Lithium battery positive plate as well as preparation method and application thereof

By applying an insulating coating of components such as ethylene-vinyl acetate polymer on the active material layer of the positive electrode sheet of the lithium battery, the problem of poor insulation layer coating during laser cutting is solved, and the safety and process of lithium batteries are improved Consistency enables effective protection of the cut edge.

CN119069629AActive Publication Date: 2024-12-03HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202411118827.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-03
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

During the lithium battery manufacturing process, metal molten beads caused by laser cutting are not covered by an effective insulating layer, resulting in the risk of diaphragm breakdown and overlap short circuit. The existing ceramic coating methods generate dust during laser cutting, affecting the production environment and products. It is difficult to control the mutual dissolution of insulating slurry and active substances.

Method used

The active material layer is directly coated with an insulating coating of special materials. The coating components include ethylene-vinyl acetate polymer, plasticizer, binder and antioxidant. It is uniformly applied during the laser cutting process through the melting state to form a The hot melt adhesive layer covers the edges of the cut to avoid mutual dissolution.

Benefits of technology

It effectively solves the insulation problem of laser cutting edges, improves the safety and process consistency of lithium batteries, provides double protection, locks metal particles and cuts port burrs, and reduces the risk of diaphragm puncture and positive and negative electrode shorting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069629A_ABST
    Figure CN119069629A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium battery positive plate and a preparation method and application thereof, the edge of the positive plate is coated with an insulating coating made of a special material, and the coating position of the insulating coating is between an active material layer and a tab blank; the insulating coating comprises the following components: an ethylene-vinyl acetate polymer, a plasticizer, a binder and an antioxidant; and the insulating coating is coated on the active material layer and covers a certain width. The insulating coating is low in viscosity, is in a solid state at normal temperature, is in a liquid state at 140 DEG C or above, can be stably and uniformly coated on the surface of a current collector, can be melted by high temperature generated in a laser cutting process, has certain flowability at the moment, and can effectively wrap burrs at an edge notch of a pole piece in a molten state in the cutting process. Therefore, the insulating coating not only has insulation protection on the edge surface of the pole piece, but also has burr coating protection on the notch end face of the pole piece, and the double protection can effectively solve the problems of diaphragm puncture and short circuit of positive and negative electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium battery positive electrode sheet and a preparation method and application thereof. Background Art

[0002] With the rapid development of new energy vehicles and consumer electronics, the market demand for lithium batteries, as an efficient and lightweight energy storage device, continues to grow. However, in the manufacturing process of lithium batteries, how to ensure the safety of batteries has always been the focus of the industry.

[0003] In the manufacturing process of lithium batteries, some abnormal cells are often encountered, such as 0 resistance in the assembly short-circuit test, low formation voltage, large self-discharge, large module pressure difference and other problems. Through the disassembly and analysis of abnormal cells, it was found that the diaphragm corresponding to the blank edge of the positive electrode sheet of the cell had a breakdown point. This is mainly due to the fact that the metal molten beads generated by the cross-sectional port of the current collector during the laser cutting process were not covered by an effective insulating layer. At the same time, the existing manufacturing process generally adopts the method of coating ceramic materials as an insulating layer in a coating process. However, this method will generate a lot of dust during the laser cutting process, which will not only affect the production environment, but also may have an adverse effect on product quality. In addition, the ceramic coating mainly acts on the surface of the foil, and the coating effect on the edge of the laser cutting incision is not good. The burrs generated during the cutting process may still lead to the risk of overlapping short circuits.

[0004] Patent CN113488743A proposes a coating method for modified ceramic slurry, which improves the insulation performance by changing the peeling force after coating. However, this method is still limited to the protective effect of ceramic materials, and has not fundamentally solved the effective coating of the laser cutting cross section.

[0005] Therefore, developing an insulating coating technology that can effectively cover the edge of the laser cutting cut has become an important measure to improve the safety of lithium batteries. At the same time, in order to avoid the problem of mutual dissolution of the insulating slurry and the active material slurry or the difficulty in controlling the gap between the integrated die coating during the process, it is necessary to develop a new insulating layer coating process to meet the safety requirements in the lithium battery manufacturing process. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a lithium battery positive electrode sheet and a preparation method and application thereof, which transfers the difficulty to the laser cutting process and directly applies an insulating coating on the dry material (active substance) positive electrode sheet, thereby effectively solving the problem of mutual dissolution between wet materials.

