Die attach film and method for manufacturing semiconductor device
The die attach film with a high-low modulus design addresses the issue of thermal stress-induced peeling by using a high-modulus first layer to stabilize the chip and a low-modulus second layer to accommodate thermal deformation, enhancing bonding reliability.
Patent Information
- Application Number
- JP2023068470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Semiconductor chips are becoming thinner, and when mounted on a support, the stress from thermal deformation causes peeling due to a low elastic modulus of the die attach film, which cannot effectively suppress chip deformation.
A die attach film with a first adhesive layer having a higher storage modulus and a second adhesive layer with a lower storage modulus, where the second adhesive layer is designed to adapt to thermal deformation, reducing stress and suppressing chip deformation during bonding.
The die attach film effectively reduces stress and suppresses deformation of semiconductor chips during bonding, ensuring reliable attachment to the support.
Smart Images

Figure 2024154576000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a die attach film and a method for manufacturing a semiconductor device. [Background technology]
[0002] A die attach film is a film-like adhesive used to fix a semiconductor chip when mounting a semiconductor chip on a support such as a substrate in a semiconductor package, and when mounting semiconductor chips in a stacked manner.
[0003] By using a die attach film to fix the position of the semiconductor chip, it is possible to prevent connection failures caused by misalignment when connecting the support and the semiconductor chip by wire bonding or the like.
[0004] The die attach film generally contains a thermoplastic resin, and the semiconductor chip and the support are bonded by heating the die attach film. When the die attach film is heated, the semiconductor chip and the support are also heated, and due to thermal deformation of these, a stress is applied in a direction in which the semiconductor chip peels off from the support. In order to suppress the peeling of the semiconductor chip from the support due to this stress, it has been proposed to reduce the elastic modulus of the die attach film.
[0005] For example, Patent Document 1 discloses a die attach film made of a curable resin composition containing a curable compound, a curing agent, and polyimide particles. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-82480 A Summary of the Invention [Problem to be solved by the invention]
[0007] Semiconductor chips to be mounted are becoming thinner and thinner, and when mounting a semiconductor chip on a support, if the elastic modulus of the die attach film is small, the stress in the direction in which the semiconductor chip peels off from the support is reduced, but deformation of the semiconductor chip cannot be suppressed.
[0008] The present invention aims to provide a die attach film that can suppress deformation of a semiconductor chip while reducing the stress applied to the semiconductor chip when the semiconductor chip is attached to an adherend by heating, and a method for manufacturing a semiconductor device. [Means for solving the problem]
[0009] In order to achieve the above object, the present invention has the following configuration.
[0010] [1] A die attach film that adheres a semiconductor chip to an adherend by being heated to a predetermined adhesion temperature, comprising a first adhesive layer that is adhered to the semiconductor chip and a second adhesive layer that is adhered to the adherend, wherein the storage modulus of the second adhesive layer at the adhesion temperature is lower than the storage modulus of the first adhesive layer at the adhesion temperature. [2] A die attach film as described in [1], having adhesive properties on the surface of the first adhesive layer. [3] A die attachment sheet comprising the die attachment film described in [1] or [2] and a protective sheet, wherein the protective sheet is attached to the surface of the second adhesive layer by adhesive force, and the peel strength between the protective sheet and the second adhesive layer is lower than the peel strength between the first adhesive layer and the second adhesive layer. [4] A method for manufacturing a semiconductor device, in which a workpiece having a semiconductor chip set on a support with a die attach film sandwiched therebetween is heated to a predetermined bonding temperature to bond the semiconductor chip to the support, wherein the die attach film has a first adhesive layer bonded to the semiconductor chip and a second adhesive layer bonded to the support, and the storage modulus of the second adhesive layer at the bonding temperature is lower than the storage modulus of the first adhesive layer at the bonding temperature. [5] A method for manufacturing a semiconductor device in a workpiece in which a plurality of semiconductor chips are stacked on a support, and a die attach film is sandwiched between the support and the semiconductor chips, and between adjacent semiconductor chips, by heating the die attach film to a predetermined bonding temperature to bond the semiconductor chip to the support, and adjacent semiconductor chips, wherein the die attach film has a first adhesive layer bonded to the semiconductor chip farther from the support, and a second adhesive layer bonded to the support or the semiconductor chip closer to the support, and the storage modulus of the second adhesive layer at the bonding temperature is lower than the storage modulus of the first adhesive layer at the bonding temperature. [6] The method for manufacturing a semiconductor device described in [5], wherein in the workpiece, a portion of the surface of the second adhesive layer of the die attach film sandwiched between two adjacent semiconductor chips is in contact with the semiconductor chip. Effect of the Invention
[0011] According to the present invention, it is possible to provide a die attach film and a method for manufacturing a semiconductor device that can reduce the stress applied to a semiconductor chip and suppress deformation of the semiconductor chip when the semiconductor chip is adhered to an adherend by heating. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic diagram showing an example of the cross-sectional configuration of a die attach film according to one embodiment of the present invention. [Diagram 2] 1 is a schematic diagram showing a configuration of a die attach sheet according to an example of one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing the configuration of a die attach sheet according to another example of one embodiment of the present invention. [Figure 4] 5A to 5C are schematic diagrams illustrating a lamination step in an example of a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Diagram 5] 5A to 5C are schematic diagrams illustrating a dicing step in an example of a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 6] 5A to 5C are schematic diagrams illustrating a pick-up step in an example of a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 7] 5A to 5C are schematic diagrams illustrating a bonding step in an example of a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 8] 5A to 5C are schematic diagrams illustrating a wiring step in an example of a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 9] 11A to 11C are schematic diagrams illustrating a bonding step in a manufacturing method of a semiconductor device according to another example of an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. In the description of the drawings, the same elements are given the same reference numerals, and duplicated explanations are omitted. In addition, the dimensional ratios of the drawings are not limited to the illustrated ratios.
