Apparatus for producing calcium carbonate, parts used in the apparatus, and method for producing calcium carbonate
The calcium carbonate production apparatus addresses the challenge of continuous production by using a fine bubble generator and static mixer to convert carbon dioxide into calcium carbonate efficiently, minimizing emissions and ensuring continuous operation.
Patent Information
- Application Number
- JP2023068730
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing calcium carbonate production methods face challenges in continuously producing the compound while minimizing carbon dioxide emissions to the atmosphere, particularly due to insufficient stirring and mixing, and the need to manage pressure in closed containers.
A calcium carbonate production apparatus is designed with a slurry supply section, carbon dioxide supply section, and slurry recovery section connected by a connection line, incorporating a fine bubble generator and static mixer to ensure thorough mixing and reaction of calcium hydroxide and carbon dioxide, allowing for continuous production without significant carbon dioxide release.
The apparatus efficiently converts carbon dioxide into calcium carbonate, reducing atmospheric emissions and enabling continuous production with a simple device configuration, promoting environmental sustainability.
Smart Images

Figure 2024154733000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an apparatus for producing calcium carbonate, parts used in the apparatus, and a method for producing calcium carbonate. More particularly, the present invention relates to an apparatus for continuously producing calcium carbonate, parts used in the apparatus, and a method for continuously producing calcium carbonate. [Background technology]
[0002] Carbon dioxide (CO2) is a greenhouse gas that has a major impact on environmental issues such as global warming, so there is a need to significantly reduce emissions. For this reason, progress is being made in the development of technology to selectively capture and immobilize carbon dioxide emitted from thermal power plants, factories, etc.
[0003] As a technique for recovering and fixing carbon dioxide, for example, a method for fixing carbon dioxide as a carbonate (e.g., calcium carbonate or magnesium carbonate) by a chemical reaction is known. Patent documents 1 and 2 describe a method for producing calcium carbonate. Various techniques have been proposed for producing calcium carbonate, and Patent document 3 discloses a method for precipitating calcium carbonate and / or magnesium carbonate in the presence of ultrafine bubbles containing carbon dioxide gas. Patent document 4 discloses a method for fixing carbon dioxide as calcium carbonate without releasing it to the outside by using a fine bubble generator equipped with a porous part having fine pores in a sealed container. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 3995761 [Patent Document 2] Patent No. 4961074 [Patent Document 3] Patent No. 6742867 [Patent Document 4] Patent No. 7196254 Summary of the Invention [Problem to be solved by the invention]
[0005] In the apparatus having the configuration disclosed in Fig. 6 of Patent Document 3, ultrafine bubbles are supplied to an open container in a state where they are not sufficiently stirred and mixed after being blown in. This may result in a large amount of carbon dioxide being released into the atmosphere. In addition, when a closed container such as that disclosed in Patent Document 4 is used, it is necessary to remove the reacted slurry in an amount equal to the amount of calcium hydroxide newly replenished in order to prevent an increase in the pressure inside the container, which still poses a problem from the viewpoint of continuously producing calcium carbonate.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a calcium carbonate production apparatus capable of continuously producing calcium carbonate with almost no emission of carbon dioxide to the outside. Another object of the present invention is to provide parts used in the production apparatus, and a method for producing calcium carbonate. [Means for solving the problem]
[0007] In order to achieve the above object, a calcium carbonate manufacturing apparatus is disclosed herein. The calcium carbonate manufacturing apparatus disclosed herein includes a slurry supplying section that supplies a slurry containing calcium hydroxide, a carbon dioxide supplying section that supplies carbon dioxide as fine bubbles to the slurry, a slurry recovery section that recovers the generated calcium carbonate-containing slurry, and a connection line that connects the slurry supplying section, the carbon dioxide supplying section, and the slurry recovery section. The carbon dioxide supplying section has a fine bubble generating device arranged on the upstream side along the flow direction of the slurry, and a static mixer arranged on the downstream side, and when a configuration of one fine bubble generating device and one static mixer is considered as one unit, the apparatus has at least two units of the unit along the flow direction of the slurry.
[0008] According to this configuration, the calcium hydroxide and carbon dioxide are mixed suitably by supplying carbon dioxide as fine bubbles from the fine bubble generator. Then, the slurry is sufficiently stirred and mixed by the dividing action and converting action of the static mixer, so that the carbonation reaction can be completed quickly. When one fine bubble generator and one static mixer constitute one unit, the carbonation reaction can be almost completed by having two or more such units. Therefore, according to this configuration, calcium carbonate can be continuously produced with almost no carbon dioxide released to the outside. Also, according to this configuration, carbon dioxide can be suitably fixed as calcium carbonate.
[0009] In a preferred embodiment of the production apparatus disclosed herein, the fine bubble generating device includes a fine bubble generating tube made of a porous body having fine pores. According to this configuration, fine bubbles containing carbon dioxide can be suitably generated.
[0010] In a preferred embodiment of the production apparatus disclosed herein, the micro-bubble generating device has a mean pore size of the micro-pores of 0.5 μm or more and 10 μm or less. According to this configuration, fine bubbles containing carbon dioxide can be suitably generated.
[0011] In a preferred embodiment of the manufacturing apparatus disclosed herein, the fine bubble generator generates fine bubbles having an average particle size of 100 μm or less, including at least ultrafine bubbles having a particle size of less than 1 μm. According to this configuration, the calcium hydroxide and carbon dioxide in the slurry are mixed more suitably, and the carbonation reaction proceeds quickly.
[0012] In a preferred embodiment of the manufacturing apparatus disclosed herein, the slurry supply section has an open supply tank, and the slurry recovery section has an open recovery tank, and the supply tank, the fine bubble generator, the static mixer, and the recovery tank are connected by the connection line. In the manufacturing apparatus disclosed herein, as described above, calcium hydroxide and carbon dioxide react quickly by using a fine bubble generator and a static mixer, so that carbon dioxide can be fixed as calcium carbonate with almost no release of carbon dioxide to the outside, even if an open recovery tank is used.
[0013] In a preferred embodiment of the manufacturing apparatus disclosed herein, each of the fine bubble generators is connected to a carbon dioxide supply line that supplies carbon dioxide, and when the flow rate of the slurry flowing through the connecting line is defined as flow rate X and the supply amount of carbon dioxide supplied to the carbon dioxide supply line is defined as supply amount Y, the ratio (Y / X) of supply amount Y to flow rate X is less than 1. According to this configuration, the supplied carbon dioxide can be more suitably fixed as calcium carbonate.
[0014] In a preferred embodiment of the production apparatus disclosed herein, when one unit is constituted by one fine bubble generator and one static mixer, the apparatus has 2 to 50 such units along the flow direction of the slurry. According to this configuration, the carbonation reaction can be suitably completed.
[0015] As another aspect of the technology disclosed herein, there is provided a part used in the calcium carbonate production apparatus. The part of the calcium carbonate production apparatus disclosed herein includes one fine bubble generator arranged on the upstream side along the flow direction of the slurry, one static mixer arranged on the downstream side, and a connection line connecting the fine bubble generator and the static mixer. By installing parts having such a configuration on a line for supplying slurry of an existing calcium carbonate manufacturing apparatus, carbon dioxide can be suitably fixed as calcium carbonate.
[0016] As another aspect of the technology disclosed herein, there is provided a method for producing calcium carbonate. The method disclosed herein includes a step of supplying a slurry containing calcium hydroxide, a step of supplying carbon dioxide as fine bubbles to the slurry, and a step of recovering the produced slurry containing calcium carbonate. The carbon dioxide supply step is characterized in that, when a configuration of one fine bubble generator arranged on the upstream side along the flow direction of the slurry and one static mixer arranged on the downstream side is regarded as one unit, the slurry is passed through the unit at least two times. According to this configuration, the reaction between calcium hydroxide and carbon dioxide can be quickly completed, thereby realizing a method for continuously producing calcium carbonate with almost no release of carbon dioxide to the outside.
[0017] In a preferred embodiment of the manufacturing apparatus disclosed herein, when the flow rate of the slurry in the slurry supplying step is defined as flow rate X and the supply amount of carbon dioxide in the carbon dioxide supplying step is defined as supply amount Y, the flow rate of the slurry and the supply amount of carbon dioxide are adjusted so that the ratio of the supply amount Y to the flow rate X is less than 1. According to this configuration, carbon dioxide can be more suitably fixed as calcium carbonate.
