Surface protective film and optical component to which the film is attached
The multilayer surface protection film with controlled adhesive strengths addresses the challenge of strong peeling forces in optical components, enabling easy peeling and removal, thus improving handling and process efficiency.
Patent Information
- Application Number
- JP2024140092
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2038-11-19
AI Technical Summary
Existing surface protection films for optical components, particularly those used in thin and high-definition displays, face challenges with strong peeling forces that complicate handling and require reapplication or wiping during transportation, which hinders process efficiency and workability.
A surface protection film with a multilayer structure comprising a first transparent film, a first adhesive layer with low adhesive strength, a second transparent film, and a second adhesive layer with even lower adhesive strength, designed to facilitate easy peeling and removal without residue, using acrylic-based adhesives and controlled adhesive forces to balance curl suppression and peeling ease.
The film effectively suppresses curling and improves handling properties, allowing easy peeling and removal, reducing the need for reapplication or wiping, thereby enhancing process efficiency and workability in manufacturing and transportation.
Smart Images

Figure 2024152919000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface protection film and an optical component to which the surface protection film is attached. [Background technology]
[0002] Optical films such as polarizing plates, retardation plates, lens films for displays, anti-reflection films, hard coat films, transparent conductive films for touch panels, etc. are used in optical products such as displays. When manufacturing and transporting optical films or optical components, a surface protective film is attached to the surface of the optical film to prevent the surface from being soiled or scratched in the subsequent process. Appearance inspection of the optical film may be performed with the surface protective film attached.
[0003] A surface protection film according to the prior art typically has a configuration in which a pressure-sensitive adhesive layer having a weak adhesive strength is provided on one side of a base film. The pressure-sensitive adhesive layer is a layer for attaching the surface protection film to an optical film. The pressure-sensitive adhesive layer is made weakly adhesive so that when a used surface protection film is peeled off from the surface of the optical film, it can be peeled off smoothly and no adhesive residue is left behind.
[0004] In recent years, displays have become thinner and more highly detailed, and accordingly, optical films have also become thinner. In order to make optical films thinner, not only are the thicknesses of the components reduced, but also changes to the structure have been made, such as removing unnecessary components or reducing the number of components by giving one component the functions of multiple components. For example, the number of polarizing plates having a structure in which a polarizer protective layer is laminated on only one side of a polarizer layer, rather than on both sides, is increasing. In the case of a polarizing plate in which only one polarizer protective layer is provided for a polarizer layer, the structure sandwiching the polarizer is asymmetric between the front and back, and therefore the polarizer tends to bend (curl) toward one side. For this reason, a method for suppressing curling of optical films has been proposed.
[0005] For example, in Patent Document 1, the bending resistance according to the Gurley method is 1.0×10 2 mgf or higher, 1.0×10 5 A manufacturing method has been proposed in which a protective film (surface protection film) with a hardness of 100 mgf or less is attached to prevent curling of the polarizing plate. A specific example is a protective film made of a biaxially oriented polyester resin with a thickness of 25 μm or more and 120 μm or less.
[0006] Patent Document 2 proposes a polarizing plate in which the bending resistance of a laminate consisting of a polarizing plate body and a protective film (surface protection film) is specified. As a specific example, a polarizing plate using a protective film with a thickness of 50 μm, which is a base film made of a biaxially oriented polyester resin, is given.
[0007] Patent Document 3 proposes a protective film capable of effectively suppressing warping (curling) of a polarizing plate. Specifically, the protective film proposed has a first resin layer, an adhesive layer, a second resin layer, and a pressure-sensitive adhesive layer in this order. The ratio of the thickness of the adhesive layer to the sum of the thicknesses of the first resin layer and the second resin layer is 0.40 or less. The storage modulus of the adhesive layer at 23° C. is 8.0×10 4 Pa or more 1.0×10 7 The thickness is less than 1 Pa. The protective film is attached to the surface of the polarizing plate as an integral part, and is peeled off as an integral part.
[0008] The surface protection films disclosed in Patent Documents 1 to 3 have a thick base film or use a laminate film having a resin layer / adhesive layer / resin layer laminated thereto as the base film, which makes the film stiff and provides an effect of suppressing curling of the optical film. However, there is a problem in that the peeling force becomes strong when the surface protection film is peeled off after use. When peeling off the surface protection film, it is peeled off at a peeling angle close to 180° from the optical film. The peeling force of the surface protection film at this time is the sum of the force with which the adhesive of the surface protection film adheres to the optical film (the adherend) and the force required to bend the surface protection film itself 180°. If the surface protection film becomes stiffer, the force required to bend the surface protection film itself 180° also increases, resulting in a stronger peeling force for the surface protection film. In recent years, displays have become thinner and more highly detailed, and larger in size for television and digital signage applications. The surface protection films described above are difficult to use for optical films used on such large displays because of the strong peeling force required for peeling.
[0009] Traditionally, in display manufacturing, parts such as liquid crystal panels, backlight units, and surface filters were procured by panel manufacturers in a set format. This is called module procurement. However, in recent years, a procurement format called "open cell procurement" has become mainstream, especially for television applications. With open cell procurement, parts such as liquid crystal panels, backlight units, and surface filters are procured separately and assembled by television manufacturers or OEM companies. For this reason, liquid crystal panels are increasingly being distributed in a semi-finished state.
