Hydraulic composition

The hydraulic composition with specific cement and aggregate ratios enhances fluidity and prevents material separation in medium-flow concrete, addressing cost and quality control issues in high-flow concrete and medium-flow concrete separation challenges.

JP2024153973APending Publication Date: 2024-10-30TOKUYAMA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023067521
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30

AI Technical Summary

Technical Problem

High-flow concrete requires large amounts of cement and admixtures, increasing costs and complicating quality control, while medium-flow concrete is prone to material separation due to prolonged compaction times and high water-to-powder ratios.

Method used

A hydraulic composition comprising Portland cement clinker, fly ash, gypsum, a high-performance AE water reducer, coarse and fine aggregates, and water, with a fine aggregate ratio of 55 to 60%, maintains fluidity and prevents material separation by adjusting the cement composition and aggregate ratios.

Benefits of technology

The composition achieves material separation resistance without lowering fluidity, ensuring stable performance during compaction times of up to 10 seconds, even for medium-flow concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153973000001
    Figure 2024153973000001
  • Figure 2024153973000002
    Figure 2024153973000002
  • Figure 2024153973000003
    Figure 2024153973000003
Patent Text Reader

Abstract

To provide a medium-flow concrete having improved resistance to material separation without lowering a water-powder ratio, while maintaining the same flowability as a medium-flow concrete made by using only normal Portland cement.SOLUTION: A hydraulic composition comprises: a binder (a total amount of the binder is 100 pts.mass) comprising 57 to 94 pts.mass of Portland cement clinker, 5 to 40 pts.mass of fly ash, and 1 to 3 pts.mass of gypsum; a high-performance AE water-reducing agent containing a thickening agent; coarse aggregate; fine aggregate; and water, wherein the ratio of the fine aggregate to the aggregate is 55 to 60%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydraulic composition, and more particularly to a hydraulic composition that has fluidity while also having resistance to material separation, and is unlikely to cause material separation due to compaction. [Background technology]

[0002] In recent years, there have been an increasing number of cases in which it is difficult to fill concrete into formwork due to factors such as the more complex shapes of components and the increased amount of rebar used. In addition, the current situation is one in which workability is inevitably declining due to a decrease in the number of workers and engineers.

[0003] To address these issues, high-fluidity concrete, which does not require compaction, has been developed and used. However, this high-fluidity concrete inevitably increases costs because it requires the use of large amounts of powders such as cement and admixtures such as high-performance air-entraining water-reducing agents during production, and it also has problems such as complicated quality control due to its nature.

[0004] In order to solve the above problems in construction work and the problems with high-fluidity concrete, the use of "high-fluidity concrete requiring compaction (hereinafter referred to as medium-fluidity concrete)," which has higher fluidity than regular concrete but requires compaction during construction, is gradually being promoted. For example, several cases of its application to tunnel lining concrete have been reported (for example, see Non-Patent Document 1). [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Kazuhiko Suwazono and 3 others, "Construction of tunnel lining using thickener-based medium flow concrete - South Kyushu Westbound Expressway Tsunagi Tunnel (provisional name)", Concrete Engineering, April 2012, Vol. 50, No. 4, pp. 366-371(368) Summary of the Invention [Problem to be solved by the invention]

[0006] Medium-fluidity concrete has the advantage of being highly fluid and can be filled with only a little compaction. However, due to the nature of the need to reduce the amount of cement used, it tends to have a high water-to-powder ratio and a large unit water content, and has the disadvantage that material separation is likely to occur if the compaction time is extended. [Means for solving the problem]

[0007] The present inventors conducted research to solve the above problems, and discovered that by changing the cement used in medium flow concrete to fly ash by internal substitution, by using a high performance air entraining water reducing agent containing a thickening component, and by adjusting the fine aggregate ratio to a predetermined value, it is possible to improve the resistance to material separation while maintaining the fluidity of the concrete without lowering the water-powder ratio, and thus completed the present invention.

