Photocatalyst coated body

A balanced concentration and thickness of visible light-responsive photocatalyst particles in the photocatalyst coated body maintain high photocatalytic activity and light resistance, addressing discoloration and fading issues in existing coatings.

JP2024152581APending Publication Date: 2024-10-25TOTO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023211462
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2023-12-14
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing photocatalyst coatings face issues with discoloration and fading when the concentration of photocatalyst particles is increased to enhance antibacterial and antiviral performance, leading to impaired appearance and photocatalytic action.

Method used

A photocatalyst coated body with a specific balance of visible light-responsive photocatalyst particle concentration (1-30% by mass) and film thickness (0.5-10.0 μm) that maintains high photocatalytic activity and light resistance, using a resin and optional aggregates to minimize discoloration and fading.

Benefits of technology

The solution achieves both high photocatalytic activity and good light resistance, suppressing discoloration and fading, while reducing costs due to the thin film thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152581000001
    Figure 2024152581000001
  • Figure 2024152581000002
    Figure 2024152581000002
  • Figure 2024152581000003
    Figure 2024152581000003
Patent Text Reader

Abstract

To provide a photocatalyst coated body which has a photocatalyst layer that achieves both high photocatalyst activity and good light resistance even when the photocatalyst layer contains visible light-responsive photocatalyst particles in high concentration and has a small film thickness, or contains visible light-responsive photocatalyst particles in low concentration and has a small film thickness.SOLUTION: A photocatalyst coated body includes at least a base material, and a photocatalyst layer provided on the surface of the base material, wherein the photocatalyst layer contains at least visible light-responsive photocatalyst particles and a resin, when the total amount of a total solid contained in the photocatalyst layer is 100 mass%, a ratio of the amount of the visible light-responsive photocatalyst particles is 1 mass% or more and 30 mass% or less, the average film thickness of the photocatalyst layer is 0.5 μm or more and 10.0 μm or less, and a color difference ΔE*=[(L1*-L0*)2+(a1*-a0*)2+(b1*-b0*)2]1 / 2 calculated from color measurement values (L0*, a0*, b0*) by the SCE method of the photocatalyst layer, and color measurement values (L1*, a1*, b1*) by the SCE method of the obtained photocatalyst layer after 0.8 g / 10 cm2 of 1 mass% of silver nitrate solution is coated onto the surface of the photocatalyst layer, and the surface is irradiated with ultraviolet light at a wavelength of 300 to 400 nm at intensity of 1.0 mW / cm2 for two minutes is 7 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photocatalyst-coated body, and more specifically to a photocatalyst-coated body having both high photocatalytic activity and good light resistance. [Background technology]

[0002] In recent years, the use of photocatalytic coatings on various materials, such as interior building materials, has been on the rise. Titanium dioxide (TiO2), a type of photocatalyst, generates excited electrons and holes using the energy of light. The generated excited electrons and holes are converted to O2 - , O - This generates reactive oxygen species such as ·OH (· indicates an unpaired electron and means that it is a radical species). The radical properties of these reactive oxygen species can be used to oxidize and decompose harmful substances such as bacteria and viruses.

[0003] For example, in JP 2019-011418 A (Patent Document 1), it is described that in a coating composition containing photocatalytic titanium oxide, a resin, and a pigment (calcium carbonate, zeolite, etc.), the ratio of the content of photocatalytic titanium oxide to the total amount of these three components is relatively low (0.03 to 2.8% by mass), and the concentration ratio of the above three components is specified under that condition, thereby obtaining a coating film (photocatalytic layer) with excellent antibacterial and antiviral performance and suppressed discoloration. According to Patent Document 1, it is specifically shown that when the content concentration of photocatalytic titanium oxide is high (6.3% by mass), the coating film discolored (ΔL*≧5) (see the discoloration evaluation result of Comparative Example 4 in Table 3 (paragraph number 0069)). Note that Patent Document 1 does not specifically describe the film thickness of the coating film, but as described later, it is estimated that the film thickness is relatively thick from the solid content (total concentration of the above three components) and application amount of the coating composition specifically disclosed in the patent document. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-011418 A Summary of the Invention [Problem to be solved by the invention]

[0005] In coatings with a relatively low photocatalyst concentration as disclosed in Patent Document 1, the common method is to increase the photocatalyst concentration or to thicken the coating thickness in order to obtain good robustness and to achieve higher antibacterial and antiviral performance, but on the other hand, increasing the photocatalyst concentration increases the photocatalytic action (oxidizing power) caused by light in the environment, causing discoloration of the resin and pigment in the coating, the metal particles carried by the photocatalyst, and the organic components contained in the coating base, which may result in a loss of design of the coated object. Also, increasing the coating thickness may result in a loss of appearance of the coating, in coatings that require transparency.

