Method for producing lithium sulfide
The method addresses impurity removal in lithium sulfide production by using controlled hydrogen sulfide injections and heat treatments, producing high-purity lithium sulfide suitable for solid electrolytes with enhanced performance and reduced solvent use.
Patent Information
- Application Number
- JP2024044368
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Existing methods for producing lithium sulfide face challenges in effectively removing impurities, particularly carbonate-based impurities, which affect the performance of sulfide-based solid electrolytes, and often require high temperatures that are difficult to implement in commercial processes.
A method involving pretreatment of lithium hydroxide in an inert gas atmosphere, followed by primary and secondary injections of hydrogen sulfide gas, with controlled temperature adjustments and heat treatment, to produce high-purity lithium sulfide without using solvents, minimizing impurities.
The method effectively reduces impurities, especially carbonate-based impurities, resulting in high-purity lithium sulfide suitable for solid electrolytes, with improved performance and reduced process complexity.
Smart Images

Figure 2024152632000002 
Figure 2024152632000001
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority based on Korean Patent Application No. 10-2023-0049611 dated April 14, 2023, and all contents disclosed in the documents of said Korean patent application are incorporated herein by reference. The present invention relates to a method for producing lithium sulfide, more specifically, to a method for producing high purity lithium sulfide by using hydrogen sulfide in a treatment step after the production of lithium sulfide. [Background technology]
[0002] Recently, with the development of the secondary battery industry, the use of solid electrolyte materials is becoming more feasible. Among them, sulfide-based solid electrolytes, which are synthesized using lithium sulfide (Li2S), lithium chloride (LiCl), and phosphorus pentasulfide (P2S5) as raw materials, are considered to have higher ionic conductivity and are stable over a wide voltage range compared to oxide-based solid electrolytes.
[0003] Lithium sulfide, the main raw material of sulfide-based solid electrolytes, is generally produced by reacting a solid lithium precursor with a gaseous sulfur precursor. Conventional research into the production of lithium sulfide has focused on the synthesis method of lithium sulfide, which is related to the selection of lithium sulfide precursors. Since then, in addition to the synthesis of lithium sulfide, research into improving the performance of the produced lithium sulfide has been attracting attention. The improvement of lithium sulfide performance mainly relates to a technology for controlling the produced lithium sulfide particles, and as an example, a technology for controlling the particle size of lithium sulfide or the specific surface area of lithium sulfide (JP2019-156691A) has been presented.
[0004] Meanwhile, in terms of the performance of the solid electrolyte, impurities contained in lithium sulfide may adversely affect the performance of the solid electrolyte. Therefore, in addition to technology for controlling lithium sulfide particles themselves, some research is being conducted to reduce impurities in lithium sulfide. Methods for producing lithium sulfide include a wet process using a solvent and a dry process not using a solvent. In the wet process, the impurity content can be reduced only by effectively removing the solvent after producing lithium sulfide. However, in this case, there is a limit to how effectively the solvent can be removed, and there is a problem in that additional costs are incurred for removing the solvent.
[0005] In addition, lithium hydroxide (LiOH), one of the lithium precursors used in the production of lithium sulfide, generally contains some carbonate impurities. In order to convert the carbonate impurities present in lithium hydroxide to lithium sulfide, a method has been proposed in which lithium hydroxide is heated at a temperature of 1,000°C or higher to convert both into lithium oxide (Li2O) form, and then lithium sulfide is synthesized. However, this requires extremely high temperatures, making it difficult to apply to commercial processes.
