Boron nitride agglomerated powder, heat radiation sheet, and semiconductor device module

By specifying pore volume, area, and elastic modulus ranges, the boron nitride agglomerated powder addresses dielectric breakdown issues, enhancing the withstand voltage and thermal conductivity of heat dissipation sheets for semiconductor devices.

JP2024152598APending Publication Date: 2024-10-25MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024006015
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-01-18
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing boron nitride agglomerated powders face issues with dielectric breakdown voltage due to insufficient deformation and residual voids during the pressing process, which are exacerbated by inadequate pore volume and elastic modulus, leading to compromised withstand voltage characteristics in heat dissipation sheets.

Method used

The development of boron nitride agglomerated powder with specific ranges for intra-particle pore volume (0.35-0.50 ml/g), intra-particle pore area (3-6.5 m^2/g), and average elastic modulus (70-150 MPa) ensures improved deformation and resin compatibility, resulting in a 'house of cards' structure that enhances withstand voltage characteristics.

Benefits of technology

The optimized boron nitride agglomerated powder improves the withstand voltage characteristics of heat dissipation sheets, enabling highly reliable semiconductor device modules with enhanced thermal conductivity and dielectric breakdown performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152598000001
    Figure 2024152598000001
  • Figure 2024152598000002
    Figure 2024152598000002
  • Figure 2024152598000003
    Figure 2024152598000003
Patent Text Reader

Abstract

To provide a boron nitride agglomerated powder capable of improving the breakdown voltage characteristic of a heat radiation sheet, a heat radiation sheet containing the boron nitride agglomerated powder, and a semiconductor device module using the heat radiation sheet.SOLUTION: Boron nitride agglomerated powder satisfies the following requirements a), b), and c). a): intraparticle pore volume measured by a mercury injection method is greater than 0.35 ml / g and less than 0.50 ml / g; b): intraparticle pore area measured by the mercury injection method is greater than 3 m2 / g and less than 6.5 m2 / g; and c): average elastic modulus measured by single particle compression test is greater than 70 MPa and less than 150 MPa.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a boron nitride agglomerated powder suitable for use in a heat dissipation sheet for a semiconductor device module, a heat dissipation sheet containing the boron nitride agglomerated powder, and a semiconductor device module using this heat dissipation sheet. [Background technology]

[0002] Boron nitride (BN) is an insulating ceramic and is known to have various crystal types, such as c-BN with a diamond structure, h-BN with a graphite structure, α-BN with turbostratic structure, and β-BN. Among these, h-BN has the same layered structure as graphite, is relatively easy to synthesize, and has excellent thermal conductivity, solid lubricity, chemical stability, and heat resistance, and is therefore widely used in the field of electrical and electronic materials.

[0003] In recent years, heat generation due to the increasing density of integrated circuits has become a major problem, especially in the electrical and electronics fields, and heat dissipation has become an urgent issue. h-BN is attracting attention as a thermally conductive filler for such heat dissipation components, taking advantage of its characteristic of having high thermal conductivity despite being an insulating material. However, it is known that h-BN particles have anisotropic thermal conductivity along the crystal axis. In order to suppress the anisotropy of properties due to orientation, studies have been conducted on obtaining heat dissipation components with higher voltage resistance and thermal conductivity by using agglomerated particles of h-BN that meet specific conditions.

[0004] Patent Document 1 proposes a BN agglomerated powder having a predetermined intraparticle pore volume and interparticle space volume measured by mercury intrusion porosimetry. Patent Document 2 proposes a BN agglomerated powder having a specified particle size distribution and agglomeration strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2022-149288 [Patent Document 2] Patent No. 7069485 Summary of the Invention [Problem to be solved by the invention]

[0006] With the BN agglomerated powder of Patent Document 1, there is concern that in some cases there may be insufficient deformation during the pressing process and / or residual voids, resulting in a decrease in the dielectric breakdown voltage. In the case of the BN agglomerated powder of Patent Document 2, when the pore volume inside and outside the particle is small, there is a concern that the breakdown voltage will decrease due to insufficient deformation and remaining voids in the pressing process, as in Patent Document 1. In addition, depending on the average elastic modulus of the BN agglomerated powder, there is a concern that the breakdown voltage will decrease due to insufficient deformation and remaining voids, as in the case above.

[0007] The present invention aims to provide a boron nitride agglomerated powder that can improve the voltage resistance characteristics of a heat dissipation sheet, a heat dissipation sheet containing this boron nitride agglomerated powder, and a semiconductor device module using this heat dissipation sheet. [Means for solving the problem]

[0008] The inventors conducted extensive research to solve the above problems and discovered that when the intra-particle pore volume and intra-particle pore area of ​​boron nitride agglomerated powder are within specific ranges in pore volume measurement by mercury intrusion porosimetry, and when the average elastic modulus is within a specific range in a single particle crush test, high voltage resistance characteristics are achieved when the boron nitride agglomerated powder is combined with a resin. That is, the present invention relates to the following.

[0009] [1] A boron nitride agglomerated powder that satisfies the following conditions a), b), and c).

[0010] a): Intraparticle pore volume measured by mercury intrusion porosimetry is greater than 0.35 ml / g and less than 0.50 ml / g b) The pore area within the particle measured by mercury intrusion porosimetry is 3 m 2 / g or greater, 6.5m 2 / g or less c) The average elastic modulus measured by single particle compression test is greater than 70 MPa and less than 150 MPa

[0011] [2] The boron nitride agglomerated powder according to [1], comprising boron nitride agglomerated particles having a house-of-cards structure. [3] A boron nitride agglomerated powder according to [1] or [2], having a particle void volume of 0.50 ml / g or more and 0.95 ml / g or less as measured by mercury intrusion porosimetry. [4] A heat dissipation sheet comprising the boron nitride agglomerated powder according to any one of [1] to [3]. [5] A semiconductor device module comprising the heat dissipation sheet according to [4]. Effect of the Invention

[0012] The boron nitride agglomerated powder of the present invention can provide a heat dissipation sheet having excellent voltage resistance characteristics, and by using this heat dissipation sheet, a semiconductor device module having good voltage resistance performance and high reliability can be realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following embodiments and can be modified in various ways within the scope of the invention.

[0014] [Boron nitride agglomerated powder] In the present invention, the boron nitride agglomerated powder (hereinafter may be simply referred to as "BN agglomerated powder") refers to a powder that is an aggregate of boron nitride agglomerated particles (hereinafter may be simply referred to as "BN agglomerated particles").

[0015] [mechanism] The mechanism by which a heat dissipation sheet with excellent withstand voltage characteristics can be obtained using the BN agglomerated powder of the present invention is estimated as follows. Although it is known that the withstand voltage characteristics are closely related to the filling rate of the BN agglomerated powder (Patent Document 2), the pore shape and the range of the average elastic modulus of the BN agglomerated powder for realizing high filling are not known.

[0016] For example, regarding the pore volume inside the particles, if the pore volume inside the particles is too small, the particles will have high strength and insufficient deformation, resulting in no improvement in the filling rate. If the pore volume inside the particles is too large, a large amount of resin will be retained inside the particles, and there will be insufficient resin to fill the spaces between the particles. Also, if the pore area inside the particles is too small, the compatibility with the resin will deteriorate, and it will be difficult for the resin to penetrate to the inside of the particles, so voids are likely to be generated. On the other hand, if the pore area inside the particles is too large, there will be insufficient resin to wet the surface of the BN agglomerated particles, resulting in poor dispersibility in the coating slurry, and thus the filling rate of the BN agglomerated particles in the sheet will decrease.

[0017] Furthermore, if the average elastic modulus is too small, excessive deformation of the particles will occur in the pressing process, and density unevenness is likely to occur in the sheet. On the other hand, if the average elastic modulus is too large, the particles will not deform, and the withstand voltage characteristics will not improve. It is known that the pore shape of the BN agglomerated powder is closely related to the particle strength (Patent Document 1). Therefore, it is considered that high withstand voltage characteristics can be obtained by adding BN agglomerated powder having an appropriate pore volume inside the particles, pore area inside the particles, and average elastic modulus to the resin.

[0018] [BN Agglomerated Particles] The BN agglomerated particles according to the present invention are formed by aggregation of BN primary particles, preferably h-BN primary particles, and may contain components other than h-BN primary particles as long as the effects of the present invention are not impaired. Examples of components other than h-BN primary particles include components derived from binders, surfactants, and solvents that may be added to the slurry, as described in the [Method for Producing BN Agglomerated Particle Powder] described later.

[0019] <Shape of BN Agglomerated Particles in BN Agglomerated Powder> The shape of the BN agglomerated particles in the BN agglomerated powder of the present invention is not particularly limited. For example, it may be any shape of agglomerated particles that can be produced by aggregating BN primary particles, such as spherical, ellipsoidal, cylindrical, hexagonal columnar, etc. In particular, in order to obtain high thermal conductivity, it is preferably card house type BN agglomerated particles having a card house structure. The card house structure is described, for example, in Ceramics 43 NO.2 (published by The Ceramic Society of Japan in 2008), and it is a structure in which plate-like particles are stacked complexly without orientation. More specifically, the BN agglomerated particles having a card house structure are an aggregate of BN primary particles, and are BN agglomerated particles having a structure in which the planar portion and the end face portion of the BN primary particles are in contact, and are preferably spherical. Also, the card house structure is preferably the same structure inside the particles. The aggregation form and internal structure of these BN agglomerated particles can be confirmed by a scanning electron microscope (SEM).

[0020] Note that the BN agglomerated particles according to the present invention preferably have a card house structure and are formed by aggregating BN primary particles, preferably h-BN primary particles, but components other than h-BN primary particles (binders, surfactants, components derived from solvents that may be added to the slurry) may be included as long as the effects of the present invention are not impaired. That is, the BN agglomerated powder of the present invention preferably is an aggregate of BN agglomerated particles including BN agglomerated particles having a card house structure, and more preferably is an aggregate of BN agglomerated particles that are BN agglomerated particles having a card house structure.

[0021] <Physical properties of BN agglomerated powder> (Tap density) The tap density of the BN agglomerated powder of the present invention is preferably 0.6 g / ml or more, more preferably 0.61 g / ml or more, even more preferably 0.63 g / ml, and particularly preferably 0.65 g / ml or more. It is also preferably less than 0.8 g / ml, more preferably 0.79 g / ml or less, and even more preferably 0.78 g / ml. Furthermore, it is preferably 0.6 g / ml or more and less than 0.8 g / ml, more preferably 0.61 g / ml or more and 0.79 g / ml or less, more preferably 0.63 g / ml or more and 0.78 g / ml or less, and particularly preferably 0.65 g / ml or more and 0.78 g / ml or less. By being in the above range, the voltage resistance characteristics are further improved.

[0022] (Intraparticle pore volume) The intraparticle pore volume of the BN agglomerated powder of the present invention is greater than 0.35 ml / g, preferably 0.40 ml / g or more. It is also less than 0.5 ml / g, preferably 0.47 ml / g or less. By being in the above range, the strength of the BN agglomerated powder and the amount of resin between the BN agglomerated particles when made into a sheet are appropriate, and voids in the sheet are suppressed, thereby further improving the voltage resistance characteristics.

