Semiconductor device
The semiconductor device addresses high contact resistance and miniaturization challenges in oxide transistors by using a specific conductive film arrangement, ensuring high on-state current and reduced resistance in miniaturized designs.
Patent Information
- Application Number
- JP2024122273
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2011-09-22
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2032-09-18
AI Technical Summary
Transistors using oxide semiconductors face challenges with high contact resistance between the semiconductor film and the source or drain electrodes, leading to reduced on-current and difficulty in miniaturization due to overlapping electrodes, which hinder the improvement of on-state current and increase resistance.
The semiconductor device incorporates a unique configuration with a pair of first and second conductive films acting as source or drain electrodes, separated by a third conductive film functioning as a gate electrode, allowing for non-overlapping placement and reduced resistance, thereby maintaining a high on-state current even with miniaturization.
This configuration enhances the on-state current of transistors by minimizing contact resistance and electrode overlap, enabling efficient operation even in miniaturized designs.
Smart Images

Figure 2024153784000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor device using an insulated gate field effect transistor. [Background technology]
[0002] In recent years, the high mobility achieved by polysilicon and microcrystalline silicon and the high mobility achieved by amorphous silicon have been Oxide semiconductors are being developed as new semiconductor materials that combine uniform device characteristics obtained by the use of Metal oxides, which are called conductors and exhibit semiconducting properties, are attracting attention. For example, indium oxide, a well-known metal oxide, is used in liquid It is used as a transparent electrode material in liquid crystal display devices. Examples of the oxides include tungsten oxide, tin oxide, indium oxide, and zinc oxide. Transistors that use metal oxides that exhibit such semiconducting properties in the channel formation region are already known. It has been reported (Patent Document 1 and Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-123861 A [Patent Document 2] JP 2007-96055 A Summary of the Invention [Problem to be solved by the invention]
[0004] By the way, in silicon transistors, the addition of a small amount of impurities to the semiconductor film However, in transistors using oxide semiconductors, the valence electrons are controlled by the Unlike transistors using valence electrons, technology for controlling valence electrons by adding impurities has been established. Therefore, in a transistor using an oxide semiconductor, In some cases, a conductive film that functions as a semiconductor film is directly connected to a channel forming region of the semiconductor film. Therefore, in a transistor using an oxide semiconductor, The contact resistance between the drain electrode and the gate electrode is large, which hinders the improvement of the on-current. do.
[0005] In addition, in the case of a silicon-based transistor, a gate electrode and a resist are used as a mask. By adding impurities to the semiconductor film, a source region and a drain region are formed. The channel length can be controlled by adjusting the size of the gate electrode and resist. On the other hand, in a transistor using an oxide semiconductor, the channel length is controlled by the source electrode and the drain electrode. This is done by adjusting the spacing between the in-electrodes. The distance between the source and drain electrodes needs to be shortened, and depending on the size of the gate electrode In addition, the gate electrode and the source electrode or the drain electrode may partially overlap each other.
[0006] In the case of a top-gate transistor in which the gate electrode is located on top of the semiconductor film, the source electrode It is preferable to provide the source and drain electrodes under the semiconductor film. In order to ensure the step coverage of the semiconductor film at the edge of the doped electrode, It is necessary to reduce the film thickness of the source electrode and the drain electrode. Therefore, the resistance of the source and drain electrodes increases. However, it is difficult to increase the on-state current of a transistor.
[0007] In light of the above technical background, the present invention is capable of increasing the on-current of a transistor. It is an object of the present invention to provide a semiconductor device which can [Means for solving the problem]
[0008] In one aspect of the present invention, a semiconductor device includes a transistor, and a pair of first conductive films on an insulating surface. a semiconductor film on the pair of first conductive films; and a pair of semiconductor films connected to the pair of first conductive films, a second conductive film, an insulating film on the semiconductor film, and a second insulating film provided at a position overlapping the semiconductor film on the insulating film; The pair of first conductive films and the pair of second conductive films are connected to the source electrode. The first conductive film can function as a gate electrode or a drain electrode, and the third conductive film can function as a gate electrode. It is possible.
[0009] In one embodiment of the present invention, the direction in which carriers move in the semiconductor film, i.e., the channel length direction, The distance between the source electrode and the drain electrode can be determined by the distance between the pair of first conductive films. Therefore, the distance between the pair of second conductive films is longer than the distance between the pair of first conductive films. Thus, the arrangement of the pair of second conductive films can be determined. When it becomes necessary to shorten the distance between the source electrode and the drain electrode due to miniaturization of transistors, In this case, the distance between the pair of first conductive films may be shortened, and the pair of second conductive films and third conductive films may be formed by semiconductor The distance between the pair of second conductive films can be increased so as not to overlap on the conductive film. Specifically, a pair of second conductive films are formed on the semiconductor film so as to sandwich the third conductive film therebetween and spaced apart from each other. Therefore, even if the transistor is miniaturized, the third conductive film can be formed. Since the electric field applied to the semiconductor film is not easily blocked by the pair of second conductive films, a high on-state current is obtained. You can get the flow.
[0010] In one embodiment of the present invention, a pair of first conductive films is provided under a semiconductor film, and a pair of first conductive films is provided on the semiconductor film. The third conductive film is present. Therefore, as the transistor is miniaturized, the gap between the pair of first conductive films By shortening the distance, the third conductive film functioning as the gate electrode and the pair of first conductive films overlap each other. However, the electric field applied to the semiconductor film from the third conductive film is blocked by the pair of first conductive films. Therefore, even if the transistor is miniaturized, a high on-state current can be obtained.
[0011] In order to improve the step coverage of the semiconductor film at the ends of the pair of first conductive films, Even if the thickness of the pair of first conductive films is kept small, the thickness of the pair of first conductive films and the pair of second conductive films By connecting the first conductive film and the second conductive film to each other, Therefore, the resistance of the source electrode or drain electrode can be kept low.
[0012] Alternatively, in a semiconductor device according to an aspect of the present invention, in addition to the above configuration, a pair of second conductive films It may be located on the semiconductor film.
[0013] When the pair of second conductive films is located on the semiconductor film, the pair of second conductive films is spaced apart from the semiconductor film. In the case where a pair of first conductive films and a pair of second conductive films functioning as a source electrode or a drain electrode are provided, In addition, a large area can be secured for the contact between the pair of second conductive films and the semiconductor film. Even if the transistor is miniaturized, the transistor is composed of a pair of first conductive films and a pair of second conductive films. The contact resistance between the source electrode or drain electrode and the semiconductor film can be reduced. Therefore, a high on-current can be obtained. Effect of the Invention
[0014] In one embodiment of the present invention, a semiconductor device including a transistor with high on-state current having the above structure is provided. It is possible to achieve this. [Brief description of the drawings]
[0015] [Figure 1] 1A and 1B are diagrams illustrating a structure of a transistor included in a semiconductor device according to one embodiment of the present invention. [Diagram 2] 1A and 1B are diagrams illustrating a structure of a transistor included in a semiconductor device according to one embodiment of the present invention. [Diagram 3] 1A and 1B are diagrams illustrating a structure of a transistor included in a semiconductor device according to one embodiment of the present invention. [Figure 4] 1A and 1B are diagrams illustrating a structure of a transistor included in a semiconductor device according to one embodiment of the present invention. [Diagram 5] 1A and 1B are diagrams illustrating a structure of a transistor included in a semiconductor device according to one embodiment of the present invention. [Figure 6] 1A to 1C illustrate a method for manufacturing a semiconductor device. [Figure 7] 1A to 1C illustrate a method for manufacturing a semiconductor device. [Figure 8] 1A to 1C illustrate a method for manufacturing a semiconductor device. [Figure 9] FIG. 2 is a diagram showing the configuration of a memory cell. [Figure 10] FIG. 2 is a diagram showing the configuration of a storage device. [Figure 11] FIG. 2 is a diagram showing the configuration of an inverter. [Figure 12] Electronic devices illustration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following description, and the embodiments and aspects of the present invention may be modified without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various modifications may be made to the details. However, the present invention should not be construed as being limited to the description of the following embodiment.
[0017] The present invention can be applied to any device using transistors, such as integrated circuits, RF tags, and semiconductor display devices. The category includes all semiconductor devices. Control circuit, DSP (Digital Signal Processor), Microcomputer Large Scale Integrated Circuit (LSI), including the t), FPGA (Field Programmable Gate Array) and C Programmable logic circuits such as PLD (Complex PLD) The category includes semiconductor devices such as ammable logic devices. The display device uses light-emitting elements such as liquid crystal displays and organic light-emitting diodes (OLEDs) for each pixel. Equipped with light-emitting device, electronic paper, DMD (Digital Micromirror D device), PDP (Plasma Display Panel), FED (Fie LD Emission Display, etc., which have transistors in the drive circuit Semiconductor display devices are included in this category.
[0018] (Embodiment 1) FIG. 1 illustrates a structure of a transistor in a semiconductor device according to one embodiment of the present invention. ) is an example of a cross-sectional view of the transistor in the channel length direction.
[0019] The transistor shown in FIG. 1A has a first conductive film 101 and a first conductive film 102 on an insulating surface. A semiconductor film 103 on the first conductive film 101 and the first conductive film 102, and a semiconductor film 103 on the first conductive film 101 and and a second conductive film 104 and a second conductive film 105 connected to the first conductive film 102, respectively. , an insulating film 106 on the semiconductor film 103, and a second conductive film 10 A third conductive film is provided between the second conductive film 105 and the semiconductor film 103. and a membrane 107.
[0020] What are the first conductive film 101 and the second conductive film 104, and the first conductive film 102 and the second conductive film 105? The third conductive film 107 functions as a gate electrode. It works.
[0021] The semiconductor film 103 does not completely cover the first conductive film 101 and the first conductive film 102. The first conductive film 101 and the second conductive film 102 are partially covered with the first conductive film 101 and the second conductive film 102. The portions of the film 101 and the first conductive film 102 that are not covered by the semiconductor film 103 are all That is, in the portion other than the portion overlapping with the semiconductor film 103, the first conductive film 101 and The first conductive film 102 is connected to the second conductive film 104 and the second conductive film 105. There are.
[0022] The first conductive film 101 and the first conductive film 102, and the second conductive film 104 and the second conductive film 10 The connection between the first conductive film 101 and the second conductive film 104 or the first conductive film 105 is not necessarily the same as the connection between the first conductive film 101 and the second conductive film 104. This does not mean that the second conductive film 102 and the second conductive film 105 are in direct contact with each other. An insulating film such as a native oxide film having a thickness small enough to ensure an electrical connection is formed on the first conductor. Between the conductive film 101 and the second conductive film 104, or between the first conductive film 102 and the second conductive film 105 It may be provided in.
[0023] In one embodiment of the present invention, the end 107 of the third conductive film 107 on the semiconductor film 103 A second conductive film 104 and a second conductive film 105 are provided on either side of the insulating film e. That is, the second conductive film 104, the second conductive film 105, and the third conductive film 107 are semiconductor It does not overlap on the membrane 103 .
[0024] In addition, in the channel length direction, the end 104e of the second conductive film 104 and the end 104f of the second conductive film 105 Between the ends 105e, an end 101e of the first conductive film 101 located under the semiconductor film 103; and an end 102e of the first conductive film 102 are located. 102e is the end of the first conductive film 101 located at the closest position in the channel length direction. and the end of the first conductive film 102. The distance Lsd between the end 104e of the first conductive film 104 and the end 105e of the second conductive film 105 is 1 and an end 102e of the first conductive film 102.
[0025] In one embodiment of the present invention, the first conductive film 101 and A semiconductor film 1 is disposed between the first conductive film 102 and a third conductive film 107 functioning as a gate electrode. Therefore, the third conductive film 107 and the semiconductor film 103 are located in the insulating film 106. Unlike the case where the first conductive film 101 and the first conductive film 102 are provided between the transistors, Even if the distance Lc becomes shorter due to miniaturization of the stanchion, the electric field imparted from the third conductive film 107 to the semiconductor film 103 The electric field obtained is unlikely to be hindered by the first conductive film 101 and the first conductive film 102. Therefore, even if the transistor is miniaturized, a high on-current can be obtained.