[0006] There is a need to study a technology for solving the above problems in the method for producing lithium sulfide and for producing high-purity lithium sulfide. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention relates to a method for producing lithium sulfide, which can effectively remove impurities during the production of lithium sulfide to obtain high-purity lithium sulfide. [Means for solving the problem]
[0008] The present invention provides a method for producing lithium sulfide, comprising: a step (step 1) of pretreating a lithium hydroxide raw material under an inert gas atmosphere; a step (step 2) of primarily introducing hydrogen sulfide gas to cause a dry reaction between the pretreated lithium hydroxide raw material and hydrogen sulfide; a step (step 3) of heating the reaction product under an inert gas atmosphere after completion of the reaction in step 2; and a step (step 4) of secondly introducing hydrogen sulfide gas to perform a heat treatment. The present invention also provides lithium sulfide produced by the production method of the present invention. Effect of the Invention
[0009] The method for producing lithium sulfide according to the present invention can produce high-purity lithium sulfide by minimizing impurities in lithium sulfide. More specifically, it can produce lithium sulfide having excellent performance as a raw material for a solid electrolyte by minimizing carbonate-based impurities in the produced lithium sulfide. [Brief description of the drawings]
[0010] [Figure 1] 1 is a graph showing the results of X-ray diffraction (XRD) analysis of lithium sulfide prepared according to an embodiment and commercial lithium sulfide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In the present invention, the terms "first", "second", etc. are used to describe various components, and the terms are used only for the purpose of distinguishing one component from another component. Furthermore, the terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, terms such as "comprise", "comprise", or "have" are intended to describe implemented features, numbers, steps, components, or combinations thereof, but do not exclude the possibility of one or more other features, numbers, steps, components, combinations or additions thereof. Additionally, in this specification, when a layer or element is referred to as being "on" or "on top of" another layer or element, this means that the layer or element is formed directly on the layer or element, or that other layers or elements can be additionally formed between layers, on the object, or on the substrate. Since the present invention can be modified in various ways and can have various forms, specific embodiments are exemplified and described in detail below, but it should be understood that the present invention is not limited to the specific disclosed forms, and includes all modifications, equivalents, or alternatives within the spirit and technical scope of the present invention.
[0012] The present invention will be described in detail below.
[0013] The present invention provides a method for producing lithium sulfide, comprising: a step (step 1) of pretreating a lithium hydroxide raw material under an inert gas atmosphere; a step (step 2) of primarily introducing hydrogen sulfide gas to cause a dry reaction between the pretreated lithium hydroxide raw material and hydrogen sulfide; a step (step 3) of heating the reaction product under an inert gas atmosphere after completion of the reaction in step 2; and a step (step 4) of secondly introducing hydrogen sulfide gas to perform a heat treatment.
[0014] In the present specification, the "lithium hydroxide raw material" is not particularly limited as long as it is in the form of a lithium hydroxide salt, and may be, for example, lithium hydroxide monohydrate. In addition, in the present specification, the "lithium hydroxide raw material" may be in a form containing a trace amount of impurities. In addition, in the present invention, the particle size of the "lithium hydroxide raw material" is not particularly limited.
[0015] Lithium hydroxide or lithium hydroxide monohydrate has a lower decomposition temperature than other lithium salts, making it possible to synthesize lithium sulfide under relatively mild conditions, making it suitable for use as a lithium precursor when manufacturing lithium sulfide. However, lithium hydroxide and lithium hydroxide monohydrate are hygroscopic, and when exposed to the atmosphere, they are rapidly converted into lithium carbonate (Li2CO3) by carbon dioxide (CO2), but the converted lithium carbonate is decomposed only at high temperatures, making it difficult to remove using general methods, and it may remain as an impurity even after lithium sulfide is manufactured, causing adverse effects such as a decrease in solid electrolyte performance, i.e., ionic conductivity.
[0016] Therefore, the inventors of the present invention have confirmed that it is possible to effectively reduce unreacted raw materials and lithium carbonate and produce high-purity lithium sulfide by additionally performing a step of first introducing hydrogen sulfide gas, which is used as a sulfur precursor in the production of lithium sulfide, to react with lithium hydroxide raw material, and then secondly introducing hydrogen sulfide gas and performing heat treatment, thereby completing the present invention. Furthermore, since the present invention does not use a solvent in the reaction of the lithium hydroxide raw material and hydrogen sulfide gas described above, it is possible to prevent the possibility of additional impurities being generated due to the use of a solvent.
