Method for producing single crystal, single crystal, piezoelectric element, ultrasonic motor, optical device, vibration device, dust removing device, imaging device, ultrasonic probe, ultrasonic diagnosis device, ultrasonic diagnosis system, and electronic device
A controlled two-step temperature increase process with specific compositions of Ba, Ti, Zr, and Mn stabilizes single crystal growth, addressing the challenge of producing single crystals with high piezoelectric constants and mechanical quality factors for diverse material compositions, enhancing their applicability in piezoelectric elements and devices.
Patent Information
- Application Number
- JP2024045263
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-25
AI Technical Summary
Existing methods struggle to produce single crystals with large piezoelectric constants and mechanical quality factors for a wide range of material compositions, particularly in perovskite-type oxides like BaTiO3, as abnormal grain growth is difficult to achieve solely through heat treatment temperature adjustments.
A method involving a controlled two-step temperature increase process is used to produce single crystals, where the second temperature increase step has a lower rate than the first, combined with specific compositions of Ba, Ti, Zr, and Mn to stabilize the growth of single crystals, ensuring a wider compatibility with various material compositions.
This approach enables the production of single crystals with enhanced piezoelectric constants and mechanical quality factors, suitable for applications in piezoelectric elements and devices, overcoming the limitations of conventional methods.
Smart Images

Figure 2024152635000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a single crystal and the single crystal. The present invention also relates to a piezoelectric element, an ultrasonic motor, an optical device, a vibration device, a dust removal device, an imaging device, an ultrasonic probe, an ultrasonic diagnostic device, an ultrasonic diagnostic system, and an electronic device using the single crystal. [Background technology]
[0002] Patent Document 1 discloses a solid-phase method for producing single crystals of materials such as barium titanate, in which a seed single crystal is bonded to a matrix and heat-treated to cause abnormal grain growth in which only a single crystal grain grows, and then the abnormal grain is cut out to obtain a single crystal. Patent Document 1 describes that barium titanate may be substituted with Zr or Mn, and also describes the heat treatment temperature, but does not particularly describe the temperature rise rate or time during the temperature rise process during the heat treatment.
[0003] As a result of extensive research, the present inventors have found that there are some material compositions in which it is difficult to induce abnormal grain growth, which enlarges a single crystal grain, simply by adjusting the heat treatment temperature.
[0004] On the other hand, when using piezoelectric single crystals in resonant devices such as ultrasonic motors, the piezoelectric constant and mechanical quality factor, which represents the sharpness of the resonance, are required to be large. If the piezoelectric constant and mechanical quality factor are small, the power required for operation will be high. Therefore, single crystals with large piezoelectric constants and mechanical quality factors are required. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 3507821 Summary of the Invention [Problem to be solved by the invention]
[0006] There are some material compositions in which abnormal grain growth, which enlarges only a single crystal grain, is difficult to achieve by simply adjusting the heat treatment temperature as in conventional techniques, and there has been a problem in that single crystals of such compositions cannot be obtained.
[0007] The present invention has been made to solve such problems, and one of its objects is to provide a method for producing single crystals that can accommodate a wider range of material compositions, thereby having a larger piezoelectric constant and mechanical quality factor when made into a piezoelectric element. Another object of the present invention is to provide a single crystal that has a larger piezoelectric constant and mechanical quality factor when used as a piezoelectric element. Additionally, an object of the present invention is to provide an ultrasonic motor, optical equipment, vibration device, dust removal device, imaging device, ultrasonic probe, ultrasonic diagnostic device, ultrasonic diagnostic system, and electronic device that use a piezoelectric element having a larger piezoelectric constant and mechanical quality factor. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention provides A method for producing a single crystal by heating a matrix, comprising the steps of: A first preparation step of preparing a matrix and a seed single crystal; a second preparation step of preparing an integral body in which a surface of the matrix and a surface of the seed single crystal are arranged in contact with each other; A first heating step of heating the integrated body from room temperature to a liquid phase initiation temperature of the matrix; a second heating step of heating the integrated body from the liquid phase start temperature to a liquid phase finish temperature of the matrix; a heating step of heating the integral body at the liquid phase finish temperature; obtaining a single crystal from the monolith after the heating; Including, This is a method for producing a single crystal, wherein the temperature increase rate in the second temperature increase step is smaller than the temperature increase rate in the first temperature increase step.
[0009] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: A single crystal containing a perovskite-type oxide containing Ba, Ti, and Zr and Mn, x, which is a molar ratio of the Zr to the sum of the Ti and the Zr, is 0.01≦x≦0.13; The single crystal has a Mn content of 0.04 parts by mass or more and 1.16 parts by mass or less in terms of metal relative to 100 parts by mass of the oxide.
[0010] The present invention also provides a piezoelectric element having a plurality of electrodes and the above-mentioned single crystal. The present invention also provides an ultrasonic motor having a vibrating body on which the above-mentioned piezoelectric element is disposed, and a moving body in contact with the vibrating body. The present invention also relates to an optical device having the above-mentioned ultrasonic motor in a drive section. The present invention also provides a vibration device having a vibrating body with the above-mentioned piezoelectric element disposed on a diaphragm. The present invention also provides a dust removing device having the above-mentioned vibration device in a vibration section. The present invention also provides an imaging device having the above-mentioned dust removal device and an imaging element unit, in which a diaphragm of the above-mentioned dust removal device is provided on the light receiving surface side of the imaging element unit. The present invention also provides an ultrasonic probe having the above-mentioned piezoelectric element, which transmits and receives signals by means of the piezoelectric element. The present invention also provides an ultrasonic diagnostic apparatus having the above-mentioned ultrasonic probe and an image output unit. The present invention also provides an ultrasound diagnostic system having the above-mentioned ultrasound probe, a transmitting unit that transmits a signal output from the above-mentioned ultrasound probe, and a receiving unit that receives the signal transmitted from the transmitting unit. The present invention also relates to an electronic device equipped with a piezoelectric acoustic component having the above-mentioned piezoelectric element. Effect of the Invention
[0011] According to the present invention, there is provided a method for producing a single crystal that can accommodate a wide range of material compositions, such as a composition containing Mn and a perovskite-type oxide containing Ba, Ti, and Zr, which could not be produced by conventional methods, and the single crystal. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram for explaining a first embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram for explaining a first embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic diagram for explaining a first embodiment of the present invention. [Figure 4] FIG. 1 is a schematic diagram for explaining a first embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic diagram for explaining a temperature rise profile of a heat treatment according to the first embodiment of the present invention. [Figure 6] 1 is a schematic diagram showing an embodiment of the configuration of a piezoelectric element of the present invention. [Figure 7] 1 is a schematic diagram showing an embodiment of the configuration of an ultrasonic motor of the present invention. [Figure 8A] 1 is a schematic diagram showing an embodiment of an optical instrument of the present invention. [Figure 8B] FIG. 2 is a schematic diagram showing another embodiment of the optical instrument of the present invention. [Figure 9] 1 is a schematic diagram showing an embodiment of an optical instrument of the present invention. [Figure 10A] 1 is a schematic diagram showing an embodiment in which a vibration device of the present invention is used as a dust removing device. [Figure 10B] FIG. 11 is a schematic diagram showing another embodiment in which the vibration device of the present invention is used as a dust removing device. [Figure 11A] 2 is a schematic diagram showing an example of a configuration of a piezoelectric element in the dust removing device of the present invention. FIG. [Figure 11B] 5 is a schematic diagram showing another example of the configuration of a piezoelectric element in the dust removing device of the present invention. FIG. [Figure 11C] 5 is a schematic diagram showing another example of the configuration of a piezoelectric element in the dust removing device of the present invention. FIG. [Figure 12A] 3A and 3B are schematic diagrams illustrating an example of the vibration principle of the dust removing device of the present invention. [Figure 12B]5A and 5B are schematic diagrams showing another example of the vibration principle of the dust removing device of the present invention. [Figure 13] 1 is a schematic diagram showing an embodiment of an imaging device of the present invention. [Figure 14] 1 is a schematic diagram showing an embodiment of an imaging device of the present invention. [Figure 15] 1 is a schematic diagram showing an embodiment of an ultrasonic probe of the present invention. [Figure 16] 1 is a schematic diagram showing an embodiment of an ultrasonic diagnostic apparatus of the present invention. [Figure 17] 1 is a schematic diagram showing an embodiment of an ultrasound diagnostic system of the present invention. [Figure 18] 1 is a schematic diagram showing an embodiment of an ultrasound diagnostic system of the present invention. [Figure 19] 1 is a schematic diagram showing an embodiment of an electronic device of the present invention. [Figure 20] FIG. 2 is a diagram illustrating the state of a matrix after heat treatment in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described. The present invention provides a method for producing a single crystal that can be adapted to a wide range of material compositions, and a single crystal obtained thereby. Furthermore, the single crystal of the present invention can be used as a piezoelectric element in various applications, such as electronic devices such as semiconductors, light-emitting elements, optical elements, energy conversion elements, and sensors.
[0014] <First embodiment> The first embodiment relates to a method for producing a single crystal. The method for producing a single crystal of the present invention comprises the steps of: A method for producing a single crystal by heating a matrix, comprising the steps of: A first preparation step of preparing a matrix and a seed single crystal; a second preparation step of preparing an integral body in which a surface of the matrix and a surface of the seed single crystal are arranged in contact with each other; A first heating step of heating the integrated body from room temperature to a liquid phase initiation temperature of the matrix; a second heating step of heating the integrated body from the liquid phase start temperature to a liquid phase finish temperature of the matrix; a heating step of heating the integral body at the liquid phase finish temperature; obtaining a single crystal from the monolith after the heating; Including, The temperature increase rate in the second temperature increase step is smaller than the temperature increase rate in the first temperature increase step. Each item will be explained below together with an explanation of basic matters for understanding the invention. Some substances such as single crystals will also be explained in the second embodiment.
[0015] [Explanation 1 for understanding the invention] (Description of single crystal) A single crystal is one that is made up of a single crystal grain, and the crystal axis, which is the direction of the atomic arrangement, is the same in every part of the inside of the crystal grain. However, the single crystal of the present invention may contain lattice defects such as dislocations, holes, and voids inside the single crystal. In addition, it may contain a domain structure that occurs due to differences in crystal systems caused by phase transitions or differences in the direction of spontaneous polarization.
[0016] (Perovskite type) Perovskite-type oxides refer to a perovskite structure (also called perovskite structure) that is ideally a cubic crystal structure, as described in the Iwanami Dictionary of Physics and Chemistry, 5th Edition (Iwanami Shoten, published February 20, 1998). Perovskite-type oxides are generally expressed by the chemical formula ABO3. The molar ratio of the elements in the A and B sites to the O element is expressed as 1:3, but even if the ratio of the amount of elements is slightly different (for example, 1.00:2.94 to 1.00:3.06), the oxide can be said to be a perovskite-type oxide as long as it has a perovskite-type main phase.
[0017] In addition, when the coordinates of the A element, the B element, and the O element are slightly shifted from the symmetrical positions of the unit lattice, the perovskite-type unit lattice is distorted, resulting in a crystal system such as a tetragonal crystal, a rhombohedral crystal, or an orthorhombic crystal. The single crystal of the present invention is preferably made of a perovskite-type oxide, and the crystal system of the single crystal can be not only a cubic crystal but also a tetragonal crystal, a rhombohedral crystal, or an orthorhombic crystal system depending on the single or multiple elements constituting A and B. Whether an oxide is a perovskite-type and what its crystal system is can be determined, for example, by structural analysis using X-ray diffraction or electron beam diffraction. In this case, the sample may be powdered before measurement as necessary.
[0018] A specific method for producing the single crystal of the present invention will now be described. FIG. 1 is a schematic diagram showing one embodiment of an integral body of a seed single crystal 2 and a matrix 1 according to the present invention. In FIG. 1, a seed single crystal 2 is provided on top of a matrix 1, and the surface of the matrix 1 and the surface of the seed single crystal 2 are disposed in contact with each other to form an integrated body. The method for producing a single crystal according to the present invention is, for example, a method for producing a single crystal by heating a monolithic matrix 1 as shown in FIG.
[0019] [First preparation step] The method for producing a single crystal of the present invention includes a first preparation step of preparing a matrix 1 and a seed single crystal 2 . (Matrix explanation) The matrix 1 of the present invention is preferably a molded body or a sintered body. The shape of the matrix 1 is not particularly limited, but a shape having a flat surface such as a rectangular parallelepiped or disk shape is preferable because it is easy to arrange the matrix 1 in contact with the seed single crystal 2.