[0023] (Intraparticle pore area) The intraparticle pore area of ​​the BN agglomerated powder of the present invention is 3 m 2 / g, preferably 3.5m 2 / g or more, more preferably 4m 2 / g or more. Also, 6.5m 2 / g, preferably less than 6m 2 When the BN content is within the above range, the BN agglomerated particles in the coating slurry are well dispersed, and voids in the sheet are suppressed, resulting in further improved voltage resistance characteristics.

[0024] (particle interstitial volume) The interparticle volume of the BN agglomerated powder of the present invention is preferably 0.50 ml / g or more, more preferably 0.55 ml / g or more, even more preferably 0.58 ml / g or more, and particularly preferably 0.6 ml / g or more. Also, it is preferably 0.95 ml / g or less, more preferably 0.8 ml / g or less. By being in the above range, the amount of resin between the BN agglomerated particles when made into a sheet is appropriate, and voids in the sheet are suppressed, thereby further improving the voltage resistance characteristics.

[0025] The intraparticle pore volume, intraparticle pore area, and interparticle volume were each measured in accordance with JIS R1655:2003 "Test method for pore size distribution of fine ceramics molded bodies by mercury intrusion method." Specifically, a Micromeritics Autopore IV mercury porosimeter was used, 200 mg of sample was filled into a measurement cell, and the sample was subjected to a reduced pressure treatment (50 μmHg or less) for 10 minutes, after which the total pore volume was determined and the mercury intrusion / extrusion curve was measured. A pore size distribution curve was created with the pore size on the horizontal axis and the logarithmic differential pore volume on the vertical axis, and the diameter (division diameter) where the logarithmic differential pore volume was the minimum value with respect to the pore size was read between peak a, which represents the intraparticle pores, and peak b, which represents the interparticle pores, assuming that the pores are cylindrical. The interparticle void volume (ml / g) was calculated from the integral value of the mercury intrusion / extrusion curve in the region where the pore size is larger than the division diameter.

[0026] The intra-particle pore volume was calculated by subtracting the inter-particle volume from the total pore volume. Furthermore, assuming that the pores are cylindrical, the pore side areas calculated from the pore volumes for each pore diameter were integrated, and the integral value in the region where the pore diameter was smaller than the above division diameter was calculated as the intra-particle pore area.

[0027] (Average particle diameter (D 50 )) The average particle size (D 50 ) is not particularly limited, but is preferably 20 μm or more, more preferably 25 μm or more, further preferably 30 μm or more, and particularly preferably 40 μm or more. On the other hand, D of the BN agglomerated powder50 is preferably 150 μm or less, more preferably 130 μm or less, further preferably 100 μm or less, and particularly preferably 95 μm or less. 50 When the BN agglomerated powder has a surface roughness of 1.5 mm or less, the thermal conductivity of the BN agglomerated powder itself is high. ...

[0028] Here, the average particle diameter of the BN agglomerated powder (D 50 ) refers to the particle size at which a cumulative volume of the BN agglomerated powder used in the measurement is 50% when a cumulative curve is drawn assuming the volume of the powder to be measured to be 100%. Examples of the measurement method include a wet measurement method in which a sample in which BN agglomerated particles are dispersed in a pure water medium containing sodium hexametaphosphate as a dispersion stabilizer is measured using a laser diffraction / scattering particle size distribution measurement device, and a dry measurement method in which measurement is performed using "MORPHOLOGI" manufactured by MALVERN.

[0029] (Average circularity) The average circularity of the BN agglomerated powder of the present invention is not particularly limited, but is preferably 0.8 or more, and more preferably 0.85 or more. The upper limit is not particularly limited and may be 1. By being within these ranges, the interparticle volume is in an appropriate range, and the effects of the present invention tend to be easily achieved.

[0030] The average circularity of the BN agglomerated powder was determined by dispersing the BN agglomerated powder in a pressure pulse sample dispersion unit using a MORPHOLOGIG3S manufactured by MALVERN and performing image analysis.

[0031] (Compressive strength) The compressive strength of the BN agglomerated particles constituting the BN agglomerated powder of the present invention has a distribution of preferably 15 MPa or less, more preferably 13 MPa or less, and even more preferably 10 MPa or less. It is also preferably 3 MPa or more, more preferably 4 MPa or more, even more preferably 5 MPa or more, and particularly preferably 6 MPa or more. By being within these ranges, the BN agglomerated particles can be appropriately deformed, and when a heat dissipation sheet is produced, the thermal conductivity of the heat dissipation sheet is improved.

[0032] The compressive strength of the BN agglomerated particles was measured using a micro-compression tester MCT-510 manufactured by Shimadzu Corporation, using a test force, loading speed, and upper pressure indenter according to the particle size. One BN agglomerate particle was selected and tested, and this was repeated at least five times to determine the compressive strength. The compressive strength was calculated using formula (1). The average compressive strength was calculated by dividing the total compressive strength by the number of tests. Cs=2.48P / πd 2 (1) Cs: compressive strength (MPa), P: test force (N), d: particle size (mm)

[0033] (Average elastic modulus) The average elastic modulus of the BN agglomerated powder of the present invention is greater than 70 MPa, preferably 80 MPa or more, and more preferably 90 MPa or more. Also, it is less than 150 MPa, preferably 140 MPa or less, and more preferably 130 MPa or less. When the average elastic modulus of the BN agglomerated powder is within these ranges, the BN agglomerated particles can be appropriately deformed, and when a heat dissipation sheet is produced, the voltage resistance characteristic of the heat dissipation sheet is improved.

[0034] The elastic modulus of the BN agglomerated particles was calculated from the test force (N), compression displacement (μm), and particle diameter (mm) obtained from a compression test of the BN agglomerated particles (compression test using a Shimadzu microcompression tester) using the following formula (2) (Patent Document WO2014136959A1), with reference to Busshi Kenkyu, Yoshimi Tanaka, 85(4), 499-518, 2006. The average elastic modulus is the average value of the elastic modulus, and is preferably the average value obtained from 5 or more BN agglomerated particles.

[0035] E = 3 × (1-ν 2 )×P / (4×(d / 2) 1 / 2 ×δ 3 / 2 ) (2) E: Elastic modulus (MPa), ν: Poisson's ratio (-) (Poisson's ratio was set to 0.13) P: test force (N), d: particle size (mm), δ: compression displacement (μm)

[0036] In order to set the intra-particle pore volume, intra-particle pore area, and average elastic modulus within the above ranges, for example, there can be mentioned a method of setting a holding temperature in the range of 1550°C to 1750°C during the heat treatment of the BN agglomerated granulated particles, a method of changing the holding time at the above temperature, a method of adjusting the amount of boron oxide in the raw material, or a method of adjusting by removing boron oxide by carbothermal reduction.

[0037] [Method of manufacturing BN agglomerated powder] There is no limitation on the method for producing the BN agglomerated powder of the present invention, but it is particularly preferable to pulverize the raw material boron nitride (hereinafter, together with the pulverized product, it may be referred to as "raw BN powder") in a pulverization step, granulate by agglomeration in a granulation step, and then pass through a heating step in which heat treatment is performed. More specifically, it is preferable to disperse the raw material BN powder in a medium once to make a slurry of the raw material BN powder (hereinafter, it may be referred to as "BN slurry"), perform a dispersion treatment, and then granulate the obtained slurry into spherical particles, and perform a heat treatment to crystallize the granulated BN agglomerated particles.

[0038] <Raw material BN powder> As the raw BN powder, any of commercially available h-BN, commercially available α- and β-BN, BN produced by the reduction-nitridation method of a boron compound and ammonia, and BN synthesized from a boron compound and a nitrogen-containing compound such as melamine can be used without limitation, but h-BN is particularly preferred in that it more effectively exerts the effects of the present invention.

[0039] As the form of the raw material BN powder, powdered BN particles having a wide half-width of the peak obtained by powder X-ray diffraction measurement and low crystallinity are suitable. That is, it is possible to use plate-shaped h-BN as the raw material, but non-plate-shaped nanoparticles are also preferably used. As a guideline for crystallinity, the peak half-width of the (002) plane obtained by powder X-ray diffraction measurement is usually 0.4° or more, preferably 0.45° or more, and more preferably 0.5° or more, in terms of 2θ angle. Also, it is usually 2.0° or less, preferably 1.5° or less, and more preferably 1° or less. When the peak half-width of the (002) plane is equal to or less than the above upper limit, crystal growth is easily controlled and productivity tends to improve. When the peak half-width of the (002) plane is equal to or more than the above lower limit, it is easy to control the primary particle size within an appropriate range, and therefore it is easy to control the compression displacement, compression strength, and elastic modulus of the BN aggregate particles to a desired distribution. In addition, the dispersion stability during slurry preparation tends to improve.

[0040] From the viewpoint of BN crystal growth, it is preferable that oxygen atoms are present to a certain extent in the raw BN powder, and in the present invention, the total oxygen concentration in the raw BN powder is preferably 1 mass% or more, more preferably 2 mass% or more, even more preferably 3 mass% or more, particularly preferably 4 mass% or more, and preferably 10 mass% or less, more preferably 9 mass% or less. By having the total oxygen concentration be equal to or less than the upper limit, crystal growth is not excessive, and the compressive displacement, compressive strength, and elastic modulus of the BN aggregate particles can be controlled within appropriate ranges. By having the total oxygen concentration be equal to or more than the lower limit, residual oxygen after heat treatment is suppressed, and the effect of improving thermal conductivity is enhanced.

[0041] Methods for adjusting the total oxygen concentration of the raw BN powder to fall within the above range include, for example, synthesizing BN at a low temperature of 1500°C or less, or heat treating the raw BN powder in an oxidizing atmosphere at a low temperature of 500°C to 900°C. The total oxygen concentration of the raw material BN powder can be measured by an inert gas fusion-infrared absorption method using an oxygen / nitrogen analyzer manufactured by Horiba, Ltd.

[0042] The total pore volume of the raw BN powder is preferably 1.5 cm 3 / g or less, more preferably 0.3 cm 3 / g or more 1.5cm 3 / g or less, more preferably 0.5 cm 3 / g or more 1.5cm 3 / g or less. The total pore volume is 1.5 cm 3 / g or less, the raw material BN powder is dense, making it possible to form granules with high sphericity.

[0043] The specific surface area of ​​the raw BN powder is preferably 50 m 2 / g or more, more preferably 60m 2 / g or more, more preferably 70m 2 On the other hand, it is preferably 1000m 2 / g or less, more preferably 500m 2 / g or less, more preferably 300m 2 / g or less. The specific surface area of ​​the raw BN powder is 50m 2 / g or more, the dispersed particle diameter in the BN slurry used for spheroidization by granulation can be made small, which is preferable. 2 / g or less is preferable because it is possible to suppress an increase in the slurry viscosity.

[0044] The total pore volume of the raw material BN powder can be measured by the nitrogen adsorption method and the mercury intrusion method, and the specific surface area can be measured by the BET one-point method (adsorption gas: nitrogen).