[0017] Step 1 of the present invention is a step of pretreating a lithium hydroxide raw material under an inert gas atmosphere, and is a step of raising the temperature of the lithium hydroxide raw material through step 1 to prepare for a reaction so as to facilitate a reaction with hydrogen sulfide in the reaction step of step 2. In addition, when lithium hydroxide monohydrate is used as the lithium hydroxide raw material, the lithium hydroxide monohydrate can be converted to anhydrous through step 1 of the present invention, thereby enabling a reaction with hydrogen sulfide gas in the step described below.
[0018] The inert gas is not particularly limited, but examples thereof include nitrogen, argon, helium, and mixtures thereof.
[0019] Also, step 1 may be performed at 170°C to 450°C. If step 1 is performed at less than 170°C, moisture in the lithium hydroxide raw material may not be easily removed, and moisture in the raw material may not be sufficiently removed, which may cause adverse effects such as a reverse reaction during lithium sulfide synthesis, and if step 1 is performed at more than 450°C, the lithium hydroxide raw material may melt, so it is preferable to perform step 1 within the above range. Preferably, step 1 may be performed at 175°C or more, 180°C or more, 185°C or more, 190°C or more, or 195°C or more, and 225°C or less, 220°C or less, 215°C or less, 210°C or less, or 205°C or less.
[0020] Step 2 of the present invention is a step of first inputting hydrogen sulfide gas and dry-reacting the pretreated lithium hydroxide raw material with hydrogen sulfide. As described above, the present invention relates to a production method in which a solid lithium hydroxide raw material is used as a lithium precursor, and gaseous hydrogen sulfide is used as a sulfur precursor, and they are dry-reacted in the absence of a solvent.
[0021] Step 2 of the present invention may be carried out at a temperature that is the same as or different from the temperature of the pretreatment step of step 1. More specifically, the reaction step of step 2 may be carried out at the same temperature as the pretreatment step of the raw material, or may be carried out by increasing the temperature to 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C, or decreasing the temperature to 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C, based on the temperature of step 1.
[0022] Preferably, in step 2, hydrogen sulfide gas may be initially introduced so that the molar ratio of lithium hydroxide raw material to hydrogen sulfide gas in step 1 is 1:0.5 to 1:50. If the molar ratio of hydrogen sulfide gas to lithium hydroxide raw material is less than 1:0.5, the reactivity of hydrogen sulfide and lithium hydroxide raw material may be low, resulting in a long reaction time and reduced process efficiency. More preferably, hydrogen sulfide gas may be initially introduced so that the molar ratio of lithium hydroxide to hydrogen sulfide gas is 1:1 to 1:40, or 1:1 to 1:35, or 1:1 to 1:30.
[0023] In addition, step 2 of the present invention may be performed while removing water. By removing water generated in the reaction between the lithium hydroxide raw material and hydrogen sulfide gas in the reaction system, it is possible to prevent aggregation phenomenon due to moisture absorption of lithium hydroxide and promote the reaction. As a method for removing water in the reaction step, a technique well known in the art can be used. For example, water can be removed by condensing vapor water generated together with hydrogen sulfide gas into a liquid form using a condenser, and introducing gaseous hydrogen sulfide back into the reactor. If even a small amount of water cannot be properly removed in the above process, lithium sulfide may be converted back into lithium hydroxide by a reverse reaction, and lithium hydroxide may remain in the reaction product containing lithium sulfide.
[0024] Step 3 of the present invention is a step of heating the reaction product under an inert gas atmosphere after the reaction of step 2 is completed. The completion of the reaction of step 2 can be confirmed by observing whether water is generated in the reaction of the lithium hydroxide raw material and hydrogen sulfide gas. That is, step 3 of the present invention is a step of heating the reaction product under an inert gas atmosphere after it is confirmed that no additional water is generated, to prepare for a heat treatment step by secondary injection of hydrogen sulfide gas.
