Radome for flying object

A self-healing ceramic radome with a laminated structure addresses thermal shock and aerodynamic heating issues by recrystallizing at the tip to prevent cracks and maintain structural integrity, enhancing durability and performance.

JP2024154820AActive Publication Date: 2024-10-31MITSUBISHI ELECTRIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023068921
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

Flying objects experience thermal shock and cracks due to rapid temperature changes at the radome tip, leading to potential structural failure from thermal stress and aerodynamic heating, especially at supersonic or hypersonic speeds.

Method used

A radome made of self-healing ceramic material with a laminated structure, where the tip is composed of a ceramic layer with a healing active layer that recrystallizes upon thermal shock, and the rear end has a thicker layer without the active layer, allowing for crack self-healing and reduced thermal conductivity.

Benefits of technology

The radome provides high thermal shock resistance and prevents crack propagation, maintaining structural integrity and reducing wear from aerodynamic heating and rain erosion without external heating or electricity, while allowing for smooth turning maneuvers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154820000001_ABST
    Figure 2024154820000001_ABST
Patent Text Reader

Abstract

To provide a radome for a flying object with high thermal shock resistance.SOLUTION: A radome for a flying object is installed in a front part of a flying object flying toward a target and is made of ceramic material with a pointed tip. The ceramic material at the tip of the radome is made of a self-repairing ceramic material whose recrystallization is accelerated by heat against cracks. The tip of the radome is subject to aerodynamic loading and aerodynamic heating, and is easily cracked. However, the present invention makes it possible to suppress crack propagation by self-repairing cracks using the aerodynamic heating during flight, even if cracks occur at the tip of the radome during flight.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a radome for an aircraft that protects an antenna for the aircraft. [Background technology]

[0002] A missile that flies toward a specific target by radio wave guidance is equipped with a radar antenna at its tip to detect the target. The tip of the missile is a part that is easily affected by aerodynamic load and aerodynamic heating. For this reason, the tip of the missile is generally made pointed (e.g., Cone, Ogive, Von Karman shape) to reduce aerodynamic resistance and enable high-speed flight.

[0003] In addition, since the radome needs to transmit the radio waves transmitted and received by the radar antenna, it must be made of a dielectric material, which includes ceramics such as alumina (Al2O3), cordierite (2MgO·2Al2O3·5SiO2), fused silica (SiO2), and sintered silicon nitride (Si3N4), as well as FRP (Fiber Reinforced Plastics).

[0004] The radomes of supersonic flying objects are mainly made of ceramic materials, which have excellent heat resistance and thermal shock resistance. The airframe of the object is generally made of materials with high rigidity and high thermal expansion coefficient (10 to 30×10-E6 / ℃), such as iron or aluminum. The radome and the airframe are made of different materials, and there is a concern about thermal stress caused by their combination. For this reason, the radome is generally fixed to the airframe via a ring made of FRP, which has high rigidity and a relatively low thermal expansion coefficient, and the radome and the ring are generally fixed with an adhesive.

[0005] Meanwhile, as a publicly known ceramic technology, there is a disclosure of a self-repairing ceramic material (e.g., Patent Documents 1 and 2). In a self-repairing ceramic material, recrystallization is promoted by a chemical reaction caused by heat and electricity in response to cracks that occur during manufacturing or handling, as well as thermal shock. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special table number 2018-511167 [Patent Document 2] International Publication No. 2013 / 008646 Summary of the Invention [Problem to be solved by the invention]

[0007] Some flying objects reach supersonic or hypersonic speeds in as short as a few seconds. Others fly for long periods of time, exposing the aircraft to high temperatures due to aerodynamic heating. The tip of the radome is near the stagnation point of aerodynamic heating, and in the past, it was prone to thermal shock due to a sudden rise in temperature. When thermal shock occurs, there is a problem that minute defects occur around the tip, which can lead to cracks in the radome. [Means for solving the problem]