[0010] In module procurement, the surface protection film attached to the polarizing plate was peeled off after panelization. However, with the adoption of open cell procurement, in order to prevent the adhesion of dust and foreign matter during the transportation of the liquid crystal panel, it is becoming common to not peel off the surface protection film until just before the panelization. When shipping and transporting liquid crystal panels, it is becoming more common to replace the surface protection film that became dirty during panelization or to wipe off the dirt on the surface protection film to keep the surface protection film clean. With the surface protection films shown in Patent Documents 1 to 3, it is necessary to replace the surface protection film or wipe off the dirt on the surface protection film before shipping the liquid crystal panel, which does not lead to process reduction or improvement of workability. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2012-053078 A [Patent Document 2] Republished WO2016 / 039296 [Patent Document 3] Patent No. 5461640 Summary of the Invention [Problem to be solved by the invention]
[0012] One aspect of the present invention has been made in consideration of the above circumstances, and has an object to provide a surface protective film that has a high effect of suppressing curling of an optical film, improves the handleability of an optical film to which the surface protective film is attached, and is easy to peel and remove after use, eliminating the need to replace the surface protective film or wipe off dirt during shipment, and an optical component using the same. [Means for solving the problem]
[0013] In one embodiment of the present invention, a first transparent film, a first pressure-sensitive adhesive layer, a second transparent film, and a second pressure-sensitive adhesive layer are laminated in this order, and the storage modulus of the first pressure-sensitive adhesive layer at 23° C. is 1.0×10 4 Pa or more 8.0×10 4 The present invention provides a surface protection film, wherein the adhesive strength of the first adhesive layer to glass is 5 N / 25 mm or less.
[0014] The second pressure-sensitive adhesive layer may use a (meth)acrylic polymer as a base polymer.
[0015] It is preferable that the adhesive strength of the second adhesive layer to glass is 0.5 N / 25 mm or less, and that the adhesive strength of the first adhesive layer to glass is higher than that of the second adhesive layer to glass.
[0016] The surface resistivity of the second pressure-sensitive adhesive layer is 1×10 13 It is preferable that the resistance is less than [Ω / □].
[0017] Another aspect of the present invention provides an optical component having the above-mentioned surface protection film attached thereto. Effect of the Invention
[0018] According to one aspect of the present invention, it is possible to provide a surface protective film that has a high effect of suppressing curling of an optical film, improves the handleability of an optical film to which the surface protective film is attached, and is easy to peel and remove after use, eliminating the need to replace the surface protective film or wipe off dirt when shipping a liquid crystal panel, and an optical component using the same. [Brief description of the drawings]
[0019] [Figure 1] 1 is a schematic configuration diagram of a surface protection film according to an embodiment. [Diagram 2] FIG. 1 is a schematic diagram illustrating an example of an optical component using a surface protection film according to an embodiment. [Diagram 3] 3 is a schematic diagram showing a configuration in which an adhesive film made of a first transparent film and a first adhesive layer is peeled off and removed from the optical component shown in FIG. 2. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, the present invention will be described in detail based on the embodiments. FIG. 1 is a schematic diagram of a surface protective film P according to an embodiment. As shown in FIG. 1, the surface protective film P includes a first transparent film 1 and a first adhesive layer 2 on one side thereof. A second transparent film 3 is provided on the opposite side of the first adhesive layer 2 to the first transparent film 1. A second adhesive layer 4 is provided on the opposite side of the second transparent film 3 to the first adhesive layer 2. A release film 5 for protecting the adhesive surface is superimposed on the surface of the second adhesive layer 4. That is, the surface protective film P is configured by laminating the first transparent film 1, the first adhesive layer 2, the second transparent film 3, the second adhesive layer 4, and the release film 5 in this order. Note that the film obtained by removing the release film 5 from the surface protective film P shown in FIG. 1, that is, the film obtained by laminating the first transparent film 1, the first adhesive layer 2, the second transparent film 3, and the second adhesive layer 4 in this order, is sometimes referred to as the surface protective film P.
[0021] A transparent plastic film is used as the first transparent film 1 (base film). The first transparent film 1 and the second transparent film 3 have transparency, so that the appearance inspection of the optical component can be performed with the surface protective film P attached. As the plastic film for the first transparent film 1, a polyester film such as polyethylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, or polybutylene terephthalate is preferably used. In addition to polyester films, other plastic films can be used as long as they have the necessary strength and optical suitability. The first transparent film 1 may be a non-stretched film or may be uniaxially or biaxially stretched. The first transparent film 1 may be a plastic film in which the stretching ratio or the angle of the axial direction formed by crystallization during stretching is controlled.
[0022] The thickness of the first transparent film 1 is not particularly limited, but is, for example, about 12 to 100 μm, and particularly often about 20 to 50 μm. If necessary, the first transparent film 1 may be provided on the side opposite the first adhesive layer 2 (the upper surface in Figure 1) with an antifouling layer for preventing surface contamination, an antistatic layer, or a hard coat layer for preventing scratches, or may be subjected to an adhesion enhancing treatment such as a corona discharge treatment or an anchor coat treatment.
[0023] The first pressure-sensitive adhesive layer 2 is used for the purpose of absorbing and alleviating stress caused by curling of the optical film when the surface protection film P is attached to the optical film. The material of the first pressure-sensitive adhesive layer 2 is not particularly limited as long as it satisfies the properties such as no adverse effect on the adhesion to the transparent film, adhesive properties, stability, etc., and known materials can be used.