[0006] The present inventors have now come up with the idea that in order to achieve both excellent antiviral performance and suppression of discoloration, the balance between the concentration of the photocatalyst contained in the photocatalyst layer and the film thickness of the photocatalyst layer must be appropriately maintained. Then, taking into consideration the balance between the photocatalyst concentration and the film thickness, the ratio of the amount of visible light responsive photocatalyst particles to the total amount of all solids contained in the photocatalyst layer and the film thickness of the photocatalyst layer are controlled within a specific range, and the photocatalytic activity expressed by the photocatalyst layer having these characteristics is controlled within a specific range, thereby confirming that a photocatalyst layer can be obtained in which the photocatalytic function such as antiviral performance is fully exerted and discoloration (deterioration of light resistance) of the coating film due to the photocatalytic action expressed by light is suppressed. As a result, it has been found that a photocatalyst layer having both high photocatalytic activity and good light resistance can be formed even when the content concentration of the photocatalyst particles is increased and the film thickness is thin, or when the content concentration of the photocatalyst particles is decreased and the film thickness is thin. The present invention is based on such findings.

[0007] The present invention aims to provide a photocatalyst-coated body having a photocatalyst layer that achieves both high photocatalytic activity and good light resistance, whether the photocatalyst particle content is high and the film thickness is thin, or whether the photocatalyst particle content is low and the film thickness is thin. [Means for solving the problem]

[0008] The photocatalyst-coated body according to the present invention is The photocatalyst layer includes at least a substrate and a photocatalyst layer provided on a surface of the substrate. The photocatalyst layer contains at least visible light responsive photocatalyst particles and a resin, The content ratio of the visible light responsive photocatalyst particles is 1% by mass or more and 30% by mass or less when the total of all solid contents contained in the photocatalyst layer is 100% by mass, The average thickness of the photocatalyst layer is 0.5 μm or more and 10.0 μm or less, The color measurement values ​​(L0*, a0*, b0*) of the photocatalyst layer by the SCE method and the surface of the photocatalyst layer were measured by applying 0.8 g / 10 cm of a 1% by mass silver nitrate solution. 2 and irradiate the skin with ultraviolet light of 300-400 nm at 1.0 mW / cm 2 After irradiating the photocatalyst layer for 2 minutes at an intensity of 1000 nm, the color difference calculated from the color measurement values ​​(L1*, a1*, b1*) of the photocatalyst layer obtained by the SCE method is: ΔE*=[(L1*-L0*) 2 +(a1*-a0*) 2 +(b1*-b0*) 2 ] 1 / 2 is 7 or more. Effect of the Invention

[0009] According to the present invention, even if the photocatalyst particle content concentration is high and the film thickness is thin, or even if the photocatalyst particle content concentration is low and the film thickness is thin, the photocatalyst function such as antiviral performance is sufficiently exhibited, and discoloration (deterioration) due to photocatalysis is suppressed, that is, a photocatalyst-coated body having a photocatalyst layer with good light resistance is provided. In addition, since the photocatalyst layer has a thin film thickness, there is also an advantage that the cost can be suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Photocatalytic coating The photocatalyst-coated body according to the present invention comprises a substrate and a photocatalyst layer provided on the surface of the substrate.

[0011] photocatalyst layer composition In the present invention, the photocatalyst layer contains at least visible light responsive photocatalyst particles and a resin. The photocatalyst-coated body according to the present invention is characterized in that the content ratio of the visible light responsive photocatalyst particles (hereinafter, also referred to as the "content concentration of visible light responsive photocatalyst particles") is 1 mass% or more and 30 mass% or less when the total amount of all solids contained in the photocatalyst layer is 100 mass%. This makes it possible to obtain a photocatalyst layer that has both high photocatalytic activity and good light resistance, even when the content concentration of the visible light responsive photocatalyst particles is high and the film thickness is thin, or when the content concentration of the visible light responsive photocatalyst particles is low and the film thickness is thin. In the present invention, the "solid content" refers to solid components contained in the photocatalyst layer, such as visible light responsive photocatalyst particles, resin, etc. In other words, the content concentration of the visible light responsive photocatalyst particles is expressed as the ratio (percentage) of the content of the visible light responsive photocatalyst particles when the total of the content of the visible light responsive photocatalyst particles, the content of the resin, and the content of other solids, if necessary, contained in the photocatalyst layer is taken as 100 mass%. The content concentration of the visible light responsive photocatalyst particles is preferably 5% by mass or more and 30% by mass or less.

[0012] Film Thickness The photocatalyst-coated body according to the present invention is characterized in that the average film thickness of the photocatalyst layer is 0.5 μm or more and 10.0 μm or less. Such a thin film thickness makes it difficult for visible light to scatter and makes discoloration of the coating film components less noticeable. As a result, the light resistance of the photocatalyst-coated body can be improved. Furthermore, such a thin film thickness makes it difficult for visible light to scatter, allowing visible light to reach the visible light-responsive photocatalyst particles located below the photocatalyst layer (on the substrate side), making it possible to efficiently express the photocatalytic action. It is believed that this makes it possible to obtain sufficient photocatalytic activity even with a thin film.

[0013] The thickness of the photocatalyst layer is measured by cutting the photocatalyst-coated body and observing the cross section of the coating film with a scanning electron microscope (SEM). On the other hand, in the present invention, the estimated thickness obtained from the actually measured thickness by the method described below may be used as the thickness of the photocatalyst layer. That is, it is considered that a proportional relationship is established between the thickness of the photocatalyst layer and the dry weight obtained by multiplying the solid content concentration and application amount of the coating composition for forming the photocatalyst layer, and the estimated thickness is obtained by the following formula. Estimated film thickness of photocatalyst layer=(Actual film thickness of photocatalyst layer)×(Dry weight of coating composition for forming photocatalyst layer to obtain estimated film thickness / Dry weight of coating composition for forming photocatalyst layer to obtain actual film thickness) The solid content of the coating composition for forming a photocatalyst layer is adjusted in advance so that the photocatalyst layer to be formed has the above-mentioned composition.