[0008] The present invention has been made to solve these problems, and provides an aircraft radome that is installed in front of the aircraft, is made of a ceramic material and has a pointed tip, wherein the ceramic material at the tip is made of a self-repairable ceramic material in which recrystallization is promoted by heat in the event of cracks. Effect of the Invention

[0009] According to the present invention, there can be provided a radome for a flying object which is installed in front of the flying object and has high resistance to thermal shock caused by aerodynamic heating. [Brief description of the drawings]

[0010] [Figure 1] 1 is a side view of a flying object equipped with a flying object radome according to a first embodiment of the present invention. [Diagram 2] 1 is a diagram illustrating a cross section of an aircraft radome in accordance with a first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A radome for an airborne vehicle according to an embodiment of the present invention will be described below. Note that the present invention is not limited to the embodiment.

[0012] Embodiment 1 Fig. 1 is a side view showing a radome 100 according to this embodiment. The radome 100 is a ceramic object, and is installed in front of a body 200 of an aircraft. Fig. 2 is a cross-sectional view of the radome 100 according to this embodiment, taken along the line A-A' shown in Fig. 1. The radome 100 has a pointed shape and is made of a thin ceramic material S. The ceramic material S will be described in detail later. The inside of the radome 100 formed of the ceramic material S is a cavity, which is represented by a cavity 101 .

[0013] 1 and 2, the pointed end of the radome 100 is referred to as a tip portion 100A. The end portion opposite the front end portion 100A that is connected to the aircraft body 200 is referred to as a rear end portion 100B. In addition, the portion located between the front end portion 100A and the rear end portion 100B is referred to as an intermediate portion 100C.

[0014] An antenna (not shown) for a missile is installed in the cavity 101. The antenna is isolated from the surroundings of the radome 100 by the radome 100. The rear end 100B of the radome 100 as viewed from the airframe 200 to which the radome is connected has a round shape with an empty space inside, and the outer periphery is formed by the thin ceramics S.

[0015] As described above, the radome 100 is made of the ceramic material S. More specifically, it is made of laminated ceramics in which two layers of different ceramic materials are laminated. Of the two layers of ceramic material, the ceramic material located outside the radome 100 and in contact with the outside air surrounding the radome is referred to as a first ceramic material S1, and the ceramic material located inside the radome 100 and arranged on the cavity 101 side is referred to as a second ceramic material S2. The layer thickness of the first ceramic material S1 is t1, and the layer thickness of the second ceramic material S2 is t2. The layer thicknesses t1 and t2 differ depending on the position from the tip of the radome 100, as described later.

[0016] Hereinafter, each part of the radome 100 formed of the ceramic material S in which the first ceramic material S1 and the second ceramic material S2 are laminated will be described with reference to FIG.

[0017] 2, the front end 100A, rear end 100B, and middle portion 100C of the radome 100 are surrounded by dashed lines. Also, (a), (b), and (c) show the stacking conditions of the first ceramic material S1 and the second ceramic material S2 in the cross sections of the ceramic material S at the front end 100A, rear end 100B, and middle portion 100C.

[0018] First, the ceramic material S in the intermediate portion 100C is constructed by stacking a first ceramic material S1 having a layer thickness t1 and a second ceramic material S2 having a layer thickness t2 as shown in Figure 2(c), with the first ceramic material S1 being arranged on the surface that will be the outer side of the radome 100 and the second ceramic material S2 being arranged on the surface that will be the inner side.

[0019] On the other hand, the ceramic material S in the tip portion 100A is composed only of the first ceramic material S1 as shown in (a) of Fig. 2. The second ceramic material S2 is not laminated in the tip portion 100A.

[0020] As shown in FIG. 2(b), the ceramic material S at the rear end portion 100B has a thick layer of the second ceramic material S2, and the first ceramic material S1 is not laminated or is laminated only thinly.

