Alkali dispersion type hot-melt adhesive composition, container to which label is adhered with the adhesive composition
The hot melt adhesive composition addresses adhesive strength and label displacement issues by using a specific blend of thermoplastic elastomer, solid tackifier, wax, and polybutene, ensuring strong adhesion and easy removal from PET bottles.
Patent Information
- Application Number
- JP2023066851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Existing alkali-dispersed hot melt adhesive compositions for PET bottles face issues with adhesive strength, resistance to label displacement due to bottle expansion, and difficulty in removing labels without leaving residue, especially in thin films and carbonated containers.
A hot melt adhesive composition comprising a thermoplastic elastomer, a solid tackifier with an acid value of 100 to 300 mgKOH/g, a wax with a melting point of 70 to 150°C, polybutene with a kinematic viscosity of 70 to 1000 mm²/s, and a process oil in specific proportions, ensuring high adhesive strength, impact resistance, and easy removal with hot alkaline solutions.
The composition maintains strong adhesion, prevents label displacement during bottle expansion, and allows easy removal without residue, meeting recycling standards for PET bottles and other containers.
Smart Images

Figure 2024153144000001 
Figure 2024153144000002 
Figure 2024153144000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an alkali dispersible hot melt pressure sensitive adhesive composition and a container having a label attached thereto using said pressure sensitive adhesive composition. [Background technology]
[0002] In recent years, the amount of polyethylene terephthalate (hereinafter referred to as PET) bottles used for beverages has been increasing along with the production volume of PET bottles. PET bottles usually have a plastic label attached to the outside of the body to display the product name, etc. There are several methods for attaching a plastic label to the outside of the body of a PET bottle, including the "wrap-around label method," "stretch label method," and "shrink label method."
[0003] In either method, it is required that used PET bottles are collected and can be recycled as raw materials. For example, the "Self-regulation Guidelines for Designated PET Bottles" issued by the PET Bottle Recycling Promotion Council lists the following indicators. That is, when pellets made by cutting bottles with labels are immersed in a 1.5% sodium hydroxide solution at 90°C at a pellet concentration of 10% (weight ratio) and stirred for 15 minutes, the label peels off from the PET pellets and printing ink, adhesives, etc. do not remain on the PET pellets. In order to peel off the label during the recycling process (alkali dispersion type), an alkali dispersion type hot melt adhesive composition has been developed and is used as an adhesive for labels on containers such as PET bottles.
[0004] On the other hand, if the contents contain carbon dioxide, the PET bottle will expand if it is left at high temperatures (40 to 50°C), such as during transportation in the summer. The expansion of the PET bottle puts a load on the label wrapped around the body, which can cause the plastic film at the end of the label to shift from the plastic film located inside. It is therefore required that the end of the label does not shift easily, and even if it does shift, it does not peel off (suitability for actual application). For this reason, it is required that the adhesive strength (peel strength) between the plastic films that are the base material constituting the label is high, and that the hot melt adhesive composition has resistance and conformability to the label shift caused by bottle expansion.
[0005] Furthermore, in recent years, due to environmental considerations, the plastic films and adhesives used in labels have become thinner (normal: 30 to 50 μm, thin: 5 to 20 μm), and it is required that there is no stringiness during coating, and that the label does not peel off due to the impact when the labeled container is dropped. In particular, in containers that are not round, such as those for non-carbonated drinks, the labels tend to peel off due to the impact when dropped, and a hot melt adhesive composition that has excellent impact resistance regardless of the shape of the container is required.
[0006] Patent Document 1 discloses a water-dispersible hot melt adhesive composition containing a copolyester. However, the copolyester described in Patent Document 1 has poor heat resistance and is partially thermally decomposed, which causes a problem that the adhesive strength of the adhesive composition is not stable.
[0007] Patent Document 2 discloses a hot melt adhesive comprising a thermoplastic elastomer (A), a rosin-based tackifier (B) having an acid value of 100 to 300 mgKOH / g, a terpene phenol resin (C), a process oil (D), and a polypropylene wax (E) graft-polymerized with maleic anhydride.
[0008] Patent Document 3 discloses a hot melt adhesive containing a thermoplastic elastomer (A), a rosin-based tackifier (B) having an acid value of 100 to 300 mgKOH / g, a process oil (C), a wax (D) having a needle penetration at 25°C of 10 dmm or less, and a polyethylene glycol (E) having a number average molecular weight of 1,000 or more.
[0009] Patent Document 4 discloses a hot melt adhesive comprising a thermoplastic elastomer (A), a solid tackifier (B) having an acid value of 100 to 300 mgKOH / g, a liquid tackifier (C), a wax (D), and a specific nonionic surfactant (E).
[0010] The labels using the hot melt adhesives disclosed in the cited documents 2 to 4 have sufficiently high adhesive strength and holding power between alkali dispersion-type plastic films, but the adhesive strength is significantly reduced by making the film thickness of the hot melt adhesive composition thin. Furthermore, there are problems in that the resistance and conformability of the hot melt adhesive composition to the displacement of the label due to bottle expansion is lost, causing the label to peel off.