[0024] Examples of materials for the first adhesive layer 2 include rubber-based, acrylic-based, and urethane-based adhesives. The rubber-based adhesive is an adhesive in which a tackifier, a softener, an antioxidant, a filler, etc. are blended with an elastomer such as natural rubber or synthetic rubber, and a crosslinking agent may be added as necessary. The acrylic adhesive is, for example, an adhesive obtained by adding a curing agent or a tackifier to a (meth)acrylic polymer as necessary. The (meth)acrylic polymer is generally a polymer obtained by copolymerizing a main monomer such as butyl acrylate (e.g., n-butyl acrylate), 2-ethylhexyl acrylate, isooctyl acrylate, or isononyl acrylate, a comonomer such as acrylonitrile, vinyl acetate, methyl acrylate, methyl methacrylate, or ethyl acrylate, and a functional monomer such as acrylic acid, methacrylic acid, hydroxyethyl acrylate, hydroxybutyl acrylate, glycidyl methacrylate, dimethylacrylamide, N-methylol methacrylamide, a hydroxyl group-containing acrylic monomer, a carboxyl group-containing acrylate, or a polyoxyalkylene group-containing acrylic monomer. The (meth)acrylic polymer may have an appropriate composition selected according to the desired properties. The (meth)acrylic polymer is used as a base polymer.
[0025] Examples of the curing agent include an isocyanate compound, an epoxy compound, a melamine compound, a metal chelate compound, etc. Examples of the tackifier include a rosin-based, a coumarone-indene-based, a terpene-based, a petroleum-based, a phenol-based, etc. Additives such as a curing catalyst, a pot life extender, an antistatic agent, an ultraviolet absorber, and an antioxidant may be added as necessary to the first pressure-sensitive adhesive layer 2. As a material for the first pressure-sensitive adhesive layer 2, a pressure-sensitive adhesive may be used in which a photoinitiator and a photocurable monomer or oligomer are added to the above pressure-sensitive adhesive, and the monomer or oligomer is polymerized after irradiation with light, thereby changing the adhesive strength.
[0026] The urethane-based adhesive may be one in which the types and composition ratios of hard and soft segments are adjusted. As the material for the first pressure-sensitive adhesive layer 2, an acrylic pressure-sensitive adhesive is particularly preferable in view of heat resistance, durability, adhesiveness to the second transparent film 3, and the like.
[0027] The first adhesive layer 2 may be an adhesive containing an ultraviolet initiator and an ultraviolet curing monomer or oligomer, and whose adhesive strength decreases when irradiated with ultraviolet light. The use of this adhesive makes it easier to peel and remove the first transparent film and the first adhesive layer from the second transparent film when shipping and transporting the liquid crystal panel. The first adhesive layer 2 may be an adhesive to which a thermal foaming agent is added within a range that does not impair transparency, and whose adhesive strength decreases when heated.
[0028] The first pressure-sensitive adhesive layer 2 is a pressure-sensitive adhesive layer having an adhesive strength to glass of 5 N / 25 mm or less. The first pressure-sensitive adhesive layer 2 desirably has an adhesive strength to glass of 5 N / 25 mm or less at a 180° peel speed of 300 mm / min. If the adhesive strength of the first adhesive layer 2 to glass is greater than 5 N / 25 mm, the peeling force required to peel and remove the surface protective film P will be high, which may reduce workability. Also, if the adhesive strength of the first adhesive layer 2 to glass is greater than 5 N / 25 mm, it may be difficult to peel the adhesive film consisting of the first transparent film 1 and the first adhesive layer 2 from the second transparent film 3 when necessary (such as when the liquid crystal panel is shipped).
[0029] The adhesive strength of the first adhesive layer 2 to glass may be, for example, 1 N / 25 mm or more. When the adhesive strength of the first adhesive layer 2 to glass is 1 N / 25 mm or more, accidental peeling of the adhesive film consisting of the first transparent film 1 and the first adhesive layer 2 is unlikely to occur.
[0030] Considering the ease of operation when peeling and removing the surface protective film P, it is desirable that the adhesive strength of the first adhesive layer 2 is higher than that of the second adhesive layer 4. This makes it easier to peel the adhesive film consisting of the first transparent film 1 and the first adhesive layer 2 from the second transparent film 3, for example, when shipping the liquid crystal panel.
[0031] The storage modulus of the first pressure-sensitive adhesive layer 2 at 23° C. is 1.0×10 4 Pa or more 8.0×10 4 The storage modulus of the first pressure-sensitive adhesive layer 2 is less than 1.0×10 4 If the storage modulus of the first pressure-sensitive adhesive layer 2 is less than 8.0×10 Pa, problems such as the pressure-sensitive adhesive protruding from the edge portion or foreign matter easily adhering to the edge portion may occur when the surface protection film P is wound up in a roll and stored. In addition, the curl suppression effect of the optical film may be reduced. 4 If it is more than Pa, the peeling force required to peel and remove the surface protective film P becomes too high, which may reduce workability.
[0032] The thickness of the first pressure-sensitive adhesive layer 2 is not particularly limited, but is generally about 3 to 30 μm. By making the thickness of the first pressure-sensitive adhesive layer 2 3 μm or more, a predetermined adhesive strength can be obtained. By making the thickness of the first pressure-sensitive adhesive layer 2 30 μm or less, costs can be suppressed.
[0033] A known method may be used to form the first adhesive layer 2 on the first transparent film 1. For example, a method of coating the first transparent film 1 with an adhesive, drying and curing the same, or a method of coating the second transparent film with an adhesive, drying and curing the same, and then laminating the first transparent film, may be used. Specifically, a known coating method such as reverse coating, comma coating, gravure coating, slot die coating, Mayer bar coating, or air knife coating may be used.
[0034] A plastic film having transparency is used as the second transparent film 3. The first transparent film 1 and the second transparent film 3 have transparency, so that the appearance inspection of the optical component can be performed with the surface protection film attached. As the plastic film for the second transparent film 3, a polyester film such as polyethylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, or polybutylene terephthalate is preferably used. In addition to polyester films, other plastic films can be used as long as they have the necessary strength and optical suitability. The second transparent film 3 may be a non-stretched film or may be uniaxially or biaxially stretched. The second transparent film 3 may be a plastic film in which the stretching ratio or the angle of the axial direction formed by the crystallization of stretching is controlled.