[0020] (Raw material powder for making the matrix) The raw material used for the matrix 1 of the present invention is a solid powder of an oxide, carbonate, nitrate, oxalate, or the like containing the constituent elements constituting the single crystal of the present invention, or a mixed powder of these. It is more preferable that the lead (Pb) content in the raw materials is less than 1000 ppm, since this reduces the burden on the environment.
[0021] Preferred elements constituting the raw material of matrix 1 include, for example, Li, Na, Mg, Al, Si, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Zn, Ge, Sr, Y, Zr, Nb, Mo, Sn, Sb, Ba, Hf, Ta, Bi, La, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, and Yb.
[0022] The raw materials may be heat-treated for the purpose of homogenization, or may be crushed after heat treatment. It is preferable to perform the heat treatment for homogenizing the raw materials at a temperature in the range of 800° C. to 1300° C., since the raw materials are easily crushed after the heat treatment.
[0023] When producing the single crystal of the present invention, a general method can be adopted in which a molded body is made from solid powder of oxides, carbonates, nitrates, oxalates, acetates, etc. containing the constituent elements, and the molded body is sintered under normal pressure. The raw materials are composed of compounds such as Ba compounds, Ti compounds, Zr compounds, Mn compounds, and Bi compounds.
[0024] Usable Ba compounds include barium oxide, barium carbonate, barium oxalate, barium acetate, barium nitrate, barium titanate, barium zirconate, etc. It is preferable to use commercially available high-purity Ba compounds (e.g., 99.99% or more purity).
[0025] Usable Ti compounds include titanium oxide, barium titanate, barium titanate zirconate, etc. When these Ti compounds contain alkaline earth metals such as barium, it is preferable to use commercially available high-purity compounds (e.g., purity of 99.99% or more). It may contain Nb to the extent that it is contained as an unavoidable component in commercially available raw materials for Ti, and Hf to the extent that it is contained as an unavoidable component in commercially available raw materials for Zr.
[0026] Usable Zr compounds include zirconium oxide, barium zirconate, barium zirconate titanate, etc. When these Zr compounds contain alkaline earth metals such as barium, it is preferable to use commercially available high-purity compounds (e.g., purity of 99.99% or more).
[0027] Usable Mn compounds include manganese carbonate, manganese oxide, manganese dioxide, manganese acetate, and trimanganese tetroxide.
[0028] Usable Bi compounds include dibismuth trioxide, bismuth nitrate, bismuth fluoride, bismuth carbonate, and bismuth hydroxide.
[0029] In addition, the raw material for adjusting the amount of Ba present at the A site of the piezoelectric material according to the present invention and the molar ratio of Ti and Zr at the B site, a, is not particularly limited. The same effect can be obtained with any of Ba compounds, Ti compounds, and Zr compounds.
[0030] (Granulation of raw materials for preparing the matrix) The raw material of the matrix 1 used in the method for producing a single crystal of the present invention may be granulated, and the granulation method is not particularly limited. Examples of binders that can be used in granulation include PVA (polyvinyl alcohol), PVB (polyvinyl butyral), and acrylic resins. The amount of binder added to the mixed powder is preferably 1 part by mass to 10 parts by mass, and more preferably 2 parts by mass to 5 parts by mass from the viewpoint of increasing the density of the molded body. The most preferable granulation method is the spray drying method from the viewpoint of making the particle size of the granulated powder more uniform.
[0031] (Molded body of raw material for producing matrix) The molded body of the matrix 1 used in the method for producing the single crystal of the present invention is a molded body obtained by solidifying the above-mentioned raw materials into a desired shape, and the method for producing the molded body is not particularly limited. The molded body is a solid body produced from raw material powder, granulated powder (binder), or slurry.
[0032] The molded body can be produced by uniaxial pressing, cold isostatic pressing, warm isostatic pressing, casting, extrusion, etc. Alternatively, the raw material in a slurry state may be formed into a sheet using a doctor blade method and dried, and the sheets may be stacked and molded into a desired shape. It is preferable to perform a degassing step before drying the sheet, since this increases the density, and therefore the density of the matrix 1 using the sheet also increases, and the density of the single crystal produced using the matrix 1 also increases.
[0033] It is preferable that the matrix 1 in the method for producing a single crystal of the present invention is a molded body. Furthermore, it is preferable that the matrix 1 is a polycrystal containing elements constituting the single crystal produced by the method for producing a single crystal of the present invention. In this way, a single crystal with a large area can be obtained. In this case, as shown in FIG. 1, a seed single crystal 2 is placed on the matrix 1 and the matrix 1 and the seed single crystal 2 are arranged in contact with each other. When heat treatment is performed in this state, the matrix 1 shrinks and the seed single crystal 2 slightly bites into the matrix 1, so that the matrix 1 and the seed single crystal 2 are in closer contact with each other. In other words, the contact area between the matrix 1 and the seed single crystal 2 becomes larger.
[0034] Although there is a method of placing the seed single crystals 2 in a molded body during molding, there is a risk of significant deformation or breakage or cracks occurring during heat treatment due to the difference in the amount of shrinkage between the molded body and the seed single crystals 2. Therefore, when the matrix 1 is a molded body, it is preferable to place the seed single crystals 2 in contact with each one of the surfaces of the matrix 1.
[0035] It is preferable to arrange the matrix 1 and the seed single crystal 2 one above the other so that they are in contact with each other. Furthermore, it is preferable to place a weight on the matrix 1 and the seed single crystal 2, since this facilitates contact between the matrix 1 and the seed single crystal 2. Even if a force acts in a direction that separates the matrix 1 and the seed single crystal 2 due to deformation during heat treatment or the like, the weight acts in a direction that suppresses this force, so that they are more likely to come into contact with each other.
[0036] The area of the surface of the seed single crystal 2 in contact with the matrix 1 is preferably equal to or smaller than the area of the surface of the matrix 1 in contact with the seed single crystal 2. The portion of the seed single crystal 2 larger than the matrix 1 is wasted because it does not contribute to the single crystallization of the matrix 1. Therefore, it is preferable that the seed single crystal 2 is as small as possible.
[0037] However, if the seed single crystal 2 is too small, the heat treatment time required to expand the single crystal region to the entire matrix becomes long. Therefore, the area of the face of the seed single crystal 2 in contact with the matrix 1 is preferably 50% or more and 100% or less of the area of the face of the matrix 1 in contact with the seed single crystal 2.
[0038] (Sintering) When matrix 1 is used as a sintered body, the above molded body may be sintered by any method, and examples of the sintering method include sintering in an electric furnace, sintering in a gas furnace, hot pressing, electric current heating, microwave sintering, millimeter wave sintering, HIP (hot isostatic pressing), and flash sintering. Hot pressing, electric current heating, and HIP, which generate high pressure at high temperatures, are preferred because they can reduce the size or number of voids in the matrix. If the volume of the voids in the matrix is small, the density of the single crystal obtained from matrix 1 is high, which is preferred.
[0039] The relative density of the matrix 1 is preferably 93% or more and 100% or less. When the relative density of the matrix 1 is 93% or more and 100% or less, the density of the single crystal obtained from the matrix 1 also becomes high. The relative density is the ratio of the theoretical density calculated from the lattice constant of the piezoelectric material and the atomic weight of the constituent elements of the piezoelectric material to the measured density. The lattice constant can be measured by, for example, X-ray diffraction analysis. The density can be measured by, for example, Archimedes method.
[0040] When the ratio of the measured density (ρmeas.) to the theoretical density (ρcalc.) calculated from the composition and lattice constant of the sintered body, that is, the relative density (ρcalc. / ρmeas.), is 93% or higher, the relative density can be said to be sufficiently high.
[0041] (Seed single crystal) The seed single crystal 2 used in the method for producing a single crystal of the present invention may be a bulk or a thin film, but since stress may be generated in the seed single crystal 2 due to a mismatch in lattice constant with the matrix 1 or a difference in thermal expansion in the region in contact with the matrix 1, which may cause the seed single crystal 2 to break, it is preferable that the seed single crystal 2 be a bulk having a thickness of 10 μm or more in terms of high strength. In addition, it is preferable that the matrix 1 and the seed single crystal 2 have approximately the same composition. The seed single crystal 2 may be prepared by selecting from commercially available oxide single crystals, semiconductor single crystals, fluoride / alkali halide single crystals, metal single crystals, alloy single crystals, etc., but a perovskite-type single crystal is preferable because stress is less likely to be generated due to a mismatch in lattice constant with the matrix 1 or a difference in thermal expansion.
[0042] The seed single crystal 2 used in the method for producing a single crystal of the present invention is preferably a single crystal containing Ba, Ti, and Zr as main components. Also, the seed single crystal 2 used in the method for producing a single crystal of the present invention is preferably a single crystal containing Ba, Ti, and Ca as main components.
[0043] When the seed single crystal 2 is a single crystal mainly composed of Ba, Ti, and Zr or Ba, Ti, and Ca, it is preferable because the lattice constant and linear expansion coefficient are close to those of the matrix 1, so that stress is less likely to occur and the produced single crystal is less likely to crack.
[0044] The perovskite type single crystals used as the seed single crystal 2 include BaTiO3, BaZrO3, SrTiO3, CaTiO3, Pb(Mg 1 / 3 Nb 2 / 3 )O3, KTaO3, KNbO3, SrRuO3, LiNbO3, LaNiO3, AgNbO3, CdTiO3, and solid solutions thereof. As the seed single crystal 2 used in the production method of the present invention, a single crystal obtained by the production method of a single crystal of the present invention may be used.
[0045] [Second preparation step] The method for producing a single crystal of the present invention includes a second preparation step of preparing an integral body in which the surface of the matrix 1 and the surface of the seed single crystal 2 are arranged in contact with each other. (polishing) The method for producing a single crystal of the present invention preferably includes a step of polishing the matrix 1 and the seed single crystal 2 obtained by sintering as described above, and the contact area can be increased by arranging the polished surfaces of the matrix 1 and the seed single crystal 2 in contact with each other to form an integrated body. If the polished surface is a mirror surface, this is preferable because it further increases the contact area between the seed single crystal 2 and the matrix 1. When the matrix 1 is used as a molded body, it is preferable that the surface of the mold used to produce the molded body is a mirror surface, since the surface of the molded body pressed against that surface will also be a mirror surface.
[0046] Polishing methods include mechanical polishing, chemical polishing, and CMP polishing, and these may be combined for polishing. Mechanical polishing refers to polishing using a machine, and when performing mechanical polishing, a polishing machine, lapping machine, polishing machine, buffing machine, or the like may be selected and used. In addition, a process using a precision grinding machine with a fine grinding wheel can also be used as the polishing process. Chemical polishing is a polishing method in which a sample is immersed in a polishing solution and the surface of the sample is corroded by a chemical reaction using the power of acid or alkali. For example, a rotary type polishing method is used in which a polishing pad is attached to a disk-shaped surface plate, and a liquid abrasive containing chemical components and fine particles is dripped onto the pad and polished while rotating. CMP polishing is a technique that combines mechanical polishing and chemical polishing. It not only uses the mechanical action of abrasive grains to scrape the surface of the sample, but also creates a chemical reaction between the abrasive grains and the sample, and between the abrasive grains and the polishing or grinding fluid, resulting in a planarization of the surface through physical polishing and chemical reactions. The mirror surface can be produced by chemical polishing or CMP polishing.
[0047] (casket, setter, beads, weights) Figures 2, 3, and 4 are schematic diagrams showing an example of a configuration for producing a single crystal of the present invention. In Figure 2, a weight 4 is placed on an integral body of a matrix 1 and a seed single crystal 2, and the integral body is placed on a setter 6 via beads 5. In Figure 3, these are placed in a sagger 7, and in Figure 4, the sagger 7 of Figure 3 is covered with a lid 8. The sagger 7 with the lid 8 is placed in an electric furnace and heated.
[0048] It is preferable that the matrix 1 and the seed single crystal 2 are arranged above and below so as to be in contact with each other. Furthermore, it is preferable to place a weight 4 on the matrix 1 and the seed single crystal 2, since this facilitates contact between the matrix 1 and the seed single crystal 2. Even if a force acts in a direction that separates the matrix 1 and the seed single crystal 2 due to deformation during heat treatment or the like, the weight 4 acts in a direction that suppresses this force, so that they can be more easily in contact with each other.
[0049] When the matrix 1 is heated, it is preferable to heat-treat the matrix 1 and the seed single crystal 2 in a sagger 7, and a box-shaped sagger with a lid is preferable since it is less susceptible to the effects of furnace contamination.