[0007] The present invention is achieved through the following technical solutions:

[0008] A lithium battery positive electrode sheet, the edge of which is coated with an insulating coating of a special material, the insulating coating being applied between an active material layer and a tab blank; the insulating coating comprising ethylene-vinyl acetate polymer, a plasticizer, a binder and an antioxidant; the insulating coating being applied on the active material layer and covering a certain width.

[0009] By applying an insulating coating of a special material (in a molten state when applied and forming a hot melt adhesive layer after cooling and solidification) on the active material layer (dry material), the problem of mutual dissolution between wet materials can be effectively solved.

[0010] Preferably, the insulating coating has a width of 6 to 8 mm and a thickness of 10 to 15 μm.

[0011] Preferably, the ethylene-vinyl acetate polymer is prepared from ethylene and vinyl acetate by an emulsion method, has a molecular weight of 1280, and has the following structural formula:

[0012]

[0013] Preferably, the mass ratio of each component in the insulating coating is as follows:

[0014] Ethylene-vinyl acetate polymer: plasticizer: binder: antioxidant = 80-85: 0.5-1: 10-15: 1-2.

[0015] Preferably, the plasticizer is dibutyl phthalate or dioctyl phthalate; the binder is polyvinylidene fluoride or polystyrene; and the antioxidant is butylated hydroxyanisole or butylated hydroxytoluene.

[0016] Preferably, the active material layer is lithium iron phosphate or ternary lithium.

[0017] The method for preparing the above-mentioned lithium battery positive electrode sheet comprises the following steps:

[0018] Step 1) In a high pressure reactor, vinyl acetate and K2S2O8 or (NH4)2S2O8 initiator are first added to the prepared emulsion reaction medium, and then ethylene is added at 85°C and 90kg / cm 2 Polymerize under pressure to obtain ethylene-vinyl acetate polymer latex with a vinyl acetate content of 75%;

[0019] Step 2) at a high temperature of 150° C., adding a plasticizer, a binder and an antioxidant to the ethylene-vinyl acetate polymer latex obtained in step 1) in a mass ratio of 0.5-1:10-15:1-2 in sequence; at a high temperature of 220° C., uniformly dispersing and stirring to obtain an insulating coating glue solution; after filtering, cooling to room temperature, and obtaining a solid insulating coating;

[0020] Step 3) using a heating furnace to heat the solid insulating coating obtained in step 2) to above 170° C. to melt it into a flowable glue; the melt flow rate is 170° C. / 2.0 kg, 190° C. / 2.2 kg;

[0021] Step 4) introducing the molten glue obtained in step 3) to the glue coating head through an electric heating tube, wherein the temperature of the heating furnace and the electric heating tube is controlled to be 170° C., and continuous heating is achieved;

[0022] Step 5) starting the electric heating module at a heating temperature of 220° C. to further melt the insulating coating;

[0023] Step 6) The entire glue coating device is installed after the laser cutting and unwinding position and before the laser cutting position. The laser cut electrode sheet that is unwinding and tape-feeding passes horizontally through the conveying roller, and the glue coating device is installed just above the conveying roller; the laser cutting and tape-feeding process is realized by moving the telescopic cylinder up and down to evenly coat the edge of the positive electrode sheet collector, that is, the junction of the positive electrode material area and the blank area; after the front side coating is completed, the cache return mechanism needs to be used to coat the back side;

[0024] Step 7) applying the melted hot melt adhesive to the tab forming area and covering at least a portion of the active material layer, and cooling and solidifying to form a hot melt adhesive layer;

[0025] Step 8) Laser directly cuts the surface of the insulating coating to obtain the preset ear shape and excess waste edge.

[0026] Preferably, in step 8), the width of the insulating coating remaining on the pole piece after laser cutting is 3-4 mm, and both the coating area and the cutting area are located on the pole ear side.

[0027] The above-mentioned lithium battery positive electrode sheet, or the application of the lithium battery positive electrode sheet prepared by the above-mentioned preparation method in the preparation of lithium batteries, is to use the lithium battery positive electrode sheet through a winding or lamination process, and to match it with a diaphragm and a negative electrode sheet to prepare a qualified winding core, and then to form a lithium battery together with an electrolyte and a shell structure.

[0028] Preferably, the winding or lamination process adopts staggered coating to achieve the negative electrode cut corresponding to the positive electrode insulation layer, specifically as follows: in the laser cutting process, the positive electrode cuts the insulation layer and the negative electrode cuts the active material area; during the assembly process, the negative electrode active material area covers the positive electrode active material area, and the positive electrode insulation layer covers the negative electrode active material area.