[0008] That is, the present invention is a hydraulic composition containing a binder consisting of 57-94 parts by mass of Portland cement clinker, 5-40 parts by mass of fly ash and 1-3 parts by mass of gypsum (total amount of binder is taken as 100 parts by mass), a high performance AE water reducing agent containing a thickening component, coarse aggregate, fine aggregate and water, characterized in that the fine aggregate ratio is 55-60%. In the hydraulic composition of the present invention, it is preferable that the slump flow value is 40-50 cm and the air content is 3.0-6.0%. Effect of the Invention

[0009] The hydraulic composition of the present invention makes it possible to provide medium-fluidity concrete that has improved resistance to segregation without lowering the water-powder ratio while maintaining the same fluidity as medium-fluidity concrete made using only ordinary Portland cement, and that does not experience segregation even at a compaction time of 10 seconds, which is a time when segregation can occur in normal medium-fluidity concrete. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The binder used in the hydraulic composition of the present invention comprises Portland cement clinker, fly ash and gypsum.

[0011] There are no particular limitations on the Portland cement clinker, so long as it is a clinker used in the manufacture of ordinary Portland cement according to the JIS standard. In general, the mineral composition as shown by the Bogue formula is approximately 50-67% C3S, 12-20% C2S, 7-15% C3A, and 7-15% C4AF.

[0012] The fineness of the Portland cement clinker may be in the range of general use, and is generally in the range of 3000 to 4500 cm 2 The fineness of the powder may be adjusted by adding gypsum.

[0013] There is no particular limitation on the method for producing Portland cement clinker, and it can be easily obtained by preparing and mixing known cement (clinker) raw materials in a predetermined ratio so as to obtain the desired mineral ratio and coefficient, and burning it by a known method (for example, an SP kiln or an NSP kiln, etc.).

[0014] The method for preparing and mixing the cement raw materials may be any known method as appropriate. For example, the compositions of waste materials, by-products, and other raw materials (CaO sources such as limestone, quicklime, and slaked lime, SiO2 sources such as silica stone, Al2O3 sources such as clay, Fe2O3 sources such as iron, etc.) may be measured in advance, and the mixing ratio of each raw material may be calculated so as to fall within the above range from the ratio of each component in these raw materials, and the raw materials may be mixed in that ratio.

[0015] The raw materials used in the production of Portland cement clinker are the same as those used in the conventional production of Portland cement clinker, and are not particularly limited. Of course, waste materials, by-products, etc. can also be used.

[0016] In the manufacture of Portland cement clinker, it is preferable to use one or more of waste materials, by-products, etc., from the viewpoint of promoting the effective use of waste materials, by-products, etc. Specific examples of waste materials and by-products that can be used include blast furnace slag, steel slag, non-ferrous slag, coal ash, sewage sludge, water purification sludge, paper sludge, construction waste soil, foundry sand, soot and dust, incineration fly ash, molten fly ash, chlorine bypass dust, wood chips, waste clay, slag, waste tires, shells, urban waste and its incineration fly ash, etc. (Note that some of these can be used as a cement raw material as well as a thermal energy source).

[0017] The binder used in the hydraulic composition of the present invention contains fly ash and gypsum as essential components in addition to the above-mentioned Portland cement clinker.

[0018] As the fly ash, any fly ash known as a cement admixture can be used. Specifically, any fly ash conforming to JIS A 6201 "Fly ash for concrete" can be used without any restrictions. The fineness of the fly ash may be within the range of general use, and is generally within the range of 2500 to 5000 cm 2 It is preferable that the molecular weight is adjusted to 1 / g.

[0019] Regarding gypsum, any known gypsum may be used as a raw material for cement production, such as gypsum dihydrate, gypsum hemihydrate, anhydrous gypsum, etc., without any particular limitation. Specific examples include by-product gypsum dihydrate such as flue gas desulfurized gypsum and phosphate gypsum, natural gypsum dihydrate, gypsum hemihydrate, and type II anhydrous gypsum.

