Composition for forming organic film, method for forming organic film, and patterning process

The composition with specific structural units and a fluorine content addresses the issues of in-plane uniformity and embedding properties, enhancing semiconductor manufacturing by suppressing humps and ensuring precise pattern transfer.

JP2024154795AActive Publication Date: 2024-10-31SHIN ETSU CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023068874
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-31
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

Existing organic film compositions used in semiconductor manufacturing face challenges in achieving in-plane uniformity and embedding properties, leading to hump formation during the EBR process, which can cause defects in the dry etching process.

Method used

A composition comprising an organic film-forming resin, specific structural units represented by general formulas (I), (II), and (III), and a solvent, with a fluorine content of 5% to 16% by mass, forming a random copolymer to enhance film uniformity and suppress hump formation.

Benefits of technology

The composition achieves excellent in-plane uniformity and embedding properties, effectively suppressing hump formation during the EBR process, enabling precise pattern transfer in semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154795000102
    Figure 2024154795000102
  • Figure 2024154795000103
    Figure 2024154795000103
  • Figure 2024154795000104
    Figure 2024154795000104
Patent Text Reader

Abstract

To provide a composition for forming an organic film that has excellent film-formability on a substrate and filling characteristics, and that inhibits humps in EBR process; and a method for forming an organic film and a patterning process, each using this composition.SOLUTION: The present invention provides a composition comprising: a resin for forming an organic film; a polymer having a structural unit represented by the formula (I) and a structural unit represented by the formula (II); and a solvent. The structural units of the formulae (I) and (II) form a random copolymer, and the polymer has a fluorine content of 5 mass% to 16 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for forming an organic film for forming an organic film for a multilayer resist for microfabrication in the manufacture of a semiconductor device or the like, or an organic film for planarization in the manufacture of a semiconductor device or the like, a method for forming an organic film using the composition, and a method for forming a pattern using the composition. [Background technology]

[0002] In recent years, with the increasing integration and speed of semiconductor elements, there is a demand for finer pattern rules. In the lithography using light exposure, which is currently used as a general-purpose technology, various technological developments are being made to fabricate finer and more accurate patterns for the light source used.

[0003] As a light source for lithography used in forming resist patterns, light exposure using mercury lamps' g-line (436 nm) or i-line (365 nm) light sources is widely used in areas with low integration. On the other hand, in areas with high integration and requiring finer detail, lithography using shorter wavelengths such as KrF excimer lasers (248 nm) and ArF excimer lasers (193 nm) has also been put to practical use, and for the most advanced generation requiring even finer detail, extreme ultraviolet (EUV, 13.5 nm) lithography is approaching practical use.

[0004] As the resist pattern becomes thinner, it is well known that the ratio of the pattern height to the pattern line width (aspect ratio) increases in the single-layer resist method used as a typical resist pattern forming method, and the pattern collapses due to the surface tension of the developer during development. Therefore, it is known that a multi-layer resist method in which films with different dry etching characteristics are laminated to form a pattern with a high aspect ratio on a stepped substrate is superior, and a two-layer resist method (Patent Document 1) that combines a photoresist layer made of a silicon-containing photosensitive polymer with an organic polymer containing carbon, hydrogen, and oxygen as main constituent elements, such as a novolac polymer, as well as a three-layer resist method (Patent Document 2) that combines a photoresist layer made of an organic photosensitive polymer used in the single-layer resist method with an intermediate layer made of a silicon-based polymer or a silicon-based CVD film and an organic polymer underlayer have been developed.

[0005] In this three-layer resist method, for example, an organic film made of novolac or the like is uniformly formed on a substrate to be processed as a resist underlayer film, a silicon-containing film is formed on the organic film as a resist middle film, and a normal organic photoresist film is formed on the organic film as a resist upper layer film. For dry etching with fluorine-based gas plasma, the organic resist upper layer film has a good etching selectivity to the silicon-containing resist middle film, so the resist pattern is transferred to the silicon-containing resist middle film by using dry etching with fluorine-based gas plasma. According to this method, even if a resist composition that is difficult to form a pattern with a sufficient thickness for directly processing the substrate to be processed or a resist composition that does not have sufficient dry etching resistance for processing the substrate is used, a pattern can be transferred to the silicon-containing film, and then, by performing pattern transfer using dry etching with oxygen-based gas plasma, a novolac film pattern with sufficient dry etching resistance for processing can be obtained.

[0006] Although many technologies for the organic underlayer film as described above are already known (e.g., Patent Document 3), the recent progress in miniaturization has led to an increasing need for excellent filling properties in addition to dry etching properties. There is a need for organic underlayer film materials that can be uniformly formed on the underlying substrate to be processed even on substrates with complex shapes and materials, and that have filling properties that enable filling the required pattern without voids.

[0007] The organic underlayer film described above is formed using a coater / developer capable of performing processes such as spin coating, EBR, and baking when manufacturing semiconductor substrates. The EBR (Edge Bead Removal) process is a process in which, after a coating is formed on a substrate (wafer) by spin coating, the coating on the edge of the substrate is removed with a remover in order to prevent contamination of the substrate transport arm of the coater / developer. The remover used in the EBR process is a mixture (30% by mass:70% by mass) of propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether, which is widely used in the EBR process of resist films, silicon-containing intermediate films, and organic underlayer films.

[0008] The remover used in the EBR process can cause the outer periphery of the organic underlayer film to become thick (a hump). Since humps can cause defects in the dry etching process used in the above-mentioned substrate processing, there is a demand for organic underlayer films that suppress humps. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 6-118651 [Patent Document 2] Patent No. 4355943 [Patent Document 3] JP 2004-205685 A Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a composition for forming an organic film that has excellent film-forming properties (in-plane uniformity) and filling properties on a substrate (wafer) and that suppresses humps during an EBR process, and a method for forming an organic film and a method for forming a pattern using the composition. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention provides a composition for forming an organic film, the composition comprising a resin for forming an organic film, a polymer containing a structural unit represented by the following general formula (I) and at least one of a structural unit represented by the following general formula (II) and a structural unit represented by the following general formula (III), and a solvent, wherein the structural unit represented by the following general formula (I) and at least one of the structural units represented by the following general formula (II) and a structural unit represented by the following general formula (III) form a random copolymer, and the polymer has a fluorine content of 5% by mass to 16% by mass. [ka] (In the formula, R 1 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 2 is an organic group having 1 to 20 carbon atoms and containing a fluorine atom, which does not contain a sulfonyl group or an amino group. [ka] (In the formula, R 3 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 4 and R 5 each represents a divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched; R 6 is a hydrogen atom or an alkyl group or a phenyl group having 1 to 4 carbon atoms, m1 is 0 to 23, n1 is 0 to 23, and 23≧m1+n1≧2. [ka] (In the formula, R 7and R 8 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 9 and R 10 each represents a divalent alkylene group having 1 to 4 carbon atoms which may be linear or branched, m2 represents 0 to 23, n2 represents 0 to 23, and 23≧m2+n2≧2.

[0012] Such a composition for forming an organic film makes it possible to form an organic film that is excellent in in-plane uniformity and filling characteristics, and in which the formation of humps caused by the remover in the EBR process is suppressed.

[0013] In addition, R of the structural unit represented by the general formula (I) of the polymer 2 It is preferable that the organic film-forming composition contains a structure represented by the following general formula (IV) or (V). [ka] (In the formula, * indicates the bond position.)

[0014] A composition for forming an organic film containing such a polymer is preferable because the formed organic film has better in-plane uniformity.

[0015] In the composition for forming an organic film, the resin for forming an organic film is preferably a resin having an aromatic skeleton.

[0016] Resins having such an aromatic skeleton are preferable because they have better etching resistance, optical properties, heat resistance, and the like.

[0017] In addition, the composition for forming an organic film preferably contains the polymer in an amount of 0.01 to 5 parts by mass based on 100 parts by mass of the resin for forming an organic film.

[0018] A composition for forming an organic film containing the polymer in such an amount is preferable because the formed organic film has better in-plane uniformity.

[0019] In addition, the composition for forming an organic film preferably contains the resin for forming an organic film in an amount of 10 to 40 parts by mass, based on 100 parts by mass of the composition for forming an organic film.

[0020] In the case of such a content of the resin for forming an organic film, the composition for forming an organic film can have excellent in-plane uniformity and filling properties, and therefore can be preferably used.

[0021] The effect of the present invention can be fully achieved with the above-mentioned organic film-forming composition.

[0022] The present invention also provides a method for forming an organic film used in the manufacturing process of a semiconductor device, which comprises spin-coating the above-mentioned composition for forming an organic film on a substrate to be processed, and heat-treating the substrate coated with the composition for forming an organic film at a temperature of 100°C to 600°C for a period of 10 seconds to 600 seconds, thereby forming a cured film.

[0023] According to the organic film forming method of the present invention, the above-mentioned composition for forming an organic film can be spin-coated to fill a pattern having a complex shape on a substrate to be processed, and an organic film having excellent in-plane uniformity can be formed. The organic film obtained by the above-mentioned method is preferable because it can be removed from the edge of the organic film while suppressing humps in the EBR process.

[0024] The present invention also provides a pattern forming method, which includes forming an organic film on a workpiece using the above-mentioned organic film-forming composition, forming a resist intermediate film on the organic film using a resist intermediate film material containing silicon atoms, forming a resist upper layer film on the resist intermediate film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the resist intermediate film by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.

[0025] In this way, a pattern formation method by a three-layer resist process using the organic film-forming composition of the present invention, a silicon-containing resist intermediate film, and a resist top layer film can be provided. Such a pattern formation method of the present invention makes it possible to transfer and form the circuit pattern of the resist top layer film onto a workpiece with high precision.

[0026] The present invention also provides a pattern forming method, which comprises forming an organic film on a workpiece using the above-mentioned organic film-forming composition, forming a resist intermediate film on the organic film using a resist intermediate film material containing silicon atoms, forming an organic antireflective film or adhesive film on the resist intermediate film, forming a resist upper layer film on the organic antireflective film or adhesive film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film or adhesive film and the resist intermediate film by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.

[0027] In this way, a pattern formation method by a four-layer resist process using the organic film-forming composition of the present invention, a silicon-containing resist intermediate film, an organic antireflective film or adhesion film, and a resist top layer film can be provided. Such a pattern formation method of the present invention makes it possible to transfer and form the circuit pattern of the resist top layer film onto a workpiece with high precision.

[0028] The present invention also provides a pattern formation method, which comprises forming an organic film on a workpiece using the above-mentioned composition for forming an organic film, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film, forming a resist upper layer film on the inorganic hard mask using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the inorganic hard mask by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.