[0014] In the following description, the storage modulus is a value measured by the following method. First, a sample having a width of 4 mm and a length of 20 mm is obtained, in which 12 test pieces (e.g., die attach films) each having a thickness of 25 μm are laminated. For the obtained sample, a dynamic modulus measuring device (manufactured by UBM, product name: E4000HP) is used to determine the relationship between temperature and the storage modulus in the length direction of the sample at a temperature rise rate of 3° C. / min and a frequency of 10 Hz in the range of 20 to 200° C. Based on the relationship obtained here, the storage modulus of the sample at a predetermined temperature is determined.
[0015] <1. Die attach film> [1-1. Composition of the die attach film] 1 is a schematic diagram showing an example of the cross-sectional configuration of a die attach film 10 according to this embodiment. The die attach film 10 according to this embodiment bonds a semiconductor chip and an adherend by being heated to a predetermined bonding temperature. The adherend may be a support such as a substrate. The adherend may also be a semiconductor chip, in which case the die attach film 10 bonds two adjacent semiconductor chips.
[0016] The die attach film 10 according to this embodiment comprises a first adhesive layer 1 that is adhered to a semiconductor chip, and a second adhesive layer 2 that is adhered to an adherend. The storage modulus of the second adhesive layer 2 at the adhesion temperature is lower than the storage modulus of the first adhesive layer 1 at the adhesion temperature.
[0017] The adhesion temperature is the temperature at which adhesion is performed by the die attach film 10. For example, in a configuration in which a thermosetting resin is contained in one or both of the first adhesive layer 1 and the second adhesive layer 2 described later, and adhesion is performed by curing the thermosetting resin, the adhesion temperature is the temperature at which the thermosetting resin is cured. The adhesion temperature may be 120°C. The adhesion temperature may also have a range. For example, the adhesion temperature may be 60°C or higher, 80°C or higher, or 100°C or higher. For example, the adhesion temperature may be 200°C or lower, 160°C or lower, or 140°C or lower.
[0018] (1-1-1. First adhesive layer) The storage modulus G1 of the first adhesive layer 1 at the adhesion temperature is preferably 0.50 MPa or more, more preferably 0.70 MPa or more, and even more preferably 0.90 MPa or more. This is because the rigidity of the first adhesive layer 1 is improved, and deformation of the semiconductor chip is suppressed during the mounting process of the semiconductor chip using the die attach film 10.
[0019] The storage modulus G1 of the first adhesive layer 1 at the adhesion temperature is preferably 10 MPa or less, more preferably 5.0 MPa or less, even more preferably 2.0 MPa or less, and particularly preferably 1.3 MPa or less. This is to suppress an increase in stress on the semiconductor chip by allowing the first adhesive layer 1 to follow the deformation of the semiconductor chip to some extent in the mounting process of the semiconductor chip using the die attach film 10.
[0020] The thickness t1 of the first adhesive layer 1 is not particularly limited, but is preferably 1.0 μm or more, more preferably 2.0 μm or more, and even more preferably 4.0 μm or more, in order to improve the rigidity of the first adhesive layer 1 and suppress deformation of the semiconductor chip during the mounting process of the semiconductor chip using the die attach film 10.
[0021] The thickness t1 of the first adhesive layer 1 is not particularly limited, but is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less. This is to enable the first adhesive layer 1 to follow the deformation of the semiconductor chip to some extent in the mounting process of the semiconductor chip using the die attachment film 10, thereby suppressing an increase in stress applied to the semiconductor chip. This is also to make the die attachment film 10 thinner. The thickness t1 of the first adhesive layer 1 may be 20 μm or less, or may be 10 μm or less.
[0022] It is preferable that the surface of the first adhesive layer 1 (the surface not in contact with the second adhesive layer 2) has adhesiveness. This is because by temporarily fixing the semiconductor chip to the die attach film 10, the workability is improved when placing the semiconductor chip on the adherend.
[0023] (1-1-2. Second adhesive layer) The storage modulus G2 of the second adhesive layer 2 at the bonding temperature may be 0.10 MPa or more, 0.20 MPa or more, 0.30 MPa or more, or 0.40 MPa or more.
[0024] The storage modulus G2 of the second adhesive layer 2 at the adhesion temperature is preferably 1.0 MPa or less, more preferably 0.80 MPa or less, and even more preferably 0.60 MPa or less, in order to suppress an increase in stress applied to the semiconductor chip due to deformation of the second adhesive layer 2 during the mounting process of the semiconductor chip using the die attach film 10.
[0025] The thickness t2 of the second adhesive layer 2 is not particularly limited, but is preferably 1.0 μm or more, more preferably 2.0 μm or more, and even more preferably 4.0 μm or more in order to suppress an increase in stress applied to the semiconductor chip due to deformation of the second adhesive layer 2 during the mounting process of the semiconductor chip using the die attach film 10.