[0020] The binder used in the hydraulic composition of the present invention is composed of 57-94 parts by mass of Portland cement clinker, 5-40 parts by mass of fly ash, and 1-3 parts by mass of gypsum (total amount of binder is 100 parts by mass). Outside this range, fluidity decreases and abnormal setting occurs. The range of 67-89 parts by mass of Portland cement clinker, 10-30 parts by mass of fly ash, and 1-3 parts by mass of gypsum is preferable.

[0021] Regarding the grinding method for adjusting the fineness of Portland cement clinker, fly ash and gypsum constituting the binder used in the hydraulic composition of the present invention, any known technique can be used without particular limitation, and each component may be ground separately and then mixed, or may be ground after mixing. As the grinding machine, a ball mill, a vertical mill, etc. can be used. It can also be produced by mixing Portland cement and fly ash that have been produced separately.

[0022] Here, each of the binder materials used in the present invention may be used alone, or a combination of Portland cement (a mixture of Portland cement clinker and gypsum) and fly ash may be used, or fly ash cement (a mixture of Portland cement and fly ash) may be used.

[0023] The hydraulic composition of the present invention contains, in addition to the binder, a high-range air-entraining water-reducing agent containing a thickening component, coarse aggregate, fine aggregate and water.

[0024] The thickening component-containing high-range AE water-reducing agent is a substance that is mainly composed of a polycarboxylic acid-based compound containing a thickening component, and can be used if it complies with JIS A 6204 "Chemical admixture for concrete". The addition rate of the thickening component-containing high-range AE water-reducing agent is within the range of the manufacturer's recommended value, but it is preferably 1.0 to 1.5% based on the powder mass. An example of a thickening component-containing high-range AE water-reducing agent is Floric SF500F manufactured by Floric Co., Ltd.

[0025] The coarse aggregate and fine aggregate may be any known material used in general concrete manufacturing without any particular restrictions. Specifically, crushed stone / crushed sand, river gravel, dune sand, sea sand, limestone aggregate, etc. The size of the coarse aggregate is preferably 10 to 25 mm. The amount of coarse aggregate used is 700 to 1000 kg / m 3 It is preferable to use fine aggregate with a coarse aggregate ratio of about 2.4 to 2.8, or a mixture of several types of fine aggregate to achieve a specified coarse aggregate ratio. The amount of fine aggregate used is 900 to 1200 kg / m3 The volume ratio of fine aggregate to the total aggregate, including coarse aggregate and fine aggregate (hereinafter referred to as fine aggregate ratio) is 55-60%. Outside this range, material separation resistance and fluidity decrease. The preferred range of fine aggregate ratio is 56.5-58.5%.

[0026] There are no particular restrictions on the water used in general concrete manufacturing. Specifically, tap water, groundwater, etc., can be used as long as it complies with JIS A 5308 "Ready Mixed Concrete."

[0027] The slump flow value and air content are preferably within the ranges conforming to JIS A 5308 "Ready Mixed Concrete", specifically, the slump flow value is preferably 40-50 cm and the air content is preferably 3.0-6.0%. By setting the values ​​within these ranges, it is possible to improve the material separation resistance while maintaining the fluidity of the concrete, and furthermore, since it conforms to JIS A 5308 "Ready Mixed Concrete", it is possible to provide a highly versatile hydraulic composition.

[0028] The slump flow value and air content are values ​​measured according to JIS A 1150 "Test method for slump flow of concrete" and JIS A 1128 "Test method for air content of fresh concrete by pressure."

[0029] The hydraulic composition of the present invention is classified as normal strength concrete controlled by slump flow in the category of JIS A 5308 "ready mixed concrete", and a slump flow value of 40 to 50 cm generally corresponds to medium fluidity concrete.

[0030] In the present invention, the method for producing a hydraulic composition by kneading (mixing) Portland cement, fly ash, a high-range air-entraining water-reducing agent containing a thickening component, coarse aggregate, fine aggregate, and water can be any conventional method used in a ready-mix concrete plant or a secondary concrete product plant, without any particular restrictions.