[0029] In this way, a pattern formation method by a three-layer resist process using the organic film-forming composition of the present invention, an inorganic hard mask, and a resist top layer film can be provided. Such a pattern formation method of the present invention makes it possible to transfer and form a circuit pattern of the resist top layer film onto a workpiece with high precision.

[0030] The present invention also provides a pattern forming method, which comprises forming an organic film on a workpiece using the above-mentioned composition for forming an organic film, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film, forming an organic antireflective film or an adhesion film on the inorganic hard mask, forming a resist upper layer film on the organic antireflective film or adhesion film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film or adhesion film and the inorganic hard mask by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic antireflective film or adhesion film and the inorganic hard mask by etching using the inorganic hard mask on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.

[0031] In this way, a pattern formation method by a four-layer resist process using the organic film-forming composition of the present invention, an inorganic hard mask, an organic antireflective film or adhesion film, and a resist top layer film can be provided. Such a pattern formation method of the present invention makes it possible to transfer and form the circuit pattern of the resist top layer film onto a workpiece with high precision.

[0032] Moreover, it is preferable that the inorganic hard mask is formed by a CVD method or an ALD method.

[0033] In the pattern formation method of the present invention, for example, an inorganic hard mask can be formed by such a method.

[0034] In forming the circuit pattern, it is preferable to form the circuit pattern by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination of these.

[0035] In forming the circuit pattern, it is preferable to develop the circuit pattern using an alkali developer or an organic solvent.

[0036] In the pattern forming method of the present invention, such a circuit pattern forming means and developing means can be suitably used.

[0037] It is also preferable that the workpiece is a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.

[0038] The metal constituting the workpiece is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, molybdenum, or an alloy thereof.

[0039] According to the pattern forming method of the present invention, a pattern can be formed by processing the above-mentioned workpiece. Effect of the Invention

[0040] As described above, the present invention can provide an organic film-forming composition that has excellent film-forming properties (in-plane uniformity) and burying properties on a substrate (wafer) and suppresses humps during the EBR process. In addition, since such an organic film-forming composition of the present invention has excellent film-forming properties and burying properties and suppresses humps that occur during the EBR process, it is extremely useful as an organic film material used in multilayer resist processes such as a two-layer resist process, a three-layer resist process using a silicon-containing resist intermediate film or an inorganic hard mask, or a four-layer resist process using a silicon-containing resist intermediate film or an inorganic hard mask and an organic anti-reflective film or an adhesive film, or as an organic film-forming material for manufacturing a semiconductor device. In addition, the organic film-forming method of the present invention can form an organic film with suppressed humps, so that semiconductor elements and the like can be efficiently manufactured. [Brief description of the drawings]

[0041] [Figure 1] 1 is a graph showing the results of measuring the height of a hump using a contact profiler in an example (Comparative ULD-1) of a comparative example of the composition for forming an organic film of the present invention. [Diagram 2] 1 is a graph showing the results of measuring the hump height using a contact profiler for an example (ULD-4) of the composition for forming an organic film of the present invention. [Diagram 3] FIG. 2 is an explanatory diagram of an example of a pattern forming method using a three-layer resist process of the present invention. [Figure 4] FIG. 2 is an explanatory diagram of a method for evaluating embedding characteristics in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] As described above, there has been a demand for the development of a composition for forming an organic film that has excellent film-forming properties (in-plane uniformity) and filling properties on a substrate (wafer) and that suppresses humps during the EBR process.

[0043] Typically, when forming an organic film, a resin for forming the organic film and additives are dissolved in an organic solvent to form a composition, which is then applied by a coater / developer onto a substrate on which structures, wiring, etc. have been formed. The composition is spread as the substrate rotates, the composition at the edges is removed in an EBR process, and the substrate is then baked to form the organic film. If the fluidity of the above composition is insufficient, voids will occur when filling holes or trenches with very high aspect ratios, and if the resin or additives used to form the organic film have poor solubility in the remover used in the EBR process, a hump will occur on the outer periphery of the organic film.

[0044] The present inventors have further conducted intensive studies and have found that a composition for forming an organic film comprising a resin for forming an organic film, a polymer containing a structural unit represented by the following general formula (I) and at least one of a structural unit represented by the following general formula (II) and a structural unit represented by the following general formula (III), and a solvent, wherein the structural unit represented by the following general formula (I) and at least one of the structural units represented by the following general formula (II) and the structural unit represented by the following general formula (III) form a random copolymer, and the polymer has a fluorine content of 5% by mass to 16% by mass, can be blended into the composition for forming an organic film to provide a composition for forming an organic film that is excellent in film-forming properties, high-level embedding properties, and suppression of humps during an EBR process, thereby completing the present invention. [ka] (In the formula, R 1 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 2 is an organic group having 1 to 20 carbon atoms and containing a fluorine atom, which does not contain a sulfonyl group or an amino group. [ka] (In the formula, R3 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 4 and R 5 each represents a divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched; R 6 is a hydrogen atom or an alkyl group or a phenyl group having 1 to 4 carbon atoms, m1 is 0 to 23, n1 is 0 to 23, and 23≧m1+n1≧2. [ka] (In the formula, R 7 and R 8 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 9 and R 10 each represents a divalent alkylene group having 1 to 4 carbon atoms which may be linear or branched, m2 represents 0 to 23, n2 represents 0 to 23, and 23≧m2+n2≧2.

[0045] That is, the present invention relates to a composition for forming an organic film, the composition comprising a resin for forming an organic film, a polymer containing a structural unit represented by the following general formula (I) and at least one of a structural unit represented by the following general formula (II) and a structural unit represented by the following general formula (III), and a solvent, wherein the structural unit represented by the following general formula (I) and at least one of the structural units represented by the following general formula (II) and a structural unit represented by the following general formula (III) form a random copolymer, and the fluorine content of the polymer is 5% by mass to 16% by mass. [ka] (In the formula, R 1 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 2 is an organic group having 1 to 20 carbon atoms and containing a fluorine atom, which does not contain a sulfonyl group or an amino group. [ka] (In the formula, R 3 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 4 and R 5each represents a divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched; R 6 is a hydrogen atom or an alkyl group or a phenyl group having 1 to 4 carbon atoms, m1 is 0 to 23, n1 is 0 to 23, and 23≧m1+n1≧2. [ka] (In the formula, R 7 and R 8 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 9 and R 10 each represents a divalent alkylene group having 1 to 4 carbon atoms which may be linear or branched, m2 represents 0 to 23, n2 represents 0 to 23, and 23≧m2+n2≧2. The fluorine content of the polymer used in the present invention is calculated from the mass ratio of fluorine atoms to the total amount of the raw material monomers used.

[0046] The present invention will be described in detail below, but the present invention is not limited thereto.

[0047] [Composition for organic film formation] The composition for forming an organic film of the present invention comprises a resin for forming an organic film, a polymer containing a structural unit represented by the following general formula (I) and at least one of a structural unit represented by the following general formula (II) and a structural unit represented by the following general formula (III), and a solvent, wherein the structural unit represented by the following general formula (I) and at least one of the structural units represented by the following general formula (II) and (III) form a random copolymer, and the polymer has a fluorine content of 5% by mass to 16% by mass. [ka] (In the formula, R 1 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 2 is an organic group having 1 to 20 carbon atoms and containing a fluorine atom, which does not contain a sulfonyl group or an amino group. [ka] (In the formula, R 3 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 4 and R 5 each represents a divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched; R 6 is a hydrogen atom or an alkyl group or a phenyl group having 1 to 4 carbon atoms, m1 is 0 to 23, n1 is 0 to 23, and 23≧m1+n1≧2. [ka] (In the formula, R 7 and R 8 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 9 and R 10 each represents a divalent alkylene group having 1 to 4 carbon atoms which may be linear or branched, m2 represents 0 to 23, n2 represents 0 to 23, and 23≧m2+n2≧2.

[0048] In the composition for forming an organic film of the present invention, the resin for forming an organic film, the polymer and the solvent may each be used alone or in combination of two or more kinds.

[0049] [A polymer comprising a structural unit represented by general formula (I) and at least one of a structural unit represented by general formula (II) and a structural unit represented by general formula (III), wherein the structural unit represented by general formula (I) and at least one of the structural units represented by general formula (II) and (III) form a random copolymer, and the fluorine content of the polymer is 5% by mass to 16% by mass] The organic film-forming composition of the present invention includes a structural unit represented by general formula (I) and at least one of the structural units represented by general formula (II) and the structural unit represented by general formula (III), and includes a polymer in which the structural unit represented by the general formula (I) and at least one of the structural units represented by the general formula (II) and the structural unit represented by the general formula (III) form a random copolymer, and the fluorine content of the polymer is 5% by mass to 16% by mass. These structural units are polymerized to form a random copolymer because they have excellent compatibility with organic film-forming resins and solvents. This polymer contains an oxyalkylene group, which makes it excellent in flexibility, and the fluorine content is set within an appropriate range to control the aggregation state of the polymer, thereby improving the flowability of the organic film-forming composition and improving the embedding characteristics. Furthermore, this polymer has excellent solubility in the removal solution in the EBR process, which suppresses humps. In addition, the surface tension is reduced by containing fluorine, and the in-plane uniformity of the organic film-forming composition is also improved. The upper limit of the fluorine content is 16% by mass, preferably 14% by mass from the viewpoint of suppressing humps, and most preferably 12% by mass from the viewpoint of filling properties. From the viewpoint of in-plane uniformity, the lower limit of the fluorine content is 5 mass %, and 7 mass % is preferable.

[0050] Above R 1 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specific examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an s-butyl group, a t-butyl group, an isobutyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, and a decyl group. Among these, a hydrogen atom and a methyl group are more preferred.

[0051] Above R 2 is an organic group having 1 to 20 carbon atoms and containing a fluorine atom, which does not contain a sulfonyl group or an amino group. In the present invention, the term "organic group" refers to a group containing at least one carbon atom, and may further contain hydrogen, nitrogen, oxygen, sulfur, silicon, halogen atoms, and the like. An organic group having 1 to 20 carbon atoms and containing a fluorine atom is preferred, and an organic group having 1 to 20 carbon atoms and in which the substituent having a fluorine atom is represented by the following general formula (IV) or (V) is more preferred. [ka] (In the formula, * indicates the bond position.) R 2 The reason why sulfonyl and amino groups are not included is that these structures increase the polarity, limiting the types of suitable solvents. The polymer containing such a structure reduces the surface tension of the composition for forming an organic film and also has excellent compatibility with solvents, making it possible to form an organic film with better in-plane uniformity by spin coating.