[0021] In this manner, from the tip portion 100A to the intermediate portion 100C of the radome 100, the layer thickness of the second ceramic material S2 that is not laminated at the tip portion 100A gradually increases, while the layer thickness of the first ceramic material S1 gradually decreases. From the intermediate portion 100C to the rear end portion 100B, the layer thickness of the second ceramic material S2 further increases, and the layer thickness of the first ceramic material S1 decreases. As a result, the ratio of the layer thickness t1 of the first ceramic material S1 to the layer thickness t2 of the second ceramic material S2 changes continuously from the front end portion 100A to the rear end portion 100B.

[0022] Thus, the ceramic material S forming the radome 100 is composed only of the first ceramic material S1 at the front end of the radome 100, with no layer of the second ceramic material S2, and the layer thickness of the first ceramic material S1 decreases while the layer thickness of the second ceramic material S2 increases toward the rear end of the radome 100. At the rear end of the radome 100, there is no layer of the first ceramic material S1 or only a thin layer, and the layer configuration is such that the second ceramic material S2 is thickly layered. As a result, the ratio of the layer thickness of the first ceramic material S1 to the layer thickness of the second ceramic material S2 changes continuously from the front end portion 100A to the rear end portion 100B.

[0023] In this embodiment, the first ceramic material S1 is a ceramic material including a healing active layer. Ceramic materials containing a healing active layer are ceramics such as cordierite (2MgO 2Al2O3 5SiO2), fused silica (SiO2), and silicon nitride (Si3N4) sintered bodies, and refer to ceramics that are sintered after adding alumina (Al2O3) as an additive to liquid cordierite (2MgO 2Al2O3 5SiO2), fused silica (SiO2), silicon nitride (Si3N4), etc. before sintering. Ceramic materials containing a healing active layer are self-repairing ceramic materials, and in response to cracks that occur during manufacturing or handling as well as thermal shock, recrystallization is promoted by chemical reactions caused by heat and electricity.

[0024] On the other hand, the second ceramic material S2 is a ceramic material that does not have a healing active layer. Ceramic materials without a healing active layer are ceramics such as cordierite (2MgO 2Al2O3 5SiO2), fused silica (SiO2), and silicon nitride (Si3N4) sintered bodies, which do not contain any additives and are made by sintering liquid cordierite (2MgO 2Al2O3 5SiO2), fused silica (SiO2), silicon nitride (Si3N4), etc., before sintering.

[0025] Table 1 shows, as an example of an embodiment of the present invention, the layer thickness of the ceramic (first ceramic material S1) including a healing active layer and the layer thickness of the ceramic (second ceramic material S2) without a healing active layer at each distance from the tip of the radome 100.

[0026] [Table 1]

[0027] Next, the function of the first ceramic material S1 at the tip of the radome 100 while the flying object is in flight will be described.

[0028] In the radome 100 according to this embodiment, a ceramic material including a healing active layer is disposed at the tip portion, which is susceptible to the aerodynamic load and aerodynamic heating and where cracks are likely to occur. The healing active layer is a layer in which recrystallization is promoted in cracks due to a chemical reaction caused by heat and electricity, and its application to capacitors and electrical devices has been disclosed. In the healing active layer, for example, silicon carbide contained in the ceramic reacts to synthesize silicon dioxide, and this silicon dioxide reacts with alumina added to the ceramic as a filler to crystallize, promoting recrystallization of the cracks.

[0029] In this embodiment, ceramics including a healing active layer are placed at the tip of the radome 100, and even if a crack occurs due to a tiny defect that occurs around the tip, the crack can be self-repaired by utilizing the aerodynamic heating during flight, thereby making it possible to suppress the crack from progressing. For example, immediately after launch, a projectile experiences a large thermal shock due to the sudden change in speed, which is thought to make it more likely to develop defects, but at the same time, there is also a large temperature rise due to aerodynamic heating immediately after launch. Even if cracks are caused by the thermal shock immediately after launch, the temperature rise due to aerodynamic heating immediately after launch can provide the heat required for self-repair, and the propagation of the cracks can be suppressed.