[0050] The matrix 1 and the seed single crystal 2 may be placed on a setter 6 that is less reactive with the matrix 1 or the seed single crystal and then heat-treated. The material of the setter 6 may be, for example, alumina, zirconia, alumina with a zirconia surface coating, stabilized zirconia, silicon carbide, silicon nitride, or the like. Beads 5 such as stabilized zirconia, powder obtained by sintering and pulverizing the matrix 1 at high temperature, or a platinum sheet may be placed on the setter 6, and the matrix 1 and the seed single crystal 2 may be placed on top of the beads. If it is difficult to determine whether a material is less reactive, it is sufficient to actually try each material and select the one that leaves the least traces when heated.
[0051] [Explanation 2 for understanding the invention] (liquid phase of matrix) The matrix 1 used in the method for producing a single crystal of the present invention has a liquidus start temperature and a liquidus finish temperature.
[0052] (liquid phase) In the present invention, the liquid phase refers to a state in which at least a part of the matrix 1 is in a liquid phase, and also refers to a state in which the solid phase and the liquid phase coexist. The state and temperature can be confirmed, for example, by placing a sample on a microscope heating stage (manufactured by LINKAM Co., Ltd.), heating the sample, and observing the surface of the matrix 1 under a microscope. Specifically, the temperature at which the matrix 1 becomes liquid when at least a part of the grain boundaries of the matrix 1 cannot be confirmed during heating is the liquid phase start temperature, and the temperature at which at least a part of the grain boundaries of the matrix 1 appear with further heating is the liquid phase end temperature.
[0053] As another method, since the liquid phase becomes amorphous when it is rapidly cooled, matrix 1 can be heated to near the liquidus temperature, and the heated matrix 1 can be placed directly into tap water at room temperature and rapidly cooled. After that, the structure can be analyzed by X-ray diffraction, and the temperature at which it becomes liquid can be confirmed by the presence or absence of amorphous regions.
[0054] However, the liquid phase start temperature in the present invention varies due to the influence of impurity contamination in the preparation process, uneven pressure during molding, voids, etc. Therefore, the liquid phase start temperature is set to a range of ±50°C from the minimum temperature at which the liquid phase can be confirmed by the above means. Also, the liquid phase end temperature is set to a range of ±50°C from the maximum temperature at which the liquid phase can be confirmed by the above means.
[0055] When the interface between the seed single crystal 2 and the matrix 1 becomes liquid, the interface of the single crystal region of the seed single crystal 2 gradually spreads toward the matrix 1. At this time, it is considered that the crystal grains of the matrix 1 are incorporated into the single crystal due to the difference in surface energy. Therefore, if the crystal grains of the matrix 1 are too large, the difference in surface energy becomes small, making it difficult for the matrix 1 to be incorporated into the single crystal.
[0056] Therefore, when preparing the matrix 1 as a sintered body, it is preferable to sinter it at a temperature at which the crystal grains do not become too large during sintering. As a means for preventing the crystal grains from becoming too large, a method of sintering in which the atmosphere during heating is a reducing atmosphere such as nitrogen or argon may be used. When using the matrix 1 as a sintered body, the preferred crystal grain size of the matrix 1 is 50 μm or less, more preferably 10 μm or less.
[0057] Here, "grain size" refers to the "projected area circle equivalent diameter" generally referred to in microscopic observation, and refers to the diameter of a perfect circle having the same area as the projected area of a crystal grain. In the present invention, the method for measuring grain size is not particularly limited. For example, the grain size can be obtained by photographing the surface of a sample with a polarizing microscope or a scanning electron microscope, and then processing the resulting photographic image. Since the optimal magnification differs depending on the grain size of interest, an optical microscope and an electron microscope may be used separately. The circle equivalent diameter may also be obtained from an image of a polished surface or cross section of a sample, rather than from the surface.
[0058] (Heating method) In the first heating step, the second heating step and the heating step described below, the method for heating the integral body of the matrix 1 and the seed single crystal 2 is not particularly limited, but sintering using an electric furnace is preferable in that a large number of bodies can be heated at once and production costs can be reduced.
[0059] [First heating step] FIG. 5 is a schematic diagram showing a temperature increasing step in the method for producing a single crystal of the present invention. As shown in FIG. 5, the method for producing a single crystal of the present invention includes a first heating step 51 in which the temperature of the monolith is raised from room temperature to the liquid phase start temperature of the matrix.
[0060] In the first heating step 51, in which the temperature is raised to the liquid phase start temperature, crystal grains grow almost uniformly in the matrix. As described above, if the crystal grains of the matrix 1 become too large, it becomes difficult for the matrix 1 to be incorporated into the single crystal, so it is preferable to set the first heating step 51 for a short period of time so that the crystal grains do not become too large.
[0061] (atmosphere) Here, if the atmosphere during heating contains oxygen, the liquid phase spreads more easily, and large single crystals can be produced more quickly, so the atmosphere during heating preferably contains oxygen.
[0062] (Numerical limit for the first heating rate) In the method for producing a single crystal of the present invention, the temperature increase rate in the first temperature increase step 51 is preferably 100° C. or more per hour on a time average. When the average heating rate in the first heating step 51 is a time-averaged rate of 100° C. or more per hour, more preferably 150° C. or more per hour, the crystal grains in the matrix 1 do not become too large in the first heating step 51, and a single crystal consisting of a single crystal grain can be more stably spread from the seed single crystal 2.
[0063] [Second heating step] 5, the method for producing a single crystal of the present invention includes a second heating step 52 for heating the integrated body from the liquid phase start temperature to the liquid phase finish temperature of the matrix. The atmosphere is similar, so a description thereof will be omitted.
[0064] In the second heating step 52, the interface between the seed single crystal 2 and the matrix 1 becomes liquid, and the single crystal interface spreads toward the matrix 1. However, if the temperature varies depending on the location due to differences in the orientation of the crystal grains of the matrix 1 in contact with the seed single crystal 2, the interfaces of the crystal grains with different orientations in the matrix 1 also spread at the same time, and a single crystal that is a single crystal grain may not be obtained.
[0065] Therefore, by making the temperature increase rate from the liquid phase start temperature to the liquid phase end temperature in the second heating step 52 smaller than the rate from room temperature to the liquid phase start temperature in the first heating step 51, a single crystal consisting of a single crystal grain can be spread from the seed single crystal 2. After the temperature is increased, the single crystal that spreads from the seed single crystal 2 can be made even larger by maintaining the temperature at the liquid phase end temperature.
[0066] (Numerical limit for the second heating rate) In the method for producing a single crystal of the present invention, the temperature increase rate in the second temperature increase step 52 is smaller than the temperature increase rate in the first temperature increase step 51 . In the method for producing a single crystal of the present invention, the temperature increase rate in the second temperature increase step 52 is preferably 1° C. or less per hour on a time average. It is preferable that the average temperature increase rate in the second temperature increase step 52 is 1°C or less per hour on a time average, and more preferably 0.65°C or less per hour on a time average, because this makes it possible to more stably spread a single crystal consisting of a single crystal grain from the seed single crystal 2.
[0067] [Heating process] The method for producing a single crystal of the present invention includes a heating step of heating the monolith at a liquid phase finish temperature. The heating method is as described above. It is preferable that the heating step is performed successively after the second heating step, and the heating time in heating at the liquid phase finish temperature is preferably 250 to 350 hours, and more preferably about 300 hours. In this way, a single crystal with a large area can be grown.
[0068] [Step of obtaining single crystal] The method for producing a single crystal of the present invention includes a step of obtaining a perovskite-type single crystal from the integrated body after heating. After the second heating step, which regions in the matrix are single crystals can be determined by checking with a microscope whether there are grain boundaries. If there are no grain boundaries, the material is a single crystal consisting of a single crystal grain. This can also be confirmed by structural analysis using X-ray diffraction or electron beam diffraction.
[0069] The polycrystalline parts and the two seed single crystal parts other than the single crystal region can be removed using a wire saw, a dicing saw, water jet cutting, electric discharge machining, laser machining, polishing, or the like to obtain only the single crystal region.
[0070] A single crystal can also be obtained from the matrix 1 by the same method when the liquid phase finish temperature is maintained for a certain period of time after the second heating step.
[0071] The single crystal of the present invention preferably contains Ba, Ti, Zr and Mn, and by doing so, a perovskite type single crystal can be stably obtained. In particular, by containing both Zr and Mn in addition to Ba and Ti, abnormal grain growth is less likely to occur in parts other than the interface between the seed single crystal 2 and the matrix 1. If abnormal grain growth occurs in parts other than the interface between the seed single crystal 2 and the matrix 1, those parts will hinder the growth of the single crystal spreading from the interface between the seed single crystal 2 and the matrix 1.
[0072] The single crystal of the present invention is a single crystal containing Mn and a perovskite oxide containing Ba, Ti, and Zr, and preferably has a molar ratio x of Zr to the sum of Ti and Zr of 0.01≦x≦0.13 and a metal content of Mn of 0.04 parts by mass or more and 1.16 parts by mass or less per 100 parts by mass of the oxide. This makes it more difficult for abnormal grain growth to occur in areas other than the interface between the seed single crystal 2 and the matrix 1.
[0073] <Second embodiment> The second embodiment is for a single crystal. The single crystal of the present invention is A single crystal containing a perovskite-type oxide containing Ba, Ti, and Zr and Mn, x, which is a molar ratio of the Zr to the sum of the Ti and the Zr, is 0.01≦x≦0.13; The content of the Mn is 0.04 parts by mass or more and 1.16 parts by mass or less in terms of metal relative to 100 parts by mass of the oxide.
[0074] Here, the content of Mn in "metal conversion" refers to the following. The contents of each metal, Ba, Ti, Zr, and Mn, are measured from the single crystal by X-ray fluorescence analysis (XRF), ICP emission spectrometry, atomic absorption spectrometry, etc. From the contents, the elements constituting the oxide represented by the following general formula (1) are converted into oxides, and the value is calculated as the ratio of the Mn mass to the total mass of 100. Ba a (Ti 1-x ,Zr x )O3(1) The single crystal containing Mn and the perovskite oxide containing Ba, Ti, and Zr has piezoelectricity and has a high piezoelectric constant and mechanical quality factor among lead-free piezoelectric materials. The single crystal of the present invention has a small load on the environment because it does not use lead.
[0075] When using piezoelectric single crystals in resonant devices such as ultrasonic motors, they are required to have a large mechanical quality factor, which indicates the sharpness of the resonance. If the mechanical quality factor is small, the power required for operation will be high, or the piezoelectric element will heat up, making drive control difficult. For this reason, single crystals with a large mechanical quality factor are required. Furthermore, if the piezoelectric constant of a single crystal is small, the drive voltage must be large to obtain the required vibration amplitude, and increasing the drive voltage will result in a large current flowing due to the capacitance component of the material as a dielectric, resulting in higher power consumption.
[0076] The oxide represented by the general formula (1) means that the element located at the A site is Ba, and the elements located at the B site are Ti and Zr. However, some Ba may be located at the B site. Similarly, some Ti and Zr may be located at the A site. In the general formula (1), the molar ratio of the B site element to the O element is 1:3, but the ratio of the amounts of the elements may vary slightly (for example, 1.00:2.94 to 1.00:3.06).
[0077] In the single crystal of the present invention, in the general formula (1), the ratio a of the molar amount of Ba at the A site to the molar amounts of Ti and Zr at the B site is preferably in the range of 0.965≦a≦1.020.
[0078] The single crystal of the present invention preferably contains the perovskite-type oxide represented by the general formula (1) as the main component in an amount of 90 mol % or more, more preferably 95 mol % or more. If a is smaller than 0.965, many voids may occur, which may reduce the strength, whereas if a is larger than 1.020, the grain size of matrix 1 may become too large in the first heating step, which may make it difficult to expand the single crystal region during heating, which may make it difficult to produce the single crystal. The preferable range of a, in which the voids become small and the single crystal region becomes easy to expand upon heating, is 0.985≦a≦1.000.
[0079] In the general formula (1), x, which indicates the molar ratio of Zr in the B site, is in the range of 0.01≦x≦0.13. If x is greater than 0.13, the Curie temperature becomes too low and high-temperature durability becomes insufficient, and if x is less than 0.01, the piezoelectric constant at room temperature becomes small.
[0080] The Curie temperature (Tc) is the temperature at which the ferroelectricity of a material disappears. Normally, the piezoelectricity of a piezoelectric material also disappears above Tc. There are two methods for measuring Tc: directly measuring the temperature at which the ferroelectricity disappears while changing the measurement temperature, and measuring the relative dielectric constant while changing the measurement temperature using a small AC electric field, and determining the temperature at which the relative dielectric constant is maximized.
[0081] The means for measuring the composition of the single crystal of the present invention is not particularly limited. Examples of the means include X-ray fluorescence analysis, ICP emission spectrometry, atomic absorption spectrometry, etc. Any of the means can calculate the mass ratio and composition ratio of each element contained in the single crystal.