[0052] More specific examples of the structural unit represented by the above general formula (I) include, but are not limited to, the following: As described above, among these, those having a perfluoroalkyl group having 3 or 4 carbon atoms are preferred. [ka]

[0053] Above R 3 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specific examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an s-butyl group, a t-butyl group, an isobutyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, and a decyl group. Among these, a hydrogen atom and a methyl group are more preferred.

[0054] Above R 4 and R 5Each of R represents a divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched. Specific examples of the divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched, include a methylene group, an ethylene group, a propylene group, a butylene group, a trimethylene group, and a tetramethylene group. Among these, an ethylene group is more preferable from the viewpoint of embedding properties. (R 4 O) and (R 5 The arrangement of O) may be random, block or multiblock.

[0055] Above R 6 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group. Specific examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, an allyl group, an n-butyl group, an s-butyl group, a t-butyl group, and an isobutyl group. Among these, a hydrogen atom, a methyl group or an ethyl group, and a phenyl group are more preferred.

[0056] The above m1 is 0 to 23, n1 is 0 to 23, and 23≧m1+n1≧2. Here, m1 and n1 represent the average number of repetitions. The upper limit of m1+n2 is 23, and from the viewpoint of low-temperature storage stability, 13 is more preferable.

[0057] More specific examples of the structural unit represented by the above general formula (II) include, but are not limited to, those shown below. [ka]

[0058] [ka]

[0059] Above R 7 and R 8represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specific examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an s-butyl group, a t-butyl group, an isobutyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, and a decyl group. Among these, a hydrogen atom and a methyl group are more preferred.

[0060] Above R 9 and R 10 Each of R represents a divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched. Specific examples of the divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched, include a methylene group, an ethylene group, a propylene group, a butylene group, a trimethylene group, and a tetramethylene group. Among these, an ethylene group is more preferable. (R 9 O) and (R 10 O) may be arranged randomly or in blocks.

[0061] The above m2 is 0 to 23, n2 is 0 to 23, and 23 ≧ m2 + n2 ≧ 2. Here, m2 and n2 represent the average number of repetitions. The upper limit of m2 + n2 is 23, and 13 is more preferable from the viewpoint of low-temperature storage stability.

[0062] More specific examples of the structural unit represented by the above general formula (III) include, but are not limited to, those shown below. [ka]

[0063] The polymer can be synthesized by polymerizing a monomer that provides a structural unit represented by general formula (I) and at least one monomer selected from a monomer that provides a structural unit represented by general formula (II) and a monomer that provides a structural unit represented by general formula (III) in a mixing ratio that provides a predetermined content ratio according to the structure of each polymer by a known method.

[0064] In addition, the polymer may use one or more types of monomers each selected from the monomers giving the structural unit represented by general formula (I), the monomers giving the structural unit represented by general formula (II), and the monomers giving the structural unit represented by general formula (III).

[0065] By combining a plurality of structural units, the structure becomes complex, which makes it possible to suppress aggregation of the polymer and to appropriately adjust the solvent solubility.

[0066] The polymer can be obtained by polymerizing a polymerizable monomer by a known method, and the structural unit represented by the general formula (I) and at least one of the structural units represented by the general formula (II) and the general formula (III) are polymerized to form a random copolymer. When obtaining a polymer, it is also possible to synthesize a polymer by polymerizing each monomer protected by a protecting group as necessary, and then performing a deprotection reaction as necessary. The reaction method for obtaining a polymer is not particularly limited, and can be appropriately selected according to the reactivity of the monomer using a method such as radical polymerization or cationic polymerization.

[0067] When radical polymerization is used, a method is available in which monomers having polymerizable unsaturated bonds are mixed, and a radical initiator is added in a solvent to carry out heat polymerization, thereby obtaining a polymerized product. Polymerization conditions can be selected from a variety of options depending on the monomers used, the target molecular weight, and other factors. Specific examples of solvents used during polymerization include toluene, benzene, tetrahydrofuran, diethyl ether, dioxane, 2-butanone, methyl isobutyl ketone, propylene glycol monomethyl ether acetate, cyclohexanone, γ-butyrolactone, ethyl acetate, and butyl acetate. Examples of polymerization initiators include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl 2,2-azobis(2-methylpropionate), benzoyl peroxide, and lauroyl peroxide. In addition, thiols such as octanethiol and 2-mercaptoethanol may be added as chain transfer agents during polymerization. The polymerization reaction can be carried out by heating preferably to a temperature of from 40° C. to the boiling point of the reaction solvent. The reaction time is 0.5 to 100 hours, preferably 1 to 48 hours.

[0068] When cationic polymerization is used, a method is used in which monomers having polymerizable unsaturated bonds are mixed and a cationic polymerization initiator is added to carry out polymerization, thereby obtaining a polymer. The polymerization conditions can be selected from a variety of conditions depending on the monomers used, the target molecular weight, and the like. Specific examples of the solvent used during polymerization include hexane, heptane, octane, toluene, methylene chloride, 1,2-dichloroethane, ethyl ether, and butyl ether. Examples of catalysts used as cationic polymerization initiators include protonic acids such as acid, sulfuric acid, perchloric acid, trifluoroacetic acid, methanesulfonic acid, trifluoromethanesulfonic acid, chlorosulfonic acid, and fluorosulfonic acid, and Lewis acids such as boron trifluoride, aluminum chloride, titanium tetrachloride, stannic chloride, and ferric chloride. When a Lewis acid is used as a catalyst, a proton supply source such as an acid, water, or alcohol may be added in an amount equivalent to that of the catalyst, since the cationic polymerization activity is improved. The polymerization reaction is not particularly limited as long as the reaction proceeds at a temperature at which the reaction proceeds, but is preferably carried out by heating to a temperature between -10°C and the boiling point of the reaction solvent. The reaction time is 0.5 to 100 hours, preferably 1 to 48 hours.

[0069] The polymer has a weight average molecular weight (Mw) of preferably 1000 to 30000, more preferably 2000 to 20000, and further preferably 3000 to 15000. When Mw is 1000 or more, excellent in-plane uniformity is exhibited. On the other hand, when Mw is 30000 or less, coating defects due to insufficient solubility in a solvent can be suppressed. Furthermore, the molecular weight distribution (Mw / Mn) is preferably 1.0 to 3.0, and more preferably 1.0 to 2.0. In the present invention, Mw and molecular weight distribution are values ​​measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.

[0070] The blending amount of the polymer is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, and particularly preferably 0.5 to 2 parts by mass, based on 100 parts by mass of the resin for forming an organic film. If the blending amount of the polymer is 0.01 parts by mass or more, the blending effect can be sufficiently obtained. In addition, the polymer is decomposed by heat during baking, which deteriorates the in-plane uniformity and filling properties, but it can be used preferably if it is within the range of 5 parts by mass or less.

[0071] [Organic film forming resin] The organic film-forming resin that can be used in the organic film composition of the present invention is not particularly limited as long as it is a compound containing a resin that satisfies the film-forming properties and curing properties of spin coating. From the viewpoints of etching resistance, optical properties, heat resistance, etc., it is more preferable to use a compound that contains an aromatic skeleton.

[0072] Examples of the aromatic skeleton include benzene, naphthalene, anthracene, pyrene, indene, fluorene, furan, pyrrole, thiophene, phosphole, pyrazole, oxazole, isoxazole, thiazole, pyridine, pyrazine, pyrimidine, pyridazine, triazine, carbazole, etc. Among these, benzene, naphthalene, fluorene, and carbazole are particularly preferable.

[0073] Examples of the organic film-forming resin that can be used in the present invention include resins containing the following structures described in JP-A Nos. 2012-1687 and 2012-77295. [ka] (In formula (1), the ring structures Ar1 and Ar2 represent a benzene ring or a naphthalene ring. X represents a single bond or an alkylene group having 1 to 20 carbon atoms. m represents 0 or 1. n represents any natural number such that the molecular weight is 100,000 or less. Note that the symbols in the formula are only applicable within this formula.)

[0074] [ka] (In formula (2), the ring structures Ar1 and Ar2 represent a benzene ring or a naphthalene ring. n represents any natural number such that the weight average molecular weight calculated as polystyrene by gel permeation chromatography is 100,000 or less. Note that the symbols in the formula are only applied within this formula.)

[0075] Further examples of organic film-forming resins applicable to the present invention include resins containing the following structures described in JP-A Nos. 2004-264710, 2005-043471, 2005-250434, 2007-293294, and 2008-65303. [ka] (In formula (3) and formula (4), R 1 and R 2 represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or an aryl group; R 3 represents an alkyl group having 1 to 3 carbon atoms, a vinyl group, an allyl group, or an aryl group which may be substituted, n represents 0 or 1, and m represents 0, 1, or 2. The symbols in the formula are applicable only within this formula.)

[0076] [ka] (In formula (5), R1 is a monovalent atom or group other than a hydrogen atom, and n is an integer of 0 to 4. However, when n is 2 to 4, multiple R1 may be the same or different. R2 and R3 are independently a monovalent atom or group. X is a divalent group. Note that the symbols in the formula apply only within this formula.)

[0077] [ka] In formula (6), R1 is a hydrogen atom or a methyl group. R2 is a single bond, a linear, branched or cyclic alkylene group having 1 to 20 carbon atoms, or an arylene group having 6 to 10 carbon atoms, and may have any of an ether, ester, lactone or amide. R 3 , R 4are each a hydrogen atom or a glycidyl group. X represents a polymer of any one of a hydrocarbon having an indene skeleton, a cycloolefin having 3 to 10 carbon atoms, and maleimide, and may have any one of an ether, an ester, a lactone, and a carboxylic acid anhydride. R 5 , R 6 R is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group. 7 is any one of a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, a hydroxyl group and an alkoxycarbonyl group. p and q are each an integer of 1 to 4. r is an integer of 0 to 4. a, b and c are each in the ranges of 0.5≦a+b+c≦1, 0≦a≦0.8, 0≦b≦0.8, 0.1≦a+b≦0.8 and 0.1≦c≦0.8. The symbols in the formula are applied only within this formula.

[0078] [ka] (In formula (7), R1 represents a hydrogen atom or a monovalent organic group, and R2 and R3 each independently represent a monovalent atom or a monovalent organic group. Note that the symbols in the formula apply only within this formula.)