[0014] Silver nitrate coloration The photocatalyst-coated body according to the present invention has color measurement values ​​(L0*, a0*, b0*) of the photocatalyst layer measured by the SCE method, and the surface of the photocatalyst layer is coated with a 1% by weight silver nitrate solution at 0.8 g / 10 cm 2 and irradiate the skin with ultraviolet light of 300-400 nm at 1.0 mW / cm 2 After irradiating the photocatalyst layer for 2 minutes at an intensity of 1000 nm, the color difference calculated from the color measurement values ​​(L1*, a1*, b1*) of the photocatalyst layer obtained by the SCE method is: ΔE*=[(L1*-L0*) 2 +(a1*-a0*) 2 +(b1*-b0*) 2 ]1 / 2 is 7 or more. The photocatalyst-coated body according to the present invention can express its characteristics using the color difference (ΔE* value) measured by the silver nitrate coloration test described later as an index. In the present invention, the photocatalytic activity expressed using the color difference (ΔE* value) measured by the silver nitrate coloration test as an index is called silver nitrate coloration. The silver nitrate coloration test evaluates the photocatalytic activity of the photocatalyst-coated body using the phenomenon that when a silver nitrate solution is applied to the surface and the photocatalyst layer penetrated into the interior (depth direction) is irradiated with ultraviolet light, silver ions that come into contact with the visible light responsive photocatalyst particles contained in the photocatalyst layer are reduced, silver precipitates, and the photocatalyst layer turns black as an index. When visible light is irradiated to the visible light responsive photocatalyst particles and the photocatalyst particles exhibit photocatalytic activity, i.e., oxidation-reduction action, reduction reaction and oxidation reaction occur inextricably linked, and it is considered that the degree of reduction power and oxidation power generated by these reactions are equal. Furthermore, since the number of oxidation-reduction reactions changes depending on the amount of visible light responsive photocatalyst particles contained in the photocatalyst layer, it is considered that the degree of coloration of the photocatalyst layer also changes. From these findings, the reducing power of the visible light responsive photocatalyst particles, which is the basis for the degree of coloration of the photocatalyst layer, can be used as an index, and the visible light responsive photocatalyst particles can be evaluated as having an oxidizing power equal to the above reducing power, which is the opposite of the above reducing power.

[0015] Silver nitrate color test The test procedure is as follows: A 1% by weight solution of silver nitrate was applied to the surface of the photocatalytic layer of the photocatalytic coating body at a rate of 0.8 g / 10 cm. 2 For example, a BL lamp is used to apply ultraviolet light with a wavelength of 300 to 400 nm at 1.0 mW / cm 2 After that, wipe off the excess silver nitrate solution and measure the L1*, a1*, and b1* values ​​of the photocatalyst-coated body using the SEC method. Meanwhile, the L0*, a0*, and b0* values ​​of the photocatalyst-coated body are measured before the test. As described above, the color difference before and after the test of the photocatalyst coating body (ΔE*=[(L1*-L0*) 2 +(a1*-a0*) 2 +(b1*-b0*) 2 ] 1 / 2) is measured. As the color difference meter, for example, a color difference meter (CR-400, manufactured by Konica Minolta) can be used.

[0016] The photocatalyst-coated body according to the present invention has the above-mentioned composition, film thickness, and silver nitrate coloration, and therefore can combine high photocatalytic activity and good light resistance, even if the visible light-responsive photocatalyst particle content concentration is high and the film thickness is thin, or even if the visible light-responsive photocatalyst particle content concentration is low and the film thickness is thin.

[0017] In the photocatalyst-coated body according to the present invention, the content concentration of the visible light responsive photocatalyst particles in the photocatalyst layer is within the above-mentioned specific range, and further, the film thickness of the photocatalyst layer is within the above-mentioned specific range, so that a balance is maintained between the two to achieve both high photocatalytic activity and good light resistance. Furthermore, the characteristics of the photocatalyst-coated body according to the present invention can be expressed as an index of the amount of visible light responsive photocatalyst particles per unit area of ​​the photocatalyst layer taking into consideration the above-mentioned balance, and when the amount is 25 mg / m 2 More than 500mg / m 2 It is preferable that:

[0018] performance <Antiviral activity> The photocatalyst-coated body according to the present invention has excellent antiviral activity due to the above-mentioned composition, film thickness, and silver nitrate coloration. In the present invention, the antiviral activity of the photocatalyst-coated body can be expressed as an index of the antiviral activity value (V) obtained according to JIS R1756 (2020) Visible Light B Conditions in Bright Place. Specifically, an antiviral test is performed using bacteriophage Qβ according to JIS R1756 (2020) Visible Light B Conditions. A 20W white fluorescent lamp (Toshiba Lighting & Technology Corporation, "Neoline" FL20S·W) is used as a light source, and irradiation is performed at an illuminance of 500 lux through an ultraviolet cut filter (Nitto Plastics Co., Ltd., N-169). The illuminance is measured using an illuminometer: IM-5 manufactured by Topcon Corporation. The antiviral activity value (V) in bright place was calculated using the following formula, assuming that the visible light irradiation time was 4 hours.