[0026] In addition, at the end 101e of the first conductive film 101 and the end 102e of the first conductive film 102, In order to increase the step coverage of the semiconductor film 103, the first conductive film 101 and the first conductive film Even if the thickness of the first conductive film 101 and the second conductive film 102 is kept small, The conductive film 104 and the second conductive film 105 are connected to each other, so that the first conductive film 101 and The source electrode is made up of the first conductive film 102, the second conductive film 104 and the second conductive film 105. Therefore, the resistance of the source or drain electrode can be kept low.
[0027] Next, FIG. 1B shows a top view of a transistor having the cross-sectional structure shown in FIG. An example is shown in FIG. 1B. In order to clarify the layout of the transistors, The insulating film 106 is omitted in this top view. The cross-sectional view corresponds to FIG.
[0028] In the top view shown in FIG. 1B, the semiconductor film 103 has an opening 108 and an opening 109. In the opening 108, the first conductive film 101 and the second conductive film 104 are connected. In addition, the first conductive film 102 and the second conductive film 105 are connected in the opening 109. is.
[0029] Next, FIG. 1C shows a top view of a transistor having the cross-sectional structure shown in FIG. Another example is shown in FIG. 1C. However, in order to clarify the layout of the transistors, 1C is a top view in which the insulating film 106 is omitted. The cross-sectional view in this case corresponds to FIG.
[0030] In the top view shown in FIG. 1C, the semiconductor film 103 is separated into three. The space between the semiconductor film 103 corresponds to the opening 108 and the opening 109. In the opening 10, the first conductive film 101 and the second conductive film 104 are connected. In FIG. 9, a first conductive film 102 and a second conductive film 105 are connected.
[0031] In the transistor shown in FIG. 1, the second conductive film 104 or the second conductive film 105 is The conductive film 101 is connected only to the upper portion of the first conductive film 102. However, in one embodiment of the present invention, the second conductive film 104 or the second conductive film 105 is Connected to the upper and end portions of the conductive film 101 or the upper and end portions of the first conductive film 102 is also good.
[0032] FIG. 2 illustrates a structure of a transistor in a semiconductor device according to one embodiment of the present invention. 2B is an example of a cross-sectional view of the transistor shown in FIG. 2B is an example of a top view of a transistor having a cross-sectional structure. In order to clarify the layout of the transistors, a top view is shown in which the insulating film 106 is omitted. Also, the cross-sectional view taken along dashed line B1-B2 in FIG. 2(B) corresponds to FIG. 2(A).
[0033] The transistor shown in FIG. 2 includes a first conductive film 101 and a second conductive film 102 on an insulating surface. A semiconductor film 103 on the first conductive film 101 and the first conductive film 102, and a semiconductor film 103 on the first conductive film 101 and the first conductive film 102 A second conductive film is connected to the conductive film 102 and is located on the semiconductor film 103. The film 104 and the second conductive film 105, the insulating film 106 on the semiconductor film 103, and a third conductive film 107 provided at a position overlapping with the semiconductor film 103.
[0034] In the transistor shown in FIG. 2, the second conductive film 104 and the second conductive film 105 are the first conductive film. The upper part of the conductive film 101 or the upper part of the first conductive film 102, as well as the end part of the first conductive film 101 1 in that it is also connected to the end of the first conductive film 102. Therefore, the first conductive film 101 and the first conductive film 102 are formed on the insulating surface. The area (occupied area) of the region where the transistor is provided is different between the transistor shown in FIG. 1 and the transistor shown in FIG. If the transistor shown in FIG. 2 is the same as the transistor shown in FIG. The area of the portion where the first conductive film 102 and the second conductive film 104 are connected, or the area of the portion where the first conductive film 102 and the second conductive film The area of the portion where the film 105 is connected is secured to be larger than that of the transistor shown in FIG. Therefore, the contact resistance between the first conductive film 101 and the second conductive film 104 or the first The contact resistance between the conductive film 102 and the second conductive film 105 can be reduced.
[0035] In addition, in FIG. 1 and FIG. 2, the second conductive film 104 and the second conductive film 105 are semiconductor films. However, in one embodiment of the present invention, the second conductive film 10 The fourth or second conductive film 105 may be separated from the semiconductor film 103 .
[0036] FIG. 3 illustrates a structure of a transistor in a semiconductor device according to one embodiment of the present invention. 3B is an example of a cross-sectional view of the transistor shown in FIG. 3B is an example of a top view of a transistor having a cross-sectional structure. In order to clarify the layout of the transistors, a top view is shown in which the insulating film 106 is omitted. Also, the cross-sectional view taken along dashed line C1-C2 in FIG. 3(B) corresponds to FIG. 3(A).
[0037] The transistor shown in FIG. 3 includes a first conductive film 101 and a second conductive film 102 on an insulating surface. A semiconductor film 103 on the first conductive film 101 and the first conductive film 102, and a semiconductor film 103 on the first conductive film 101 and the first conductive film 102 The second conductive film 102 is connected to the conductive film 102 and is separated from the semiconductor film 103. a conductive film 104 and a second conductive film 105, an insulating film 106 on the semiconductor film 103, and an insulating film 106 A third conductive film 107 is provided on the semiconductor film 103 at a position overlapping the semiconductor film 103 .
[0038] In the transistor shown in FIG. 3, the second conductive film 104 or the second conductive film 105 is a semiconductor film 10 1 and 2 in that it is separated from 3. The structure is different.
[0039] As shown in FIG. 1 and FIG. 2, the second conductive film 104 and the second conductive film 105 are When the semiconductor film 103 is in contact with the second conductive film 104, as shown in FIG. The semiconductor film 105 is more likely to function as a source electrode or a drain electrode than when it is separated from the semiconductor film 103. The first conductive film 101 and the second conductive film 104 functioning together, and the first conductive film 102 and the second conductive film The contact area between the semiconductor film 105 and the semiconductor film 103 can be made large. Even if the transistor is miniaturized, the second conductive film 104 and the second conductive film 105 are each a semiconductor By making the first conductive film 101 and the second conductive film 104 contact with each other, The contact resistance of the conductive film 103, or the contact resistance between the first conductive film 102 and the second conductive film 105 and the semiconductor film 1 The contact resistance of 03 can be kept small, and a high on-current can be obtained.
[0040] In addition, the transistor of the semiconductor device according to one aspect of the present invention includes a first conductive film 101 or a first A fourth conductive film may be provided under the conductive film 102. 1 illustrates an example of a cross-sectional view of a transistor of a semiconductor device according to the present invention.
[0041] The transistor shown in FIG. 4A has the cross-sectional structure shown in FIG. , a fourth conductive film 110 and a fourth conductive film 111 are added. The transistor shown in FIG. 1A includes a first conductive film 101 and a first conductive film 102, and a first conductive film 1 The semiconductor film 103 on the first conductive film 101 and the first conductive film 102, 2, the second conductive film 104 and the second conductive film 105, which are connected to the semiconductor film 103, and a first insulating film 106 on the first insulating film 106 at a position overlapping the semiconductor film 103. and a third conductive film 107 formed on the first conductive film 1. 101 and the first conductive film 102, respectively. The fourth conductive film 110 and the fourth conductive film 111 are connected to each other. The layer has a second insulating film 120 provided between the first insulating film 1 and the second insulating film 120. Chemical Mechanical Polishin (CMP) g) Alternatively, it is preferable to flatten the surface by etching or the like.
[0042] The fourth conductive film 110 and the fourth conductive film 111 are formed in a first conductive film 101 and a first conductive film 102. The second conductive film 104 and the second conductive film 105 together form a source electrode or a drain electrode of a transistor. Therefore, by providing the fourth conductive film 110 and the fourth conductive film 111, , the first conductive film 101 and the second conductive film 104 functioning as a source electrode or a drain electrode. , and the resistance of the entire fourth conductive film 110, and the resistance of the first conductive film 102, the second conductive film 105, and the fourth conductive film 110. The resistance of the entire conductive film 111 can be kept low.
[0043] The fourth conductive film 110 or the fourth conductive film 111 and the first conductive film 101 or the first conductive film A semiconductor film may be provided between the electrodes 102. 1 illustrates an example of a cross-sectional view of a transistor of a semiconductor device according to an embodiment.
[0044] The transistor shown in FIG. 4B includes a first conductive film 101, a first conductive film 102, and a fourth conductive film. A semiconductor film 112 and a semiconductor film 113 are provided between the film 110 and the fourth conductive film 111, respectively. In this respect, the structure of the transistor in FIG.
[0045] In FIG. 4, a fourth conductive film is provided under the transistor having the cross-sectional structure shown in FIG. However, one embodiment of the present invention is not limited to this configuration. A fourth conductive film is provided under a transistor having a cross-sectional structure shown in FIG. That's fine.
[0046] In the transistors shown in FIGS. 1 to 4, the first conductive film 101 and the first conductive film 102 However, it overlaps with the third conductive film 107 via the semiconductor film 103 and the insulating film 106. In one embodiment of the present invention, the first conductive film 101, the first conductive film 102, and the third conductive film 107 The second conductive film 107 must overlap the first conductive film 107 through the semiconductor film 103 and the insulating film 106. is also good.
[0047] FIG. 5A shows a cross-sectional structure of the transistor shown in FIG. 1A. The distance Lc between the end 101e of the first conductive film 101 and the end 102e of the first conductive film 102 in the channel length direction 5A shows the relationship between the length Lg of the third conductive film 107 and the spacing Lc In the transistor shown in FIG. 5A, the third conductive film 107 is a semiconductor film 103 and the Lov region 114 overlapping the first conductive film 101 with the insulating film 106 sandwiched therebetween. The third conductive film 107 is disposed between the first conductive film 10 and the semiconductor film 103 and the insulating film 106. 2 and Lov region 115 overlapping therewith.
[0048] By providing the Lov region 114 or the Lov region 115, the on-current of the transistor can be increased. It can be done.
[0049] FIG. 5B shows a cross-sectional structure of the transistor shown in FIG. 1A. The distance Lc between the end 101e of the first conductive film 101 and the end 102e of the second conductive film 102, and the channel length 5B shows the relationship between the length Lg of the third conductive film 107 in the direction of the arrow. In FIG. The transistor shown in FIG. 5B has a first conductive film 101 and a first Between the conductive films 102, the third conductive film 107 and the first conductive film 101 do not overlap. region, i.e., a region where the third conductive film 107 and the first conductive film 101 are provided. The transistor shown in FIG. Between the first conductive film 101 and the first conductive film 102, the third conductive film 107 and the first conductive film In the region where the third conductive film 107 and the first conductive film 102 do not overlap, that is, the region where the third conductive film 107 and the first conductive film 102 are provided The Loff region 117 corresponds to a region different from the region where the Loff region is located.
[0050] By providing the Loff region 116 or the Loff region 117, the first conductive film 101 and Since the parasitic capacitance between the first conductive film 102 and the third conductive film 107 is suppressed to a small value, This allows the operation speed of the star to be increased.
[0051] In the transistor of the semiconductor device according to one embodiment of the present invention, the semiconductor film 103 is A wide-gap semiconductor such as an oxide semiconductor can be used for the semiconductor film 103. When a conductor is used, dopants are added to the semiconductor film 103 to form source regions or An impurity region that functions as a drain region may be formed. The dopant may be, for example, helium, argon, xenon, etc. rare gases, and group 15 atoms such as nitrogen, phosphorus, arsenic, and antimony can be used. For example, when nitrogen is used as a dopant, the concentration of nitrogen atoms in the impurity region is 5× 10 19 / cm 3 More than 1×10 22 / cm 3 It is desirable that the following:
[0052] The oxide semiconductor contains at least indium (In) or zinc (Zn). It is preferable that the oxide contains In and Zn. In addition to these, as a stabilizer to reduce the variation in the electrical characteristics of the transistors It is preferable to have gallium (Ga). Also, tin (Sn) is used as a stabilizer. It is preferable that the stabilizer contains hafnium (Hf). It is also preferable to have aluminum (Al) as a stabilizer.