[0026] The thickness t2 of the second adhesive layer 2 is not particularly limited, but is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less, in order to reduce the thickness of the die attachment film 10. The thickness t2 of the second adhesive layer 2 may be 20 μm or less, or may be 10 μm or less.
[0027] It is preferable that the surface of the second adhesive layer 2 (the surface not in contact with the first adhesive layer 1) has adhesiveness, because this can prevent the semiconductor chip from moving on the adherend after it is placed on the adherend until each adhesive layer is cured.
[0028] (1-1-3. Relationship between storage modulus of first adhesive layer and second adhesive layer) The ratio G2 / G1 of the storage modulus G2 at the adhesion temperature of the second adhesive layer 2 to the storage modulus G1 at the adhesion temperature of the first adhesive layer 1 is preferably 0.90 or less, more preferably 0.80 or less, even more preferably 0.70 or less, and particularly preferably 0.60 or less. This is to suppress deformation of the semiconductor chip while suppressing an increase in stress applied to the semiconductor chip during the mounting process of the semiconductor chip using the die attach film 10.
[0029] The above ratio G2 / G1 may be 0.10 or more, 0.20 or more, 0.30 or more, or 0.40 or more.
[0030] (1-1-4. Relationship between the thickness of the first adhesive layer and the second adhesive layer) The ratio t1 / t2 of the thickness t1 of the first adhesive layer 1 to the thickness t2 of the second adhesive layer 2 is preferably 0.40 or more, more preferably 0.60 or more, and even more preferably 0.80 or more, in order to improve the rigidity of the first adhesive layer 1 while suppressing an increase in the thickness of the die attach film 10, and to suppress deformation of the semiconductor chip during the mounting process of the semiconductor chip using the die attach film 10.
[0031] The ratio t1 / t2 of the thickness t1 of the first adhesive layer 1 to the thickness t2 of the second adhesive layer 2 is preferably 1.6 or less, more preferably 1.4 or less, and even more preferably 1.2 or less, in order to suppress an increase in the thickness of the die attachment film 10 while suppressing an increase in the stress applied to the semiconductor chip due to deformation of the second adhesive layer 2 in the mounting process of the semiconductor chip using the die attachment film 10.
[0032] The thickness t1 of the first adhesive layer 1 and the thickness t2 of the second adhesive layer 2 may be the same, ie, t1 / t2 may be 1.0.
[0033] The sum t1+t2 of the thickness t1 of the first adhesive layer 1 and the thickness t2 of the second adhesive layer 2 is preferably 300 μm or less, more preferably 150 μm or less, and even more preferably 50 μm or less, in order to make the die attachment film 10 thinner.
[0034] (1-1-5. Materials of the first adhesive layer and the second adhesive layer) The material of the first adhesive layer 1 and the second adhesive layer 2 is not particularly limited, but preferably contains a thermosetting resin, and more preferably contains 30 mass% or more of a thermosetting resin. An example of the thermosetting resin is, but is not limited to, an epoxy resin. The storage modulus G1 of the first adhesive layer 1 and the storage modulus G2 of the second adhesive layer 2 can be controlled, for example, by the type of functional group of the thermosetting resin and the chemical structure other than the functional group.
[0035] The first adhesive layer 1 and the second adhesive layer 2 may also contain a curing agent for curing the thermosetting resin. When the thermosetting resin in the first adhesive layer 1 and the second adhesive layer 2 contains an epoxy resin, the curing agent may be, for example, a phenolic resin, but is not limited thereto. The storage modulus G1 of the first adhesive layer 1 and the storage modulus G2 of the second adhesive layer 2 can be controlled, for example, by the type of functional group of the curing agent and the chemical structure other than the functional group.
[0036] The first adhesive layer 1 and the second adhesive layer 2 may contain resin components other than the thermosetting resin, inorganic fillers, coupling agents, curing accelerators, etc. The storage modulus G1 of the first adhesive layer 1 and the storage modulus G2 of the second adhesive layer 2 can be controlled by the type and content of the components other than the thermosetting resin and the curing agent.
[0037] <2. Die attach sheet> [2-1. Die attach sheet configuration example 1] 2 is a schematic diagram showing the configuration of a die attachment sheet 100 according to one example of the present embodiment. The die attachment sheet 100 according to this example includes a die attachment film 10 and a protective sheet 3, and the protective sheet 3 is attached by adhesive force to the surface of the second adhesive layer 2 (the surface not in contact with the first adhesive layer 1). It is preferable that the second adhesive layer 2 and the protective sheet 3 are peelable at the interface.
[0038] According to this configuration, in the manufacturing process of the semiconductor device described below, after a semiconductor wafer is attached to the first adhesive layer 1, until a support is attached to the second adhesive layer 2, the second adhesive layer 2 is protected by the protective sheet 3 against adhesion of foreign matter, for example, in a dicing process described below.
[0039] The peel strength between the protective sheet 3 and the second adhesive layer 2 is lower than the peel strength between the first adhesive layer 1 and the second adhesive layer 2. This configuration makes it possible to prevent the first adhesive layer 1 and the second adhesive layer 2 from peeling off when the protective sheet 3 is peeled off from the second adhesive layer 2 in order to attach the second adhesive layer 2 to a support.
