Method for dividing composite material
By forming processed grooves with widths equal to or larger than the laser beam spot diameter, the method effectively divides composite materials with resin layers on brittle material layers without causing cracks, addressing the inefficiencies of previous methods and enabling more straightforward automation.
Patent Information
- Application Number
- JP2024132120
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-03-11
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-25
AI Technical Summary
Existing methods for dividing composite materials with a resin optical functional layer and a resin protective layer laminated on opposite sides of a brittle material layer often result in cracks on the end faces due to delicate adjustments required for laser beam output, making automation difficult and inefficient.
A method involving the formation of first and second processed grooves using laser beams to remove the resin layers, with the width of the second groove equal to or larger than the spot diameter of the ultrashort pulse laser beam, ensuring the brittle material layer is separated without cracks by effectively utilizing the energy to remove the resin layers.
The method allows for the precise division of composite materials without cracks on the brittle material layer, simplifying the process and reducing the need for delicate adjustments, thereby enhancing automation and efficiency.
Smart Images

Figure 2024152835000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for dividing a composite material having a brittle material layer on one side of which a resin optical functional layer (e.g., a polarizing film) is laminated and a resin protective layer (e.g., a protective film) is laminated on the other side of which, and in particular to a method capable of dividing a composite material without causing cracks on the end surface of the brittle material layer. [Background technology]
[0002] In recent years, LCD panels have become thinner and more highly detailed, and in order to add variety to interfaces, LCD panels equipped with on-screen touch sensor functions are now being used in a wide range of fields, from mobile phones to information displays. Recently, from the viewpoint of reducing thickness and weight, liquid crystal panels having in-cell type liquid crystal cells in which a touch sensor is incorporated into the glass substrate of the liquid crystal cell have appeared.
[0003] Meanwhile, a film-like glass called thin glass is gaining attention as a front panel to be placed on the top surface of a liquid crystal panel. Thin glass can be wound into a roll, so it has the advantage of being adaptable to the so-called roll-to-roll manufacturing process, and a glass polarizing film integrated with a polarizing film has been proposed (for example, see Patent Document 1). Glass polarizing film can be used to produce an LCD panel equipped with a touch sensor function simply by bonding it to an in-cell type LCD cell, making the manufacturing process much simpler than that of conventional LCD panels that use tempered glass as a front panel.
[0004] Patent Document 2 proposes a method for cutting a composite material, such as the above-mentioned glass polarizing film, in which a brittle material layer made of glass or the like and an optically functional layer made of a polarizing film or the like are laminated together, into a desired shape and size depending on the application. The method described in Patent Document 2 is a method for dividing a composite material by irradiating an optical functional layer (resin layer in Patent Document 2) of the composite material with laser light emitted from a laser light source such as a CO2 laser light source along the planned dividing line of the composite material to remove the resin that forms the optical functional layer, and then irradiating a brittle material layer with laser light (ultrashort pulse laser light) emitted from an ultrashort pulse laser light source along the planned dividing line of the composite material to remove the brittle material that forms the brittle material layer. The method described in Patent Document 2 has the advantage that no cracks occur on the end faces of the brittle material layer after cutting.
[0005] Here, as in the above-mentioned glass polarizing film, a composite material in which a brittle material layer made of glass or the like and an optical functional layer made of a polarizing film or the like are laminated is generally shipped with a protective layer such as a protective film laminated on the surface of the cut composite piece opposite to the surface of the brittle material layer on which the optical functional layer is laminated. Since it takes time to perform the step of laminating a protective layer for each cut composite piece, in order to eliminate this time and reduce the number of steps, a method is desired for cutting a composite material in which an optical functional layer is laminated on one surface side of a brittle material layer and a protective layer is laminated on the other surface side of the brittle material layer at once.
[0006] However, Patent Document 2 does not propose a method for cutting, in one go, a composite material in which an optical functional layer is laminated on one side of a brittle material layer and a protective layer is laminated on the other side of the brittle material layer.
[0007] Non-Patent Document 1 describes that in a processing technique using an ultrashort pulsed laser beam, the filamentation phenomenon of the ultrashort pulsed laser beam is utilized, and a multi-focus optical system or a Bessel beam optical system is applied to an ultrashort pulsed laser light source. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2013 / 175767 [Patent Document 2] JP 2019-122966 A [Non-patent literature]
[0009] [Non-Patent Document 1] John Lopez et al., “Glass Cutting Using Ultrashort Pulsed Bessel Beams,” [online], October 2015, International Congress on Applications of Lasers & Electro-Optics (ICALEO), [Retrieved July 8, 2019], Internet (URL: https: / / www.researchgate.net / publication / 284617626_GLASS_CUTTING_USING_ULTRASHORT_PULSED_BESSEL_BEAMS) Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made to solve the problems of the conventional technology as described above, and has an object to provide a method for dividing a composite material in which a resin optical function layer is laminated on one side of a brittle material layer and a resin protective layer is laminated on the other side of the brittle material layer, the method being capable of dividing a composite material without generating cracks on the end surface of the brittle material layer. [Means for solving the problem]
[0011] In order to solve the above problems, the present inventors have considered applying the method described in the above-mentioned Patent Document 2. Specifically, in a composite material in which a resin optical functional layer is laminated on one side of a brittle material layer and a resin protective layer is laminated on the other side of the brittle material layer, a machined groove (first machined groove) is formed in the optical functional layer along the planned dividing line of the composite material by a laser beam oscillated from a CO2 laser light source, etc., and a machined groove (second machined groove) is formed in the protective layer along the planned dividing line of the composite material by a laser beam oscillated from a CO2 laser light source, etc. Then, in order to prevent serious thermal degradation from occurring on the end face of the optical functional layer after dividing (there is less discolored area due to thermal degradation), it was thought that it would be good to irradiate the brittle material layer along the planned dividing line of the composite material with a laser beam (ultrashort pulsed laser beam) oscillated from an ultrashort pulsed laser light source through the second machined groove.
[0012] However, when the inventors actually conducted tests on the above method, it was found that if the output of the laser light for forming the second groove is small and the depth of the second groove is too small, when the brittle material layer is irradiated with the ultrashort pulse laser light, a processing mark penetrating the brittle material layer in the thickness direction cannot be formed, and the composite cannot be divided. On the other hand, it was found that if the output of the laser light for forming the second groove is too large, the brittle material layer is thermally damaged, and when the brittle material layer is irradiated with the ultrashort pulse laser light, cracks are generated on the end surface of the brittle material layer starting from the thermally damaged area. And, it was found that extremely delicate adjustment is required to set the output of the laser light for forming the second groove to an appropriate value so that processing marks can be formed on the brittle material layer and cracks are not generated on the end surface of the brittle material layer, and automation is difficult.
[0013] As a result of further intensive research, the inventors discovered that if the second groove is formed so that its width is greater than or equal to the spot diameter at the irradiating position of the ultrashort pulse laser light on the brittle material layer, it is possible to cut the composite material without causing cracks on the end surface of the brittle material layer, without requiring delicate adjustment of the output of the laser light to form the second groove, and thus completed the present invention.
[0014] The present invention has been completed based on the above-mentioned findings of the present inventors. That is, in order to solve the above-mentioned problems, the present invention provides a method for dividing a composite material having a resin optical functional layer laminated on one surface side of a brittle material layer and a resin protective layer laminated on the other surface side of the brittle material layer, the method comprising: irradiating the optical functional layer with a laser beam emitted from a first laser light source along a planned dividing line of the composite material to remove the resin that forms the optical functional layer, thereby forming a first processed groove along the planned dividing line; and irradiating the protective layer with a laser beam emitted from a second laser light source along the planned dividing line to remove the resin that forms the protective layer, thereby forming a second processed groove along the planned dividing line. The present invention provides a method for dividing a composite material, the method including: a machining groove forming step for forming a groove; and a machining mark forming step for, after the machining groove forming step, irradiating the brittle material layer with laser light oscillated from an ultrashort pulse laser light source from the second machining groove side along the planned division line to remove the brittle material that forms the brittle material layer, thereby forming a machining mark along the planned division line, wherein, in the machining groove forming step, resin that forms the protective layer is removed so that the width of the second machining groove is equal to or greater than the spot diameter at the irradiating position of the brittle material layer with the laser light oscillated from the ultrashort pulse laser light source in the machining mark forming step.
[0015] According to the method of the present invention, in the groove forming step, the resin forming the optical function layer and the resin forming the protective layer are removed to form a first groove and a second groove along the planned division line, and then in the mark forming step, the brittle material forming the brittle material layer is removed from the second groove side to form a mark along the same planned division line. The width of the second groove formed in the groove forming step is formed to be equal to or larger than the spot diameter at the irradiation position of the laser light (ultrashort pulse laser light) oscillated from the ultrashort pulse laser light source in the mark forming step. This makes it possible to divide the brittle material layer without causing cracks on the end face of the brittle material layer, as found by the inventors above. As in the method of the present invention, by making the width of the second processing groove greater than or equal to the spot diameter at the irradiating position of the ultrashort pulse laser light on the brittle material layer, the energy of the ultrashort pulse laser light is less likely to be consumed in removing the resin that forms the protective layer, and is fully used to remove the brittle material that forms the brittle material layer, so that processing marks can be formed in the brittle material layer while preventing cracks from occurring on the end face of the brittle material layer.