[0019] Antiviral activity value: V=Log 10 (UV / TV) TV: Bacteriophage infectivity (pfu) per photocatalyst-coated body after light irradiation UV: Bacteriophage infectivity (pfu) per control after light exposure As a control, a substrate that has not been subjected to antiviral treatment, that is, a substrate that has not been formed with a photocatalyst layer, is used.

[0020] By setting the amount of visible light responsive photocatalyst particles per unit area of ​​the photocatalyst layer within the above-mentioned range, the antiviral activity value (V) of the photocatalyst-coated body can be made 2 or more.

[0021] <Antibacterial activity> The photocatalyst-coated body according to the present invention has excellent antibacterial activity due to the above-mentioned composition, film thickness, and silver nitrate coloration. In the present invention, the antibacterial activity of the photocatalyst-coated body can be expressed as an index of the antibacterial activity value (R) obtained in accordance with JIS R1752 (2020) visible light B condition, bright place. Specifically, an antibacterial test is performed using Staphylococcus aureus in accordance with JIS R1752 (2020) visible light B condition. A 20W white fluorescent lamp (Toshiba Lighting & Technology Corporation, "Neoline" FL20S·W) is used as a light source, and irradiation is performed at an illuminance of 500 lux through an ultraviolet cut filter (Nitto Resin Industrial Co., Ltd., N-169). The illuminance is measured using an illuminometer: IM-5, manufactured by Topcon Corporation. The antibacterial activity value (R) in bright place is calculated by the following formula, assuming that the irradiation time of visible light is 8 hours.

[0022] Antibacterial activity value: R=Log 10 (UB / TB) TB: Number of viable bacteria (cfu) per photocatalyst-coated body after light irradiation UB: Viable bacteria count (cfu) per control after light exposure As a control, a substrate that has not been subjected to antibacterial treatment, that is, a substrate that has not been formed with a photocatalyst layer, is used.

[0023] By setting the amount of visible light responsive photocatalyst particles per unit area of ​​the photocatalyst layer within the above-mentioned range, the antibacterial activity value (R) of the photocatalyst-coated body can be made 2 or more.

[0024] Incidentally, before carrying out the above-mentioned antiviral and antibacterial tests, the photocatalyst-coated body may be sterilized by a conventional method.

[0025] <Light resistance (anti-discoloration ability)> The photocatalyst-coated body according to the present invention has excellent light resistance due to the above-mentioned composition, film thickness and silver nitrate coloration. In the present invention, the light resistance of the photocatalyst-coated body can be expressed as an index of color difference: ΔE* obtained in accordance with the sunshine carbon arc lamp method described in Chapter 9, Section 8 of JIS K5400 (1990). Specifically, a weather resistance test is carried out using a sunshine carbon arc lamp weather resistance tester (S-300, manufactured by Suga Test Instruments Co., Ltd.) in accordance with the sunshine carbon arc lamp method described in Chapter 9, Section 8 of JIS K5400 (1990). The test time is 8 hours, and the L*, a*, and b* values ​​of the photocatalyst-coated body before and after the test are measured using the SCE method, and the color difference: ΔE*=[(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2 A color difference meter (Konica Minolta, CR-400) can be used as the color difference meter.

[0026] By setting the amount of visible light responsive photocatalyst particles per unit area of ​​the photocatalyst layer within the above-mentioned range, the light resistance of the photocatalyst-coated body can be made to have a ΔE* value of 4 or less.

[0027] <Methylene blue decomposition activity> In the present invention, the photocatalytic activity of the photocatalyst-coated body can be expressed by the decomposition performance of methylene blue as an index. Specifically, the decomposition activity index (R) obtained by the method described in JIS R1703-2 (2014) can be used as an index of photocatalytic activity. The amount of visible light responsive photocatalyst particles per unit area of ​​the photocatalyst layer is 25 mg / m 2 More than 500mg / m2 By satisfying the following conditions, the methylene blue decomposition activity index (R) of the photocatalyst-coated body can be made 5.0 or more.

[0028] Above, we have explained the composition, film thickness, and silver nitrate color property of the photocatalyst layer in the present invention, and the performance of the photocatalyst-coated body according to the present invention achieved by these characteristics. Below, we will further explain each component of the photocatalyst layer.

[0029] Visible light responsive photocatalyst particles The visible light responsive photocatalyst particles contained in the photocatalyst layer of the photocatalyst-coated body according to the present invention are semiconductor metal oxide particles that are excited by irradiation with visible light and have a band gap sufficient to exert photocatalytic functions such as the oxidative decomposition of harmful substances such as bacteria and viruses.