[0053] Other stabilizers include the lanthanides lanthanum (La) and cerium ( Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), hol Ho, Erbium, Thulium, Ytterbium, Ru It may contain one or more of the elements tetraethium (Lu).
[0054] For example, oxide semiconductors include indium oxide, tin oxide, zinc oxide, and oxides of binary metals. In-Zn oxide, Sn-Zn oxide, Al-Zn oxide, Zn-Mg oxide, Oxides, Sn-Mg oxides, In-Mg oxides, In-Ga oxides, ternary metal oxides In-Ga-Zn oxide (also written as IGZO), In-Al-Zn oxide Oxides, In-Sn-Zn oxides, Sn-Ga-Zn oxides, Al-Ga-Zn oxides oxides, Sn-Al-Zn oxides, In-Hf-Zn oxides, In-La-Zn oxides In-Ce-Zn oxides, In-Pr-Zn oxides, In-Nd-Zn oxides , In-Sm-Zn oxide, In-Eu-Zn oxide, In-Gd-Zn oxide, In-Tb-Zn oxide, In-Dy-Zn oxide, In-Ho-Zn oxide, I n-Er-Zn oxide, In-Tm-Zn oxide, In-Yb-Zn oxide, In -Lu-Zn oxides, In-Sn-Ga-Zn oxides, which are oxides of quaternary metals, I n-Hf-Ga-Zn oxide, In-Al-Ga-Zn oxide, In-Sn-Al- Zn-based oxide, In-Sn-Hf-Zn-based oxide, In-Hf-Al-Zn-based oxide are used. The oxide semiconductor may contain silicon.
[0055] For example, In-Ga-Zn oxide means an oxide containing In, Ga, and Zn. The ratio of In, Ga, and Zn is not important. In addition, metal elements other than In, Ga, and Zn In-Ga-Zn oxides have a sufficiently high resistance when no electric field is present, and therefore, Since it is possible to sufficiently reduce the current and the mobility is high, it is suitable for use in semiconductor devices. It is suitable as a semiconductor material.
[0056] For example, In:Ga:Zn=1:1:1 (=1 / 3:1 / 3:1 / 3) or In:G In-Ga-Zn oxide with an atomic ratio of a:Zn=2:2:1 (=2 / 5:2 / 5:1 / 5) The oxides of In:Sn:Zn=1: 1:1(=1 / 3:1 / 3:1 / 3), In:Sn:Zn=2:1:3(=1 / 3:1 / 6:1 / 2) or In:Sn:Zn=2:1:5(=1 / 4:1 / 8:5 / 8) It is advisable to use an In-Sn-Zn oxide having a molecular ratio or an oxide having a composition close to that.
[0057] For example, high mobility can be obtained relatively easily with In-Sn-Zn oxides. Therefore, in the case of In-Ga-Zn oxides, the mobility can be increased by reducing the defect density in the bulk. It can be done.
[0058] In addition, impurities such as moisture and hydrogen, which act as electron donors, are reduced, and the acid The reduced electron vacancies result in a highly purified oxide semiconductor. A de semiconductor is an i-type (intrinsic semiconductor) or is very close to an i-type. Therefore, the off-state current of a transistor including the oxide semiconductor is extremely low. The band gap of the oxide semiconductor is 2 eV or more, preferably 2.5 eV or more. More preferably, the concentration of impurities such as moisture or hydrogen is sufficiently reduced. In addition, an oxide semiconductor film that has been highly purified by reducing oxygen vacancies is used. This allows the off-state current of the transistor to be reduced.
[0059] Specifically, the off-state current of a transistor using a highly purified oxide semiconductor for a semiconductor film is low. For example, when the channel width is 1×10 6 μm Even in a device with a channel length of 10 μm, the voltage between the source and drain electrodes (drain voltage When the applied voltage is in the range of 1V to 10V, the off-state current is measured by a semiconductor parameter analyzer. Below the limit, i.e. 1×10 -13 In this case, the characteristic of A or less can be obtained. The off-state current, which is the off-state current divided by the channel width of the transistor, is 100zA / μ m or less. Also, by connecting the capacitance element and the transistor, A circuit that controls the charge flowing in or out of a capacitor using the transistor is used to In the measurement, a highly purified oxide semiconductor film was formed on the transistor. It is used in the channel formation region, and the charge amount per unit time of the capacitance element is used to calculate the capacitance of the transistor. The off-state current of the transistor was measured. It was found that an even lower off-state current of several tens of yA / μm can be obtained when the Therefore, a transistor in which a highly purified oxide semiconductor film is used for a channel formation region has the following characteristics: The off-state current is significantly lower than that of a transistor using crystalline silicon.
[0060] Unless otherwise specified, in this specification, the off-state current is In this case, the drain electrode is set at a higher potential than the source and gate electrodes. When the potential of the gate electrode is 0 or less with respect to the potential of the source electrode, The off-state current in this specification refers to the current that flows between the drain electrode and the p In a channel type transistor, the drain electrode is lower than the source electrode and the gate electrode. When the potential of the gate electrode is set to a reference potential, the potential of the gate electrode is less than 0. This refers to the current that flows between the source and drain electrodes when the potential is above the threshold.
[0061] For example, the oxide semiconductor film may be formed using In (indium), Ga (gallium), and Zn ( It can be formed by sputtering using a target containing In-Ga- When the Zn-based oxide semiconductor film is formed by a sputtering method, the atomic ratio is preferably In :Ga:Zn=1:1:1, 4:2:3, 3:1:2, 1:1:2, 2:1:3, or A target of In-Ga-Zn oxide with the atomic ratio of 3:1:4 is used. The oxide semiconductor film is formed by using an In-Ga-Zn oxide target having the above structure. Polycrystals or CAAC (C Axis Aligned Crystal) are formed. In addition, the filling rate of the target containing In, Ga, and Zn is 90% or more. 0% or less, preferably 95% or more and less than 100%. Use a target with a high filling rate. As a result, the formed oxide semiconductor film becomes a dense film.
[0062] When an In-Zn oxide material is used as the oxide semiconductor, The atomic ratio of the metal elements is In:Zn=50:1 to 1:2 (converted to a molar ratio of In 2 O 3 ZnO=25:1 to 1:4), preferably In:Zn=20:1 to 1:1 (molar In terms of ratio, 2 O 3 ZnO=10:1 to 1:2), more preferably In:Zn = 1.5:1 to 15:1 (converted to molar ratio of In 2 O 3 :ZnO=3:4~15:2 For example, a target used for forming an oxide semiconductor film made of an In-Zn oxide is When the atomic ratio is In:Zn:O=X:Y:Z, Z>1.5X+Y. The ratio of Zn By keeping the ratio within the above range, it is possible to realize an improvement in mobility.
[0063] The oxide semiconductor film may be in a single crystal, polycrystalline (also referred to as polycrystalline), amorphous, or other state. Take a stance.
[0064] Preferably, the oxide semiconductor film is a CAAC-OS (C Axis Aligned Cr The film is a crystalline oxide semiconductor.
[0065] The CAAC-OS film is neither completely single crystalline nor completely amorphous. is an oxide semiconductor film with a crystalline-amorphous mixed phase structure having crystalline and amorphous parts in the amorphous phase. The crystal part must be small enough to fit within a cube with one side less than 100 nm. In addition, transmission electron microscopes (TEM) In the observation image by a microscope, the amorphous part and the The boundary between the crystal and the crystalline part is not clear. Therefore, the CAAC-OS film does not have any in-boundary defects. The resulting decrease in electron mobility is suppressed.
[0066] The crystal parts in the CAAC-OS film have c-axes that are normal vectors to the surface on which the CAAC-OS film is formed. The triangle is aligned parallel to the normal vector of the ab plane and perpendicular to the ab plane. The metal atoms are arranged in a layered or hexagonal shape when viewed perpendicular to the c-axis. Metal atoms and oxygen atoms are arranged in layers. The orientation of the a and b axes may be different. In this specification, when it is simply described as vertical, it means that The range of 5° to 95° is also included. This also includes the range from 1° to 5°.
[0067] In the CAAC-OS film, the distribution of the crystal parts may not be uniform. In the process of forming the C-OS film, when crystal growth is performed from the surface side of the oxide semiconductor film, The proportion of crystalline parts may be higher near the surface than near the growth surface. By adding impurities to the AC-OS film, the crystalline part becomes amorphous in the impurity-added region. It may also be pawned.
[0068] The c-axis of the crystal part in the CAAC-OS film is the normal vector of the surface on which the CAAC-OS film is formed. The CAAC-OS film shape (the shape of the film on which the film is formed) is Depending on the cross-sectional shape of the surface or the cross-sectional shape of the surface, the directions may differ from each other. The direction of the c-axis of the crystal is the normal vector of the surface on which the CAAC-OS film is formed. The direction of the crystal is parallel to the normal vector of the film or surface. is formed by carrying out a crystallization treatment such as a heat treatment after the film formation.
[0069] The electrical characteristics of transistors using CAAC-OS films change when irradiated with visible or ultraviolet light. Therefore, the transistor has high reliability.
[0070] The CAAC-OS film can be formed, for example, by sputtering a polycrystalline oxide semiconductor target. The sputtering target is used to form a film by sputtering. Upon impact, the crystalline regions in the sputtering target cleave from the ab plane, forming a -b: The particles peel off as plate-like or pellet-like sputtered particles with surfaces parallel to the surface. In this case, the plate-like sputtered particles may be crystalline and may be crystalline. By reaching the plate, a CAAC-OS film can be formed.
[0071] In addition, the following conditions are preferably applied to form the CAAC-OS film.
[0072] By reducing the amount of impurities mixed in during film formation, it is possible to prevent the crystal state from being destroyed by impurities. For example, the concentration of impurities (hydrogen, water, carbon dioxide, nitrogen, etc.) present in the film formation chamber is In addition, the impurity concentration in the deposition gas may be reduced. A deposition gas having a temperature of -80°C or lower, preferably -100°C or lower, is used.
[0073] In addition, by increasing the substrate heating temperature during film formation, the migration of sputtered particles after they reach the substrate is reduced. Specifically, the substrate heating temperature is set to 100° C. or higher and 740° C. or lower, preferably The deposition temperature is set to 200°C or higher and 500°C or lower. When a plate-shaped sputtered particle reaches a substrate, migration occurs on the substrate, The flat surface of the sputtered particle adheres to the substrate.
[0074] In addition, by increasing the oxygen ratio in the deposition gas and optimizing the power, plasma damage during deposition is reduced. The oxygen ratio in the deposition gas is preferably 30% by volume or more, and more preferably 100% by volume or more. The product is %.
[0075] As an example of a sputtering target, an In-Ga-Zn-O compound target is The details are shown below.
[0076] InO X powder, GaO Y Powder and ZnO Z The powders are mixed in a specified number of moles and then pressurized. By heat treatment at a temperature between 1000 and 1500℃, polycrystalline In-Ga -Zn-O compound target, where X, Y and Z are any positive numbers. , the predetermined molar ratio is, for example, InO X powder, GaO Y Powder and ZnO Z Powder, 2 :2:1, 8:4:3, 3:1:1, 1:1:1, 4:2:3 or 3:1:2. The type of powder and the molar ratio of the powder to be mixed depend on the sputtering target to be prepared. The setting can be changed as appropriate depending on the kit.
[0077] (Embodiment 2) The semiconductor device according to one embodiment of the present invention may have a stacked structure of transistors. In particular, a transistor having the structure shown in FIG. The fourth conductive film 111 is used as a gate electrode, a source electrode, or a drain electrode of a transistor in a lower layer. By making it function as a contact electrode, the increase in element area caused by the contact region is suppressed. To realize miniaturization of semiconductor devices or to realize a reduction in the number of manufacturing steps of transistors. can be done.
[0078] In this embodiment, a memory device, which is one of the semiconductor devices, is taken as an example. The present invention has a structure in which another transistor is provided below a transistor having a structure. A method for manufacturing a semiconductor device according to one embodiment will be described.
[0079] First, before describing a manufacturing method, a configuration of a memory cell included in a memory device will be described. .