[0016] In the method according to the present invention, "irradiating the optical functional layer with a laser beam along the planned dividing line of the composite" means irradiating the optical functional layer with a laser beam along the planned dividing line when viewed from the thickness direction of the composite (the stacking direction of the optical functional layer, the brittle material layer, and the protective layer). In the method according to the present invention, "irradiating the protective layer with a laser beam along the planned dividing line" means irradiating the protective layer with a laser beam along the planned dividing line when viewed from the thickness direction of the composite (the stacking direction of the optical functional layer, the brittle material layer, and the protective layer). Furthermore, "irradiating the brittle material layer with a laser beam from the second processing groove side along the planned dividing line" means irradiating the protective layer with a laser beam from the second processing groove side along the planned dividing line when viewed from the thickness direction of the composite (the stacking direction of the optical functional layer, the brittle material layer, and the protective layer). In the method according to the present invention, "irradiating along the planned dividing line" means irradiating on the planned dividing line, or irradiating a position in the vicinity of the planned dividing line parallel to the planned dividing line. Furthermore, in the method according to the present invention, the "width of the second groove" means the dimension of the bottom of the second groove in the direction perpendicular to the intended division line.
[0017] In the method according to the present invention, the types of the first laser light source and the second laser light source used in the machining groove forming step are not particularly limited as long as the resin can be removed by the oscillating laser light. However, it is preferable to use a CO2 laser light source or a CO laser light source that oscillates a laser light with a wavelength in the infrared range, since it is possible to increase the relative moving speed (machining speed) of the laser light with respect to the composite material. The first laser light source and the second laser light source may be the same type or different types. In addition, the first laser light source and the second laser light source do not necessarily need to be prepared separately, and the first laser light source can also be used as the second laser light source. When the first laser light source and the second laser light source are prepared separately, the first laser light source is arranged on the optical functional layer side, and the second laser light source is arranged on the protective layer side, and the first laser light source is used to form the first groove in the optical functional layer, and the second laser light source is used to form the second groove in the protective layer. Also, the second laser light source may be used to form the second groove in the protective layer, and the first laser light source may be used to form the first groove in the optical functional layer. Furthermore, the first laser light source and the second laser light source may be used to simultaneously form the first groove and the second groove. In addition, when the first laser light source is also used as the second laser light source, the first laser light source (second laser light source) can be arranged on the side facing either the optical functional layer or the protective layer, and the first laser light source (second laser light source) can be used to form a first processing groove in the optical functional layer (or form a second processing groove in the protective layer), and then the composite material can be inverted so that the first laser light source (second laser light source) faces the other of the optical functional layer and the protective layer, and the first laser light source (second laser light source) can be used to form a second processing groove in the protective layer (or form the first processing groove in the optical functional layer).
[0018] Furthermore, in the method according to the present invention, the processing marks formed in the processing mark forming step can be exemplified by perforated through holes along the planned dividing line as described in Patent Document 2. In this case, the composite material can be divided by applying an external force along the planned dividing line after the processing mark forming step. Examples of the method of applying an external force to the composite material include mechanical breaking (mountain folding), heating the area near the planned dividing line with infrared laser light, applying vibration with an ultrasonic roller, and suction and lifting with a suction cup. When the method of applying an external force to the composite material involves heating the area near the planned dividing line with infrared laser light, the thermal stress generated in the brittle material layer causes a crack to develop along the planned dividing line so as to connect the perforated through holes, and the brittle material layer is divided (cut). In addition, if resin residue remains at the bottom of the first processing groove, after applying an external force as described above to divide the brittle material layer, for example, a mechanical external force can be further applied to the optical function layer to divide the composite material. Even if further mechanical external force is applied to the optical function layer and therefore the brittle material layer, no cracks will occur at the end faces of the brittle material layer because the brittle material layer has already been divided at this point. In the method according to the present invention, the processing marks formed in the processing mark forming step are not necessarily limited to perforated through holes. In the processing mark forming step, if the relative movement speed between the laser light oscillated from the ultrashort pulse laser light source and the brittle material layer along the planned dividing line is set to be small, or the repetition frequency of the pulse oscillation of the ultrashort pulse laser light source is set to be large, a through hole (long hole) integrally connected along the planned dividing line is formed as the processing mark. In this case, the brittle material layer can be divided without applying an external force along the planned dividing line after the processing mark forming step. However, if a resin residue remains at the bottom of the first processing groove, for example, a mechanical external force may be applied to the optical function layer after dividing the brittle material layer to divide the composite material.
[0019] In the method according to the present invention, in order to make the width of the second processed groove formed in the processed groove forming step equal to or larger than the spot diameter at the irradiation position of the brittle material layer with the laser light (ultrashort pulse laser light) oscillated from the ultrashort pulse laser light source in the processed mark forming step, it is possible to, for example, shift the irradiation position of the laser light oscillated from the second laser light source in a direction perpendicular to the planned division line, irradiate the protective layer with the laser light at each irradiation position, and then peel off the resin forming the protective layer present between each irradiation position. If the dimension of the part where this resin is peeled off (the dimension in the direction perpendicular to the planned division line) is equal to or larger than the spot diameter at the irradiation position of the brittle material layer with the ultrashort pulse laser light, the width of the second processed groove can be equal to or larger than the spot diameter at the irradiation position of the brittle material layer with the ultrashort pulse laser light. That is, preferably, in the processing groove forming process, the irradiation position of the laser light emitted from the second laser light source onto the protective layer is shifted in a direction perpendicular to the planned division line, and the laser light is irradiated onto the protective layer along the planned division line at each irradiation position, and then the resin forming the protective layer present between each irradiation position is peeled off to form the second processing groove.
[0020] According to the above-mentioned preferred method (hereinafter, appropriately referred to as "peeling method"), for example, in the groove forming step, the laser light emitted from the second laser light source is irradiated to positions at equal distances in a direction perpendicular to the planned division line based on the planned division line, and the resin forming the protective layer existing between them is peeled off. In this way, after forming the second groove with the planned division line as the center in the width direction, if the planned division line is irradiated with ultrashort pulsed laser light, the irradiation position of the laser light emitted from the second laser light source and the irradiation position of the ultrashort pulsed laser light will be shifted by 1 / 2 the width of the second groove. Therefore, even if the output of the laser light emitted from the second laser light source is set to a certain level in the processing groove forming process, and the resin forming the protective layer is removed to expose the surface of the brittle material layer and cause some thermal damage, it is difficult for the ultrashort pulse laser light to be irradiated to the same location, and therefore cracks are unlikely to occur on the end surface of the brittle material layer. The resin forming the protective layer between the irradiation positions can be peeled off by using a known peeling device as appropriate.
[0021] In the method according to the present invention, the method for making the width of the second groove formed in the groove forming process equal to or larger than the spot diameter of the ultrashort pulsed laser light at the irradiation position on the brittle material layer is not limited to the peeling method described above. For example, in the processing groove forming process, the irradiation position of the laser light emitted from the second laser light source onto the protective layer may be sequentially shifted in a direction perpendicular to the planned division line, and the laser light may be irradiated onto the protective layer along the planned division line at each irradiation position to form the second processing groove (hereinafter referred to as the "offset method" as appropriate). By setting the range for shifting the irradiation position of the laser light emitted from the second laser light source (the range in the direction perpendicular to the planned division line) to be greater than or equal to the spot diameter at the irradiating position of the ultrashort pulsed laser light on the brittle material layer, the width of the second processing groove can be made greater than or equal to the spot diameter at the irradiating position of the ultrashort pulsed laser light on the brittle material layer.
[0022] In the present invention, the spot diameter of the ultrashort pulse laser light at the irradiated position on the brittle material layer is set to, for example, 100 μm. Therefore, in the processing groove forming process, it is preferable to remove the resin forming the protective layer so that the width of the second processing groove is 100 μm or more, and it is more preferable to remove the resin forming the protective layer so that the width of the second processing groove is 150 μm or more. When the spot diameter of the ultrashort pulsed laser light at the irradiation position on the brittle material layer is 100 μm, the spot diameter on the surface of the brittle material layer on the optical function layer side is condensed to, for example, 1.2 μm. When the spot diameter of the ultrashort pulsed laser light at the irradiation position on the brittle material layer is 100 μm, the spot diameter at the position corresponding to the surface of the protective layer (the surface opposite to the surface on the brittle material layer side) is, for example, 154 μm.
[0023] Preferably, the protective layer comprises a base layer and an adhesive layer arranged on the brittle material layer side, and in the processing groove forming process, the resin forming the protective layer is removed so that a portion of the adhesive layer in the thickness direction remains.
[0024] According to the above-mentioned preferred method, in the processing groove formation process, the resin forming the protective layer is removed so that a portion of the adhesive layer in the thickness direction remains, so that the brittle material layer is less susceptible to thermal damage and cracks are even less likely to occur at the end faces of the brittle material layer.
[0025] The adhesive that forms the adhesive layer that the protective layer has can be, for example, an acrylic adhesive. However, in order to prevent the generation of fumes when forming the second groove in the protective layer in the groove formation process, it is preferable to use a urethane adhesive, which is less likely to generate fumes, as the adhesive. That is, preferably, the protective layer includes a base layer and a urethane-based pressure-sensitive adhesive layer disposed on the brittle material layer side.
[0026] According to the above-mentioned preferred method, it is possible to prevent the generation of fumes from the adhesive layer of the protective layer in the groove forming process. The above-mentioned preferred method is particularly effective when the offset method described above is applied in the groove forming process. That is, when the offset method is applied, there are more irradiation points of the laser light oscillated from the second laser light source on the protective layer than when the peeling method is applied, so that fumes are more likely to be generated from the adhesive layer of the protective layer. Therefore, the above-mentioned preferred method capable of preventing the generation of fumes is particularly effective when the offset method is applied.