[0079] Specific examples of the organic film-forming resin that can be used in the present invention include resins containing the following structures described in JP-A Nos. 2004-205685, 2007-171895, and 2009-14816. [ka] (In formula (8) and formula (9), R 1 ~R 8 are each independently a hydrogen atom, a hydroxyl group, a substitutable alkyl group having 1 to 6 carbon atoms, a substitutable alkoxy group having 1 to 6 carbon atoms, a substitutable alkoxycarboxyl group having 2 to 6 carbon atoms, a substitutable aryl group having 6 to 10 carbon atoms, a hydroxyalkyl group having 1 to 6 carbon atoms, an isocyanate group, or a glycidyl group. m and n are positive integers. Note that the symbols in the formula are only applicable within this formula.)

[0080] [Chemical formula] (In formula (10), R 1 , R 6 is a hydrogen atom or a methyl group. R 2 , R 3 , R 4 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group, a hydroxy group, an acetoxy group or an alkoxycarbonyl group, or an aryl group having 6 to 10 carbon atoms, and R 5 is a condensed polycyclic hydrocarbon group having 13 to 30 carbon atoms, -O-R 7 , -C(=O)-O-R 7 , -O-C(=O)-R 7 , or -C(=O)-NR 8 -R 7 , m is 1 or 2, n is an integer from 0 to 4, and p is an integer from 0 to 6. R 7 is an organic group having 7 to 30 carbon atoms, R 8 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. Z is any one of a methylene group, -O-, -S-, -NH-. a, b, c, d, e are respectively in the range of 0 < a < 1.0, 0 ≤ b ≤ 0.8, 0 ≤ c ≤ 0.8, 0 ≤ d ≤ 0.8, 0 ≤ e ≤ 0.8, 0 < b + c + d + e < 1.0. Note that the symbols in the formula are applicable only within this formula.)

[0081]

化

[0082] For example, the following compounds are exemplified. [ka]

[0083] [ka]

[0084] Examples of the organic film-forming resin applicable to the present invention include resins containing the following structures described in JP-A-2007-199653, JP-A-2008-274250, and JP-A-2010-122656. [ka] (In formula (12), R 1 and R 2 are independently the same or different hydrogen atoms, linear, branched or cyclic alkyl groups having 1 to 10 carbon atoms, aryl groups having 6 to 10 carbon atoms, or alkenyl groups having 2 to 10 carbon atoms; R 3 is a single bond, or an alkylene group having a linear, branched or cyclic structure and having 1 to 30 carbon atoms, which may have a bridged cyclic hydrocarbon group, a double bond, a hetero atom or an aromatic group having 6 to 30 carbon atoms; R 4 and R 5 are each independently a hydrogen atom or a glycidyl group, and n is an integer of 1 to 4. The symbols in the formula are applicable only within this formula.

[0085] [ka] (In formula (13), R 1 and R 2 are independently the same or different hydrogen atoms, linear, branched or cyclic alkyl groups having 1 to 10 carbon atoms, aryl groups having 6 to 10 carbon atoms, or alkenyl groups having 2 to 10 carbon atoms; R 3 is a single bond, or an alkylene group having a linear, branched or cyclic structure and having 1 to 30 carbon atoms, which may have a bridged cyclic hydrocarbon group, a double bond, a hetero atom or an aromatic group having 6 to 30 carbon atoms; R 4 and R 5 are each independently a hydrogen atom or a glycidyl group; R 6 is a single bond, or a linear or branched alkylene group having 1 to 10 carbon atoms. The symbols in the formula are only applicable within this formula.)

[0086] [ka] (In formula (14), ring Z 1 and ring Z 2 is a condensed polycyclic aromatic hydrocarbon ring, R 1a , R 1b , R 2a , and R 2b are the same or different and represent a substituent. k1 and k2 are the same or different and represent an integer of 0 or 1 to 4, m1 and m2 are each an integer of 0 or 1 or more, and n1 and n2 are each an integer of 0 or 1 or more, provided that n1+n2≧1. The symbols in the formulae are only applicable within this formula.

[0087] [ka] (In formula (15), R 1 , R 2 R are the same or different and are a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms. 3 , R 4is each a hydrogen atom or a glycidyl group, R 5 is a single bond or a linear or branched alkylene group having 1 to 10 carbon atoms, R 6 , R 7 is a benzene ring or a naphthalene ring. p and q are each 1 or 2. n is 0 < n ≤ 1. Note that the symbols in the formula are applicable only within this formula.)

[0088] For example, the following compounds are exemplified.

Chemical formula

[0089]

Chemical formula

[0090]

Chemical formula

[0091]

Chemical formula

[0092]

Chemical formula

[0093]

Chemical formula

[0094] Examples of the resin for forming an organic film applied to the present invention include resins containing the following structures described in JP-A-2012-214720.

Chemical formula

[0095] Examples of the organic film-forming resin that can be used in the present invention include resins described in JP-A-2014-29435, WO2012 / 077640, and WO2010 / 147155. [ka] (In formula (17), A represents a structure having carbazole, B represents a structure having an aromatic ring, and C represents a structure having a hydrogen atom, an alkyl group, or an aromatic ring, and B and C may form a ring together. The combined structure of A, B, and C has 1 to 4 carboxyl groups or salts thereof, or carboxylate groups. The symbols in the formula are only applicable within this formula.)

[0096] Further, an example of the polymer includes a unit structure represented by the following formula (18) described in International Publication WO2012 / 077640 and a unit structure represented by the following formula (19), in which the ratio of the unit structure represented by formula (18) to the unit structure represented by formula (19) is 3 to 97:97 to 3 in molar ratio. [ka] In formula (18), R1 and R2 each independently represent a hydrogen atom, a halogen atom, a nitro group, an amino group, a hydroxy group, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, or a combination of these groups which may contain an ether bond, a ketone bond, or an ester bond. R3 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, or a combination of these groups which may contain an ether bond, a ketone bond, or an ester bond. R4 represents a hydrogen atom, or an aryl group having 6 to 40 carbon atoms which may be substituted with a halogen atom, a nitro group, an amino group, or a hydroxy group, or a heterocyclic group; R5 represents a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms which may be substituted with a halogen atom, a nitro group, an amino group, or a hydroxy group, or an aryl group having 6 to 40 carbon atoms, or a heterocyclic group; R4 and R5 may form a ring together; n1 and n2 each represent an integer of 1 to 3. The symbols in the formula are applied only within this formula. [ka] In formula (19), Ar represents an aromatic ring group having 6 to 20 carbon atoms, R6 represents a hydroxy group, R7 represents a hydrogen atom, a halogen atom, a nitro group, an amino group, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, or a combination of these groups which may contain an ether bond, a ketone bond, or an ester bond, and R8 may be substituted with a hydrogen atom, a halogen atom, a nitro group, an amino group, or a hydroxy group. R8 represents an aryl group having 6 to 40 carbon atoms or a heterocyclic group, R9 represents a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms which may be substituted with a halogen atom, a nitro group, an amino group, or a hydroxy group, or an aryl group having 6 to 40 carbon atoms or a heterocyclic group, and R8 and R9 may form a ring together. n6 represents an integer of 1 to p, and n7 represents an integer of p-n6. Here, p represents the maximum number of groups which may be substituted on the aromatic ring group Ar. The symbols in the formula are only applicable within this formula.

[0097] An example of the organic film-forming resin applicable to the present invention is a polymer containing a unit structure represented by the following formula (20) described in International Publication WO2010 / 147155. [ka] (In formula (20), R1 and R2 are each selected from the group consisting of a hydrogen atom, a halogen group, a nitro group, an amino group, a hydroxyl group, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, and a combination thereof, and the alkyl group, the alkenyl group, or the aryl group represents a group which may contain an ether bond, a ketone bond, or an ester bond; R3 is selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, and a combination thereof, and the alkyl group, the alkenyl group, or the aryl group represents a group which may contain an ether bond, a ketone bond, or an ester bond; Or the aryl group represents a group which may contain an ether bond, a ketone bond or an ester bond, R4 represents an aryl group or heterocyclic group having 6 to 40 carbon atoms which may be substituted with a halogen group, a nitro group, an amino group or a hydroxy group, R5 represents a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms, an aryl group or heterocyclic group having 6 to 40 carbon atoms which may be substituted with a halogen group, a nitro group, an amino group or a hydroxy group, R4 and R5 may form a ring together with the carbon atom to which they are bonded, and n1 and n2 are each an integer of 1 to 3. Note that the symbols in the formula are only applicable within this formula.)

[0098] Examples of organic film-forming resins applicable to the present invention include novolak resins obtained by reacting one or more of phenols such as phenol, cresol, xylenol, catechol, resorcinol, hydroquinone, pyrogallol, hydroxyquinol, and phloroglucinol with one or more of aldehyde sources such as formaldehyde, paraformaldehyde, and trioxane using an acidic catalyst, and resins containing a repeating unit structure represented by the following formula (21) described in International Publication WO2012 / 176767. [ka] (In formula (21), A represents a hydroxy-substituted phenylene group derived from polyhydroxybenzene, and B represents a monovalent fused aromatic hydrocarbon ring group in which 2 to 6 benzene rings are fused. Note that the symbols in the formula are only applicable within this formula.)

[0099] Examples of organic film-forming resins applicable to the present invention include novolak resins having a fluorene or tetrahydrospirobiindene structure described in JP-A-2005-128509, JP-A-2006-259249, JP-A-2006-259482, JP-A-2006-293298, and JP-A-2007-316282, and resins containing a repeating unit structure represented by the following formula (22-1) or (22-2). [ka] (In formula (22-1) and formula (22-2), R 1 , R 2 , R 6 , R 7 are independently a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an allyl group, or a halogen atom; R 3 , R 4 , R 8 , R 9are independently a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, a linear, branched or cyclic alkenyl group having 2 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, or a glycidyl group; R 5 , R 14 are each independently a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 10 carbon atoms. n, m, p and q are each an integer of 1 to 3. R 10 ~R 13 are independently a hydrogen atom, a halogen atom, a hydroxyl group, a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, or a linear, branched or cyclic alkoxy group having 1 to 6 carbon atoms. Note that the symbols in the formula are only applicable within this formula.)