[0025] Meanwhile, the inert gas in step 3 may be the same as or different from that in step 1, and the description of the inert gas is as described above.
[0026] Preferably, step 3 may be performed at 230°C to 400°C. If it is performed at less than 230°C, there is a problem that lithium carbonate, an impurity, cannot be effectively removed in step 4 described below, and if it is performed at more than 400°C, there is a problem that the process efficiency is low. More preferably, it may be performed at 235°C or more, 240°C or more, 245°C or more, or 250°C or more, and 390°C or less, 380°C or less, 370°C or less, 360°C or less, or 350°C or less. Furthermore, step 3 of the present invention may be heated to a temperature higher than step 1.
[0027] Step 4 of the present invention is a step of secondly introducing hydrogen sulfide gas and performing heat treatment. As described above, unreacted lithium hydroxide raw material and lithium carbonate may exist in the lithium sulfide produced through steps 1 to 3. Therefore, this is a process for converting unreacted lithium hydroxide and lithium carbonate to lithium sulfide. By secondly introducing hydrogen sulfide gas and performing heat treatment separately from the first introduction step of hydrogen sulfide gas in step 2 described above, unreacted lithium hydroxide raw material and lithium carbonate in lithium sulfide can be removed, and high purity lithium sulfide can be produced.
[0028] On the other hand, step 4 of the present invention may be performed under temperature conditions that are the same as or different from the temperature raised in step 3, and may be performed at the same temperature as that of step 3, for example.
[0029] Preferably, in step 4, hydrogen sulfide may be added secondarily so that the molar ratio of lithium hydroxide raw material and hydrogen sulfide gas in step 1 is 1:5 to 1:50. Adding hydrogen sulfide gas in the amount within this range is advantageous for lithium carbonate contained in lithium sulfide to be converted to lithium sulfide by facilitating contact with hydrogen sulfide, and if the amount is outside this range, a problem may occur in which lithium carbonate is not effectively converted to lithium sulfide. More preferably, the molar ratio of lithium hydroxide and hydrogen sulfide gas in step 1 may be 1:6 to 1:45, or 1:7 to 1:40, or 1:8 to 1:35, or 1:9 to 1:30.
[0030] Also, preferably, the molar ratio of the hydrogen sulfide gas introduced first in step 2 to the hydrogen sulfide gas introduced second in step 4 may be 1:0.5 to 1:50. Introducing hydrogen sulfide gas in this range is advantageous in terms of facilitating contact between hydrogen sulfide and lithium hydroxide and improving reactivity, and if introduced in a small amount outside this range, reactivity may decrease and unreacted lithium hydroxide may remain, and if introduced in an excessive amount, process efficiency may decrease. More preferably, the molar ratio of the hydrogen sulfide gas introduced first to the hydrogen sulfide gas introduced second may be 1:8 to 1:45, or 1:10 to 1:40, or 1:10 to 1:30.
[0031] Meanwhile, the heat treatment step of step 4 may be performed for 3 to 10 hours. If the heat treatment step is performed for less than 3 hours, impurities may not be effectively removed, and if it is performed for more than 10 hours, process efficiency may decrease. More preferably, the heat treatment step of step 4 may be performed for 4 hours or more, or 5 hours or more, and 8 hours or less, or 7 hours or less.
[0032] Meanwhile, according to one embodiment of the present invention, steps 1 to 4 may be carried out in a one-pot process. Here, the term "one-pot process" means that the steps of the present invention are carried out in a single reaction vessel without isolation of any intermediates before recovery of the final product.