[0035] The thickness of the second transparent film 3 is not particularly limited, but is, for example, about 12 to 100 μm, and particularly often about 19 to 50 μm. If necessary, the second transparent film 3 may be subjected to an adhesion enhancing treatment or an antistatic treatment, such as a corona discharge treatment or an anchor coat treatment, on the side in contact with the first pressure-sensitive adhesive layer 2. In addition, the second transparent film 3 may be subjected to an adhesion enhancing treatment, such as an antistatic layer, a corona discharge treatment or an anchor coat treatment, on the side opposite to the first pressure-sensitive adhesive layer 2 (the lower surface in FIG. 1).
[0036] The second adhesive layer 4 is provided to attach the surface protection film P to the optical film, which is the adherend. The second adhesive layer 4 is a layer made of an adhesive with weak adhesion. An adhesive with weak adhesion is used so that the surface protection film P does not peel off during the manufacturing process of the optical film, and can be peeled off smoothly and without leaving any adhesive residue when the surface protection film P is peeled off and removed from the optical film surface after use.
[0037] The material of the second adhesive layer 4 is not particularly limited, and known materials such as rubber-based, acrylic-based, and urethane-based adhesives can be used, with acrylic-based adhesives being particularly preferred. The acrylic adhesive is, for example, an adhesive obtained by adding a curing agent or a tackifier to a (meth)acrylic polymer as necessary. The (meth)acrylic polymer is generally a polymer obtained by copolymerizing a main monomer such as butyl acrylate (e.g., n-butyl acrylate), 2-ethylhexyl acrylate, isooctyl acrylate, or isononyl acrylate, a comonomer such as acrylonitrile, vinyl acetate, methyl acrylate, methyl methacrylate, or ethyl acrylate, and a functional monomer such as acrylic acid, methacrylic acid, hydroxyethyl acrylate, hydroxybutyl acrylate, glycidyl methacrylate, dimethylacrylamide, N-methylol methacrylamide, a hydroxyl group-containing acrylic monomer, a carboxyl group-containing acrylate, or a polyoxyalkylene group-containing acrylic monomer. The (meth)acrylic polymer may have an appropriate composition selected according to the desired properties. The (meth)acrylic polymer is used as a base polymer.
[0038] Examples of the curing agent include isocyanate compounds, epoxy compounds, melamine compounds, metal chelate compounds, etc. Examples of the tackifier include rosin-based, coumarone-indene-based, terpene-based, petroleum-based, phenol-based, etc. Additives such as curing catalysts, pot life extenders, antistatic agents, ultraviolet absorbers, and antioxidants may be added to the acrylic adhesive as necessary.
[0039] The antistatic agent is preferably one that has good dispersibility or compatibility with the (meth)acrylic polymer, and examples thereof include surfactants, ionic liquids, ionic solids, alkali metal salts, metal oxides, metal fine particles, conductive polymers, carbon, carbon nanotubes, etc. As the antistatic agent, surfactants, ionic liquids, ionic solids, alkali metal salts, etc. are preferred in terms of transparency and affinity with the (meth)acrylic polymer.
[0040] Examples of the surfactant include nonionic, cationic, anionic, and amphoteric surfactants. Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene fatty acid esters, glycerin fatty acid esters, propylene glycol fatty acid esters, and polyoxyalkylene-modified silicones. Examples of the cationic surfactant include alkyl trimethyl ammonium salts, dialkyl dimethyl ammonium salts, and alkyl benzyl dimethyl ammonium salts. Examples of the anionic surfactant include monoalkyl sulfates, alkyl polyoxyethylene sulfates, alkyl benzene sulfonates, and monoalkyl phosphates. Examples of the amphoteric surfactant include alkyl dimethyl amine oxide and alkyl carboxy betaine.
[0041] Ionic liquids are non-polymeric substances that contain anions and cations and are liquid at room temperature. Examples of the cationic portion include cyclic amidine ions such as imidazolium ions, pyridinium ions, ammonium ions, sulfonium ions, and phosphonium ions. Examples of the anionic portion include C n H 2n+1 COO - , C n F 2n+1 COO - , N03 - , C n F 2n+1 SO3 - , (C n F 2n+1 SO2)2N - , (C n F 2n+1 SO2)3C - , PO4 2- , AlCl4 - , Al2Cl7 - , ClO4 - , BF4 - , PF6 - , AsF6 - , SbF6 - etc.
[0042] An ionic solid is a non-polymeric substance that contains anions and cations and is solid at room temperature. Examples of the cationic portion include nitrogen-containing onium ions such as pyridinium ions, imidazolium ions, pyrimidinium ions, pyrazolium ions, pyrrolidinium ions, and ammonium ions, as well as phosphonium ions and sulfonium ions. Examples of the anionic portion include hexafluorophosphate (PF6 - ), thiocyanate (SCN - ), alkylbenzene sulfonate (RC6H4SO3 - ), perchlorate (ClO4 - ), tetrafluoroborate (BF4 - By selecting the alkyl group chain length, the position of the substituent, the number of the substituents, etc., it is possible to obtain a compound that is solid at room temperature.
[0043] Examples of the alkali metal salt include metal salts containing alkali metals such as lithium, sodium, potassium, etc. An example of the alkali metal salt is lithium trifluoromethylsulfonate (CF3LiO3S). A compound containing a polyoxyalkylene structure may be added to the antistatic agent in order to stabilize the ionic substance.