[0027] The method according to the present invention is preferably used in the case where, for example, the brittle material layer includes glass and the optically functional layer includes a polarizing film. Effect of the Invention
[0028] According to the present invention, a composite material having a resin optical functional layer laminated on one side of a brittle material layer and a resin protective layer laminated on the other side of the brittle material layer can be divided without causing cracks on the end surface of the brittle material layer. [Brief description of the drawings]
[0029] [Figure 1] 1 is a cross-sectional view showing a schematic configuration of a composite material to which a cutting method according to an embodiment of the present invention is applied. [Diagram 2] FIG. 2 is an explanatory diagram for explaining a schematic outline of a procedure of a method for dividing a composite material according to one embodiment of the present invention. [Diagram 3] 1A to 1C are cross-sectional views for explaining an outline of a peeling method in a processed groove forming step. [Figure 4] FIG. 11 is a plan view for explaining a schematic outline of the procedure of a peeling method and a machining mark forming step in a machining groove forming step when dividing a composite material into four rectangular composite material pieces. [Diagram 5] 1A to 1C are cross-sectional views for explaining an outline of the procedure of an offset method in a processed groove forming process. [Figure 6] FIG. 11 is a plan view for explaining a schematic outline of the offset method in the machining groove forming step and the machining mark forming step when cutting a composite material into four rectangular composite material pieces. [Figure 7] As an example, an example of the results when a peeling method is applied in the groove forming process will be shown. [Figure 8] As an example, an example of test conditions and test results when the offset method is applied in the machined groove forming process will be described. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, a method for dividing a composite material according to one embodiment of the present invention will be described with reference to the accompanying drawings as appropriate.
[0031] <Composite material composition> First, the configuration of a composite material to which the cutting method according to this embodiment is applied will be described. FIG. 1 is a cross-sectional view showing a schematic configuration of a composite material to which a cutting method according to this embodiment is applied. Please note that Figure 1 is for reference purposes only, and the dimensions, scale, and shapes of the components shown in the figure may differ from the actual ones. The same applies to the other figures. 1, the composite material 10 has a laminated configuration of a brittle material layer 1, a resin-made optical functional layer 2 laminated on one surface side (the lower side in the example shown in FIG. 1) of the brittle material layer 1, and a resin-made protective layer 3 laminated on the other surface side (the upper side in the example shown in FIG. 1) of the brittle material layer 1. The protective layer 3 includes a base layer 3a and an adhesive layer 3b arranged on the brittle material layer 1 side. The cutting method according to this embodiment is a method for cutting the composite material 10 in the thickness direction (the lamination direction of the optical functional layer 2, the brittle material layer 1, and the protective layer 3, the vertical direction in FIG. 1, the Z direction).
[0032] The brittle material layer 1, the optical functional layer 2, and the protective layer 3 are laminated by any appropriate method. For example, the brittle material layer 1, the optical functional layer 2, and the protective layer 3 can be laminated by a so-called roll-to-roll method. For example, the long brittle material layer 1 and the main body of the long optical functional layer 2 (for example, a polarizing film, an adhesive, and a release film constituting the optical functional layer 2, in that order from the top in FIG. 1. However, in FIG. 1, the polarizing film, the adhesive, and the release film are omitted) are transported in the longitudinal direction, and are laminated together with an adhesive (not shown) so that the longitudinal directions of the layers are aligned. Thus, the brittle material layer 1 and the optical functional layer 2 (the main body of the optical functional layer 2 and the adhesive) can be laminated. Next, the long laminate of the brittle material layer 1 and the optical functional layer 2 and the base layer 3a of the long protective layer 3 are transported in the longitudinal direction, and are bonded to each other via the adhesive layer 3b so that their longitudinal directions are aligned, thereby laminating the brittle material layer 1, the optical functional layer 2, and the protective layer 3. However, the brittle material layer 1 and the main body of the optical functional layer 2 may be cut into a predetermined shape, and then laminated via an adhesive. Also, the laminate of the brittle material layer 1 and the optical functional layer 2 and the base layer 3a of the protective layer 3 may be cut into a predetermined shape, and then laminated via the adhesive layer 3b.
[0033] Examples of the brittle material that forms the brittle material layer 1 include glass and single crystal or polycrystalline silicon. Preferably, glass is used. Glass can be classified according to composition, such as soda-lime glass, borate glass, aluminosilicate glass, quartz glass, and sapphire glass. Glass can be classified according to alkali content, such as non-alkali glass and low-alkali glass. The content of alkali metal components (e.g., Na2O, K2O, Li2O) in glass is preferably 15% by weight or less, and more preferably 10% by weight or less.
[0034] The thickness of the brittle material layer 1 is preferably 150 μm or less, more preferably 120 μm or less, and further preferably 100 μm or less. On the other hand, the thickness of the brittle material layer 1 is preferably 30 μm or more, and more preferably 80 μm or more. If the thickness of the brittle material layer 1 is in such a range, lamination with the optical functional layer 2 by roll-to-roll is possible.
[0035] When the brittle material forming the brittle material layer 1 is glass, the light transmittance of the brittle material layer 1 at a wavelength of 550 nm is preferably 85% or more. When the brittle material forming the brittle material layer 1 is glass, the refractive index of the brittle material layer 1 at a wavelength of 550 nm is preferably 1.4 to 1.65. When the brittle material forming the brittle material layer 1 is glass, the density of the brittle material layer 1 is preferably 2.3 g / cm 3 ~3.0g / cm 3 and more preferably 2.3 g / cm 3 ~2.7g / cm 3 It is.
[0036] When the brittle material forming the brittle material layer 1 is glass, a commercially available glass plate may be used as it is, or may be polished to a desired thickness and used as the brittle material layer 1. Examples of commercially available glass plates include "7059", "1737" or "EAGLE2000" manufactured by Corning Incorporated, "AN100" manufactured by Asahi Glass Co., Ltd., "NA-35" manufactured by NH Techno Glass Co., Ltd., "OA-10G" manufactured by Nippon Electric Glass Co., Ltd., and "D263" or "AF45" manufactured by Schott.
[0037] Examples of the main body of the optical functional layer 2 include a single-layer film formed of a plastic material such as polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), acrylic resin such as polymethyl methacrylate (PMMA), cyclic olefin polymer (COP), cyclic olefin copolymer (COC), polycarbonate (PC), urethane resin, polyvinyl alcohol (PVA), polyimide (PI), polytetrafluoroethylene (PTFE), polyvinyl chloride (PVC), polystyrene (PS), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), ethylene-vinyl acetate (EVA), polyamide (PA), silicone resin, epoxy resin, liquid crystal polymer, and various resin foams, or a laminate film consisting of multiple layers.
[0038] When the main body of the optical functional layer 2 is a laminated film composed of a plurality of layers, various pressure-sensitive adhesives such as acrylic pressure-sensitive adhesives, urethane pressure-sensitive adhesives, and silicone pressure-sensitive adhesives, or adhesives may be interposed between the layers. Moreover, on the surface of the main body of the optical function layer 2, a conductive inorganic film such as indium tin oxide (ITO), Ag, Au, Cu, or the like may be formed. The cutting method according to this embodiment is particularly suitable for use when the main body of the optical functional layer 2 is a polarizing film, a retardation film, or the like used in a display. The thickness of the main body of the optical functional layer 2 is preferably 20 to 500 μm, and more preferably 50 to 300 μm.
[0039] In this embodiment, as described above, the main body of the optical functional layer 2 is a laminated film in which a polarizing film, an adhesive, and a release film are laminated in this order from the top in Fig. 1. The main body of the optical functional layer 2 is laminated with the brittle material layer 1 via an adhesive (not shown). In this embodiment, the combination of the main body of the optical functional layer 2 (polarizing film, adhesive, and release film) and the adhesive is referred to as the optical functional layer 2.
[0040] The polarizing film constituting the main body of the optical functional layer 2 has a polarizer and a protective film disposed on at least one side of the polarizer. The thickness of the polarizer is not particularly limited, and an appropriate thickness can be adopted depending on the purpose. The thickness of the polarizer is typically about 1 to 80 μm. In one embodiment, the thickness of the polarizer is preferably 30 μm or less. The polarizer is an iodine-based polarizer. More specifically, the polarizer can be composed of a polyvinyl alcohol-based resin film containing iodine.
[0041] Examples of methods for producing a polarizer constituting the above polarizing film include the following methods 1 and 2. (1) Method 1: A method of stretching and dyeing a polyvinyl alcohol resin film alone. (2) Method 2: A method in which a laminate (i) having a resin substrate and a polyvinyl alcohol-based resin layer is stretched and dyed. Method 1 is a method well known and commonly used in the art, and therefore a detailed description thereof will be omitted. Method 2 preferably includes a step of stretching and dyeing a laminate (i) having a resin substrate and a polyvinyl alcohol-based resin layer formed on one side of the resin substrate to produce a polarizer on the resin substrate. The laminate (i) can be formed by applying a coating liquid containing a polyvinyl alcohol-based resin onto a resin substrate and drying it. Alternatively, the laminate (i) may be formed by transferring a polyvinyl alcohol-based resin film onto the resin substrate. Details of Method 2 are described in, for example, JP 2012-73580 A, which is incorporated herein by reference.
[0042] The protective film constituting the polarizing film is disposed on one or both sides of the polarizer. As the protective film, a triacetyl cellulose film, an acrylic film, a cycloolefin film, a polyethylene terephthalate film, or the like can also be used. The polarizing film may further include a retardation film as appropriate. The retardation film may have any suitable optical properties and / or mechanical properties depending on the purpose.
[0043] The release film constituting the main body of the optical functional layer 2 has a role of protecting the adhesive layer constituting the main body of the optical functional layer 2 until the composite material 10 is put to practical use. Examples of materials constituting the release film include plastic films such as polyethylene, polypropylene, polyethylene terephthalate, and polyester films, porous materials such as paper, cloth, and nonwoven fabric, and appropriate thin materials such as nets, foam sheets, metal foils, and laminates thereof, among which plastic films are preferably used because of their excellent surface smoothness.