[0045] <medium> The medium used in preparing the BN slurry is not particularly limited, and water and / or various organic solvents can be used. From the viewpoints of ease of spray drying and simplification of the equipment, however, it is preferable to use water, and pure water is more preferable. The medium used in preparing the BN slurry is preferably added in an amount that gives the BN slurry a viscosity of 200 to 5000 mPa·s.

[0046] Specifically, the amount of the medium used to prepare the BN slurry is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, and is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 60% by mass or less, relative to the BN slurry. When the amount of the medium used is equal to or less than the upper limit, the slurry viscosity does not become too low, so that sedimentation and the like are suppressed, and the uniformity of the BN slurry tends to be obtained. Therefore, the tap density of the obtained BN agglomerated powder tends to be in the desired range. When the amount of the medium used is equal to or more than the lower limit, the slurry viscosity does not become excessively high, and granulation tends to be easy.

[0047] <Surfactant> Various surfactants may be added to the BN slurry in order to adjust the viscosity of the slurry and to improve the dispersion stability (suppression of aggregation) of the raw BN powder in the slurry. As the surfactant, anionic surfactants, cationic surfactants, nonionic surfactants, etc. can be used, and these may be used alone or in combination of two or more kinds.

[0048] <Binder> The BN slurry may contain a binder to effectively granulate the raw BN powder into particles. The binder acts to firmly bind the BN primary particles and stabilize the granulated particles. The binder used in the BN slurry may be any that can increase the adhesion between BN particles. In the present invention, however, since the granulated particles are heat-treated after granulation, it is preferable that the binder has heat resistance to the high temperature conditions in this heat treatment process.

[0049] As such binders, metal oxides such as aluminum oxide, magnesium oxide, yttrium oxide, calcium oxide, silicon oxide, boron oxide, cerium oxide, zirconium oxide, titanium oxide, etc. are preferably used. Among these, from the viewpoints of thermal conductivity as an oxide, heat resistance, and the binding force for binding BN particles to each other, aluminum oxide and yttrium oxide are suitable. Note that a liquid binder such as alumina sol may be used as the binder, and it may react during the heat treatment and be converted into other inorganic components. These binders may be used alone or in combination of two or more.

[0050] The amount of the binder used (in the case of a liquid binder, the amount used as a solid content) is preferably 0 mass% or more and 30 mass% or less, more preferably 0 mass% or more and 20 mass% or less, and still more preferably 0 mass% or more and 15 mass% or less with respect to the raw material BN powder in the BN slurry. When the amount of the binder used is below the above upper limit value, crystal growth can be obtained, and a tendency to obtain a thermal conductivity improvement effect when used as a filler for thermal conductivity is observed.

[0051] <BN Slurry Preparation Method> The method for preparing the BN slurry is not particularly limited as long as the raw material BN powder, the medium, and further, if necessary, the binder and the surfactant are uniformly dispersed and adjusted to a desired viscosity range. However, when using the raw material BN powder, the medium, and further, if necessary, the binder and the surfactant, it is preferably prepared as follows.

[0052] Weigh a predetermined amount of the raw material BN powder into a resin bottle, and then add a predetermined amount of the binder. Further, after adding a predetermined amount of the surfactant as necessary, add zirconia ceramic balls and stir for about 0.5 to 5 hours on a pot mill turntable until a desired viscosity is reached. The order of addition is not particularly limited, but since agglomerates such as lumps are likely to form when a large amount of raw BN powder is made into a slurry, it is also possible to prepare an aqueous solution by adding a surfactant and a binder to water, add a predetermined amount of raw BN powder little by little, add zirconia ceramic balls to this, and disperse and slurried on a pot mill rotating table.

[0053] For dispersion, a dispersing device such as a bead mill or a planetary mixer may be used in addition to a pot mill. When forming the slurry, the temperature of the slurry is preferably 10° C. or more and 60° C. or less. When the slurry temperature is equal to or more than the lower limit, an increase in the viscosity of the slurry tends to be suppressed, and when the slurry temperature is equal to or less than the upper limit, the raw material BN powder can be suppressed from decomposing into ammonia in the slurry. The temperature of the slurry is more preferably 15°C or more and 50°C or less, further preferably 15°C or more and 40°C or less, and particularly preferably 15°C or more and 35°C or less.

[0054] <Granulation> To obtain granulated particles from the BN slurry, a general granulation method such as a spray-drying method, a rolling method, a fluidized bed method, or a stirring method can be used, and among these, the spray-drying method is preferred. In the spray drying method, it is possible to produce granulated particles of a desired size by adjusting the concentration of the raw material slurry, the amount of liquid fed per unit time into the device, and the compressed air pressure and amount of compressed air when spraying the fed slurry, and it is also possible to obtain spherical granulated particles. There is no restriction on the spray drying device used, but in order to obtain larger spherical granulated particles, a rotary disk type device is optimal. Examples of such devices include the spray dryer F series manufactured by Okawara Kakoki Co., Ltd., the spray dryer "MDL-050M" manufactured by Fujisaki Electric Co., Ltd., and the spray dryer "P260" manufactured by PRIS.

[0055] When the volume-based average particle size of the BN agglomerated powder of the present invention is set to a range of 20 μm to 150 μm, the average particle size of the granulated particles obtained by granulation is defined as the volume-based average particle size D 50The volume-based average particle diameter D of the granulated particles is preferably 20 μm or more and 150 μm or less. 50 can be measured using a device such as Malvern's "Morphorogi."

[0056] <Heat treatment> The above-mentioned granulated BN powder can be further heat-treated in a non-oxidizing gas atmosphere to produce an agglomerated BN powder. Here, the non-oxidizing gas atmosphere refers to an atmosphere of nitrogen gas, helium gas, argon gas, ammonia gas, hydrogen gas, methane gas, propane gas, carbon monoxide gas, etc. The crystallization speed of the BN agglomerated particles varies depending on the type of atmospheric gas used. In order to perform crystallization in a short time, nitrogen gas or a mixed gas of nitrogen gas and other gases is particularly preferably used.

[0057] The heat treatment temperature is preferably 1400°C or higher and 2300°C or lower, more preferably 1500°C or higher and 2000°C or lower, and further preferably 1600°C or higher and 2000°C or lower. When the heat treatment temperature is equal to or higher than the lower limit, the BN primary particles grow sufficiently, and the thermal conductivity of the BN agglomerated powder tends to be increased. When the heat treatment temperature is equal to or lower than the upper limit, decomposition of the BN agglomerated powder tends to be suppressed.

[0058] The heat treatment time is preferably 5 hours or more and 20 hours or less, more preferably 5 hours or more and 15 hours or less. When the heat treatment time is equal to or more than the lower limit, the growth of the BN primary particles is sufficient, and when the heat treatment time is equal to or less than the upper limit, the decomposition of BN tends to be suppressed. Therefore, the compression displacement, compression strength, and elastic modulus of the BN aggregate particles can be controlled within the desired range. Since the heat treatment is carried out in a non-oxidizing gas atmosphere, the inside of the firing furnace is usually evacuated with a vacuum pump, and then the furnace is heated to a desired temperature while introducing a non-oxidizing gas. When the atmosphere in the calcination furnace can be sufficiently replaced with a non-oxidizing gas, the temperature may be increased while introducing the non-oxidizing gas under normal pressure. Examples of the calcination furnace include batch furnaces such as muffle furnaces, tubular furnaces, and atmospheric furnaces, and continuous furnaces such as rotary kilns, screw conveyor furnaces, tunnel furnaces, belt furnaces, pusher furnaces, and vertical continuous furnaces, and these are used according to the purpose.

[0059] Usually, the BN agglomerated powder to be heat-treated is heated and sintered in a graphite crucible with a lid in order to reduce the non-uniformity of the composition during sintering. At this time, in addition to reducing the non-uniformity of the composition, a graphite partition may be inserted in order to suppress sintering of the BN agglomerated particles during sintering. The number of divisions by partitions is not particularly limited as long as sintering can be suppressed, but is usually 2 to 16. By setting the number of divisions to the upper limit or less and the lower limit or more, sintering can be suppressed and the growth of h-BN primary particles can be controlled. Therefore, the compression displacement, compression strength, and elastic modulus of the BN aggregate particles can be controlled within the desired range.

[0060] <Classification> The BN agglomerated powder after the heat treatment is preferably classified to narrow the particle size distribution and suppress the increase in viscosity when blended into a resin composition containing the BN agglomerated powder. This classification is usually performed after the heat treatment, but it may be performed on the granulated particles before the heat treatment and then subjected to the heat treatment.

[0061] The classification may be either wet or dry, but dry classification is preferred from the viewpoint of suppressing the decomposition of BN, and is particularly preferred when the binder is water-soluble. Dry classification includes classification using a sieve, as well as air classification, which classifies based on the difference between centrifugal force and fluid drag, but it can also be performed using a classifier such as a swirling air classifier, a forced vortex centrifugal classifier, or a semi-free vortex centrifugal classifier. Of these, a swirling air classifier is used to classify small particles in the submicron to single micron range, and a semi-free vortex centrifugal classifier is used to classify relatively larger particles, depending on the particle size of the particles to be classified.

[0062] [BN agglomerated powder-containing resin composition] To manufacture the heat dissipation sheet of the present invention containing the BN agglomerated powder of the present invention, a resin composition containing at least the BN agglomerated powder of the present invention as an inorganic filler and a resin (hereinafter, sometimes referred to as the "composition containing the BN agglomerated powder of the present invention" or the "composition of the present invention") is prepared, and the prepared composition of the present invention is formed into a sheet to obtain the heat dissipation sheet of the present invention. The composition containing the BN agglomerated powder of the present invention will be described below.

[0063] The BN agglomerated powder-containing resin composition of the present invention is usually composed of a resin component, preferably a thermosetting resin component, an inorganic filler containing the BN agglomerated powder of the present invention, a curing agent, a curing catalyst, other components used as necessary, a solvent for preparing a coating slurry, etc. In addition, when preparing a composite molded product as described below, the composition of the present invention preferably contains a compound having a heterocyclic structure containing a nitrogen atom from the viewpoint of improving adhesion to metals.

[0064] [Ingredients other than BN agglomerated powder] <Thermosetting resin component> The thermosetting resin contained in the composition of the present invention is not particularly limited as long as it is cured in the presence of a curing agent or a curing catalyst. Specific examples of the thermosetting resin include epoxy resins, phenolic resins, polycarbonate resins, unsaturated polyester resins, urethane resins, melamine resins, and urea resins. Among these, epoxy resins are preferred from the viewpoints of viscosity, heat resistance, moisture absorption, and handling. Examples of the epoxy resin include epoxy group-containing silicon compounds, aliphatic epoxy resins, bisphenol A or F epoxy resins, novolac epoxy resins, alicyclic epoxy resins, glycidyl ester epoxy resins, multifunctional epoxy resins, and polymeric epoxy resins.

[0065] (Epoxy resin) Epoxy resin is a general term for compounds having one or more oxirane rings (epoxy groups) in the molecule. The oxirane rings (epoxy groups) contained in the epoxy resin may be either alicyclic epoxy groups or glycidyl groups, but from the viewpoint of reaction speed or heat resistance, glycidyl groups are more preferable.