[0080] FIG. 9A shows a circuit diagram of a memory cell. The memory cell shown in FIG. The gate of the transistor 202 is connected to the gate of the capacitor 203. The source electrode of the transistor 202 is connected to the first word line WLa. One of the source electrode and the drain electrode is connected to the data line DL, and the other is connected to the transistor 2. The transistor 201 has a source electrode and a drain electrode connected to the gate electrode of the transistor 201. One of the electrodes is connected to the data line DL, and the other is a node to which a predetermined potential is applied. One of a pair of electrodes of the capacitor 203 is connected to the transistor 201. and the other end is connected to a second word line WLb.
[0081] In the memory cell shown in FIG. 9A, the transistor 202 is turned on when data is written. The potential of a signal including data is input from the data line DL to the transistor 202. The potential of the signal is applied to the gate electrode of the transistor 201. The gate capacitance of 201 and the amount of charge stored in the capacitance element 203 are controlled. Data is written to the transistor 201 and the capacitor element 203 .
[0082] When data is held, the transistor 202 is turned off and the transistor 201 is turned off. The charge stored in the gate capacitance and the capacitor 203 is held. In the case where an oxide semiconductor is used for the semiconductor film, the off-state current of the transistor 202 can be made extremely small. Therefore, the stored charge is less likely to leak, and the transistor 202 It retains data for a longer period of time than semiconductor materials such as silicon. It is possible.
[0083] When reading data, the potential of the second word line WLb is changed. Since the potential difference between the pair of electrodes connected to the second word line WL The change in potential of b is applied to the gate electrode of transistor 201. The threshold voltage of a transistor varies depending on the amount of charge stored in its gate capacitance. The potential of the gate electrode of the transistor 201 is changed. The difference in the amount of accumulated charge can be read from the magnitude of the drain current, and data can be obtained. can be read out.
[0084] Note that the transistor 201 may include an oxide semiconductor in its semiconductor film. Alternatively, the transistor 201 may have a semiconductor film made of silicon or germanium. The semiconductor films of all the transistors in the memory cell may be made of oxide semiconductor. By using a thin film, the process can be simplified. The semiconductor film may be made of a material other than an oxide semiconductor, such as polycrystalline or single-crystalline silicon. By using a semiconductor with high mobility, data can be read from memory cells at high speed. This can be done.
[0085] In this embodiment, silicon is used for the semiconductor film of the lower transistor 201, and The case where an oxide semiconductor is used for the semiconductor film of the transistor 202 will be taken as an example. However, as described above, the lower layer transistor 201 is made of silicon. In addition to silicon, we also manufacture semiconductor materials such as germanium, silicon germanium, and single crystal silicon carbide. For example, a silicon-based transistor may be manufactured by a silicon wafer or the like. Which single crystal semiconductor substrate, silicon thin film produced by SOI method, and vapor phase epitaxy method Alternatively, the lower transistor 2 may be formed using a silicon thin film or the like. Like the transistor in the upper layer, the transistor 01 may be formed using an oxide semiconductor.
[0086] In this embodiment, first, as shown in FIG. 6A, an insulating film 701 and a single layer are formed on a substrate 700. A semiconductor film 702 separated from a crystalline semiconductor substrate is formed.
[0087] There is no particular limitation on the material that can be used for the substrate 700, but at least the material that can be used for subsequent processing should be The substrate 700 must have sufficient heat resistance to withstand heat treatment. Glass substrates manufactured by the fusion method or float method, quartz substrates, semiconductor substrates, ceramic A glass substrate can be used if the temperature of the subsequent heat treatment is high. It is advisable to use a material with a strain point of 730°C or higher.
[0088] In this embodiment mode, the semiconductor film 702 is made of single crystal silicon. A method for manufacturing the transistor 201 will be described below. An example of a method for manufacturing the film 702 will be briefly described. An ion beam consisting of ions accelerated by an electric field is injected into the bond substrate, and the surface of the bond substrate is A brittle layer is formed in a region at a certain depth from the surface, where the crystal structure is disrupted and locally weakened. The depth of the region where the embrittlement layer is formed depends on the acceleration energy of the ion beam and the The incident angle can be adjusted. Then, a bond substrate and an insulating film 701 are formed. The insulating film 701 is sandwiched between the substrate 700 and the insulating film 701. After the bond substrate and the substrate 700 are superimposed, a 1N / cm 2 More than 500N / cm 2 Less than 11N / cm, preferably 11N / cm 2 More than 20N / cm 2 below When pressure is applied, the bond substrate and the insulating film 701 are bonded from that portion. The bonding process begins, and eventually the entire surface is bonded. Then, by heat treatment, The volume of the microvoids in the embrittlement layer increases, and the microvoids merge with each other. As a result, At the embrittlement layer, the single crystal semiconductor film, which is a part of the bond substrate, is separated from the bond substrate. The temperature of the heat treatment is set so as not to exceed the distortion point of the substrate 700. The conductive film is processed into a desired shape by etching or the like to form a semiconductor film 702. This can be done.
[0089] The semiconductor film 702 is doped with boron, aluminum, gallium, or the like in order to control the threshold voltage. Impurity elements that impart p-type conductivity, or elements such as phosphorus and arsenic that impart n-type conductivity An impurity element may be added. The addition of an impurity element for controlling the threshold voltage is performed by patterning. This may be performed on the semiconductor film before it is patterned, or on the semiconductor film 7 formed after patterning. The doping of impurity elements for controlling the threshold voltage may be performed on the BON. Alternatively, the doping of impurity elements may be performed on the substrate to roughly adjust the threshold voltage. To fine-tune the threshold voltage, a bond substrate was used. This is performed on the previous semiconductor film or on the semiconductor film 702 formed by patterning. That's fine.
[0090] In this embodiment mode, an example in which a single crystal semiconductor film is used is described. For example, a multilayer film formed on the insulating film 701 by vapor deposition may be used. A crystalline, microcrystalline, or amorphous semiconductor film may be used, and the semiconductor film may be fused by a known technique. Known crystallization methods include laser crystallization using a laser beam, and a method using a catalyst element. Alternatively, a crystallization method using a catalytic element and a laser crystallization method may be combined. In addition, when a substrate having excellent heat resistance such as quartz is used, In this case, the thermal crystallization method using an electric furnace, the lamp annealing crystallization method using infrared light, and the catalytic element Alternatively, a crystallization method using a high-temperature annealing method at about 950° C. may be used.
[0091] Next, as shown in FIG. 6B, after forming a gate insulating film 703 on the semiconductor film 702, A mask 705 is formed on the gate insulating film 703, and an impurity element that gives conductivity is doped on the semiconductor film By doping a part of 702 , an impurity region 704 is formed.
[0092] The gate insulating film 703 is formed by performing high density plasma treatment, heat treatment, etc. The surface of the 2 can be oxidized or nitrided. For example, rare gases such as He, Ar, Kr, and Xe, oxygen, nitrogen oxide, ammonia, nitrogen, and hydrogen. In this case, the plasma is excited by the introduction of microwaves. This allows the generation of high-density plasma at low electron temperature. Zuma-generated oxygen radicals (which may also contain OH radicals) and nitrogen radicals (NH The surface of the semiconductor film is oxidized or nitrided by a method that may include radicals. An insulating film having a thickness of 1 to 20 nm, preferably 5 to 10 nm, can be formed so as to be in contact with the semiconductor film. For example, nitrous oxide (N 2 O) is diluted 1 to 3 times (flow ratio) with Ar and kept at 10 Pa to 30 A microwave (2.45 GHz) power of 3 kW to 5 kW was applied at a pressure of 10 Pa to the semiconductor film. The surface of 702 is oxidized or nitrided. This treatment reduces the thickness by 1 nm to 10 nm (preferably An insulating film of 2nm to 6nm is then formed. 2 O) and silane (SiH 4 ) The microwave (2.45GHz) of 3kW to 5kW was introduced at a pressure of 10Pa to 30Pa. ) Electric power is applied to form a silicon oxynitride film by vapor phase growth to form a gate insulating film. By combining solid-state reactions and vapor-phase growth reactions, the interface state density is low and the dielectric strength is high. Therefore, a gate insulating film having excellent properties can be formed.
[0093] The oxidation or nitridation of the semiconductor film by the above-mentioned high-density plasma treatment proceeds as a solid-phase reaction. The interface state density between the insulating film 703 and the semiconductor film 702 can be made extremely low. The insulating film formed by directly oxidizing or nitriding the semiconductor film 702 by high-density plasma treatment In addition, when the semiconductor film has crystallinity, it is possible to suppress the variation in the thickness of the insulating film. By using a plasma treatment to oxidize the surface of the semiconductor film through a solid-phase reaction, This prevents oxidation from progressing too quickly at the interface, and provides a gate with good uniformity and low interface state density. The insulating film formed by the high density plasma treatment is then applied to the gate The transistor formed by including the insulating film in part or in whole can suppress the variation in characteristics. can be done.
[0094] In addition, silicon oxide, silicon nitride oxide, and oxide can be formed by using a plasma CVD method or a sputtering method. Silicon nitride, silicon nitride, hafnium oxide, aluminum oxide or tantalum oxide, yttrium oxide Thorium, hafnium silicate (HfSi x O y (x>0, y>0)), nitrogen is added Hafnium Silicate (HfSi x O y (x>0, y>0)), nitrogen-added ha HfAl x O y(x>0, y>0)) etc., in a single layer, The gate insulating film 703 may be formed by stacking.
[0095] In this specification, an oxynitride is a material having a composition in which oxygen is more abundant than nitrogen. Nitrogen oxide is a substance that contains more nitrogen than oxygen. It means substance.
[0096] The thickness of the gate insulating film 703 is, for example, 1 nm or more and 100 nm or less, preferably 10 nm or less. In this embodiment, the thickness can be set to 50 nm or less by using a plasma CVD method. A single layer insulating film containing silicon oxide is used as the gate insulating film 703 .
[0097] Next, after removing the mask 705, as shown in FIG. 6(C), a part of the gate insulating film 703 is The portion is removed, and an opening 706 is formed in the region overlapping the impurity region 704 by etching or the like. After that, a conductive film 707 and a conductive film 708 are formed. 01 and the source or drain electrode of the transistor 202. The conductive film 708 is a source electrode or a drain electrode of the transistor 201, and serves as a source electrode or a drain electrode of the transistor 202.
[0098] The conductive film 707 and the conductive film 708 are formed by forming a conductive film so as to cover the opening 706 and then The conductive film 7 can be formed by processing (patterning) the conductive film into a predetermined shape. The conductive film 708 is in contact with the impurity region 704 at the opening 706. The VD method, sputtering method, vapor deposition method, spin coating method, etc. can be used. The conductive film is made of tantalum (Ta), tungsten (W), titanium (Ti), and molybdenum (Mo). , aluminum (Al), copper (Cu), chromium (Cr), niobium (Nb), etc. An alloy containing the above metal as a main component may be used, or a compound containing the above metal may be used. Alternatively, a multi-layer semiconductor film may be formed by doping a semiconductor film with an impurity element such as phosphorus that provides electrical conductivity. It may be formed using a semiconductor such as crystalline silicon.
[0099] Note that in this embodiment mode, the conductive films 707 and 708 are formed using a single-layer conductive film. However, this embodiment is not limited to this structure. The conductive film 707 and the conductive film 708 are stacked. It may be formed of a plurality of conductive films.
[0100] The combination of two conductive layers is tantalum nitride or tantalum for the first layer and tantalum for the second layer. In addition to the above examples, tungsten nitride and tungsten, nitride can be used. Examples include molybdenum and molybdenum, aluminum and tantalum, and aluminum and titanium. Tungsten and tantalum nitride have high heat resistance, so they can be used in the process after forming the two-layer conductive film. In the process, a heat treatment for the purpose of thermal activation can be performed. As a combination, for example, silicon doped with an impurity element that imparts n-type conductivity and nickel silicide, and silicon and tantalum doped with impurity elements that give n-type conductivity. Alternatively, tungsten silicide or the like can be used.
[0101] In the case of a three-layer structure in which three conductive films are laminated, a molybdenum film, an aluminum film, and a molybdenum film are laminated. It is advisable to employ a laminated film structure.
