ink-coated surface of the printed matter on the polypropylene film of Examples 1 to 22 and Comparative Examples 1 to 6, and the adhesiveness was evaluated based on the degree to which the ink-coated film peeled off from the film when the tape was quickly peeled off. The evaluation was performed after leaving the printed matter at 25°C for 24 hours after printing. Evaluation criteria A. The ink layer is not removed from the film. B. The ink layer has been removed from the film and the area that has peeled off from the film is less than 5%. C. The area of ​​the ink layer that has peeled off from the film is 5% or more but less than 15%. D. The area of ​​the ink layer that has peeled off from the film is 15% or more but less than 50%. E. The area of ​​the ink layer that has peeled off from the film is 50% or more. Incidentally, A, B and C are within the ranges where there are no practical problems.

[0100] <PVC blocking resistance> The prints on the polypropylene film of Examples 1 to 22 and Comparative Examples 1 to 6 were cut into 4 cm squares, and a soft polyvinyl chloride sheet cut to the same size was placed on top of the ink-coated surface of the prints, and the prints were pressed against each other with a pressure of 0.5 kg / cm. 2After applying a load of 10 ... Evaluation criteria A. The ink layer is not removed from the film. B. The ink layer has been removed from the film and the area that has peeled off from the film is less than 5%. C. The area of ​​the ink layer that has peeled off from the film is 5% or more but less than 15%. D. The area of ​​the ink layer that has peeled off from the film is 15% or more but less than 50%. E. The area of ​​the ink layer that has peeled off from the film is 50% or more. Incidentally, A, B and C are within the ranges where there are no practical problems.

[0101] <Anti-fog film blocking resistance> The surface-printed gravure prints printed on the anti-fog films of Examples 1 to 22 and Comparative Examples 1 to 6 were subjected to a pressure of 100 kg / cm 2 The printed matter was then wound up under a load of 0.01 g and left for 24 hours in an atmosphere at 60° C. After that, the printed surface and the non-printed surface of the wound printed matter were peeled off, and the blocking resistance was evaluated based on the degree of ink peeling. Evaluation criteria A. The ink layer is not removed from the film. B. The ink layer has been removed from the film and the area that has peeled off from the film is less than 5%. C. The area of ​​the ink layer that has peeled off from the film is 5% or more but less than 15%. D. The area of ​​the ink layer that has peeled off from the film is 15% or more but less than 50%. E. The area of ​​the ink layer that has peeled off from the film is 50% or more. Incidentally, A, B and C are within the ranges where there are no practical problems.

[0102] <Printability> The gravure printing inks for front printing obtained in Examples 1 to 22 and Comparative Examples 1 to 6 were adjusted in viscosity to 15 seconds (25°C) using a Zahn cup No. 3 with a dilution solvent (n-propyl acetate: ethyl acetate: isopropyl alcohol: methylcyclohexane = 35:30:20:15 (weight ratio)), and the plate was run on a printing press at a printing speed of 300 m / min for 90 minutes at room temperature of 35°C and humidity of 80%, after which the area of ​​the plate fogging portion was visually determined and evaluated. Evaluation criteria A. The plate cover cannot be visually confirmed. B. The plate cover can be visually confirmed and the plate cover area is less than 5%. C. Plate cover area is 5% or more but less than 10% D. Plate cover area is 10% or more but less than 20% E. Plate cover area is 20% or more Incidentally, A, B and C are within the ranges where there are no practical problems.