[0082] When the single crystal of the present invention contains Mn within the above range, the mechanical quality factor is improved in the room temperature region. Here, the mechanical quality factor is a coefficient that represents the elastic loss due to vibration when the piezoelectric material is evaluated as an oscillator, and the magnitude of the mechanical quality factor is observed as the sharpness of the resonance curve in impedance measurement. In other words, it is a constant that represents the sharpness of the resonance of the oscillator. Since the higher the mechanical quality factor, the less energy is lost due to vibration, and therefore, when the mechanical quality factor is improved, the power consumption is reduced when the single crystal is used as a piezoelectric element and driven by applying a voltage.
[0083] If the Mn content is less than 0.04 parts by mass, the mechanical quality factor is less than 150 in the room temperature region. If the mechanical quality factor is small, the power consumption increases when the piezoelectric element consisting of the single crystal and a pair of electrodes is driven as a resonant device. A preferable mechanical quality factor is 200 or more, more preferably 400 or more. An even more preferable mechanical quality factor is 700 or more. Within this range, an extreme increase in power consumption does not occur when the device is driven. On the other hand, if the Mn content is greater than 1.16 parts by mass, the insulation properties of the single crystal decrease. For example, the dielectric loss tangent at a frequency of 1 kHz of the single crystal may exceed 0.01, or the resistivity may fall below 1 GΩcm. The dielectric loss tangent can be measured using an impedance analyzer. If the dielectric loss tangent is 0.01 or less, stable operation can be obtained even when a high voltage is applied when the single crystal is used as a piezoelectric element. If the single crystal has a resistivity of 1 GΩcm, it can be polarized and driven as a piezoelectric element, and a more preferable resistivity is 50 GΩcm or more.
[0084] Mn is not limited to metal Mn, and may be contained in the single crystal as a Mn component, and the form of inclusion is not important. For example, it may be solid-solved in the B site, or may be contained in the interface with the voids in the single crystal. Alternatively, the Mn component may be contained in the single crystal in the form of metal, ion, oxide, metal salt, complex, etc. More preferably, Mn is present from the viewpoint of insulation and sinterability. The valence of Mn can generally be 4+, 2+, or 3+. This is because, when conductive electrons exist in the crystal (for example, when oxygen defects exist in the crystal or when a donor element occupies the A site), the valence of Mn is lowered from 4+ to 3+ or 2+, etc., trapping conductive electrons and improving insulation resistance.
[0085] On the other hand, when the valence of Mn is lower than 4+, such as 2+, Mn becomes an acceptor. When Mn exists as an acceptor in a perovskite single crystal, holes are generated in the crystal or oxygen vacancies are formed in the single crystal.
[0086] If the valence of the added Mn is 2+ or 3+, the holes cannot be compensated for by the introduction of oxygen vacancies alone, and the insulation resistance decreases. Therefore, it is preferable that the majority of Mn is 4+. However, a very small amount of Mn may have a valence lower than 4+ and occupy the B site of the perovskite structure as an acceptor, forming oxygen vacancies. This is because Mn with a valence of 2+ or 3+ and oxygen vacancies form defect dipoles, which can improve the mechanical quality factor of the single crystal. If trivalent Bi occupies the A site, Mn will tend to have a valence lower than 4+ in order to achieve charge balance.
[0087] The valence of a small amount of Mn added to a non-magnetic (diamagnetic) material can be evaluated by measuring the temperature dependence of magnetic susceptibility. Magnetic susceptibility can be measured using a superconducting quantum interference device (SQUID), a vibrating sample magnetometer (VSM), or a magnetic balance. The magnetic susceptibility χ obtained by the measurement generally follows the Curie-Weiss law, which is expressed by Equation 2. (Formula 2) χ=C / (T-θ) (C: Curie constant, θ: paramagnetic Curie temperature)
[0088] Generally, when a small amount of Mn is added to a non-magnetic material, the spin S=5 / 2 is when the valence is 2+, S=2 is when the valence is 3+, and S=3 / 2 is when the valence is 4+. Therefore, the Curie constant C converted per unit amount of Mn corresponds to the spin S value at each Mn valence. Therefore, the average valence of Mn in a sample can be evaluated by deriving the Curie constant C from the temperature dependence of the magnetic susceptibility χ.
[0089] (longest part) The single crystal of the present invention preferably has a longest portion of 1 mm or more and 100 mm or less. By setting the longest part within this range, it can be applied to a wide range of devices. If the longest part is 1 mm or more, processing becomes easy. On the other hand, if the longest part exceeds 100 mm, it takes a very long time to produce a single crystal, so it is preferable in terms of production costs that the longest part is 100 mm or less.
[0090] (Relative Density) The single crystal of the present invention preferably has a relative density of 93% or more and 100% or less. If the relative density is less than 93%, the mechanical strength may decrease.
[0091] The relative density of the piezoelectric material of the present invention is more preferably in the range of 95% to 100%, and even more preferably in the range of 97% to 100%. If the relative density is 95% or more, the material is less likely to be damaged during processing, and if it is 97% or more, chipping during cutting and polishing is reduced.
[0092] (Mechanical Quality Factor) The single crystal of the present invention preferably has a mechanical quality factor Qm of 500 or more. If the mechanical quality factor of the single crystal is 500 or more, the power required to drive it is small, and heat generation in the single crystal can be suppressed.
[0093] (Tetragonal single crystal) In the single crystal of the present invention, it is preferable that x, which is a molar ratio of Zr to the sum of the Ti and the Zr, is 0.01≦x≦0.03, a molar ratio a of Ba to the sum of the Ti and the Zr is 0.976≦a≦1.020, and the single crystal further contains Bi, and the content of Bi is 0.04 parts by mass or more and 0.53 parts by mass or less, calculated as metal, per 100 parts by mass of the oxide.
[0094] When a piezoelectric single crystal is used in a device such as an ultrasonic motor, a large coercive field indicating the withstand voltage is preferable (for example, 2.5 kV / cm or more). A single crystal with a large coercive field is less likely to deteriorate in piezoelectric performance even when driven at a high voltage.
[0095] The perovskite oxide containing Ba, Ti, and Zr and the single crystal containing Mn and Bi have large piezoelectric constants, mechanical quality factors, and coercive fields among lead-free piezoelectric materials.
[0096] In the single crystal of the present invention, the Bi content is 0.04 parts by mass or more and 0.53 parts by mass or less per mole of the metal oxide, so that trivalent Bi can occupy the A site, which makes it easier for Mn in the B site to have a valence lower than 4+ in order to achieve charge balance, thereby further enhancing the effect of Mn in improving the mechanical quality factor.
[0097] In the general formula (1), x, which indicates the molar ratio of Zr in the B site, is in the range of 0.01≦x≦0.03. When x is 0.03 or less, the single crystal is tetragonal at room temperature (25° C.), and the coercive field is large and the voltage resistance is excellent. When x is 0.01 or more, a high piezoelectric constant is obtained at room temperature (25° C.).
[0098] When the single crystal of the present invention contains 0.002 to 0.050 moles of Mn per mole of the metal oxide, the coercive field increases at room temperature, 25° C. As described above, when Mn with a valence of 2+ or 3+ forms a defect dipole with an oxygen vacancy to generate an internal electric field, the internal electric field prevents the reversal of polarization due to an external electric field, improving the coercive field.
[0099] <Application Examples> An application example of the present invention will be described below. (Piezoelectric element) The piezoelectric element of the present invention has a plurality of electrodes and the above-mentioned single crystal. 6 is a schematic diagram showing one embodiment of the configuration of a piezoelectric element of the present invention. The piezoelectric element of the present invention is a piezoelectric element having at least a first electrode 11, a single crystal portion 22, and a second electrode 33, and is characterized in that the single crystal portion 22 is the single crystal of the present invention.
[0100] The single crystal according to the present invention can be used to evaluate the piezoelectric constant by forming it into a piezoelectric element having at least a first electrode 11 and a second electrode 33. The first electrode 11 and the second electrode 33 are made of conductive layers having a thickness of about 5 nm to 10 μm. The material is not particularly limited, and may be any material that is commonly used in piezoelectric elements. For example, metals such as Ti, Pt, Ta, Ir, Sr, In, Sn, Au, Al, Fe, Cr, Ni, Pd, Ag, and Cu, alloys, and compounds thereof can be mentioned.
[0101] The first electrode 11 and the second electrode 33 may be made of one of these materials, or may be made by laminating two or more of these materials. The first electrode 11 and the second electrode 33 may be made of different materials.
[0102] The manufacturing method of the first electrode 11 and the second electrode 33 is not limited, and they may be formed by baking a metal paste, or by sputtering, vapor deposition, etc. In addition, both the first electrode 11 and the second electrode 33 may be patterned into a desired shape before use.
[0103] (Polarization treatment) It is more preferable that the polarization axis of the piezoelectric element is aligned in a certain direction, since the polarization axis is aligned in a certain direction, the piezoelectric constant of the piezoelectric element is large.
[0104] The method of polarization of the piezoelectric element is not particularly limited. The polarization process may be performed in air or in silicone oil. The temperature during polarization is preferably a temperature at which the single crystal undergoes phase transition. For example, a temperature of 60°C to 150°C is preferable, but the optimal conditions vary somewhat depending on the composition of the single crystal constituting the element. The electric field applied for polarization is preferably 8 kV / cm to 20 kV / cm, and it is preferable to end the application of the electric field after lowering the environmental temperature to a temperature at which the single crystal has the same crystal structure as at room temperature, in order to obtain a good piezoelectric constant.
[0105] The piezoelectric element according to the present invention also includes a laminated piezoelectric element in which a number of single crystals of the present invention are laminated, or a number of piezoelectric elements are laminated to form a rod-like shape and the displacement in the thickness direction is utilized.
[0106] (Ultrasonic motor) The ultrasonic motor of the present invention has a vibrating body with the above-mentioned piezoelectric element and a moving body in contact with the vibrating body. In this way, an ultrasonic motor having driving efficiency equal to or higher than that of a piezoelectric element containing lead can be provided. Figure 7 is a schematic diagram showing one embodiment of the configuration of the ultrasonic motor of the present invention. Figure 7 shows an ultrasonic motor in which the piezoelectric element of the present invention is made of a single plate. The ultrasonic motor includes a vibrator 201, a rotor 202 that is in contact with the sliding surface of the vibrator 201 by the pressure of a pressure spring (not shown), and an output shaft 203 that is integral with the rotor 202. The vibrator 201 is composed of a metal elastic ring 2011, a piezoelectric element 2012 of the present invention, and an organic adhesive 2013 (epoxy, cyanoacrylate, etc.) that bonds the piezoelectric element 2012 to the elastic ring 2011. The piezoelectric element 2012 of the present invention is composed of a single crystal sandwiched between a first electrode 11 and a second electrode 33 (not shown). When a two-phase alternating voltage with a phase difference of an odd multiple of π / 2 is applied to the piezoelectric element of the present invention, a bending traveling wave is generated in the vibrator 201, and each point on the sliding surface of the vibrator 201 performs an elliptical motion. When the rotor 202 is pressed against the sliding surface of the vibrator 201, the rotor 202 receives a frictional force from the vibrator 201 and rotates in the opposite direction to the bending traveling wave. The driven body (not shown) is joined to the output shaft 203 and is driven by the rotational force of the rotor 202. When a voltage is applied to the single crystal, it expands and contracts due to the piezoelectric transverse effect. The efficiency of this conversion from electrical energy to mechanical energy depends on the magnitude of the electromechanical coupling coefficient. When an elastic body such as metal is bonded to the piezoelectric element with an adhesive or the like, the elastic body is bent by the expansion and contraction of the single crystal via the adhesive. The type of ultrasonic motor described here utilizes this principle.
[0107] (optical equipment) The optical device of the present invention includes the ultrasonic motor described above in a driving section, and thus it is possible to provide an optical device having an operating speed and operating efficiency equal to or greater than those of a piezoelectric element containing lead.
[0108] Figures 8A and 8B are cross-sectional views of the main parts of an interchangeable lens barrel for a single-lens reflex camera, which is an example of a preferred embodiment of the optical apparatus of the present invention. Also, Figure 9 is an exploded perspective view of an interchangeable lens barrel for a single-lens reflex camera, which is an example of a preferred embodiment of the optical apparatus of the present invention. Fixed barrel 712, linear guide barrel 713, and front group barrel 714 are fixed to a detachable mount 711 for the camera. These are fixed members of the interchangeable lens barrel.
[0109] A linear guide groove 713a in the optical axis direction for the focus lens 702 is formed in the linear guide barrel 713. Cam rollers 717a, 717b protruding radially outward are fixed to a rear group barrel 716 holding the focus lens 702 by shaft screws 718, and the cam roller 717a fits into the linear guide groove 713a.