[0011] In other words, there has been a demand for an alkali-dispersible hot-melt pressure-sensitive adhesive composition which is unlikely to cause stringiness even when applied as a thin film, has sufficient adhesive strength, has high hot-melt resistance and conformability to label shifting due to bottle expansion, prevents the label from shifting during long-term storage, and enables the adhered article to be easily peeled off from a container with a hot alkaline aqueous solution without leaving any adhesive residue. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Special Publication No. 11-512134 [Patent Document 2] JP 2010-90185 A [Patent Document 3] JP 2010-280878 A [Patent Document 4] JP 2012-1624 A Summary of the Invention [Problem to be solved by the invention]
[0013] The object of the present invention is to provide an alkali dispersible-type hot melt pressure-sensitive adhesive composition which is resistant to stringiness even when applied as a thin film, has sufficient adhesive strength, has high hot melt resistance and conformability to label shifting due to bottle expansion, prevents the label from shifting during long-term storage, and enables the adhered material to be easily peeled off from the container with a hot alkaline aqueous solution without leaving any adhesive residue, and a container to which a label is affixed using the hot melt pressure-sensitive adhesive composition. [Means for solving the problem]
[0014] The present disclosure provides the following alkali dispersible-type hot melt pressure sensitive adhesive composition and a container to which a label is attached using the pressure sensitive adhesive composition. [1]: Contains a thermoplastic elastomer (A), a solid tackifier (B) having an acid value of 100 to 300 mg KOH / g, a wax (C), polybutene (D) and a process oil (E); 1. An alkali-dispersible hot-melt pressure-sensitive adhesive composition, wherein the content of a process oil (E) is 0 to 50 mass % relative to 100 mass % of the hot-melt pressure-sensitive adhesive composition. [2]: The alkali-dispersible hot melt pressure-sensitive adhesive composition according to the above [1], wherein the thermoplastic elastomer (A) comprises a styrene-based elastomer (A-1) having a styrene content of 25 to 50 mass% and a styrene-based elastomer (A-2) having a styrene content of 5 mass% or more but less than 25 mass%. [3]: The kinetic viscosity of polybutene (D) at 100°C is 70 to 1000 mm 2 The alkali dispersible hot melt pressure sensitive adhesive composition according to the above [1] or [2], wherein [4]: The alkali dispersible-type hot melt pressure-sensitive adhesive composition according to any one of the above [1] to [3], wherein the wax (C) has a melting point of 70 to 150°C. [5]: The alkali-dispersible hot-melt pressure-sensitive adhesive composition according to any one of the above [1] to [4], wherein, based on 100 mass% of the alkali-dispersible hot-melt pressure-sensitive adhesive composition, the content of the thermoplastic elastomer (A) is 5 to 40 mass%, the content of the solid tackifier (B) is 20 to 70 mass%, the content of the wax (C) is 1 to 20 mass%, and the content of the polybutene (D) is 5 to 40 mass%. [6]: A container having a label attached thereto using the alkali dispersible-type hot melt pressure sensitive adhesive composition according to any one of the above [1] to [5]. [7]: The container according to [6] above, wherein the label is a body-wrapped label. [8]: The container according to [6] or [7] above, wherein the material is polyethylene terephthalate. [9]: A container according to any one of [6] to [8] above, which is for carbonated beverages. Effect of the Invention
[0015] The present invention provides an alkali-dispersible hot-melt adhesive composition which is resistant to stringiness even when coated as a thin film, has sufficient adhesive strength, has high resistance and conformability to label displacement caused by bottle expansion, and prevents labels from displacing during long-term storage, particularly in PET bottles for carbonated beverages, which have a large bottle expansion rate, and in addition, when immersed in a hot alkaline aqueous solution, the label is easily peeled off from the container without leaving any adhesive residue and does not reattach. Also provided is a container to which a label is adhered using the alkali-dispersible hot-melt adhesive composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present disclosure will be described in detail below. It should be noted that other embodiments are of course included in the scope of the present invention as long as they conform to the spirit of the present invention.
[0017] In this specification, a numerical range specified by using "~" includes the numerical values before and after "~" as the lower and upper limit ranges. In addition, unless otherwise noted, each of the various components appearing in this specification may be used independently, either alone or in combination of two or more types. In addition, "parts" and "%" represent "parts by mass" and "% by mass", respectively, unless otherwise specified. In this specification, the alkali dispersible hot melt pressure-sensitive adhesive composition may be abbreviated as “hot melt pressure-sensitive adhesive composition.” “Hot melt” refers to a property of being in a solid or viscous state at room temperature and melting and softening to a fluid or liquid state when heated.
[0018] <Alkaline Dispersible Hot Melt Pressure Sensitive Adhesive Composition> The alkali-dispersible hot-melt pressure-sensitive adhesive composition of the present invention contains a thermoplastic elastomer (A), a solid tackifier (B) having an acid value of 100 to 300 mgKOH / g, a wax (C), a polybutene (D) and a process oil (E), and contains 0 to 50 mass% of the process oil (E) per 100 mass% of the hot-melt pressure-sensitive adhesive composition.
[0019] It is preferable that the alkali dispersion-type hot melt adhesive composition contains 5 to 40 mass% of thermoplastic elastomer (A), 20 to 70 mass% of solid tackifier (B), 1 to 20 mass% of wax (C), and 5 to 40 mass% of polybutene (D) based on 100 mass% of the alkali dispersion-type hot melt adhesive composition. By making the thermoplastic elastomer (A) 5 to 40 mass%, the adhesiveness (cohesion) is kept good, by making the solid tackifier (B) 20 to 70 mass%, the adhesiveness (adhesion) is kept good, by making the wax (C) 1 to 20 mass%, the cohesion is kept good, and by making the polybutene (D) 5 to 40 mass%, the label does not peel off when dropped, regardless of the shape of the container.
[0020] In 100% by mass of the alkali dispersion-type hot melt pressure-sensitive adhesive composition, the total content of the thermoplastic elastomer (A), the solid tackifier (B), the wax (C), the polybutene (D) and the process oil (E) is preferably 60 to 100% by mass. By setting it in this range, the adhesiveness and impact resistance can be more effectively brought out. A more suitable range is 70 to 100% by mass, and an even more suitable range is 80 to 100% by mass.
[0021] (Thermoplastic elastomer (A)) Thermoplastic elastomer (A) is a type of thermoplastic elastomer. Thermoplastic elastomers are elastic materials that have the same properties as vulcanized rubber at room temperature, and at high temperatures, they are polymeric materials that can be used with existing molding machines, just like ordinary thermoplastic resins. Thermoplastic elastomers have both elastic rubber components (soft segments: soft phase) in the molecules and molecular restraint components (hard segments: hard phase) to prevent plastic deformation, so they have properties between rubber and plastic. Styrene elastomers generally have a polystyrene block and a rubber middle block, the polystyrene part forms a physical crosslink (domain) and becomes a crosslinking point, and the middle rubber block gives the product rubber elasticity. The middle soft segment includes polybutadiene (B), polyisoprene (I) and polyolefin elastomers (ethylene-propylene (EP), ethylene-butylene (EB), butylene-butadiene (BB)), and depending on the arrangement with the hard segment polystyrene (S), they are divided into linear type and branched type (radial type).
[0022] The content of the thermoplastic elastomer (A) in 100% by mass of the hot melt pressure sensitive adhesive composition is preferably from 5 to 40% by mass, more preferably from 10 to 30% by mass. By including the thermoplastic elastomer (A) in the above range, both cohesive strength and adhesiveness can be achieved.