[0018] In a preferred embodiment of the production apparatus disclosed herein, the concentration of calcium hydroxide in the slurry containing the calcium hydroxide is 0.1 mol / L or more and 4 mol / L or less. According to this configuration, calcium carbonate can be produced efficiently.
[0019] In a preferred embodiment of the production apparatus disclosed herein, in the carbon dioxide supplying step, carbon dioxide is supplied as fine bubbles having an average particle size of 100 μm or less, including ultrafine bubbles having a particle size of at least less than 1 μm. According to this configuration, the stirring force is improved by the fine bubbles, and the contact specific surface area of the carbon dioxide is increased, so that the calcium hydroxide and the carbon dioxide can react with each other more quickly.
[0020] A preferred embodiment of the production apparatus disclosed herein further comprises a second carbon dioxide supplying step of supplying carbon dioxide to the slurry recovered in the slurry recovery step. This configuration can further increase the carbonation rate. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a diagram illustrating a calcium carbonate manufacturing apparatus according to one embodiment. [Diagram 2] FIG. 2 is a diagram illustrating a schematic configuration of a fine bubble generating device according to one embodiment. [Diagram 3] FIG. 3 is a schematic diagram of a static mixer according to an embodiment. [Figure 4] FIG. 4 is a diagram illustrating another example of the apparatus for producing calcium carbonate according to the embodiment. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, a preferred embodiment of the present invention will be described with reference to the drawings as appropriate. Any matters other than those specifically mentioned in this specification that are necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field. In this specification, the expression "A to B" indicating a numerical range means "A or more and B or less" unless otherwise specified.
[0023] Fig. 1 is a diagram showing a schematic diagram of a manufacturing apparatus 100 for calcium carbonate disclosed herein. The arrows in Fig. 1 indicate the flow direction of the slurry. In this specification, the side close to the slurry supplying part 110 along the flow of the slurry is referred to as the upstream side, and the side away from the slurry supplying part 110 is referred to as the downstream side. Hereinafter, each component of the manufacturing apparatus 100 disclosed herein will be described with reference to Fig. 1 etc.
[0024] As shown in FIG. 1, the manufacturing apparatus 100 includes a slurry supplying section 110, a carbon dioxide supplying section 120, a slurry collecting section 130, and a connection line 140. The slurry supplying section 110, the carbon dioxide supplying section 120, and the slurry collecting section 130 are connected by a connection line 140 configured to allow the slurry to flow. The carbon dioxide supplying section 120 includes at least a fine bubble generating device 20 and a static mixer 30, which will be described later, and the fine bubble generating device 20 is disposed on the upstream side and the static mixer 30 is disposed on the downstream side along the flow direction of the slurry. The manufacturing apparatus 100 disclosed herein has at least two units of a configuration of one fine bubble generating device 20 and one static mixer 30 along the flow direction of the slurry, assuming that the configuration of one fine bubble generating device 20 and one static mixer 30 is one unit. This makes it possible to continuously manufacture calcium carbonate with almost no carbon dioxide released to the outside, despite the simple device configuration. According to the manufacturing apparatus 100, carbon dioxide can be suitably fixed as calcium carbonate.
[0025] Here, "immobilizing carbon dioxide" means converting carbon dioxide into a carbonate compound by chemically reacting it with a solution or the like. For example, according to the technology disclosed herein, carbon dioxide is converted (immobilized) into calcium carbonate by chemically reacting fine bubbles containing carbon dioxide with a slurry containing calcium hydroxide. In this way, by converting carbon dioxide into a useful carbonate compound, the amount of carbon dioxide emitted into the atmosphere can be significantly reduced, and since carbon dioxide is recycled, it can contribute to solving environmental problems such as global warming. There is no particular limitation on the supply (generation) source of carbon dioxide to be immobilized. For example, carbon dioxide generated from factories, thermal power plants, automobiles, etc. can be collected and immobilized as calcium carbonate.
[0026] The slurry supplying unit 110 is for supplying a slurry containing calcium hydroxide. The configuration of the slurry supplying unit 110 is not particularly limited. For example, as shown in FIG. 1, the slurry supplying unit 110 may include a supply line 111 having a space in which the raw material (slurry) can flow, a valve 112 for opening and closing the supply line 111, a supply tank 113 for temporarily storing the slurry, and a liquid sending pump 114 for supplying the slurry to a connection line 140. When the valve 112 is opened, the raw material (slurry) is supplied to the supply tank 113 from a raw material tank (not shown), and when the valve 112 is closed, the supply of the raw material is stopped. The supply tank 113 stores a slurry in which calcium hydroxide is dissolved or dispersed in an aqueous solvent (e.g., water).
[0027] The supply tank 113 may be an open tank or a closed tank. From the viewpoint of improving the manufacturing efficiency, it is preferable that the supply tank 113 is an open tank. The shape of the supply tank 113 is not particularly limited, and may be, for example, substantially cylindrical or substantially rectangular. The supply tank 113 may be, for example, a substantially cylindrical container having a ratio (H / D) of the height H of the container to the inner diameter D of the container of about 1.0 to 1.5. Alternatively, the supply tank 113 may be, for example, a substantially cylindrical container that is elongated in the height direction and has a ratio (H / D) of the height H of the container to the inner diameter D of the container of more than 1.5 and about 2 or less. In addition, the supply tank 113 may be configured to be convex toward the lower side in a cross-sectional view along the height direction, as shown in FIG. 1. This allows the slurry containing calcium hydroxide to be suitably supplied to the connection line 140.
[0028] Although not particularly limited, the slurry supply unit 110 may include an agitator 115 as shown in Fig. 1. The agitator 115 is disposed inside the supply tank 113 and agitates the slurry stored in the supply tank 113. Although not particularly limited, the agitator 115 includes, for example, an agitator blade and a motor connected to the agitator blade via an agitator shaft. By including the agitator 115 in the slurry supply unit 110, the slurry in the supply tank can be kept in a suitable state without settling.
[0029] The flow rate X of the slurry flowing through the connection line 140 can be appropriately adjusted by the liquid feed pump 114. The flow rate X of the slurry is not limited to a specific value because it is appropriately changed depending on the relationship with the supply amount Y of carbon dioxide, but is preferably, for example, about 800 ml / min to 2500 ml / min.
[0030] The carbon dioxide supply unit 120 is for supplying a gas containing carbon dioxide to the slurry flowing through the connection line 140. The gas supplied by the carbon dioxide supply unit 120 is preferably a gas containing 90% or more (more preferably 95% or more) of carbon dioxide (e.g., carbon dioxide gas). The carbon dioxide supply unit 120 includes at least a fine bubble generator 20 and a static mixer 30. The fine bubble generator 20 is a device for blowing fine bubbles containing carbon dioxide into the slurry. The static mixer 30 is a member for mixing the fine bubbles containing carbon dioxide supplied from the fine bubble generator 20 with the slurry. In addition to the fine bubble generator 20 and the static mixer 30 described above, the carbon dioxide supply unit 120 may include a gas storage unit 122 for storing carbon dioxide gas (carbon dioxide gas), a carbon dioxide supply line 124 having a space through which carbon dioxide can flow, a pressure adjustment valve 126 for adjusting the supply pressure of carbon dioxide, and a needle valve 128 for adjusting the supply amount (flow rate) of carbon dioxide. The carbon dioxide supply line 124 is connected to each of the multiple fine bubble generators 20.
[0031] Here, in this specification, "fine bubbles containing carbon dioxide" refers to fine bubbles formed by, for example, injecting a gas (carbon dioxide gas) containing 90% or more (more preferably 95% or more) of carbon dioxide into a fine bubble generator. In addition, in this specification, "fine bubbles" includes at least "microbubbles" and "ultrafine bubbles." The definitions of microbubbles and ultrafine bubbles comply with the standards of the International Organization for Standardization (ISO), where microbubbles are bubbles with an average diameter of 1 μm or more and less than 100 μm, and ultrafine bubbles are bubbles with an average diameter of less than 1 μm.