[0103] [Table 2]

[0104] [Table 3]

[0105] From the above, in Comparative Example 1, the aliphatic dibasic acid in the urethane resin (A) did not contain 80 mass% or more of an aliphatic dibasic acid having 7 to 16 carbon atoms, so the adhesion and anti-fog film blocking resistance were poor. In Comparative Example 2, the urethane resin (A) was not contained, so the adhesion, PVC blocking resistance, anti-fog film blocking resistance, and printability were poor. In Comparative Example 3, the rosin resin was not contained, so the PVC blocking resistance, anti-fog film blocking resistance, and printability were poor. In Comparative Example 4, the acid value of the rosin resin was less than 50 mgKOH / g, so the PVC blocking resistance, anti-fog film blocking resistance, and printability were poor. In Comparative Example 5, the acid value of the rosin resin was more than 250 mgKOH / g, so the anti-fog film blocking resistance was poor. In Comparative Example 6, since no chelating agent was contained, the PVC blocking resistance, anti-fog film blocking resistance, and printability were poor. On the other hand, in the examples, a gravure printing ink for surface printing containing a urethane resin (A), a rosin resin, a chelating agent, and an organic solvent is used, and the urethane resin (A) contains a polyester-derived structural unit consisting of an aliphatic dibasic acid and a diol, the aliphatic dibasic acid contains 80 mass% or more of an aliphatic dibasic acid having 7 to 16 carbon atoms, and the acid value of the rosin resin is 50 to 250 mgKOH / g, so that the ink had good adhesion, PVC blocking resistance, anti-fog film blocking resistance, and printability. In particular, with regard to blocking resistance, the printed matter is stored in a state of being wound around a paper tube, so that the printing layer and the printing substrate are in contact with each other during storage and are under a load. In particular, the load applied to the printed matter becomes larger toward the center of the winding, making blocking very likely to occur, and therefore high blocking resistance is required. Therefore, the anti-fog film blocking resistance test in the present invention was carried out under unprecedented high load conditions. In addition, with regard to printability, due to the influence of recent global warming, there is a demand for adaptability to printing environments under high temperature and high humidity, and high-speed printing is also required from the viewpoint of production efficiency. Therefore, the printability test of the present invention was carried out under unprecedented conditions of high temperature, high humidity, and high-speed printing (idling). Even under these conditions, the ink of the present invention had good anti-fog film blocking properties and printability.

Claims

1. A gravure printing ink for surface printing, comprising a urethane resin (A), a rosin resin, a chelating agent, and an organic solvent, The urethane resin (A) contains a structural unit derived from a polyester composed of an aliphatic dibasic acid and a diol, The aliphatic dibasic acid contains 80% by mass or more of an aliphatic dibasic acid having 7 to 16 carbon atoms, The rosin resin has an acid value of 50 to 250 mgKOH / g.

2. 2. The gravure printing ink for surface printing according to claim 1, wherein the amine value of the urethane resin (A) is 1 to 20 mgKOH / g.

3. The gravure printing ink for surface printing according to claim 1 , further comprising a vinyl chloride resin and / or a cellulose resin.

4. 2. The gravure printing ink for front printing according to claim 1, wherein the chelating agent comprises an acetylacetone-based titanium chelate and / or an alkyl acetoacetate-based titanium chelate.

5. The gravure printing ink for surface printing according to claim 1, further comprising a fatty acid amide and / or a polyamide resin.

6. 6. The gravure printing ink for surface printing according to claim 5, wherein the fatty acid amide has a weight average molecular weight of 500 to 2,000.

7. 6. The gravure printing ink for surface printing according to claim 5, wherein the weight average molecular weight of the polyamide resin is 1,000 to 20,000.

8. 7. The gravure printing ink for front printing according to claim 5 or 6, wherein the fatty acid constituting the fatty acid amide includes an unsaturated fatty acid.

9. 7. The gravure printing ink for surface printing according to claim 5 or 6, wherein the fatty acid amide comprises a bisamide.

10. 10. The gravure printing ink for surface printing of claim 1 further comprising hydrocarbon wax particles.

11. A printed matter having a printing layer comprising the gravure printing ink for surface printing according to claim 1 on a substrate.

Citation Information

Patent Citations

  • Gravure ink composition for front printing

    JP2012012597A

  • Gravure ink composition for front printing

    JP2013256551A

  • Surface gravure printed material

    JP2016043600A

  • Gravure printing ink composition for surface printing and surface-printed gravure printed matter

    JP2017025256A

  • Gravure printing ink composition for surface printing and printed article

    JP2019183112A