[0066] The epoxy resin used in the present invention may be an aromatic oxirane ring (epoxy group)-containing compound. Specific examples thereof include bisphenol-type epoxy resins obtained by glycidylating bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetramethyl bisphenol A, tetramethyl bisphenol F, tetramethyl bisphenol AD, tetramethyl bisphenol S, and tetrafluorobisphenol A, biphenyl-type epoxy resins, dihydroxynaphthalene, 9,9-bis(4-hydroxyphenyl)fluorene, and other divalent phenols, glycidylating trisphenols such as 1,1,1-tris(4-hydroxyphenyl)methane, and other epoxy resins obtained by glycidylating tetrakisphenols such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, and novolac-type epoxy resins obtained by glycidylating novolacs such as phenol novolac, cresol novolac, bisphenol A, novolac, and brominated bisphenol A novolac.

[0067] Hereinafter, an epoxy resin (hereinafter sometimes referred to as a "specific epoxy resin") suitable as the epoxy resin used in the present invention and a polyfunctional epoxy resin that is preferably used in combination with this specific epoxy resin will be described. In the following, the term "organic group" includes any group containing a carbon atom, and specific examples thereof include an alkyl group, an alkenyl group, an aryl group, etc., which may be substituted with a halogen atom, a group having a heteroatom, or another hydrocarbon group.

[0068] (Specific epoxy resin) The specific epoxy resin includes an epoxy resin having at least one structure selected from a structure represented by the following structural formula (1) (hereinafter, sometimes referred to as "Structure (1)") and a structure represented by the following structural formula (2) (hereinafter, sometimes referred to as "Structure (2)").

[0069] [ka]

[0070] (In structure (1), R 1 and R 2 Each of R represents an organic group, at least one of which is an organic group having a molecular weight of 16 or more. In the structure (2), R 3 represents a divalent cyclic organic group.) The specific epoxy resin may also be an epoxy resin having a structure represented by the following structural formula (3) (hereinafter sometimes referred to as "structure (3)").

[0071] [ka]

[0072] (In structure (3), R 4 , R 5 , R 6 , R 7 Each represents an organic group having a molecular weight of 15 or more. In the above structure (1), R 1 and R 2 At least one of R represents an organic group having a molecular weight of 16 or more, preferably a molecular weight of 16 to 1000, and examples of such groups include alkyl groups such as ethyl, propyl, butyl, pentyl, hexyl, and heptyl groups, and aryl groups such as phenyl, tolyl, xylyl, naphthyl, and fluorenyl groups. 1 and R 2may both be organic groups having a molecular weight of 16 or more, or one may be an organic group having a molecular weight of 16 or more and the other an organic group having a molecular weight of 15 or less or a hydrogen atom; however, preferably, one is an organic group having a molecular weight of 16 or more and the other an organic group having a molecular weight of 15 or less, and in particular, one of them being a methyl group and the other a phenyl group, which is preferable from the standpoint of easier control of handleability such as the resin viscosity and of the strength of the cured product.

[0073] In structure (2), R 3 is a divalent cyclic organic group, which may be an aromatic ring structure such as a benzene ring structure, a naphthalene ring structure, or a fluorene ring structure, or an aliphatic ring structure such as cyclobutane, cyclopentane, or cyclohexane. They may also independently have a substituent such as a hydrocarbon group or a halogen atom. The divalent bond may be a divalent group on a single carbon atom, or a divalent group on different carbon atoms. Preferred examples include divalent aromatic groups having 6 to 100 carbon atoms, and groups derived from cycloalkanes having 2 to 100 carbon atoms such as cyclopropane and cyclohexane. In particular, the 3,3,5-trimethyl-1,1-cyclohexylene group represented by the following structural formula (4) is preferred from the viewpoints of controlling the handleability such as the resin viscosity and the strength of the cured product.

[0074] [ka]

[0075] In structure (3), R 4 , R 5 , R 6 , R 7 Each of R is an organic group having a molecular weight of 15 or more, preferably an alkyl group having a molecular weight of 15 to 1000, and particularly preferably R 4 , R 5 , R 6 , R 7 It is preferable that all of the above be methyl groups from the viewpoints of controlling the handleability of the resin, such as viscosity, and strength of the cured product.

[0076] The specific epoxy resin is preferably an epoxy resin containing either one of Structure (1) and Structure (2) and Structure (3), from the viewpoint of achieving both reduced moisture absorption and strength retention of the resulting cured heat dissipation sheet. Since such specific epoxy resins contain more hydrophobic hydrocarbon and aromatic structures than general epoxy resins having bisphenol A or bisphenol F skeletons, by blending the specific epoxy resins, it is possible to reduce the moisture absorption amount of the heat dissipation sheet obtained as a cured product.

[0077] From the viewpoint of reducing the amount of moisture absorption, the specific epoxy resin preferably contains a large amount of structures (1), (2), and (3), which are hydrophobic structures. Specifically, the specific epoxy resin is preferably an epoxy resin having a weight-average molecular weight of 10,000 or more, more preferably an epoxy resin having a weight-average molecular weight of 20,000 or more, and even more preferably an epoxy resin having a weight-average molecular weight of 30,000 or more, for example, 30,000 to 40,000.

[0078] In addition, the specific epoxy resin is preferably more hydrophobic, and specifically, the epoxy equivalent of the specific epoxy component is preferably larger, and is preferably 5,000 g / equivalent or more, more preferably 7,000 g / equivalent or more, for example, 8,000 to 15,000 g / equivalent. Here, the weight average molecular weight of the epoxy resin is a value calculated in terms of polystyrene measured by gel permeation chromatography. The epoxy equivalent is defined as "the weight of the epoxy resin containing one equivalent of epoxy groups" and can be measured in accordance with JIS K7236. Such specific epoxy resins may be used alone or in combination of two or more kinds.

[0079] (Multifunctional epoxy resin) A multifunctional epoxy resin is an epoxy resin that has three or more oxirane rings (epoxy groups) per molecule. From the viewpoint of increasing the storage modulus of the cured product after thermal curing, particularly the storage modulus at high temperatures which is important when a large amount of heat is generated such as in a semiconductor device module, an epoxy resin having two or more oxirane rings (epoxy groups) in the molecule is preferred, an epoxy resin having three or more oxirane rings (epoxy groups) in the molecule is more preferred, and an epoxy resin having four or more glycidyl groups in the molecule is even more preferred. By having a plurality of oxirane rings (epoxy groups), particularly glycidyl groups, in the molecule, the crosslink density of the cured product is improved, and the heat dissipation sheet obtained as the cured product has a higher strength. As a result, when internal stress occurs in the heat dissipation sheet during a moisture absorption reflow test, the heat dissipation sheet does not deform or break, but maintains its shape, thereby suppressing the occurrence of voids and other voids in the heat dissipation sheet.

[0080] Furthermore, from the viewpoint of increasing the storage modulus of the heat dissipation sheet after thermal curing, the molecular weight of the polyfunctional epoxy resin is preferably 1,000 or less, and more preferably 100-800. In addition, by adding a polyfunctional epoxy resin, it is possible to introduce highly polar oxirane rings (epoxy groups) at a high density, which increases the effects of physical interactions such as van der Waals forces and hydrogen bonds, and improves the adhesion between the metal in the composite molded body described below and the heat dissipation sheet of the present invention, which is the resin cured product. In addition, by adding a polyfunctional epoxy resin, it is possible to increase the storage modulus of the heat dissipation sheet after thermal curing, and as a result, after the cured product of the thermosetting resin composition penetrates into the unevenness of the metal to be adhered, a strong anchor effect is exerted, and the adhesion between the metal and the heat dissipation sheet can be improved.

[0081] On the other hand, the introduction of a polyfunctional epoxy resin tends to increase the hygroscopicity of the thermosetting resin composition, but by improving the reactivity of the oxirane ring (epoxy group), the amount of hydroxyl groups during the reaction can be reduced and the increase in hygroscopicity can be suppressed. In addition, by combining the specific epoxy resin and a polyfunctional epoxy resin described above to produce a thermosetting resin composition, it is possible to achieve both high elasticity and low hygroscopicity in the obtained heat dissipation sheet.

[0082] Specifically, the polyfunctional epoxy resin is preferably an epoxy resin having three or more epoxy groups, and for example, EX321L, DLC301, DLC402, etc. manufactured by Nagase ChemteX Corporation can be used. These polyfunctional epoxy resins may be used alone or in combination of two or more.

[0083] (Content) The composition of the present invention preferably contains 5 to 99 mass %, particularly 50 to 98 mass %, of a thermosetting resin component based on 100 mass % of the composition of the present invention excluding the solvent and inorganic filler. When the content of the thermosetting resin component is equal to or more than the above lower limit, the moldability is good, and when it is equal to or less than the above upper limit, the content of other components can be secured, and thermal conductivity can be increased. The composition of the present invention preferably contains an epoxy resin in an amount of 20 to 100 mass %, particularly 45 to 100 mass %, in the thermosetting resin component.

[0084] In addition, the composition of the present invention preferably contains the specific epoxy resin, which is the above-mentioned suitable epoxy resin, in an amount of 50% by mass or less, for example 5 to 50% by mass, particularly 10 to 40% by mass, based on the total epoxy resin. When the content of the specific epoxy resin is equal to or more than the above-mentioned lower limit, the above-mentioned effects due to the inclusion of the specific epoxy resin can be effectively obtained. On the other hand, when the content of the specific epoxy resin is too much, the crosslinking density decreases and the cured product becomes brittle. By controlling the content of the specific epoxy resin to equal to or less than the above-mentioned upper limit, it is possible to suppress the moisture absorption of the cured product and to improve the strength performance of the cured product, thereby achieving both of these performances.

[0085] In addition, the composition of the present invention preferably contains 5 to 50 mass %, particularly 10 to 40 mass %, of the polyfunctional epoxy resin, which is the above-mentioned preferred epoxy resin, based on the total epoxy resin. When the content of the polyfunctional epoxy resin is equal to or more than the above-mentioned lower limit, the above-mentioned effect due to the inclusion of the polyfunctional epoxy resin can be effectively obtained. On the other hand, when the content of the polyfunctional epoxy resin is equal to or less than the above-mentioned upper limit, the moisture absorption of the cured product is suppressed and the strength performance of the cured product is excellent, making it possible to achieve both of these performances.

[0086] In particular, it is preferable that the composition of the present invention contains both a specific epoxy resin and a polyfunctional epoxy resin as epoxy resins in order to obtain a cured product with both high elasticity and low moisture absorption. In this case, the content ratio of the specific epoxy resin to the polyfunctional epoxy resin is preferably specific epoxy resin:polyfunctional epoxy resin=10-90:90-10, particularly 20-80:80-20 (mass ratio).