[0044] For example, a polyester adhesive, a polyurethane adhesive, a polyvinyl alcohol adhesive, or an epoxy adhesive can be used as the adhesive constituting the optical functional layer 2. In particular, it is preferable to use an epoxy adhesive since good adhesion can be obtained. If the adhesive is a thermosetting adhesive, it can be heated to cure (solidify) and thus exhibit peel resistance. If the adhesive is a light-curing adhesive such as an ultraviolet-curing adhesive, it can be cured by irradiating it with ultraviolet light or other light and thus exhibit peel resistance. Furthermore, if the adhesive is a moisture-curing adhesive, it can be cured by reacting with moisture in the atmosphere and therefore can be left to cure and exhibit peel resistance. As the adhesive, for example, a commercially available adhesive may be used, or an adhesive solution (or dispersion) may be prepared by dissolving or dispersing various curable resins in a solvent. The thickness of the adhesive is preferably 10 μm or less, more preferably 1 to 10 μm, further preferably 1 to 8 μm, and particularly preferably 1 to 6 μm.
[0045] In this embodiment, the base material layer 3a of the protective layer 3 is laminated to the brittle material layer 1 via an adhesive layer 3b. It is also possible to configure the base material layer 3a of the protective layer 3 with a self-adhesive film and laminate it to the brittle material layer 1 without an adhesive layer, but from the viewpoint of protecting the brittle material layer 1, it is preferable to laminate it to the brittle material layer 1 via the adhesive layer 3b as in this embodiment. As the base layer 3a, a film material having isotropy or close to isotropy is selected from the viewpoint of inspectability and manageability. Examples of the film material include transparent polymers such as polyester resins such as polyethylene terephthalate film, cellulose resins, acetate resins, polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, and acrylic resins. Among these, polyester resins are preferred. As the base layer 3a, a laminate of one or more film materials can be used, and a stretched product of the above film can also be used. The thickness of the base layer 3a is preferably 35 μm to 100 μm or less, and more preferably more than 38 μm to 100 μm or less.
[0046] The adhesive for forming the adhesive layer 3b may be appropriately selected from adhesives having a base polymer such as a (meth)acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, or a rubber-based polymer. From the viewpoints of transparency, weather resistance, heat resistance, and the like, an acrylic adhesive having an acrylic polymer as a base polymer is preferred. However, as described later, in order to prevent the generation of fumes when forming the second processing groove 31 in the protective layer 3, it is preferred to use a urethane adhesive having a polyurethane as a base polymer as the adhesive for forming the adhesive layer 3b. The thickness (dry film thickness) of the adhesive layer 3b is determined according to the required adhesive strength. It is usually about 1 to 100 μm, preferably 5 to 50 μm.
[0047] <How to cut composite materials> A method for dividing the composite material 10 having the above configuration will now be described. The cutting method according to the present embodiment includes a processing groove forming step and a processing mark forming step. The cutting method according to the present embodiment also includes a composite material cutting step as necessary. Each step will be described below in order.
[0048] [Groove formation process] Fig. 2 is an explanatory diagram for explaining the outline of the procedure of the cutting method according to the present embodiment. Fig. 2(a) and (b) are cross-sectional views showing the machining groove forming step of the cutting method according to the present embodiment. Fig. 2(c) is a cross-sectional view showing the machining mark forming step of the cutting method according to the present embodiment. Fig. 2(d) is a cross-sectional view showing the composite material cutting step of the cutting method according to the present embodiment. 2(a), in the groove forming step, the laser light L1 emitted from the first laser light source 20 is irradiated onto the optical functional layer 2 along the planned dividing line of the composite material 10 to remove the resin forming the optical functional layer 2. As a result, a first groove 21 is formed along the planned dividing line. 2, for convenience, a straight line DL extending in the Y direction of the two orthogonal directions (X direction and Y direction) within the plane of the composite material 10 (within the XY two-dimensional plane) is illustrated as the planned division line, but the present invention is not limited to this, and various planned division lines can be set, for example, a planned division line in which a plurality of straight lines DL extending in the X direction and a plurality of straight lines DL extending in the Y direction are set in a grid pattern. Hereinafter, this straight line DL will be referred to as the "planned division line DL". The planned dividing line DL can be actually drawn on the composite material 10 as a visually recognizable mark, or its coordinates can be input in advance to a control device (not shown) that controls the relative positional relationship between the laser light L1 and the composite material 10 on an XY two-dimensional plane. The planned dividing line DL shown in FIG. 2 is a virtual line whose coordinates are input in advance to the control device and which is not actually drawn on the composite material 10. Note that the planned dividing line DL is not limited to a straight line and may be a curved line. By determining the planned dividing line DL according to the application of the composite material 10, the composite material 10 can be divided into any shape and size according to the application.
[0049] In this embodiment, as the first laser light source 20, a CO2 laser light source that oscillates laser light L1 with a wavelength of 9 to 11 μm in the infrared range is used. However, the present invention is not limited to this, and it is also possible to use, as the first laser light source 20, a CO laser light source that oscillates laser light L1 with a wavelength of 5 μm. Also, a visible light and ultraviolet (UV) pulsed laser light source can be used as the first laser light source 20. Examples of visible light and UV pulsed laser light sources include those emitting laser light L1 with a wavelength of 532 nm, 355 nm, 349 nm, or 266 nm (high-order harmonics of a solid-state laser light source using Nd:YAG, Nd:YLF, or YVO4 as a medium), an excimer laser light source emitting laser light L1 with a wavelength of 351 nm, 248 nm, 222 nm, 193 nm, or 157 nm, and an F2 laser light source emitting laser light L1 with a wavelength of 157 nm. It is also possible to use a pulsed laser light source having a wavelength of the oscillated laser light L1 outside the ultraviolet range and a pulse width on the order of femtoseconds or picoseconds as the first laser light source 20. If the laser light L1 oscillated from this pulsed laser light source is used, it is possible to induce ablation processing based on a multiphoton absorption process. Furthermore, as the first laser light source 20, it is also possible to use a semiconductor laser light source or a fiber laser light source that oscillates laser light L1 with a wavelength in the infrared region.
[0050] As an example of the manner in which the laser light L1 is irradiated along the planned dividing line of the composite material 10 (the manner in which the laser light L1 is scanned), for example, the sheet-like composite material 10 is placed on an XY two-axis stage (not shown) and fixed (for example, fixed by suction), and the XY two-axis stage is driven by a control signal from the control device to change the relative position of the composite material 10 on the XY two-dimensional plane with respect to the laser light L1. It is also possible to change the position of the laser light L1 irradiated to the composite material 10 on the XY two-dimensional plane by fixing the position of the composite material 10 and deflecting the laser light L1 oscillated from the first laser light source 20 using a galvanometer mirror or a polygon mirror driven by a control signal from the control device. Furthermore, it is also possible to use both the scanning of the composite material 10 using the above-mentioned XY two-axis stage and the scanning of the laser light L1 using a galvanometer mirror or the like in combination.
[0051] The oscillation form of the first laser light source 20 may be pulse oscillation or continuous oscillation. The spatial intensity distribution of the laser light L1 may be a Gaussian distribution, or may be shaped into a flat-top distribution using a diffractive optical element (not shown) or the like in order to suppress thermal damage to the brittle material layer 1 that is not a target for removal by the laser light L1. There is no restriction on the polarization state of the laser light L1, and it may be any of linear polarization, circular polarization, and random polarization.
[0052] By irradiating the optical functional layer 2 with the laser light L1 along the planned dividing line DL of the composite material 10, a local temperature rise occurs due to infrared light absorption of the resin irradiated with the laser light L1 among the resins forming the optical functional layer 2, and the resin is scattered, and the resin is removed from the composite material 10, and a first processing groove 21 is formed in the composite material 10. In order to prevent the scattered resin removed from the composite material 10 from re-adhering to the composite material 10, it is preferable to provide a dust collection mechanism in the vicinity of the planned dividing line DL. In order to prevent the width of the first processing groove 21 from becoming too large, it is preferable to focus the laser light L1 so that the spot diameter at the irradiation position on the optical functional layer 2 (the spot diameter on the surface opposite to the surface on the brittle material layer 1 side of the optical functional layer 2) is 300 μm or less, and it is more preferable to focus the laser light L1 so that the spot diameter is 200 μm or less. The spot diameter of the laser light L1 at the irradiation position on the optical function layer 2 is, for example, about 150 μm, and at this time, the spot diameter on the surface of the optical function layer 2 facing the brittle material layer 1 is condensed to, for example, 30 to 40 μm. As a result, the first processed groove 21 is formed with a width (the dimension of the bottom of the first processed groove 21 in the direction perpendicular to the planned division line DL) of 30 to 40 μm. The width of the first groove 21 is, for example, 100 μm or less, and preferably 50 μm or less.
[0053] According to the findings of the present inventors, in the case of a resin removal method based on a local temperature rise caused by infrared light absorption by a resin irradiated with laser light L1, it is possible to roughly estimate the input energy required to form the first groove 21 from the thickness of the optical functional layer 2, regardless of the type of resin or the layer structure of the optical functional layer 2. Specifically, the input energy required to form the first groove 21, which is expressed by the following formula (1), can be estimated based on the thickness of the optical functional layer 2 by the following formula (2). Input energy [mJ / mm] = average power of laser light L1 [mW] / processing speed [mm / sec] (1) Input energy [mJ / mm] = 0.5 × thickness of optical functional layer 2 [μm] (2) The input energy to be actually set is preferably set to 20 to 180% of the input energy estimated by the above formula (2), and more preferably set to 50 to 150%. The reason for providing a margin for the estimated input energy in this way is that it is considered that the input energy required to form the first processed groove 21 varies depending on the light absorptance (light absorptance at the wavelength of the laser light L1) of the resin forming the optical functional layer 2 and the thermal properties such as the melting point and decomposition point of the resin. Specifically, for example, a sample of the composite material 10 to which the cutting method according to the present embodiment is applied is prepared, and a preliminary test is performed to form the first processed groove 21 in the optical functional layer 2 of this sample with a plurality of input energies within the above preferred range, and an appropriate input energy can be determined.