[0102] In addition, the conductive film 707 and the conductive film 708 may be formed of indium oxide or a mixture of indium oxide and tin oxide. , Indium oxide zinc oxide mixture, Zinc oxide, Zinc aluminum oxide, Zinc aluminum oxide nitride Alternatively, a light-transmitting conductive oxide film such as zinc gallium oxide or zinc gallium oxide may be used. .
[0103] Note that the conductive films 707 and 708 are selectively formed by a droplet discharge method without using a mask. The droplet ejection method is a method of ejecting or spraying droplets containing a predetermined composition from a fine hole. This refers to a method of forming a specific pattern by using a laser, and the inkjet method is included in this category. can be.
[0104] The conductive films 707 and 708 are formed by ICP (Inductively Coupled Plasma) deposition. The etching method is an inductively coupled plasma (ICP) etching method. Switching conditions (power applied to the coil-type electrode layer, power applied to the substrate-side electrode layer) By appropriately adjusting the temperature of the electrode on the substrate side, etc., a desired taper shape can be obtained. The taper shape can be adjusted by changing the angle depending on the shape of the mask. The etching gas can also be chlorine, boron chloride, or silicon chloride. or chlorine-based gases such as carbon tetrachloride, fluorine-based gases such as carbon tetrafluoride, sulfur fluoride, or nitrogen fluoride. Nitrogen-based gas or oxygen can be used as appropriate.
[0105] Next, as shown in FIG. 6D, a conductive film 707 and a conductive film 708 are used as a mask to By adding an impurity element that imparts a conductive property to the semiconductor film 702, a channel overlapping with the conductive film 707 is formed. A pair of impurity regions 709 sandwiching the channel forming region 710 therebetween; The impurity region 711, which is a portion of the pure region 704 to which an impurity element is further added, is formed in the semiconductor film 7 It will be formed at 02.
[0106] In this embodiment, an impurity element (for example, boron) that imparts p-type conductivity is added to the semiconductor film 702. Let us take an example where:
[0107] Next, as shown in FIG. 7(A), the gate insulating film 703, the conductive film 707, and the conductive film 708 are Insulating films 712 and 713 are formed to cover the insulating film 712 and the insulating film 713. 713 is silicon oxide, silicon nitride, silicon nitride oxide, silicon oxynitride, aluminum nitride, nitride An inorganic insulating film such as aluminum oxide can be used. By using a low-k material for the film 713, the overlapping of various electrodes and wiring is possible. This is preferable because it is possible to sufficiently reduce the capacitance caused by the insulating film 712. The insulating film 713 may be a porous insulating film made of the above-mentioned material. Since the dielectric constant is lower than that of a high-density insulating film, the parasitic capacitance caused by electrodes and wiring can be reduced. Further reduction is possible.
[0108] In this embodiment, the insulating film 712 is made of silicon oxynitride, and the insulating film 713 is made of silicon nitride oxide. In this embodiment mode, the conductive film 707 and the conductive film 708 are formed by using the following method. In the illustrated example, an insulating film 712 and an insulating film 713 are formed on the conductive film 7 Only one insulating layer may be formed on the conductive film 707 and the conductive film 708, or a plurality of insulating layers of three or more may be formed. The insulating film may be formed in a laminated manner.
[0109] Next, as shown in FIG. 7B, the insulating film 712 and the insulating film 713 are subjected to CMP or etching. By performing etching or the like, the surfaces of the conductive films 707 and 708 are exposed. , in order to improve the characteristics of the transistor 202 to be formed later, an insulating film 712, an insulating film It is preferable to keep the surface of 713 as flat as possible.
[0110] Through the above steps, the transistor 201 can be formed.
[0111] Next, a method for manufacturing the transistor 202 will be described. First, as shown in FIG. Then, a conductive film 714 and a conductive film 715 are formed over the conductive film 707 or the conductive film 708. The conductive film 714 and the conductive film 715 are connected to a source electrode or a drain electrode of the transistor 202. It functions as such.
[0112] Specifically, the conductive films 714 and 715 are formed by the conductive films 707 and 708 and insulating films. A conductive film is formed by sputtering or vapor deposition so as to cover the insulating film 712 and the insulating film 713. The conductive film can be processed (patterned) into a desired shape. The conductive film 714 and the conductive film 715 are formed by oxidizing the conductive film 714 and the conductive film 715 in a later process. To ensure good step coverage of the semiconductor film 716, its edges are tapered. Specifically, the conductive film 714 and the conductive film 715 are preferably thin. The taper angle at the end of 715 is 20 degrees or more and 80 degrees or less, more preferably 30 degrees or more. The angle is preferably 60 degrees or less. The thickness is 10 nm or more and 300 nm or less, more preferably 100 nm or more and 200 nm or less. It is desirable to do so.
[0113] The conductive films to be the conductive films 714 and 715 may be formed of aluminum, chromium, copper, tantalum, or An element selected from titanium, molybdenum, and tungsten, or a composite material containing the above elements. The metal layer may be a gold layer or an alloy layer made of a combination of the above elements. In addition, the metal layer may be a aluminum layer, a copper layer, etc. Chromium, tantalum, titanium, molybdenum, tungsten, etc. on the underside or on the top of the metal film The metal film may be a laminate of any high melting point metal film. To avoid problems with corrosion, it is recommended to use it in combination with high melting point metal materials. Metal materials include molybdenum, titanium, chromium, tantalum, tungsten, neodymium, Scandium, yttrium, etc. can be used.
[0114] The conductive films to be the conductive films 714 and 715 may have a single-layer structure or a stacked structure of two or more layers. For example, a single layer structure of an aluminum film containing silicon, A two-layer structure in which a titanium film is laminated on top of the titanium film, and an aluminum film is laminated on top of the titanium film. A three-layer structure is also possible, in which a titanium film is formed on top of the first layer. -Al alloy, Cu-Mg-O mixed oxide, Cu-Ca-O mixed oxide, Cu-Mg-Al -O mixed oxide, Mo-Ti alloy, Ti, and Mo have high adhesion to the oxide film. The layers are composed of Cu-Mg-Al alloy, Cu-Mg-O mixed oxide, Cu-Ca-O mixed oxide, and C Conductive film consisting of u-Mg-Al-O mixed oxide, Mo-Ti alloy, Ti, or Mo A conductive film made of Cu with a low resistance value is laminated on the upper layer, and the laminated conductive film is By using the insulating film 714 and the conductive film 715, the insulating film 712 or the insulating film 713 can be an oxide film. In this case, the adhesiveness between the insulating film 712 or the insulating film 713 and the conductive film 714 or the conductive film 715 is low. In addition, the resistance of the conductive film 714 and the conductive film 715 can be reduced. This can be done.
[0115] The conductive films 714 and 715 are formed using a conductive metal oxide. The conductive metal oxide may be indium oxide, tin oxide, zinc oxide, indium oxide, or zinc oxide. Indium tin oxide mixture, indium oxide zinc oxide mixture or the above metal oxide material with silicon It is possible to use a material containing silicon or silicon oxide.
[0116] Next, as shown in FIG. 8A, an oxide semiconductor film 7 The oxide semiconductor film 716 has an opening 717 over the conductive film 714. The oxide semiconductor film 716 has an opening 718 over the conductive film 715. 12 and an oxide semiconductor film formed over the insulating film 713, the conductive film 714, and the conductive film 715. It can be formed by processing into the above shape.
[0117] The thickness of the oxide semiconductor film is 2 nm to 200 nm, preferably 3 nm to 50 nm. The oxide semiconductor film has a thickness of preferably 3 nm to 20 nm. The oxide semiconductor film is formed by sputtering using a rare gas as a target. under a rare gas (e.g. argon) atmosphere, an oxygen atmosphere, or a rare gas (e.g. argon and oxygen) atmosphere It can be formed by sputtering in a mixed atmosphere.
[0118] The oxide semiconductor film may be formed of any of the above-mentioned indium oxide, tin oxide, zinc oxide, and binary gold oxide. In-Zn oxides, Sn-Zn oxides, Al-Zn oxides, Zn -Mg oxide, Sn-Mg oxide, In-Mg oxide, In-Ga oxide, ternary In-Ga-Zn oxide (also written as IGZO), which is an oxide of In-Al -Zn oxide, In-Sn-Zn oxide, Sn-Ga-Zn oxide, Al-Ga- Zn-based oxide, Sn-Al-Zn-based oxide, In-Hf-Zn-based oxide, In-La-Z n-type oxide, In-Ce-Zn-type oxide, In-Pr-Zn-type oxide, In-Nd-Zn In-Sm-Zn oxide, In-Eu-Zn oxide, In-Gd-Zn oxide Oxide, In-Tb-Zn oxide, In-Dy-Zn oxide, In-Ho-Zn oxide oxides, In-Er-Zn oxides, In-Tm-Zn oxides, In-Yb-Zn oxides In-Lu-Zn oxides, In-Sn-Ga-Zn oxides, which are oxides of quaternary metals oxides, In-Hf-Ga-Zn oxides, In-Al-Ga-Zn oxides, In-Sn -Al-Zn oxide, In-Sn-Hf-Zn oxide, In-Hf-Al-Zn oxide The oxide semiconductor may contain silicon.
[0119] In this embodiment, a tantalum containing In (indium), Ga (gallium), and Zn (zinc) is used. A 30 nm thick In-Ga-Zn oxide semiconductor was obtained by sputtering using a Zn-type target. A thin film of a conductor is used as an oxide semiconductor film. , In 2 O 3 :Ga 2 O 3 ZnO=1:1:1 [molar ratio] oxide target was used. Also, In 2 O3 :Ga 2 O 3 :ZnO=1:1:2 [molar ratio] oxide ter A target containing In, Ga, and Zn may be used. The filling rate of the target is 90%. The target with a high filling rate is 95% or more and 100% or less, and preferably 95% or more and less than 100%. By using such a material, the oxide semiconductor film formed becomes a dense film.
[0120] In addition, when an In-Zn oxide is used as the oxide semiconductor, the metal in the target used The atomic ratio of the elements is In:Zn=50:1~1:2 (converted to In 2 O 3 : ZnO=25:1 to 1:4), preferably In:Zn=20:1 to 1:1 (molar ratio) This translates to In 2 O 3 In:ZnO=10:1 to 1:2), more preferably In:Zn=1 5:1 to 1.5:1 (converted to molar ratio: In 2 O 3 :ZnO=15:2~3:4) For example, the target used for forming an In-Zn oxide semiconductor has an atomic ratio of I When n:Zn:O=X:Y:Z, Z>1.5X+Y.
[0121] In addition, the target used for the In-Sn-Zn oxide is The ratio of In:Sn:Zn is 1:2:2, 2:1:3, 1:1:1, or 20:45: An oxide target such as 35 is used.
[0122] In this embodiment, the substrate is held in a processing chamber that is maintained in a reduced pressure state, and residual moisture in the processing chamber is removed. While removing the hydrogen and moisture, a sputtering gas from which hydrogen and moisture have been removed is introduced, and the above target is used. During the deposition, the substrate temperature is set to 100° C. or higher and 600° C. or lower, preferably. The deposition temperature may be 200° C. or more and 400° C. or less. In addition, the concentration of impurities in the oxide semiconductor film can be reduced. To remove residual moisture in the processing chamber, a suction-type vacuum pump is used. For example, a cryopump, an ion pump, a titanium sublimation pump, etc. It is preferable to use a displacement pump as the exhaust means. A cryopump may be used to evacuate the processing chamber. For example, hydrogen atoms, water (H 2 O), etc. (more preferably, a compound containing a carbon atom Since the exhaust gas contains the compound containing the compound, the oxide semiconductor film formed in the treatment chamber is The concentration of impurities can be reduced.
[0123] As an example of the deposition conditions, the distance between the substrate and the target is 100 mm, and the pressure is 0.6 Pa. The conditions were: DC power supply 0.5kW, oxygen (oxygen flow rate 100%) atmosphere. In addition, if a pulsed direct current (DC) power supply is used, dust generated during film formation can be reduced, and the film can be This is preferable since the thickness distribution is also uniform.