[0087] The epoxy resin other than the specific epoxy resin and the polyfunctional epoxy resin contained in the composition of the present invention is not particularly limited, but is preferably one or more selected from various bisphenol-type epoxy resins obtained by glycidylating bisphenols such as bisphenol A-type epoxy resins and bisphenol F-type epoxy resins, various biphenyl-type epoxy resins obtained by glycidylating biphenyls, epoxy resins obtained by glycidylating aromatic compounds having two hydroxyl groups such as dihydroxynaphthalene and 9,9-bis(4-hydroxyphenyl)fluorene, epoxy resins obtained by glycidylating trisphenols such as 1,1,1-tris(4-hydroxyphenyl)methane, epoxy resins obtained by glycidylating tetrakisphenols such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, novolac-type epoxy resins obtained by glycidylating novolacs such as phenol novolac, cresol novolac, bisphenol A novolac, and brominated bisphenol A novolac, and silicone-containing epoxy resins.

[0088] <Compounds Having a Heterocyclic Structure Containing a Nitrogen Atom> A compound having a heterocyclic structure containing a nitrogen atom (hereinafter, sometimes referred to as a "nitrogen-containing heterocyclic compound") has the effect of improving the adhesion between the cured product of the composition of the present invention and a metal. That is, when the composition of the present invention is composited with a metal, the nitrogen-containing heterocyclic compound is located at the interface between them, thereby improving the adhesion between the composition of the present invention and the metal. From this viewpoint, in order to make it easier for the nitrogen-containing heterocyclic compound to remain at the interface between the composition of the present invention and the metal, it is more preferable that the molecular weight is low, and the molecular weight of the nitrogen-containing heterocyclic compound is preferably 1,000 or less, more preferably 500 or less.

[0089] Examples of the heterocyclic structure of the nitrogen-containing heterocyclic compound include structures derived from imidazole, triazine, triazole, pyrimidine, pyrazine, pyridine, and azole. From the viewpoint of improving the insulating properties of the thermosetting resin composition and adhesion to metals, imidazole-based compounds and triazine-based compounds are preferred. Preferable imidazole compounds and triazine compounds include, for example, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl- ethyl-4'methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4-diamino-6-vinyl-s-triazine, 2,4-diamino-6-vinyl-s-triazine isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-s-triazine, 2,4-diamino-6-methacryloyloxyethyl-s-triazine isocyanuric acid adduct, and the like.

[0090] Among these, those having a structure derived from imidazole and those having a structure derived from triazine are particularly preferred, since they have high resin compatibility and a high reaction activation temperature, and thus the curing speed and physical properties after curing can be easily adjusted, thereby improving the storage stability of the composition of the present invention and further improving the adhesive strength after heat molding.As the heterocyclic structure of the nitrogen-containing heterocyclic compound, a structure derived from 1,3,5-triazine is particularly preferred. Moreover, the compound may have a plurality of the structural moieties exemplified above.

[0091] Depending on the structure, the nitrogen-containing heterocyclic compound may contain a curing catalyst, which will be described later, and therefore the composition of the present invention may contain a nitrogen-containing heterocyclic compound as a curing catalyst. The nitrogen-containing heterocyclic compound may be used alone or in combination of two or more kinds. Also, one molecule may simultaneously have a plurality of heterocyclic structures.

[0092] The nitrogen-containing heterocyclic compound is preferably contained in an amount of 0.001 to 10 mass%, particularly 0.1 to 5 mass%, based on 100 mass% of the composition of the present invention excluding the solvent and inorganic filler. When a curing catalyst described later is contained in the nitrogen-containing heterocyclic compound due to its molecular structure, the total amount including the content of the catalyst is preferably within the above range. When the content of the nitrogen-containing heterocyclic compound is equal to or more than the above lower limit, the above effects due to the inclusion of this compound can be sufficiently obtained, and when the content is equal to or less than the above upper limit, the reaction proceeds effectively, the crosslinking density is improved, the strength can be increased, and storage stability is improved.

[0093] <Hardening agent> The curing agent is not particularly limited, but the preferred curing agent is a phenol resin, an acid anhydride having an aromatic skeleton or an alicyclic skeleton, or a water additive of the acid anhydride or a modified product of the acid anhydride. By using these preferred curing agents, a resin cured product having a good balance of heat resistance, moisture resistance, and electrical properties can be obtained. The curing agent may be used alone or in combination of two or more kinds.

[0094] The phenolic resin is not particularly limited. Specific examples of the phenolic resin include phenolic novolac, o-cresol novolac, p-cresol novolac, t-butylphenol novolac, dicyclopentadiene cresol, polyparavinylphenol, bisphenol A type novolac, xylylene modified novolac, decalin modified novolac, poly(di-o-hydroxyphenyl)methane, poly(di-m-hydroxyphenyl)methane, or poly(di-p-hydroxyphenyl)methane. Among them, in order to further improve the flexibility and flame retardancy of the thermosetting resin composition and to improve the mechanical properties and heat resistance of the cured resin, a novolac type phenolic resin having a rigid main chain skeleton or a phenolic resin having a triazine skeleton is preferred. In addition, in order to improve the flexibility of the uncured thermosetting resin composition and the toughness of the cured resin, a phenolic resin having an allyl group is preferred.

[0095] Commercially available phenolic resins include MEH-8005, MEH-8000H and NEH-8015 (all manufactured by Meiwa Chemical Industry Co., Ltd.), YLH903 (manufactured by Mitsubishi Chemical Corporation), LA-7052, LA-7054, LA-7751, LA-1356 and LA-3018-50P (all manufactured by Dainippon Ink Co., Ltd.), as well as PSM6200, PS6313 and PS6492 (manufactured by Gun-ei Chemical Industry Co., Ltd.).

[0096] The acid anhydride having an aromatic skeleton, the water additive of the acid anhydride, or the modified product of the acid anhydride is not particularly limited.Specific examples include SMA resin EF30 and SMA resin EF60 (both manufactured by Sartomer Japan Co., Ltd.), ODPA-M and PEPA (both manufactured by Manac Co., Ltd.), Ricadit MTA-10, Ricadit TMTA, Ricadit TMEG-200, Ricadit TMEG-500, Ricadit TMEG-S, Ricadit TH, Ricadit MH-700, Ricadit MT-500, Ricadit DSDA and Ricadit TDA-100 (both manufactured by New Japan Chemical Co., Ltd.), EPICLON B4400, and EPICLON B570 (both manufactured by Dainippon Ink and Chemicals Co., Ltd.).

[0097] The acid anhydride having an alicyclic skeleton, the water addition product of the acid anhydride, or the modified product of the acid anhydride is preferably an acid anhydride having a polyalicyclic skeleton, the water addition product of the acid anhydride, or the modified product of the acid anhydride, or an acid anhydride having an alicyclic skeleton obtained by the addition reaction of a terpene compound and maleic anhydride, the water addition product of the acid anhydride, or the modified product of the acid anhydride.Specific examples include Ricadit HNA and Ricadit HNA-100 (both manufactured by New Japan Chemical Co., Ltd.), and Epicure YH306 and Epicure YH309 (both manufactured by Mitsubishi Chemical Corporation).

[0098] The curing agent is preferably contained in an amount of 0 to 70% by mass, particularly 0 to 55% by mass, based on 100% by mass of the composition of the present invention excluding the solvent and inorganic filler. If the content of the curing agent is equal to or more than the lower limit, sufficient curing performance can be obtained, and if it is equal to or less than the upper limit, the reaction proceeds effectively, the crosslinking density can be improved, the strength can be increased, and the film formability can be improved.

[0099] <Curing catalyst> The composition of the present invention preferably contains a curing catalyst together with the above curing agent in order to adjust the curing rate and the physical properties of the cured product. The curing catalyst is not particularly limited, but is appropriately selected depending on the type of thermosetting resin component and curing agent used. Specific examples of the curing catalyst include linear or cyclic tertiary amines, organic phosphorus compounds, quaternary phosphonium salts, diazabicycloalkenes such as organic acid salts, and the like. It is also possible to use organometallic compounds, quaternary ammonium salts, metal halides, etc. Examples of the organometallic compounds include zinc octoate, tin octoate, and aluminum acetylacetone complex.

[0100] These may be used alone or in combination of two or more. The curing catalyst is preferably contained in an amount of 0.1 to 10 mass%, particularly preferably 0.1 to 5 mass%, based on 100 mass% of the composition of the present invention excluding the solvent and inorganic filler. When the content of the curing catalyst is equal to or more than the lower limit, the progress of the curing reaction can be sufficiently promoted to achieve good curing, whereas when the content is equal to or less than the upper limit, the curing speed is not too fast, and therefore the storage stability of the composition of the present invention can be improved.

[0101] <Other ingredients> The composition of the present invention may contain other components other than the inorganic filler as long as the effects of the present invention are not impaired. Examples of other components include a surface treatment agent such as a silane coupling agent that improves the interfacial adhesive strength between the inorganic filler and the resin component when a resin cured product is produced using the composition of the present invention, an insulating carbon component such as a reducing agent, a viscosity adjuster, a dispersant, a thixotropy imparting agent, a flame retardant, a colorant, an organic filler, an organic solvent, and a thermoplastic resin.

[0102] Among these, the inclusion of a dispersant may enable the formation of a uniform resin cured product, and may improve the thermal conductivity and dielectric breakdown characteristics of the resulting resin cured product. Also, the inclusion of an organic filler or a thermoplastic resin may impart appropriate elongation to the composition, relieve the stress generated, and suppress the occurrence of cracks during a temperature cycle test.

[0103] The dispersant preferably has a functional group containing hydrogen atoms having hydrogen bonding properties. By the dispersant having a functional group containing hydrogen atoms having hydrogen bonding properties, the thermal conductivity and dielectric breakdown properties of the heat dissipation sheet, which is the cured product obtained, can be further improved. Examples of the functional group containing hydrogen atoms having hydrogen bonding properties include a carboxyl group (pKa=4), a phosphate group (pKa=7), or a phenol group (pKa=10).

[0104] The pKa of the functional group containing a hydrogen atom having hydrogen bonding ability is preferably in the range of 2 to 10, more preferably in the range of 3 to 9. When the pKa is 2 or more, the acidity of the dispersant is in an appropriate range, and the reaction of the epoxy resin in the thermosetting resin component may be easily suppressed. Therefore, when the molded product in an uncured state is stored, the storage stability tends to be improved. When the pKa is 10 or less, the function as a dispersant is sufficiently performed, and the thermal conductivity and dielectric breakdown characteristics of the heat dissipation sheet, which is the obtained cured product, tend to be sufficiently improved.

[0105] The functional group containing a hydrogen atom capable of forming a hydrogen bond is preferably a carboxyl group or a phosphate group, which can further improve the thermal conductivity and dielectric breakdown characteristics of the heat dissipation sheet. Specific examples of the dispersant include polyester-based carboxylic acid, polyether-based carboxylic acid, polyacrylic-based carboxylic acid, aliphatic carboxylic acid, polysiloxane-based carboxylic acid, polyester-based phosphoric acid, polyether-based phosphoric acid, polyacrylic-based phosphoric acid, aliphatic phosphoric acid, polysiloxane-based phosphoric acid, polyester-based phenol, polyether-based phenol, polyacrylic-based phenol, polysiloxane-based phenol, etc. Only one type of dispersant may be used, or two or more types may be used in combination.