[0030] In the present invention, preferred examples of visible light responsive photocatalyst particles include, for example, Rutile-type titanium dioxide carrying metal compounds, anatase-type titanium dioxide carrying a metal compound; and Nitrogen or sulfur doped titanium dioxide The examples include one or more types selected from the group consisting of:

[0031] As the metal element contained in the metal compound, it is preferable to use copper, silver, iron, platinum, palladium, etc., and as the metal compound, it is preferable to use metal oxide, metal hydroxide, metal sulfate, etc. By supporting the metal compound on titanium oxide particles, it is possible to excite electrons to a metal ion level slightly lower than the conduction band of titanium oxide as a semiconductor, which has the effect of assisting the interfacial charge transfer when irradiated with visible light and enhancing the photocatalytic function. In addition, since the metal compound itself has antibacterial and antiviral properties, a synergistic antibacterial and antiviral effect can be obtained in the photocatalytic particles supporting the metal compound.

[0032] These visible light responsive photocatalyst particles show photocatalytic activity in response to visible light with a wavelength of 400 nm or more, and even in environments where ultraviolet rays are not irradiated, such as indoors, the photocatalyst-coated body can exhibit antibacterial and antiviral performance as well as high light resistance. Furthermore, since these visible light responsive photocatalyst particles are less likely to deteriorate the resin, light resistance can be maintained even if the concentration contained in the photocatalyst layer is increased. By specifying the concentration of the visible light responsive photocatalyst particles, resin, and aggregate in the photocatalyst layer, as well as the film thickness, within the above-mentioned ranges, and in addition, specifying the type of visible light responsive photocatalyst particles, the photocatalytic activity and light resistance of the photocatalyst-coated body can be further improved.

[0033] In the present invention, the crystal type of the photocatalytic titanium oxide may be either the rutile type or the anatase type. The rutile type has better light resistance than the anatase type, and therefore can improve the light resistance of the photocatalyst-coated body.

[0034] In the present invention, preferred examples of the metal compound to be supported on the visible light responsive photocatalyst particles include one or more compounds selected from the group consisting of silver compounds, copper compounds, iron compounds, platinum compounds, and palladium compounds.

[0035] By supporting these metal compounds on visible light responsive photocatalyst particles, the photocatalyst particles respond more efficiently to visible light with wavelengths of 400 nm or more, and even in environments where ultraviolet light is not irradiated, such as indoors, the photocatalyst-coated body can more efficiently exhibit antibacterial and antiviral properties and exhibit high light resistance. Furthermore, since the metal compounds themselves have antibacterial and antiviral properties, a synergistic effect can be obtained with visible light responsive photocatalyst particles supporting the metal compounds.

[0036] In the present invention, for example, rutile-type titanium oxide or anatase-type titanium oxide is used depending on the application of the photocatalytic coated body, and the metal compound to be supported on the photocatalytic titanium oxide is appropriately selected, thereby optimizing the balance between photocatalytic activity and light resistance.

[0037] resin In the present invention, the resin content is expressed as a ratio (percentage) of the resin content when the total of the content of the visible light responsive photocatalyst particles contained in the photocatalyst layer, the content of the resin, and the content of other solid contents as the case may be 100 mass%, and is preferably 10 mass% or more and 70 mass% or less. By having the resin content in the above range, the photocatalyst layer can be made into a coating film with good robustness. The resin content is more preferably 10 mass% or more and 60 mass% or less. This can suppress discoloration of the resin and improve the light resistance of the photocatalyst layer.

[0038] In the present invention, preferred examples of the resin include, for example, one or more selected from the group consisting of acrylic resin, urethane resin, acrylic urethane resin, vinyl chloride resin, silicone resin, organosiloxane, and fluororesin. As the silicone resin, one or more selected from the group consisting of acrylic silicone resin, acrylic modified silicone resin, epoxy modified silicone resin, urethane modified silicone resin, silicone modified acrylic resin, silicone modified epoxy resin, and silicone modified urethane resin can be used. By using these resins, it is possible to form a thin film (0.1 μm or more and 10.0 μm or less) photocatalyst layer in which visible light responsive photocatalyst particles and aggregates are distributed in the resin matrix. In the present invention, more preferred examples of the resin include, for example, one or more selected from the group consisting of acrylic resin, vinyl chloride resin, silicone resin, organosiloxane, and fluororesin.

[0039] Other Ingredients aggregate In the present invention, the photocatalyst layer may contain components other than the visible light responsive photocatalyst particles and the resin, as long as the photocatalyst activity and light resistance are not impaired. For example, the photocatalyst layer may contain an aggregate. Preferred examples of the aggregate include one or more selected from the group consisting of silica such as matte silica and crystalline silica, silica sand, acrylic beads, talc, barium sulfate, calcium carbonate, zirconium oxide, and aluminum oxide. The aggregate preferably has a particle size smaller than or equal to the thickness of the photocatalyst layer. By using the aggregate, it is possible to prevent poor film formation of the photocatalyst layer. In addition, by adding the aggregate, the resin is adsorbed to the aggregate during the film formation process, and the volume of the resin in the photocatalyst layer is reduced, so that the visible light responsive photocatalyst particles are easily exposed to the coating surface, and the number of interfaces between the resin and the particle components (i.e., the visible light responsive photocatalyst particles and the aggregate) increases inside the photocatalyst layer, and as a result, the frequency of contact between the visible light responsive photocatalyst particles and bacteria and viruses can be increased on the surface and inside the photocatalyst layer (i.e., throughout the entire photocatalyst layer).