[0124] Note that the etching for forming the oxide semiconductor film 716 can be dry etching or wet etching. Dry etching may be used, or both may be used. Gases containing chlorine (chlorine-based gases, e.g., chlorine (Cl 2 ), boron trichloride (BCl 3 ), silicon tetrachloride (SiCl 4 ), carbon tetrachloride (CCl 4) is preferred. Gases containing fluorine (fluorine-based gases, such as carbon tetrafluoride (CF 4 ), sulfur hexafluoride (SF 6 ), Nitrogen trifluoride (NF 3 ), trifluoromethane (CHF 3 ), hydrogen bromide (HBr), Oxygen (O 2 ), and adding rare gases such as helium (He) and argon (Ar) to these gases A gas containing 100% hydrogen can be used.
[0125] As a dry etching method, parallel plate type RIE (Reactive Ion Etch) ing method and ICP (Inductively Coupled Plasma) A method of etching a silicon wafer using a plasma-coupled plasma (PPS) can be used. As shown in the figure, the etching conditions (the amount of power applied to the coil-shaped electrode, the amount of power applied to the electrode on the substrate side) The amount of power, the temperature of the electrode on the substrate, etc. are adjusted appropriately.
[0126] The etching solution used for wet etching is a mixture of phosphoric acid, acetic acid, and nitric acid. In the present embodiment, an organic acid such as phosphoric acid or oxalic acid can be used. (Kanto Chemical Co., Ltd.) is used.
[0127] The resist mask for forming the oxide semiconductor film 716 may be formed by an inkjet method. If the resist mask is formed by the inkjet method, a photomask is not used, Manufacturing costs can be reduced.
[0128] Note that moisture or hydrogen (water) may be contained as an impurity in the oxide semiconductor film formed by sputtering or the like. Water or hydrogen tends to form donor levels. Therefore, in one embodiment of the present invention, In order to reduce impurities such as moisture or hydrogen in the conductor film (dehydration or dehydrogenation), The semiconductor film 716 is etched under a reduced pressure atmosphere, an inert gas atmosphere such as nitrogen or a rare gas, or an oxygen atmosphere. Under nitrogen gas atmosphere or ultra-dry air (CRDS (Cavity Ring Down Laser Spectroscopy) When measured using a dew point meter, the moisture content is 20 ppm or less (-55°C in dew point equivalent). In an atmosphere of air (preferably 1 ppm or less, preferably 10 ppb or less), an oxide semiconductor Film 716 is subjected to a heat treatment.
[0129] By performing heat treatment on the oxide semiconductor film 716, moisture or hydrogen in the oxide semiconductor film 716 is removed. Specifically, the temperature is 250° C. or higher and 750° C. or lower, preferably 400° C. or lower. The heat treatment may be performed at a temperature of 500°C or higher and lower than the distortion point of the substrate. For example, 500°C for 3 minutes or more The heat treatment can be performed for about 6 minutes or less. If the RTA method is used for the heat treatment, dehydration or dehydration can be achieved in a short time. Since siliconization can be performed, processing can be performed at temperatures exceeding the strain point of the glass substrate.
[0130] In this embodiment, an electric furnace, which is one of the heat treatment devices, is used. The material to be treated is heated by heat conduction or heat radiation from a heating element such as a resistance heating element, not limited to an air furnace. A heating device may be provided. For example, a GRTA (Gas Rapid Therm al Anneal) equipment, LRTA (Lamp Rapid Thermal Anneal) equipment, LRTA (Lamp Rapid Thermal Anneal) equipment, Use an RTA (Rapid Thermal Anneal) device such as a LRTA devices can be used with halogen lamps, metal halide lamps, and xenon arc lamps. lamps, carbon arc lamps, high pressure sodium lamps, high pressure mercury lamps, etc. The GRTA device heats the object to be treated by radiating light (electromagnetic waves) emitted from the This equipment uses high-temperature gas to perform heat treatment. The gas can be a rare gas such as argon, or An inert gas such as nitrogen that does not react with the workpiece during heat treatment is used.
[0131] In the heat treatment, nitrogen or rare gas such as helium, neon, or argon is mixed with water or water. It is preferable that the nitrogen or helium introduced into the heat treatment device is not included. The purity of rare gases such as neon and argon is 6N (99.9999%) or more, preferably 7N (99.9999%) or more. N (99.99999%) or more (i.e., impurity concentration is 1 ppm or less, preferably 0.1 ppm pm or less).
[0132] In addition, oxide semiconductors are insensitive to impurities, and the film contains a considerable amount of metal impurities. There is no problem with using sodalite, which is inexpensive and contains a large amount of alkali metals such as sodium. It has been pointed out that ash glass can also be used (Kamiya, Nomura, Hosono, "Amorphous Oxide Semiconductors" "Current status of physical properties and device development," Solid State Physics, September 2009, Vol. 44, pp. 62 1-633.) However, this is not an appropriate indication. Alkali metals form oxide semiconductors. Alkaline earth metals are not constituent elements of oxide semiconductors and are therefore considered impurities. In particular, Na, an alkali metal, is an impurity when it is not an element that is included in the alloy. When the insulating film in contact with the semiconductor film is an oxide, Na diffuses into the insulating film. + It becomes. In addition, Na separates the bonds between the metal and oxygen that constitute the oxide semiconductor in the oxide semiconductor film. As a result, for example, the threshold voltage may shift in the negative direction. The shift leads to degradation of transistor characteristics such as normally on and reduced mobility. In addition, the transistor characteristics may vary. The deterioration and variation in characteristics occur when the hydrogen concentration in the oxide semiconductor film is sufficiently low. Therefore, the hydrogen concentration in the oxide semiconductor film is more pronounced when the hydrogen concentration is 1×10 18 / cm 3 below, Especially 1×10 17 / cm 3 If the concentration of the impurities is less than 100%, it is desirable to reduce the concentration of the impurities. Specifically, the measured value of Na concentration by secondary ion mass spectrometry is 5×10 16 / cm 3 Less than or equal to 1×10 16 / cm 3 More preferably, 1×10 15 / cm 3 Below Similarly, the measured value of Li concentration should be 5×10 15 / cm 3 Hereinafter, preferably 1×10 15 / cm 3 Similarly, the measured value of K concentration should be 5×10 15 / c m 3 Less than or equal to 1×10 15 / cm 3 The following should be used.
[0133] Through the above steps, the hydrogen concentration in the oxide semiconductor film 716 can be reduced and the oxide semiconductor film 716 can be highly purified. This makes it possible to stabilize the oxide semiconductor film. The following heat treatment produces an oxide semiconductor film with extremely low carrier density and a wide band gap. Therefore, a transistor can be manufactured using a large-area substrate. This allows for improved mass production. By using a semiconductor film, it is possible to fabricate a transistor with high voltage resistance and extremely low off-current. It is possible.
[0134] Note that the oxide semiconductor film may be amorphous or may have crystallinity. The oxide semiconductor film having the c-axis orientation (CAAC: C Axis Al Even if the oxide semiconductor contains ZnO, the reliability of the transistor is improved. This is preferable because it has the effect of increasing the
[0135] The oxide semiconductor film composed of CAAC can also be fabricated by a sputtering method. In order to obtain CAAC by sputtering, the oxide semiconductor film must be deposited at the initial stage. The method comprises the steps of: forming a hexagonal crystal by using the hexagonal crystal as a seed; and growing a crystal by using the hexagonal crystal as a seed. To achieve this, it is important to keep the target and substrate apart (for example, For example, about 150 mm to 200 mm), and the substrate heating temperature is set to 100°C to 500°C, preferably 20 The temperature is preferably 0°C to 400°C, and more preferably 250°C to 300°C. In addition, the deposited oxide semiconductor film is heat-treated at a temperature higher than the substrate heating temperature during film formation. This makes it possible to repair microscopic defects in the film and defects at the interface of the stacked layers.
[0136] CAAC-OS(C Axis Aligned Crystalline Oxide Compared to amorphous oxide semiconductors, the GaN-GaN-GaN-GaN-GaN-GaN-GaN-GaN-GaN-GaN-GaN-GaN In other words, when the oxide semiconductor is amorphous, the individual metal atoms form an ordered structure. The coordination number of the metal atom in CAAC-OS is almost constant. This reduces the microscopic oxygen vacancies and allows hydrogen atoms (including hydrogen ions) and alkalis to form. It has the effect of reducing charge transfer and instability due to the release and bonding of lithium metal atoms.
[0137] Therefore, a transistor can be manufactured using an oxide semiconductor film formed of CAAC-OS. After applying light or bias-thermal stress (BT) to the transistor, The amount of change in the threshold voltage of the transistor that occurs can be reduced. It is possible to manufacture a transistor having the above electrical characteristics.
[0138] Next, as shown in FIG. 8B, a conductive film 714 and a conductive film 716 in contact with each other are A conductive film 719 and a conductive film 720 in contact with the conductive film 715 and the oxide semiconductor film 716 are formed. The conductive films 719 and 720 are made of the same material as the conductive films 714 and 715. The laminated structure of the above can be formed by using a similar manufacturing method.
[0139] Note that in the etching for forming the conductive films 719 and 720, an oxide semiconductor The materials and etching conditions are appropriately adjusted so that the film 716 is removed as little as possible. Depending on the etching conditions, the exposed portion of the oxide semiconductor film 716 may be partially etched. As a result of this, a groove (a recess) may be formed.
[0140] In this embodiment mode, a titanium film is used for the conductive film 719 and the conductive film 720. A solution containing ammonium hydroxide and hydrogen peroxide (ammonia hydrogen peroxide) is used to selectively remove the conductive film 719 and The conductive film 720 can be wet-etched. Ammonia was prepared by mixing hydrogen chloride water, 28% ammonia water, and water in a volume ratio of 5:2:2. Use hydrogen peroxide or chlorine (Cl 2 ), boron chloride (BCl 3 ) and other gases are used. The conductive film may then be dry etched.
[0141] In addition, the oxide semiconductor film 716 and the conductive film 71 functioning as a source electrode or a drain electrode Between the insulating film 9 and the conductive film 720, zinc oxide, zinc aluminum oxide, zinc aluminum oxide nitride, Alternatively, a film of a metal oxide having electrical conductivity, such as zinc oxide or zinc gallium oxide, may be provided. For example, in the case of forming a metal oxide film, patterning for forming the metal oxide film, The conductive film 719 and the conductive film 720 are patterned together. By providing the metal oxide film, the oxide semiconductor film 716, the conductive film 719, and the conductive Since the resistance between the conductive film 720 can be reduced, high-speed operation of the transistor can be realized. In addition, by providing a metal oxide film, the withstand voltage of a transistor can be increased. can.
[0142] Next, N 2 O, N 2 Alternatively, plasma treatment using a gas such as Ar may be performed. The plasma treatment removes water and the like attached to the exposed surface of the oxide semiconductor film. Alternatively, a plasma treatment may be performed using a mixed gas of oxygen and argon.
[0143] After the plasma treatment, the conductive film 719 and the conductive film 72 are removed as shown in FIG. A gate insulating film 721 is formed to cover the oxide semiconductor film 716. A conductive film 722 is formed over the gate insulating film 721 so as to overlap with the oxide semiconductor film 716. A conductive film 723 is formed in a portion overlapping with the conductive film 719. It functions as the gate electrode of the gate electrode 202.
[0144] The gate insulating film 721 is formed using the same material and the same layered structure as the gate insulating film 703. Note that the gate insulating film 721 is formed by removing impurities such as moisture and hydrogen as much as possible. It is preferable that the insulating film does not include a single insulating film, and the insulating film may be a single insulating film or may be a laminate of multiple insulating films. When hydrogen is contained in the gate insulating film 721, the hydrogen is absorbed into the oxide semiconductor Hydrogen penetrates into the oxide semiconductor film 716 or extracts oxygen from the oxide semiconductor film 716. The film 716 may become low-resistance (n-type), and a parasitic channel may be formed. Therefore, in order to make the gate insulating film 721 a film that contains as little hydrogen as possible, the film forming method is set to include hydrogen. It is important not to use a material with high barrier properties for the gate insulating film 721. For example, a silicon nitride film, a silicon oxynitride film, or a silicon nitride film may be used as an insulating film having a high barrier property. An aluminum nitride film, an aluminum nitride oxide film, or the like can be used. When using a layered insulating film, a silicon oxide film or a silicon oxynitride film having a low nitrogen content is used. The insulating film is formed closer to the oxide semiconductor film 716 than the insulating film with high barrier property. Then, the conductive film 719, the conductive film 720, and the conductive film 721 are formed with an insulating film having a low nitrogen content therebetween. An insulating film having a high barrier property is formed so as to overlap with the oxide semiconductor film 716. By using a thick insulating film, the oxide semiconductor film 716, the gate insulating film 721, or Impurities such as moisture or hydrogen enter the interface between the oxide semiconductor film 716 and another insulating film or the vicinity thereof. In addition, the ratio of nitrogen to the oxide semiconductor film 716 can be reduced. By forming insulating films such as low-temperature silicon oxide films and silicon oxynitride films, materials with high barrier properties can be used. This can prevent the insulating film from being in direct contact with the oxide semiconductor film 716.