[0040] The peel strength between the protective sheet 3 and the second adhesive layer 2 is preferably lower than the peel strength between the first adhesive layer 1 and the semiconductor chip (described later) before bonding. With this configuration, for example, peeling of the die attach film 10 from the semiconductor chip can be suppressed during a pick-up step or the like in a manufacturing method for a semiconductor device described later.
[0041] The protective sheet 3 may be a dicing tape. The material of the protective sheet 3 is, for example, a resin film. Examples of the resin film include plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, and polyimide film. The protective sheet 3 may also be a resin film that has been subjected to a surface treatment such as primer coating, UV treatment, corona discharge treatment, polishing treatment, and etching treatment. The protective sheet 3 preferably has adhesive properties. The protective sheet 3 may be, for example, a resin film provided with adhesive properties, and may be a resin film provided with an adhesive layer on one side thereof.
[0042] [2-2. Die attach sheet configuration example 2] 3 is a schematic diagram showing the configuration of a die attachment sheet 110 according to another example of the present embodiment. The die attachment sheet 110 according to this example includes a die attachment film 10, a first protective sheet 31, and a second protective sheet 32. The first protective sheet 31 is attached to the surface of the first adhesive layer 1 of the die attachment film 10 (the surface not in contact with the second adhesive layer 2) by adhesive force. The second protective sheet 32 is attached to the surface of the second adhesive layer 2 of the die attachment film 10 (the surface not in contact with the first adhesive layer 1) by adhesive force. It is preferable that the first adhesive layer 1 and the first protective sheet 31, and the second adhesive layer 2 and the second protective sheet 32 are interfacially peelable.
[0043] The materials and configurations of the first protective sheet 31 and the second protective sheet 32 may be, for example, but are not limited to, the materials and configurations exemplified in the description of the protective sheet 3. Furthermore, the materials and configurations of the first protective sheet 31 and the second protective sheet 32 may be the same or different.
[0044] According to this configuration, the first adhesive layer 1 is protected by the first protective layer 31 until immediately before the semiconductor wafer is attached to the first adhesive layer 1. Furthermore, according to this configuration, in the manufacturing process of the semiconductor device described below, after the semiconductor wafer is attached to the first adhesive layer 1, until the second adhesive layer 2 is attached to the support, the second adhesive layer 2 is protected by the second protective sheet 32 against adhesion of foreign matter, for example, in a dicing process described below.
[0045] The peel strength between the second protective sheet 32 and the second adhesive layer 2 is lower than the peel strength between the first adhesive layer 1 and the second adhesive layer 2. This configuration makes it possible to prevent the first adhesive layer 1 and the second adhesive layer 2 from peeling off when the second protective sheet 32 is peeled off from the second adhesive layer 2 in order to attach the second adhesive layer 2 to a support.
[0046] Furthermore, in the manufacturing process of a semiconductor device, when a step of attaching a semiconductor wafer to the first adhesive layer 1 is performed before attaching the second adhesive layer 2 to a support, it is preferable that the peel strength between the first protective sheet 31 and the first adhesive layer 1 is lower than the peel strength between the second protective sheet 32 and the second adhesive layer 2. With this configuration, peeling between the second protective sheet 32 and the second adhesive layer 2 can be suppressed when the first protective sheet 31 is peeled off from the first adhesive layer 1 in order to attach the first adhesive layer 1 to the semiconductor wafer.
[0047] Furthermore, when the manufacturing process of the semiconductor device is performed in the above order, it is preferable that the peel strength between first protective sheet 31 and first adhesive layer 1 at the time of peeling them off is lower than the peel strength between second adhesive layer 2 and the semiconductor wafer. With this configuration, peeling between second adhesive layer 2 and the semiconductor wafer can be suppressed when first protective sheet 31 is peeled off from first adhesive layer 1.
[0048] <3. Manufacturing method of die attach film> Examples of the method for producing the die attachment film 10 according to this embodiment will be described below, but the method for producing the die attachment film according to this embodiment is not limited to these examples.
[0049] [3-1. Example 1 of manufacturing method for die attach film] A manufacturing method of the die attachment film 10 according to one example of the present embodiment includes a first adhesive layer forming step of forming a first adhesive layer 1 on a first substrate, a second adhesive layer forming step of forming a second adhesive layer 2 on a second substrate, and a bonding step of bonding the first adhesive layer 1 formed on the first substrate and the second adhesive layer 2 formed on the second substrate. The order of the first adhesive layer forming step and the second adhesive layer forming step is not particularly limited, and the first adhesive layer forming step may be performed first, the second adhesive layer forming step may be performed first, or the first adhesive layer forming step and the second adhesive layer forming step may be performed in parallel.
[0050] The first adhesive layer forming step involves, for example, applying a first adhesive composition to a first substrate and drying the first adhesive composition applied to the first substrate to form a first adhesive layer 1 on the first substrate.
[0051] The first base material may be, for example, the first protective sheet 31 in the die attachment sheet 110 shown in Fig. 3. The material and configuration of the first base material may be, for example, the material and configuration exemplified in the description of the protective sheet 3, but are not limited thereto.
[0052] The first adhesive composition is preferably a varnish. This is because an adhesive layer with uniform components can be formed, and the thickness of the adhesive can be easily controlled. For example, the varnish may have a configuration in which the components contained as the first adhesive layer 1 and the second adhesive layer 2 are dissolved in a solvent. Examples of the solvent include organic solvents, and examples of the organic solvent include, but are not limited to, methyl ethyl ketone and cyclohexanone. Note that the first adhesive composition is not limited to a varnish, and may be a dispersion liquid, etc.