[0030] Next, the function of the first ceramic material S1 on the outer periphery of the radome 100 during flight will be described. The flying object rotates during flight. Conventionally, the outer periphery of the radome 100 is subject to wear and tear due to rain erosion during flight, reducing its strength, and the load generated by the acceleration during rotation during flight may cause the radome to break. As a countermeasure to this, it is possible to reduce the stress generated in the radome by lowering the acceleration during rotation and reducing the load generated, but on the other hand, reducing the acceleration during rotation reduces the flight performance of the flying object.

[0031] In the radome 100 of this embodiment, a layer of ceramics including a healing active layer is arranged not only at the tip portion which is susceptible to aerodynamic loads and aerodynamic heating, but also on the entire outer periphery of the radome where strength decreases. By providing ceramics including a healing active layer with self-repair function on the entire outer periphery of the radome, resistance to wear due to rain erosion can be obtained. This allows the aircraft to turn without compromising flight performance.

[0032] In this manner, in the radome 100 of this embodiment, cracks that occur at the tip of the radome can be self-repaired by the temperature increase of the radome due to aerodynamic heating, without the need to supply heat and electricity from the outside to cause a chemical reaction and promote recrystallization. Furthermore, the outer periphery of the radome can be prevented from being worn down due to rain erosion, which would result in a decrease in strength.

[0033] Next, the functions of the first ceramic material S1 and the second ceramic material S2 at the rear end portion of the radome 100 will be described. Since the healing active layer contains a filler such as alumina, the ceramic layer including the healing active layer (first ceramic material S1) has the characteristic of having a higher density and thermal conductivity than the ceramic layer not including the healing active layer (second ceramic material S2). On the other hand, a material such as resin may be used between the rear end of the radome 100 and the airframe 200. For example, when the radome 100 and the airframe 200 are connected, the radome 100 and the airframe 200 are made of different materials, and thermal stress occurs due to the combination of the materials. For this reason, the radome 100 may be fixed to the airframe via a ring made of FRP (Fiber Reinforced Plastics) material, which has high rigidity and a relatively low thermal expansion coefficient, and in this case, an adhesive is assumed to be used between the radome 100 and the ring. Resin-based adhesives generally have low heat resistance, but ceramics containing a healing active layer have high thermal conductivity as described above, so heat flows from the front end to the rear end of the radome 100, and the rear end is likely to rise in temperature.

[0034] Therefore, in this embodiment, the ceramic material including the healing active layer is made thinner at the rear end portion of the radome 100, so that the apparent thermal conductivity of the radome 100 is changed. This makes it possible to suppress the flow of heat from the front end to the rear end, suppressing the rise in temperature and allowing the use of a resin-based adhesive.

[0035] As described above, the radome 100 according to the present embodiment is configured such that the front end portion is made of only the ceramic layer including the healing active layer, while the ceramic layer including the healing active layer is thin or absent at the rear end portion, and the ceramic layer not including the healing active layer is thick. From the front end portion to the rear end portion, the ratio of the layer thickness of the ceramic material including the healing active layer and the ceramic material not including the healing active layer is made to change continuously.

[0036] This allows the radome to self-repair any cracks that occur at the tip of the radome, suppresses wear due to rain erosion at the outer periphery of the radome that would result in a decrease in strength, and makes it possible to use a resin-based adhesive to fix the ring and radome.

[0037] In this embodiment, it has been described that alumina (Al2O3) filler is blended into the ceramic layer including the healing active layer. However, the filler to be added is not limited to alumina (Al2O3). By adding a filler with a fast reaction rate and a low change temperature, it is also possible to adjust the time for crack repair. For example, adding impurities such as manganese oxide (MnO) as a filler can speed up the reaction rate and promote the repair of cracks. In cases where the projectile is subjected to instantaneous external loads such as thermal shock, the load-bearing capacity can be improved by speeding up the repair of cracks.