[0032] The gas storage section 122 temporarily stores the carbon dioxide gas (carbon dioxide gas) to be immobilized. The origin of the carbon dioxide gas stored in the gas storage section 122 (source of carbon dioxide gas) is not particularly limited. For example, it may be exhaust gas containing carbon dioxide generated in a factory or the like. A carbon dioxide absorbent is installed at the supply (generation) source of such exhaust gas, and the adsorbed carbon dioxide is released by heating using steam or the like, so that the carbon dioxide gas originating from the exhaust gas can be stored in the gas storage section 122. Examples of such carbon dioxide absorption materials include porous materials, chemical absorption materials into which amino groups having carbon dioxide absorption capacity have been introduced, metal-organic frameworks (MOFs), carbonaceous materials, carbon dioxide adsorption materials / absorption materials made of alkali metal calcium carbonate, and the like. Such carbon dioxide absorption materials are easily miniaturized, and therefore can be implemented at a lower cost than installing piping to directly introduce carbon dioxide from a factory or the like. In a preferred embodiment, carbon dioxide adsorbed to a chemical absorption material into which amino groups having carbon dioxide absorption capacity have been introduced may be used.
[0033] FIG. 2 is a diagram showing a schematic configuration of a fine bubble generating device 20 used in the manufacturing apparatus 100 disclosed herein. As shown in FIG. 2, the fine bubble generating device 20 has a tubular fine bubble generating tube 21 made of a porous body having fine pores, and a base material portion 22 surrounding the fine bubble generating tube 21. The fine bubble generating tube 21 is connected to a connection line 140. In the example shown in FIG. 2, there is one fine bubble generating tube 21, but two or more (i.e., a plurality) fine bubble generating tubes 21 may be provided. In the following description, one end of the fine bubble generating tube 21 along the flow direction of the slurry is referred to as an upstream end 21a (the end on the right side in FIG. 2), and the other end is referred to as a downstream end 21b (the end on the left side in FIG. 2).
[0034] The base member 22 has an upstream support part 23a that supports the upstream end 21a of the fine bubble generating tube 21, a downstream support part 23b that supports the downstream end 21b, and a body part 24 that is attached between the upstream support part 23a and the downstream support part 23b and surrounds the fine bubble generating tube 21. The upstream support part 23a is provided with at least one slurry inlet 25, and the downstream support part 23b is provided with at least one slurry outlet 26. The body part 24 is also provided with at least one carbon dioxide inlet 27.
[0035] The fine bubble generator 20 is a so-called in-line type fine bubble generator 20 that supplies gas (here, carbon dioxide gas) from the outer surface side of the fine bubble generating tube 21 and supplies fine bubbles to a liquid (here, a slurry) passing through the fine bubble generating tube. In the in-line type fine bubble generator 20, carbon dioxide is supplied from the carbon dioxide inlet 27 under pressure, so that the carbon dioxide can be blown as fine bubbles into the slurry passing through the fine bubble generating tube. By blowing carbon dioxide into the slurry as fine bubbles including ultrafine bubbles and microbubbles, the stirring force and the contact specific surface area are improved, so that the calcium hydroxide and carbon dioxide can react in a shorter time.
[0036] The supply amount (flow rate) Y of carbon dioxide in the carbon dioxide supply line 124 is appropriately adjusted by a needle valve 128. The supply amount Y of carbon dioxide is not limited to a specific amount because it is appropriately changed depending on the relationship with the flow rate X of the slurry, but is preferably, for example, about 100 ml / min to 2000 ml / min.
[0037] In the manufacturing apparatus 100 disclosed herein, the ratio (Y / X) of the supply amount Y of carbon dioxide to the flow rate X of the slurry is preferably less than 1. This allows the supplied carbon dioxide to react with calcium hydroxide in the slurry without loss and be suitably fixed as calcium carbonate. The ratio (Y / X) of the supply amount Y of carbon dioxide to the flow rate X of the slurry is preferably 0.91 or less, and may be 0.83 or less, for example. From the viewpoint of manufacturing efficiency, the ratio (Y / X) of the supply amount Y of carbon dioxide to the flow rate X of the slurry is preferably 0.1 or more, and more preferably 0.27 or more. The flow rate X of the slurry and the supply amount Y of carbon dioxide gas may be set to satisfy the above-mentioned (Y / X), and may be appropriately set in consideration of the inner diameter of the connection line 140, etc. For example, even if the values of the flow rate X of the slurry and the supply amount Y of carbon dioxide exceed the above-mentioned ranges, the flow rate X of the slurry and the supply amount Y of carbon dioxide gas may be controlled to satisfy the above-mentioned range of (Y / X).
[0038] The supply pressure (MPa) of carbon dioxide is adjusted by the pressure regulating valve 126. The supply pressure of carbon dioxide can be set to a supply pressure at which ultra-fine bubbles are easily generated. For example, the supply pressure of carbon dioxide is preferably 0.01 MPa or more and 0.8 MPa or less, more preferably 0.04 MPa or more and 0.6 MPa or less, and particularly preferably 0.1 MPa or more and 0.6 MPa or less, in terms of the pressure difference between the pressure in the pipe (fine bubble generating tube) and the pressure in the distilled water in the fine bubble generating tube of the fine bubble generating device, which is set to 0. By controlling the supply pressure within the above-mentioned range, fine bubbles are supplied in a form containing ultra-fine bubbles, so that the specific surface area with calcium hydroxide in the slurry can be increased. This allows the reaction between carbon dioxide and calcium hydroxide to proceed favorably, and the reaction time can be shortened. The pressure difference between the carbon dioxide supply pressure and the pressure in the piping has an appropriate range for each average pore size of the fine bubble generating tube 21. If the carbon dioxide supply pressure is too high, ultrafine bubbles will not be generated and millibubbles with an average diameter of 100 μm or more will mainly be generated, which may result in a decrease in the reaction rate and a sudden rise in pressure in the piping.
[0039] The shape of the microbubble generating tube 21 is not particularly limited as long as it has a space through which the slurry can flow. The microbubble generating tube 21 may be, for example, a circular tube having a circular cross section and extending linearly. The shape of the microbubble generating tube 21 is not limited to this, and may be, for example, a square tube having a rectangular cross section, a hexagonal cross section, or the like. The microbubble generating tube 21 may also be shaped such that the diameter differs between the upstream side and the downstream side (for example, a cone shape). The outer diameter R1 of the microbubble generating tube 21 may be, for example, about 3 mm to 16 mm, and the inner diameter R2 may be, for example, about 1 mm to 12 mm (preferably, 3 mm to 10 mm). The effective length L of the microbubble generating tube 21 (i.e., the length of the portion capable of supplying carbon dioxide gas to the slurry 10 flowing inside the microbubble generating tube 21) is preferably, for example, about 50 mm to 1000 mm. According to the fine bubble generating tube 21 configured in this manner, by injecting gas (e.g., carbon dioxide gas) from the outside, fine bubbles containing carbon dioxide can be suitably generated in the slurry 10 flowing inside the fine bubble generating tube 21.
[0040] The microbubble generating tube 21 has interconnected pores and can be made of a porous body with a porosity of about 20 to 60%. The material of the porous body is preferably ceramic. Specific examples of the material include alumina (Al2O3), zirconia (ZrO2), magnesia (MgO), silica (SiO2), titania (TiO2), zircon (ZrSiO4), and mullite (Al6O 13 The ceramic may be an oxide ceramic such as silicon nitride (Si2), a non-oxide ceramic such as silicon nitride (Si3N4), boron nitride (BN), aluminum nitride (AlN), silicon carbide (SiC), boron carbonitride, or a composite material containing at least one of these ceramics. Among these, alumina, boehmite, silica, and titania are preferably used because they are stable in quality, inexpensive, and easily available. The chemical formulas shown in parentheses after the above substance names indicate the representative compositions of the substances, and are not intended to limit the compositions of the actual ceramics to those with these chemical formulas.
[0041] Although not particularly limited, the fine bubble generator 20 is preferably configured to generate fine bubbles having an average particle size of 100 μm or less, including ultrafine bubbles having a particle size of less than 1 μm. If the fine bubbles have an average particle size of about 100 μm or less, the stirring force is improved, and the power used for stirring can be significantly reduced. In addition, since the fine bubbles contain ultrafine bubbles, the contact specific surface area of the blown carbon dioxide is increased, and it can react with calcium hydroxide in a short time. Therefore, energy saving and reaction promotion are realized. In this specification, the "average particle size" refers to a particle size (D50, also called the median size) corresponding to a cumulative frequency of 50% from the fine particle side with a small particle size in a particle size distribution based on the number standard based on a general image analysis method. Such an image analysis method can be performed, for example, using a particle shape / particle size distribution measuring device of a dynamic image analysis type.