[0031] In the present invention, the mixer used for kneading the hydraulic composition may be any mixer generally used for kneading mortar or concrete, without any restrictions.Specific examples of the mixer include a pan mixer, a forced twin-shaft mixer, a tilting mixer, a mortar mixer, and a hand mixer. EXAMPLES

[0032] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0033] Various tests were conducted on medium-fluidity concrete mixed with ordinary Portland cement (NC), fly ash (FA), a high-performance air-entraining water-reducing agent (admixture) containing a thickening component, coarse aggregate, fine aggregate and water, and the fresh properties and resistance to material separation were evaluated.

[0034] (Materials used) NC: Ordinary Portland cement manufactured by Tokuyama Corporation (containing 98 parts by mass of Portland cement clinker and 2 parts by mass of gypsum; density 3.16 g / cm 3 , powder degree 3210cm 2 / g), FA: Eco Powder manufactured by Chugoku Electric Power Co., Inc. (density 2.29 g / cm 3 , powder degree 3410cm 2 / g), Admixture: Floric SF500F manufactured by Floric Co., Ltd. Coarse aggregate: Hard sandstone crushed stone 2010 (surface dry density 2.69 g / cm) from Miyano, Yamaguchi City, Yamaguchi Prefecture 3 ) and 1505 (surface dry density 2.69 g / cm 3 ), Fine aggregate: crushed sand from Kume-Hijiri, Shunan City, Yamaguchi Prefecture (surface dry density 2.62 g / cm 3 , coarse grain ratio 2.83) and dune sand from Onga, Fukuoka Prefecture (surface dry density 2.58 g / cm 3 , coarse grain ratio 1.21) was used.

[0035] The fine aggregate was mixed with crushed sand and dune sand at a ratio of 82.7% and 17.3% so that the coarse aggregate ratio of the composite sand was 2.55. The water to binder ratio (W / B) was set to 50%.

[0036] A 100L capacity pan-type forced mixer (TM-100) manufactured by Pacific Machinery Co., Ltd. was used for mixing. The mixing procedure was as follows: first, the powder, coarse aggregate, and fine aggregate were put into the mixer and mixed for 30 seconds, then the admixture and water were added and mixed for 90 seconds. The target fresh properties of the medium-fluidity concrete were a slump flow value of 45±5cm and an air content of 4.5±1.5%. The mixing ratio of the binder used in each example is shown in Table 1, the level of medium-fluidity concrete in Table 2, and the results of various tests in Table 3.

[0037] The various measurement methods are as follows. (1) Slump measurement: Measured by a method conforming to JIS A 1101. (2) Measurement of slump flow: Measured by a method conforming to JIS A 1150. (3) Measurement of air volume: Measured using a method conforming to JIS A 1128. (4) Measurement of residual coarse aggregate rate: This was measured in accordance with the coarse aggregate settlement test discussed by the Japan Concrete Institute, Concrete Committee 358, Subcommittee on Mix Design and Construction Technology Research for High-Fluidity Concrete Requiring Compaction.

[0038] Specifically, 20 L of concrete is poured into a bucket container with a diameter of 30 cm and a height of 35 cm, and a rod vibrator (D32D, manufactured by Exen Corporation, vibration frequency 200-242 Hz) is inserted into the center of the container, 1 cm from the bottom of the container, and vibrated for a specified time. After that, 2 L of the surface layer of the concrete is sampled and wet screened to wash out the coarse aggregate and measure the ratio of the coarse aggregate mass to the design value. Here, wet screening means that the concrete is washed out using a sieve with sieve openings smaller than the minimum size of the coarse aggregate, and separated into coarse aggregate and other materials. In this test, the greater the degree of material separation, the more the coarse aggregate sinks downward, and the less the amount of washed out coarse aggregate, resulting in a smaller test result. Regarding the vibration time, 10 seconds was set, which is the median of the recommended vibration time of "approximately 5 to 15 seconds" for normal concrete as stated in the Standard Specifications for Concrete and the Standard Specifications for Building Works / Commentary JASS5, and 6 seconds was set for medium-fluidity concrete, since the compaction time can be shorter than that of normal concrete.