[0053] Examples of methods for applying the first adhesive composition to the first substrate include knife coating, roll coating, spray coating, gravure coating, bar coating, and curtain coating.
[0054] The method for drying the first adhesive composition applied to the first substrate may be, for example, drying by heating. The heating temperature and heating time are preferably adjusted appropriately depending on the components of the first substrate and the first adhesive composition. The heating temperature and heating time are preferably within a range that can suppress a chemical reaction of the components contained in the first adhesive composition.
[0055] The second adhesive layer forming step involves, for example, applying a second adhesive composition to a second substrate and drying the second adhesive composition applied to the second substrate to form a second adhesive layer 2 on the second substrate.
[0056] The operations that may be performed in the second adhesive layer forming step are the same as those in the first adhesive layer forming step. The second adhesive layer forming step may be performed in the same manner as the first adhesive layer forming step, or may be different.
[0057] The second substrate may be, for example, the protective sheet 3 in the die attachment sheet 100 shown in Fig. 2, or the second protective sheet 32 in the die attachment sheet 110 shown in Fig. 3. The material and configuration of the second substrate may be, for example, the material and configuration exemplified in the description of the protective sheet 3, but are not limited thereto.
[0058] The configuration of the second adhesive composition is the same as that of the first adhesive composition, except that it is preferable to determine the configuration of the second adhesive composition so that the storage modulus of the second adhesive layer 2 at the adhesion temperature is lower than the storage modulus of the first adhesive layer 1 at the adhesion temperature.
[0059] In the bonding step, for example, the first adhesive layer 1 formed on the first substrate and the second adhesive layer 2 formed on the second substrate are bonded together so that they are in contact with each other. The bonding is performed using, for example, a roll laminator, a vacuum laminator, or the like. The bonding may be performed in a state in which the first adhesive layer 1 and the second adhesive layer 2 are heated, or may be performed without heating.
[0060] After the bonding step, the first substrate or the second substrate may be peeled off, or both the first substrate and the second substrate may be peeled off. If only the first substrate is peeled off after the bonding step and the second substrate is left as the protective sheet 3, the die attachment sheet 100 shown in Fig. 2 will be obtained. If both the first substrate and the second substrate are left after the bonding step, the die attachment sheet 110 shown in Fig. 3 will be obtained.
[0061] [3-2. Example 2 of manufacturing method for die attach film] A manufacturing method for a die attach film 10 according to another example of this embodiment includes a second adhesive layer formation step of applying a second adhesive composition onto a substrate and drying the applied second adhesive composition to form a second adhesive layer 2, and a first adhesive layer formation step of applying a first adhesive composition onto the second adhesive layer 2 formed on the substrate and drying the applied first adhesive composition to form a first adhesive layer 1.
[0062] The substrate may be, for example, the protective sheet 3 in the die attachment sheet 100 shown in Fig. 2, or the second protective sheet 32 in the die attachment sheet 110 shown in Fig. 3. The material and configuration of the substrate may be, for example, the material and configuration exemplified in the description of the protective sheet 3, but are not limited thereto.
[0063] <4. Manufacturing method of semiconductor device> [4-1. Example 1 of a manufacturing method for a semiconductor device] An example of a method for manufacturing a semiconductor device according to this embodiment will be described with reference to Figs. 4 to 8. In this example of the method for manufacturing a semiconductor device, a die attachment sheet 100 having the form shown in Fig. 2 is used as the die attachment film 10, but is not limited thereto. Among the steps described below, steps other than the bonding step may not be performed if they are unnecessary. Examples of unnecessary steps will be described later.
[0064] (4-1-1. Lamination process) 4 is a schematic diagram illustrating a lamination step in one example of a method for manufacturing a semiconductor device according to this embodiment. In the lamination step, a semiconductor wafer 200 is attached (laminated) to a first adhesive layer 1 of a die attachment film 10 (die attachment sheet 100). The semiconductor wafer 200 may be half-cut in advance to form a groove in the thickness direction. When laminating, pressure may be applied using a roll or the like, and either or both of the die attachment film 10 and the semiconductor wafer 200 may be heated.
[0065] When heating is performed during lamination, the temperature of the die attachment film 10 is preferably 50° C. or higher, more preferably 60° C. or higher, and even more preferably 70° C. or higher. This is because better adhesion can be obtained between the first adhesive layer 1 of the die attachment film 10 and the semiconductor wafer 200. When heating is performed during lamination, the temperature of the die attachment film 10 is preferably 120° C. or lower, more preferably 100° C. or lower, and even more preferably 90° C. or lower. This is because the flow of the first adhesive layer 1 and the second adhesive layer 2 during lamination can be suppressed, and changes in the thickness of the die attachment film 10 can be suppressed.
[0066] (4-1-2. Dicing process) 5 is a schematic diagram illustrating a dicing step in one example of the manufacturing method of the semiconductor device according to the present embodiment. In the dicing step, the semiconductor wafer 200 to which the die attachment film 10 is attached is cut (diced) into a predetermined shape to obtain a semiconductor chip 201. Examples of dicing methods include, but are not limited to, blade dicing using a rotary blade and a method of cutting with a laser. In this example, the protective sheet 3 is not cut in the dicing step. Therefore, when the semiconductor chip 201 is taken out in the following pick-up step, it can be efficiently peeled off from the protective sheet 3 from the die attachment film 10.