[0042] The average pore diameter of the fine bubble generating tube 21 is not particularly limited as long as fine bubbles including ultrafine bubbles and microbubbles can be generated. The average pore diameter of the fine bubble generating tube 21 is preferably 0.5 μm or more, more preferably 1 μm or more, and may be 1.3 μm or more, or may be 3 μm or more. If the average pore diameter is too large, fine bubbles (bubbles) of a desired size cannot be generated, so the average pore diameter is preferably 10 μm or less, may be 9 μm or less, or may be 7 μm or less. For example, the average pore diameter of the fine bubble generating tube 21 is preferably 1.3 μm to 10 μm. The average pore diameter of the fine bubble generating tube 21 can be measured by, for example, mercury intrusion porosimetry.
[0043] FIG. 3 is a schematic diagram of a static mixer used in the manufacturing apparatus 100 disclosed herein. The static mixer 30 is a stationary mixer that does not have a moving part. The static mixer 30 mixes the slurry by consuming the velocity energy when the slurry passes through a pipe. In other words, by using the static mixer 30, the slurry and the fine bubbles can be mixed using only the energy for making the slurry flow. Therefore, energy saving can be realized.
[0044] The material of the static mixer 30 is not particularly limited, and may be made of, for example, a metal material such as stainless steel or a resin material such as polyvinyl chloride. As shown in FIG. 3, the static mixer 30 has a cylindrical pipeline 32 and a mixing element 34 (hereinafter, also referred to as "element 34"). The static mixer 30 has an element 34 installed in the pipeline. The shape of the element 34 is a rectangular plate material twisted 180 degrees in opposite directions. The elements 34 are arranged along the axial direction of the pipeline 32 with the axis CL of the pipeline as the center. As shown in FIG. 3, the elements 34 are arranged such that right elements 34a and left elements 34b are alternately arranged. The pipeline 32 of the static mixer 30 is connected to a connection line 140. The slurry is subjected to inversion, division, and conversion actions by the elements 34 arranged in the pipeline during the process of passing through the pipeline, and is suitably mixed with fine bubbles.
[0045] Although not particularly limited, from the viewpoint of realizing suitable mixing, the number of elements of the static mixer 30 is preferably 6 to 36, and more preferably 12 to 24. Note that the "number of elements" refers to the number of elements 34, and for example, the number of elements of the static mixer 30 shown in Fig. 3 is 4.
[0046] The inner diameter R3 of the static mixer 30 is not particularly limited as long as the slurry is flowable. It is preferable that the inner diameter R3 of the static mixer 30 is not significantly different from the inner diameter R2 of the fine bubble generating tube 21. As an example, the inner diameter R3 of the static mixer 30 may be about 3 mm to 12 mm (preferably 6 mm to 10 mm).
[0047] As described above, in the manufacturing apparatus 100 disclosed herein, the fine bubble generator 20 is used, so that carbon dioxide can be injected into the slurry in the form of ultrafine bubbles or microbubbles. In addition, the splitting and conversion action of the static mixer 30 allows calcium hydroxide and carbon dioxide to react in a short time even in an in-line state. For this reason, by arranging the fine bubble generator 20 and the static mixer 30 in series along the flow direction of the slurry, calcium carbonate can be produced more efficiently. Specifically, in the manufacturing apparatus 100 disclosed herein, when one fine bubble generator 20 and one static mixer 30 constitute one unit, the apparatus has at least two units along the flow direction of the slurry. This allows the injected carbon dioxide to be suitably fixed as calcium carbonate while achieving a sufficient carbonation rate despite its compact form. In addition, the reaction between calcium hydroxide and carbon dioxide in the slurry that has passed through the fine bubble generator 20 and the static mixer 30 is almost complete, so that even if the recovery tank 132 described below is an open tank, there is a low possibility that carbon dioxide will be released to the outside. Therefore, calcium carbonate can be continuously produced with a simple device configuration while hardly releasing carbon dioxide to the outside.
[0048] FIG. 4 is a schematic diagram showing another example of the manufacturing apparatus 100 disclosed herein. In the manufacturing apparatus 100 shown in FIG. 4, the fine bubble generator 20 and the static mixer 30 are repeatedly connected in n units along the flow direction of the slurry. The number of units (hereinafter, simply referred to as the "number of units") when one fine bubble generator 20 and one static mixer 30 constitute one unit may be 2 units or more. For example, as shown in FIG. 4, n units may be connected. The number of units may be appropriately set according to the target carbonation rate and is not particularly limited, but from the viewpoint of manufacturing efficiency, it is preferable to set the carbonation rate to 5% or more. For example, the number of units is 2 units or more, preferably 4 units or more, more preferably 10 units or more, may be 14 units or more, may be 20 units or more, may be 24 units or more, or may be 30 units or more. As the number of units increases, the amount of carbon dioxide that can be blown into the slurry can be increased, and therefore the carbonation rate can be suitably improved. Furthermore, the upper limit of the number of units is not particularly limited, but may be, for example, 60 units or less, or 50 units or less.
[0049] A part having one fine bubble generator 20, one static mixer 30, and a connection line 140 connecting them can be easily installed in an existing open calcium carbonate production line. In other words, by using such a part in an existing calcium carbonate production line, carbon dioxide can be fixed as carbonate in a simple manner.
[0050] The slurry recovery unit 130 is disposed downstream of the carbon dioxide supply unit 120. The slurry recovery unit 130 is for recovering a slurry containing the generated calcium carbonate. The configuration of the slurry recovery unit 130 is not particularly limited. For example, as shown in FIG. 1, the slurry recovery unit 130 may include a recovery tank 132 for recovering a slurry containing the generated calcium carbonate, a recovery line 134 connected to the recovery tank 132, and a valve 136 for opening and closing the recovery line 134.
[0051] The recovery tank 132 may be an open tank or a closed tank. When the recovery tank 132 is a closed tank, it is preferable that the recovery tank 132 has a safety valve (not shown). The safety valve can be set to release the internal pressure when the internal pressure in the container rises to a predetermined level or higher for some reason. The shape of the recovery tank 132 provided in the slurry recovery unit 130 may be approximately the same as the shape of the supply tank 113 provided in the slurry supply unit 110. That is, the shape of the recovery tank 132 is not particularly limited, and may be, for example, approximately cylindrical or approximately rectangular.
[0052] 1, the slurry collecting section 130 may include an agitator 138. The agitator 138 may be an agitator having a configuration substantially similar to that of the agitator 115 that may be included in the slurry supplying section 110. By including the agitator 138 in the slurry collecting section 130, the slurry and the fine bubbles containing carbon dioxide are mixed more suitably.
[0053] The connection line 140 has a space in which the slurry can flow. The connection line 140 connects the above-mentioned slurry supply unit 110, the carbon dioxide supply unit 120, and the slurry recovery unit 130. More specifically, the connection line 140 may connect the supply tank 113, the fine bubble generator 20, the static mixer 30, and the recovery tank 132. As shown in FIG. 1, the connection line 140 may include two three-way valves 142a and 142b, and a valve 144 for controlling supply / stop to the recovery tank 132. A desired amount of the slurry stored in the supply tank 113 is supplied to the connection line 140 by operating the liquid feed pump 114. The slurry flows inside the connection line 140 and passes through the fine bubble generator 20. At this time, the fine bubble generator 20 pressurizes fine bubbles containing carbon dioxide into the passing slurry. The slurry flows again inside the connection line 140 and passes through the static mixer 30. At this time, the static mixer 30 mixes the slurry with fine bubbles containing carbon dioxide. After the injection of fine bubbles containing carbon dioxide by the fine bubble generator 20 and the mixing of the slurry with the fine bubbles by the static mixer 30 are repeated multiple times (i.e., the unit number), the slurry is fed into the recovery tank 132 via the connection line 140. With this configuration, most of the steps can be performed by the power of the liquid delivery pump 114, thereby realizing energy savings.
[0054] The inner diameter of the connection line 140 is not particularly limited as long as the slurry can flow, but it is preferable that the inner diameter is not extremely different from the inner diameter R2 of the fine bubble generating tube 21. As an example, the inner diameter of the connection line 140 may be about 3 mm to 12 mm.
[0055] In the example shown in Fig. 1, the connection line 140 is configured to input the slurry from the upper side of the collection tank 132, but the form of connection between the connection line 140 and the collection tank 132 is not limited to this. For example, the connection line 140 may be configured to input the slurry from the lower side of the collection tank 132. By inputting the slurry from the lower side of the collection tank 132, carbon dioxide supplied as fine bubbles together with the slurry moves while floating in the slurry, and is more suitably fixed as calcium carbonate. Therefore, even if the collection tank 132 is an open tank, it is possible to further suppress the release of carbon dioxide to the outside.