[0029] Preferably, the phase difference between the negative electrode active material region covering the positive electrode active material region is 3.5 mm; and the phase difference between the positive electrode insulating layer covering the negative electrode active material region is 1 mm.

[0030] A lithium battery comprises the above-mentioned lithium battery positive electrode sheet, or the lithium battery positive electrode sheet prepared by the above-mentioned preparation method.

[0031] The beneficial effects of the present invention are as follows:

[0032] (1) The principle of the present invention is that when the laser is used to cut the pole ear at the edge of the pole piece, the colloid will absorb light under a specific laser wavelength, so that the pole piece can be laser cut at a specific power without shrinking the glue layer. The insulating coating of the present invention has low viscosity, is solid at room temperature, and is liquid above 140°C. It can be stably and evenly coated on the surface of the current collector. The high temperature generated by the laser cutting process can melt the insulating coating. At this time, the coating has a certain fluidity. The molten state during the cutting process can effectively cover the burrs on the edge of the pole piece. Therefore, the insulating coating can be used in conjunction with different glue coating equipment, and has good wettability to the substrate, providing a higher adhesion force. During use, it can better lock metal particles and cutting port burrs, and has both insulation protection on the edge surface of the pole piece and burr coating protection on the end face of the pole piece cut. The double protection can effectively solve the problems of diaphragm puncture and positive and negative short circuit.

[0033] (2) The insulating coating preparation method of the present invention is simple, and the coating process avoids the coating process. Different from the current market-end insulating coating process in which the active material is coated when it is in a wet film state, the present invention breaks the convention and adopts the idea of ​​coating the insulating coating when the active material is in a dry film state for the first time, thereby avoiding the problem of mutual solubility between the active material slurry and the insulating coating, and further improving the process consistency and qualified rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a schematic diagram of the position structure of the insulating coating of the positive electrode sheet on the current collector in Example 1;

[0035] Figure 2 It is a schematic diagram of a glue coating device in the prior art;

[0036] Figure 3 This is a schematic diagram of the staggered coating of the winding core in Example 1;

[0037] Figure 1-3 Middle: 1. Insulation coating; 2. Active material layer; 3. Blank space for the tab; 4. Positive current collector; 5. Area of ​​insulation coating not cut by laser; 6. Insulation coating coating area; 7. Positive active material area; 8. Negative active material area; 9. Diaphragm; 10. Negative current collector; 11. Negative electrode sheet; 12. Positive electrode sheet; 13. Glue coating head; 14. Electric heating module; 15. Telescopic cylinder;

[0038] Figure 4 This is a laser-cut cross-sectional end electron microscope image (1000×) of the positive electrode sheet prepared in Example 2;

[0039] Figure 5 This is a laser-cut cross-sectional end electron microscope image (2000×) of the positive electrode sheet prepared in Example 3;

[0040] Figure 6 This is a laser-cut cross-sectional end electron microscope image (5000×) of the positive electrode sheet prepared in Example 4;

[0041] Figure 7 This is a laser-cut cross-sectional end electron microscope image (1000×) of the positive electrode sheet prepared in Comparative Example 1. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0043] Example 1

[0044] A lithium battery positive electrode sheet, such as Figure 1 As shown, the edge of the positive electrode sheet is coated with an insulating coating 1 of a special material, and the coating position of the insulating coating 1 is between the active material layer 2 and the tab blank 3; the components of the insulating coating 1 include ethylene-vinyl acetate polymer, plasticizer, binder and antioxidant; the insulating coating 1 is coated on the active material layer 2 (active material dry material) and is allowed to cover a certain width. In this embodiment, the width of the insulating coating 1 is 6 to 8 mm, and the coating thickness is 10 to 15 μm.

[0045] The ethylene-vinyl acetate polymer is prepared from ethylene and vinyl acetate by an emulsion method, has a molecular weight of 1280, and has the following structural formula:

[0046]

[0047] Where: x and y are natural numbers within 1-100.

[0048] In this embodiment, the mass ratio of each component in the insulating coating is as follows:

[0049] Ethylene-vinyl acetate polymer: plasticizer: binder: antioxidant = 80-85: 0.5-1: 10-15: 1-2.

[0050] In this embodiment, the plasticizer is dibutyl phthalate (DBP) or dioctyl phthalate (DOP); the binder is a resin such as polyvinylidene fluoride or polystyrene; and the antioxidant is butylated hydroxyanisole (BHA) or butylated hydroxytoluene (BHT).