[0040] In the present invention, the content concentration of the aggregate may be appropriately determined based on the content of the visible light responsive photocatalyst particles and the resin contained in the photocatalyst layer. The content concentration of the aggregate is expressed as the ratio (percentage) of the content of the aggregate when the total of the content of the visible light responsive photocatalyst particles, the content of the resin, the aggregate, and the content of other solids in the photocatalyst layer is 100% by mass, and is preferably 20% by mass or more and 80% by mass or less. By setting the content concentration of the aggregate in the above range, the contact area between the visible light responsive photocatalyst particles and the resin in the photocatalyst layer can be reduced, and as a result, discoloration of the resin can be suppressed.

[0041] In the present invention, the photocatalyst layer may contain, for example, agents (antibacterial agents, antiviral agents) such as silver zeolite, triazine-based compounds, and compounds having a cationic group. Examples of compounds having a cationic group include compounds having an antiviral effect such as polyhexamethylene biguanide, quaternary ammonium salt-based compounds, and cationic polysiloxane polymers. These compounds are considered to cause cell membrane destruction and protein denaturation due to effects such as hydrophobic and hydrophilic interactions derived from their cationic (positive charge) and molecular structure.

[0042] Base material In the present invention, the substrate may be any of various materials, whether inorganic or organic, as long as it is a material capable of forming a photocatalytic layer thereon, and its shape is not limited. In addition, a substrate whose surface contains an organic substance can be used. Examples of such substrates include resins containing organic substances, painted bodies having a surface coated with a coating containing a resin containing an organic substance, and laminates having a film containing a resin containing an organic substance laminated on the surface. Preferable examples of substrates from the viewpoint of application include interior building materials such as wallpaper, calcium silicate (decorative) boards, decks of toilets and restrooms, handrails, counters, bundles, and instruments used in hospitals. Preferable examples of substrates from the viewpoint of material include PVC, acrylic painted surfaces, SUS, artificial marble, steel plates, ceramics, glass, plastics, rubber, stone, cement, concrete, fibers, fabrics, wood, paper, combinations thereof, and laminates thereof.

[0043] Manufacturing method of photocatalyst-coated body The photocatalyst-coated body according to the present invention can be produced, for example, by the following method. That is, the method for producing the photocatalyst-coated body according to the present invention is as follows: Providing a substrate; The method includes at least a step of applying a coating composition containing at least visible light responsive photocatalyst particles, a resin, and a solvent to the surface of the substrate to form a photocatalyst layer.

[0044] In the present invention, the total concentration (solids concentration) of the visible light responsive photocatalyst particles and resin contained in the coating composition may be determined so that the concentrations of the visible light responsive photocatalyst particles and resin contained in the formed photocatalyst layer are the above-mentioned content concentrations, and is preferably 1 mass % or more and 30 mass % or less.

[0045] In the present invention, the coating amount of the coating composition per unit area on the substrate surface is 1 g / m2 or more depending on the solid content concentration of the coating composition. 2 More than 50g / m 2 Preferably, it is 2.5 g / m or less. 2More than 50g / m 2 It is more preferable that:

[0046] By applying a coating composition containing visible light responsive photocatalyst particles, a resin, and an aggregate at a solid content concentration within the above range to a substrate in an amount within the above range, a photocatalyst layer having a thin film thickness of 0.1 to 10 μm and having both high photocatalytic activity and good light resistance can be obtained.

[0047] In the present invention, it is preferable to form a photocatalyst layer by applying a coating composition to the surface of a substrate and then curing and / or drying the applied coating composition. As a result, a photocatalyst-coated body having excellent robustness can be obtained.

[0048] In the present invention, the method for applying the coating composition to the surface of the substrate is not particularly limited, but spray coating is preferred. EXAMPLES

[0049] The present invention will be described in more detail with reference to the following examples, but the present invention should not be construed as being limited to these examples.

[0050] Preparation of the Coating Composition <Material> To produce the photocatalyst-coated bodies of Examples 1 to 27, the following materials were prepared as components to be contained in the coating composition for forming the photocatalyst layer of each coated body. <Visible light responsive photocatalyst particles> Nitrogen-doped anatase-type TiO2 carrying copper compounds (dispersion, basic, solid content: 8% by mass) Rutile-type TiO2 carrying copper compound (dispersion, basic, solid content: 6% by mass) <Resin> Vinyl chloride resin (water-based emulsion, neutral, solids content: 25% by weight) Acrylic silicone resin (solvent-based resin, solid content: 80% by weight) <Aggregate> Crystalline silica (powder) Colloidal silica (solvent dispersion, solid content: 20% by weight) <Solvent> Water (however, no water was used in the preparation of the photocatalyst-coated body of Example 27.) Dilution solvent (cyclohexanone) (however, used only in the preparation of the photocatalyst-coated body in Example 27)

[0051] Preparation of aqueous coating composition for forming photocatalyst layer of photocatalyst-coated body of Examples 1 to 26 The above-mentioned visible light responsive photocatalyst particles, resin, aggregate, and water were mixed so that the contents of the visible light responsive photocatalyst particles, resin, and aggregate contained in the obtained photocatalyst layer were the contents shown in Tables 1 to 3, to prepare aqueous coating compositions for forming the photocatalyst layer of the photocatalyst-coated bodies of Examples 1 to 26.