[0023] The viscosity of a toluene solution of the thermoplastic elastomer (A) at 25° C. (solid content: 25% by mass) is preferably 100 to 2,000 mPa s. When the viscosity of the toluene solution at 25° C. (solid content: 25% by mass) is within this range, both impact resistance and stringiness can be achieved.
[0024] The thermoplastic elastomer (A) preferably contains two types of elastomers: a styrene-based elastomer (A-1) having a styrene content of 25 to 50 mass% and a styrene-based elastomer (A-2) having a styrene content of 5 mass% or more and less than 25 mass%. By simultaneously containing (A-1) and (A-2), it is possible to keep the cohesive strength, adhesiveness, and viscosity at the time of dissolution low, which is preferable. The styrene content of the thermoplastic elastomer (A-1) is more preferably from 25 to 40% by mass, and further preferably from 30 to 40% by mass. The styrene content of the thermoplastic elastomer (A-2) is more preferably 15% by mass or more and less than 25% by mass, and further preferably 15 to 20% by mass.
[0025] The styrene-based elastomer (A-1) and the styrene-based elastomer (A-2) are each preferably contained in an amount of 2.5 to 35 mass%, more preferably 5 to 20 mass%, based on 100 mass% of the alkali dispersible hot melt pressure sensitive adhesive composition. By keeping the amount of the styrene-based elastomer (A-1) within the above range, the effect of reducing the cohesive force and stringiness during labeling is enhanced. In addition, by setting the content of the styrene-based elastomer (A-2) within the above range, the effect of suppressing the cohesive strength, adhesive strength, and viscosity at dissolution is enhanced. In particular, the styrene-based elastomer (A-2), although being a polymer, can suppress the viscosity at dissolution of the hot melt pressure-sensitive adhesive composition, thereby suppressing stringiness during labeling.
[0026] Examples of styrene-based elastomers include styrene-butadiene-styrene block copolymer (hereinafter sometimes abbreviated as SBS), styrene-ethylene / butylene-styrene block copolymer (hereinafter sometimes abbreviated as SEBS), styrene-ethylene / propylene-styrene block copolymer (hereinafter sometimes abbreviated as SEPS), styrene-isoprene-styrene block copolymer (hereinafter sometimes abbreviated as SIS), and styrene-butylene / butadiene-styrene block copolymer (hereinafter sometimes abbreviated as SBBS).
[0027] (Solid tackifier (B)) The solid tackifier (B) is a tackifier that has an acid value of 100 to 300 mgKOH / g and is solid at room temperature. The solid tackifier (B) may enhance the adhesion of the hot melt adhesive composition to labels and bottles. If the acid value exceeds 300 mgKOH / g, the compatibility is poor, the melt viscosity increases, the coating property is poor, and the adhesive force (adhesion) and strength are reduced. If it is less than 100 mgKOH / g, the alkali dispersion type cannot be sufficiently exhibited. The acid value is the number of milligrams of potassium hydroxide (KOH) required to neutralize 1 g of sample, and is a value measured in accordance with JIS K5601-2-1 acid value (titration method). The method for measuring the acid value will be described in detail in the Examples section.
[0028] The solid tackifier (B) having an acid value of 100 to 300 mgKOH / g is not particularly limited, and an example thereof is a rosin-based tackifier. Examples of the rosin-based tackifier include unmodified unhydrogenated rosin, unmodified hydrogenated rosin, (meth)acrylic acid modified rosin, hydrogenated (meth)acrylic acid modified rosin, maleic acid modified rosin, hydrogenated maleic acid modified rosin, fumaric acid modified rosin, and hydrogenated fumaric acid modified rosin.
[0029] The content of the solid tackifier (B) in 100% by mass of the hot melt pressure sensitive adhesive composition is preferably from 20 to 70% by mass, more preferably from 30 to 60% by mass, and even more preferably from 40 to 55% by mass. By containing the rosin-based tackifier (B) in the above range, both alkali dispersibility and adhesiveness (adhesiveness) can be achieved, which is preferable.
[0030] (Wax (C)) The wax (C) used in the present invention is broadly classified into natural waxes: animal waxes (beeswax, ozokerite, etc.), vegetable waxes (japanese wax, rice bran wax, etc.), petroleum waxes (paraffin wax, microcrystalline wax, etc.), and synthetic waxes (Fischer-Tropsch wax, polyethylene wax, polypropylene, and acid-modified waxes, etc.). The wax (C) is used alone or in combination of two or more kinds. From the viewpoint of adhesive strength and impact resistance, the wax (C) is preferably a synthetic wax. More preferably, from the viewpoint of adhesive strength (adhesion), it is polyethylene wax, polypropylene wax, and their acid-modified waxes.
[0031] The melting point of the wax (C) measured by a differential scanning calorimeter (DSC) is preferably in the range of 70 to 150° C. When the melting point of the wax (C) is 70° C. or higher, the heat resistance and adhesiveness (cohesion) become good, and when the melting point is 150° C. or lower, the coatability and alkali dispersibility of the hot melt pressure sensitive adhesive composition become good. The melting point of the wax (C) is more preferably 90 to 150° C. The method for measuring the melting point will be described in detail in the Examples section.
[0032] The content of the wax (C) in 100% by mass of the hot melt pressure sensitive adhesive composition is preferably from 1 to 20% by mass, more preferably from 3 to 15% by mass, and even more preferably from 5 to 10% by mass. By including the wax (C) in the above range, it is possible to achieve both adhesiveness (holding power) and alkali dispersibility. If the adhesiveness (holding power) is high, the label will not peel off during storage as a label for carbonated drinks, but if the adhesiveness is too high, the alkali dispersibility will be lost.
[0033] (Polybutene (D)) Polybutene (D) is a long-chain copolymer in which isobutene is the main monomer and normal butene is partially reacted as a secondary monomer. Unlike low-molecular-weight polyisobutylene in which purified isobutylene is the main monomer, the remaining fraction obtained by extracting butadiene from the C4 fraction produced by naphtha cracking can be used as it is as the monomer (raw material) for such polybutene. Note that polybutene may be a liquid polymer in which a small amount of butene-1 is copolymerized.
[0034] The kinetic viscosity (JIS K2283) of polybutene (D) at 100°C is 70 to 1000 mm 2 The kinematic viscosity of polybutene (D) at 100°C is preferably in the range of 70 mm 2 / s or more, the adhesive strength (holding power) of the label is strong, and the 2 By setting the kinematic viscosity at 100° C. to be not more than 100 mm / s, the label can be easily peeled off in a hot alkaline aqueous solution. 2 / s, and more preferably 150 to 300 mm 2 The method for measuring the kinetic viscosity is described in the Examples section.