[0039] [Table 1]

[0040] [Table 2]

[0041] [Table 3]

[0042] In Reference Example 1, tests were conducted on ordinary concrete with a slump value of 18±1.5cm, which is commonly used in construction work. The coarse aggregate remaining rate was 75.0% when shaken for 10 seconds, which is the compaction time for ordinary concrete.

[0043] In Reference Example 2, tests were conducted on ordinary concrete with a slump value of 12±1.5 cm, which is commonly used in civil engineering works. The coarse aggregate remaining rate was 78.7% when shaken for 10 seconds, which is the compaction time for ordinary concrete.

[0044] In Reference Example 3, tests were conducted on ordinary concrete with a slump value of 12±1.5 cm, which is commonly used in civil engineering works, and which uses binders mixed in the proportions shown in Table 1. The coarse aggregate remaining rate was 84.0% when shaken for 10 seconds, which is the compaction time for ordinary concrete.

[0045] Comparative Examples 1 and 2 are examples of medium fluidity concrete that does not contain fly ash and that uses only ordinary Portland cement, which is an existing technology, and were carried out to demonstrate the effect of the binder of the present invention. Comparative Example 1 is an example of medium fluidity concrete that is designed to satisfy the target slump flow value and target air content, and the slump flow value was 46.8 cm and the air content was 4.5%, satisfying the targets, and the coarse aggregate residual rate was 70.3% at a compaction time of 6 seconds, which was good, but the coarse aggregate residual rate was 51.5% at a compaction time of 10 seconds, which was significantly lower than the value of the Reference Example. Comparative Example 2 is based on Comparative Example 1, and the water amount was increased to 170 kg / m to improve the coarse aggregate residual rate. 3 The coarse aggregate remaining rate was 88.7% at a compaction time of 6 seconds, and 69.9% at a compaction time of 10 seconds, which was an improvement over Comparative Example 1, showing a better coarse aggregate remaining rate; however, the slump flow value decreased to 37.0 cm.

[0046] Comparative Example 3 is an example in which the fine aggregate ratio is outside the range of the present invention, and a binder mixed in the same ratio as in Example 2 is used, and the fine aggregate ratio is set to 60.6%, which is outside the range of the present invention. By setting the fine aggregate ratio to more than 60%, the coarse aggregate residual ratio was 86.9% at a compaction time of 6 seconds, and 68.1% at a compaction time of 10 seconds, but the slump flow value was reduced to 36.3 cm. From the results of the comparative example, it is clear that it is difficult to improve the coarse aggregate residual ratio while ensuring the target slump flow unless the requirements of the present invention are satisfied.

[0047] Examples 1 to 4 show the results when the binders were mixed in the ratios shown in Table 1 and the mixing conditions were as shown in Table 2. It was confirmed that all of Examples 1 to 4 satisfied the target slump flow value and showed a good coarse aggregate residual ratio of 70% or more at a compaction time of 6 seconds and 55% or more at a compaction time of 10 seconds. From this, it can be seen that the present invention is capable of suppressing material separation at 6 seconds, which is an appropriate compaction time for medium fluidity concrete, and also suppressing the degree of material separation at a longer compaction time of 10 seconds, which is an appropriate compaction time for ordinary concrete, compared to Comparative Example 1, which is a normal medium fluidity concrete using only Portland cement.

Claims

1. A hydraulic composition comprising a binder consisting of 57 to 94 parts by mass of Portland cement clinker, 5 to 40 parts by mass of fly ash and 1 to 3 parts by mass of gypsum (total amount of binder being 100 parts by mass), a high-performance air-entraining water-reducing agent containing a thickening component, coarse aggregate, fine aggregate and water, wherein the hydraulic composition has a fine aggregate ratio of 55 to 60%.

2. 2. The hydraulic composition according to claim 1, which has a slump flow value of 40 to 50 cm and an air content of 3.0 to 6.0%.