[0106] As the thermoplastic resin, any generally known thermoplastic resin can be used, and specific examples thereof include vinyl polymers such as polyethylene, polypropylene, polystyrene, polyvinyl chloride, (meth)acrylic resin, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, etc., polylactic acid resin, polyethylene terephthalate, polybutylene terephthalate, etc., polyamides such as nylon and polyamidoamine, polyvinyl acetal resins such as polyvinyl acetoacetal, polyvinyl benzal, polyvinyl butyral resin, ionomer resin, polyphenylene ether, polyphenylene sulfide, polycarbonate, polyether ether ketone, polyacetal, ABS resin, LCP (liquid crystal polymer), fluororesin, urethane resin, silicone resin, various elastomers, and modified products of these resins.

[0107] These thermoplastic resins may be uniform in the resin phase of the heat dissipation sheet, or may be phase-separated and have a recognizable shape. If the thermoplastic resin is phase-separated, the shape of the thermoplastic resin in the heat dissipation sheet may be particulate or fibrous. In this way, if the shape of the thermoplastic resin is recognizable in the heat dissipation sheet, the thermoplastic resin may be recognized as an organic filler, but in the present invention, the organic filler refers to natural products such as wood flour, cellulose that may be modified, starch, various organic pigments, etc., and the thermoplastic resin is not included in the organic filler.

[0108] The inclusion of a thermoplastic resin or an organic filler may impart appropriate elongation to the composition, reduce the stress that occurs, and suppress the occurrence of cracks during a temperature cycle test. When the thermoplastic resin or organic filler is insoluble in the thermosetting resin, the viscosity of the composition of the present invention is prevented from increasing, and when the composition is molded into a sheet as described below, the smoothness of the sheet surface can be improved. In this case, by simultaneously mixing a thermoplastic resin and an organic filler that are insoluble in the thermosetting resin with a large amount of inorganic filler, the component phase that is thermoplastic and has good elongation can be efficiently dispersed in the cured product, and stress can be easily relaxed. Therefore, it is possible to suppress the occurrence of cracks in the cured product without lowering the elastic modulus of the cured product. For these reasons, polyamide resins such as nylon, cellulose resins, etc. are preferred as the thermoplastic resin, and polyamide resins such as nylon are particularly preferred.

[0109] When the shape of the thermoplastic resin that can be observed in the heat dissipation sheet that is the cured product is particulate, the upper limit of the average particle size is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less. By making the average particle size equal to or less than the above upper limit, it is possible to prepare sheet-shaped cured products of various thicknesses without the risk of a decrease in thermal conductivity. The average particle size of the particulate thermoplastic resin is determined by observing the cross section of the cured product and averaging the longest diameter of any 20 particles.

[0110] The composition of the present invention may contain an organic solvent, for example, in order to improve the coatability when the composition is subjected to a coating step to form a sheet-like cured product. Examples of organic solvents that may be contained in the composition of the present invention include methyl ethyl ketone, cyclohexanone, propylene glycol monomethyl ether acetate, butyl acetate, isobutyl acetate, propylene glycol monomethyl ether, etc. These organic solvents may be used alone or in combination of two or more.

[0111] When the composition of the present invention contains an organic solvent, the content is appropriately determined depending on the handleability during the production of the heat dissipation sheet, etc. Usually, the organic solvent is preferably used so that the solid content (total of components other than the solvent) in the composition of the present invention is 10 to 90 mass%, particularly 40 to 80 mass%.

[0112] [Inorganic filler] The composition of the present invention contains at least the BN agglomerated powder of the present invention as an inorganic filler. The composition of the present invention may contain an inorganic filler other than the BN agglomerated powder of the present invention. In this case, a preferred example of the inorganic filler other than the BN agglomerated powder of the present invention is a spherical filler.

[0113] The spherical filler used together with the BN agglomerated powder of the present invention preferably has a thermal conductivity of 10 W / m·K or more, more preferably 15 W / m·K or more, and even more preferably 20 W / m·K or more. The new Mohs hardness is preferably 3.1 or more, and more preferably 5 or more. In particular, it is preferable for the thermal conductivity to be 20 to 30 W / m·K and the new Mohs hardness to be 5 to 10. By using such a spherical filler together with the BN agglomerated powder of the present invention, it is possible to increase the adhesive strength to metal and the heat dissipation properties of the obtained heat dissipation sheet.

[0114] Here, "spherical" refers to anything that is generally recognized as being spherical, and for example, an average circularity of 0.4 or more may be considered spherical, and an average circularity of 0.6 or more may be considered spherical. Usually, the upper limit of the average circularity is 1. The circularity can be measured by subjecting the projected image to image processing, and can be measured, for example, with Sysmex Corporation's FPIA series. The spherical filler is preferably at least one selected from the group consisting of alumina, synthetic magnesite, crystalline silica, aluminum nitride, silicon nitride, silicon carbide, zinc oxide, and magnesium oxide. By using these preferred spherical fillers, the heat dissipation properties of the obtained heat dissipation sheet can be further improved.

[0115] The average particle size of the spherical filler is preferably in the range of 0.5 μm or more and 40 μm or less. It is believed that an average particle size of 0.5 μm or more allows the resin and filler to flow easily during heat molding, thereby increasing the interfacial adhesive strength of the heat dissipation sheet. In addition, an average particle size of 40 μm or less makes it easier to maintain the dielectric breakdown characteristics of the heat dissipation sheet.

[0116] As other inorganic fillers, electrically insulating ones can be used, and at least one kind of particles selected from the group consisting of carbon, metal carbide, metal oxide and metal nitride can be used. Examples of carbon include diamond. Examples of metal carbides include silicon carbide, titanium carbide, tungsten carbide, etc. Examples of metal oxides include magnesium oxide, aluminum oxide, silicon oxide, calcium oxide, zinc oxide, yttrium oxide, zirconium oxide, cerium oxide, ytterbium oxide, sialon (ceramics consisting of silicon, aluminum, oxygen and nitrogen), etc. Examples of metal nitrides include boron nitride, aluminum nitride, silicon nitride, etc. other than the BN agglomerated particles of the present invention.

[0117] The shape of the other inorganic fillers is not limited, and may be particles, whiskers, fibers, plates, or aggregates thereof. These inorganic fillers may be surface-treated with a surface treatment agent. As the surface treatment agent, a known surface treatment agent can be used. These inorganic fillers may be used alone or in any combination and ratio of two or more kinds.

[0118] The content of the inorganic filler in the composition of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, based on 100% by mass of the composition of the present invention excluding the solvent, and is preferably 99% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. By making the content of the inorganic filler equal to or more than the lower limit, the effect of improving thermal conductivity and the effect of controlling the linear expansion coefficient due to the inclusion of the inorganic filler can be sufficiently obtained, while by making the content equal to or less than the upper limit, the moldability of the cured product and the interfacial adhesion in the composite molded product described below tend to be obtained.

[0119] When the BN agglomerated powder of the present invention and a spherical filler such as alumina are used in combination as the inorganic filler, the content ratio of the BN agglomerated powder of the present invention to the spherical filler in the composition of the present invention is not particularly limited, but is preferably 90:10 to 10:90 in mass ratio, and more preferably 80:20 to 20:80. In order to effectively obtain the effects of using the BN agglomerated powder of the present invention, it is preferable that 30 mass % or more, particularly 40 mass % or more of the inorganic filler used is the BN agglomerated powder of the present invention, and in the present invention, it is preferable to use only the BN agglomerated powder of the present invention or only the BN agglomerated powder of the present invention and the above-mentioned spherical filler as the inorganic filler.

[0120] <Method of producing the composition of the present invention> The composition of the present invention can be obtained by uniformly mixing the inorganic filler containing the BN agglomerated powder of the present invention, a resin component such as a thermosetting resin, and other components added as necessary by stirring or kneading. For mixing, a general kneading device such as a mixer, a kneader, or a single-screw or twin-screw kneader can be used, and heating may be performed as necessary during mixing.

[0121] The order of mixing the various components may be arbitrary as long as there are no particular problems, such as the generation of reactions or precipitation. For example, a method may be used in which a thermosetting resin component is mixed and dissolved in an organic solvent (e.g., methyl ethyl ketone) to prepare a resin liquid, and a thoroughly mixed inorganic filler and other components are added to and mixed with the obtained resin liquid, and then an organic solvent is further added to adjust the viscosity and mixed, and then additives such as a curing agent, a curing accelerator, or a dispersing agent are further added and mixed.

[0122] [Heat dissipation sheet] A method for producing the heat dissipation sheet of the present invention as a sheet-like cured product using the composition of the present invention will be described below. The sheet-shaped cured product can be produced by a commonly used method, for example, by forming the composition of the present invention into a sheet and curing it.

[0123] The composition of the present invention can be formed into a sheet by any commonly used method. For example, when the composition of the present invention has plasticity and flowability, the composition can be molded into a desired shape, for example, by curing the composition while it is contained in a mold. In this case, injection molding, injection compression molding, extrusion molding, compression molding, and vacuum compression molding can be used.

[0124] The solvent in the composition of the present invention can be removed by a known heating method such as a hot plate, a hot air oven, an IR heating oven, a vacuum dryer, or a high-frequency heater. Alternatively, a sheet-like cured product can be obtained by cutting the cured product of the composition of the present invention into a desired shape. A sheet-like cured product can also be obtained by forming a slurry of the composition of the present invention (hereinafter sometimes referred to as "slurry for sheet") into a sheet by a doctor blade method, a solvent casting method, an extrusion film formation method, or the like. An example of a method for producing a sheet-like cured product using this sheet slurry will be described below.

[0125] <Coating process> First, a coating film is formed on the surface of a substrate using a sheet slurry. That is, the sheet slurry is used to form a coating film on a substrate by a dip method, a spin coat method, a spray coat method, a blade method, or any other method. A coating device such as a spin coater, a slit coater, a die coater, or a blade coater can be used to apply the sheet slurry, and this makes it possible to uniformly form a coating film of a predetermined thickness on the substrate. As the substrate, copper foil or polyethylene terephthalate (PET) film, which will be described later, is generally used, but there is no limitation thereto.

[0126] <Drying process> The coating film formed by applying the sheet slurry is dried usually at a temperature of 10 to 150°C, preferably 25 to 120°C, and more preferably 30 to 110°C to remove the solvent and low molecular weight components. By keeping the drying temperature at or below the upper limit, the curing of the thermosetting resin in the slurry is suppressed, and the resin flows in the subsequent pressing process, which tends to make it easier to remove voids. By keeping the drying temperature at or above the lower limit, the solvent can be effectively removed. The drying time is usually 5 minutes to 10 days, preferably 10 minutes to 3 days, more preferably 20 minutes to 1 day, and particularly preferably 30 minutes to 4 hours. When the drying time is equal to or more than the lower limit, the solvent can be sufficiently removed, and the residual solvent tends to be prevented from forming voids in the sheet-shaped cured product. When the drying time is equal to or less than the upper limit, the productivity tends to be improved, and the production cost tends to be reduced.