[0056] The slurry containing calcium carbonate recovered in the recovery tank 132 can be recovered by opening a valve 136 of the recovery line 134. The slurry recovered here is in the state of a suspension in which calcium carbonate is dispersed in liquid. The suspension can be processed into a desired form and utilized by storing, concentrating, drying, etc., using a conventionally known device, as necessary.
[0057] Although not shown, the manufacturing apparatus 100 may further include a mechanism for blowing carbon dioxide into the slurry recovered in the recovery tank 132. At this time, carbon dioxide with a high purity (for example, 99% or more) may be blown in, or exhaust gas discharged from a factory or the like may be blown in. By blowing more carbon dioxide into the slurry recovered in the recovery tank 132, the carbonation rate can be further increased. In this specification, the term "carbonation rate" refers to the amount of precipitated calcium carbonate relative to the amount of calcium hydroxide used to prepare the slurry. The "carbonation rate" can be measured by drying the recovered slurry and using a thermogravimetry-differential thermal analysis (TG-DTA).
[0058] The above describes an apparatus for suitably producing calcium carbonate. With this production apparatus, calcium carbonate can be continuously produced with almost no release of carbon dioxide to the outside, despite its simple configuration. Therefore, carbon dioxide can be more suitably fixed, and calcium carbonate can be produced efficiently. In addition, with this apparatus, a system can be constructed that indicates the amount of carbon dioxide fixed using the apparatus.
[0059] The method for producing calcium carbonate disclosed herein will be described below. The method for producing calcium carbonate disclosed herein includes at least a slurry supplying step of supplying a slurry containing calcium hydroxide, a carbon dioxide supplying step of supplying carbon dioxide as fine bubbles to the slurry, and a slurry recovery step of recovering the produced slurry containing calcium carbonate. The production method disclosed herein is characterized in that, in the carbon dioxide supplying step, when a configuration of one fine bubble generator arranged on the upstream side along the flow direction of the slurry and one static mixer arranged on the downstream side is taken as one unit, the slurry is passed through the unit at least two times, and other than this, the process may be the same as the conventional production process of calcium carbonate. In addition, other steps may be included at any stage.
[0060] The slurry supplying step is a step of supplying a slurry containing calcium hydroxide, which is a raw material for calcium carbonate. The slurry supplied in this step is in the form of a dispersion liquid or a slurry composition in which calcium hydroxide is dispersed in a liquid medium such as an aqueous solvent. Here, the aqueous solvent may be, for example, water or a mixed solution of water and alcohol. As the aqueous solvent, ion-exchanged water (deionized water), pure water, ultrapure water, distilled water, etc. can be preferably used.
[0061] The calcium hydroxide concentration of the slurry containing calcium hydroxide is preferably 0.1 mol / L or more, more preferably 0.5 mol / L or more, and may be 1 mol / L or more. The upper limit of the calcium hydroxide concentration is preferably 5 mol / L or less, more preferably 4 mol / L or less, and may be 3 mol / L or less. Within this concentration range, the carbon dioxide supplied as fine bubbles and the calcium hydroxide in the slurry react favorably, and calcium carbonate can be stably produced. The pH of the slurry supplied in the slurry supplying step is not particularly limited, but may be adjusted to, for example, about 12 to 13.
[0062] In the slurry supplying step, the prepared slurry is supplied to the connection line 140. For example, the liquid sending pump 114 connected to the supply tank 113 may be operated to supply a desired amount of slurry to the connection line 140. The flow rate X of the slurry in the slurry supplying step is appropriately changed depending on the relationship with the supply amount Y of carbon dioxide in the carbon dioxide supplying step, so is not limited to any particular value, but is preferably, for example, about 800 ml / min to 2500 ml / min.
[0063] In the carbon dioxide supplying step, carbon dioxide is supplied to the slurry as fine bubbles. In the carbon dioxide supplying step, fine bubbles containing carbon dioxide are blown into the slurry using the fine bubble generator 20 described above. Then, the slurry and the blown fine bubbles are mixed by the static mixer 30 arranged downstream of the fine bubble generator 20. With this configuration, calcium hydroxide in the slurry and carbon dioxide blown as fine bubbles can be mixed suitably. In particular, when a configuration of one fine bubble generator 20 and one static mixer 30 is regarded as one unit, calcium hydroxide and carbon dioxide can be reacted in a shorter time by passing through the unit two or more times. Therefore, according to the manufacturing method disclosed herein, calcium carbonate can be continuously manufactured without releasing almost any carbon dioxide to the outside.
[0064] In the carbon dioxide supply step, the number of times the slurry is passed through the configuration of one fine bubble generator 20 and one static mixer 30 is two or more, preferably four or more, more preferably ten or more, may be 14 or more, may be 20 or more, may be 24 or more, or may be 30 or more. As the number of units increases, the amount of carbon dioxide that can be blown into the slurry can be increased, and the carbonation rate can be suitably improved. The number of times the slurry is passed through the configuration of one fine bubble generator 20 and one static mixer 30 may be appropriately set according to the desired carbonation rate, and is not particularly limited. The upper limit of the number of units may be, for example, 60 or less, or 50 or less.
[0065] The supply amount Y of carbon dioxide in the carbon dioxide supplying step is appropriately changed depending on the relationship with the slurry flow rate X in the slurry supplying step, so is not limited in general, but is preferably, for example, about 100 ml / min to 2000 ml / min.
[0066] In the manufacturing method disclosed herein, the ratio (Y / X) of the amount of carbon dioxide supplied Y in the carbon dioxide supplying step to the flow rate X of the slurry in the slurry supplying step is preferably less than 1. This allows the supplied carbon dioxide to react with calcium hydroxide in the slurry without loss and be suitably fixed as calcium carbonate. The ratio (Y / X) of the amount of carbon dioxide supplied Y to the flow rate X of the slurry is preferably, for example, 0.91 or less, and may be 0.83 or less. From the viewpoint of manufacturing efficiency, the ratio (Y / X) of the amount of carbon dioxide supplied Y to the flow rate X of the slurry is preferably 0.1 or more, and more preferably 0.27 or more.
[0067] Although not particularly limited, in the carbon dioxide supplying step, it is preferable to supply carbon dioxide as fine bubbles having an average particle size of 100 μm or less, including ultrafine bubbles of less than 1 μm, which can improve the stirring force and the contact specific surface area, and can cause the slurry containing calcium hydroxide to react with carbon dioxide in a short time.
[0068] In the carbon dioxide supply step, the supply pressure (MPa) of carbon dioxide may be set to a supply pressure that easily generates ultrafine bubbles as described above. For example, the supply pressure of carbon dioxide is preferably 0.01 MPa or more and 0.8 MPa or less, more preferably 0.04 MPa or more and 0.6 MPa or less, and particularly preferably 0.06 MPa or more and 0.4 MPa or less, in terms of the pressure difference between the pressure in the piping (fine bubble generating tube) and the pressure in the distilled water in the fine bubble generating tube of the fine bubble generating device, which is set to 0 in a bubble point test.
[0069] In the slurry recovery step, the slurry containing the generated calcium carbonate is recovered. For example, the slurry supplied from the connection line 140 can be temporarily stored in the recovery tank 132 to recover the slurry. As described above, in the carbon dioxide supply step, carbon dioxide is blown in as fine bubbles and immediately mixed using the static mixer 30, so that the reaction between calcium hydroxide in the slurry and carbon dioxide is almost complete. Therefore, even if the slurry is recovered in the open recovery tank 132 in the slurry recovery step, carbon dioxide is hardly released to the outside. Therefore, carbon dioxide can be suitably fixed as carbonate (calcium carbonate) by a simple method. Calcium carbonate can be obtained by drying and filtering the slurry recovered in the slurry recovery step. Such calcium carbonate can be used in industries such as pigments, paints, rubber, and paper.
[0070] The manufacturing method disclosed herein may further include a second carbon dioxide supplying step of supplying carbon dioxide in a step downstream of the slurry recovery step. This can further improve the carbonation rate. This step can be carried out by blowing in carbon dioxide using a conventionally known method. In this case, it is preferable to use exhaust gas discharged from a factory or the like as the carbon dioxide gas to be blown in. This can further reduce the amount of carbon dioxide emitted into the atmosphere. When exhaust gas is used as the carbon dioxide gas, it is preferable to use gas from which dust has been removed using a filter or the like.