[0035] The content of polybutene (D) in 100% by mass of the hot melt pressure sensitive adhesive composition is preferably from 5 to 40% by mass, more preferably from 10 to 25% by mass, and even more preferably from 15 to 20% by mass. By containing the polybutene (D) in the above range, it is possible to achieve both retention power and alkali dispersibility.
[0036] (Process oil (E)) The process oil (E) used in the present invention is an oil generally used as a plasticizer for rubber, thermoplastic elastomers, etc., that is, a process oil produced in petroleum refining, etc., and is roughly classified into paraffinic process oil, naphthenic process oil, and aromatic process oil. From the viewpoint of alkali dispersibility, naphthenic oil is preferred. Process oil is a mixture of aromatic rings, naphthenic rings, and paraffin chains, and naphthenic process oil in this application refers to process oil in which naphthenic ring carbons account for 35-46% by mass of the total carbon of the process oil. In addition, process oils in which aromatic carbons account for 30% by weight or more of the total carbon are classified as aromatic process oils, and process oils in which paraffin chain carbons account for 50% by weight or more of the total carbon are classified as paraffinic process oils.
[0037] The kinetic viscosity of the process oil (E) at 40°C is 50 to 450 mm 2 The kinematic viscosity of the process oil (E) at 40°C is preferably in the range of 50 mm / s. 2 If it is less than / s, the adhesiveness (holding power) will be strong, and 2 More preferably, the pore size is 100 to 450 mm / s. 2 / s or less, and more preferably 200 to 400 mm 2 The method for measuring the kinetic viscosity is described in the Examples section.
[0038] The content of the process oil (E) in 100% by mass of the hot melt composition adhesive is preferably 0 to 50% by mass, more preferably 5 to 40% by mass, and even more preferably 10 to 30% by mass. By including the process oil (E) in the above range, both alkali dispersibility and impact resistance can be achieved. In particular, by including the process oil (E), the label will not peel off when the PET bottle is dropped and impacted, regardless of the shape of the PET bottle.
[0039] The hot melt adhesive composition of the present invention may further contain other components within the range that does not impair the effects of the present invention. Examples of other components include colorants, antiblocking agents, inorganic fillers, antioxidants, bulking agents, flame retardants, plasticizers, antistatic agents, light stabilizers, ultraviolet absorbers, heavy metal deactivators, and fluorescent whitening agents. These components may be used alone or in combination of two or more.
[0040] The colorant may be a commonly used colorant such as red, blue, green, yellow, etc. The colorant may be any of pigments, dyes, and colorants, and examples of the colorant include monoazo, dizazo, azo lake, benzimidazolone, perylene, diketopyrrolopyrrole, condensed azo, anthraquinone, quinacridone, phthalocyanine, and anthraquinone, and examples of the pigment include pigment, perylene, monoazo, condensed azo, isoindolinone, titanium oxide, and carbon.
[0041] The antiblocking agent includes silicone, unsaturated fatty acid amides such as stearic acid amide, oleic acid amide, erucic acid amide, oleic acid amide and behenic acid amide.
[0042] Examples of the inorganic filler include particles and fibers of metals, metal oxides, metal hydroxides, etc. Specific examples include glass fibers, carbon fibers, calcium silicate, calcium titanate, aluminum borate fibers, flake glass, talc, kaolin, mica, hydrotalcite, calcium carbonate, zinc carbonate, zinc oxide, calcium hydrogen phosphate, wollastonite, silica, zeolite, alumina, boehmite, aluminum hydroxide, titanium oxide, silicon oxide, magnesium oxide, calcium silicate, alumina sodium silicate, magnesium silicate, carbon nanotube, graphite, copper, silver, aluminum, nickel, iron, calcium fluoride, mica, montmorillonite, apatite, etc.
[0043] Examples of the antioxidant include pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene)bis[3-(5-t-butyl-4-hydroxy-m-tolyl]propionate, tris(2,4-di-t-butylphenyl)phosphite, bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, etc. These antioxidants may be used alone or in combination of two or more.
[0044] Examples of the filler include wet silica, aluminum hydroxide, aluminum oxide, magnesium oxide, montmorillonite, mica, smectite, organically modified montmorillonite, organically modified mica, and organically modified smectite.
[0045] Examples of the flame retardant include phosphorus-containing compound-based flame retardants, halogen-containing compound-based flame retardants, sulfonic acid metal salt-based flame retardants, and silicon-containing compound-based flame retardants.
[0046] Examples of the plasticizer include phthalate ester plasticizers, polyester plasticizers, aliphatic dibasic acid ester plasticizers, aliphatic monobasic acid ester plasticizers, phosphate ester plasticizers, citrate ester plasticizers, epoxy plasticizers, trimellitate ester plasticizers, tetrahydrophthalate ester plasticizers, glycol plasticizers, and bisphenol A alkylene oxide derivatives.
[0047] The antistatic agent may be any agent commonly used as an antistatic agent for plastics, and specific examples thereof include nonionic surfactants (e.g., fatty acid esters of polyhydric alcohols, ethylene oxide adducts of alkylamines, and fatty acid esters of ethylene oxide adducts of alkylamines), anionic surfactants (e.g., alkylbenzenesulfonates, higher alcohol sulfate salts), cationic surfactants (e.g., aliphatic amine salts, quaternary ammonium salts), and amphoteric surfactants (e.g., imidazoline type, betaine type, etc.).
[0048] Examples of the light stabilizer include hindered amine compounds and benzoate compounds.
[0049] Examples of the ultraviolet absorbing agent include a benzophenone-based ultraviolet absorbing agent, a triazine-based ultraviolet absorbing agent, and a benzotriazole-based ultraviolet absorbing agent.
[0050] The heavy metal deactivator includes a salicylic acid derivative, a hydrazide derivative, an oxalic acid amide derivative, and the like.
[0051] Examples of the fluorescent whitening agent include stilbene-based, coumarin-based, oxazole-based, and naphthalimide-based agents.
[0052] The content of other components other than the thermoplastic elastomer (A), the solid tackifier (B) having an acid value of 100 to 300 mgKOH / g, the wax (C), the polybutene (D) and the process oil (E) is preferably 0 to 40 mass%, more preferably 0 to 30 mass%, and even more preferably 0 to 20 mass%, based on 100 mass% of the alkali dispersion-type hot melt pressure sensitive adhesive composition.