[0044] The amount of the antistatic agent component added to a base polymer such as a (meth)acrylic polymer varies depending on the type of the antistatic agent component and the degree of compatibility with the base polymer, but may be set taking into consideration the surface resistivity, the tendency to stain an adherend, the adhesive properties, etc. The acrylic adhesive may contain additives such as a curing catalyst, a pot life extender, an ultraviolet absorber, and an antioxidant, if necessary.
[0045] When the surface protective film P is used in an application where there is a concern about peeling electrification voltage when peeling and removing, it is preferable to add an antistatic component (antistatic agent) to the second pressure-sensitive adhesive layer 4. In this case, the surface resistivity of the second pressure-sensitive adhesive layer 4 is preferably 1×10 13 The surface resistivity of the second pressure-sensitive adhesive layer 4 is preferably less than 1×10 13 If the resistivity is less than [Ω / □], the peeling electrification voltage when removing the surface protective film can be reduced, and therefore the antistatic performance can be improved.
[0046] The thickness of the second pressure-sensitive adhesive layer 4 is not particularly limited, but is often, for example, about 3 to 50 μm, and particularly about 5 to 30 μm.
[0047] Although it depends on the type of surface treatment of the optical film to which the surface protective film P is attached, the adhesive strength of the second adhesive layer 4 to glass is preferably 0.5 N / 25 mm or less. The adhesive strength of the second adhesive layer 4 to glass at a 180° peel speed of 300 mm / min is preferably 0.5 N / 25 mm or less. When the adhesive strength of the second adhesive layer 4 is 0.5 N / 25 mm or less, the peeling force when peeling and removing the surface protective film P is low, thereby improving workability.
[0048] The second pressure-sensitive adhesive layer 4 is preferably a low-adhesive layer having a peel strength to the surface of the adherend (optical film) of about 0.03 to 0.3 N / 25 mm. When the adhesive strength of the second pressure-sensitive adhesive layer 4 is 0.03 N / 25 mm or more, it is possible to prevent the surface protection film P from floating (i.e., being partially peeled off) during the manufacturing process and transport process of the optical film. In addition, the surface protection film P is less likely to be peeled off accidentally. When the adhesive strength of the second pressure-sensitive adhesive layer 4 is 0.3 N / 25 mm or less, it is possible to improve workability.
[0049] The lamination of the second adhesive layer 4 on the second transparent film 3 may be performed by a known method, and is not particularly limited. Specific examples include (1) a method in which an adhesive to become the second adhesive layer 4 is applied to the second transparent film 3, dried to form the second adhesive layer 4, and then a release film 5 is attached to the surface of the second adhesive layer 4, and (2) a method in which an adhesive to become the second adhesive layer 4 is applied to a release film 5, dried to form the second adhesive layer 4, and then a second transparent film 3 is attached.
[0050] The second adhesive layer 4 may be formed on the second transparent film 3 by a known method. Specifically, the adhesive may be applied by a coating means such as reverse coating, comma coating, gravure coating, slot die coating, Mayer bar coating, or air knife coating.
[0051] The surface protective film P generally has a configuration in which a first adhesive layer 2, a second transparent film 3 and a second adhesive layer 4 are formed on a first transparent film 1, and the surface of the adhesive layer 4 is protected by a release film 5. If necessary, the surface protective film P can be in the form of a product in which the first transparent film 1 / first adhesive layer 2 / second transparent film 3 / second adhesive layer 4 are rolled into a tape without using the release film 5.
[0052] The release film 5 is not particularly limited, but may be, for example, a film such as a polyester film whose surface has been subjected to a release treatment using a release agent such as a silicone-based release agent.
[0053] FIG. 2 is a schematic diagram of an optical component D, which is an example of an optical component using the surface protection film P of the embodiment. As shown in Fig. 2, the optical component D is obtained by attaching the surface protection film P shown in Fig. 1 to the surface of the optical film C using an adhesive layer 4. Examples of the optical film C include a polarizing plate, a retardation plate, a lens film, a polarizing plate that also serves as a retardation plate, and a polarizing plate that also serves as a lens film. Such an optical component D can be used in the manufacture of liquid crystal display devices such as liquid crystal display panels, various instruments, optical devices, and the like.
[0054] The surface protective film P of the embodiment has a multilayer structure having two transparent films and two pressure-sensitive adhesive layers, and is therefore highly effective in suppressing curling of the optical film C. Due to the above-mentioned structure, the surface protective film P makes it difficult for the optical film C to fold or become uneven. Therefore, the handleability of the optical film C can be improved. Generally, when a surface protection film is formed thick, the curl suppression property and handling property are improved, but the peelability of the surface protection film is reduced. In contrast, the surface protection film P of the embodiment uses the first pressure-sensitive adhesive layer 2 having the above-mentioned properties, and therefore has the advantage of being easily peeled off and removed after use.