[0071] According to the above-mentioned configuration, carbon dioxide can be suitably fixed as calcium carbonate by passing the carbon dioxide through the fine bubble generator 20 and the static mixer 30 two or more times. Therefore, the amount of carbon dioxide fixed as calcium carbonate can be calculated by measuring the amount of carbon dioxide supplied in the carbon dioxide supplying step. In other words, according to the production method disclosed herein, it is also possible to clearly indicate the extent to which carbon dioxide has been fixed as calcium carbonate.
[0072] [Test example] Hereinafter, examples of the technology disclosed herein will be described, but it is not intended that the technology disclosed herein be limited to those shown in these examples.
[0073] 1. First test <Comparative Example 1> First, an in-line type ceramic fine bubble generator (manufactured by Noritake Company Limited, average pore size: 3.4 μm, inner diameter: 3 mm, length (L): 100 mm) and a static mixer (M6-12R manufactured by Noritake Company Limited, number of elements: 12, inner diameter: 6 mm) were prepared. Next, a supply tank for storing a slurry containing calcium hydroxide, a fine bubble generator, a static mixer, and a recovery tank for recovering the slurry that had reacted with carbon dioxide were connected by a connection line. At this time, the static mixer was connected downstream of the fine bubble generator along the flow direction of the slurry. In Comparative Example 1, a device having one unit consisting of one fine bubble generator and one static mixer was constructed. Next, 3 L of 1 mol / L calcium hydroxide slurry was prepared and the slurry was put into a cylindrical supply tank. The slurry was stirred with a propeller-type agitator to prevent precipitation in the supply tank. The pH of the calcium hydroxide slurry before the reaction was about 12.55 to 12.6, and the temperature was 20°C to 22°C. Then, the liquid-transfer pump was operated to transfer the slurry stored in the supply tank. At this time, the flow rate X of the slurry to be transferred was controlled to be 1400 ml / min (the flow rate in the fine bubble generating tube was 3.3 m / s). In addition, 100% carbon dioxide gas was supplied to the fine bubble generating device prepared above while controlling the supply amount Y of the carbon dioxide to be 1270 ml / min, and fine bubbles containing carbon dioxide were blown into the slurry. The supply pressure of carbon dioxide was controlled to be 0.285 MPa to 0.290 MPa, and the differential pressure with the inside of the pipe where ultra-fine bubbles are easily generated was maintained. The liquid transfer and injection were carried out for 2 minutes. The slurry that had reacted with carbon dioxide was collected in a sealed recovery tank equipped with a safety valve. This safety valve is a mechanism for releasing gas so that pressure does not increase due to the introduction of the slurry. After the supply of the slurry was stopped, the recovery tank was kept in a completely sealed state, and it was confirmed that there was no increase in pressure inside the container due to carbon dioxide escaping into the gas phase inside the tank.
[0074] <Examples 1 to 3> In Examples 1 to 3, 10 L of 1 mol / L calcium hydroxide slurry was prepared. In addition, the number of units, where one unit is composed of one fine bubble generator and one static mixer, and the supply pressure of carbon dioxide were changed as shown in Table 1. Except for these, calcium carbonate was produced in the same manner as in Comparative Example 1.
[0075] <Comparative Example 2> In Comparative Example 2, a static mixer having 24 elements was used. The flow rate X of the slurry was controlled to 915 ml / min (flow rate in the fine bubble generating tube was 2.16 m / s), and the supply rate Y of carbon dioxide gas was controlled to 730 ml / min. The supply pressure of carbon dioxide was controlled to 0.370 MPa to 0.375 MPa, and the differential pressure with the inside of the pipe where ultrafine bubbles are easily generated was maintained. Except for these, calcium carbonate was produced in the same manner as in Comparative Example 1.
[0076] <Examples 4 to 6> In Examples 4 to 7, when one unit is constituted by one fine bubble generator and one static mixer, the number of units and the supply pressure of carbon dioxide were changed as shown in Table 1. Except for these, calcium carbonate was produced in the same manner as in Comparative Example 2.
[0077] <Reference example> In the reference examples, the number of units, where one unit is composed of one fine bubble generator and one static mixer, and the supply pressure of carbon dioxide were changed as shown in Table 1. Except for these, calcium carbonate was produced in the same manner as in Comparative Example 2. In the reference example, in order to achieve a carbonation rate of 100%, carbon dioxide was blown in at a rate greater than the stoichiometric ratio of calcium carbonate. In the reference example, when the tank was completely sealed after the supply of the slurry was stopped, a slight increase in the pressure inside the tank was confirmed due to the unreacted carbon dioxide being released into the gas phase inside the tank.
[0078] <Measurement of carbonation rate> The product (slurry) of each example was collected and dried, and the carbonation rate (%) was measured using a thermogravimetric analyzer (Thermogravimetry-Differential Thermal Analysis: TG-DTA) manufactured by Rigaku Corporation. The theoretical value (%) of the carbonation rate was calculated based on the amount of carbon dioxide gas injected, and the difference from the theoretical value (%) was calculated. The results are shown in Table 1.
[0079] <Measurement of carbon dioxide concentration> For Comparative Example 1 and Example 3, the gas discharged from the safety valve of the recovery tank was analyzed using a thermal conductivity detector type gas chromatograph (manufactured by Shimadzu Corporation). In Comparative Example 1, the CO2 concentration did not increase during the test. In Example 3, the CO2 concentration increased slightly.
[0080] [Table 1]
[0081] As shown in Table 1, the carbonation rate is less than 5% in Comparative Examples 1 and 2 in which the number of units is 1, whereas the carbonation rate is 5% or more in Examples 1 to 6 in which the number of units is 2 or more. From the viewpoint of production efficiency, it is preferable to have 2 or more units of a fine bubble generator and a static mixer. By using a production device having 2 or more units of a fine bubble generator and a static mixer, calcium carbonate can be continuously produced with almost no carbon dioxide released to the outside.
[0082] Also, as shown in Table 1, in Examples 3 and 6, in which the number of units exceeds 10, a high carbonation rate can be achieved. In particular, in Example 3, a carbonation rate of nearly 50% can be achieved, and the difference from the theoretical value is less than 1%.
[0083] In addition, in Comparative Example 1, Example 3, Example 6, and Reference Example, the pH of the slurry was confirmed. The pH of the slurry was measured in a stable state by calculating the piping volume and removing the initial outflow slurry equivalent to the piping volume. In Comparative Example 1 and Example 3, the pH was about 12.55 to 12.6 and did not change. In Example 6, the pH was about 11.9 to 12.1. In the Reference Example, the pH was 6.5. In Example 6 and Reference Example, where the carbonation rate was over 90%, the pH was clearly lower than that of the unreacted slurry.
[0084] 2. Second Exam <Example 11> First, an in-line type ceramic fine bubble generator (manufactured by Noritake Company Limited, average pore size: 3.4 μm, inner diameter: 3 mm, length (L): 100 mm) and a static mixer (M6-24R manufactured by Noritake Company Limited, number of elements: 24, inner diameter: 6 mm) were prepared. Next, a supply tank for storing a slurry containing calcium hydroxide, a fine bubble generator, a static mixer, and a recovery tank for recovering the slurry that had reacted with carbon dioxide were connected by a connection line. At this time, the static mixer was connected downstream of the fine bubble generator along the flow direction of the slurry. In Example 11, a device having six units was constructed, with one fine bubble generator and one static mixer as one unit. Next, 10 L of 2 mol / L calcium hydroxide slurry was prepared and the slurry was put into a cylindrical supply tank. The slurry was stirred with a propeller-type agitator to prevent precipitation in the supply tank. The pH of the calcium hydroxide slurry before the reaction was about 12.55 to 12.6, and the temperature was 20°C to 22°C. Next, the suction pump was operated to send the slurry stored in the supply tank. At this time, the flow rate X of the slurry to be sent was controlled to be 2010 ml / min (the flow rate in the fine bubble generating tube was 4.74 m / s). Next, 100% carbon dioxide gas was supplied to the fine bubble generating device prepared above while controlling the supply amount Y of the carbon dioxide to be 800 ml / min, and fine bubbles containing carbon dioxide were blown into the slurry. The supply pressure of carbon dioxide was controlled to be 0.37 MPa to 0.39 MPa, and the differential pressure with the inside of the pipe where ultra-fine bubbles are easily generated was maintained. The liquid transfer and injection were carried out for 2 minutes. The slurry that had reacted with carbon dioxide was collected in a sealed recovery tank equipped with a safety valve. This safety valve is a mechanism for releasing gas so that pressure does not increase due to the introduction of the slurry. After the supply of the slurry was stopped, the recovery tank was kept in a completely sealed state, and it was confirmed that there was no increase in pressure inside the container due to carbon dioxide escaping into the gas phase inside the tank.