[0033] If the drying step of the lithium hydroxide raw material, the synthesis step performed by introducing lithium sulfide, and the heat treatment step are performed in separate reactors, additional costs may be incurred in the process of transporting solid raw materials, and as described above, the lithium hydroxide raw material may be rapidly converted to lithium carbonate when exposed to the atmosphere, which may cause contamination of the dried raw materials. According to a method for producing lithium sulfide according to an embodiment, the lithium hydroxide raw material is introduced into a reactor and dried, and then hydrogen sulfide is introduced first without introducing a solvent to carry out a reaction to synthesize lithium sulfide, and after heating in a nitrogen atmosphere, hydrogen sulfide is introduced a second time and heat treatment is performed. By performing a series of processes in the same reactor, it is possible to prevent the occurrence of the contamination problems caused by the transportation and exposure to the atmosphere.
[0034] In addition, when the above-mentioned one-pot reaction is performed, the type of reactor is not particularly limited, and examples thereof include a batch reactor, a semi-batch reactor, a flow reactor, and a fluidized reactor.
[0035] According to the above-mentioned method for producing lithium sulfide of the present invention, the lithium sulfide may contain 5,000 ppm or less of lithium carbonate based on the mass of the produced lithium sulfide as a result of IC (Ion chromatography) analysis. Preferably, the lithium sulfide may contain 4,500 ppm or less, 4,200 ppm or less, 4,000 ppm or less, 3,500 ppm or less, 3,000 ppm or less, or 2,000 ppm or less of lithium carbonate based on the mass of the lithium sulfide.
[0036] Meanwhile, the present invention can provide lithium sulfide prepared by the above-mentioned preparation method. As described above, the lithium sulfide of the present invention is high-purity lithium sulfide having an amount of carbonate-based impurities that are difficult to remove of 5,000 ppm or less, and can achieve excellent performance when preparing a solid electrolyte material.
[0037] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention. However, these examples are presented only as examples of the present invention and do not define the scope of the invention.
[0038] [Example]
[0039] Example 1 17g of lithium hydroxide monohydrate (LiOH·H2O) was heated to 200℃ in a nitrogen (N2) atmosphere and maintained for 2 hours for pretreatment. Lithium hydroxide (LiOH) was then transferred to a reaction vessel, and hydrogen sulfide (H2S) was added for the first time so that the molar ratio of lithium hydroxide (LiOH) to hydrogen sulfide (H2S) was 1:1. The reaction was continued at 200℃ while removing the by-product water until no more water was generated. When it was confirmed that no more water was being generated, the injection of hydrogen sulfide (H2S) was stopped, and the reaction product containing lithium sulfide (Li2S) was recovered from the reactor and transferred to a heat treatment device. The temperature of the heat treatment device was raised to 250℃ in a nitrogen atmosphere. Hydrogen sulfide (H2S) was then added for the second time so that the molar ratio of lithium hydroxide (LiOH) to hydrogen sulfide (H2S) added initially was 1:10, and heat treatment was performed at 250℃ for 6 hours to produce lithium sulfide.
[0040] Example 2 Lithium sulfide was produced by the same production method as in Example 1, except that the heat treatment temperature was changed to 300°C.
[0041] Example 3 Lithium sulfide was produced by the same production method as in Example 1, except that the heat treatment temperature was changed to 350°C.
[0042] Example 4 Lithium hydroxide monohydrate (LiOH·H2O) was placed in a reactor and heated to 200°C in a nitrogen (N2) atmosphere. Nitrogen was injected so that the ratio of lithium hydroxide monohydrate to nitrogen was 1:5 based on the molar number. After the reactor temperature reached 200°C, the temperature was maintained for 5 hours for pretreatment. Nitrogen injection was stopped and hydrogen sulfide was added for the first time so that the molar ratio of lithium hydroxide monohydrate to hydrogen sulfide was 1:1. The reaction was carried out at 200°C for 5 hours while removing the by-product water. After confirming that no more water was being generated, hydrogen sulfide injection was stopped and the temperature was raised to 350°C in a nitrogen atmosphere. Hydrogen sulfide was then added for the second time so that the molar ratio of lithium hydroxide monohydrate to hydrogen sulfide was 1:10, and heat treatment was carried out at 350°C for 6 hours. The pretreatment, reaction and heat treatment steps of the above process were carried out in one-pot without opening the reactor to produce lithium sulfide.