[0145] In this embodiment, a silicon oxide film having a thickness of 200 nm is formed by sputtering. The gate insulating film 7 has a structure in which a silicon nitride film having a thickness of 100 nm is laminated by the method. The substrate temperature during film formation may be set to room temperature or higher and 300° C. or lower. In this case, the temperature is 100°C.
[0146] Note that heat treatment may be performed after the gate insulating film 721 is formed. , ultra-dry air or rare gas (argon, helium, etc.) atmosphere, preferably The temperature is 200°C to 400°C, for example, 250°C to 350°C. The content is 20 ppm or less, preferably 1 ppm or less, and more preferably 10 ppb or less. In this embodiment, for example, heating is performed at 250° C. for 1 hour in a nitrogen atmosphere. Alternatively, before the conductive films 719 and 720 are formed, moisture or hydrogen may be reduced. Similar to the previous heat treatment performed on the oxide semiconductor film to reduce the After the gate insulating film 721 containing oxygen is provided, heat treatment is performed. By this, the oxide semiconductor film 716 is turned into an oxide semiconductor film by the heat treatment. Even if oxygen vacancies occur in the semiconductor film 716, the oxide semiconductor Oxygen is supplied to the oxide semiconductor film 716. In the oxide semiconductor film 716, oxygen vacancies serving as donors are reduced and the stoichiometric composition is The oxide semiconductor film 716 can contain oxygen in an amount exceeding the stoichiometric composition. As a result, the oxide semiconductor film 716 can be made closer to an i-type. This reduces the variation in the electrical characteristics of transistors caused by oxygen deficiency, improving the electrical characteristics. The timing of this heat treatment depends on the shape of the gate insulating film 721. There are no particular limitations as long as it is after formation, and other processes, such as heat treatment during resin film formation, transparent conductive film This process also serves as a heat treatment to reduce the resistance of the oxide semiconductor, making it possible to manufacture the oxide semiconductor without increasing the number of processes. The membrane 716 can be made to approach an i-shape.
[0147] In addition, by performing heat treatment on the oxide semiconductor film 716 in an oxygen atmosphere, the oxide semiconductor In this case, oxygen vacancies serving as donors in the oxide semiconductor film 716 may be reduced by adding oxygen. The temperature of the heat treatment is, for example, 100° C. or higher and lower than 350° C., preferably 150° C. or higher and lower than 250° C. The oxygen gas used in the heat treatment in the oxygen atmosphere contains water, hydrogen, etc. It is preferable that the purity of the oxygen gas introduced into the heat treatment device is not more than 6N (9 9.9999%) or more, preferably 7N (99.99999%) or more (i.e., impurities in oxygen It is preferable to keep the concentration of impurities at 1 ppm or less, and preferably at 0.1 ppm or less.
[0148] Alternatively, an oxide semiconductor film 716 may be formed by adding an oxide to the oxide semiconductor film 716 by an ion implantation method, an ion doping method, or the like. The oxygen vacancies acting as donors may be reduced by adding 2.45GH Oxygen plasma generated by microwaves at 1000 nm may be added to the oxide semiconductor film 716 .
[0149] The conductive films 722 and 723 are formed after a conductive film is formed over the gate insulating film 721. The conductive film 722 and the conductive film 72 can be formed by patterning the conductive film. 3 is made of the same material as the conductive films 707 and 708, or the conductive films 714 and 715. It is possible to form the material.
[0150] The thickness of the conductive film 722 and the conductive film 723 is 10 nm to 400 nm, preferably 100 nm. In this embodiment, a sputtering method using a tungsten target is used. After forming a conductive film for a gate electrode of 150 nm, the conductive film is etched to the desired thickness. The conductive films 722 and 723 are formed by processing (patterning) the conductive films 722 and 723 into the above shapes. The resist mask may be formed by an ink-jet method. When the film is formed by the jet method, a photomask is not used, and therefore the manufacturing cost can be reduced.
[0151] Through the above steps, the transistor 202 is formed.
[0152] Note that the conductive film 719 and the conductive film 723 overlap with each other with the gate insulating film 721 therebetween. It corresponds to the capacitive element 203 .
[0153] In addition, the transistor 202 has been described as having a single gate structure. If necessary, a channel forming region can be formed by electrically connecting a plurality of gate electrodes. A transistor having a multi-gate structure can also be formed.
[0154] Note that the insulating film in contact with the oxide semiconductor film 716 (the gate insulating film 7 21 corresponds to the above.) may be made of an insulating material containing a group 13 element and oxygen. Many oxide semiconductor materials contain Group 13 elements, and insulating materials containing Group 13 elements are It has good compatibility with oxide semiconductors, and by using it for the insulating film in contact with the oxide semiconductor film, Therefore, the state of the interface with the nitride semiconductor film can be kept good.
[0155] An insulating material containing a Group 13 element means that the insulating material contains one or more Group 13 elements. Examples of insulating materials containing Group 13 elements include gallium oxide and aluminum oxide. gallium oxide, aluminum gallium oxide, and gallium aluminum oxide. Aluminum gallium is a metal whose aluminum content (atomic percent) is higher than its gallium content (atomic percent). %), and gallium aluminum oxide is a material with a high gallium content (atomic %). This indicates an aluminum content (atomic percent) or higher.
[0156] The insulating film in contact with the oxide semiconductor film 716 is subjected to heat treatment in an oxygen atmosphere or oxygen doping. It is preferable to make the insulating material have more oxygen than the stoichiometric composition by using a gas such as a gas pump. The elemental doping may be performed by using an ion implantation method or an ion doping method.
[0157] By performing oxygen doping treatment, an insulating film having a region with more oxygen than the stoichiometric composition is formed. When the insulating film having such a region is in contact with the oxide semiconductor film, As a result, excess oxygen in the insulating film is supplied to the oxide semiconductor film, and the oxygen in the oxide semiconductor film or the oxide The oxygen defects at the interface between the oxide semiconductor film and the insulating film are reduced, and the oxide semiconductor film is made i-type or It is possible to get as close as possible to the
[0158] FIG. 9B shows another circuit diagram of a memory cell included in a semiconductor device according to one embodiment of the present invention. The figure is shown.
[0159] The memory cell shown in FIG. 9B includes a transistor 204 and a capacitor 205. The gate electrode of the transistor 204 is connected to the word line WL. 204 has one of a source electrode and a drain electrode connected to a data line DL, and the other One electrode of the capacitance element 205 is connected to the ground potential. The input terminal is connected to a node to which a fixed potential, such as a potential Vout, is applied.
[0160] In the memory cell shown in FIG. 9B, the transistor 204 is turned on when data is written. The potential of a signal including data is applied from the data line DL to the capacitor element 204 via the transistor 204. The potential of the signal is applied to one electrode of the capacitor 205. Data is written to the capacitor 205 by controlling the amount of accumulated charge. can be.
[0161] Next, when data is held, the transistor 204 is turned off and the capacitor 205 The transistor 204 has the characteristic of having an extremely small off-state current. Therefore, the charge stored in the capacitor 205 is unlikely to leak, and the transistor 20 4. Data is retained for a longer period of time compared to when semiconductor materials such as silicon are used. It is possible to do so.
[0162] When reading data, the transistor 204 is turned on, and a capacitance is applied via the data line DL. The charge stored in the element 205 is extracted. Then, the difference in the amount of charge is read. The data can be read out by
[0163] FIG. 10A illustrates an example of a cross-sectional view of the memory cell illustrated in FIG. 4 is a substrate 750 having an insulating surface, a conductive film 751 and a conductive film 752, and a conductive film 751 and a semiconductor film 753 over the conductive film 752, and a conductive film 751 and a conductive film 752 are connected to each other. The conductive film 754 and the conductive film 755 are formed on the semiconductor film 753, and the insulating film 756 is formed on the semiconductor film 753. A conductive film 757 is provided over the film 756 so as to overlap with the semiconductor film 753. .
[0164] The capacitor 205 is formed by a conductive film 755 on a substrate 750 having an insulating surface and a conductive film 75 5, and a conductive film 755 formed on the insulating film 756 at a position overlapping the conductive film 755. A conductive film 758 is also provided.
[0165] Note that in the semiconductor device according to one embodiment of the present invention, a memory cell is provided below the memory cell. FIG. 10B shows a memory cell and a driver circuit. 1 illustrates an example cross-sectional view of a layered memory device.
[0166] In the memory device shown in FIG. 10B, a transistor 206 included in a driver circuit is A semiconductor film 761, an insulating film 762 on the semiconductor film 761, and an insulating A conductive film 763 provided over the film 762 in a position overlapping with the semiconductor film 761; The conductive film 764 and the conductive film 765 are connected to the semiconductor film 761. The insulating film 761, the insulating film 762, and the conductive film 763 are covered with an insulating film 766. The semiconductor film 761 is connected to the conductive film 764 and the insulating film 766 through an opening provided in the insulating film 766. It is connected to the conductive film 765.
[0167] In addition, the transistor 204 includes a conductive film 780 and a conductive insulating film 766 over the conductive film 764 and the insulating film 766. The conductive film 780 includes a conductive film 781 and an insulating film 782 provided between the conductive film 780 and the conductive film 781. The conductive film 764 is connected to the conductive film 781. 80, a conductive film 781, and an insulating film 782. A conductive film 771 and a conductive film 772 are connected to the conductive film 781, respectively. A semiconductor film 773 on the conductive film 772 and a semiconductor film 774 connected to the conductive film 771 and the conductive film 772 are The conductive films 774 and 775 are formed by stacking the semiconductor film 773, the conductive film 774, and the conductive film 775. The insulating film 776 is provided at a position overlapping with the semiconductor film 773. and a conductive film 777.
[0168] The capacitor 205 includes a conductive film 775, an insulating film 776 over the conductive film 775, and a and a conductive film 783 located over the conductive film 775 in the semiconductor device.
[0169] This embodiment mode can be implemented in appropriate combination with any of the above embodiment modes.
[0170] (Embodiment 3) A configuration example of an inverter, which is one of the semiconductor devices of one embodiment of the present invention, will be described.
[0171] FIG. 11 shows an example of an inverter according to one embodiment of the present invention. The inverter 50 shown in FIG. 0 includes transistors 501 to 505 and a capacitor 506.
[0172] The transistor 501 has a gate electrode connected to a wiring 508 and a source electrode connected to a transistor The drain electrode of the transistor 502 is connected to the wiring 507. The transistor 502 has a gate electrode connected to a wiring 509 and a source electrode is connected to the wiring 510, and its drain electrode is connected to the source electrode of the transistor 501. The transistor 503 has a gate electrode connected to a wiring 507 and a source One of the electrode and the drain electrode of the transistor 501 is the source electrode of the transistor 502. the drain electrode of the transistor 502 and the other end of the transistor 502 is connected to the gate electrode of the transistor 504. The source electrode of the transistor 504 is connected to the drain electrode of the transistor 505. The transistor 5 is connected to the line 511 and its drain electrode is connected to the wiring 507. 505 has its gate electrode connected to wiring 509 and its source electrode connected to wiring 510. The drain electrode is connected to the source electrode of the transistor 504 and the wiring 511. do.
[0173] One electrode of the capacitor 506 is connected to the gate electrode of the transistor 504. The other electrode is connected to a wiring 511 .