[0055] Since the surface protective film P uses the first adhesive layer 2 having the above-mentioned characteristics, the adhesive film consisting of the first transparent film 1 and the first adhesive layer 2 can be peeled off and removed from other parts. For example, FIG. 3 is a schematic diagram showing a configuration in which an adhesive film consisting of the first transparent film 1 and the first adhesive layer 2 is peeled off and removed from an optical component D. As shown in FIG. 3, by peeling off and removing the adhesive film, a clean surface of the surface protective film can be exposed. Therefore, there is no need to replace the surface protective film or wipe off dirt when shipping the liquid crystal panel. This makes it possible to reduce the number of steps, improve yield, productivity, and workability. The surface protective film P has a high effect of suppressing curling of the optical film, particularly for a thin optical film, and improves the handleability of the optical film to which the surface protective film is attached, and is easy to peel off and remove after use. Therefore, it is possible to improve the yield, productivity, and workability of the manufacturing process for the thin optical film. EXAMPLES
[0056] Next, the present invention will be further described with reference to examples. Hereinafter, "parts by mass" may be simply referred to as "parts". (Preparation of Surface Protection Film of Example 1) 0.3 parts of an isocyanate-based curing agent was mixed with 100 parts of a base polymer consisting of butyl acrylate, methyl acrylate, dimethylacrylamide, and a hydroxyl group-containing acrylic monomer to obtain adhesive A. The adhesive layer (coating thickness 10 μm after drying) formed by applying adhesive A to a biaxially stretched polyester film having a thickness of 38 μm had an adhesive strength of 3.8 N / 25 mm to glass.
[0057] 100 parts of a base polymer consisting of 2-ethylhexyl acrylate and a hydroxyl group-containing acrylic monomer were mixed with 3 parts of an isocyanate-based curing agent as a curing agent to obtain adhesive B. The adhesive layer (coating thickness 20 μm after drying) formed by applying adhesive B to a biaxially stretched polyester film having a thickness of 38 μm had an adhesive strength to glass of 0.2 N / 25 mm.
[0058] Pressure-sensitive adhesive A was applied to a 25 μm-thick colorless, transparent, biaxially stretched polyester film (first transparent film) so that the coating thickness after drying would be 10 μm, and then dried in a hot air circulating oven at 120° C. for 2 minutes. Next, a 38 μm-thick colorless and transparent biaxially stretched polyester film (second transparent film) was laminated to the surface (coated surface) of the adhesive A. The adhesive B was coated on the opposite side of the laminated biaxially stretched polyester film to the adhesive A so that the coating thickness after drying was 20 μm, and then dried in a hot air circulating oven at 120° C. for 2 minutes.
[0059] A release film (release film) made of a 25 μm-thick biaxially oriented polyester film coated with a silicone-based release agent was attached to the surface of adhesive B (the surface coated with adhesive B) so that the surface of adhesive B and the release agent-treated surface (the surface coated with the silicone-based release agent) were in contact with each other. The obtained sample was aged for 3 days in a 40° C. hot air circulating oven to obtain the surface protection film of Example 1. The adhesive layer formed with adhesive A was the first adhesive layer. The adhesive layer formed with adhesive B was the second adhesive layer.
[0060] (Preparation of Surface Protection Film of Example 2) 100 parts of a base polymer consisting of butyl acrylate, methyl acrylate, dimethylacrylamide, a hydroxyl group-containing acrylic monomer, and a carboxyl group-containing acrylate were mixed with 0.5 parts of an isocyanate-based curing agent as a curing agent to obtain adhesive C. The adhesive layer (coating thickness 10 μm after drying) formed by applying adhesive C to a biaxially stretched polyester film having a thickness of 38 μm had an adhesive strength of 4.8 N / 25 mm to glass. A surface protection film of Example 2 was obtained in the same manner as in Example 1, except that adhesive C was used instead of adhesive A.
[0061] (Preparation of Surface Protection Film of Example 3) 1.5 parts of an isocyanate-based curing agent was mixed with 100 parts of a base polymer consisting of butyl acrylate, methyl acrylate, dimethylacrylamide, and a hydroxyl group-containing acrylic monomer to obtain adhesive D. The adhesive layer (coating thickness 10 μm after drying) formed by applying adhesive D to a biaxially stretched polyester film having a thickness of 38 μm had an adhesive strength to glass of 1.6 N / 25 mm. A surface protective film of Example 3 was obtained in the same manner as in Example 1, except that Adhesive D was used instead of Adhesive A.
[0062] (Preparation of Surface Protection Film of Example 4) A surface protective film of Example 4 was obtained in the same manner as in Example 1, except that a 25 μm-thick colorless and transparent biaxially oriented polyester film was used instead of the 38 μm-thick biaxially oriented polyester film (second transparent film).
[0063] (Preparation of Surface Protection Film of Example 5) Adhesive E was obtained by blending 0.1 parts of lithium trifluoromethylsulfonate as an antistatic agent and 3.0 parts of an isocyanate-based curing agent as a curing agent with 100 parts of a base polymer consisting of 2-ethylhexyl acrylate, a polyoxyalkylene group-containing acrylic monomer, and a hydroxyl group-containing acrylic monomer. The adhesive strength of the adhesive layer (coating thickness after drying: 20 μm) formed by applying adhesive E to a biaxially stretched polyester film having a thickness of 38 μm to glass was 0.15 N / 25 mm, and the surface resistance of the adhesive surface was 6.0 × 10 11 It was Ω / □. A surface protective film of Example 5 was obtained in the same manner as in Example 1, except that adhesive E was used instead of adhesive B.
[0064] (Preparation of Surface Protection Film of Comparative Example 1) Pressure sensitive adhesive B was applied to a 38 μm thick colorless and transparent biaxially oriented polyester film so that the coating thickness after drying would be 20 μm, and then dried in a hot air circulating oven at 120° C. for 2 minutes. A release film (release film) made of a 25 μm-thick biaxially oriented polyester film coated with a silicone-based release agent was attached to the surface (coated surface) of adhesive B so that the surface of adhesive B and the release agent-treated surface (coated surface with silicone-based release agent) were in contact. The obtained sample was aged for 3 days in a 40° C. hot air circulating oven to obtain a surface protection film of Comparative Example 1. Adhesive B became the adhesive layer.