[0110] A cam ring 715 is rotatably fitted on the inner periphery of the linear guide barrel 713. The relative movement between the linear guide barrel 713 and the cam ring 715 in the optical axis direction is restricted by a roller 719 fixed to the cam ring 715 fitting into a circumferential groove 713b of the linear guide barrel 713. A cam groove 715a for the focus lens 702 is formed in this cam ring 715, and the above-mentioned cam roller 717b is fitted into the cam groove 715a at the same time.
[0111] A rotation transmission ring 720 is disposed on the outer periphery of the fixed barrel 712, and is held by a ball race 727 so as to be rotatable at a fixed position relative to the fixed barrel 712. In the rotation transmission ring 720, rollers 722 are rotatably held on shafts 720f extending radially from the rotation transmission ring 720, and large diameter portions 722a of the rollers 722 are in contact with a mount side end face 724b of the manual focus ring 724. In addition, small diameter portions 722b of the rollers 722 are in contact with a joining member 729. Six rollers 722 are disposed at equal intervals on the outer periphery of the rotation transmission ring 720, and each roller is configured as described above.
[0112] A low-friction sheet (washer member) 733 is disposed on the inner diameter portion of the manual focus ring 724, and this low-friction sheet is sandwiched between a mount side end face 712a of the fixed barrel 712 and a front end face 724a of the manual focus ring 724. The outer diameter surface of the low-friction sheet 733 is ring-shaped and radially fits into an inner diameter 724c of the manual focus ring 724, which in turn radially fits into an outer diameter portion 712b of the fixed barrel 712. The low-friction sheet 733 serves to reduce friction in a rotating ring mechanism in which the manual focus ring 724 rotates relatively to the fixed barrel 712 around the optical axis.
[0113] The large diameter portion 722a of the roller 722 and the mount side end surface 724b of the manual focus ring are in contact with each other under a pressure applied thereto by the force of the wave washer 726 pressing the ultrasonic motor 725 toward the front of the lens. Similarly, the small diameter portion 722b of the roller 722 and the joining member 729 are in contact with each other under a moderate pressure applied thereto by the force of the wave washer 726 pressing the ultrasonic motor 725 toward the front of the lens. The movement of the wave washer 726 in the mount direction is restricted by a washer 732 bayonet-coupled to the fixed barrel 712, and the spring force (biasing force) generated by the wave washer 726 is transmitted to the ultrasonic motor 725 and further to the roller 722, and also serves as a pressing force of the manual focus ring 724 against the mount side end surface 712a of the fixed barrel 712. In other words, the manual focus ring 724 is assembled in a state where it is pressed against the mount side end surface 712 a of the fixed barrel 712 via the low friction sheet 733 .
[0114] Therefore, when the ultrasonic motor 725 is driven to rotate relative to the fixed cylinder 712 by a control unit (not shown), the joining member 729 is in frictional contact with the small diameter portion 722b of the roller 722, so that the roller 722 rotates around the center of the shaft 720f. When the roller 722 rotates around the shaft 720f, the rotation transmission ring 720 rotates around the optical axis (autofocus operation).
[0115] Furthermore, when a rotational force about the optical axis is applied to the manual focus ring 724 from a manual operation input unit (not shown), the mount side end face 724b of the manual focus ring 724 is in pressure contact with the large diameter portion 722a of the roller 722, so that the roller 722 rotates about the axis 720f due to frictional force. When the large diameter portion 722a of the roller 722 rotates about the axis 720f, the rotation transmission ring 720 rotates about the optical axis. At this time, the ultrasonic motor 725 does not rotate due to the frictional holding force between the rotor 725c and the stator 725b (manual focus operation).
[0116] Two focus keys 728 are attached to the rotation transmission ring 720 at positions facing each other, and the focus keys 728 fit into notches 715b provided at the tip of the cam ring 715. Therefore, when an autofocus operation or a manual focus operation is performed and the rotation transmission ring 720 is rotated around the optical axis, the rotational force is transmitted to the cam ring 715 via the focus keys 728. When the cam ring is rotated around the optical axis, the rear group barrel 716, whose rotation is restricted by the cam rollers 717a and the linear guide grooves 713a, advances and retreats along the cam grooves 715a of the cam ring 715 by the cam rollers 717b. This drives the focus lens 702 and performs the focus operation.
[0117] Here, we have described an interchangeable lens barrel for a single-lens reflex camera as the optical device of the present invention, but the present invention can be applied to optical devices that have an ultrasonic motor in the drive section, regardless of the type of camera, such as compact cameras, electronic still cameras, and camera-equipped portable information terminals.
[0118] (Vibration device and dust removal device) The vibration device of the present invention has a vibrating body with the above-mentioned piezoelectric element disposed on a diaphragm, thereby providing a vibration device having vibration capabilities equal to or greater than those of a piezoelectric element containing lead. Vibration devices, which are used for transporting and removing particles, powders, and liquid droplets, are widely used in electronic devices and the like.
[0119] As an example of the vibration device of the present invention, a dust removing device using the vibration device of the present invention will be described below.
[0120] The dust removing device according to the present invention has a vibration device in a vibration section, and thus it is possible to provide a dust removing device having dust removing efficiency equal to or higher than that of a dust removing device using a piezoelectric element containing lead.
[0121] 10A and 10B are schematic diagrams showing one embodiment of a dust removal device of the present invention. Dust removal device 310 is composed of a plate-shaped piezoelectric element 330 and a vibration plate 320. The material of vibration plate 320 is not limited, but when dust removal device 310 is used in an optical device, a light-transmitting material or a light-reflective material can be used for vibration plate 320.
[0122] Figures 11A to 11C are schematic diagrams showing the configuration of piezoelectric element 330 in Figures 10A and 10B. Figures 11A and 11C show the configuration of the front and back surfaces of piezoelectric element 330, and Figure 11B shows the configuration of the side surface. As shown in Figure 10A, piezoelectric element 330 is composed of single crystal 331, first electrode 332, and second electrode 333, and first electrode 332 and second electrode 333 are arranged to face the plate surface of single crystal 331.
[0123] In FIG. 11B, the surface on which first electrode 332 protruding in front of piezoelectric element 330 is provided is referred to as first electrode surface 336, and in FIG. 11A, the surface on which second electrode 333 protruding in front of piezoelectric element 330 is provided is referred to as second electrode surface 337.
[0124] Here, the electrode surface in the present invention refers to the surface of the piezoelectric element on which the electrode is disposed. For example, the first electrode 332 may extend around the second electrode surface 337 as shown in FIGS. 11A and 11B.
[0125] 10A and 10B, the piezoelectric element 330 and the diaphragm 320 are fixed to the plate surface of the diaphragm 320 by a first electrode surface 336 of the piezoelectric element 330. Then, by driving the piezoelectric element 330, stress is generated between the piezoelectric element 330 and the diaphragm 320, and out-of-plane vibration is generated in the diaphragm. The dust removal device 310 of the present invention is a device that removes foreign matter such as dust attached to the surface of the diaphragm 320 by the out-of-plane vibration of the diaphragm 320. The out-of-plane vibration means an elastic vibration that displaces the diaphragm in the optical axis direction, that is, in the thickness direction of the diaphragm.
[0126] 12A and 12B are schematic diagrams showing the vibration principle of dust removal device 310 of the present invention. Fig. 12A shows a state in which in-phase alternating voltages are applied to a pair of left and right piezoelectric elements 330 to generate out-of-plane vibration in vibration plate 320. The polarization direction of the single crystals constituting the pair of left and right piezoelectric elements 330 is the same as the thickness direction of piezoelectric elements 330, and dust removal device 310 is driven in a seventh vibration mode. Fig. 12B shows a state in which out-of-plane vibration is generated in vibration plate 320 by applying anti-phase alternating voltages, which are 180° out of phase, to a pair of left and right piezoelectric elements 330. Dust removal device 310 is driven in a sixth vibration mode. Dust removal device 310 of the present invention is a device that can effectively remove dust adhering to the surface of the diaphragm by selectively using at least two vibration modes.
[0127] (Imaging device) An imaging apparatus of the present invention includes at least the above-described dust removal device and an imaging element unit, and the diaphragm of the above-described dust removal device is provided on the light receiving surface side of the imaging element unit. In this way, it is possible to provide an imaging device having a dust removal function equal to or better than that of a device using a piezoelectric element containing lead. Figures 13 and 14 are diagrams showing a digital single-lens reflex camera as an example of a preferred embodiment of the imaging device of the present invention.
[0128] Fig. 13 is a front perspective view of the camera body 601 as viewed from the subject side, with the photographing lens unit removed. Fig. 14 is an exploded perspective view showing a schematic configuration inside the camera, for explaining the peripheral structure of the dust removal device and the imaging unit 400 of the present invention.
[0129] A mirror box 605 to which a photographing light beam that has passed through a photographing lens is provided within the camera body 601, and a main mirror (quick return mirror) 606 is disposed within the mirror box 605. The main mirror 606 can be held at an angle of 45° with respect to the photographing optical axis in order to guide the photographing light beam in the direction of a pentagonal roof mirror (not shown), or held at a position retracted from the photographing light beam in order to guide it in the direction of an image sensor (not shown).
[0130] A mirror box 605 and a shutter unit 200 are arranged, in that order from the subject side, on the subject side of the main body chassis 300, which forms the framework of the camera body. In addition, an imaging unit 400 is arranged on the photographer side of the main body chassis 300. The imaging unit 400 is installed such that the imaging surface of the imaging element is spaced a predetermined distance from and adjusted to be parallel to the attachment surface of a mount section 602, which serves as a reference for attaching a photographing lens unit.
[0131] Here, a digital single-lens reflex camera has been described as the imaging device of the present invention, but the imaging device may be a camera with an interchangeable lens unit, such as a mirrorless digital single-lens camera that does not have a mirror box 605. The imaging device may also be applied to a video camera with an interchangeable lens unit, a copier, a facsimile, a scanner, or any other imaging device or electronic device equipped with an imaging device, particularly an apparatus that requires the removal of dust adhering to the surface of an optical component. The imaging unit 400 may be applied as the imaging element unit of the present invention.
[0132] (Ultrasound probe) The ultrasonic probe of the present invention has the above-mentioned piezoelectric element and transmits and receives by the piezoelectric element. By doing so, it is possible to provide an ultrasonic probe having transmission and reception performance equal to or better than that of a piezoelectric element containing lead.
[0133] FIG. 15 is a schematic cross-sectional view showing one embodiment of the ultrasonic probe of the present invention. The ultrasonic probe 1100 in Fig. 15 is composed of a piezoelectric element 1101, a backing material 1102, an acoustic matching layer 1103, and an acoustic lens 1104. As shown in Fig. 15, a plurality of piezoelectric elements 1101 are arranged and bonded on the backing material 1102, and an acoustic matching layer 1103 for matching acoustic impedance is provided on the opposite surface, which serves as the transmitting and receiving surface.
[0134] Acoustic matching layer 1103 may be a single layer or multiple layers, and preferably is two or more layers. Materials that can be used for acoustic matching layer 1103 include, for example, carbon, aluminum, aluminum alloy (e.g., AL-Mg alloy), magnesium alloy, Macol glass, glass, fused quartz, copper graphite, polyethylene, polypropylene, polycarbonate, ABC resin, polyphenylene ether, ABS resin, AAS resin, AES resin, nylon, polyamide-imide, polyethylene terephthalate, polycarbonate, epoxy resin, urethane resin, etc.
[0135] In addition, the backing material 1102 can be made of thermoplastic resins such as natural rubber, ferrite rubber, epoxy resin, vinyl chloride, polyvinyl butyral, ABS resin, polyurethane, polyvinyl alcohol, polyethylene, polypropylene, polyacetal, polyethylene terephthalate, fluororesin, polyethylene glycol, and polyethylene terephthalate, or these mixed with metal powder, or a super-hard material such as tungsten carbide.
[0136] The piezoelectric element 1101 may be one piece, or may be divided into several pieces. Fig. 15 shows an example in which the piezoelectric element is divided. A flexible cable (not shown) is connected to the electrodes of each piezoelectric element, allowing signals to be transmitted and received by the piezoelectric element to be input and output. Acoustic lens 1104 is bonded to acoustic matching layer 1103. Acoustic lens 1104 is a member for converging ultrasonic waves transmitted from piezoelectric element 1101 toward the subject, and has an arc shape in the example of Fig. 15. Note that, as a material for acoustic lens 1104, rubber containing silicone resin (rubber) as a main component is generally used.