[0127] <Pressing process> After the drying process, it is desirable to carry out a pressurizing process for the purpose of bonding inorganic fillers together to form a heat path, eliminating voids and gaps in the sheet, and improving adhesion to the substrate. The pressurizing process is carried out by applying a pressure of 10 kgf / cm to the dried film on the substrate. 2 It is desirable to carry out the test with a load of 20 kgf / cm or more. 2 More preferably, it is 50 kgf / cm 2 More preferably, it is 2000 kgf / cm 2 More preferably, it is 1000 kgf / cm or less. 2 , and more preferably 800 kgf / cm 2By setting the load during pressing to the above upper limit or less, the secondary particles of the inorganic filler are not destroyed, and a sheet having high thermal conductivity without voids in the sheet can be obtained. Also, by setting the load to the above lower limit or more, contact between the inorganic fillers is improved, making it easier to form a thermal conduction path, and a sheet having high thermal conductivity can be obtained.

[0128] In the pressurizing step, it is desirable to heat the dried film on the substrate at 25°C or higher. The heating temperature is preferably 40°C or higher, more preferably 50°C or higher, and even more preferably 60°C or higher. It is also desirable to heat at 300°C or lower, preferably 250°C or lower, more preferably 200°C or lower, and even more preferably 180°C or lower. By carrying out the pressurizing step within this temperature range, the melt viscosity of the resin in the coating film can be reduced, and voids and gaps in the sheet can be eliminated. If the temperature is below the upper limit of this temperature range, there is a risk that the organic components will decompose or the residual solvent will become vapor and form voids.

[0129] The time of the pressurizing step is usually 30 seconds or more, preferably 1 minute or more, more preferably 3 minutes or more, and even more preferably 5 minutes or more. It is also preferably 4 hours or less, more preferably 2 hours or less, even more preferably 1 hour or less, and particularly preferably 45 minutes or less. By keeping the pressurizing time below the upper limit, the production time of the sheet-shaped cured product can be suppressed, and the production cost tends to be reduced. On the other hand, by keeping the pressurizing time above the lower limit, the gaps and voids in the sheet-shaped cured product can be sufficiently removed, and the heat transfer performance and the voltage resistance characteristics tend to be improved.

[0130] <Curing process> The curing step for completely carrying out the curing reaction may be carried out under pressure or without pressure, but when pressure is applied, it is preferable to carry out the same conditions as the above-mentioned pressurizing step for the same reasons as above. Note that the pressurizing step and the curing step may be carried out simultaneously. In particular, in the sheet forming process which involves a pressing step and a hardening step, it is preferable to apply a load within the above range and carry out the pressing and hardening.

[0131] The thickness of the heat dissipation sheet of the present invention, which is the sheet-shaped cured product thus formed, is not particularly limited, but is preferably 50 μm or more, more preferably 100 μm or more. Also, it is preferably 400 μm or less, more preferably 300 μm or less. When the thickness of the heat dissipation sheet is equal to or greater than the above lower limit, voltage resistance characteristics are obtained and the breakdown voltage tends to improve. Also, when the thickness is equal to or less than the above upper limit, the device can be made smaller and thinner, and the thermal resistance of the obtained heat dissipation sheet tends to be suppressed.

[0132] [Composite molded body] The heat dissipation sheet of the present invention can be used as a composite molded body in which the heat dissipation sheet of the present invention and a metal part are laminated together. In this case, the metal part may be provided on only one surface of the heat dissipation sheet of the present invention, or on two or more surfaces. For example, the heat dissipation sheet of the present invention may have a metal part on only one surface, or may have a metal part on both surfaces. The metal part may also be patterned.

[0133] Such a composite molded product can be produced by using a metal part as the substrate and forming a sheet-like product made of the composition of the present invention on the substrate according to the above-mentioned method. Alternatively, the composite molded product can be produced by peeling a sheet-like product formed on a substrate other than the metal part from the substrate, and then heat-pressing the sheet-like product onto a metal member that will become the metal part. In this case, a sheet-like material made from the composition of the present invention is formed in the same manner as described above, except that it is applied to a substrate such as a PET film which may be treated with a release agent, and then the sheet-like material is peeled off from the substrate and placed on another metal plate, or sandwiched between two metal plates, and pressed to be integrated.

[0134] In this case, as the metal plate, a metal plate having a thickness of about 10 to 10,000 μm made of copper, aluminum, nickel-plated metal, or the like can be used. The surface of the metal plate may be physically roughened or chemically treated with a surface treatment agent or the like. From the viewpoint of adhesion between the resin composition and the metal plate, it is more preferable that these treatments are performed.

[0135] [Semiconductor device module] The semiconductor device module of the present invention is one in which the heat dissipation sheet of the present invention is mounted as a heat dissipation substrate. Due to its high heat conduction and heat dissipation effect and withstand voltage characteristics, high output and high density can be achieved with high reliability. In the semiconductor device module, members such as aluminum wiring, encapsulant, package material, heat sink, thermal paste, and solder other than the heat dissipation sheet of the present invention can be appropriately adopted from conventionally known members.

Examples

[0136] Hereinafter, the present invention will be described in more detail with reference to examples. However, the present invention is not limited to the following examples unless it exceeds the gist thereof. Note that the various conditions and values of the evaluation results in the following examples indicate the preferable ranges in the embodiments of the present invention. The preferable range of the present invention can be determined in consideration of the preferable ranges in the above-described embodiments and the ranges indicated by the values in the following examples or combinations of the values of the examples.

[0137] [Measurement conditions] The various characteristics and physical properties in the following examples and comparative examples were measured by the methods described below.

[0138] <Compressive strength of BN agglomerated particles> Using a Shimadzu micro compression tester MCT-510 manufactured by Shimadzu Corporation, tests were conducted with a test force, loading rate, and upper pressing plunger corresponding to the BN agglomerated particle diameter. One particle corresponding to the average particle diameter of the BN agglomerated particles was selected for the test, and this was carried out 5 times or more. The average value of the compressive strength was obtained by dividing the total value of the compressive strength of the particles for which the test was conducted by the number of test times.

[0139] Cs = 2.48P / πd 2 Cs: Compressive strength (MPa), P: Test force (N), d: Particle diameter (mm)

[0140] <Average elastic modulus of BN agglomerated powder> The elastic modulus of BN agglomerated particles was calculated using the following formula from the test force, compression displacement, and particle diameter obtained in the particle compression test. The average elastic modulus is the average value of the elastic modulus, and it is preferably the average value obtained from 5 or more BN agglomerated particles.

[0141] E = 3×(1 - ν 2 )×P / (4×(d / 2) 1 / 2 ×δ 3 / 2 ) E: Elastic modulus (MPa) ν: Poisson's ratio (Poisson's ratio was set to 0.13) (-) P: Test force (N) d: Particle diameter (mm) δ: Compression displacement (mm)

[0142] <Internal pore volume, internal pore area, and interparticle void volume of BN agglomerated powder> The internal pore volume, internal pore area, and interparticle void volume were measured in accordance with JIS R1655:2003 "Test Method for Pore Size Distribution of Fine Ceramics by Mercury Intrusion Porosimetry". Specifically, as a mercury porosimeter, AutoPore IV manufactured by Micromeritics was used. 200 mg of the sample was filled into the measurement cell, and after degassing treatment under reduced pressure (50 μmHg or less) for 10 minutes, the total pore volume was determined, and the mercury intrusion / extrusion curve was measured. A pore size distribution curve with the pore diameter on the horizontal axis and the logarithmically differentiated pore volume on the vertical axis was created. Assuming the pores are cylindrical, the diameter (division diameter) at which the logarithmically differentiated pore volume takes a minimum value with respect to the pore diameter between peak a representing the internal pores of the particles and peak b representing the interparticle pores was read. The interparticle void volume (ml / g) was determined from the integrated value of the mercury intrusion / extrusion curve in the region where the pore diameter is larger than the division diameter.

[0143] Further, the intraparticle pore volume was calculated by subtracting the interparticle void volume from the total pore volume. Furthermore, assuming the pores to be cylinders, the pore side areas calculated from the pore volume for each pore diameter were integrated, and the integral value in the region where the pore diameter was smaller than the above-mentioned divided diameter was calculated as the intraparticle pore area.

[0144] <Dielectric breakdown voltage (BDV) measurement> The sheets obtained in the examples and comparative examples were placed on a copper plate with a thickness of 2 mm and temporarily adhered to the copper plate under the pressing conditions of 20 kgf / cm 2 , 80 °C, and 5 minutes. Thereafter, a sheet-shaped molded body was obtained by thermally curing the sheet under the pressing conditions of 100 kgf / cm 2 , 175 °C, and 40 minutes. The withstand voltage of the molded body was measured in fluorinate using cylindrical electrodes. The withstand voltage characteristics were obtained by increasing the voltage by 500 V every minute, and the characteristic value was taken when a current of 10 mA or more flowed through the molded body.

[0145] [Production of BN agglomerated powder from BN slurry] The BN agglomerated powder used in the following examples and comparative examples was produced by the following method.

[0146] <Preparation of BN slurry> <Examples 1 to 5> Raw material h-BN powder (the half-value width of the (002) plane peak obtained by powder X-ray diffraction measurement is 2θ = 0.67°, total oxygen concentration = 7.5 mass%, specific surface area 116 m 2 / g, total pore volume 0.754 cm 3 / g): 10000 g Binder (「Taxelam M160L」manufactured by Takaki Chemical Co., Ltd., solid content concentration 21 mass%): 11496 g Surfactant (surfactant 「Ammonium lauryl sulfate」manufactured by Kao Corporation, solid content concentration 14 mass%): 250 g

[0147] <Examples 6 to 7> Raw material h-BN powder (the half-value width of the (002) plane peak obtained by powder X-ray diffraction measurement is 2θ = 0.67°, total oxygen concentration = 7.5 mass%, specific surface area 116 m 2 / g, total pore volume 0.754 cm3 / g): 10,000 g Binder 1 (Takiseram M160L manufactured by Taki Chemical Co., Ltd., solid content concentration 21% by mass): 2,292 g Binder 2 (Polyvinylpyrrolidone K-30 manufactured by Nippon Shokubai Co., Ltd.): 100 g Surfactant (Ammonium lauryl sulfate, surfactant manufactured by Kao Corporation, solid content concentration 14% by mass): 250 g

[0148] <Comparative Examples 1 to 8> Raw material h-BN powder (half-value width of the (002) plane peak obtained by powder X-ray diffraction measurement is 2θ = 0.67°, total oxygen concentration = 7.5% by mass, specific surface area 116 m 2 / g, total pore volume 0.754 cm3 / g): 10,000 g Binder 2 (Polyvinylpyrrolidone K-30 manufactured by Nippon Shokubai Co., Ltd.): 100 g Surfactant (Ammonium lauryl sulfate, surfactant manufactured by Kao Corporation, solid content concentration 14% by mass): 250 g

[0149] (Preparation of slurry) A predetermined amount of the raw material h-BN powder was weighed into a resin bottle, and then a predetermined amount of the binder was added. Further, after adding a predetermined amount of the surfactant, zirconia ceramic balls were added and stirred on a pot mill turntable for 1 hour to prepare a slurry.