[0085] <Examples 12 and 13> In Examples 12 and 13, when one unit is constituted by one fine bubble generator and one static mixer, the number of units, the supply amount Y of carbon dioxide, and the supply pressure of carbon dioxide were changed as shown in Table 2. Except for these, calcium carbonate was produced in the same manner as in Example 11.
[0086] <Example 14> In Example 14, a device having 30 units each consisting of one fine bubble generator and one static mixer was constructed. The carbon dioxide supply amount Y was set to 600 ml / min, and the carbon dioxide supply pressure was controlled to 0.37 MPa to 0.48 MPa. In Example 14, the recovery tank was opened, and the reacted slurry was put in, and the tank was immediately closed with a lid. It was confirmed that in Example 14, there was no increase in the pressure inside the container due to carbon dioxide being released into the gas phase in the tank. Except for these, calcium carbonate was produced in the same manner as in Example 11.
[0087] <Example 15> In Example 15, 10 L of 0.25 mol / L calcium hydroxide slurry was prepared. A static mixer with 12 elements was used, and the number of units was 14 when one unit consisted of one fine bubble generator and one static mixer. Furthermore, the slurry flow rate X was 1650 ml / min (flow rate in the fine bubble generating tube was 3.89 m / s), the carbon dioxide supply amount Y was 450 ml / min, and the carbon dioxide supply pressure was controlled to 0.28 MPa to 0.35 MPa. Calcium carbonate was produced in the same manner as in Example 11 except for these.
[0088] <Example 16> In Example 16, 10 L of 3 mol / L calcium hydroxide slurry was prepared. In addition, the number of units was 30, with one microbubble generator and one static mixer being considered as one unit. Furthermore, the slurry flow rate X was 550 ml / min (flow rate in the microbubble generating tube was 1.3 m / s), the carbon dioxide supply amount Y was 950 ml / min, and the carbon dioxide supply pressure was controlled to 0.37 MPa to 0.46 MPa. Except for these, calcium carbonate was produced in the same manner as in Example 11.
[0089] <Examples 17 and 18> In Examples 17 and 18, an in-line type ceramic fine bubble generator was used in which the average pore size of the fine bubble generating tube was 1.3 μm, and a static mixer having 12 elements was used. In addition, the number of units, when one fine bubble generator and one static mixer are regarded as one unit, the slurry concentration, the slurry flow rate X, the carbon dioxide supply amount Y, and the carbon dioxide supply pressure were each changed as shown in Table 2. Except for these, calcium carbonate was produced in the same manner as in Example 11.
[0090] <Examples 19 to 21> In Examples 19 to 21, an in-line type ceramic fine bubble generator was used in which the average pore size of the fine bubble generating tube was 10 μm, and a static mixer with 12 elements was used. In Examples 19 to 21, 10 L of 2 mol / L calcium hydroxide slurry was prepared. In addition, the number of units, when one fine bubble generator and one static mixer are considered as one unit, the flow rate X of the slurry, the supply amount Y of carbon dioxide, and the supply pressure of carbon dioxide were changed as shown in Table 2. Except for these, calcium carbonate was produced in the same manner as in Example 11.
[0091] <Examples 22 to 25> In Examples 22 to 25, an in-line type ceramic fine bubble generator was used in which the average pore size of the fine bubble generating tube was 10 μm, and a static mixer with 24 elements was used. In Examples 22 to 25, 10 L of 1 mol / L calcium hydroxide slurry was prepared. The number of units, when one fine bubble generator and one static mixer are considered as one unit, the flow rate X of the slurry, the supply amount Y of carbon dioxide, and the supply pressure of carbon dioxide were changed as shown in Table 2. Except for these, calcium carbonate was produced in the same manner as in Example 11.
[0092] <Example 26> In Example 26, an in-line type ceramic fine bubble generator was used, in which the average pore size of the fine bubble generating tube was 10 μm, and a static mixer was used, in which the number of elements was 18 and the inner diameter was 10 mm. In Example 26, 10 L of 4 mol / L calcium hydroxide slurry was prepared. The number of units, in which one fine bubble generator and one static mixer constitute one unit, the flow rate X of the slurry, the supply amount Y of carbon dioxide, and the supply pressure of carbon dioxide were each changed as shown in Table 2. Except for these, calcium carbonate was produced in the same manner as in Example 11.
[0093] <Measurement of carbonation rate> The product (slurry) of each example was collected and dried, and then the carbonation rate (%) was measured using the above-mentioned thermogravimetric analyzer (TG-DTA). In addition, the theoretical value (%) of the carbonation rate was calculated based on the amount of carbon dioxide gas injected, and the difference from the theoretical value (%) was calculated. The results are shown in Table 2. For comparison, the results of Comparative Example 1 are also shown in Table 2.
[0094] [Table 2]
[0095] As shown in Table 2, the carbonation rate is less than 5% in Comparative Example 1 in which the number of units is 1, whereas the carbonation rate is 5% or more in Examples 11 to 26 in which the number of units is 2 or more. From the viewpoint of production efficiency, it is preferable to have two or more units of a fine bubble generator and a static mixer. By using a production apparatus having two or more units of a fine bubble generator and a static mixer, calcium carbonate can be continuously produced with almost no carbon dioxide released to the outside.
[0096] As shown in Table 2, it can be seen that the carbonation rate is high in Examples 13 to 18, 20, 21, and 23 to 26, in which the number of units exceeds 10 units. From the viewpoint of further improving the carbonation rate, it is preferable that the number of units exceeds 10 units. In addition, it can be seen that in Example 16, in which the ratio (Y / X) of the gas supply amount Y to the slurry flow rate X is 1.73, the carbonation rate is good, but the difference from the theoretical value is large. In Example 16, the gas supply amount Y tends to be excessive relative to the slurry flow rate X, causing flooding, but the carbonation rate was good due to the stirring effect of the static mixer. From these results, in order to improve the carbonation rate and reduce the difference from the theoretical value, it is preferable to adjust the ratio (Y / X) of the gas supply amount Y to the slurry flow rate X to be less than 1.
[0097] In Examples 19 to 26, in which the average pore diameter of the fine bubble generator was 10 μm, ultra-fine bubbles were able to be generated effectively even at a lower carbon dioxide supply pressure, compared to Examples 11 to 16, in which the average pore diameter of the fine bubble generator was 3.4 μm, and Examples 17 and 18, in which the average pore diameter was 1.3 μm.
[0098] In Example 26, the slurry concentration was 4 mol / L, so the viscosity of the slurry was high. In Example 26, the viscosity tended to increase as the reaction proceeded, and clogging was likely to occur in the static mixer. When the slurry concentration is high, it is considered better to increase the inner diameter of the static mixer or the inner diameter of the microbubble generator.
[0099] In Example 14, the reaction slurry was poured into the recovery tank with the tank open, and the tank was immediately closed and sealed. Even in this case, no pressure rise was observed in the tank. Therefore, it is considered that the injected carbon dioxide gas is almost dissolved in the slurry in the container, and is hardly released into the gas phase (part where no slurry exists) in the tank. For example, by setting the carbonation rate to about 40% or less, it is presumed that calcium carbonate can be continuously produced without releasing carbon dioxide to the outside by simply connecting the fine bubble generator and the static mixer between existing open tanks. According to the configuration of the fine bubble generator and the static mixer disclosed herein, a system can be constructed that can clearly display the amount of fixed carbon dioxide.
[0100] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.
[0101] The technology disclosed herein includes the following items 1 to 13. The following items 1 to 13 are not limited to the above-described embodiment.
