Lithium permselective membrane and manufacturing method for lithium permselective membrane
A lithium selectively permeable membrane with a simplified structure, utilizing a metal film layer on an A 2/3-x Li 3x TiO 3 ion conductor, addresses the complexity of existing lithium concentrators, enhancing lithium ion permeation efficiency and durability.
Patent Information
- Application Number
- JP2023069601
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
AI Technical Summary
Existing lithium concentrators have complex structures due to the need for mesh-like electrodes, which complicates the assembly and reduces the efficiency of lithium ion permeation.
A lithium selectively permeable membrane with a simplified structure is achieved by forming a metal film layer on at least one surface of an ion conductor made of A 2/3-x Li 3x TiO 3, where 0.04
The simplified structure enhances adhesion and efficiency of lithium ion permeation, allowing for effective concentration and recovery of lithium ions with improved conductivity and durability.
Smart Images

Figure 2024155152000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a lithium permselective membrane used to selectively allow lithium ions to pass through a liquid containing lithium ions by applying a voltage between electrodes, and a method for producing the lithium permselective membrane. [Background technology]
[0002] Lithium is a soft, silvery-white metal at room temperature and pressure, and because of its small ionic radius, it has a large charge / ionic radius ratio for an alkali metal, and the lowest standard redox potential among metallic elements. With such properties, lithium is widely used in batteries, additives for glass and ceramics, greases and lubricants for electrical and electronic devices, medicines, nuclear fusion fuel, etc. In particular, with the recent expansion of demand for lithium-ion secondary batteries and other batteries, lithium consumption is expected to increase further in the future.
[0003] Lithium is mainly produced from ores and salt lake brines, but it is also found in large amounts in seawater, and studies are being conducted on extracting lithium from seawater. Related technologies include those described in Patent Documents 1 and 2, for example.
[0004] Patent Document 1 proposes "a metal ion recovery device for recovering metal ions from an original solution, which is an aqueous solution containing metals in the form of metal ions, into a recovery liquid, the metal ion recovery device comprising a flat plate-shaped selectively permeable membrane made of an ion conductor of the metal, a mesh-shaped positive electrode fixed to one main surface of the selectively permeable membrane, and a mesh-shaped negative electrode fixed to the other main surface of the selectively permeable membrane, the original solution and the recovery liquid being separated by the selectively permeable membrane to which the positive electrode and the negative electrode are fixed." In this "metal ion recovery device," "the selectively permeable membrane is made of Li3N, Li 10 GeP2S 12 , (La x ,Li y )TiO z(where x=2 / 3-a, y=3a-2b, z=3-b, 0<a≦1 / 6、0≦b≦0.06、y> 0), Li 1+x+y Al x (Ti,Ge) 2-x S y P 3-y O 12 (where 0≦x≦0.6, 0≦y≦0.6)."
[0005] Patent Document 2 describes a lithium permselective membrane that selectively allows lithium (Li) ions to pass from one main surface side to the other main surface side, the lithium permselective membrane being characterized by comprising a selectively permeable membrane body mainly composed of a lithium ion conductor, and a lithium adsorption layer formed on the surface of the one main surface side of the selectively permeable membrane body and selectively adsorbing the lithium ions, and in which the ion conductor is (Li x ,La y )TiO z (where x=3a-2b, y=2 / 3-a, z=3-b, 0<a≦1 / 6、0≦b≦0.06、x> Patent Document 2 also describes "a lithium recovery device comprising a mesh-shaped first electrode fixed to the one main surface side of the lithium permselective membrane, and a mesh-shaped second electrode fixed to the other main surface side of the lithium permselective membrane." [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2015 / 020121 [Patent Document 2] JP 2017-131863 A Summary of the Invention [Problem to be solved by the invention]
[0007] In the lithium concentration devices as described in Patent Documents 1 and 2, as an ion conductor that selectively transmits lithium ions, A having high ionic conductivity, excellent stability and durability 2 / 3-x Li 3x TiO3 (0.04 < x < 0.14, A: one or more elements selected from lanthanoids) is considered to be effective.
[0008] By the way, in Patent Documents 1 and 2, those in which mesh-shaped positive and negative electrodes are fixed to each of both surfaces of a flat plate-shaped ion conductor by bonding or the like are used. In this case, it is necessary to attach the mesh-shaped electrodes to the ion conductor, and there is room for considering an alternative from the viewpoint of simplifying the structures of the ion conductor and the electrodes.