[0051] In this embodiment, the active material layer is conventional lithium iron phosphate or ternary lithium, and the core is made by winding or lamination.

[0052] A method for preparing a lithium battery positive electrode sheet, the specific steps are as follows:

[0053] (1) Preparation of insulating coating

[0054] (1-1) In a high-pressure reactor, vinyl acetate and K2S2O8 or (NH4)2S2O8 initiator are first added to the prepared emulsion reaction medium, and then ethylene is added. 2 The polymerization was carried out under pressure to obtain ethylene-vinyl acetate polymer latex having a vinyl acetate content of 75%.

[0055] (1-2) At a high temperature of 150°C, a plasticizer, a binder and an antioxidant are added to the ethylene-vinyl acetate polymer latex prepared above in a mass ratio of 0.5-1:10-15:1-2, wherein the ethylene-vinyl acetate polymer accounts for 80-85wt%; at a high temperature of 220°C, the insulating coating adhesive is uniformly dispersed and stirred to obtain an insulating coating adhesive; after filtering, the adhesive is cooled to room temperature to obtain a solid insulating coating.

[0056] (2) Preparation of positive electrode sheet with insulating coating

[0057] (2-1) The solid insulating coating prepared above is heated to above 170°C in a heating furnace to melt it into a flowable adhesive; the melt flow rate is 2.0 kg / 10 min at 170°C and 2.2 kg / 10 min at 190°C.

[0058] (2-2) The molten glue obtained above is introduced into the glue coating head 13 through the electric heating tube ( Figure 2 ), where the temperature of the heating furnace and the electric heating tube is controlled at 170°C and continuous heating is achieved.

[0059] (2-3) Start the electric heating module 14 ( Figure 2 ), the heating temperature is 220℃ to further melt the insulating coating.

[0060] (2-4) The entire glue coating device (existing technology, such as Figure 2 The laser cutting device is installed after the laser unwinding position and before the laser cutting position. The laser cutting device passes horizontally through the conveying roller after unwinding, and the gluing device is installed just above the conveying roller. Figure 2 ) moves up and down to achieve uniform coating on the edge of the positive electrode current collector (the junction of the positive electrode material area and the blank area) during the laser cutting process; after completing the front side coating, it is necessary to use a cache return mechanism to coat the back side.

[0061] (2-5) The molten hot melt adhesive is applied to the tab forming area and covers at least a portion of the active material layer, and is cooled and solidified to form a hot melt adhesive layer.

[0062] (2-6) Cutting is performed using a pulsed laser, and the laser directly cuts the surface of the insulating coating to obtain a preset ear shape and excess waste edge, thereby obtaining the lithium battery positive electrode sheet. The width of the insulating coating left on the electrode sheet after laser cutting is 3 to 4 mm, and both the coating area and the cutting area are located on the ear side.

[0063] (3) The positive electrode sheet obtained by the above laser cutting process is wound or laminated, and matched with the separator and the negative electrode sheet to produce a qualified winding core, such as Figure 3 As shown, the separator 9 entirely covers the negative electrode sheet 11 and the positive electrode sheet 12, the negative electrode sheet 11 covers the positive electrode sheet 12 in the middle layer, and the positive electrode sheet 12 is located in the innermost layer.

[0064] Among them, the negative electrode sheet 11 includes a negative electrode active material area 8 and a negative electrode current collector 10 (copper foil), and the positive electrode sheet 12 includes a positive electrode active material area 7, an insulating coating coating area 6 (located at the edge of the positive electrode sheet), an insulating coating area 5 that is not cut by laser (located on the pole ear) and a positive electrode current collector 4 (aluminum foil).

[0065] The winding or lamination process adopts staggered coating to achieve the negative electrode cut corresponding to the positive electrode insulating layer, which is as follows: in the laser cutting process, the positive electrode cuts the insulating layer (the insulating coating coating area 6 located at the edge of the positive electrode sheet), and the negative electrode cuts the active material area (the negative electrode active material area 8); during the assembly process, the negative electrode active material area (negative electrode active material area 8) covers the positive electrode active material area (positive electrode active material area 7), and the positive electrode insulating layer (insulating coating coating area 6) covers the negative electrode active material area (negative electrode active material area 8).

[0066] like Figure 3 As shown, the phase difference of the negative electrode active material area (negative electrode active material area 8) covering the positive electrode active material area (positive electrode active material area 7) is 3.5mm; the phase difference of the positive electrode insulating layer (insulating coating coating area 6) covering the negative electrode active material area (negative electrode active material area 8) is 1mm.