[0054] 2(b), in the groove forming step, the protective layer 3 is irradiated with laser light L2 emitted from a second laser light source 30 along the planned dividing line of the composite material 10 to remove the resin forming the protective layer 3. This forms a second groove 31 (see FIG. 2(c)) along the planned dividing line. In this embodiment, a peeling method or an offset method is used to form the second groove 31, the specific details of which will be described later. In this embodiment, the second processed groove 31 is formed after the first processed groove 21 is formed, but the present invention is not limited to this, and it is also possible to form the first processed groove 21 after forming the second processed groove 31. Also, as shown in Fig. 2, when the first laser light source 20 and the second laser light source 30 are prepared separately, it is also possible to form the first processed groove 21 and the second processed groove 31 at the same time.
[0055] In this embodiment, the second laser light source 30 uses a CO2 laser light source of the same type as the first laser light source 20. However, the present invention is not limited to this, and other laser light sources such as a CO laser light source can be used, as described above for the first laser light source 20. The second laser light source 30 may be of the same type as the first laser light source 20, or may be of a different type. As a mode in which the laser light L2 is irradiated along the planned division line DL (a mode in which the laser light L2 is relatively scanned), a mode using an XY two-axis stage, a galvanometer mirror, or the like can be adopted, as described above for the laser light L1. The laser light L2 is focused so that the spot diameter at the irradiation position on the protective layer 3 (the spot diameter on the surface of the protective layer 3 opposite to the surface on the brittle material layer 1 side) is, for example, 120 to 130 μm. As a result, a groove having a width of 20 to 30 μm at the bottom is formed.
[0056] The second machining groove 31 is formed so that its width W (see FIG. 2(c)) is greater than or equal to the spot diameter D (see FIG. 2(c)) at the irradiating position on the brittle material layer 1 of the laser light L3 emitted from the ultrashort pulse laser light source 40 in the machining mark formation process described below. Specifically, the width W of the second groove 31 in this embodiment is preferably 100 μm or more, and more preferably 150 μm or more. The upper limit of the width W of the second groove 31 is, for example, 1000 μm or less, preferably 500 μm or less, and more preferably 300 μm or less. As described above, the width W of the second groove 31 is preferably 100 μm or more, and is preferably greater than the width of the first groove 21, which is preferably 100 μm or less.
[0057] In the example shown in Figure 2, a first laser light source 20 is arranged on the side facing the optical functional layer 2, and a second laser light source 30 separate from the first laser light source 20 is arranged on the side facing the protective layer 3, but the present invention is not limited to this, and it is also possible for the first laser light source 20 to also serve as the second laser light source 30. When the first laser light source 20 is also used as the second laser light source 30, for example, as shown in Figure 2 (a), the first laser light source 20 (second laser light source 30) is placed on the side facing the optical functional layer 2, and a first processing groove 21 is formed in the optical functional layer 2 using the first laser light source 20 (second laser light source 30), and then the composite material 10 is inverted upside down using a known inversion mechanism so that the first laser light source 20 (second laser light source 30) faces the protective layer 3, and a second processing groove 31 is formed in the protective layer 3 using the first laser light source 20 (second laser light source 30). Alternatively, as shown in Figure 2(b), a first laser light source 20 (second laser light source 30) is placed on the side facing the protective layer 3, and a second processing groove 31 is formed in the protective layer 3 using the first laser light source 20 (second laser light source 30).After that, the composite material 10 is inverted upside down using a known inversion mechanism so that the first laser light source 20 (second laser light source 30) faces the optical functional layer 2, and the first processing groove 21 is formed in the optical functional layer 2 using the first laser light source 20 (second laser light source 30).
[0058] In addition, in the processed groove forming step, as a preferred embodiment, it is also possible to remove the resin forming the optical functional layer 2 so that a part of the optical functional layer 2 in the thickness direction remains as a residue. In addition, in the present embodiment, as a preferred embodiment, the resin forming the protective layer 3 is removed so that a part of the pressure-sensitive adhesive layer 3b of the protective layer 3 in the thickness direction remains as a residue. The thickness of the residue is preferably 1 to 30 μm, and more preferably 1 to 10 μm, for both the optical functional layer 2 and the protective layer 3. In this way, by removing the resin so that a residue remains, the thermal damage to the brittle material layer 1 is reduced compared to the case where the resin forming the optical functional layer 2 and the protective layer 3 along the planned division line DL is completely removed, and the edge surface of the brittle material layer 1 is less likely to develop cracks, which is an advantage.
[0059] [Machining mark formation process] As shown in Figure 2 (c), in the machining mark forming process, after the machining groove forming process, laser light (ultrashort pulse laser light) L3 oscillated (pulsed) from an ultrashort pulse laser light source 40 is irradiated to the brittle material layer 1 along the planned dividing line DL from the second machining groove 31 side to remove the brittle material that forms the brittle material layer 1, thereby forming a machining mark 11 along the planned dividing line DL. The manner in which the laser light L3 is irradiated along the planned division line DL (the manner in which the laser light L3 is scanned relatively) can be the same as the manner in which the laser light L1 described above is irradiated along the planned division line DL, so a detailed explanation will be omitted here.
[0060] The brittle material forming the brittle material layer 1 is removed by utilizing the filamentation phenomenon of the laser light L3 emitted from the ultrashort pulse laser light source 40, or by applying a multi-focus optical system (not shown) or a Bessel beam optical system (not shown) to the ultrashort pulse laser light source 40. The use of the filamentation phenomenon of ultrashort pulsed laser light and the application of a multi-focus optical system or a Bessel beam optical system to an ultrashort pulsed laser light source are described in Non-Patent Document 1. Trumpf, Germany, also sells products related to glass processing in which a multi-focus optical system is applied to an ultrashort pulsed laser light source. As described above, the use of the filamentation phenomenon of ultrashort pulsed laser light and the application of a multi-focus optical system or a Bessel beam optical system to an ultrashort pulsed laser light source are publicly known, and therefore detailed description thereof will be omitted here.
[0061] The processing marks 11 formed in the processing mark forming step of this embodiment are perforated through holes along the planned dividing line DL as described in Patent Document 2, for example. The pitch of the through holes along the planned dividing line DL is determined by the repetition frequency of the pulse oscillation and the relative moving speed (processing speed) of the laser light L3 with respect to the composite material 10. In order to simply and stably perform the composite material dividing step described later, the pitch of the through holes is preferably set to 10 μm or less, and more preferably set to 5 μm or less. In many cases, the diameter of the through holes is 5 μm or less. However, the processing marks 11 are not limited to perforated through holes along the planned division line DL. If the relative movement speed along the planned division line DL between the laser light L3 oscillated from the ultrashort pulse laser light source 40 and the brittle material layer 1 is set to be slow, or if the repetition frequency of the pulse oscillation of the ultrashort pulse laser light source 40 is set to be high, a through hole (long hole) that is integrally connected along the planned division line DL is formed as the processing marks 11.
[0062] The wavelength of the laser light L3 emitted from the ultrashort pulse laser light source 40 is preferably 500 nm to 2500 nm, which shows high light transmittance when the brittle material forming the brittle material layer 1 is glass. In order to effectively induce a nonlinear optical phenomenon (multiphoton absorption), the pulse width of the laser light L3 is preferably 100 picoseconds or less, and more preferably 50 picoseconds or less. The oscillation form of the laser light L3 may be single pulse oscillation or burst mode multi-pulse oscillation. As shown in FIG. 2(c), the spot diameter D at the irradiated position of the laser beam L3 on the brittle material layer 1 is set to, for example, 100 μm, and as described above, the width W of the second processed groove 31 is equal to or larger than this spot diameter D.
[0063] The method may further include a cleaning step of removing the resin residue forming the protective layer 3 by applying various wet or dry cleaning methods to the second processed groove 31 formed in the processed groove forming step before the processed mark forming step. If the resin residue forming the protective layer 3 is removed in the cleaning step, even if the brittle material layer 1 is irradiated with the laser light L3 oscillated from the ultrashort pulse laser light source 40 from the second processed groove 31 side in the processed mark forming step, the laser light L3 is not affected by the resin residue, and a more appropriate processed mark 11 can be formed in the brittle material layer 1.
[0064] [Composite material cutting process] As shown in Fig. 2(d), in the composite material dividing step, after the processing mark forming step, an external force is applied along the planned dividing line DL to divide the composite material 10. In the example shown in Fig. 2(d), the composite material 10 is divided into composite material pieces 10a and 10b. The composite dividing step is particularly necessary when the processing marks 11 formed in the processing mark forming step are perforated through holes along the planned dividing line DL, or when the resin forming the optical functional layer 2 is removed so that a part of the optical functional layer 2 in the thickness direction remains as a residue (residue remains at the bottom of the first processing groove 21). When the processing marks 11 are through holes (long holes) integrally connected along the planned dividing line DL, and no residue remains at the bottom of the first processing groove 21, the composite material 10 can be divided at the same time as the processing mark forming step is performed, and therefore the composite dividing step is not necessarily required. Examples of methods for applying an external force to the composite material 10 include mechanical breaking (mountain folding), heating the area near the planned cutting line DL with infrared laser light, applying vibration with an ultrasonic roller, and suction and lifting with a suction cup.
[0065] Hereinafter, the peeling method and offset method used when forming the second groove 31 in the groove forming step of the dividing method according to this embodiment will be described in order.