[0137] When using this ultrasonic probe 1100, an alternating voltage is applied to the piezoelectric element 1101 through a flexible cable, and the piezoelectric element is vibrated by the piezoelectric effect, causing the piezoelectric element 1101 to transmit ultrasonic waves. At this time, if the acoustic impedance of the subject on which the ultrasonic waves are applied is small, or if the ultrasonic waves are applied to the subject through water or air, the presence of the acoustic matching layer 1103 makes it possible to suppress reflected waves caused by large changes in acoustic impedance, and the ultrasonic waves can be efficiently irradiated to the subject. Then, at the time of reception, the piezoelectric element 1101 vibrates due to the ultrasonic waves reflected from inside the subject, and this vibration is electrically converted by the piezoelectric effect to obtain a received signal. At the time of transmission and reception, conversion between electrical energy and mechanical energy is performed, and the conversion efficiency at this time depends on the magnitude of the electromechanical coupling coefficient.
[0138] (Ultrasound diagnostic equipment) The ultrasonic diagnostic device of the present invention has at least the ultrasonic probe and an image output unit (also referred to as an image display unit). In this way, an ultrasonic diagnostic device having a driving efficiency equal to or higher than that of a piezoelectric element containing lead can be provided. FIG. 16 is a schematic diagram showing one embodiment of the ultrasonic diagnostic device of the present invention. The ultrasonic diagnostic device 1110 of FIG. 16 is composed of an ultrasonic probe 1100, a cable 1111, a drive control unit 1113, an image display unit 1112, and an image processing unit 1114. The flexible cable of the ultrasonic probe 1100 and the drive control unit 1113 are connected by a cable 1111, and an alternating voltage is applied from the drive control unit 1113 to the piezoelectric element 1101 of the ultrasonic probe 1100 via the cable 1111. When ultrasonic waves are irradiated from the ultrasonic probe 1100 into the subject, ultrasonic waves reflected from inside the subject are converted into electrical signals again by the ultrasonic probe and input to the image processing unit 1114 through the cable 1111. The image processing unit 1114 creates image data by performing calculations based on changes in delay time and signal intensity relative to the alternating voltage output from the drive control unit 1113. The created image data is output to the image display unit 1112.
[0139] (Ultrasound diagnostic system) The ultrasonic diagnostic system of the present invention includes the ultrasonic probe described above, a transmitting unit that transmits a signal output from the ultrasonic probe described above, and a receiving unit that receives a signal transmitted from the transmitting unit. In this way, an ultrasonic diagnostic system having a driving efficiency equal to or higher than that of a piezoelectric element containing lead can be provided. FIG. 17 and FIG. 18 are schematic diagrams showing an embodiment of the ultrasonic diagnostic system of the present invention. In the ultrasonic diagnostic system 1120 of FIG. 17, a signal obtained by the ultrasonic probe is transmitted from a transmitting unit 1121, and the signal is received by a receiving unit 1122. Image data is created from the received signal by an image processing unit 1114, and is output by an image display unit 1112. The distance between the transmitting unit 1121 and the receiving unit 1122 may be far. The means for transmission and reception may be wireless communication such as Wi-Fi (registered trademark) or Bluetooth (registered trademark), or may be via a network line by connecting a network cable. 18, image data is created from the output signal by image processing unit 1114, and the data is transmitted as a signal from transmission unit 1121, and the signal is received by reception unit 1122. The received signal is output by image display unit 1112.
[0140] (electronic equipment) Next, the electronic device of the present invention will be described. The electronic device of the present invention is provided with a piezoelectric acoustic component having the above-mentioned piezoelectric element or the above-mentioned laminated piezoelectric element. In this way, it is possible to provide an electronic device that has sound generation properties equal to or better than those of a piezoelectric element containing lead. Piezoelectric acoustic components include speakers, buzzers, microphones, and surface acoustic wave (SAW) elements.
[0141] 19 is an overall perspective view seen from the front of a digital camera body 931, which is an example of a preferred embodiment of an electronic device of the present invention. On the front of body 931, optical device 901, microphone 914, strobe light emission unit 909, and fill light unit 916 are arranged. Microphone 914 is shown by a dashed line as it is built into the body. A hole is provided in front of microphone 914 to pick up sound from the outside.
[0142] A power button 933, a speaker 912, a zoom lever 932, and a release button 908 for performing a focusing operation are arranged on the top surface of the main body 931. The speaker 912 is incorporated inside the main body 931 and is indicated by a dashed line. A hole is provided in front of the speaker 912 to transmit sound to the outside.
[0143] The piezoelectric acoustic component of the present invention is used in at least one of the microphone 914, the speaker 912, and the surface acoustic wave element.
[0144] Here, a digital camera has been described as an example of the electronic device of the present invention, but the electronic device of the present invention can also be applied to electronic devices having various piezoelectric acoustic components, such as audio playback devices, audio recording devices, mobile phones, and information terminals.
[0145] As described above, the piezoelectric element of the present invention is suitable for use in ultrasonic motors, optical instruments, vibration devices, dust removal devices, imaging devices, ultrasonic probes, ultrasonic diagnostic devices and electronic devices.
[0146] In addition to the above-mentioned devices, the single crystal and piezoelectric element of the present invention can be used in devices such as motors, liquid discharge heads, liquid discharge apparatuses, piezoelectric actuators, piezoelectric sensors, and ferroelectric memories. EXAMPLES
[0147] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The single crystal and piezoelectric element of the present invention were produced by the method described below.
[0148] Example 1 The raw powders used were barium titanate (BaTiO3, Ba / Ti=0.999) with an average particle size of 100 nm, barium zirconate (BaZrO3, Ba / Zr=1.002), trimanganese tetroxide (Mn3O4), and titanium oxide to adjust the ratio a of the sum of the moles of Ti and Zr to the sum of the moles of Ba. These raw powders were mixed together with titanium and barium as the main components in the composition formula Ba0.985 (Ti 0.93 ,Zr 0.07 )O3 ratio. Mn was added so that the content was 0.12 parts by mass in terms of metal per 100 parts by mass of this oxide. Furthermore, this oxide to which Mn was added was mixed by dry mixing for 24 hours using a ball mill. In order to granulate the obtained mixed powder, 3 parts by mass of PVA binder was attached to the surface of the mixed powder using a spray dryer device.
[0149] Next, the obtained granulated powder was filled into a metal mold with a mirror-finished surface on the sample side, and a molding pressure of 200 MPa was applied using a press molding machine to produce two rectangular parallelepiped molded bodies. These molded bodies may be further compressed using a cold isostatic pressing machine.
[0150] Next, one of the above molded bodies was placed on a microscope heating stage (manufactured by LINKAM) and heated, and the surface of matrix 1 was observed under a microscope.The liquid phase start temperature was 1320°C and the liquid phase end temperature was 1385°C.
[0151] Next, the other molded body was placed in an electric furnace and held at a maximum temperature of 1300°C for 5 hours, and then sintered in air for a total of 24 hours to obtain a rectangular solid matrix measuring 12 mm x 18 mm x 1.3 mm.
[0152] The average equivalent circle diameter (based on JIS R1670) and relative density of the crystal grains constituting the obtained matrix 1 were evaluated. As a result, the average equivalent circle diameter was 4 μm and the relative density was 98%. A polarizing microscope was mainly used to observe the crystal grains. A scanning electron microscope (SEM) was used to identify the grain size of small crystal grains. The average equivalent circle diameter was calculated from the observation results. As mentioned above, the relative density is the measured density relative to the theoretical density. The theoretical density was calculated from the lattice constant and the weighed composition obtained from X-ray diffraction, and the measured density was evaluated using the Archimedes method.
[0153] Next, both sides of the obtained rectangular solid-shaped matrix were polished using a polishing machine while changing the grit size of the abrasive grains so that the thickness became 1.0 mm, and finally, chemical polishing was performed as a finishing step to obtain a mirror surface.
[0154] Next, a zirconia-coated alumina sagger was prepared as the sagger 7, a zirconia setter as the setter 6, a zirconia setter (size 50 mm x 50 mm x 1 mm, weight 20 g) as the weight 4, and zirconia beads as the beads 5. These were then arranged as shown in Figure 3, and placed in an electric furnace with the lid 8 closed as shown in Figure 4, and heated.
[0155] The seed single crystal 2 used here was a 10 mm x 10 mm x 1 mm BaTiO3 (manufactured by Physcience Opto-electronics) substrate with both the main surface and side surface being (100) planes, and both surfaces were mirror polished.
[0156] As shown in Fig. 5, the heating profile during heating was as follows: in the first heating step 51, the temperature was raised from room temperature to the liquid phase start temperature of 1320°C over 8.8 hours at a heating rate of 150°C / h, and then in the second heating step 52, the temperature was raised from 1320°C to the liquid phase end temperature of 1385°C over 100 hours at a heating rate of 0.65°C / h. Then, in the heating step, the temperature was held at 1385°C for 300 hours, and finally, the temperature was lowered to room temperature by natural cooling. The first heating step 51 and the second heating step 52 were performed in the air.
[0157] Figure 20 shows the matrix 1 after heating, from which it can be seen that the single crystal growth portion 3 has spread out from the seed single crystal 2. When the matrix after heating was observed with an optical microscope, it was confirmed that the single crystal growth portion 3 (the region spreading out from the seed single crystal) was a single crystal without grain boundaries.
[0158] Next, the seed single crystal 2 portion was removed by polishing, and the single crystal portion was cut out with a dicing saw to obtain a single crystal. The longest portion of the obtained single crystal was 17 mm.
[0159] Next, the crystal structure of the polished single crystal was analyzed by X-ray diffraction. As a result, only peaks corresponding to the perovskite type (100) oriented single crystal were observed. In addition, the relative density of the obtained single crystal was measured and found to be 97%.
[0160] Next, the composition of the obtained single crystal was evaluated by ICP emission spectroscopy. The results are shown in Table 1. As a result, the weighed composition of Ba, Ti, Zr, and Mn was consistent with the composition after heating.
[0161] Next, gold electrodes with a thickness of 400 nm were formed on both main surfaces of the single crystal by DC sputtering, and a titanium film with a thickness of 30 nm was formed between the electrodes and the single crystal as an adhesive layer. The single crystal with electrodes was cut to a size of 10 mm x 2.5 mm x 0.5 mm so that the long sides were in the 45° direction, i.e., the (100) plane was the top and bottom faces and the (110) plane was the side faces, to produce a rectangular piezoelectric element of the present invention. The obtained piezoelectric element was subjected to polarization treatment by setting the surface of a hot plate to 60°C to 100°C and applying an electric field of 1 kV / mm on the hot plate for 30 minutes.
[0162] Next, as the static characteristics of the piezoelectric element having the single crystal of the present invention, the piezoelectric constant d 31 The mechanical quality factor Qm was evaluated by the resonance-antiresonance method at room temperature (25°C) using an impedance analyzer (4294A manufactured by Agilent Technologies). The results are shown in Table 2. The resonance-antiresonance method is a method in which the resonance frequency and antiresonance frequency are measured using an impedance analyzer, and the measurement results are used to calculate the quality factor Qm based on the Japan Electronics and Information Technology Industries Association standard (JEITA EM-4501).
[0163] Next, the coercive electric field of the piezoelectric element was evaluated. Using a ferroelectric / piezoelectric evaluation system (LCII manufactured by RADIANT TECHNOLOGIES. INC.), the electric field at the time of zero polarization was read from the PE hysteresis curve obtained from the polarization amount against the electric field, and this value was taken as the coercive electric field. The coercive electric field at this time was 1.6 kV / cm.
[0164] Next, the power consumption of the rectangular piezoelectric element was evaluated. The power consumption was measured with a power meter when an alternating voltage was applied and the magnitude and frequency of the alternating voltage were changed so that the displacement was 1.0 μm. The displacement was measured with a laser Doppler vibrometer. The power consumption in this case was 16 mW.
[0165] Example 2 As shown in Table 1, a single crystal and a piezoelectric element of the present invention were obtained in the same manner as in Example 1, except that the molded body was used as Matrix 1. Next, in the same manner as in Example 1, the composition, the longest part, the relative density, and the piezoelectric constant d 31 The mechanical quality factor Qm and power consumption were evaluated. The results are shown in Tables 1 and 2.
[0166] Example 3 As shown in Table 1, the molded body was used as the matrix 1 and (Ba 0.78 Ca 0.22 A single crystal and a piezoelectric element of the present invention were obtained in the same manner as in Example 1, except that TiO3 was used. Seed single crystal 2 (Ba 0.78 Ca 0.22 ) The TiO3 used was prepared by the floating zone method. Next, in the same manner as in Example 1, the composition, the longest part, the relative density, and the piezoelectric constant d 31 The mechanical quality factor Qm and power consumption were evaluated. The results are shown in Tables 1 and 2.