[0053] The alkali-dispersible hot melt adhesive composition of the present invention can be used as an adhesive for adhering paper, plastic film, etc. to various substrates such as glass, plastic, and metal. The alkali-dispersible hot melt adhesive composition of the present invention can easily peel off the attached paper, film, etc. with hot alkaline water, so that it is preferably used as an adhesive for labels of glass containers such as glass bottles used for soft drinks, seasonings, detergents, shampoos, edible oils, cosmetics, medicines, etc. and plastic containers such as PET (polyethylene terephthalate) bottles. However, the use of the adhesive of the present invention is not limited to this label use, and it can be used as an adhesive for all conventionally known uses such as packing tape, clear case, and assembly. However, as specifically shown in the examples, the alkali-dispersible adhesive composition of the present invention satisfies the label peeling requirements with hot alkaline water in the "Voluntary Regulation Guideline for Designated PET Bottles" issued by the PET Bottle Recycling Promotion Council, and has the followability of the hot melt adhesive composition against the displacement of the label due to bottle expansion, so that it is particularly preferable to use it as an adhesive for adhering a label to a PET bottle, that is, an adhesive suitable for recycling of PET bottles.
[0054] As the label substrate for PET bottles, biaxially oriented polypropylene (OPP), polyethylene (PE), PET, and even paper are usually used. In addition, the label is used with a suitable printing on the side opposite to the side to which the alkali dispersible hot melt adhesive composition is applied, i.e., the surface of the label, or on the side to which the alkali dispersible hot melt adhesive composition is applied, i.e., the backside of the label. The alkali dispersible hot melt adhesive composition of the present invention can be applied to the printed side of a label that has been printed, or of course, it can be applied to a label that has not been printed. In either case, it exhibits a predetermined adhesiveness, peelability, and hot alkaline water solubility. In addition, the printing may be performed on the entire backside of the label, or may be performed on only a part of the surface. The printing may be performed by any of the conventionally known printing methods, such as gravure printing and UV printing.
[0055] (Production of alkali-dispersible hot melt adhesive composition) The alkali-dispersible hot-melt pressure-sensitive adhesive composition of the present invention can be produced, for example, by mixing and dispersing the thermoplastic elastomer (A) into a mixture of wax (C), polybutene (D), and optionally process oil (E) in a melting pot equipped with a stirrer, and then adding and mixing the solid tackifier (B).
[0056] The hot melt pressure sensitive adhesive composition of the present invention may be used after mixing the components and molding them into a desired shape. Examples of the desired shape include granules, pellets, sheets, and blocks. These methods can be performed by using known methods without any restrictions.
[0057] (container) The container in the present invention refers to a container to which a label is attached using an alkali dispersible hot melt pressure sensitive adhesive composition. The material of the container may be glass, plastic, paper, etc., but is not particularly limited. The shape of the container may be round or non-round, such as rectangular. A specific example is a polyethylene terephthalate (PET) bottle to which a label is attached.
[0058] In the case of PET bottles, in addition to those in which a label is attached to a part of the body of the PET bottle, a body-wrapped label that is wrapped around the body of the bottle to cover it in a circumferential manner is used, and the hot melt adhesive composition of the present invention is also preferably used for bonding the body-wrapped label. OPP films are often used as such body-wrapped labels. The alkali-dispersible hot melt adhesive composition of the present invention can provide good adhesion to body-wrapped labels such as OPP films, whether they are printed on the back or not. The alkali-dispersible hot melt adhesive composition of the present invention may be applied to the entire back surface of the label, or the adhesive may be applied to a part of the back surface of the label. Examples of application methods include an open wheel method, a closed gun method, and a direct coat method. As methods that do not leave glue on the PET bottle when peeled off, the open wheel method and the direct coat method are preferred.
[0059] The coating amount of the alkali dispersible hot melt adhesive composition of the label to be attached to the container of the present invention is 10 to 300 g / m 2 The coating amount is preferably 10 to 300 g / m 2 As a result, excellent effects are exhibited in terms of alkali dispersibility, adhesiveness, etc. EXAMPLES
[0060] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the following examples. In the examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0061] [viscosity] A solution at 25° C. was prepared by dissolving the styrene-based elastomer in toluene so that the solid content was 25% by mass, and the viscosity was measured using a B-type viscometer.
[0062] [Acid value] The acid value was measured in accordance with JIS K5601-2-1 Acid Value (Titration Method). Specifically, 1 g of sample was precisely weighed and placed in a 250 ml flask, 50 ml of ethanol or an equal volume mixture of ethanol and ether was added, and the sample was dissolved by heating, and titrated with 0.1N potassium hydroxide solution while shaking occasionally (indicator: phenolphthalein). The end point of the titration was the point at which the light pink color of the solution remained for 30 seconds. Next, a blank test was performed in the same manner to make corrections, and the acid value was calculated from the following formula. Acid value = [amount of 0.1N potassium hydroxide solution consumed (ml) x 5.611] / [amount of sample (g)]
[0063] [Melting point] The melting point of the wax was measured using a differential scanning calorimeter (FT / IR-4X, manufactured by JASCO Corporation). Approximately 5 mg of sample was taken and cooled to 0°C, then heated to 170°C at a heating rate of 10°C / min, and then cooled to 0°C at a cooling rate of -20°C / min. After holding at 0°C for 1 minute, it was heated again at a heating rate of 10°C / min, and the amount of heat released and absorbed when heated to 170°C was measured. The melting peak when the wax melted was taken as the melting point.
[0064] [Kinematic viscosity] The kinetic viscosity of polybutene (D) and process oil (E) was measured in accordance with JIS K2283. The kinetic viscosity of polybutene (D) was measured at 100°C, and the kinetic viscosity of process oil (E) was measured at 40°C.
[0065] Next, the present invention will be described based on specific examples in comparison with comparative examples, but the present invention is not limited to these. In the examples, "parts" and "%" respectively represent "parts by mass" and "% by mass" unless otherwise specified.
[0066] Hot melt pressure sensitive adhesive compositions of Examples and Comparative Examples The raw materials used are shown below.