[0066] (peeling method) Fig. 3 is a cross-sectional view for explaining the outline of the procedure of the peeling method in the groove forming process. The peeling method is carried out in the order of Fig. 3(a), (b) and (d). Fig. 3(c) is an enlarged view of the area surrounded by the dashed line C in Fig. 3(b). As shown in Figures 3(a) and 3(b), in the peeling method, the irradiation position of the laser light L2 emitted from the second laser light source 30 on the protective layer 3 is shifted in a direction perpendicular to the planned division line DL (X direction in the example shown in Figure 3), and the laser light L2 is irradiated to the protective layer 3 along the planned division line DL at each irradiation position (position A1 shown in Figure 3(a) and position A2 shown in Figure 3(b)). Specifically, in this embodiment, the laser light L2 emitted from the second laser light source 30 is irradiated to positions A1 and A2 that are equidistant from the planned division line DL in a direction perpendicular to the planned division line DL (X direction) based on the planned division line DL. As a result, processed grooves 31a and 31b are formed at each irradiation position A1 and A2. The distance between the processed grooves 31a, 31b in the X direction (the distance between the irradiation positions A1, A2) is set to be equal to or larger than the spot diameter D (see Figure 2 (c)) at the irradiation position of the ultrashort pulse laser light L3 on the brittle material layer 1 in the processed mark formation process. As described above, in the present embodiment, as a preferred embodiment, the resin forming the protective layer 3 is removed by irradiating the protective layer 3 with the laser beam L2 so that a part of the pressure-sensitive adhesive layer 3b of the protective layer 3 in the thickness direction remains as a residue (see FIG. 3(c)). As described above, the thickness T of the residue is preferably 1 to 30 μm, and more preferably 1 to 10 μm.
[0067] Next, as shown in Fig. 3(d), in the peeling method, the resin forming the protective layer 3 present between the irradiation positions A1 and A2 is peeled off to form the second processed groove 31. The resin can be peeled off by appropriately using a known peeling device. As described above, since the separation distance between the processed grooves 31a and 31b is equal to or larger than the spot diameter D of the ultrashort pulsed laser light L3, the width W (see Fig. 2(c)) of the second processed groove 31 is also equal to or larger than the spot diameter D of the ultrashort pulsed laser light L3. In addition, when the resin forming the protective layer 3 between each of the irradiation positions A1 and A2 is peeled off by the peeling method, as can be seen from Figure 3(c) or (d), a part of the adhesive layer 3b in the thickness direction will remain as a residue in the vicinity of each of the irradiation positions A1 and A2, but in other parts, the entire protective layer 3 including the adhesive layer 3b will peel off, and it is expected that the surface of the brittle material layer 1 will be exposed.
[0068] According to the peeling method described above, when the ultrashort pulse laser light L3 is irradiated onto the intended cutting line DL (see Figure 2 (c)), the irradiation positions A1, A2 of the laser light L2 emitted from the second laser light source 30 and the irradiation position of the ultrashort pulse laser light L3 will be shifted by 1 / 2 the width W of the second processing groove 31. Therefore, even if the output of the laser light L2 emitted from the second laser light source 30 is set to a relatively large value in the processing groove forming process, and the resin forming the protective layer 3 is removed to expose the surface of the brittle material layer 1 and cause some thermal damage, the ultrashort pulse laser light L3 is unlikely to be irradiated to the same location, and therefore cracks are unlikely to occur on the end surface of the brittle material layer 1.
[0069] Fig. 4 is a plan view for explaining the outline of the procedure of the peeling method and the processing mark forming step in the processing groove forming step when dividing the composite material 10 into four rectangular composite material pieces. Fig. 4(a) to (c) show the outline of the procedure of the peeling method, and Fig. 4(d) shows the outline of the procedure of the processing mark forming step. In Fig. 4, the second laser light source 30 and the ultrashort pulse laser light source 40 are shown in a perspective view for the sake of convenience. As shown in Fig. 4(a), in the peeling method, the irradiation position of the laser light L2 emitted from the second laser light source 30 on the protective layer 3 is shifted in a direction perpendicular to the planned division line DL, and the laser light L2 is irradiated to the protective layer 3 along the planned division line DL at each irradiation position. Specifically, in the example shown in Fig. 4(a), the laser light L2 is irradiated to a position (position shown by a solid line) shifted inward from the planned division line DL by 1 / 2 the width W (see Fig. 2(c)) of the second processed groove 31. The parts indicated by the symbols 31a and 31b in Fig. 4(a) correspond to the processed grooves 31a and 31b shown in Fig. 3.
[0070] Next, in the peeling method, the resin forming the protective layer 3 present between each irradiation position is peeled off to form a second processed groove 31. Fig. 4(b) shows the resin forming the peeled protective layer 3, and Fig. 4(c) shows the composite material 10 after peeling. In the example shown in Fig. 4(b), not only the resin forming the protective layer 3 present between each irradiation position (the resin present in the cross-shaped region in Fig. 4(b)), but also the resin forming the protective layer 3 located outside the irradiation positions is peeled off at the same time.
[0071] Next, as shown in FIG. 4(d), in the processing mark forming step, ultrashort pulsed laser light L3 oscillated from an ultrashort pulsed laser light source 40 is irradiated onto the intended division line DL. This (or by further performing a composite cutting step) allows the composite to be cut into four rectangular pieces.
[0072] (Offset method) 5A to 5D are cross-sectional views for explaining the outline of the offset method in the groove forming step. The offset method is carried out in the order of FIG. As shown in Fig. 5(a) to (c), in the offset method, the irradiation position of the laser light L2 oscillated from the second laser light source 30 on the protective layer 3 is sequentially shifted in a direction perpendicular to the planned division line DL (X direction in the example shown in Fig. 5), and the laser light L2 is irradiated to the protective layer 3 along the planned division line DL at each irradiation position (position B1 shown in Fig. 5(a), position B2 shown in Fig. 5(b), and position B3 shown in Fig. 5(c). Specifically, in this embodiment, the laser light L2 oscillated from the second laser light source 30 is sequentially shifted at a predetermined pitch (for example, a pitch of about 30 μm, which is the same size as the spot diameter of the laser light L2) from position B1 to position B3, which are equidistant in a direction perpendicular to the planned division line DL (X direction) based on the planned division line DL, and is irradiated to each position. As a result, the width of the processed groove 31c formed at each irradiation position is sequentially increased, and finally, as shown in Fig. 5(d), the second processed groove 31 is formed. By setting the range for shifting the irradiation position of the laser light L2 (the distance between irradiation positions B1, B3) to be greater than or equal to the spot diameter D (see Figure 2(c)) at the irradiation position of the ultrashort pulsed laser light L3 on the brittle material layer 1 in the processing mark formation process, the width W (see Figure 2(c)) of the second processing groove 31 can be made greater than or equal to the spot diameter D of the ultrashort pulsed laser light L3.
[0073] In addition, in a preferred embodiment of the offset method, the protective layer 3 is irradiated with the laser light L2 to remove the resin forming the protective layer 3 so that a part of the adhesive layer 3b of the protective layer 3 in the thickness direction remains as a residue. In particular, when the offset method is applied, the protective layer 3 is irradiated with the laser light L2 oscillated from the second laser light source 30 at more locations than when the peeling method is applied, so that the brittle material layer 1 is more susceptible to thermal damage. Therefore, leaving a part of the adhesive layer 3b in the thickness direction as a residue is particularly effective when the offset method is applied. Furthermore, when the offset method is applied, the laser light L2 emitted from the second laser light source 30 is irradiated to more locations on the protective layer 3 than when the peeling method is applied, and this makes it easier for fumes to be generated from the adhesive layer 3b of the protective layer 3. Therefore, in order to prevent the generation of fumes when the offset method is applied, it is preferable that the adhesive layer 3b be a urethane-based adhesive layer.
[0074] Fig. 6 is a plan view for explaining the outline of the offset method and the machining mark forming step in the machining groove forming step when dividing the composite material 10 into four rectangular composite material pieces. Fig. 6(a) shows the outline of the offset method, and Fig. 6(b) shows the outline of the machining mark forming step. In Fig. 6, the second laser light source 30 and the ultrashort pulse laser light source 40 are shown in perspective for the sake of convenience. As shown in Fig. 6(a), in the offset method, the irradiation position of the laser light L2 emitted from the second laser light source 30 on the protective layer 3 is sequentially shifted in a direction perpendicular to the planned division line DL, and the laser light L2 is irradiated to the protective layer 3 along the planned division line DL at each irradiation position. Specifically, in the example shown in Fig. 6(a), the laser light L2 is irradiated to a range of positions (positions shown by solid lines) shifted inward and outward by 1 / 2 of the width W (see Fig. 2(c)) of the second processed groove 31 from the planned division line DL, so that the width of the processed groove 31c formed at each irradiation position is sequentially increased. As a result, the second processed groove 31 (the area not hatched with diagonal lines in Fig. 6(b)) is formed as shown in Fig. 6(b).
[0075] Next, as shown in FIG. 6(b), in the processing mark forming step, ultrashort pulsed laser light L3 oscillated from an ultrashort pulsed laser light source 40 is irradiated onto the intended division line DL. This (or by further performing a composite cutting step) allows the composite to be cut into four rectangular pieces.
[0076] According to the above-described dividing method according to the present embodiment, in the cutting groove forming step, the resin forming the optical function layer 2 and the resin forming the protective layer 3 are removed to form the first cutting groove 21 and the second cutting groove 31 along the planned dividing line DL, and then in the cutting mark forming step, the brittle material forming the brittle material layer 1 is removed from the second cutting groove 31 side to form the cutting mark 11 along the same planned dividing line DL. The second cutting groove 31 formed in the cutting groove forming step is formed so that its width W is equal to or greater than the spot diameter D at the irradiation position of the laser light (ultrashort pulse laser light) L3 oscillated from the ultrashort pulse laser light source 40 in the cutting mark forming step on the brittle material layer 1, so that the brittle material layer 1 can be divided without causing cracks on the end face of the brittle material layer 1.