[0102] Item 1 relates to a calcium carbonate manufacturing apparatus. The calcium carbonate manufacturing apparatus in Item 1 comprises: a slurry supply unit that supplies a slurry containing calcium hydroxide; A carbon dioxide supply unit that supplies carbon dioxide to the slurry in the form of fine bubbles; a slurry recovery unit that recovers a slurry containing the produced calcium carbonate; A connection line connecting the slurry supply unit, the carbon dioxide supply unit, and the slurry recovery unit; Equipped with The carbon dioxide supply unit is The apparatus includes a microbubble generator disposed upstream and a static mixer disposed downstream along a flow direction of the slurry, When one microbubble generator and one static mixer are regarded as one unit, at least two such units are provided along the flow direction of the slurry.
[0103] Item 2 is the manufacturing apparatus according to item 1, The fine bubble generating device is provided with a fine bubble generating tube made of a porous body having fine pores.
[0104] Item 3 is the manufacturing apparatus according to item 2, In the microbubble generating device, the micropores have an average pore size of 0.5 μm or more and 10 μm or less.
[0105] Item 4 is a manufacturing apparatus according to any one of items 1 to 3, The fine bubble generating device is Fine bubbles are generated so that the average particle size is 100 μm or less, and ultra-fine bubbles having a particle size of at least less than 1 μm are included.
[0106] Item 5 is a manufacturing apparatus according to any one of items 1 to 4, The slurry supply unit has an open supply tank, The slurry recovery section has an open recovery tank, The supply tank, the fine bubble generator, the static mixer, and the recovery tank are connected by the connection lines.
[0107] Item 6 is a manufacturing apparatus according to any one of items 1 to 5, Each of the microbubble generating devices is connected to a carbon dioxide supply line for supplying carbon dioxide, When the flow rate of the slurry flowing through the connection line is defined as a flow rate X, and the supply amount of carbon dioxide supplied to the carbon dioxide supply line is defined as a supply amount Y, The ratio (Y / X) of the supply amount Y to the flow rate X is less than 1.
[0108] Item 7 is a manufacturing apparatus according to any one of items 1 to 6, When one microbubble generator and one static mixer are regarded as one unit, the number of such units is from 2 to 50 in the flow direction of the slurry.
[0109] Item 8 relates to a part used in the manufacturing apparatus according to any one of items 1 to 7. The part in item 8 is: A micro-bubble generator disposed upstream along the flow direction of the slurry; one static mixer located downstream; A connection line connecting the fine bubble generating device and the static mixer; Equipped with.
[0110] Item 9 relates to a method for producing calcium carbonate. The method for producing calcium carbonate in Item 9 is as follows: providing a slurry comprising calcium hydroxide; supplying carbon dioxide to the slurry in the form of fine bubbles; A step of recovering the produced slurry containing calcium carbonate; Including, In the carbon dioxide supply step, The method is characterized in that, when one unit is composed of one fine bubble generator arranged upstream along the flow direction of the slurry and one static mixer arranged downstream, the slurry is passed through the unit at least two times.
[0111] Item 10 is the production method according to item 9, When the flow rate of the slurry in the slurry supplying step is a flow rate X and the supply amount of carbon dioxide in the carbon dioxide supplying step is a supply amount Y, The flow rate of the slurry and the supply amount of carbon dioxide are adjusted so that the ratio of the supply amount Y to the flow rate X is less than 1.
[0112] Item 11 is the production method according to item 9 or 10, The concentration of calcium hydroxide in the slurry containing calcium hydroxide is 0.1 mol / L or more and 4 mol / L or less.
[0113] Item 12 is a production method according to any one of items 9 to 11, In the carbon dioxide supply step, Carbon dioxide is supplied in the form of fine bubbles having an average particle size of 100 μm or less, including ultra-fine bubbles having a particle size of at least less than 1 μm.
[0114] Item 13 is a production method according to any one of items 9 to 12, The method further includes a second carbon dioxide supplying step of supplying carbon dioxide to the slurry recovered in the slurry recovery step. [Explanation of symbols]
[0115] 20 Microbubble generator 21 Microbubble generating tube 21a Upstream end 21b Downstream end 22 Base material part 23a Upstream support part 23b Downstream support part 24 Torso 25 Slurry inlet 26 Slurry outlet 27 Carbon dioxide inlet 30 Static Mixer 32 Conduit 34 Mixing element 34a Right Element 34b Left element 100 Manufacturing equipment 110 Slurry supply section 111 Supply Line 112 Valve 113 Supply Tank 114 Liquid delivery pump 115 Mixer 120 Carbon dioxide supply unit 122 Gas storage section 124 Carbon Dioxide Supply Line 126 Pressure Regulating Valve 128 Needle Valve 130 Slurry recovery section 132 Recovery Tank 134 Recovery Line 136 Valve 138 Mixer 140 Connection Line 142a Three-way valve 142b Three-way valve 144 Valve
Claims
1. An apparatus for producing calcium carbonate, comprising: a slurry supply unit that supplies a slurry containing calcium hydroxide; A carbon dioxide supply unit that supplies carbon dioxide to the slurry in the form of fine bubbles; a slurry recovery unit that recovers a slurry containing the produced calcium carbonate; A connection line connecting the slurry supply unit, the carbon dioxide supply unit, and the slurry recovery unit; Equipped with The carbon dioxide supply unit is The apparatus includes a microbubble generator disposed upstream and a static mixer disposed downstream along a flow direction of the slurry, The calcium carbonate production apparatus has at least two units, each unit being composed of one fine bubble generator and one static mixer, arranged along the flow direction of the slurry.
2. 2. The manufacturing apparatus according to claim 1, wherein the microbubble generating device comprises a microbubble generating tube made of a porous body having micropores.
3. The manufacturing apparatus according to claim 2 , wherein the micropores in the microbubble generating device have an average pore size of 0.5 μm or more and 10 μm or less.
4. The fine bubble generating device is 2. The manufacturing apparatus according to claim 1, wherein fine bubbles are generated so as to include ultra-fine bubbles having an average particle size of 100 μm or less and at least an average particle size of less than 1 μm.
5. The slurry supply unit has an open supply tank, The slurry recovery section has an open recovery tank, The manufacturing apparatus according to claim 1 , wherein the supply tank, the fine bubble generator, the static mixer, and the recovery tank are connected by the connection line.
6. Each of the microbubble generating devices is connected to a carbon dioxide supply line for supplying carbon dioxide, When the flow rate of the slurry flowing through the connection line is defined as a flow rate X, and the supply amount of carbon dioxide supplied to the carbon dioxide supply line is defined as a supply amount Y, The manufacturing apparatus according to claim 1 , wherein a ratio (Y / X) of a supply amount Y to a flow rate X is less than 1.
7. 2. The manufacturing apparatus according to claim 1, wherein when one micro-bubble generator and one static mixer are regarded as one unit, the apparatus has 2 to 50 such units along the flow direction of the slurry.
8. A part used in the manufacturing apparatus according to claim 1, One micro-bubble generating device is disposed upstream along the flow direction of the slurry; one static mixer disposed downstream; A connection line connecting the fine bubble generating device and the static mixer; A part that includes:
9. A method for producing calcium carbonate, comprising the steps of: providing a slurry comprising calcium hydroxide; supplying carbon dioxide to the slurry in the form of fine bubbles; A step of recovering the produced slurry containing calcium carbonate; Including, In the carbon dioxide supply step, The method for producing calcium carbonate, characterized in that, when a unit is constituted of one fine bubble generator arranged on the upstream side along the flow direction of the slurry and one static mixer arranged on the downstream side, the slurry is passed through the unit at least two times.
10. When the flow rate of the slurry in the slurry supplying step is a flow rate X and the supply amount of carbon dioxide in the carbon dioxide supplying step is a supply amount Y, The method according to claim 9 , further comprising adjusting a flow rate of the slurry and a supply rate of the carbon dioxide so that a ratio of the supply rate Y to the flow rate X is less than 1.
11. The method according to claim 9, wherein the concentration of calcium hydroxide in the slurry containing calcium hydroxide is 0.1 mol / L or more and 4 mol / L or less.
12. In the carbon dioxide supply step, The method according to claim 9, wherein the carbon dioxide is supplied in the form of fine bubbles having an average particle size of 100 μm or less, including ultrafine bubbles having a particle size of at least less than 1 μm.
13. The method according to claim 9 , further comprising a second carbon dioxide supplying step of supplying carbon dioxide to the slurry recovered in the slurry recovery step.
Citation Information
Patent Citations
JP1974061074A
Method for producing light calcium carbonate
JP3995761B2
Method for producing inorganic carbonates
JP6742867B2