[0100] An example of the organic film-forming resin that can be used in the present invention is a reaction product obtained by the method described in JP-A-2012-145897. More specifically, examples of the polymers include polymers obtained by condensing one or more compounds represented by the following general formulae (23-1) and / or (23-2) with one or more compounds represented by the following general formulae (24-1) and / or (24-2) and / or their equivalents. [ka] (In formula (23-1) and formula (23-2), R 1 ~R 8 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an isocyanato group, a glycidyloxy group, a carboxyl group, an amino group, an alkoxy group having 1 to 30 carbon atoms, an alkoxycarbonyl group having 1 to 30 carbon atoms, an alkanoyloxy group having 1 to 30 carbon atoms, or an optionally substituted saturated or unsaturated organic group having 1 to 30 carbon atoms. 1 ~R 4 or R 5 ~R 8 Two substituents arbitrarily selected from the following may be bonded to form a cyclic substituent. The symbols in the formula are applicable only within this formula.) [ka] (In formula (24-1) and formula (24-2), Q is an organic group having 1 to 30 carbon atoms which may be substituted, and further, two Qs selected arbitrarily in the molecule may be bonded to form a cyclic substituent. n1 to n6 are the numbers of each substituent, n1 to n6=0, 1, 2, and in formula (24-1), hydroxybenzaldehyde is excluded. In addition, in formula (24-2), the relationships of 0≦n3+n5≦3, 0≦n4+n6≦4, 1≦n3+n4≦4 are satisfied. Note that the symbols in the formulas are applicable only within this formula.)

[0101] Further, examples of the polymers include polymers obtained by condensing one or more compounds represented by the above general formula (23-1) and / or (23-2), one or more compounds represented by the above general formula (24-1) and / or (24-2) and / or their equivalents, and one or more compounds represented by the following general formula (25) and / or their equivalents. [ka] (In formula (25), Y is a hydrogen atom or a monovalent organic group having 30 or less carbon atoms which may have a substituent, and formula (25) is different from formula (24-1) and formula (24-2). Note that the symbols in the formula apply only within this formula.)

[0102] Examples of the organic film-forming resin applicable to the present invention include resins having the following structure described in JP-A-2017-119671. [ka] (In formula (26-1), R is a single bond or an organic group having 1 to 50 carbon atoms, X is a group represented by the following general formula (26-2), and m1 is an integer satisfying 2≦m1≦10. Note that the symbols in the formula apply only within this formula.) [ka] (In the formula, X 2 is a divalent organic group having 1 to 10 carbon atoms, n1 is 0 or 1, n2 is 1 or 2, and X 3is a group represented by the following general formula (26-3), and n5 is 0, 1 or 2. The symbols in the formula apply only within this formula. [ka] (In the formula, R 10 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the hydrogen atom on the benzene ring in the formula may be substituted with a methyl group or a methoxy group. Note that the symbols in the formula are only applicable within this formula.)

[0103] For example, the following compounds are exemplified. [ka]

[0104] [ka]

[0105] Examples of the organic film-forming resin applicable to the present invention include a polymer having a repeating unit represented by the following general formula (27-1) described in JP-A-2019-44022. [ka] In formula (27-1), AR1 and AR2 each represent a benzene ring or a naphthalene ring which may have a substituent, and R 1 , R 2 are each independently a hydrogen atom or an organic group having 1 to 30 carbon atoms, R 1 and R 2 When is an organic group, R 1 and R 2may form a cyclic organic group by bonding intramolecularly. n is 0 or 1, and when n=0, AR1 and AR2 do not form a bridged structure between the aromatic rings of AR1 and AR2 via Z, and when n=1, AR1 and AR2 form a bridged structure between the aromatic rings of AR1 and AR2 via Z, and Z is either a single bond or the following formula (27-2). Y is a group represented by the following formula (27-3). Note that the symbols in the formula are only applicable within this formula.) [ka]

[0106] [ka] (In the formula, R 3 is a single bond or a divalent organic group having 1 to 20 carbon atoms, and R 4 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, and the dashed line indicates a bond. Note that the symbols in the formula are only applicable within this formula.)

[0107] For example, the following polymers are exemplified. [ka]

[0108] [ka]

[0109] [ka]

[0110] The organic film-forming resin may be synthesized by a known method, or a commercially available product may be used.

[0111] The amount of the organic film-forming resin is not particularly limited as long as the film-forming properties of the spin coating of the organic film-forming composition are satisfied, but the amount of the organic film-forming resin is preferably 10 to 40 parts by mass, more preferably 10 to 30 parts by mass, and even more preferably 10 to 25 parts by mass, based on 100 parts by mass of the organic film-forming composition. For example, when filling holes or trenches with a very high aspect ratio of a 3D NAND memory architecture with an organic film-forming composition, it is necessary to increase the amount of the organic film-forming resin, but on the other hand, such an organic film-forming composition has a high viscosity, and the in-plane uniformity and filling properties after spin coating are deteriorated. Even with the above-mentioned blending ratio of the organic film-forming resin, the organic film-forming composition of the present invention can be suitably applied because it is possible to form an organic film with excellent in-plane uniformity and filling properties.

[0112] [solvent] The solvent that can be used in the organic film-forming composition of the present invention is not particularly limited as long as it can dissolve the organic film-forming resin and the polymer, and it is preferable that the solvent can also dissolve the acid generator, crosslinking agent, surfactant, etc. described below. Specific examples of the ketones include 2-heptanone, cyclopentanone, and cyclohexanone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; and esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, γ-butyrolactone, and propylene glycol mono tert-butyl ether acetate. These may be used alone or in combination of two or more, but are not limited thereto.

[0113] Among these, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, γ-butyrolactone, and mixtures of two or more of these are preferably used.

[0114] [Other ingredients] In addition, an acid generator or a crosslinking agent for further promoting the crosslinking reaction can be added to the organic film-forming composition of the present invention. As the acid generator, there are those that generate an acid by thermal decomposition and those that generate an acid by light irradiation, and either of them can be added. Specific examples of the acid generator include those described in paragraphs (0061) to (0085) of JP-A-2007-199653.

[0115] Specific examples of the crosslinking agent include those described in paragraphs (0055) to (0060) of JP-A No. 2007-199653.

[0116] In addition, a surfactant may be added to the organic film-forming composition of the present invention in order to further improve the in-plane uniformity in spin coating. Specific examples of the surfactant include those described in paragraphs (0142) to (0147) of JP-A-2009-269953.

[0117] Furthermore, a basic compound can be added to the organic film-forming composition of the present invention to improve storage stability. The basic compound acts as a quencher for the acid to prevent a small amount of acid generated from the acid generator from proceeding with the crosslinking reaction. Specific examples of such basic compounds include those described in paragraphs (0086) to (0090) of JP2007-199653A.

[0118] As described above, the organic film-forming composition of the present invention is an organic film-forming composition that is excellent in suppressing hump during EBR process.Therefore, the organic film-forming composition of the present invention is extremely useful as a resist underlayer film material for multi-layer resist processes such as a two-layer resist process, a three-layer resist process using a silicon-containing resist intermediate film or a silicon-containing inorganic hard mask, and a four-layer resist process using a silicon-containing resist intermediate film or a silicon-containing inorganic hard mask and an organic anti-reflective film or an adhesive film.

[0119] [Organic film formation method] The present invention provides a method for forming an organic film used in the manufacturing process of a semiconductor device, which comprises spin-coating the above-mentioned composition for forming an organic film of the present invention on a substrate to be processed, and heat-treating the substrate coated with the composition for forming an organic film at a temperature of 100° C. or higher and 600° C. or lower for 10 to 600 seconds, thereby forming a cured film.

[0120] In this organic film forming method, first, the organic film forming composition of the present invention described above is spin-coated (spin-coated) onto a substrate to be processed. By using the spin-coating method, good embedding properties can be obtained. After removing the coating from the edge in the EBR process, baking (heat treatment) is performed to promote the crosslinking reaction. This baking can evaporate the solvent in the composition, so mixing can be prevented even when a resist top layer film or a silicon-containing resist intermediate film is formed on the organic film.

[0121] Baking is performed at a temperature of 100° C. to 600° C. for 10 to 600 seconds, preferably at a temperature of 200° C. to 500° C. for 10 to 300 seconds. In consideration of the effect on device damage and wafer deformation, the upper limit of the heating temperature in the lithography wafer process is preferably 600° C. or less, more preferably 500° C. or less. By carrying out heat treatment under such conditions, the crosslinking reaction is promoted, and an organic film that does not mix with the film formed on the upper layer can be formed.

[0122] [Pattern formation method] [Three-layer resist process using silicon-containing resist intermediate film] The present invention provides a pattern forming method, which comprises forming an organic film on a workpiece using the above-mentioned organic film-forming composition of the present invention, forming a resist intermediate film on the organic film using a resist intermediate film material containing silicon atoms, forming a resist upper layer film on the resist intermediate film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the resist intermediate film by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.

[0123] As the workpiece, it is preferable to use a semiconductor device substrate, or the semiconductor device substrate on which any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film is formed. More specifically, although not limited to, a substrate such as Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al, or the like, or a substrate on which the above-mentioned metal film or the like is formed as a workpiece layer, may be used.

[0124] As the processed layer, various low-k films such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si, and their stopper films are used, and can be formed to a thickness of usually 50 to 10,000 nm, particularly 100 to 5,000 nm. When forming the processed layer, the substrate and the processed layer are made of different materials.

[0125] The metal constituting the workpiece is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, molybdenum, or an alloy thereof.

[0126] When forming an organic film on a workpiece using the organic film-forming composition of the present invention, the above-mentioned organic film-forming method of the present invention may be applied.

[0127] Next, a resist intermediate film (silicon-containing resist intermediate film) is formed on the organic film using a resist intermediate film material containing silicon atoms. As the resist intermediate film material containing silicon atoms, a polysiloxane-based intermediate film material is preferable. By imparting an anti-reflection effect to the silicon-containing resist intermediate film, reflection can be suppressed. In particular, for 193 nm exposure, if a material containing many aromatic groups and having high etching selectivity with the substrate is used as the organic film forming composition, the k value becomes high and the substrate reflection becomes high, but by imparting absorption to an appropriate k value as the silicon-containing resist intermediate film, it becomes possible to suppress reflection, and the substrate reflection can be reduced to 0.5% or less. As the silicon-containing resist intermediate film having an anti-reflection effect, anthracene is preferably used for 248 nm and 157 nm exposure, and polysiloxane having a pendant structure with a light-absorbing group having a phenyl group or a silicon-silicon bond for 193 nm exposure, which is crosslinked by acid or heat.

[0128] Next, a resist upper layer film is formed on the resist intermediate film using a resist upper layer film material consisting of a photoresist composition. The resist upper layer film material may be either positive or negative, and the same as a commonly used photoresist composition can be used. After spin-coating the resist upper layer film material, it is preferable to perform pre-baking at 60 to 180°C for 10 to 300 seconds. Thereafter, exposure is performed according to a conventional method, and further post-exposure baking (PEB) and development are performed to obtain a resist upper layer film pattern. The thickness of the resist upper layer film is not particularly limited, but is preferably 30 to 500 nm, and particularly preferably 50 to 400 nm.