[0043] Comparative Example 1 17g of lithium hydroxide (LiOH) was added and heated to 200℃ in a nitrogen (N2) environment. After reaching 200℃, hydrogen sulfide (H2S) was added in the first batch so that the molar ratio of lithium hydroxide (LiOH) to hydrogen sulfide (H2S) was 1:1, and the reaction was continued while removing the by-product water until no more water was produced.
[0044] Experimental Example 1: X-ray diffraction analysis X-ray diffraction (XRD) analysis was performed on the lithium sulfide prepared in Example 1. The XRD equipment used was Rigaku's Ultima IV, and the measurement was performed at room temperature. The results are shown in FIG. As can be seen from FIG. 1, the XRD analysis results showed that the lithium sulfide prepared according to the embodiment of the present invention had peaks at the same positions as those of the commercial lithium sulfide powder used as a reference material.
[0045] Experimental Example 2: Analysis of lithium carbonate content The lithium carbonate (Li2CO3) content of the lithium sulfide prepared in the examples and comparative examples was measured based on the mass of the raw material or lithium sulfide using ion chromatography (IC). The IC analyzer used was Thermofisher's ICS-6000, and the results are shown in Table 1 below.
[0046] [Table 1]
[0047] As can be seen from Table 1 above, according to the method for producing lithium sulfide of the present invention, it was confirmed that it is possible to effectively remove carbonate-based impurities contained in raw materials and produce high-purity lithium sulfide.
Claims
1. A step (step 1) of pretreating a lithium hydroxide raw material under an inert gas atmosphere; A step (step 2) of first introducing hydrogen sulfide gas to dry react the pretreated lithium hydroxide raw material with hydrogen sulfide; After the reaction of step 2 is completed, a step (step 3) of heating the reaction product under an inert gas atmosphere; and (4) a step of subjecting the mixture to a second heat treatment by introducing hydrogen sulfide gas. How lithium sulfide is produced.
2. Step 1 is carried out at 170 to 450° C. The method for producing lithium sulfide according to claim 1.
3. In step 2, hydrogen sulfide gas is first introduced so that the molar ratio of lithium hydroxide raw material to hydrogen sulfide gas in step 1 is 1:0.5 to 1:50; The method for producing lithium sulfide according to claim 1.
4. Step 2 is carried out while removing water. The method for producing lithium sulfide according to claim 1.
5. Step 3 is to increase the temperature to 230° C. to 400° C. The method for producing lithium sulfide according to claim 1.
6. In step 4, hydrogen sulfide is added for a second time so that the molar ratio of the lithium hydroxide raw material and hydrogen sulfide gas in step 1 is 1:5 to 1:
50. The method for producing lithium sulfide according to claim 1.
7. The molar ratio of the hydrogen sulfide gas primarily introduced in step 2 to the hydrogen sulfide gas secondarily introduced in step 4 is 1:0.5 to 1:
50. The method for producing lithium sulfide according to claim 1.
8. Step 4 is carried out for 3 to 10 hours. The method for producing lithium sulfide according to claim 1.
9. Steps 1 to 4 are carried out in a one-pot process; The method for producing lithium sulfide according to claim 1.
10. According to the IC (Ion Chromatography) analysis, the lithium carbonate content is 5,000 ppm or less based on the mass of the lithium sulfide produced. The method for producing lithium sulfide according to claim 1.
11. Lithium sulfide produced by the method according to any one of claims 1 to 10.
Citation Information
Patent Citations
Production of lithium sulfide
JP1997110404A
Method of producing alkali metal sulfide
JP2015071516A
Lithium sulfide and method for producing the same
JP2017222567A
Lithium sulfide powder and manufacturing method therefor
JP2019094255A
Manufacturing method of modified lithium sulfide powder and modified lithium sulfide powder
JP2019156691A