[0150] (Granulation) Granulation from the BN slurry was carried out using a spray dryer P260 manufactured by Pulice Co., Ltd. at a disk rotation speed of 15,000 to 20,000 rpm and a drying temperature of 85°C.

[0151] (Preparation of BN agglomerated powder) After pre-firing the above BN granulated powder (700°C, 5 h), the powder after pre-firing was heat-treated at 1,400°C to 2,000°C under a nitrogen flow.

[0152] The BN agglomerated powder used in Examples 1 to 5 was prepared by the following procedure. The powder after the calcination was filled in a circular graphite crucible with a lid in a disk shape so that the packed bed height was 10 mm, and the inside of the furnace was replaced with nitrogen gas at normal pressure at room temperature. The temperature was raised to 700°C in 3 hours while passing nitrogen gas, and then the temperature was raised to the desired temperature (1st holding temperature) at a heating rate of 125°C / hour and held for 15 hours, and then the temperature was raised to 1950°C at the same heating rate and held for 5 hours. Then, it was cooled to room temperature. The part that had been in contact with the graphite was removed from the sintered material taken out of the crucible, and crushed manually using a mortar and pestle, and then processed with a roll mill to obtain spherical boron nitride agglomerated particles having a card house structure. The obtained boron nitride agglomerated particles were sieved using a sieve with an opening of 90 μm, and only the particles that passed through the sieve were used as the thermally conductive filler.

[0153] When re-firing, 30 g of the powder after the first firing was filled into a new BN crucible (φ60 mm with lid) listed in Table 1, and then placed inside the BN inner crucible. The BN inner crucible was set in an atmospheric firing furnace and heated to 2000°C at a heating rate of 1200°C / hr under N2 flow. Then, heat treatment was performed at 2000°C (re-firing temperature) for 2 hours. After natural cooling, the sample was collected.

[0154] The BN agglomerated powder used in Examples 6 and 7 was prepared by the following procedure. The powder after the calcination was filled in a circular graphite crucible with a lid in a disk shape so that the packed bed height was 10 mm, and the inside of the furnace was replaced with nitrogen gas at normal pressure at room temperature. The temperature was raised to 700°C in 3 hours while passing nitrogen gas, and then the temperature was raised to the desired temperature (1st holding temperature) at a heating rate of 125°C / hour and held for 15 hours, and then the temperature was raised to 1700°C at the same heating rate and held for 5 hours. Then, it was cooled to room temperature. The part that had been in contact with the graphite was removed from the sintered material taken out of the crucible, and crushed manually using a mortar and pestle, and then processed with a roll mill to obtain spherical boron nitride agglomerated particles having a card house structure. The obtained boron nitride agglomerated particles were sieved using a sieve with an opening of 90 μm, and only the particles that passed through the sieve were used as the thermally conductive filler.

[0155] When re-firing was performed, the re-firing was performed in accordance with the methods of Examples 1 to 5, except that the heat treatment temperature (re-firing temperature) was changed to 1800°C.

[0156] The BN agglomerated powders used in Comparative Examples 1 to 4 were prepared by the following procedure. The powder after the calcination was filled in a circular graphite crucible with a lid in a disk shape so that the packed bed height was 10 mm, and the inside of the furnace was replaced with nitrogen gas at normal pressure at room temperature. The temperature was raised to 700°C in 3 hours while passing nitrogen gas, and then the temperature was raised to the desired temperature (1st holding temperature) at a heating rate of 125°C / hour and held for 15 hours, and then the temperature was raised to 1700°C at the same heating rate and held for 5 hours. Then, it was cooled to room temperature. The part that had been in contact with the graphite was removed from the sintered material taken out of the crucible, and crushed manually using a mortar and pestle, and then processed with a roll mill to obtain spherical boron nitride agglomerated particles having a card house structure. The obtained boron nitride agglomerated particles were sieved using a sieve with an opening of 90 μm, and only the particles that passed through the sieve were used as the thermally conductive filler.

[0157] When re-firing was performed, the re-firing was performed in accordance with the methods of Examples 1 to 5, except that the heat treatment temperature (re-firing temperature) was changed to 1700°C.

[0158] The BN agglomerated powders used in Comparative Examples 5 to 8 were prepared by the following procedure. The powder after calcination was filled in a crucible with a circular graphite lid in a disk shape so that the packed bed height was 10 mm. The inside of the furnace was purged with nitrogen gas at room temperature and normal pressure while flowing nitrogen gas. After heating up to 700 °C in 3 hours while flowing nitrogen gas, it was heated up to the desired temperature (1st holding temperature) at a heating rate of 125 °C / hour and held for 15 hours. Then, it was heated up to the desired temperature (2nd holding temperature) at the same heating rate and held for 1 hour. Further, it was heated up to 1700 °C at the same heating rate and held for 5 hours. Thereafter, it was cooled to room temperature. The part in contact with graphite was removed from the fired product taken out from the crucible, and it was manually crushed using a mortar and a pestle, and then processed with a roll mill to obtain spherical boron nitride aggregated particles having a card house structure. The obtained boron nitride aggregated particles were sieved using a sieve with an opening of 90 μm, and only the particles passing through the sieve were used as the thermal conductivity filler.

[0159] When performing re-firing, re-firing was carried out in accordance with the methods of Examples 1 to 5 except that the heat treatment temperature (re-firing temperature) was changed to 1700 °C.

[0160] The production conditions of the BN aggregated powder are summarized in Table 1. Note that all of the BN aggregated powders were confirmed by SEM observation to be aggregates of BN aggregated particles having a card house structure.

[0161] [Table 1]

[0162] [Production and Evaluation of Sheet-shaped Moldings (Heat Dissipation Sheets)] In the following Examples and Comparative Examples, the BN aggregated powder obtained above was used as an inorganic filler, respectively, and a resin composition containing BN aggregated powder was prepared by the following method, and a sheet-shaped molding was produced.

[0163] [Preparation of Resin Composition Containing BN Aggregated Powder] The raw materials used were as follows.

[0164] (Thermosetting Resin Component) Resin component 1: A resin having the structure (2) (R 3 = Structure (4)) and Structure (3) (R 4 ,R 5 ,R 6 ,R 7 (=methyl group) Weight average molecular weight in polystyrene equivalent: 30,000 Epoxy equivalent: 9,000g / equivalent Resin component 2: Bisphenol A type liquid epoxy resin manufactured by Mitsubishi Chemical Corporation Resin component 3: Nagase ChemteX Corporation Multifunctional epoxy resin containing a structure having four or more glycidyl groups per molecule

[0165] (Inorganic filler component) Inorganic filler 1: BN agglomerated powder obtained in each example Inorganic filler 2: Spherical alumina particles manufactured by Admatechs New Mohs hardness: 9 Volume average particle size: 6.5 μm Thermal conductivity: 20~30W / m K

[0166] <Hardening agent component> Hardener 1: Meiwa Chemical Industries, Ltd. "MEH-8000H" Phenol Resin Hardener

[0167] <Curing catalyst component> Curing catalyst 1: Shikoku Kasei "2E4MZ-A" 2,4-Diamino-6-[2'-ethyl-4'-methylimidazolyl-(17')]-ethyl-s-triazine (having both imidazole-derived and triazine-derived structures in one molecule) Molecular weight: 247, Properties: Solid, Melting point: 215-225℃ Curing catalyst 2: Shikoku Kasei "2PHZ-PW" 2-Phenyl-4,5-dihydroxymethylimidazole Molecular weight: 204, Properties: Solid, Melting point: Dec.230, so the melting point is 230℃ or higher

[0168] <Example 8> Using a planetary stirring device, a mixture was prepared so that the resin component 1 was 6.3% by mass, the resin component 2 was 10.2% by mass, the resin component 3 was 5.1% by mass, the curing agent 1 was 3.5% by mass, the curing catalyst 1 was 0.25% by mass, the curing catalyst 2 was 0.25% by mass, the inorganic filler 1 was 54.1% by mass, and the inorganic filler 2 was 20.3% by mass. In addition, when preparing the mixture, 18.6% by mass of methyl ethyl ketone and cyclohexanone were used so that the mixture was 62.8% by mass (solid concentration) of the coating slurry.

[0169] The obtained coating slurry (slurry for sheets) was applied to a PET substrate by the doctor blade method, and then heated and dried at 60°C for 120 minutes. After that, the coating slurry was heated and dried at 42°C and 1500 kgf / cm 2 The mixture was pressed at 400° C. for 10 minutes to obtain a sheet-like molded product having a thickness of 150 μm. The total content of methyl ethyl ketone and cyclohexanone in the sheet-like molded product was 1% by mass or less. The intraparticle pore volume, intraparticle pore area, and average elastic modulus of the BN agglomerated powder used are shown in Table 2. Table 2 also shows the dielectric breakdown voltage of the sheet-like molded article obtained using the BN agglomerated powder.

[0170] <Examples 9 to 14 and Comparative Examples 13 to 16> The evaluation results of sheet-like molded articles produced in accordance with the method of Example 8, except that the BN agglomerated powder was changed, are shown in Table 2.

[0171] <Comparative Examples 9 to 12> Table 2 shows the evaluation results of a sheet-like molded product produced in accordance with the method of Example 8, except that the solid content concentrations in the BN agglomerated powder and the coating slurry were changed to the following values. Comparative example 9: 60.8% by mass Comparative example 10: 60% by mass Comparative example 11: 60% by mass Comparative example 12: 60% by mass

[0172] [Table 2]

[0173] From Table 2, it can be seen that when the BN agglomerated powder of the present invention is used, high breakdown voltage is obtained, and therefore high voltage resistance characteristics can be obtained. Therefore, by using a BN agglomerated powder with specific ranges of intraparticle pore volume, intraparticle pore area, and average elastic modulus, a heat dissipation sheet with excellent voltage resistance characteristics can be realized.

Claims

1. A boron nitride agglomerated powder that satisfies the following conditions a), b), and c). a): Intraparticle pore volume measured by mercury intrusion porosimetry is greater than 0.35 ml / g and less than 0.50 ml / g b): The pore area within the particle measured by mercury intrusion porosimetry is 3 m 2 / g or more, 6.5m 2 / g or less c): Average elastic modulus measured by single particle compression test is greater than 70 MPa and less than 150 MPa

2. 10. The boron nitride agglomerated powder of claim 1 comprising boron nitride agglomerated particles having a house of cards structure.

3. 3. The boron nitride agglomerated powder according to claim 1, wherein the interparticle void volume measured by mercury intrusion porosimetry is 0.50 ml / g or more and 0.95 ml / g or less.

4. A heat dissipation sheet comprising the boron nitride agglomerated powder according to claim 1 or 2.

5. A semiconductor device module comprising the heat dissipation sheet according to claim 4.

Citation Information

Patent Citations

  • Thermally conductive resin composition, thermally conductive resin sheet, laminated heat-radiation sheet, heat-radiation circuit board, and power semiconductor device

    JP2022149288A

  • Hexagonal boron nitride powder, its manufacturing method, and composition and heat dissipation material using the same

    JP7069485B2