[0067] Example 2

[0068] A method for preparing a positive electrode sheet for a lithium battery, wherein the specific steps are the same as those of Example 1, wherein the composition ratio of the insulating coating is as follows:

[0069] Ethylene-vinyl acetate polymer accounts for 83.5wt%, plasticizer accounts for 0.5wt%, binder accounts for 15wt%, and antioxidant accounts for 1wt%.

[0070] Example 3

[0071] A method for preparing a positive electrode sheet for a lithium battery, wherein the specific steps are the same as those of Example 1, wherein the composition ratio of the insulating coating is as follows:

[0072] Ethylene-vinyl acetate polymer accounts for 85wt%, plasticizer accounts for 0.5wt%, binder accounts for 13wt%, and antioxidant accounts for 1.5wt%.

[0073] Example 4

[0074] A method for preparing a positive electrode sheet for a lithium battery, wherein the specific steps are the same as those of Example 1, wherein the composition ratio of the insulating coating is as follows:

[0075] Ethylene-vinyl acetate polymer accounts for 87.5wt%, plasticizer accounts for 0.5wt%, binder accounts for 10wt%, and antioxidant accounts for 2wt%.

[0076] Comparative Example 1

[0077] A method for preparing a lithium battery positive electrode sheet, the specific steps are as follows:

[0078] (1) Using the traditional PVDF (polyvinylidene fluoride) + boehmite + NMP (N-methylpyrrolidone) solution, the coating process is evenly coated on the edge of the active material.

[0079] (2) Cut the positive electrode sheet obtained above using a pulsed laser to obtain a formed electrode ear.

[0080] Test Example 1

[0081] 1. Test items

[0082] (1) The insulation layer resistance data of the positive electrode sheets prepared in Examples 2-4 and Comparative Example 1 were tested and recorded, and the insulation layer coating at the laser cut position was observed using an electron microscope.

[0083] (2) The positive electrode sheets prepared in Examples 2-4 and Comparative Example 1 were immersed in electrolyte at two high temperatures, wherein the immersion time was 20 days at 45° C. and 10 days at 60° C., and the shedding of the insulating layer was observed.

[0084] 2. Test results

[0085] The test results are summarized in Table 1 below:

[0086] Table 1 Test results

[0087]

[0088]

[0089] From Table 1 and Figure 4-7It can be seen that the insulation level of Examples 2-4 and Comparative Example 1 is basically the same, and both can meet the basic insulation requirements; however, the electrolyte immersion resistance of Examples 2-4 at high temperature is better than that of Comparative Example 1; at the same time, Examples 2-4 are also better than Comparative Example 1 in terms of laser cutting burr coating ( Figure 4-6 Electron microscope images of different magnifications of Examples 2-4 are shown respectively, wherein Figure 4 This is a picture taken under a 1000x microscope. Figure 7 The magnification of the comparative example 1 is the same, and the two are in sharp contrast).

[0090] It can be seen from the above test results that the present invention meets the process requirements in terms of laser cutting insulation protection capability and is superior to the current traditional insulation coating method.

[0091] The embodiments described above are only some embodiments of the present invention, rather than all embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. The scope of protection of the present invention shall be subject to the scope required by the claims. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work shall fall within the scope of protection of the present invention.

Claims

1. A lithium battery positive electrode sheet, characterized in that: The edge of the positive electrode sheet is coated with an insulating coating of special material, and the coating position of the insulating coating is between the active material layer and the blank space of the tab; the components of the insulating coating include ethylene-vinyl acetate polymer, plasticizer, binder and antioxidant; the insulating coating is coated on the active material layer and covers a certain width.

2. A lithium battery positive electrode sheet according to claim 1, characterized in that: The insulating coating has a width of 6 to 8 mm and a thickness of 10 to 15 μm.

3. A lithium battery positive electrode sheet according to claim 1, characterized in that: The ethylene-vinyl acetate polymer is prepared from ethylene and vinyl acetate by an emulsion method, has a molecular weight of 1280, and has the following structural formula:

4. A lithium battery positive electrode sheet according to claim 1, characterized in that: The mass ratio of each component in the insulating coating is as follows: Ethylene-vinyl acetate polymer: plasticizer: binder: antioxidant = 80-85: 0.5-1: 10-15: 1-2.

5. A lithium battery positive electrode sheet according to claim 1, characterized in that: The plasticizer is dibutyl phthalate or dioctyl phthalate; the binder is polyvinylidene fluoride or polystyrene; and the antioxidant is butylated hydroxyanisole or butylated hydroxytoluene.