[0067] (4-1-3. Pick-up process) 6 is a schematic diagram illustrating a pick-up step in an example of a manufacturing method for a semiconductor device according to this embodiment. In the pick-up step, the semiconductor chip 201 is taken out with the die attach film 10 attached to the semiconductor chip 201. In this example of the manufacturing method, in the pick-up step, the die attach film 10 laminated with the semiconductor chip 201 is peeled off from the protective sheet 3. In this step, the semiconductor chips 201 may be picked up one by one, or multiple semiconductor chips 201 may be picked up at the same time.
[0068] (4-1-4. Adhesion process) 7 is a schematic diagram illustrating a bonding step in one example of the manufacturing method of the semiconductor device according to the present embodiment. In the bonding step, in a work 700 in which a semiconductor chip 201 is set on a support 300 with a die attachment film 10 sandwiched therebetween, the die attachment film 10 is heated to a predetermined bonding temperature to bond the semiconductor chip 201 to the support 300.
[0069] In the manufacturing method according to this example, the semiconductor chip 201 taken out in the pick-up process is set at a predetermined position on the support 300 so that the die attach film 10 attached to the semiconductor chip 201 contacts the support 300, and this is used as the work 700. The die attach film 10 in the work 700 is heated to a predetermined adhesion temperature to adhere the semiconductor chip 201 and the support 300 to each other.
[0070] The support 300 is, for example, a substrate on which an electric circuit 301 is formed on the surface to which the semiconductor chip 201 is attached. The shape of the support 300 in a plan view is not particularly limited, and examples of the shape include a polygon such as a rectangle, a circle, an ellipse, and the like.
[0071] The bonding temperature is a temperature at which the adhesive function of the die attach film 10 is fully exerted. When at least one of the first adhesive layer 1 and the second adhesive layer 2 contains a thermosetting resin, the bonding temperature can be lowered as the bonding time is longer, and needs to be higher as the bonding time is shorter. In addition, pressure may be applied between the semiconductor chip 201 and the support 300 during bonding.
[0072] After bonding, the first adhesive layer 1 becomes a first adhesive layer, and the second adhesive layer 2 becomes a second adhesive layer.
[0073] In the bonding process, after the semiconductor chip 201 is set on the support 300, until the semiconductor chip 201 and the support 300 are bonded to each other, the second adhesive layer 2 may be made adhesive so that the semiconductor chip 201 does not move easily, and the die attach film 10 and the support 300 may be fixed together by adhesive force.
[0074] (4-1-5. Wiring process) 8 is a schematic diagram illustrating a wiring step in an example of a method for manufacturing a semiconductor device according to this embodiment. In the wiring step, for example, wiring 302 is formed to electrically connect an electric circuit 301 formed on a support 300 and a semiconductor chip 201. The wiring 302 is formed by, for example, wire bonding or the like.
[0075] That is, the wiring step provides a configuration including support 300 on which electric circuit 301 is formed, an adhesive layer formed on the surface of support 300 on which electric circuit 301 is formed, semiconductor chip 201 formed on the adhesive layer, and wiring 302 for electrically connecting semiconductor chip 201 and electric circuit 301, the adhesive layer having a first adhesive layer in contact with semiconductor chip 201 and a second adhesive layer in contact with support 300. This configuration shown in FIG. 8 may be used as semiconductor device 800.
[0076] (4-1-6. Other processes, etc.) The example of the manufacturing method of the semiconductor device is not limited to the steps described above. For example, when the die attachment sheet 110 shown in FIG. 3 is used instead of the die attachment sheet 100, a step of peeling the protective sheet 31 from the die attachment sheet 110 may be performed before the lamination step.
[0077] Furthermore, for example, when a die attachment film 10 without a protective sheet is used instead of the die attachment sheet 100, a step of attaching a dicing tape to the first adhesive layer 1 may be carried out between the lamination step and the dicing step.
[0078] Also, for example, if a semiconductor chip of a desired shape is available, the dicing step may not be performed. Also, if a die attach film 10 without a protective sheet is attached to a semiconductor chip of a desired shape in advance, the lamination step, dicing step, and pick-up step may not be performed.
[0079] Also, for example, in the case of shipping a semiconductor device that does not have wiring between the support 300 and the semiconductor chip 201 described later, the wiring process may not be performed. In this case, a semiconductor device is obtained that includes the support 300, an adhesive layer formed on the support 300, and the semiconductor chip 201 formed on the adhesive layer, and the adhesive layer has a first adhesive layer in contact with the semiconductor chip 201 and a second adhesive layer in contact with the support 300, that is, the configuration shown in FIG.
[0080] [4-2. Example 2 of a manufacturing method for a semiconductor device] 9 is a schematic diagram illustrating a bonding step in a method for manufacturing a semiconductor device according to another example of this embodiment. In this configuration, hereinafter, the side closer to the support 300 may be referred to as the lower side, and the side farther from the support 300 may be referred to as the upper side.
[0081] In a work 900 in the manufacturing method of a semiconductor device according to this example, a plurality of semiconductor chips 201(1) to 201(n) (n is an integer of 2 or more, the smaller the n, the closer the semiconductor chip is to the support 300, and so forth) are stacked on a support 300. A die attach film 10 is sandwiched between the support 300 and the semiconductor chip 201(1) and between adjacent semiconductor chips 201(k-1) and 201(k) (k is an integer and 1≦k≦n, the smaller the k, the closer the semiconductor chip is to the support 300, and so forth). In the manufacturing method of a semiconductor device according to this example, the die attach film 10 is heated to a predetermined bonding temperature to bond the semiconductor chip 201 to the support 300 and the adjacent semiconductor chips 201(k-1) and 201(k).