[0065] (Preparation of Surface Protection Film of Comparative Example 2) A surface protective film of Comparative Example 2 was obtained in the same manner as in Comparative Example 1, except that a colorless and transparent biaxially oriented polyester film having a thickness of 75 μm was used instead of the biaxially oriented polyester film having a thickness of 38 μm.
[0066] (Preparation of Surface Protection Film of Comparative Example 3) A surface protective film of Comparative Example 3 was obtained in the same manner as in Comparative Example 1, except that a colorless and transparent biaxially oriented polyester film having a thickness of 100 μm was used instead of the biaxially oriented polyester film having a thickness of 38 μm.
[0067] (Preparation of Surface Protection Film of Comparative Example 4) Adhesive F was obtained by mixing 0.2 parts of an isocyanate-based curing agent as a curing agent with 100 parts of a base polymer consisting of butyl acrylate, methyl acrylate, dimethylacrylamide, a hydroxyl group-containing acrylic monomer, and a carboxyl group-containing acrylate. The adhesive layer (coating thickness 10 μm after drying) formed by applying adhesive F to a biaxially stretched polyester film having a thickness of 38 μm had an adhesive strength of 6.5 N / 25 mm against glass. A surface protection film of Comparative Example 4 was obtained in the same manner as in Example 1, except that adhesive F was used instead of adhesive A.
[0068] (Preparation of Surface Protection Film of Comparative Example 5) 0.3 parts of an isocyanate-based curing agent was mixed with 100 parts of a base polymer consisting of butyl acrylate, methyl acrylate, 2-ethylhexyl acrylate, and a hydroxyl group-containing acrylic monomer to obtain adhesive G. The adhesive layer (coating thickness 10 μm after drying) formed by applying adhesive G to a biaxially stretched polyester film having a thickness of 38 μm had an adhesive strength of 3.2 N / 25 mm to glass. A surface protection film of Comparative Example 5 was obtained in the same manner as in Example 1, except that Adhesive G was used instead of Adhesive A.
[0069] (Preparation of Surface Protection Film of Comparative Example 6) 2.0 parts of an isocyanate-based curing agent was mixed with 100 parts of a base polymer consisting of 2-ethylhexyl acrylate, a hydroxyl group-containing acrylic monomer, and a carboxyl group-containing acrylic monomer to obtain adhesive H. The adhesive layer (coating thickness 20 μm after drying) formed by applying adhesive H to a biaxially stretched polyester film having a thickness of 38 μm had an adhesive strength to glass of 0.6 N / 25 mm. A surface protection film of Comparative Example 6 was obtained in the same manner as in Example 1, except that adhesive H was used instead of adhesive B.
[0070] The evaluation test method is described below. (Measurement of adhesive strength of adhesive layer) An adhesive is applied to a 38μm-thick biaxially oriented polyester film, and then dried in a 120℃ hot air circulating oven for 2 minutes. A release film made of a 25μm-thick biaxially oriented polyester film coated with a silicone release agent is attached to the adhesive surface (adhesive-coated surface). The resulting sample is aged for 3 days in a 40℃ hot air circulating oven. Cut the sample to a width of 25 mm and a length of 150 mm. After removing the release film from the sample, the sample (surface protection film) is attached to a glass plate. A 2 kg rubber roller is rolled back and forth on the sample once to press the sample against the glass plate. The sample and glass plate are then left for 1 hour under conditions of a temperature of 23°C and a relative humidity of 50%, and the strength is measured using a tensile tester when the surface protection film is peeled off at a peel angle of 180° and a peel speed of 300 mm / min.
[0071] (Measurement of storage modulus) The adhesive was applied to a 38μm thick biaxially oriented polyester film, and then dried in a 120℃ hot air circulating oven for 2 minutes. A release film made of a 25μm thick biaxially oriented polyester film coated with a silicone release agent was attached to the surface of the adhesive (the adhesive-coated surface). The obtained sample was aged for 3 days in a 40℃ hot air circulating oven. The adhesive became the adhesive layer. After peeling the release film from the sample, the storage modulus of the adhesive layer at 23℃ was measured using a viscoelasticity measuring device (ABM Dynamic Viscoelasticity Measuring Device Reogel-E4000).
[0072] (Evaluation of handling) A polarizing plate sample (total thickness 48 μm) with a triacetyl cellulose film laminated to one side of a polarizer made of iodine and polyvinyl alcohol is cut to A4 size (210 mm x 297 mm). A surface protective film is laminated to the polarizing plate using a desktop laminator. One of the four corners of the polarizing plate with the surface protective film laminated is held and shaken back and forth 30 times, after which the polarizing plate is visually observed for appearance defects such as folds and unevenness. Those without defects are marked with an O, and those with defects are marked with an X.
[0073] (Evaluation of Curl Suppression) A polarizing plate sample (total thickness 48 μm) with a triacetyl cellulose film attached to one side of a polarizer made of iodine and polyvinyl alcohol was cut to A4 size (210 mm x 297 mm). A surface protection film was attached to the polarizing plate using a desktop laminator. The plate was placed on the laboratory bench with the curled convex side facing down. The distance that each of the four corners was lifted from the surface of the bench was measured, and the largest value was taken as the curl amount. Curls of less than 10 mm were marked with an O, those between 10 mm and 20 mm with a △, and those of 20 mm or more with an X.