[0129] Next, a circuit pattern (resist upper layer film pattern) is formed on the resist upper layer film. In forming the circuit pattern, it is preferable to form the circuit pattern by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination of these.

[0130] Examples of the exposure light include high-energy rays with a wavelength of 300 nm or less, specifically far ultraviolet rays, KrF excimer laser light (248 nm), ArF excimer laser light (193 nm), F2 laser light (157 nm), Kr2 laser light (146 nm), Ar2 laser light (126 nm), soft X-rays (EUV) of 3 to 20 nm, electron beams (EB), ion beams, X-rays, and the like.

[0131] In forming the circuit pattern, it is preferable to develop the circuit pattern using an alkali developer or an organic solvent.

[0132] Next, the resist upper layer film on which the circuit pattern is formed is used as a mask to transfer the pattern to the resist intermediate film by etching. The etching of the resist intermediate film performed using the resist upper layer film pattern as a mask is preferably performed using a fluorocarbon gas. In this way, a silicon-containing resist intermediate film pattern is formed.

[0133] Next, the pattern is transferred to the organic film by etching using the resist intermediate film to which the pattern has been transferred as a mask. Since the silicon-containing resist intermediate film exhibits resistance to etching by oxygen gas or hydrogen gas, the etching of the organic film using the silicon-containing resist intermediate film pattern as a mask is preferably performed using an etching gas mainly composed of oxygen gas or hydrogen gas. In this way, an organic film pattern is formed.

[0134] Next, the pattern is transferred to the workpiece by etching using the organic film with the transferred pattern as a mask. The next etching of the workpiece (working layer) can be performed by a conventional method. For example, if the workpiece is SiO2, SiN, or a silica-based low dielectric constant insulating film, etching is performed mainly with fluorocarbon gas, and if it is p-Si, Al, or W, etching is performed mainly with chlorine or bromine gas. If the substrate is processed by etching with fluorocarbon gas, the silicon-containing resist intermediate film pattern is peeled off at the same time as the substrate is processed. On the other hand, if the substrate is processed by etching with chlorine or bromine gas, a separate dry etching stripping with fluorocarbon gas must be performed after the substrate is processed in order to strip the silicon-containing resist intermediate film pattern.

[0135] An organic film obtained by using the organic film-forming composition of the present invention can have excellent etching resistance when etching the workpiece as described above.

[0136] [Four-layer resist process using silicon-containing resist intermediate film and organic anti-reflective or adhesive film] The present invention also provides a pattern forming method, which includes forming an organic film on a workpiece using the organic film-forming composition of the present invention described above, forming a resist intermediate film on the organic film using a resist intermediate film material containing silicon atoms, forming an organic antireflective film or adhesive film on the resist intermediate film, forming a resist upper layer film on the organic antireflective film or adhesive film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film or adhesive film and the resist intermediate film by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.

[0137] This method can be carried out in the same manner as the three-layer resist process using the silicon-containing resist intermediate film described above, except that an organic antireflective coating (BARC) or an adhesion film is formed between the resist intermediate film and the resist top layer film.

[0138] The organic anti-reflection film and adhesion film can be formed by spin coating using a known organic anti-reflection film material or adhesion film material.

[0139] [Three-layer resist process using inorganic hard mask] The present invention also provides a pattern formation method by a three-layer resist process using the above-mentioned organic film-forming composition of the present invention, which includes forming an organic film on a workpiece using the above-mentioned organic film-forming composition of the present invention, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film, forming a resist upper layer film on the inorganic hard mask using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the inorganic hard mask by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.

[0140] This method can be carried out in the same manner as the three-layer resist process using the silicon-containing resist intermediate film described above, except that an inorganic hard mask is formed on the organic film instead of the resist intermediate film.

[0141] The inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film (SiON film) can be formed by a CVD method, an ALD method, or the like. Methods for forming a silicon nitride film are described in, for example, JP-A-2002-334869 and WO-A-2004 / 066377. The thickness of the inorganic hard mask is preferably 5 to 200 nm, more preferably 10 to 100 nm. As the inorganic hard mask, a SiON film, which has a high effect as an anti-reflection film, is most preferably used.

[0142] [4-layer resist process using inorganic hard mask and organic anti-reflective or adhesive film] The present invention also provides a pattern formation method by a four-layer resist process using the organic film-forming composition of the present invention described above, which includes forming an organic film on a workpiece using the organic film-forming composition of the present invention described above, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film, forming an organic antireflective film or an adhesion film on the inorganic hard mask, forming a resist upper layer film on the organic antireflective film or adhesion film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film or adhesion film and the inorganic hard mask by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic antireflective film or adhesion film and the inorganic hard mask by etching using the inorganic hard mask to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.

[0143] This method can be performed in the same manner as the above-mentioned three-layer resist process using an inorganic hard mask, except that an organic antireflective coating (BARC) or an adhesion film is formed between the inorganic hard mask and the resist top layer film.

[0144] In particular, when a SiON film is used as the inorganic hard mask, the two-layer anti-reflection coating of the SiON film and BARC makes it possible to suppress reflections even in immersion lithography with a high NA exceeding 1.0. Another advantage of forming a BARC is that it has the effect of reducing the tailing of the resist top layer pattern directly above the SiON film.

[0145] Here, an example of a pattern forming method by the three-layer resist process of the present invention is shown in Figures 3(A) to (F). In the case of the three-layer resist process, as shown in Figure 3(A), an organic film 3 is formed on a workpiece layer 2 formed on a substrate 1 using the organic film-forming composition of the present invention, and then a silicon-containing resist intermediate film 4 is formed thereon, and a resist upper layer film 5 is formed thereon. Then, as shown in Figure 3(B), the exposed portion 6 of the resist upper layer film 5 is exposed to light, and PEB (post-exposure bake) is performed. Then, as shown in Figure 3(C), development is performed to form a resist upper layer film pattern 5a. Then, as shown in Figure 3(D), the silicon-containing resist intermediate film 4 is dry-etched using a fluorocarbon gas with the resist upper layer film pattern 5a as a mask, to form a silicon-containing resist intermediate film pattern 4a. Then, as shown in Figure 3(E), after removing the resist upper layer film pattern 5a, the organic film 3 is oxygen plasma etched with the silicon-containing resist intermediate film pattern 4a as a mask, to form an organic film pattern 3a. 3(F), after removing the silicon-containing resist intermediate film pattern 4a, the processing layer 2 is etched using the organic film pattern 3a as a mask to form a pattern 2a. By suppressing the hump during the formation of the organic film, defects caused by the hump in the organic film during the dry etching process in (D), (E), and (F) are reduced. It is possible to reduce the

[0146] When an inorganic hard mask is formed, the silicon-containing resist intermediate film 4 may be changed to an inorganic hard mask, and when a BARC or an adhesion film is formed, the BARC or adhesion film may be formed between the silicon-containing resist intermediate film 4 and the resist upper layer film 5. The etching of the BARC may be performed consecutively prior to the etching of the silicon-containing resist intermediate film 4, or the etching of only the BARC may be performed, and then the etching of the silicon-containing resist intermediate film 4 may be performed by changing the etching device, for example.

[0147] As described above, the pattern formation method of the present invention makes it possible to form a fine pattern on a workpiece with high precision by a multilayer resist process, and also to reduce defects resulting from humps in the organic film by suppressing the formation of humps in the organic film. EXAMPLES

[0148] The present invention will be described in more detail below with reference to Synthesis Examples, Comparative Synthesis Examples, Examples, and Comparative Examples, but the present invention is not limited to these. The molecular weight was specifically measured by the following method: The weight average molecular weight (Mw) and number average molecular weight (Mn) in terms of polystyrene were determined by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent (solvent), and the polydispersity (Mw / Mn) was calculated.

[0149] [Preparation of Polymers (A-1 to 24, a-1 to 10)] The polymers (A-1) to (A-24) and the comparative polymers (a-1) to (a-10) used in preparing the compositions for forming organic films were synthesized using the following monomers (B-1) to (B-6), (C-1) to (C-8), (D-1), and (E-1) to (E-3). [ka]

[0150] [Synthesis Example 1] Synthesis of Polymer (A-1) 6.0 g of propylene glycol monomethyl ether acetate (PGMEA) was heated and stirred at 80°C under a nitrogen atmosphere. To this, 3.18 g (0.010 mol) of (B-1), 7.74 g (0.035 mol) of (C-1), a mixture of 0.473 g of dimethyl 2,2-azobis(2-methylpropionate) and 34 g of PGMEA was added dropwise for 4 hours. After further heating and stirring for 16 hours, the mixture was cooled to room temperature to obtain a PGMEA solution of the target polymer (A-1). Analysis showed that the weight average molecular weight (Mw) of the polymer (A-1) was 6900 and the dispersity (Mw / Mn) was 1.4. [ka]

[0151] [Synthesis Examples 2 to 34] Synthesis of Polymers (A-2) to (A-24) and Comparative Polymers (a-1) to (a-10) Except for changing the type and molar ratio of the raw material monomers used according to the structure of each polymer, the following polymers (A-2) to (A-24) and comparative polymers (a-1) to (a-10) were obtained as products by the method according to Synthesis Example 1. The weight average molecular weight (Mw) and dispersity (Mw / Mn) determined by GPC and the fluorine content calculated from the raw material monomers and their blending ratios are also shown. The above polymers are all random copolymers.