[0082] The portion surrounded by the two-dot chain line and the solid line in Fig. 9 includes one or more configurations having a die attach film 10 on the support 300 side and a semiconductor chip 201(k) thereon. In the example shown in Fig. 9, an electric circuit on the support 300 is not shown, but an electric circuit may be formed on the support 300 as in the examples of Figs. 7 and 8. In the example shown in Fig. 9, n is 4 or more, but n may be 2 or 3. In the following description, when referring to an unspecified semiconductor chip among the semiconductor chips 201(1) to 201(n), it is referred to as the semiconductor chip 201.
[0083] In the die attach film 10 in this example of the method for manufacturing a semiconductor device, the first adhesive layer 1 is adhered to the semiconductor chip 201(k) farther from the support 300, and the second adhesive layer 2 is adhered to the support 300 (when k=1) or the semiconductor chip 201(k-1) (when k≧2) closer to the support 300.
[0084] In the workpiece 900 of this example, a portion of the surface of the second adhesive layer 2 of the die attach film 10 sandwiched between two adjacent semiconductor chips 201(k), 201(k-1) is in contact with the semiconductor chip 201(k-1).
[0085] 9, n semiconductor chips 201(1) to 201(n) to be stacked have the same shape, and are stacked with a certain amount of offset in a predetermined direction parallel to the main surface of the support 300. The stacking configuration is not limited to this example, and at least one of or both of the offset direction and distance between adjacent semiconductor chips may be different from those between other adjacent semiconductor chips.
[0086] However, without being limited to this configuration, the workpiece 900 may be configured such that a portion of the surface of the second adhesive layer 2 of the die attachment film 10 sandwiched between the semiconductor chip 201(1) and the support 300 is in contact with the support 300. Also, for example, the workpiece may be configured such that a portion of the surface of the first adhesive layer 1 of the die attachment film 10 sandwiched between two adjacent semiconductor chips 201(k), 201(k-1) is in contact with the semiconductor chip 201(k).
[0087] Furthermore, for example, multiple semiconductor chips of the same shape may be stacked together, i.e., the entire surfaces of the upper and lower semiconductor chips may overlap each other (i.e., without offset). Also, some or all of the semiconductor chips may have a different shape from the other semiconductor chips.
[0088] An example of the bonding process of the manufacturing method according to this embodiment will be described below. Note that the processes other than the bonding process are the same as those in the above embodiment, and therefore will not be described. In addition, the semiconductor chip 201(k) may be referred to as the k-th semiconductor chip 201(k) here.
[0089] First, the first semiconductor chip 201(1) taken out in the pick-up process is set at a predetermined position on the support 300 so that the die attach film 10 attached to the first semiconductor chip 201(1) contacts the support 300.
[0090] Thereafter, when k≧2, the kth semiconductor chip 201(k) removed in the pick-up process is set at a predetermined position on the (k-1)th semiconductor chip 201(k-1) so that the die attach film 10 is in contact with the first semiconductor chip 201(k-1), thereby producing the workpiece 900.
[0091] Thereafter, the die attach film 10 in the workpiece 900 is heated to a predetermined adhesion temperature to bond the semiconductor chip 201 to the support 300. The relationship between the adhesion temperature and the adhesion time is as explained in the above example. After bonding, the first adhesive layer 1 becomes the first adhesive layer, and the second adhesive layer 2 becomes the second adhesive layer.
[0092] During the preparation of the work 900, i.e., before the nth semiconductor chip 201(n) is set, the already set die attach film 10 may be intermediately heated once or twice or more times. The conditions for the intermediate heating may be the same as those for the heating of the work 900, or may be different.
[0093] Also, wiring may be formed to electrically connect the semiconductor chips 201 with each other and to electrically connect the semiconductor chips 201 with an electric circuit on the support 300. The wiring is formed by, for example, wire bonding or the like. The wiring may be formed during or after the bonding process.
[0094] The semiconductor device manufactured by the manufacturing method of this example has a plurality of semiconductor chips 201(1) to 201(n) stacked on a support 300, and has adhesive layers between the support 300 and the semiconductor chip 201(1) and between adjacent semiconductor chips 201(k) and 201(k-1), the adhesive layers including a first adhesive layer in contact with the semiconductor chip 201(k) farther from the support 300, and a second adhesive layer in contact with the support 300 (when k=1) or the semiconductor chip 201(k-1) closer to the support 300 (when k≧2).
[0095] In this semiconductor device, the shape of each semiconductor chip 201 and the positional relationship (e.g., offset direction and distance) between adjacent semiconductor chips 201(k) and 201(k-1) are not particularly limited, and examples are as described above.
[0096] <5. Effects of this embodiment> The die attach film 10 according to this embodiment is heated to a predetermined adhesion temperature to adhere the semiconductor chip 201 to the adherend. The die attach film 10 according to this embodiment includes a first adhesive layer 1 adhered to the semiconductor chip 201 and a second adhesive layer 2 adhered to the adherend, and the storage modulus of the second adhesive layer 2 at the adhesion temperature is lower than the storage modulus of the first adhesive layer at the adhesion temperature.