[0174] In the case where the transistor 502 and the transistor 505 are n-channel transistors, specifically, A high-level potential VDD is applied to the wiring 507, and a low-level potential VSS is applied to the wiring 510. A potential CL of a clock signal is applied to the wiring 508, and a potential CL of a clock signal is applied to the wiring 509. A potential Vin is applied to the line 511. A potential Vin that inverts the polarity of the potential Vin is applied to the line 512. The potential Vinb obtained by this is output.
[0175] In the semiconductor device according to one embodiment of the present invention, even if the transistor is miniaturized, the source electrode or It is possible to keep the resistance of the conductive film that functions as the drain electrode low and ensure a high on-current. Therefore, by applying the configuration of the present invention to the inverter 500, the inverter 500 Even if the size is reduced, a high operating speed can be ensured and the current supply capacity can be increased.
[0176] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0177] (Embodiment 4) A semiconductor device according to one aspect of the present invention includes a display device, a personal computer, and a recording medium. Image playback devices with advanced functions (typically DVD: Digital Versatile Disc (Devices having a display capable of playing back recording media such as 3D models and displaying the images) In addition, an electronic device in which the semiconductor device according to one embodiment of the present invention can be used Mobile phones, handheld game consoles, personal digital assistants, e-books, video cameras, digital cameras, etc. Talstill camera, goggle-type display (head-mounted display), navigation audio systems, audio playback devices (car audio, digital audio players, etc.), Copiers, fax machines, printers, printer-combination machines, automated teller machines (AT M), vending machines, etc. Specific examples of these electronic devices are shown in Figure 12.
[0178] FIG. 12A shows a portable game machine, which includes a housing 5001, a housing 5002, a display unit 5003, Display unit 5004, microphone 5005, speaker 5006, operation keys 5007, The semiconductor according to one embodiment of the present invention is used in a driver circuit of a portable game machine. By using the device, it is possible to provide a portable game machine with a high operating speed. By using a semiconductor device according to one embodiment of the present invention, a portable game console can be made smaller. The portable game machine shown in FIG. 12A has two display units 5003 and a display However, the number of displays that the portable game machine has is not limited to this. do not have.
[0179] FIG. 12B shows a display device, which includes a housing 5201, a display portion 5202, a support stand 5203, and the like. By using a semiconductor device according to one embodiment of the present invention for a driver circuit of a display device, the operating speed can be improved. Alternatively, a display device with high display speed can be provided by using a semiconductor device according to one embodiment of the present invention. By using this technology, it is possible to make the display device smaller. This includes all information display devices such as for global computers, TV broadcast reception, and advertisement displays. Can be enjoyed.
[0180] FIG. 12C shows a notebook personal computer, which includes a housing 5401 and a display unit 5402. 5403, a pointing device 5404, etc. By using a semiconductor device according to one embodiment of the present invention for a driver circuit of a mobile computer, the operating speed can be improved. It is possible to provide a notebook type personal computer with high speed. By using the semiconductor device according to the embodiment, the size of a notebook personal computer can be reduced. It is possible.
[0181] FIG. 12D shows a portable information terminal, which includes a first housing 5601, a second housing 5602, a first display unit, and a 5603, a second display unit 5604, a connection unit 5605, and operation keys 5606. The display unit 5603 is provided in the first housing 5601, and the second display unit 5604 is provided in the second housing 5602. The first housing 5601 and the second housing 5602 are connected to each other via a connection portion 5602. 5605, and the angle between the first housing 5601 and the second housing 5602 is The image on the first display unit 5603 can be changed by the connection The switching is performed according to the angle between the first housing 5601 and the second housing 5602 at the portion 5605. In addition, at least the first display unit 5603 and the second display unit 5604 may be configured to display the image. On the other hand, a semiconductor display device having a function as a position input device may be used. The function as a position input device can be realized by providing a touch panel on the semiconductor display device. Alternatively, the function as a position input device can be added to a photo sensor. The light can also be added by providing a photoelectric conversion element having the same characteristics as the light source in a pixel portion of a semiconductor display device. By using a semiconductor device according to one embodiment of the present invention for a driver circuit of a portable information terminal, the operating speed can be improved. Alternatively, a semiconductor device according to one embodiment of the present invention can be provided. By using this, it is possible to realize miniaturization of portable information terminals.
[0182] FIG. 12E shows a mobile phone, which includes a housing 5801, a display portion 5802, an audio input portion 5803, The device has a voice output unit 5804, an operation key 5805, a light receiving unit 5806, etc. By converting the light received in the mobile phone into an electrical signal, it is possible to capture an image from the outside. By using a semiconductor device according to one embodiment of the present invention for a driver circuit of a mobile phone, the operation speed can be increased. A mobile phone can be provided. This makes it possible to reduce the size of mobile phones.
[0183] This embodiment mode can be implemented in appropriate combination with other embodiment modes. [Explanation of symbols]
[0184] 101 Conductive film 101e End 102 Conductive film 102e end 103 Semiconductor Film 104 Conductive film 104e end 105 Conductive film 105e end 106 Insulating film 107 Conductive Film 107e End 108 Opening 109 Opening 110 Conductive film 111 Conductive film 112 Semiconductor film 113 Semiconductor Film 114 Lov area 115 Lov area 116 Loff area 117 Loff area 120 Insulating film 201 Transistor 202 Transistor 203 Capacitive element 204 Transistor 205 Capacitive element 206 Transistor 500 Inverter 501 Transistor 502 Transistor 503 Transistor 504 Transistor 505 Transistor 506 Capacitive element 507 Wiring 508 Wiring 509 Wiring 510 Wiring 511 Wiring 700 Substrates 701 Insulating film 702 Semiconductor film 703 Gate insulating film 704 Impurity region 705 Mask 706 Opening 707 Conductive Film 708 Conductive Film 709 Impurity region 710 Channel formation region 711 Impurity region 712 Insulating film 713 Insulating film 714 Conductive film 715 Conductive Film 716 Oxide Semiconductor Film 717 Opening 718 Opening 719 Conductive Film 720 Conductive Film 721 Gate insulating film 722 Conductive Film 723 Conductive Film 750 Board 751 Conductive Film 752 Conductive film 753 Semiconductor Film 754 Conductive film 755 Conductive Film 756 Insulating film 757 Conductive Film 758 Conductive Film 760 Substrate 761 Semiconductor Film 762 Insulating film 763 Conductive Film 764 Conductive Film 765 Conductive Film 766 Insulating Film 771 Conductive Film 772 Conductive Film 773 Semiconductor Film 774 Conductive Film 775 Conductive Film 776 Insulating Film 777 Conductive Film 780 Conductive Film 781 Conductive Film 782 Insulating Film 783 Conductive Film 5001 Case 5002 Case 5003 Display section 5004 Display section 5005 Microphone 5006 Speaker 5007 Operation key 5008 Stylus 5201 Case 5202 Display section 5203 Support stand 5401 Case 5402 Display section 5403 Keyboard 5404 Pointing Device 5601 Case 5602 Case 5603 Display section 5604 Display section 5605 Connection 5606 Operation key 5801 Case 5802 Display section 5803 Audio input unit 5804 Audio output unit 5805 Operation key 5806 Light receiving section
Claims
1. a first transistor having a channel formation region in a silicon film; a second transistor having a channel formation region in an oxide semiconductor film; A capacitive element; having one of a source and a drain of the second transistor is electrically connected to a gate of the first transistor; the other of the source and the drain of the second transistor is electrically connected to one of the source and the drain of the first transistor; a first electrode of the capacitance element electrically connected to a gate of the first transistor, a first conductive film having a function as a gate of the first transistor and having a region disposed on the silicon film; an insulating film having a region disposed above the silicon film; a second conductive film having a region disposed above the insulating film and a region disposed below the oxide semiconductor film; a third conductive film that functions as a gate of the second transistor and has a region located above the oxide semiconductor film; a fourth conductive film that functions as one of a source and a drain of the second transistor and one of electrodes of the capacitor and has a region located above the oxide semiconductor film; a fifth conductive film which functions as the other of the source and the drain of the second transistor and has a region located above the oxide semiconductor film; a sixth conductive film having a function as the other electrode of the capacitance element and having a region disposed above the fourth conductive film; having the second conductive film overlaps with the third conductive film; the oxide semiconductor film has a first region overlapping with the third conductive film, a second region overlapping with the fourth conductive film, and a third region overlapping with the fifth conductive film; the first region, the second region, and the third region are spaced apart from one another; the second conductive film has a gap and an overlap between the first region and the second region; the sixth conductive film overlaps with the first conductive film; Semiconductor device.
2. a first transistor having a channel formation region in a silicon film; a second transistor having a channel formation region in an oxide semiconductor film; A capacitive element; having one of a source and a drain of the second transistor is electrically connected to a gate of the first transistor; the other of the source and the drain of the second transistor is electrically connected to one of the source and the drain of the first transistor; a first electrode of the capacitance element electrically connected to a gate of the first transistor, a first conductive film having a function as a gate of the first transistor and having a region disposed on the silicon film; an insulating film having a region disposed above the silicon film; a second conductive film having a region disposed above the insulating film and a region disposed below the oxide semiconductor film; a third conductive film that functions as a gate of the second transistor and has a region located above the oxide semiconductor film; a fourth conductive film that functions as one of a source and a drain of the second transistor and one of electrodes of the capacitor and has a region located above the oxide semiconductor film; a fifth conductive film which functions as the other of the source and the drain of the second transistor and has a region located above the oxide semiconductor film; a sixth conductive film having a function as the other electrode of the capacitance element and having a region disposed above the fourth conductive film; having the second conductive film overlaps with the third conductive film; the oxide semiconductor film has a first region overlapping with the third conductive film, a second region overlapping with the fourth conductive film, and a third region overlapping with the fifth conductive film; the first region, the second region, and the third region are spaced apart from one another; the second conductive film has a gap and an overlap between the first region and the second region; a region where the fourth conductive film and the sixth conductive film overlap with each other and has an overlap with the first conductive film; Semiconductor device.
3. a first transistor having a channel formation region in a silicon film; a second transistor having a channel formation region in an oxide semiconductor film; A capacitive element; having one of a source and a drain of the second transistor is electrically connected to a gate of the first transistor; the other of the source and the drain of the second transistor is electrically connected to one of the source and the drain of the first transistor; a first electrode of the capacitance element electrically connected to a gate of the first transistor, a first conductive film having a function as a gate of the first transistor and having a region disposed on the silicon film; an insulating film having a region disposed above the silicon film; a second conductive film having a region disposed above the insulating film and a region disposed below the oxide semiconductor film; a third conductive film that functions as a gate of the second transistor and has a region located above the oxide semiconductor film; a fourth conductive film that functions as one of a source and a drain of the second transistor and one of electrodes of the capacitor and has a region located above the oxide semiconductor film; a fifth conductive film which functions as the other of the source and the drain of the second transistor and has a region located above the oxide semiconductor film; a sixth conductive film having a function as the other electrode of the capacitance element and having a region disposed above the fourth conductive film; having the second conductive film overlaps with the third conductive film; the oxide semiconductor film has a first region overlapping with the third conductive film, a second region overlapping with the fourth conductive film, and a third region overlapping with the fifth conductive film; the first region, the second region, and the third region are spaced apart from one another; the second conductive film has a gap and an overlap between the first region and the second region; the sixth conductive film overlaps with the silicon film; Semiconductor device.
4. In any one of claims 1 to 3, the oxide semiconductor film contains In, Ga, and Zn; Semiconductor device.
5. In any one of claims 1 to 4, the oxide semiconductor film contains indium oxide; Semiconductor device.
6. In any one of claims 1 to 5, the sixth conductive film contains any one of Ta, W, Ti, Mo, Al, Cu, Cr, and Nb; Semiconductor device.
Citation Information
Patent Citations
Semiconductor device and manufacturing method therefor
JP2008270773A
Method for manufacturing transistor
JP2010166030A
Semiconductor device
JP2011151377A
Semiconductor device and method for manufacturing semiconductor device
JP2011181906A
Semiconductor device and driving method therefor
JP2011187940A