6. A lithium battery positive electrode sheet according to claim 1, characterized in that: The active material layer is lithium iron phosphate or ternary lithium.

7. A method for preparing a lithium battery positive electrode sheet according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1) In a high pressure reactor, vinyl acetate and K2S2O8 or (NH4)2S2O8 initiator are first added to the prepared emulsion reaction medium, and then ethylene is added at 85°C and 90kg / cm 2 Polymerize under pressure to obtain ethylene-vinyl acetate polymer latex with a vinyl acetate content of 75%; Step 2) at a high temperature of 150° C., a plasticizer, a binder and an antioxidant are sequentially added to the ethylene-vinyl acetate polymer latex obtained in step 1) at a mass ratio of 0.5-1:10-15:1-2; at a high temperature of 220° C., the insulating coating glue is uniformly dispersed and stirred to obtain; after filtering, the mixture is cooled to room temperature to obtain a solid insulating coating; Step 3) the solid insulating coating obtained in step 2) is heated to above 170° C. in a heating furnace to melt the solid insulating coating into a flowable glue; the melt flow rate is 170° C. / 2.0 kg, 190° C. / 2.2 kg; Step 4) introducing the molten glue obtained in step 3) to the glue coating head through an electric heating tube, wherein the temperature of the heating furnace and the electric heating tube is controlled to be 170° C., and continuous heating is achieved; Step 5) starting the electric heating module at a heating temperature of 220° C. to further melt the insulating coating; Step 6) The entire glue coating device is installed after the laser cutting and unwinding position and before the laser cutting position. The laser cut electrode sheet that is unwinding and tape-feeding passes horizontally through the conveying roller, and the glue coating device is installed just above the conveying roller; the laser cutting and tape-feeding process is realized by moving the telescopic cylinder up and down to evenly coat the edge of the positive electrode sheet collector, that is, the junction of the positive electrode material area and the blank area; after the front side coating is completed, the cache return mechanism needs to be used to coat the back side; Step 7) applying the melted hot melt adhesive to the tab forming area and covering at least a portion of the active material layer, and cooling and solidifying to form a hot melt adhesive layer; Step 8) Laser directly cuts the surface of the insulating coating to obtain the preset ear shape and excess waste edge.

8. The method for preparing a lithium battery positive electrode sheet according to claim 7, characterized in that: In the step 8), the width of the insulating coating remaining on the pole piece after laser cutting is 3 to 4 mm, and both the coating area and the cutting area are located on the pole ear side.

9. Use of the lithium battery positive electrode sheet according to any one of claims 1 to 6, or the lithium battery positive electrode sheet prepared by the preparation method according to claim 7 or 8 in preparing a lithium battery, characterized in that: The positive electrode sheet of the lithium battery is wound or laminated, and is matched with a separator and a negative electrode sheet to produce a qualified winding core, which is then combined with an electrolyte and a shell structure to form a lithium battery.

10. The use according to claim 9, characterized in that: The winding or lamination process adopts staggered coating to achieve the negative electrode cut corresponding to the positive electrode insulation layer, which is as follows: in the laser cutting process, the positive electrode cuts the insulation layer and the negative electrode cuts the active material area; during the assembly process, the negative electrode active material area covers the positive electrode active material area, and the positive electrode insulation layer covers the negative electrode active material area.

11. The use according to claim 10, characterized in that: The phase difference between the negative electrode active material region covering the positive electrode active material region is 3.5 mm; the phase difference between the positive electrode insulating layer covering the negative electrode active material region is 1 mm.

12. A lithium battery, characterized in that: It includes a lithium battery positive electrode sheet as described in any one of claims 1 to 6, or a lithium battery positive electrode sheet prepared by the preparation method as described in claim 7 or 8.

Citation Information

Patent Citations

  • Positive plate of high-safety lithium-ion laminated battery and preparation method of positive plate

    CN105244470A

  • Positive pole piece of lithium-ion battery and lithium-ion battery

    CN106129327A

  • Dry-method dual-electrode lithium battery and preparation method thereof

    CN114784387A

  • Adhesive tape, preparation method of adhesive tape and preparation method of lithium ion battery

    CN115466581A

  • Non-oriented silicon steel insulating coating liquid for improving secondary coating of electrophoretic paint as well as preparation method and application of non-oriented silicon steel insulating coating liquid

    CN115595010A

Cited By

  • Battery monomer, battery device, energy storage device and power utilization device

    CN121282473A