[0152] [ka]

[0153] (a-1) to (a-5) are comparative polymers because their fluorine contents are outside the range shown in Table 1, and (a-6) to (a-10) are comparative polymers because they contain structural units different from those of formula (II) or formula (III). [ka]

[0154] [Table 1-1]

[0155] [Table 1-2]

[0156] [Organic film forming resin] F-1: Resin represented by the following formula (F-1) F-2: Resin represented by the following formula (F-2) F-3: Resin represented by the following formula (F-3) F-4: Resin represented by the following formula (F-4) F-5: Resin represented by the following formula (F-5) F-6: Resin represented by the following formula (F-6)

[0157] [ka]

[0158] [ka]

[0159] [solvent] G-1: Propylene glycol monomethyl ether acetate G-2: Propylene glycol monoethyl ether

[0160] [Preparation of organic film-forming compositions (UDL-1 to 102, comparative UDL-1 to 33)] The above polymers (A-1) to (A-24), (a-1) to (a-10), organic film-forming resins (F-1) to (F-6), and solvents were dissolved in the ratios shown in Table 2, and the resulting solution was filtered through a 0.1 μm fluororesin filter to prepare organic film materials (ULD-1 to 102, and comparative examples UDL-1 to 33). All of these organic film compositions contain a random copolymer. [Table 2-1]

[0161] [Table 2-2]

[0162] [Table 2-3]

[0163] [Table 2-4]

[0164] [Table 2-5]

[0165] [Preparation of silicon wafers with organic cured films formed using organic film-forming compositions (UDL-1 to 102, comparative ULD-1 to 33)] Using a coater / developer "CLEAN TRACK LITHIUS Pro AP" manufactured by Tokyo Electron Ltd., 2 mL of the organic film-forming composition (UDL-1 to 102, comparative UDL-1 to 33) prepared above was discharged onto the center of a silicon wafer, and the silicon wafer was rotated at a rotation speed that would result in the average film thickness shown in Table 3 after baking, and the composition was spread to form a film. While rotating the silicon wafer at a speed of 1000 rpm, the removal solution discharge nozzle was moved at a speed of 5 mm / s from the outer periphery of the silicon wafer to a position 3 mm from the center while discharging the removal solution (a mixture of propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether (30:70, mass ratio)) at a discharge rate of 2 mL / s, and the removal solution was discharged at that position for 5 seconds at a discharge rate of 2 mL / s. After that, the discharge of the discharge solution was stopped, and the wafer was rotated at a speed of 1000 rpm for another 30 seconds. Next, the silicon wafer on which the organic film-forming composition was formed was heated at 350° C. for 60 seconds to obtain a silicon wafer on which an organic cured film was formed.

[0166] [Solvent resistance evaluation: Examples 1-1 to 1-102, Comparative Examples 1-1 to 1-33] The organic film-forming compositions (UDL-1 to 102, Comparative UDL1-1 to 1-33) were formed on silicon wafers by the above method, the film thickness was measured, PGMEA solvent was dispensed thereon, left for 30 seconds, spin-dried, and baked at 100°C for 60 seconds to evaporate the PGMEA, and the film thickness was measured. The film thickness before dispensing the PGMEA solvent was X, the film thickness after dispensing the PGMEA solvent was X1, and the absolute value of the value calculated by (X1-X) / X×100 was taken as the film thickness change rate (%), and the results are shown in Table 3. A film thickness change rate of less than 0.5% was considered good, and a film thickness change rate of 0.5% or more was considered bad.

[0167] [In-plane uniformity evaluation: Examples 1-1 to 1-102, Comparative Examples 1-1 to 1-33] The organic film-forming compositions (UDL-1 to 102, Comparative UDL1-1 to 1-33) were formed on silicon wafers by the above method, and the film thickness within a radius of 145 mm from the center of the organic cured film was measured. The maximum film thickness Xmax, the minimum film thickness Xmin, and the average film thickness X average As, (X max -X min ) / X average The value obtained by the above was taken as the in-plane uniformity (%), and the results are shown in Table 3. When the in-plane uniformity was less than 2%, it was rated as A (good), when it was 2% or more but less than 3%, it was rated as B, and when it was 3% or more, it was rated as C (poor).

[0168] [Low temperature storage stability evaluation: Examples 1-1 to 1-102, Comparative Examples 1-1 to 1-33] The organic film-forming compositions (UDL-1 to 102, Comparative UDL1-1 to 1-33) were stored in a freezer set at -20°C for one week. If no precipitate was observed, the result was considered good. If precipitate was observed, the result was considered bad. The results are shown in Table 3.

[0169] [Table 3-1]

[0170] [Table 3-2]

[0171] [Table 3-3]

[0172] [Table 3-4]

[0173] [Table 3-5]

[0174] [Hump suppression evaluation: Examples 2-1 to 2-102, Comparative Examples 2-1 to 2-25] The organic film-forming compositions (UDL-1 to 102, Comparative UDL-1 to 6, 8, 10 to 14, 21 to 33) were formed on silicon wafers by the above method, and the height change from the outer peripheral edge of the organic film to the center of the silicon wafer at a position of 1000 μm was measured using Alpha-Step D-600 (contact profiler) manufactured by KLA-TENCOR. When the height of the silicon wafer is set to 0, as shown in FIG. 2, if the maximum height is less than 110% of the film thickness, it is evaluated as A (good), if the maximum height is 110% or more but less than 150%, it is evaluated as B, and if an area with a maximum height of 150% or more occurs as shown in FIG. 1, it is evaluated as C (poor), and the results are shown in Table 4.

[0175] [Embedding evaluation-1: Examples 2-1 to 2-102, Comparative examples 2-1 to 2-25] As shown in FIG. 4, on a SiO2 wafer substrate having a dense hole pattern (hole diameter 0.2 μm, hole depth 1.0 μm, distance between the centers of two adjacent holes 0.4 μm), organic film-forming compositions (UDL-1 to 102, comparative UDL-1 to 6, 8, 10 to 14, 21 to 33) were formed by the above method to form a resist underlayer film 8. The substrate used was a base substrate (SiO2 wafer substrate) 7 having a dense hole pattern as shown in FIG. 4(G) (overhead view) and (H) (cross-sectional view). The cross-sectional shape of each of the obtained wafer substrates was observed using a scanning electron microscope (SEM) to confirm whether the holes were filled with the resist underlayer film without any voids inside. When a resist underlayer film material with poor filling properties was used, voids were generated inside the holes. When a resist underlayer film material with good filling properties was used, in this evaluation, the resist underlayer film was filled without voids inside the holes as shown in FIG. 4(I). If no voids were formed, the sample was rated as good, and if voids were formed, the sample was rated as bad.

[0176] [Embedding evaluation-2: Examples 2-1 to 2-102, Comparative examples 2-1 to 2-25] As shown in FIG. 4, on a SiO2 wafer substrate having a dense hole pattern (hole diameter 0.2 μm, hole depth 2.0 μm, distance between the centers of two adjacent holes 0.4 μm), organic film-forming compositions (UDL-1 to 102, comparative UDL-1 to 6, 8, 10 to 14, 21 to 33) were formed by the above method to form a resist underlayer film 8. The substrate used was a base substrate (SiO2 wafer substrate) 7 having a dense hole pattern as shown in FIG. 4(G) (overhead view) and (H) (cross-sectional view). The cross-sectional shape of each of the obtained wafer substrates was observed using a scanning electron microscope (SEM) to confirm whether the resist underlayer film was filled without voids inside the holes. When a resist underlayer film material with poor filling properties was used, voids were generated inside the holes. When a resist underlayer film material with good filling properties was used, in this evaluation, the resist underlayer film was filled without voids inside the holes as shown in FIG. 4(I). When no voids were generated, the result was evaluated as good, and when voids were generated, the result was evaluated as bad. In addition, when the ratio of the organic film-forming resin to the organic film-forming composition was small and the amount of resin was insufficient to fill the holes, film formation was defective.

[0177] [Table 4-1]

[0178] [Table 4-2]

[0179] [Table 4-3]

[0180] [Table 4-4]

[0181] [Table 4-5]

[0182] As shown in Tables 3-1 to 3-5 and Tables 4-1 to 4-5, it was confirmed that the organic film-forming compositions of the present invention (UDL-1 to 102) were superior to the comparative examples in solvent resistance, in-plane uniformity, hump suppression, and filling properties.

[0183] [Pattern formation test: Examples 3-1 to 3-88] Using the above method, an organic cured film was formed on a SiO2 wafer substrate using an organic film-forming composition (UDL-1 to 88), and the following silicon-containing resist intermediate film material (SOG1) was applied thereon and baked at 200°C for 60 seconds to form a silicon-containing resist intermediate film with a thickness of 35 nm. The following ArF single layer resist was applied thereon as a resist upper layer film material and baked at 105°C for 60 seconds to form a photoresist film with a thickness of 100 nm. The following immersion protective film material (TC-1) was applied on the photoresist film and baked at 90°C for 60 seconds to form a protective film with a thickness of 50 nm.

[0184] As a silicon-containing resist intermediate film material (SOG1), a 2% solution of the following polymer in propylene glycol ethyl ether was prepared. [ka]

[0185] The resist top layer film material (ArF single layer resist) was prepared by dissolving a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) in a solvent containing 0.1 mass% FC-430 (Sumitomo 3M Limited) in the proportions shown in Table 5, and filtering the solution through a 0.1 μm fluororesin filter. [Table 5]

[0186] The polymer (RP1), acid generator (PAG1), and basic compound (Amine1) are shown below. [ka]

[0187] The immersion protective film material (TC-1) was prepared by dissolving the polymer (PP1) in an organic solvent in the ratio shown in Table 6, and filtering the solution through a 0.1 μm fluorine resin filter. [Table 6]

[0188] The polymer (PP1) is shown below. [ka]

[0189] Next, the film was exposed using an ArF immersion exposure apparatus (Nikon Corporation; NSR-S610C, NA 1.30, σ 0.98 / 0.65, 35 degree dipole s-polarized illumination, 6% halftone phase shift mask), baked at 100°C for 60 seconds (PEB), and developed in a 2.38 mass% tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds to obtain a 55 nm 1:1 positive line and space pattern (resist upper layer film pattern).

[0190] Next, the silicon-containing resist intermediate film was dry-etched (pattern transferred) using the resist upper layer film pattern as a mask by using a Tokyo Electron etching device Telius, the resulting silicon-containing resist intermediate film pattern was used as a mask to dry-etch (pattern transferred) the organic film, and the resulting organic film pattern was used as a mask to dry-etch (pattern transferred) the SiO2 wafer substrate (SiO2 film). The etching conditions are as shown below.

[0191] (Transfer conditions of resist top layer film pattern to silicon-containing resist intermediate film) Chamber pressure 10.0Pa RF power 1,500W CF4 gas flow rate: 75mL / min O2 gas flow rate: 15mL / min Time 15sec

[0192] (Conditions for transferring silicon-containing resist intermediate film pattern to organic film) Chamber pressure 2.0Pa RF power 500W Ar gas flow rate: 75mL / min O2 gas flow rate: 45mL / min Time 120sec

[0193] (Transfer conditions for organic film pattern onto SiO2 wafer substrate) Chamber pressure 2.0Pa RF power: 2,200W C5F 12 Gas flow rate: 20mL / min C2F6 gas flow rate: 10mL / min Ar gas flow rate: 300mL / min O2 gas flow rate: 60mL / min Time 90sec

[0194] The cross section of the obtained pattern was observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd. The results are shown in Tables 7-1 to 7-3. [Table 7-1]

[0195] [Table 7-2]

[0196] [Table 7-3]

[0197] As shown in Tables 7-1 to 7-3, in Examples 3-1 to 3-88 in which the organic film-forming composition of the present invention (UDL-1 to 88) was used, the resist top layer film pattern was successfully transferred to the SiO2 wafer substrate, and it was confirmed that the organic film-forming composition of the present invention is suitable for use in microfabrication using the multilayer resist method.