[0067] [Thermoplastic elastomer (A)] Kraton G1650 (Kraton Polymers), styrene content: 30% by mass, viscosity of 25% solids in toluene solution: 8,000 mPa s, SEBS Kraton G1651 (Kraton Polymers), styrene content: 33% by mass, viscosity of 25% solids in toluene solution: 50,000 mPa·s or more, SEBS Kraton G1652 (Kraton Polymers), styrene content: 30% by mass, viscosity of 25% solids in toluene solution: 1,800 mPa s, SEBS Kraton G1726 (Kraton Polymers), styrene content: 30% by mass, viscosity of 25% solids in toluene solution: 200 mPa s, SEBS Kraton D1102 (Kraton Polymers), styrene content: 28% by mass, viscosity of 25% solids in toluene solution: 1,100 mPa s, SBS Kraton D1162 (Kraton Polymers), styrene content: 43% by mass, viscosity of 25% solids in toluene solution: 120 mPa s, SIS Kraton G1645 (Kraton Polymers), styrene content: 13% by mass, viscosity of 25% solids in toluene solution: 120 mPa·s or less, SEBS Kraton D1161 (Kraton Polymers), styrene content: 15% by mass, viscosity of 25% solids in toluene solution: 1,200 mPa s, SIS Kraton G1643 (Kraton Polymers), styrene content: 19% by mass, viscosity of 25% solids in toluene solution: 200 mPa s, SEBS Kraton D1111 (Kraton Polymers), styrene content: 22% by mass, viscosity of 25% solids in toluene solution: 1,100 mPa s, SIS
[0068] [Solid tackifier (B)] RHR-301 (Wuzhou Sun Shine Forestry & Chemicals Co., LTD. Of Guangxi), hydrogenated rosin, acid value: 165mgKOH / g KE-604B: Pine Cristal KE-604B (manufactured by Arakawa Chemical Industries, Ltd.), alkali-modified rosin, acid value: 246 mg KOH / g Haritac AQ-90A (Harima Chemicals), acid value: 105 mg KOH / g [Other tackifiers] Alcon P-100 (Arakawa Chemical Co., Ltd.), alicyclic saturated hydrocarbon resin, acid value 0 mg KOH / g KR-120: Pine Crystal KR-120 (Arakawa Chemical Co., Ltd.), acid-modified ultra-light-colored rosin, acid value: 320 mg KOH / g KR-50M: Pine Crystal KR-50M (manufactured by Arakawa Chemical Co., Ltd.), ultra-light-colored rosin, acid value: 95 mg KOH / g
[0069] Wax HNP-11 (Nippon Seiro Co., Ltd.) Paraffin wax, melting point: 68°C Ricothene PPMA6252 (Client Chemicals), acid-modified polypropylene wax, melting point: 140°C POLYWAX655 (NuCera Solutions) Polyethylene wax, melting point: 95℃ Viscol 660P (Sanyo Chemical Industries, Ltd.), polyethylene wax, melting point: 136°C
[0070] [Polybutene (D)] HV-35 (ENEOS) 100℃ kinematic viscosity: 85mm 2 / s HV-50 (ENEOS) 100℃ kinematic viscosity: 110mm 2 / s HV-100 (ENEOS) 100℃ kinematic viscosity: 220mm 2 / s HV-300 (ENEOS) 100℃ kinematic viscosity: 590mm 2 / s
[0071] [Process oil (E)] PW-32: Diana Process Oil PW-32 (Idemitsu Kosan Co., Ltd.), 40°C kinematic viscosity: 31mm 2 / s PW-90: Diana Process Oil PW-90 (Idemitsu Kosan Co., Ltd.), 40°C kinematic viscosity: 95mm 2 / s PW-150: Diana Process Oil PW-150 (Idemitsu Kosan Co., Ltd.), 40°C kinematic viscosity: 145mm 2 / s PW-380: Diana Process Oil PW-380 (Idemitsu Kosan Co., Ltd.), 40°C kinematic viscosity: 381mm 2 / s PS-430: Diana Process Oil PS-430 (Idemitsu Kosan Co., Ltd.), 40°C kinematic viscosity: 438mm 2 / s
[0072] [Antioxidants] IRG1010 (IRG1010, manufactured by BASF), pentaerythritol tetrakis[3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]
[0073] Example 1 <Production of alkali-dispersible hot melt pressure sensitive adhesive composition> In a stainless steel beaker equipped with a stirrer, 7 parts of wax (C): HNP-11, 21 parts of polybutene (D): HV-100, and 0.5 parts of other components: IRG1010 were added and melted by heating. Heating was performed carefully so that the contents would be at 130 to 150°C. After melting, stirring was performed to obtain a uniform molten solution, and then 7 parts of Kraton D1102 as a styrene-based elastomer (A-1) and 25 parts of Kraton G1645 as (A-2) were gradually added to the melt while maintaining the temperature at 130 to 150°C and continuing to stir, and after the addition was completed, the mixture was heated and stirred at a temperature of 130 to 150°C to completely melt the styrene-based elastomer (A). Then, 40 parts of solid tackifier (B): RHR-301 were added to obtain a molten uniform mixture, which was then cooled to prepare an alkali-dispersible hot melt adhesive composition.
[0074] (Examples 2 to 12, Comparative Examples 1 and 4) According to the compositions shown in Tables 1 and 3, the styrene-based elastomers (A-1) and (A-2), the solid tackifier (B), the wax (C), the polybutene (D) and other components were melted and mixed in the same manner as in Example 1 to prepare hot melt pressure sensitive adhesive compositions, which were then evaluated in the same manner.
[0075] Example 13 In a stainless steel beaker equipped with a stirrer, 2 parts of wax (C): Ricosene PPMA6252, 5 parts of polybutene (D): HV-100, 35 parts of process oil (E): PW-380, and 0.5 parts of other component IRG1010 were added and melted by heating. Heating was performed carefully so that the contents were kept at 130 to 150°C. After melting, stirring was performed to obtain a uniform molten solution, and then 3 parts of Kraton G1651 as a styrene-based elastomer (A-1) and 10 parts of Kraton G1645 as (A-2) were gradually added to the melt while maintaining the temperature at 130 to 150°C and continuing to stir. After the addition was completed, the mixture was heated and stirred at a temperature of 130 to 150°C to completely melt the styrene-based elastomer (A). Thereafter, 45 parts of solid tackifier (B): RHR-301 was added, and the mixture was made into a molten homogeneous mixture, which was then cooled to prepare an alkali dispersion-type hot melt pressure sensitive adhesive composition.