[0052] Preparation of a solvent-based coating composition for forming a photocatalyst layer of the photocatalyst-coated body of Example 27 The above-mentioned visible light responsive photocatalyst particles, resin, aggregate, and dilution solvent were mixed so that the contents of visible light responsive photocatalyst particles, resin, and aggregate contained in the obtained photocatalyst layer were the contents shown in Tables 1 to 3, to prepare an aqueous coating composition for forming a photocatalyst layer of the photocatalyst-coated body of Example 27. The respective concentrations (wt%) of the visible light responsive photocatalyst particles, resin, and aggregate in Tables 1 to 3 are the ratios of the weight of the visible light responsive photocatalyst particles, resin, and aggregate to the total solid weight in the coating composition. Since the photocatalyst layer is formed (constituted) by the total solid content in the coating composition, the respective concentrations of the visible light responsive photocatalyst particles, resin, and aggregate in the coating composition are equal to the respective concentrations of the visible light responsive photocatalyst particles, resin, and aggregate in the photocatalyst layer.

[0053] The total solids concentration (wt %) of each of the prepared coating compositions was as shown in Tables 1 to 3.

[0054] Preparation of photocatalyst-coated body A white tile (50 mm × 50 mm × 5 mmT) with a smooth surface was prepared as a substrate. Each coating composition was applied to the surface of this substrate in the amount (g / m2) shown in Tables 1 to 3. 2The substrate to which the coating composition was applied was cured at room temperature for 1 day and then dried at 80°C for 30 minutes to obtain photocatalyst-coated bodies of Examples 1 to 27 in which a photocatalyst layer was formed on the surface of the substrate.

[0055] Measurement and Evaluation The photocatalyst-coated bodies of Examples 1 to 27 were subjected to the following measurements and evaluations.

[0056] Photocatalyst layer thickness The photocatalyst-coated body of Example 1 was cut, and the cross section of the coating was observed with an SEM (HITACHI SE8220), and the film thickness was measured at a total of 25 points (5 visual fields x 5 locations). The average value of the measurements at the 25 points was taken as the film thickness of the photocatalyst layer of the photocatalyst-coated body of Example 1. The film thickness was 0.5 μm.

[0057] Regarding the film thickness of the photocatalyst layer of the photocatalyst-coated bodies other than Example 1 (Examples 2 to 27), based on the actual measured film thickness (0.5 μm) of the photocatalyst layer of the photocatalyst-coated body of Example 1, it was assumed that a proportional relationship would be established between the dry weight obtained by multiplying the solid concentration of each coating composition by the application amount and the film thickness of the photocatalyst layer of each photocatalyst-coated body, and the expected film thickness was theoretically calculated using the following formula. Estimated thickness of the photocatalyst layer of the photocatalyst-coated body other than Example 1 = (Actual thickness of the photocatalyst layer of the photocatalyst-coated body of Example 1 [0.5 μm]) × (Dry weight of the coating composition for forming the photocatalyst layer other than Example 1 / Dry weight of the coating composition for forming the photocatalyst layer of Example 1) For example, the assumed thickness of the photocatalyst layer of the photocatalyst-coated body of Example 5 is 0.5 [μm] × (5 [g / m 2 ] / 0.25[g / m 2 ]) = 10 [μm]. Similarly, the estimated film thickness of the photocatalyst layer of the photocatalyst-coated bodies of Examples 2 to 4 and 6 to 27 was calculated, and the results are shown in Tables 1 to 2.

[0058] The solid content of the coating composition specifically disclosed in Patent Document 1 is in the range of 55.4% by mass (Example 15) to 105.4% by mass (Example 13), and the coating amount of the coating composition is 200 g / m 2(paragraph 0057), the dry weight of the coating composition obtained by multiplying these is about 110 g / m 2 ~210g / m 2 Therefore, the expected thickness of the resulting coating film is calculated to be about 110 μm to 210 μm according to the above formula.

[0059] Antiviral Antiviral tests were conducted using bacteriophage Qβ according to JIS R1756 (2020) visible light B conditions. A 20W white fluorescent lamp (Toshiba Lighting & Technology Corporation, "Neoline" FL20S·W) was used as the light source, and irradiation was performed at an illuminance of 500 lux through an ultraviolet cut filter (Nitto Resin Industrial Co., Ltd., N-169). The illuminance was measured using an illuminometer: Topcon Corporation, IM-5. The antiviral activity value (V) in bright light was calculated using the following formula, assuming a visible light irradiation time of 4 hours.

[0060] Antiviral activity value: V=Log 10 (UV / TV) TV: Bacteriophage infectivity (pfu) per photocatalyst-coated body after light irradiation UV: Bacteriophage infectivity (pfu) per control after light exposure The control was a glass plate that had not been treated with an antiviral agent.

[0061] The measured antiviral activity value (V) in bright light was evaluated according to the following evaluation criteria. An evaluation criterion of "2" or higher was considered to be acceptable. The results are shown in Tables 1 to 3. (Evaluation Criteria) 4: 4≦V 3: 3≦V<4 2: 2≦V<3 1: 1≦V<2 0: 0≦V<1

[0062] Before evaluating the antiviral properties, the front and back surfaces of the photocatalyst-coated body were sterilized by irradiating them with a germicidal lamp in a clean bench. Two 15W germicidal lamps (wavelength 254 nm) were installed, one on each side of the clean bench, and the distance from the coated body to the light source was 30 cm to 60 cm. The germicidal lamp irradiation time was 15 minutes.