[0077] Hereinafter, an example of the results of a test performed to cut the composite material 10 using the cutting method according to this embodiment (Examples 1 to 5) and the cutting methods according to comparative examples (Comparative Examples 1 and 2) will be described. Fig. 7 shows an example of main test conditions and test results when the peeling method is applied in the groove forming process as an embodiment. Fig. 8 shows an example of main test conditions and test results when the offset method is applied in the groove forming process as an embodiment.
[0078] <Example 1> [Fabrication of optical functional layer 2] As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a glass transition temperature (Tg) of about 75° C. was used, and one side of this resin substrate was subjected to a corona treatment. On the other hand, 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1 was added to 13 parts by weight of potassium iodide and dissolved in water to prepare a PVA aqueous solution (coating liquid). The above-mentioned aqueous PVA solution was applied to the corona-treated surface of the above-mentioned resin substrate and dried at 60° C. to form a PVA-based resin layer having a thickness of 13 μm, thereby producing a laminate.
[0079] The laminate produced as described above was uniaxially stretched 2.4 times in the longitudinal direction (machine direction) in an oven at 130° C. (auxiliary in-air stretching treatment). Next, the uniaxially stretched laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the above laminate was immersed in a dye bath (iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the finally obtained polarizer would be a desired value (dyeing treatment). Next, the laminate was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40°C for 30 seconds (crosslinking treatment). Next, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching process). Next, the above laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Finally, the above laminate was brought into contact with a stainless steel heated roll having a surface temperature maintained at about 75° C. while being dried in an oven maintained at about 90° C. (drying shrinkage treatment). In this manner, a polarizer having a thickness of about 5 μm was formed on the resin substrate, and a laminate having a resin substrate / polarizer structure was produced.
[0080] Next, an acrylic protective film (thickness: 40 μm) was attached to one surface (the surface opposite to the resin substrate side) of the polarizer constituting the above laminate to prepare a polarizing film. Then, the resin substrate was peeled off from the polarizing film, and a polyethylene terephthalate release film (thickness: 38 μm) was attached to the peeled surface via an acrylic adhesive (thickness: 20 μm) to prepare the main body of the optical functional layer 2. In addition, an epoxy adhesive was prepared as the adhesive by mixing 70 parts by weight of Celloxide 2021P (manufactured by Daicel Chemical Industries, Ltd.), 5 parts by weight of EHPE3150, 19 parts by weight of Aron Oxetane OXT-221 (manufactured by Toa Gosei Co., Ltd.), 4 parts by weight of KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.), and 2 parts by weight of CPI101A (manufactured by San-Apro Co., Ltd.). The combination of the main body of the optical functional layer 2 and the adhesive constitutes the optical functional layer 2.
[0081] [Preparation of Laminate of Brittle Material Layer 1 and Optical Functional Layer 2] As the brittle material layer 1, a glass film (manufactured by Nippon Electric Glass Co., Ltd., product name "OA-10G", thickness: 100 μm) was prepared. Next, the brittle material layer 1 and the main body of the optical functional layer 2 were bonded together via the adhesive. At this time, the main body of the optical functional layer 2 was arranged so that the acrylic protective film was on the brittle material layer 1 side. Next, the adhesive was irradiated with ultraviolet light (500 mJ / cm 2 ) from a high-pressure mercury lamp. 2 ) and the adhesive was cured to produce a laminate of a brittle material layer 1 and an optical functional layer 2. The adhesive had a thickness of 5 μm after curing.
[0082] [Preparation of composite material 10] Next, as shown in FIG. 7, a surface protection film having an acrylic adhesive layer (manufactured by Nitto Denko Corporation, product name "RP207") was prepared as the protection layer 3. The base layer 3a of the protective layer 3 is formed from an untreated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Polyester Corporation, Diafoil T100 #38) having a thickness of 38 μm. The adhesive layer 3b of the protective layer 3 is prepared as follows. First, 100 parts by weight of 2-ethylhexyl acrylate and 4 parts by weight of 2-hydroxyethyl acrylate are copolymerized in ethyl acetate so that the monomer content is 35% to obtain a solution containing an acrylic polymer having a weight average molecular weight of 600,000. Next, 4 parts by weight of an isocyanate crosslinking agent (Coronate HX, manufactured by Nippon Polyurethane Industry Co., Ltd.) having an isocyanurate ring is mixed with 100 parts by weight of the acrylic polymer (dry weight) in this solution, and ethyl acetate is further added to prepare an adhesive solution in which the solid content concentration is adjusted to 20%. Finally, this adhesive solution is applied to the base layer 3a so that the dry film thickness is 20 μm, and dried at 140° C. for 2 minutes to form the adhesive layer 3b. The protective layer 3 (RP207) includes the base layer 3a and the adhesive layer 3b prepared as described above. The protective layer 3 and the brittle material layer 1 of the laminate of the brittle material layer 1 and the optical function layer 2 were bonded together via the adhesive layer 3b of the protective layer 3 to prepare a composite material 10.
[0083] [Groove formation process (forming first groove 21)] After the composite material 10 produced as described above was separated into sheets, the first processed groove 21 was formed in the optical function layer 2. Specifically, a TLSU series (CO2 laser light source with an oscillation wavelength of 9.4 μm, a pulse oscillation repetition frequency of 12.5 kHz, and a power of 250 W of the laser light L1) manufactured by Takei Electric Co., Ltd. was used as a laser processing device equipped with an optical system and a control device for controlling the scanning of the first laser light source 20 and the laser light L1, the output of the laser light L1 oscillated from the first laser light source 20 was set to 11.8 W, and the laser light L1 was focused to a spot diameter of 150 μm at the irradiation position on the optical function layer 2 using a focusing lens, and was irradiated to the optical function layer 2 along the planned division lines DL (plurality of planned division lines set in a lattice pattern) of the composite material 10. The relative movement speed (processing speed) of the laser light L1 with respect to the composite material 10 was set to 400 mm / sec. As a result, the resin forming the optical function layer 2 was removed, and the first processed groove 21 was formed along the planned division lines DL. At this time, the resin was removed so that a part of the resin forming the optical functional layer 2 remained as a residue (thickness: 10 to 20 μm) on the bottom of the first processed groove 21.
[0084] [Groove forming process (forming second groove 31)] Next, the second processed groove 31 was formed in the protective layer 3. Specifically, as in the case of forming the first processed groove 21, a TLSU series (CO2 laser light source with an oscillation wavelength of 9.4 μm, a repetition frequency of pulse oscillation of 12.5 kHz, and a power of the laser light L2 of 250 W) manufactured by Takei Electric Co., Ltd. was used as a laser processing device equipped with an optical system and a control device for controlling the scanning of the second laser light source 30 and the laser light L2. As shown in FIG. 7, the output of the laser light L2 oscillated from the second laser light source 30 was set to 10.5 W, and the laser light L2 was focused to a spot diameter of 120 to 130 μm at the irradiation position on the protective layer 3 using a focusing lens, and the protective layer 3 was irradiated along the planned division lines DL of the composite material 10 (a plurality of planned division lines set in a lattice pattern). The relative movement speed (processing speed) of the laser light L2 with respect to the composite material 10 was set to 400 mm / sec. Then, by applying a peeling method, the second processed groove 31 with a width of 200 μm was formed as shown in FIG. 7. When the protective layer 3 was irradiated with the laser beam L2, the resin was removed so that no part of the resin forming the protective layer 3 remained as a residue at the irradiated position (thickness: 0 μm) as shown in FIG.
[0085] [Machining mark formation process] After the above-mentioned groove forming process, a trace forming process was carried out. Specifically, an ultrashort pulse laser light source 40 with an oscillation wavelength of 1064 nm, a pulse width of 10 picoseconds for the laser light L3, a repetition frequency of pulse oscillation of 50 kHz, and an average power of 10 W was used, and the laser light L3 emitted from the ultrashort pulse laser light source 40 was irradiated onto the brittle material layer 1 of the composite material 10 from the second groove 31 side through a multi-focus optical system. The spot diameter D at the irradiation position of the laser light L3 on the brittle material layer 1 was set to 100 μm. When the relative movement speed (processing speed) of the laser light L3 with respect to the composite material 10 was set to 100 mm / sec and the laser light L3 was scanned along the planned division line DL, a perforated through hole (diameter about 1 to 2 μm) with a pitch of 2 μm was formed as the trace 11.
[0086] [Composite material cutting process] After the above-mentioned machining mark forming process, the composite material cutting process was carried out. Specifically, a Keyence MLG-9300 (oscillation wavelength 10.6 μm, laser light power 30 W) was used as a laser processing device equipped with a CO2 laser light source and an optical system and a control device for controlling the scanning of the laser light, and the output of the laser light emitted from the laser light source was set to 80% (i.e., output 24 W) and focused to a spot diameter of 0.7 mm using a focusing lens (energy density at this time was 62 W / m 2 ), the brittle material layer 1 was irradiated from the protective layer 3 side along the planned dividing line DL of the composite material 10. At this time, the relative moving speed of the laser light with respect to the composite material 10 was set to 500 mm / sec. Finally, a mechanical external force was applied to the composite material 10 to break up the resin residue remaining at the bottom of the first groove 21 after the groove formation step, and the composite material 10 was broken up.