[0167] Example 4 As shown in Table 1, the molded body was used as the matrix 1 and Ba was used as the seed single crystal 2.0.990 (Ti 0.93 Zr 0.07 A single crystal and a piezoelectric element of the present invention were obtained in the same manner as in Example 1, except that 03 was used. Seed single crystal 2: Ba 0.990 (Ti 0.93 Zr 0.07 )O3 was prepared by the same process as in Example 1, and was obtained by cutting out a single crystal portion that had expanded from a seed single crystal portion. Here, this single crystal was used as the seed single crystal. Next, in the same manner as in Example 1, the composition, the longest part, the relative density, and the piezoelectric constant d 31 The mechanical quality factor Qm and power consumption were evaluated. The results are shown in Tables 1 and 2.
[0168] (Examples 5 and 6) As shown in Table 1, the single crystal and piezoelectric element of the present invention were obtained in the same manner as in Example 1, except that the molded body was used as matrix 1 and the first heating rate or the second heating rate was changed. Next, in the same manner as in Example 1, the composition, the longest part, the relative density, and the piezoelectric constant d 31 The mechanical quality factor Qm and power consumption were evaluated. The results are shown in Tables 1 and 2.
[0169] (Examples 7 to 12) As shown in Table 1, the single crystal and piezoelectric element of the present invention were obtained by the same process as in Example 1, except that the molded body was used as Matrix 1 and the amounts of barium titanate, barium zirconate, trimanganese tetroxide, and titanium oxide added were changed. Next, in the same manner as in Example 1, the composition, the longest part, the relative density, and the piezoelectric constant d 31 The mechanical quality factor Qm and power consumption were evaluated. The results are shown in Tables 1 and 2.
[0170] (Examples 13 to 17) As shown in Table 1, a single crystal and a piezoelectric element of the present invention were obtained in the same manner as in Example 1, except that the molded body was used as Matrix 1, the amounts of barium titanate, barium zirconate, trimanganese tetroxide, and titanium oxide added were changed, and dibismuth trioxide was added. Next, in the same manner as in Example 1, the composition, the longest part, the relative density, and the piezoelectric constant d 31 The mechanical quality factor Qm and power consumption were evaluated. The results are shown in Tables 1 and 2.
[0171] Comparative Example 1 The raw powders used were barium titanate (BaTiO3, Ba / Ti=0.999) with an average particle size of 100 nm, barium zirconate (BaZrO3, Ba / Zr=1.002), trimanganese tetroxide (Mn3O4), and titanium oxide to adjust the ratio a of the sum of the moles of Ti and Zr to the sum of the moles of Ba. These raw powders were mixed together with titanium and barium as the main components in the composition formula Ba 0.985 (Ti 0.93 ,Zr 0.07 )O3 ratio. Mn was added so that the content was 0.12 parts by mass in terms of metal per 100 parts by mass of this metal oxide. Furthermore, this oxide to which Mn was added was mixed by dry mixing for 24 hours using a ball mill. In order to granulate the obtained mixed powder, 3 parts by mass of PVA binder was attached to the surface of the mixed powder using a spray dryer device.
[0172] Next, the obtained granulated powder was filled into a metal mold with a mirror-finished surface on the sample side, and a molding pressure of 200 MPa was applied using a press molding machine to produce two rectangular parallelepiped molded bodies. These molded bodies may be further compressed using a cold isostatic pressing machine.
[0173] Next, one of the above molded bodies was placed on a microscope heating stage (manufactured by LINKAM) and heated, and the surface of matrix 1 was observed under a microscope.The liquid phase start temperature was 1320°C and the liquid phase end temperature was 1385°C.
[0174] Next, the other molded body was placed in an electric furnace and held at a maximum temperature of 1300°C for 5 hours, and then sintered in an air atmosphere for a total of 24 hours to obtain a rectangular solid matrix 1 having dimensions of 12 mm x 18 mm x 1.3 mm.
[0175] The average equivalent circular diameter and relative density of the crystal grains constituting the obtained matrix 1 were evaluated. As a result, the average equivalent circular diameter was 4 μm and the relative density was 98%. A polarizing microscope was mainly used to observe the crystal grains. A scanning electron microscope (SEM) was used to identify the grain size of small crystal grains. The average equivalent circular diameter was calculated from the observation results. The relative density was evaluated using the theoretical density calculated from the lattice constant obtained from X-ray diffraction and the weighed composition, and the actual density measured by the Archimedes method.
[0176] Next, both sides of the obtained rectangular solid matrix 1 were polished using a polishing machine while changing the grit size of the abrasive grains so that the thickness became 1.0 mm, and finally, chemical polishing was performed as a finishing step to obtain a mirror surface.
[0177] Next, a zirconia-coated alumina sagger was prepared as the sagger 7, a zirconia setter as the setter 6, a zirconia setter (size 50 mm x 50 mm x 1 mm, weight 20 g) as the weight 4, and zirconia beads as the beads 5. These were then arranged as shown in Figure 3, and placed in an electric furnace with the lid on as shown in Figure 4, and heated.
[0178] The seed single crystal 2 used here was a 10 mm x 10 mm x 1 mm BaTiO3 (manufactured by Physcience Opto-electronics) substrate with the top, bottom and side surfaces all being (100) planes, and both surfaces were mirror polished.
[0179] The heating profile was as follows: the temperature was raised from room temperature to the liquid phase start temperature of 1320°C over 8.8 hours at a rate of 150°C / h, and then the temperature was raised from 1320°C to the liquid phase end temperature of 1385°C at the same rate of 150°C / h. The temperature was then held at 1385°C for 300 hours, and finally cooled to room temperature.
[0180] In the matrix after heating, no region in which the single crystal portion spreads from the seed single crystal was observed, and a single crystal could not be obtained.
[0181] Comparative Example 2 As shown in Table 1, the same steps as in Comparative Example 1 were carried out, except that the first temperature increase rate and the second temperature increase rate were changed. In the matrix 1 after heating, no region in which the single crystal portion spreads from the seed single crystal was observed, and a single crystal could not be obtained.
[0182] Comparative Example 3 As shown in Table 1, the same steps as in Comparative Example 1 were carried out, except for changing the amounts of barium titanate, barium zirconate, trimanganese tetroxide, and titanium oxide added, and adding dibismuth trioxide. In the matrix 1 after heating, no region in which the single crystal portion spreads from the seed single crystal was observed, and a single crystal could not be obtained.
[0183] Comparative Example 4 The raw powders were barium titanate (BaTiO3, Ba / Ti = 0.999) with an average particle size of 100 nm, barium zirconate (BaZrO3, Ba / Zr = 1.002), and titanium oxide was used to adjust the ratio a of the sum of the moles of Ti and Zr to the sum of the moles of Ba. These raw powders were treated with the composition formula Ba 0.985 (Ti 0.93 ,Zr 0.07 The powders were mixed by dry mixing for 24 hours using a ball mill. To granulate the resulting mixed powder, 3 parts by mass of PVA binder was attached to the surface of the mixed powder using a spray dryer device.
[0184] Next, the obtained granulated powder was filled into a mold having a mirror-finished surface on the sample side, and a molding pressure of 200 MPa was applied using a press molding machine to produce a rectangular solid. This molded body may be further compressed using a cold isostatic pressing machine.
[0185] Next, the molded body was placed in an electric furnace and held at a maximum temperature of 1300°C for 5 hours, and then sintered in air for a total of 24 hours to obtain a rectangular sintered body measuring 12 mm x 18 mm x 1.3 mm.
[0186] Next, both sides of the obtained rectangular parallelepiped sintered body were polished using a polishing machine while changing the grit size of the abrasive grains so that the thickness became 1.0 mm, and finally, chemical polishing was performed as a finishing step to obtain a mirror surface.
[0187] Next, a zirconia-coated alumina sagger was prepared as the sagger 7, a zirconia setter as the setter 6, a zirconia setter (size 50 mm x 50 mm x 1 mm, weight 20 g) as the weight 4, and zirconia beads as the beads 5. These were then arranged as shown in Figure 3, and placed in an electric furnace with the lid on as shown in Figure 4, and heated.
[0188] The seed single crystal 2 used here was a 10 mm x 10 mm x 1 mm BaTiO3 (manufactured by Physcience Opto-electronics) substrate with both the main surface and side surface being (100) planes, and both surfaces were mirror polished.
[0189] The heating profile was as follows: the temperature was raised from room temperature to the liquid phase start temperature of 1320°C over 8.8 hours at a rate of 150°C / h, and then the temperature was raised from 1320°C to the liquid phase end temperature of 1385°C at the same rate of 150°C / h. The temperature was then held at 1385°C for 300 hours, and finally cooled to room temperature.
[0190] After heating, the matrix 1 had a single crystal growth portion 3 extending from the seed single crystal, and when the heated matrix 1 was observed with an optical microscope, it was confirmed that the single crystal growth portion 3 (the region extending from the seed single crystal) was a single crystal without grain boundaries. Next, the seed single crystal portion was removed by polishing, and the single crystal portion was cut out with a dicing saw to obtain the single crystal of Comparative Example 4.
[0191] Next, the crystal structure of the polished single crystal was analyzed by X-ray diffraction, and only the peaks corresponding to the (100)-oriented perovskite single crystal were observed. The relative density of the obtained single crystal was 97%. The longest part of the obtained single crystal was 15 mm.
[0192] Next, the composition of the obtained single crystal was evaluated by ICP emission spectroscopy.The results showed that the weighed composition of Ba, Ti, and Zr was consistent with the composition after heating.
[0193] Next, 400 nm-thick gold electrodes were formed on the front and back of the single crystal by DC sputtering, and a 30 nm-thick titanium film was formed between the electrodes and the single crystal as an adhesive layer.
[0194] This single crystal with electrodes was cut to a size of 10 mm x 2.5 mm x 0.5 mm so that the long sides were in the 45° direction, i.e., so that the (100) planes were the top and bottom faces and the (110) planes were the side faces, to produce a rectangular piezoelectric element of Comparative Example 4. The obtained piezoelectric element was subjected to a polarization treatment by setting the surface of a hot plate to 60°C to 100°C and applying an electric field of 1 kV / mm on the hot plate for 30 minutes.
[0195] Next, as the static characteristics of the piezoelectric element having the single crystal of Comparative Example 4, the piezoelectric constant d 31 The mechanical quality factor Qm was evaluated by the resonance-antiresonance method at room temperature (25°C) using an impedance analyzer (4294A manufactured by Agilent Technologies). The results are shown in Table 2.
[0196] Next, the coercive electric field of the piezoelectric element was evaluated. Using a ferroelectric / piezoelectric evaluation system (LCII manufactured by RADIANT TECHNOLOGIES. INC.), the electric field at the time of zero polarization was read from the PE hysteresis curve obtained from the polarization amount against the electric field, and this value was taken as the coercive electric field. The coercive electric field at this time was 0.8 kV / cm.
[0197] Next, the power consumption of the rectangular piezoelectric element was evaluated. The power consumption was measured with a power meter when an alternating voltage was applied and the magnitude and frequency of the alternating voltage were changed so that the displacement was 1.0 μm. The displacement was measured with a laser Doppler vibrometer. The power consumption in this case was 31 mW.
[0198] In Table 1 below, if a single crystal is obtained as a result of carrying out the examples and comparative examples, an A is entered in the column "Whether it is a single crystal?", and if a single crystal is not obtained, a B is entered in the column "Whether it is a single crystal?".
[0199] [Table 1]
[0200] [Table 2]
[0201] (Example 18) An ultrasonic motor shown in Fig. 7 was fabricated using the piezoelectric element of Example 4. In the fabricated ultrasonic motor, rotation of the motor in response to application of an alternating voltage was confirmed.
[0202] (Example 19) 9 was fabricated using the ultrasonic motor of Example 13. In the fabricated optical device, autofocus operation in response to application of an alternating voltage was confirmed.
[0203] (Example 20) A dust removal device shown in Figures 10A and 10B was manufactured using the piezoelectric element of Example 4. When plastic beads were scattered in the manufactured dust removal device and an alternating voltage was applied, a good dust removal rate was confirmed.
[0204] Example 21 13 was fabricated using the dust removal device of Example 15. When the fabricated imaging device was operated, dust on the surface of the imaging unit was successfully removed, and an image without dust defects was obtained.
[0205] Example 22 An ultrasonic probe shown in Fig. 15 was fabricated using the piezoelectric element of Example 4. In the fabricated ultrasonic probe, ultrasonic waves were transmitted by application of an alternating voltage, and a received signal due to reflection from inside the subject was confirmed.
[0206] (Example 23) Using the ultrasonic probe of Example 17, an ultrasonic diagnostic apparatus shown in FIG. 16 was produced. When the constructed ultrasound diagnostic device was operated, a clear image of the inside of the subject was output.