[0063] Light resistance (discoloration prevention ability) A weathering test was carried out using a sunshine carbon arc lamp weathering tester (Suga Test Instruments, S-300) in accordance with the sunshine carbon arc lamp method described in Chapter 9, Section 8 of JIS K5400 (1990). The test time was 8 hours, and the L*, a*, and b* values ​​of the photocatalyst coating before and after the test were measured using the SCE method, and the color difference was: ΔE* = [(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2 The color difference meter used was a color difference meter (Konica Minolta, CR-400).

[0064] The light resistance of the photocatalyst-coated body was evaluated based on the obtained color difference (ΔE* value) according to the following evaluation criteria. Evaluation criteria of "2" or higher were considered to be acceptable. The results are shown in Tables 1 to 3. (Evaluation Criteria) 3: ΔE*≦2 2: 2<ΔE*≦4 1: 4<ΔE*≦8 0: 8<ΔE*

[0065] Silver nitrate coloration According to the procedure of the silver nitrate color test described later, the photocatalytic activity was evaluated by measuring the color difference (ΔE* value) of the photocatalyst-coated body before and after the test. Silver nitrate color test procedure A 1% silver nitrate solution was applied at 0.8g / 10cm to the surface of the photocatalyst layer of the photocatalyst-coated body. 2 Using a BL lamp, ultraviolet light with a wavelength of 300 to 400 nm was applied at 1.0 mW / cm 2The photocatalyst-coated body was exposed to light for 2 minutes at an intensity of 1000 nm. After that, the excess silver nitrate solution was wiped off, and the L1*, a1*, and b1* values ​​of the photocatalyst-coated body were measured using the SEC method. Meanwhile, the L0*, a0*, and b0* values ​​of the photocatalyst-coated body before the test were measured. As described above, the color difference before and after the test of the photocatalyst coating body (ΔE*=[(L1*-L0*) 2 +(a1*-a0*) 2 +(b1*-b0*) 2 ] 1 / 2 ) was measured. A color difference meter (CR-400, manufactured by Konica Minolta) was used as the color difference meter.

[0066] The measured color difference (ΔE*) was evaluated according to the following evaluation criteria. A rating of 2 or higher was considered to be acceptable. The results are shown in Tables 1 to 3. (Evaluation Criteria) 3: 15≦ΔE* 2: 7≦ΔE*<15 1: 4≦ΔE*<7 0: ΔE*<4

[0067] [Table 1]

[0068] [Table 2]

[0069] [Table 3]

Claims

1. A photocatalyst-coated body comprising at least a substrate and a photocatalyst layer provided on a surface of the substrate, The photocatalyst layer contains at least visible light responsive photocatalyst particles and a resin, The ratio of the amount of the visible light responsive photocatalyst particles to the total amount of all solids contained in the photocatalyst layer is 1 mass% or more and 30 mass% or less, The average thickness of the photocatalyst layer is 0.5 μm or more and 10.0 μm or less, The color measurement value (L 0 *, a 0 *, b 0 *) and 0.8 g / 10 cm of 1% by weight silver nitrate solution was applied to the surface of the photocatalyst layer. 2 and irradiating the surface with ultraviolet light of 300-400 nm at 1.0 mW / cm 2 After irradiating the photocatalyst layer with an intensity of 1000 nm for 2 minutes, the color measurement value (L 1 *, a 1 *, b 1 Color difference calculated from: ΔE*=[(L 1 *-L 0 *) 2 + (a 1 *-a 0 *) 2 + (b 1 *-b 0 *) 2 ] 1/2 A photocatalytic coated body, wherein the photocatalytic coefficient is 7 or more.

2. The visible light responsive photocatalyst particles are Rutile-type titanium dioxide carrying metal compounds, - anatase type titanium oxide carrying a metal compound, and Nitrogen or sulfur doped titanium dioxide The photocatalyst-coated body according to claim 1, which is one or more semiconductor metal oxides excited by visible light irradiation selected from the group consisting of:

3. The photocatalyst-coated body according to claim 2 , wherein the metal compound comprises one or more compounds selected from the group consisting of silver compounds, copper compounds, iron compounds, platinum compounds, and palladium compounds.

4. The photocatalyst-coated body according to any one of claims 1 to 3, wherein the resin comprises one or more selected from the group consisting of acrylic resin, vinyl chloride resin, silicone resin, organosiloxane, and fluororesin.

5. A coating composition for forming a photocatalyst layer provided on the photocatalyst-coated body according to any one of claims 1 to 4, The coating composition contains at least visible light responsive photocatalyst particles, a resin, and a solvent.

6. A method for producing a photocatalyst-coated body according to any one of claims 1 to 4, A method comprising at least the step of applying the coating composition according to claim 5 to a surface of a substrate to form a photocatalytic layer.

7. The coating amount of the coating composition on the surface of the substrate is 1 g / m 2 50g / m or more 2 7. The method of claim 6, wherein:

Citation Information

Patent Citations

  • Coating composition

    JP2019011418A