[0009] This invention addresses such problems, and its object is to provide a lithium selective permeation membrane capable of constructing a lithium concentration device with a relatively simple structure, and a method for manufacturing the lithium selective permeation membrane.
Means for Solving the Problems
[0010] The lithium selective permeation membrane of this invention selectively transmits the lithium ions by applying a voltage between electrodes in a liquid containing lithium ions, and has a membrane main body portion containing an ion conductor of lithium ions, and a metal film layer formed by being fixed to at least one of both surfaces of the membrane main body portion and used as the electrode, and the ion conductor contains a sintered body of an oxide represented by the following general formula (I). A 2 / 3-x Li 3x TiO3 (I) (In the general formula (I), x satisfies 0.04 < x < 0.14, and A is one or more elements selected from lanthanoids.)
[0011] The metal film layer preferably contains at least one selected from platinum group elements, and particularly preferably contains platinum.
[0012] The film thickness of the metal film layer is preferably 0.05 μm or more and less than 10 μm.
[0013] It is preferable that the lithium selective permeable membrane has the metal film layer formed on each of both surfaces of the film main body portion.
[0014] The metal film layer may be formed on the entire surface of the film main body portion, or may be partially formed so as to leave an exposed portion on the film main body portion. When formed partially, the metal film layer is preferably a network pattern continuously conducting with the current conducting portion for voltage application.
[0015] The method for manufacturing a lithium selective permeable membrane of the present invention is a method for manufacturing a lithium selective permeable membrane that selectively permeates lithium ions by applying a voltage between electrodes in a liquid containing lithium ions, comprising: performing electroless plating on a film-like member containing an ionic conductor of lithium ions using a plating solution containing metal ions, a complexing agent, and a reducing agent, to deposit a metal on at least one of both surfaces of the film-like member to form a metal film layer; and after the plating step, heating the film-like member having the metal film layer formed on at least one of both surfaces at a maximum reaching temperature of 700 °C or higher and a total heating time of 1 hour or longer, wherein the ionic conductor includes a sintered body of an oxide represented by the following general formula (I), and the method manufactures a lithium selective permeable membrane having a film main body portion as the film-like member and a metal film layer formed by adhering to at least one of both surfaces of the film main body portion and used as the electrode. A 2 / 3-x Li 3x TiO3(I) (In the general formula (I), x satisfies 0.04 < x < 0.14, and A is one or more elements selected from lanthanoids.)
[0016] The plating solution preferably contains at least one selected from the group consisting of boron hydride compounds, aminoborane compounds, and hydrazine compounds.
[0017] It is preferable that the plating solution further contains a hydroxymethyl compound represented by the following general formula (II) and / or a salt thereof. R1-CH2-OH (II) (In general formula (II), R1 is an atomic group having an aldehyde group or a ketone group.)
[0018] The plating solution preferably contains at least one soluble salt selected from the platinum group elements, particularly a platinum salt. Effect of the Invention
[0019] According to the lithium permselective membrane of the present invention, a lithium concentrating device can be constructed with a relatively simple structure. The method for producing the lithium permselective membrane of the present invention is suitable for producing such a lithium permselective membrane. [Brief description of the drawings]
[0020] [Figure 1] 1 is a cross-sectional view taken along a thickness direction, which diagrammatically illustrates a lithium permselective membrane according to one embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view taken along the depth direction, which diagrammatically illustrates a lithium concentrating device including the lithium permselective membrane of FIG. 1. FIG. [Diagram 3] FIG. 2 is a cross-sectional view taken along the thickness direction, which diagrammatically illustrates a lithium permselective membrane according to another embodiment of the present invention. [Figure 4] 4 is a cross-sectional view taken along the depth direction, which diagrammatically shows a lithium concentrating device including the lithium permselective membrane of FIG. 3. FIG. [Diagram 5] 1 is a photograph of the lithium permselective membrane of Example 1 after a peel test. [Figure 6] 1 is a photograph of the lithium permselective membrane of Comparative Example 1 after a peel test. [Figure 7] 1 is a photograph of the lithium permselective membrane of Comparative Example 2 after a peel test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0022] (Lithium selective permeable membrane) The lithium selective permeable membrane 1 illustrated in FIG. 1 has a membrane main body portion 2 containing an ion conductor, and metal film layers 3a and 3b formed by adhering to at least one of both surfaces 2a and 2b of the membrane main body portion 2, and in the embodiment of FIG. 1, to each of both surfaces 2a and 2b.