[0097] When the die attach film 10 is heated to the adhesion temperature, the semiconductor chip 201 and the adherend in contact with the die attach film 10 are also heated and thermally deformed. However, according to the configuration of this embodiment, the first adhesive layer 1, which has a high storage modulus, is in contact with the semiconductor chip 201, so the first adhesive layer 1 suppresses deformation of the semiconductor chip 201. Furthermore, according to this configuration, the second adhesive layer 2, which has a low storage modulus, is in contact with the adherend, so the soft second adhesive layer 2 deforms in accordance with the thermal deformation of the semiconductor chip 201 and the thermal deformation of the adherend, suppressing the application of stress to the semiconductor chip 201.
[0098] From the above, according to the die attach film 10 of this embodiment, when the semiconductor chip 201 is adhered to an adherend by heating, it is possible to reduce the stress applied to the semiconductor chip 201 while suppressing deformation of the semiconductor chip 201.
[0099] Furthermore, according to the manufacturing method of the semiconductor device of this embodiment, by using the die attach film 10, it is possible to suppress deformation of the semiconductor chip 201 while reducing the stress applied to the semiconductor chip 201 when the semiconductor chip 201 is adhered to an adherend by heating.
[0100] Furthermore, in the manufacture of a semiconductor device in which a plurality of semiconductor chips 201 are stacked on the support 300, stress and thermal deformation on the semiconductor chips 201 are more likely to accumulate. Therefore, in such a configuration, the effect of applying the die attachment film 10 and the manufacturing method for a semiconductor device according to the present embodiment is greater.
[0101] For example, when a workpiece (e.g., workpiece 900 shown in FIG. 9) is used in which a portion of a die attach film sandwiched between two adjacent semiconductor chips is in contact with the semiconductor chips, i.e., one semiconductor chip partially overlaps the other semiconductor chip, the following problem occurs. Stress in a direction that peels off the semiconductor chips is likely to concentrate at the boundary between the portion of the die attach film that is in contact with the semiconductor chips and the portion that is not in contact with them. Also, the portion of one semiconductor chip that does not overlap the other semiconductor chip makes it difficult to suppress deformation of the other semiconductor chip.
[0102] In response to this issue, the application of the die attach film 10 and semiconductor device manufacturing method according to the present embodiment (for example, the configuration shown in FIG. 9 ) has an even greater effect. This is because not only can the second adhesive layer 2, which has a low storage modulus, deform and suppress the concentration of stress at the above-mentioned boundary, but also the first adhesive layer 1, which has a high storage modulus, can suppress deformation of the semiconductor chip 201(k) in contact with the first adhesive layer 1. [Explanation of symbols]
[0103] 10: Die attach film 1: First adhesive layer 2: Second adhesive layer 3: Protective sheet 31: First protective sheet 32: Second protective sheet 100, 110: Die attach sheet 200: Semiconductor wafers 201, 201(1), 201(2)...201(n): Semiconductor chip 300: Support 301: Electrical circuits 302: Wiring
Claims
1. A die attach film that adheres a semiconductor chip to an object to be attached by being heated to a predetermined adhesion temperature, a first adhesive layer attached to the semiconductor chip; A second adhesive layer that is adhered to the adherend, A die attach film, characterized in that the storage modulus of the second adhesive layer at the adhesive temperature is lower than the storage modulus of the first adhesive layer at the adhesive temperature.
2. The die attach film according to claim 1 , wherein the surface of the first adhesive layer is adhesive.
3. A die attachment sheet comprising the die attachment film described in claim 1 or 2, and a protective sheet, wherein the protective sheet is attached to the surface of the second adhesive layer by adhesive force, and the peel strength between the protective sheet and the second adhesive layer is lower than the peel strength between the first adhesive layer and the second adhesive layer.
4. A method for manufacturing a semiconductor device, comprising the steps of: heating a die attach film to a predetermined bonding temperature in a workpiece in which a semiconductor chip is set on a support with a die attach film sandwiched therebetween, thereby bonding the semiconductor chip to the support, the method comprising the steps of: The die attach film comprises a first adhesive layer adhered to the semiconductor chip and a second adhesive layer adhered to the support, and the storage modulus of the second adhesive layer at the adhesion temperature is lower than the storage modulus of the first adhesive layer at the adhesion temperature.
5. A method for manufacturing a semiconductor device, comprising the steps of: heating a die attach film to a predetermined bonding temperature in a workpiece in which a plurality of semiconductor chips are stacked on a support, and a die attach film is sandwiched between the support and the semiconductor chips and between adjacent semiconductor chips, and bonding the semiconductor chips to the support and adjacent semiconductor chips, the method comprising the steps of: The method for manufacturing a semiconductor device, wherein the die attach film comprises a first adhesive layer adhered to a semiconductor chip farther from the support, and a second adhesive layer adhered to the support or a semiconductor chip closer to the support, and the storage modulus of the second adhesive layer at the adhesion temperature is lower than the storage modulus of the first adhesive layer at the adhesion temperature.
6. The method for manufacturing a semiconductor device according to claim 5 , wherein in the workpiece, a portion of the surface of the second adhesive layer of the die attach film sandwiched between two adjacent semiconductor chips is in contact with the semiconductor chips.
Citation Information
Patent Citations
Die attach film and dicing die attach film
JP2011082480A