[0198] From the above, the organic film-forming composition of the present invention has excellent film-forming properties, advanced filling characteristics, and hump suppression properties, and is therefore extremely useful as an organic film material for use in multilayer resist processes. Furthermore, the pattern formation method of the present invention using this composition is capable of filling holes and trenches with extremely high aspect ratios without voids, and is also capable of forming fine patterns with high precision. In addition, it is possible to form an organic film with suppressed humps, making it possible to efficiently manufacture semiconductor elements, etc.

[0199] The present specification includes the following aspects. [1]: A composition for forming an organic film, comprising: a resin for forming an organic film; a polymer containing a structural unit represented by the following general formula (I) and at least one of a structural unit represented by the following general formula (II) and a structural unit represented by the following general formula (III); and a solvent, wherein the structural unit represented by the following general formula (I) and at least one of the structural units represented by the following general formula (II) and a structural unit represented by the following general formula (III) form a random copolymer, and the polymer has a fluorine content of 5% by mass to 16% by mass. [ka] (In the formula, R 1 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 2 is an organic group having 1 to 20 carbon atoms and containing a fluorine atom, which does not contain a sulfonyl group or an amino group. [ka] (In the formula, R 3is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 4 and R 5 each represents a divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched; R 6 is a hydrogen atom or an alkyl group or a phenyl group having 1 to 4 carbon atoms, m1 is 0 to 23, n1 is 0 to 23, and 23≧m1+n1≧2. [ka] (In the formula, R 7 and R 8 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 9 and R 10 each represents a divalent alkylene group having 1 to 4 carbon atoms which may be linear or branched, m2 represents 0 to 23, n2 represents 0 to 23, and 23≧m2+n2≧2. [2]: R of the structural unit represented by the general formula (I) of the polymer 2 The composition for forming an organic film according to [1], characterized in that it contains a structure represented by the following general formula (IV) or (V): [ka] (In the formula, * indicates the bond position.) [3]: The composition for forming an organic film according to [1] or [2], wherein the resin for forming an organic film is a resin having an aromatic skeleton. [4]: The composition for forming an organic film according to any one of [1] to [3], characterized in that the content of the polymer is 0.01 parts by mass to 5 parts by mass, based on 100 parts by mass of the resin for forming an organic film. [5]: The composition for forming an organic film according to any one of [1] to [4], characterized in that the content of the resin for forming an organic film is 10 parts by mass to 40 parts by mass, based on 100 parts by mass of the composition for forming an organic film. [6]: A method for forming an organic film used in a manufacturing process of a semiconductor device, comprising spin-coating a composition for forming an organic film according to any one of [1] to [5] on a substrate to be processed, and heat-treating the substrate coated with the composition for forming an organic film at a temperature of 100°C to 600°C for 10 seconds to 600 seconds, thereby forming a cured film. [7]: A pattern forming method comprising the steps of forming an organic film on a workpiece using the organic film-forming composition according to any one of [1] to [5], forming a resist intermediate film on the organic film using a resist intermediate film material containing silicon atoms, forming a resist upper layer film on the resist intermediate film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the resist intermediate film by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the resist intermediate film on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask. [8]: A pattern forming method comprising the steps of forming an organic film on a workpiece using the organic film-forming composition according to any one of [1] to [5], forming a resist intermediate film on the organic film using a resist intermediate film material containing silicon atoms, forming an organic antireflective film or an adhesive film on the resist intermediate film, forming a resist upper layer film on the organic antireflective film or the adhesive film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film or the adhesive film and the resist intermediate film by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask. [9]: A pattern forming method comprising the steps of forming an organic film on a workpiece using the organic film-forming composition according to any one of [1] to [5], forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film, forming a resist upper layer film on the inorganic hard mask using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the inorganic hard mask by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.

[10] : A pattern forming method comprising the steps of forming an organic film on a workpiece using the organic film-forming composition according to any one of [1] to [5], forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film, forming an organic antireflective film or an adhesion film on the inorganic hard mask, forming a resist upper layer film on the organic antireflective film or the adhesion film using a resist upper layer film material consisting of a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film or adhesion film and the inorganic hard mask by etching using the resist upper layer film on which the circuit pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.

[11] : The pattern formation method according to [9] or

[10] , wherein the inorganic hard mask is formed by a CVD method or an ALD method.

[12] : The method for forming a pattern according to any one of [7] to

[11] , characterized in that in forming the circuit pattern, the circuit pattern is formed by lithography using light having a wavelength of 10 nm to 300 nm, direct writing with an electron beam, nanoimprinting, or a combination thereof.

[13] : The method for forming a pattern according to any one of [7] to

[12] , wherein in forming the circuit pattern, the circuit pattern is developed using an alkali developer or an organic solvent.

[14] : The pattern forming method according to any one of [7] to

[13] , characterized in that the workpiece is a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.

[15] : The pattern formation method according to

[14] , characterized in that the metal constituting the workpiece is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, molybdenum, or an alloy thereof.

[0200] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0201] 1...substrate; 2...processed layer; 2a...pattern formed on the processed layer; 3...organic film, 3a...organic film pattern, 4...silicon-containing resist intermediate film, 4a...silicon-containing resist intermediate film pattern, 5...resist upper layer film, 5a...resist upper layer film pattern, 6...exposed portion, 7...underlying substrate, 8...resist underlayer film

Claims

1. A composition for forming an organic film, comprising: a resin for forming an organic film; a polymer containing a structural unit represented by the following general formula (I) and at least one of a structural unit represented by the following general formula (II) and a structural unit represented by the following general formula (III); and a solvent, wherein the structural unit represented by the following general formula (I) and at least one of the structural units represented by the following general formula (II) and (III) form a random copolymer, and the polymer has a fluorine content of 5% by mass to 16% by mass. 【Chemistry 1】 (In the formula, R 1 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 2 is an organic group having 1 to 20 carbon atoms and containing a fluorine atom, which does not contain a sulfonyl group or an amino group. 【Chemistry 2】 (In the formula, R 3 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 4 and R 5 each represents a divalent alkylene group having 1 to 4 carbon atoms, which may be linear or branched; R 6 is a hydrogen atom or an alkyl group or a phenyl group having 1 to 4 carbon atoms, m1 is 0 to 23, n1 is 0 to 23, and 23≧m1+n1≧2. 【Chemistry 3】 (In the formula, R 7 and R 8 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, R 9 and R 10 are each a divalent alkylene group having 1 to 4 carbon atoms which may be linear or branched, m2 is 0 to 23, n2 is 0 to 23, and 23≧m2+n2≧2.

2. The structural unit R of the polymer represented by the general formula (I) 2 The composition for forming an organic film according to claim 1, characterized in that it contains a structure represented by the following general formula (IV) or (V): 【Chemistry 4】 (In the formula, * indicates the bond position.)

3. 2. The composition for forming an organic film according to claim 1, wherein the resin for forming an organic film is a resin having an aromatic skeleton.

4. 2. The composition for forming an organic film according to claim 1, wherein the content of the polymer is 0.01 to 5 parts by mass based on 100 parts by mass of the resin for forming an organic film.

5. 2. The composition for forming an organic film according to claim 1, wherein the content of the resin for forming an organic film is 10 parts by mass to 40 parts by mass, based on 100 parts by mass of the composition for forming an organic film.

6. A method for forming an organic film used in a manufacturing process of a semiconductor device, comprising spin-coating the composition for forming an organic film according to any one of claims 1 to 5 onto a substrate to be processed, and heat-treating the substrate coated with the composition for forming an organic film at a temperature of 100°C to 600°C for a period of 10 seconds to 600 seconds to form a cured film.

7. 6. A pattern forming method comprising the steps of: forming an organic film on a workpiece using the organic film-forming composition according to claim 1; forming a resist intermediate film on the organic film using a resist intermediate film material containing silicon atoms; forming a resist upper layer film on the resist intermediate film using a resist upper layer film material consisting of a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the resist intermediate film by etching using the resist upper layer film on which the circuit pattern has been formed as a mask; transferring the pattern to the organic film by etching using the resist intermediate film on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.

8. 6. A pattern forming method comprising the steps of: forming an organic film on a workpiece using the organic film-forming composition according to claim 1; forming a resist intermediate film on the organic film using a resist intermediate film material containing silicon atoms; forming an organic antireflective film or an adhesion film on the resist intermediate film; forming a resist upper layer film on the organic antireflective film or the adhesion film using a resist upper layer film material consisting of a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the organic antireflective film or the adhesion film and the resist intermediate film by etching using the resist upper layer film on which the circuit pattern has been formed as a mask; transferring the pattern to the organic film by etching using the resist intermediate film to which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.

9. 6. A pattern forming method comprising the steps of: forming an organic film on a workpiece using the composition for forming an organic film according to claim 1; forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming a resist upper layer film on the inorganic hard mask using a resist upper layer film material consisting of a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask by etching using the resist upper layer film on which the circuit pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.

10. 6. A pattern forming method comprising the steps of: forming an organic film on a workpiece using the composition for forming an organic film according to claim 1; forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming an organic antireflective film or an adhesion film on the inorganic hard mask; forming a resist upper layer film on the organic antireflective film or the adhesion film using a resist upper layer film material consisting of a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the organic antireflective film or the adhesion film and the inorganic hard mask by etching using the resist upper layer film on which the circuit pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.

11. 10. The pattern formation method according to claim 9, wherein the inorganic hard mask is formed by a CVD method or an ALD method.

12. 11. The pattern formation method according to claim 10, wherein the inorganic hard mask is formed by a CVD method or an ALD method.

13. 8. The pattern forming method according to claim 7, wherein the circuit pattern is formed by lithography using light having a wavelength of 10 nm to 300 nm, direct drawing with an electron beam, nanoimprinting, or a combination thereof.

14. 8. The method for forming a pattern according to claim 7, wherein in forming the circuit pattern, the circuit pattern is developed with an alkali developer or an organic solvent.

15. 8. The pattern forming method according to claim 7, wherein the workpiece is a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.

16. 16. The pattern formation method according to claim 15, wherein the metal constituting the workpiece is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, molybdenum, or an alloy thereof.

Citation Information

Patent Citations

  • Polymer compound containing fluoroaliphatic group

    JP2003221419A

  • Positive photosensitive composition

    JP2003262952A

  • Positive type resist material

    JP1994118651A

  • Pattern forming method, and material for forming underlayer film

    JP2004205685A

  • Photoresist underlayer film forming material and pattern forming method

    JP4355943B2