[0087] When the end face of the brittle material layer 1 of the composite material 10 (composite material piece) cut by the cutting method of Example 1 was visually observed, it was found that the brittle material layer 1 was cut without any problems and no cracks were generated, as shown in Figure 7.
[0088] <Example 2> As shown in Figure 7, when forming the second processing groove 31, the output of the laser light L2 emitted from the second laser light source 30 was set to 8.0 W, and the composite material 10 was divided under the same conditions as in Example 1, except that the resin was removed so that a portion of the resin (adhesive layer 3b) forming the protective layer 3 remained as a residue (thickness: 10 μm) at the irradiated position. When the end face of the brittle material layer 1 of the composite material 10 (composite material piece) cut by the cutting method of Example 2 was visually observed, it was found that the brittle material layer 1 was cut without any problems and no cracks were generated, as shown in Figure 7.
[0089] <Comparative Example 1> An attempt was made to divide the composite material 10 under the same conditions as in Example 1, except that, when forming the second processed groove 31, the laser light L2 oscillated from the second laser light source 30 was irradiated only once (without applying the peeling method) onto the protective layer 3 on the planned dividing lines DL of the composite material 10 (plural planned dividing lines set in a lattice pattern). As shown in Fig. 7, the width of the second processed groove 31 formed in Comparative Example 1 was 30 µm, which was smaller than the spot diameter D (100 µm) at the irradiation position of the laser light L3 oscillated from the ultrashort pulse laser light source 40 on the brittle material layer 1 in the processed mark forming step. As shown in FIG. 7, in the cutting method according to Comparative Example 1, no processed traces 11 penetrating the brittle material layer 1 were formed, and the composite material 10 could not be cut.
[0090] <Example 3> A composite material 10 was produced under the same conditions as in Example 1, except for the following points (1) to (3), and the composite material 10 was cut. (1) As shown in FIG. 8, a surface protection film having a urethane adhesive layer (manufactured by Nitto Denko Corporation, product name "AW700EC") was prepared as the protection layer 3. The base material layer 3a of the protective layer 3 is formed from a base material made of polyester resin, "Lumirror S10" (thickness: 38 μm, manufactured by Toray Industries, Inc.). The adhesive layer 3b of the protective layer 3 is prepared as follows. First, as the polyol, Preminol S3011 (manufactured by Asahi Glass Co., Ltd., Mn=10000), which is a polyol having three OH groups, Sannix GP-3000 (manufactured by Sanyo Chemical Industries Co., Ltd., Mn=3000), which is a polyol having three OH groups, and Sannix GP-1000 (manufactured by Sanyo Chemical Industries Co., Ltd., Mn=1000), which is a polyol having three OH groups, are used. As the polyfunctional isocyanate compound, Coronate HX (manufactured by Nippon Polyurethane Industry Co., Ltd.), which is a polyfunctional alicyclic isocyanate compound, is used. As the catalyst, "Nasem Ferric" (trade name) manufactured by Nippon Chemical Industries Co., Ltd. is used. As the deterioration inhibitor, Irganox1010 (manufactured by BASF) is used. As the fatty acid ester, isopropyl myristate (manufactured by Kao Corporation, trade name "Exepar IPM", Mn = 270) or cetyl 2-ethylhexanoate (manufactured by Nisshin Oillio Group, trade name "Salacos 816T", Mn = 368) is used. Then, 1-ethyl-3-methylimidazolium bis(fluoromethanesulfonyl)imide (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., trade name "AS110"), both-end type polyether modified silicone oil (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KF-6004"), and ethyl acetate as a dilution solvent are added to these and mixed and stirred to prepare a urethane-based adhesive composition. Then, the prepared urethane-based adhesive composition is applied to the above-mentioned base layer 3a with a fountain roll so that the thickness after drying is 10 μm, and cured and dried under conditions of a drying temperature of 130°C and a drying time of 30 seconds to form an adhesive layer 3b. The protective layer 3 (AW700EC) includes the base layer 3a and the adhesive layer 3b prepared as described above. The protective layer 3 and the brittle material layer 1 of the laminate of the brittle material layer 1 and the optical function layer 2, which are the same as those in Example 1, were bonded together through the adhesive layer 3b of the protective layer 3 to prepare a composite material 10. (2) When forming the second groove 31, the offset method is applied. (3) As shown in Figure 8, when forming the second groove 31, the output of the laser light L2 emitted from the second laser light source 30 was set to 4.3 W, and the resin forming the protective layer 3 (adhesive layer 3b) was removed so that a portion of the resin (thickness: 7.5 μm) remained as a residue at the irradiated position. When the end face of the brittle material layer 1 of the composite 10 (composite piece) cut by the cutting method of Example 3 was visually observed, it was found that the brittle material layer 1 was cut without any problems and no cracks were generated, as shown in Figure 8.
[0091] <Example 4> As shown in Figure 8, when forming the second processing groove 31, the output of the laser light L2 emitted from the second laser light source 30 was set to 4.9 W, and the composite material 10 was divided under the same conditions as in Example 3, except that the resin (adhesive layer 3b) forming the protective layer 3 was removed so that a portion of the resin (adhesive layer 3b) remained as a residue with a thickness of 2.1 μm at the irradiation position. When the end face of the brittle material layer 1 of the composite 10 (composite piece) cut by the cutting method of Example 4 was visually observed, it was found that the brittle material layer 1 was cut without any problems and no cracks were generated, as shown in Figure 8.
[0092] <Example 5> As shown in Figure 8, when forming the second processing groove 31, the output of the laser light L2 emitted from the second laser light source 30 was set to 5.1 W, and the composite material 10 was divided under the same conditions as in Example 3, except that the resin was removed so that no part of the resin forming the protective layer 3 remained as residue at the irradiated position (thickness: 0 μm). When the end face of the brittle material layer 1 of the composite 10 (composite piece) cut by the cutting method of Example 5 was visually observed, it was found that the brittle material layer 1 was cut without any problems and no cracks were generated, as shown in Figure 8.
[0093] <Comparative Example 2> An attempt was made to divide the composite material 10 under the same conditions as in Example 5, except that, when forming the second processed groove 31, the laser light L2 oscillated from the second laser light source 30 was irradiated only once (the offset method was not applied) onto the protective layer 3 on the planned dividing lines DL of the composite material 10 (plural planned dividing lines set in a lattice pattern) of the composite material 10. As shown in Fig. 8, the width of the second processed groove 31 formed in Comparative Example 2 was 30 µm, which was smaller than the spot diameter D (100 µm) at the irradiation position of the laser light L3 oscillated from the ultrashort pulse laser light source 40 in the processing mark forming step on the brittle material layer 1. As shown in FIG. 8, in the cutting method according to Comparative Example 2, no processed traces 11 penetrating the brittle material layer 1 were formed, and the composite material 10 could not be cut. [Explanation of symbols]
[0094] 1...brittle material layer 2...Optical functional layer 3...Protective layer 3a...Base material layer 3b...Adhesive layer 10...Composite material 11... Machining marks 20...First laser light source 21...1st machining groove 30...Second laser light source 31...2nd machining groove 40 Ultrashort pulse laser light source D Spot diameter DL... Planned division line L1, L2, L3...Laser light W: Width of second machining groove
Claims
1. A method for dividing a composite material having a brittle material layer on one side of which a resin optical functional layer is laminated, and a resin protective layer on the other side of which the brittle material layer is laminated, comprising the steps of: a processing groove forming step of irradiating the optical functional layer with a laser beam emitted from a first laser light source along a planned dividing line of the composite material to remove a resin forming the optical functional layer, thereby forming a first processing groove along the planned dividing line, and irradiating the protective layer with a laser beam emitted from a second laser light source along the planned dividing line to remove a resin forming the protective layer, thereby forming a second processing groove along the planned dividing line; and a processing mark forming step of irradiating the brittle material layer with a laser beam oscillated from an ultrashort pulse laser source along the planned dividing line from the second processing groove side after the processing groove forming step, thereby removing the brittle material forming the brittle material layer, thereby forming a processing mark along the planned dividing line, In the processing groove forming step, the resin forming the protective layer is removed so that the width of the second processing groove is equal to or larger than the spot diameter at the irradiation position of the brittle material layer with the laser light oscillated from the ultrashort pulse laser light source in the processing mark forming step. How to separate composite materials.
2. In the processing groove forming step, the irradiation position of the laser light oscillated from the second laser light source onto the protective layer is sequentially shifted in a direction perpendicular to the planned division line, and the laser light is irradiated onto the protective layer along the planned division line at each irradiation position, thereby forming the second processing groove. A method for dividing a composite material according to claim 1.
3. In the groove forming step, the resin forming the protective layer is removed so that the width of the second groove is 100 μm or more. A method for dividing a composite material according to claim 1 or 2.
4. The protective layer includes a base layer and a pressure-sensitive adhesive layer disposed on the brittle material layer side, In the processing groove forming step, the resin forming the protective layer is removed so that a part of the pressure-sensitive adhesive layer in the thickness direction remains. A method for dividing a composite material according to any one of claims 1 to 3.
5. The protective layer includes a base layer and a urethane-based pressure-sensitive adhesive layer disposed on the brittle material layer side. A method for dividing a composite material according to any one of claims 1 to 4.
6. The second laser light source is CO 2 A laser light source. A method for dividing a composite material according to any one of claims 1 to 5.
7. The brittle material layer includes glass, and the optical functional layer includes a polarizing film. A method for dividing a composite material according to any one of claims 1 to 6.
Citation Information
Patent Citations
Controlled ablation and surface modification for marking an electronic device
CN110666360A
Dividing method of semiconductor wafer
JP2005142398A
Reinforced glass member working method
JP2014043363A
Production method of flexible film
JP2017145188A
Cutting method and cutting device of metal film-equipped brittle material substrate
JP2018170475A