[0076] (Examples 14 to 25, Comparative Examples 2, 3, 5 to 8) According to the compositions shown in Tables 2 and 3, the styrene-based elastomers (A-1) and (A-2), the solid tackifier (B), the wax (C), the polybutene (D), the process oil (E) and other components were melted and mixed in the same manner as in Example 1 to prepare hot melt pressure sensitive adhesive compositions, which were then evaluated in the same manner.
[0077] The resulting alkali-dispersible hot-melt pressure-sensitive adhesive composition was evaluated for adhesion (adhesion), adhesion (cohesion), impact resistance, alkali dispersibility and stringiness by the following methods. The results are shown in Table 3.
[0078] <Adhesiveness (adhesion)> (Sample preparation method) The label with adhesive composition is made by applying hot melt adhesive to the printed surface of OPP with a thickness of 30 μm and a coating weight of approximately 20 g / m2. 2 The label with the hot melt adhesive composition was applied at 23° C. to the non-printed surface of a 30 μm-thick OPP film, and the label was pressed by rolling it back and forth once with a hand roller, and cut to a width of 15 mm. (Test Method) Adhesion (tightness) was evaluated by measuring the peel strength at 180 degrees peeling (peel speed: 300 mm / min) with a tensile tester in a thermostatic room at a temperature of 23% and a relative humidity of 50%. A stronger peel strength is better, with evaluation results of 2 to 5 being considered pass and evaluation result 1 being considered fail. (Evaluation Criteria) 5: 3.5N / 15mm or more 4: 2.5N / 15mm or more, less than 3.5N / 15mm 3: 1.5N / 15mm or more, less than 2.5N / 15mm 2: 1.0N / 15mm or more, less than 1.5N / 15mm 1: Less than 1.0N / 15mm
[0079] <Adhesiveness (cohesive force)> (Sample preparation method) A hot melt adhesive composition heated to 150°C was hand-applied to both ends of a printed OPP film (30μm thick) measuring 325mm long and 62mm wide to prepare a test label. The label attached to a 1.5-liter PET bottle containing Coca-Cola was peeled off in advance, and the bottle was opened and immediately sealed, after which the prepared test label was affixed to the original label position (one end was affixed to the PET bottle, and the other was affixed so that the labels overlapped). (Test Method) The bottle was placed in a thermostatic oven at 40°C, and the appearance was observed after one week. The peeling state and the amount of displacement of the label were measured to evaluate the adhesiveness (cohesive strength). Evaluation results of 2 to 5, in which the label was displaced but not peeled, were considered to be acceptable, and evaluation result 1, in which the label was peeled off, was considered to be unacceptable. The less the label was displaced, the better the result. (Evaluation Criteria) 5: Label misalignment is less than 3 mm 4: Label misalignment is between 3mm and 5mm 3: Label misalignment is between 5mm and 8mm 2: The label is misaligned by 8mm or more, but the label does not peel off. 1: The label peels off
[0080] <Impact resistance 1 (round carbonated beverage container)> (Sample preparation method) A hot melt adhesive composition heated to 150°C was hand-applied to both ends of a printed OPP film (30μm thick) measuring 325mm long and 62mm wide to create a test label. The label attached to a 1.5-liter PET bottle containing Coca-Cola was peeled off in advance, and the test label was attached to the original label position (one end was attached to the PET bottle, and the other end was attached so that the labels overlapped). (Test Method) The bottles with the labels were dropped horizontally onto PVC tiles from heights of 50cm, 80cm, 120cm, and 150cm in order, and the heights were measured to see if the labels peeled off. Evaluation results of 2 to 5, in which the label did not peel off when dropped from a height of 50cm, were deemed to be acceptable, and evaluation result 1, in which the label peeled off when dropped from a height of 50cm, was deemed to be unacceptable. It is better if the label does not peel off even when dropped from a higher height. (Evaluation Results) 5: The label will not peel off even if it is dropped from a height of 50cm, 80cm, 120cm, or 150cm. 4: When dropped from a height of 50cm, 80cm, or 120cm, the film did not peel off, but when dropped from a height of 150cm, it peeled off. 3: When dropped from heights of 50cm and 80cm, the film did not peel off, but when dropped from heights of 120cm and 150cm, the film peeled off. 2: When dropped from 50cm, the film did not peel off, but when dropped from heights of 80cm, 120cm, and 150cm, it peeled off. 1: The label peeled off when dropped from any height: 50cm, 80cm, 120cm, or 150cm.
[0081] <Impact resistance 2 (non-round containers containing non-carbonated beverages)> (Sample preparation method) A hot melt adhesive composition heated to 150°C was hand-applied to both ends of a printed surface of an OPP film (thickness 30μm) with a length of 348mm and width of 83mm to prepare a test label. The label was removed from a 2-liter PET bottle of Itoen Barley Tea in advance, and the prepared test label was affixed to the original label position (one end was affixed to the PET bottle, and the other was affixed so that the labels overlapped). (Test Method) The labeled bottles thus produced were dropped horizontally onto PVC tiles from heights of 50cm, 80cm, 120cm, and 150cm in order, and the heights were measured to see if the labels peeled off. Evaluation results 2 to 5, in which the label did not peel off when dropped from a height of 50cm, were deemed acceptable, and evaluation result 1, in which the label peeled off when dropped from a height of 50cm, was deemed unacceptable. It is better if the label does not peel off even when dropped from a higher height. (Evaluation Results) 5: The label will not peel off even if it is dropped from a height of 50cm, 80cm, 120cm, or 150cm. 4: When dropped from a height of 50cm, 80cm, or 120cm, the film did not peel off, but when dropped from a height of 150cm, it peeled off. 3: When dropped from heights of 50cm and 80cm, the film did not peel off, but when dropped from heights of 120cm and 150cm, the film peeled off. 2: When dropped from 50cm, the film did not peel off, but when dropped from heights of 80cm, 120cm, and 150cm, it peeled off. 1: The label peeled off when dropped from any height: 50cm, 80cm, 120cm, or 150cm.