[0074] (Evaluation of protective film peelability) A polarizing plate (total thickness 48 μm) is prepared by laminating a triacetyl cellulose film on one side of a polarizer. A sample of the surface protection film (protection film) is cut to a width of 25 mm and a length of 150 mm. After peeling off the release film from the sample, the sample is attached to the triacetyl cellulose film surface of the polarizing plate. A 2 kg rubber roller is rolled back and forth on the sample once to press the sample toward the polarizing plate. After that, the sample and the polarizing plate are left for 24 hours under conditions of a temperature of 23°C and a relative humidity of 50%, and then the strength is measured when the surface protection film is peeled off at a peel angle of 180° and a peel speed of 30 m / min using a high-speed peel tester. Less than 1.8 N / 25 mm is marked as ○, 1.8 N / 25 mm or more but less than 2.5 N / 25 mm is marked as △, and 2.5 N / 25 mm or more is marked as ×.
[0075] (Releasability of the first adhesive layer) A polarizing plate (total thickness 48 μm) is prepared, which has a triacetyl cellulose film laminated on one side of a polarizer, and an adhesive layer and a release film attached to the surface of the adhesive layer on the opposite side of the polarizer from the triacetyl cellulose film. A sample of the surface protection film is cut to a width of 25 mm and a length of 150 mm. After peeling the release film from the sample, the sample is attached to the triacetyl cellulose film surface of the polarizing plate to obtain a polarizing plate with a surface protection film. A 2 kg rubber roller is rolled back and forth on the sample to press the sample against the polarizing plate. Then, the release film attached to the polarizing plate is peeled off, and the polarizing plate with the surface protective film is attached to a glass plate using a table laminator. After that, the polarizing plate with the surface protective film and the glass plate are left for 24 hours under conditions of a temperature of 23°C and a relative humidity of 50%, and then, while holding the second transparent film portion with a hand, the adhesive film consisting of the first transparent film and the first adhesive layer is peeled off from the second transparent film. If the second adhesive layer does not peel off but peels off, it is evaluated as good (◯), and if peeling or lifting occurs in the second adhesive layer, it is evaluated as bad (×).
[0076] The measurement results for each sample are shown in Table 1. In addition, as a reference value, the measurement results of the charged voltage when the surface protective film of Example 1 and Example 5 was peeled off are shown in Table 2.
[0077] [Table 1]
[0078] [Table 2]
[0079] From Tables 1 and 2, the following can be seen: The surface protection films of Examples 1 to 5 had a high suppression effect on the curling of the optical film, and the optical film to which the surface protection film was attached had good handleability. As can be seen from the results of the peeling force, the surface protection films of Examples 1 to 5 were surface protection films that were easy to peel and remove after use. From the results of the peeling property of the first adhesive layer, the surface protection films of Examples 1 to 5 were capable of peeling and removing the adhesive film consisting of the first transparent film and the first adhesive layer. In Example 5, in which an antistatic agent was added to the second pressure-sensitive adhesive layer, the surface protection film had a low peeling electrification voltage when the surface protection film was removed.
[0080] In contrast, the surface protection films of Comparative Examples 1 to 3, in which only the second pressure-sensitive adhesive layer was provided on the polyester film, showed improved handling properties and curl suppression properties by increasing the thickness of the film, but the peelability was reduced. That is, the surface protection films of Comparative Examples 1 to 3 could not improve all of the curl suppression properties, handling properties, and peelability. The surface protection film of Comparative Example 4, in which the adhesive strength of the first pressure-sensitive adhesive layer was high, showed good handling properties and curl suppression properties, but the peel strength and the peelability of the first pressure-sensitive adhesive layer were not good. The surface protection film of Comparative Example 5, in which the first pressure-sensitive adhesive layer had a low storage modulus, showed poor curl suppression properties. Perhaps due to curling, the peelability also deteriorated. The surface protection film of Comparative Example 6 in which the second pressure-sensitive adhesive layer had high adhesive strength was excellent in handleability and curl suppression, but the peelability was not good. [Industrial Applicability]
[0081] The present invention can be used, for example, in the production process of optical films such as polarizing plates, retardation plates, and lens films, and optical components, etc., by adhering to the surfaces of the optical components, etc. to protect the surfaces. In particular, for thin optical films, the effect of suppressing curling of the optical film is high, and the handleability of the optical film to which the surface protective film is attached is improved, and further, it is easy to peel off and remove after use. Therefore, the yield and productivity of the manufacturing process of thin optical films can be improved. In addition, the need to replace the surface protective film or wipe off dirt during shipping is eliminated, leading to improved workability and productivity. [Explanation of symbols]
[0082] 1...first transparent film, 2...first adhesive layer, 3...second transparent film, 4...second adhesive layer, 5...release film, C...optical film, D...optical component, P...surface protection film.
Claims
1. A first transparent film, a first pressure-sensitive adhesive layer, a second transparent film, and a second pressure-sensitive adhesive layer are laminated in this order, The storage modulus of the first pressure-sensitive adhesive layer at 23° C. is 1.0×10 4 Pa or more 8.0×10 4 is less than Pa, the adhesive strength of the first pressure-sensitive adhesive layer is higher than the adhesive strength of the second pressure-sensitive adhesive layer; The adhesive strength of the second pressure-sensitive adhesive layer to glass is 0.5 N / 25 mm or less; Surface protection film.
2. An optical component having the surface protective film according to claim 1 attached thereto.
Citation Information
Patent Citations
Retardation plate having protective film, manufacturing method therefor, adhesive type retardation plate having protective film and adhesive type optical material having protective film
JP2006058560A
Surface protective film, and optical component to which the same is adhered
JP2020083948A
Optical filters for display screens
JP3090774U
Method for manufacturing an adhesive composition, method for manufacturing an adhesive film, raw material composition for adhesives, and adhesive film
JP4937327B2
optical film adhesive sheet
JP6142396B1