[0207] Example 24 An ultrasonic diagnostic system shown in Fig. 17 was fabricated using the ultrasonic probe of Example 17. When the fabricated ultrasonic diagnostic system was operated and an image was displayed on the image display unit, an image of the inside of the subject was clearly output.
[0208] (Example 25) 19 was fabricated using the piezoelectric element of Example 4. In the fabricated electronic device, speaker operation in response to application of an alternating voltage was confirmed. [Industrial Applicability]
[0209] The method for producing the single crystal of the present invention can be used for a wide range of material compositions, and the single crystal of the present invention has a large piezoelectric constant and mechanical quality factor, so that the single crystal of the present invention can be used without problems in many devices such as ultrasonic motors, dust removal devices, and ultrasonic probes.
[0210] The present invention includes the following embodiments. (Method 1) A method for producing a single crystal by heating a matrix, comprising the steps of: A first preparation step of preparing a matrix and a seed single crystal; a second preparation step of preparing an integral body in which a surface of the matrix and a surface of the seed single crystal are arranged in contact with each other; A first heating step of heating the integrated body from room temperature to a liquid phase initiation temperature of the matrix; a second heating step of heating the integrated body from the liquid phase start temperature to a liquid phase finish temperature of the matrix; a heating step of heating the integral body at the liquid phase finish temperature; obtaining a single crystal from the monolith after the heating; Including, A method for producing a single crystal, wherein a temperature increase rate in the second temperature increase step is smaller than a temperature increase rate in the first temperature increase step. (Method 2) The method for producing a single crystal according to method 1, wherein the single crystal contains Ba, Ti, Zr and Mn. (Method 3) The single crystal contains a perovskite-type oxide containing Ba, Ti, and Zr, and Mn; x, which is a molar ratio of the Zr to the sum of the Ti and the Zr, is 0.01≦x≦0.13; 3. The method for producing a single crystal according to method 1 or 2, wherein the Mn content is 0.04 parts by mass or more and 1.16 parts by mass or less in terms of metal relative to 100 parts by mass of the oxide. (Method 4) The single crystal contains a perovskite-type oxide containing Ba, Ti, and Zr, x, which is a molar ratio of the Zr to the sum of the Ti and the Zr, is 0.01≦x≦0.03; a, which is a molar ratio of Ba to the sum of the Ti and the Zr, is 0.976≦a≦1.020; The single crystal contains Mn and Bi, The content of the Mn is, in terms of metal, 0.04 parts by mass or more and 1.16 parts by mass or less per 100 parts by mass of the oxide, The method for producing a single crystal according to method 1, wherein the content of Bi is 0.04 parts by mass or more and 0.53 parts by mass or less in terms of metal relative to 100 parts by mass of the oxide. (Method 5) 4. The method for producing a single crystal according to any one of Methods 1 to 3, wherein the seed single crystal is a single crystal containing Ba, Ti, and Zr as main components. (Method 6) 5. The method for producing a single crystal according to any one of Methods 1 to 4, wherein the seed single crystal is a single crystal containing Ba, Ti, and Ca as main components. (Method 7) 6. The method for producing a single crystal according to any one of Methods 1 to 5, wherein the matrix is a molded body. (Method 8) 7. The method for producing a single crystal according to any one of Methods 1 to 6, wherein the relative density of the matrix is 93% or more and 100% or less. (Method 9) 8. The method for producing a single crystal according to any one of Methods 1 to 7, wherein the matrix is a polycrystal containing the elements that constitute the single crystal. (Method 10) 9. The method for producing a single crystal according to any one of Methods 1 to 8, wherein the temperature increase rate in the second temperature increase step is 1° C. or less per hour on a time average. (Configuration 1) A single crystal containing a perovskite-type oxide containing Ba, Ti, and Zr and Mn, x, which is a molar ratio of the Zr to the sum of the Ti and the Zr, is 0.01≦x≦0.13; The single crystal has a Mn content of 0.04 parts by mass or more and 1.16 parts by mass or less, calculated as metal, per 100 parts by mass of the oxide. (Configuration 2) x, which is a molar ratio of the Zr to the sum of the Ti and the Zr, is 0.01≦x≦0.03; a, which is a molar ratio of Ba to the sum of the Ti and the Zr, is 0.976≦a≦1.020; The single crystal according to configuration 1, further comprising Bi, the content of Bi being 0.04 parts by mass or more and 0.53 parts by mass or less in terms of metal relative to 100 parts by mass of the oxide. (Configuration 3) 3. The single crystal according to aspect 1 or 2, wherein the longest portion is 1 mm or more and 100 mm or less. (Configuration 4) 3. The single crystal according to aspect 1 or 2, having a relative density of 93% or more and 100% or less. (Configuration 5) 5. The single crystal according to any one of aspects 1 to 4, having a mechanical quality factor Qm of 500 or more. (Configuration 6) A piezoelectric element having a plurality of electrodes and the single crystal according to any one of configurations 1 to 5. (Configuration 7) 7. An ultrasonic motor comprising: a vibrating body on which the piezoelectric element according to configuration 6 is disposed; and a moving body in contact with the vibrating body. (Configuration 8) An optical device having an ultrasonic motor according to configuration 7 in a drive section. (Configuration 9) A vibration device having a vibration body in which the piezoelectric element according to configuration 6 is arranged on a vibration plate. (Configuration 10) A dust removing device having a vibration section including the vibration device according to configuration 9. (Configuration 11) 11. An imaging device having the dust removal device according to configuration 10 and an imaging element unit, wherein a vibration plate of the dust removal device is provided on the light receiving surface side of the imaging element unit. (Configuration 12) 7. An ultrasonic probe having the piezoelectric element according to configuration 6, for transmitting and receiving by the piezoelectric element. (Configuration 13) 13. An ultrasonic diagnostic apparatus comprising the ultrasonic probe according to claim 12 and an image output unit. (Configuration 14) 13. An ultrasound diagnostic system comprising: the ultrasound probe according to claim 12; a transmitter that transmits a signal output from the ultrasound probe; and a receiver that receives the signal transmitted from the transmitter. (Configuration 15) 7. An electronic device including a piezoelectric acoustic component having the piezoelectric element according to claim 6. [Explanation of symbols]
[0211] 1 Matrix 2 Single crystals 3. Single crystal 4. Weights 5 Beads 6 Setter 7. Box 8 Lid 11 First electrode 22 Single crystal section 33 Second electrode 51 First heating step 52 Second heating step 201 Transducer 202 Rotor 203 Output shaft 2011 Elastic Ring 2012 Piezoelectric element 2013 Organic adhesives 310 Dust removal equipment 320 diaphragm 330 Piezoelectric element 331 Single Crystal 332 First electrode 333 Second Electrode 336 First electrode surface 337 Second electrode surface 601 Camera body 602 Mounting section 605 Mirror Box 606 Main Mirror 200 Shutter unit 300 Main Chassis 400 Imaging unit 701 Front lens 702 Rear lens (focus lens) 711 Detachable Mount 712 Fixed tube 713 Straight guide tube 714 Front group tube 715 Cam Ring 716 Rear group tube 717 Cam Roller 718 Axle screw 719 Lola 720 Rotation Transmission Ring 722 Coro 724 Manual Focus Ring 725 Ultrasonic Motor 726 Wave washer 727 Ball Race 728 Focus Key 729 Joint materials 732 Washer 733 Low Friction Sheet 901 Optical equipment 908 Release button 909 Strobe light emitter 912 Speaker 914 Mike 916 Auxiliary Light Unit 931 Main unit 932 Zoom Lever 933 Power button 1100 Ultrasound Probe 1101 Piezoelectric element 1102 Backing layer 1103 Acoustic matching layer 1104 Acoustic Lens 1110 Ultrasound diagnostic equipment 1111 Cable 1112 Image display unit 1113 Drive control unit 1114 Image processing section 1120 Ultrasound diagnostic system 1121 Transmitter 1122 Receiving section
Claims
1. A method for producing a single crystal by heating a matrix, comprising the steps of: A first preparation step of preparing a matrix and a seed single crystal; a second preparation step of preparing an integral body in which a surface of the matrix and a surface of the seed single crystal are arranged in contact with each other; a first heating step of heating the integrated body from room temperature to a liquid phase initiation temperature of the matrix; a second heating step of heating the integrated body from the liquid phase start temperature to a liquid phase finish temperature of the matrix; a heating step of heating the integral body at the liquid phase finish temperature; obtaining a single crystal from the monolith after the heating; Including, A method for producing a single crystal, wherein a temperature increase rate in the second temperature increase step is smaller than a temperature increase rate in the first temperature increase step.
2. The method for producing a single crystal according to claim 1 , wherein the single crystal contains Ba, Ti, Zr and Mn.
3. The single crystal contains a perovskite-type oxide containing Ba, Ti, and Zr, and Mn; x, which is a molar ratio of Zr to the sum of Ti and Zr, is 0.01≦x≦0.13; 2. The method for producing a single crystal according to claim 1, wherein the content of said Mn is 0.04 parts by mass or more and 1.16 parts by mass or less in terms of metal with respect to 100 parts by mass of said oxide.
4. The single crystal contains a perovskite-type oxide containing Ba, Ti, and Zr, x, which is a molar ratio of Zr to the sum of Ti and Zr, is 0.01≦x≦0.03; a, which is a molar ratio of Ba to the sum of the Ti and the Zr, is 0.976≦a≦1.020; The single crystal contains Mn and Bi, The content of the Mn is 0.04 parts by mass or more and 1.16 parts by mass or less in terms of metal relative to 100 parts by mass of the oxide, 2. The method for producing a single crystal according to claim 1, wherein the content of Bi is 0.04 parts by mass or more and 0.53 parts by mass or less in terms of metal per 100 parts by mass of the oxide.
5. The method for producing a single crystal according to claim 1 , wherein the seed single crystal is mainly composed of Ba, Ti, and Zr.
6. The method for producing a single crystal according to claim 1 , wherein the seed single crystal is mainly composed of Ba, Ti, and Ca.
7. 2. The method for producing a single crystal according to claim 1, wherein the matrix is a molded body.
8. 2. The method for producing a single crystal according to claim 1, wherein the relative density of the matrix is 93% or more and 100% or less.
9. The method for producing a single crystal according to claim 1 , wherein the matrix is a polycrystal containing the elements that constitute the single crystal.
10. 2. The method for producing a single crystal according to claim 1, wherein the temperature increase rate in the second temperature increase step is 1° C. or less per hour on a time average.
11. A single crystal containing a perovskite-type oxide containing Ba, Ti, and Zr and Mn, x, which is a molar ratio of Zr to the sum of Ti and Zr, is 0.01≦x≦0.13; The single crystal has a Mn content of 0.04 parts by mass or more and 1.16 parts by mass or less in terms of metal, per 100 parts by mass of the oxide.
12. x, which is a molar ratio of Zr to the sum of Ti and Zr, is 0.01≦x≦0.03; a, which is a molar ratio of Ba to the sum of the Ti and the Zr, is 0.976≦a≦1.020; The single crystal further contains Bi, The single crystal according to claim 11, wherein the content of Bi is 0.04 parts by mass or more and 0.53 parts by mass or less in terms of metal per 100 parts by mass of the oxide.
13. 12. The single crystal according to claim 11, wherein the longest portion is from 1 mm to 100 mm.
14. 12. The single crystal according to claim 11, having a relative density of 93% or more and 100% or less.
15. The single crystal according to claim 11, having a mechanical quality factor Qm of 500 or more.
16. A piezoelectric element comprising a plurality of electrodes and the single crystal according to claim 11 .
17. 17. An ultrasonic motor comprising: a vibrating body on which the piezoelectric element according to claim 16 is disposed; and a moving body in contact with the vibrating body.
18. An optical device comprising the ultrasonic motor according to claim 17 in a drive section.
19. A vibration device having a vibrating body in which the piezoelectric element according to claim 16 is disposed on a vibration plate.
20. A dust removing device having a vibration section comprising the vibration device according to claim 19.
21. An imaging device comprising the dust removing device according to claim 20 and an imaging element unit, an imaging device in which a vibration plate of the dust removing device is provided on the light receiving surface side of the imaging element unit;
22. An ultrasonic probe comprising the piezoelectric element according to claim 16, for transmitting and receiving by said piezoelectric element.
23. An ultrasonic diagnostic apparatus comprising the ultrasonic probe according to claim 22 and an image output unit.
24. 23. An ultrasonic diagnostic system comprising: the ultrasonic probe according to claim 22; a transmitting section that transmits a signal output from the ultrasonic probe; and a receiving section that receives the signal transmitted from the transmitting section.
25. An electronic device comprising a piezoelectric acoustic part comprising the piezoelectric element according to claim 16.
Citation Information
Patent Citations
Single crystal growth method of barium titanate and barium titanate solid solution
JP3507821B2