[0082] <Alkaline dispersibility> (Sample preparation method) A hot melt adhesive composition heated to 150°C was hand coated to a thickness of 20μm on the printed surface of a label printed on a 30μm thick OPP film to prepare a test label with adhesive. The prepared test label was cut to the same size as a 500ml Coca-Cola PET bottle label, attached to a 500ml Coca-Cola PET bottle from which the label had been removed, and cut to approximately 8mm x 8mm square to prepare an evaluation sample (pellet). (Test Method) In a 1000 ml round flask, 180 g of 2.0 mass % sodium hydroxide aqueous solution at 85 to 90°C and 20 g of the pellets were placed and stirred at 120 rpm (stirring blade: propeller). After 10 minutes, the mixture was filtered through a filter, and the residual rate (area %) of the adhesive remaining on the PET pellets was visually observed and evaluated. The better the label was peeled off from the PET pellets and the less hot melt adhesive composition there was, the better. Evaluation results of 2 to 5 were considered to be acceptable, and evaluation result 1, in which the label remained on the PET pellets, was considered to be unacceptable. (Evaluation Criteria) 5: The label with the hot melt adhesive composition and the hot melt adhesive composition do not remain on the PET pellets. 4: No label with the hot melt adhesive composition remains, but less than 30% of the hot melt adhesive composition remains on the PET pellet. 3: No label with hot melt adhesive composition remains, but 30% or more but less than 50% of the hot melt adhesive composition remains on the PET pellet 2: No label with hot melt adhesive composition remains, but 50% or more of the hot melt adhesive composition remains on the PET pellets 1: The label with the hot melt adhesive composition remains on the PET.
[0083] <Stringiness> The evaluation of stringiness with a labeler depends on the viscosity at the coating temperature, so the viscosity was measured at 150° C. The higher the temperature, the lower the viscosity of the hot-melt pressure-sensitive adhesive composition. However, if the temperature is higher than 150° C., fumes are generated from the hot-melt pressure-sensitive adhesive composition, which contaminates the labeler, so the evaluation was performed at 150° C. The viscosity was measured according to the "Japanese Industrial Standards", JIS K6862 (Method A). 300 g of the hot melt adhesive composition, which had been melted to about 160°C in advance, was placed in a test container, and the mixture was thoroughly stirred in the air with a rod thermometer until the temperature reached 150°C. The viscosity was measured using a B-type thermometer (TOKIMEC VISCOMETER MODEL: BM, manufactured by Toki Sangyo Co., Ltd.) (an appropriate rotor was used as necessary). Evaluation results 2 to 5, which were viscosities of less than 2500 mPa / s at 150°C, were considered to be pass, and evaluation result 1, which was 2500 mPa / s or more at 150°C, was considered to be fail. The lower the viscosity at 150°C, the better the stringiness. (Evaluation Criteria) 5: Viscosity at 150℃ is less than 1000mPa / s 4: Viscosity at 150℃ is 1000mPa / s or more and less than 2000mPa / s 3: Viscosity at 150℃ is 2000mPa / s or more but less than 3000mPa / s 2: Viscosity at 150℃ is 3000mPa / s or more but less than 5000mPa / s 1: Viscosity at 150℃ is 5000mPa / s or more
[0084] [Table 1]
[0085] [Table 2]
[0086] [Table 3]
[0087] From Tables 1 and 2, the hot melt pressure sensitive adhesive composition of the present invention has strong adhesive strength, adhesion (cohesion) and impact resistance of the hot melt pressure sensitive adhesive composition against label displacement caused by bottle expansion due to carbonated water, and has thermal alkali dispersibility. Furthermore, the occurrence of stringing during labeling is low. On the other hand, Comparative Examples 1 to 8 (Table 3) did not obtain results that satisfied all of the requirements for adhesion (adhesion and cohesion), impact resistance, alkali dispersibility, and occurrence of stringing during labeling. [Industrial Applicability]
[0088] As described above, the alkali dispersible hot melt adhesive composition of the present invention allows the labels to be easily peeled off when recycling used containers, and allows the containers to be easily separated by immersing them in a hot alkaline aqueous solution. It is suitable for PET bottles for beverages, but it has been found that it exhibits similar performance not only in PET bottles but also in glass containers, and is a hot melt adhesive composition suitable for recycling glass containers.
Claims
1. The present invention comprises a thermoplastic elastomer (A), a solid tackifier (B) having an acid value of 100 to 300 mgKOH / g, a wax (C), a polybutene (D) and a process oil (E), An alkali-dispersible hot-melt pressure-sensitive adhesive composition, comprising: a process oil (E) in an amount of 0 to 50 mass % based on 100 mass % of the hot-melt pressure-sensitive adhesive composition.
2. The alkali dispersible hot melt pressure sensitive adhesive composition according to claim 1, characterized in that the thermoplastic elastomer (A) comprises a styrene-based elastomer (A-1) having a styrene content of 25 to 50 mass% and a styrene-based elastomer (A-2) having a styrene content of 5 mass% or more and less than 25 mass%.
3. The kinetic viscosity of polybutene (D) at 100°C is 70 to 1000 mm 2 2. The alkali dispersible hot melt pressure sensitive adhesive composition according to claim 1, wherein the alkali dispersible hot melt pressure sensitive adhesive composition is a hydroxy group-containing amine.
4. 2. The alkali dispersible hot melt pressure sensitive adhesive composition according to claim 1, wherein the wax (C) has a melting point of 70 to 150°C.
5. The alkali-dispersible hot-melt pressure-sensitive adhesive composition according to claim 1, characterized in that, based on 100 mass% of the alkali-dispersible hot-melt pressure-sensitive adhesive composition, the content of the thermoplastic elastomer (A) is 5 to 40 mass%, the content of the solid tackifier (B) is 20 to 70 mass%, the content of the wax (C) is 1 to 20 mass%, and the content of the polybutene (D) is 5 to 40 mass%.
6. A container having a label adhered thereto using the alkali dispersible hot melt pressure sensitive adhesive composition according to any one of claims 1 to 5.
7. 7. The container of claim 6, wherein the label is a wraparound label.
8. 7. The container according to claim 6, characterized in that the material is polyethylene terephthalate.
9. 9. The container according to claim 8, characterized in that it is for carbonated beverages.
Citation Information
Patent Citations
Roll shrink label and container with the label
JP2011118102A
Hot-melt adhesive and plastic label with hot-melt adhesive
JP2016204588A
Alkali dispersion type hot-melt adhesive
JP2021095448A
Water-dispersible adhesive composition
JP1999512134A
Alkali-dispersible hot-melt adhesive composition, method for producing the same, method for attaching label, and container
JP2010090185A