[0038] The radome according to this embodiment has the following advantages during its manufacturing process. Throughout the life cycle of the radome, including during its manufacture, defects may occur on the surface of the radome. However, as in the radome of this embodiment, defects that occur in the ceramic layer including the healing active layer can be repaired by locally applying heat using a heater, which crystallizes the healing active layer. Alternatively, by applying a potential to a ceramic layer including a defective healing active layer while it is immersed in a reaction solution, an oxidation reaction progresses, causing the healing active layer to crystallize and be repaired. In this case, even if the radome is connected to the airframe, it is possible to partially repair defects that have occurred on the surface of the radome without having to detach it from the airframe and disassemble it.

[0039] Here, a method for manufacturing a radome will be described in which the front end portion of the radome 100 in this embodiment is made up of only the first ceramic material S1 (ceramic layer including a healing active layer) and does not have a layer of the second ceramic material S2 (ceramic layer without a healing active layer), and the thickness of the first ceramic material S1 decreases from the front end portion to the rear end portion while the thickness of the second ceramic material S2 increases, and at the rear end portion, the layer of the first ceramic material S1 is not laminated or is only thinly laminated, and the layer of the second ceramic material S2 is thickly laminated. A radome with such a layered structure can be manufactured, for example, by molding a radome without a self-healing layer, and then using the molded radome as an inner mold for casting and casting a liquid (slurry) containing an additive for the self-healing layer. [Explanation of symbols]

[0040] 100 radome, 100A tip portion, 100B rear end portion, 100C middle portion, 101 cavity, S ceramic material, S1 first ceramic material, S2 second ceramic material, 200 body of the missile.

Claims

1. A radome for an aircraft is installed in front of the aircraft, is made of a ceramic material, and has a pointed tip, 13. A radome for a spacecraft, comprising: a ceramic material at said tip, said ceramic material being capable of self-repair in which recrystallization is promoted by the application of heat to cracks.

2. 2. The airborne vehicle radome according to claim 1, characterized in that the self-repairable ceramic material is a sintered ceramic of cordierite (2MgO.2Al2O3.5SiO2), or fused silica (SiO2), or silicon nitride (Si3N4), and is sintered with alumina (Al2O3) or manganese oxide (MnO) added as an additive.

3. The ceramic material has a laminated structure in which a first ceramic material and a second ceramic material are laminated, the first ceramic material is disposed on an outer surface of the airframe radome that is in contact with the surrounding air, and the second ceramic material is disposed on an inner surface opposite to the outer surface; the ceramic material at the tip is composed only of the first ceramic material; The ceramic material at the rear end portion is composed of the first ceramic material and the second ceramic material having a layer thickness greater than that of the first ceramic material, or is composed of only the second ceramic material; From the front end to the rear end, the layer thickness of the first ceramic material becomes thinner and the layer thickness of the second ceramic material becomes thicker, the first ceramic material is the self-repairable ceramic material; 3. The radome for a spacecraft according to claim 1 or 2, characterized in that the second ceramic material is the non-self-repairable ceramic material, and is a ceramic of a sintered body of cordierite (2MgO.2Al2O3.5SiO2), or fused silica (SiO2), or silicon nitride (Si3N4), and is a ceramic material obtained by sintering liquid cordierite (2MgO.2Al2O3.5SiO2), or fused silica (SiO2), or silicon nitride (Si3N4) without adding any additives before sintering.

Citation Information

Patent Citations

  • Self-recovery function coating material and its production

    JP1995089779A

  • Radome for flying body

    JP2020186888A

  • Composite article having a ceramic nanocomposite layer

    US20110206937A1

  • Self-repairing capacitor and method for manufacturing the same

    JP2018511167A

  • Self-repairing laminated structure and self-bonding insulated wire

    WO2013008646A1