[0023] Here, the ion conductor constituting the membrane main body portion 2 has ion conductivity with respect to lithium ions as a so-called super lithium ion conductor, and inside thereof, lithium atoms or ions move and diffuse through sites in the crystal lattice. Thereby, the membrane main body portion 2 containing the ion conductor can selectively permeate substantially only lithium ions while inhibiting the permeation of other cations and anions. As a material for realizing this, in this embodiment, the ion conductor of the membrane main body portion 2 has the general formula (I): A 2 / 3-x Li 3x TiO3 (0.04 <x <0.14, A: one or more elements selected from lanthanoids) contains a sintered body of an oxide represented by. Note that in a cation exchange membrane used in general electrodialysis, not only lithium ions but also other cations permeate, so selective permeation of lithium ions cannot be achieved.
[0024] Also here, the metal film layers 3a and 3b are those that can be energized and are used as electrodes to which a voltage is applied. Details of the metal film layers 3a and 3b will be described later.
[0025] Such a lithium selective permeable membrane 1 can be used, for example, in the lithium concentration device 51 illustrated in FIG. 2. The lithium concentration device 51 in FIG. 2 includes a container-shaped concentration tank 52 capable of storing a liquid containing lithium ions therein, and the above-described lithium selective permeable membrane 1 disposed by being immersed in the liquid inside the concentration tank 52. The inside of the concentration tank 52 is partitioned into a stock solution chamber 52a and a concentration chamber 52b by the lithium selective permeable membrane 1 disposed therein.
[0026] When using the lithium concentrating device 51, the raw solution Ld containing lithium ions such as seawater is stored in the concentration tank 52, and a voltage is applied between the electrodes, with one metal coating layer 3a as the anode and the other metal coating layer 3b as the cathode. Then, as shown by the arrow in FIG. 2, the lithium ions in the raw solution Ld in the raw solution chamber 52a move toward the lithium selective permeable membrane 1, pass through the metal coating layer 3a, and reach the membrane body part 2. The lithium ions then permeate the inside of the membrane body part 2 due to the presence of an ion conductor, and further pass through the metal coating layer 3b to move to the concentration chamber 52b side. In this way, the raw solution Ld on the raw solution chamber 52a side has a decreased lithium ion concentration, while the liquid on the concentration chamber 52b side has an increased lithium ion concentration and becomes a concentrated solution Lc. Therefore, according to this, the lithium ions in the liquid can be concentrated. For example, by performing crystallization or the like on the concentrated solution Lc, the lithium contained therein can be recovered as lithium salt or the like.
[0027] Here, in the lithium selective permeable membrane 1 of this embodiment, the metal coating layers 3a and 3b are fixed to at least one of the two surfaces 2a and 2b of the membrane body 2. This eliminates the need to attach, for example, a mesh-shaped electrode member to the membrane body 2 by separate bonding or the like, and can simplify the structures of the electrodes and ion conductors of the lithium selective permeable membrane 1. Furthermore, compared to the case where a mesh-shaped electrode member is bonded to the membrane body 2, it is considered that the adhesion between the metal coating layers 3a and 3b and the membrane body 2 is improved, and the applied voltage is efficiently used for the permeation of lithium ions.
[0028] In the lithium selective permeable membrane 1 shown in Figures 1 and 2, the metal coating layers 3a and 3b are formed on both sides 2a and 2b of the membrane body 2, respectively, but as shown in Figure 3, a lithium selective permeable membrane 21 may be formed with a metal coating layer 23a on only one of both sides 22a and 22b of the membrane body 2. Even in the lithium selective permeable membrane 21 in which the metal coating layer 23a is provided on only one of both sides 22a and 22b, the above-mentioned advantages can be obtained for that one side.
[0029] As shown in FIG. 4, for example, the lithium selective permeable membrane 21 in FIG. 3 can be used in the lithium concentration device 51 by attaching a mesh-like electrode member 61 to the other one of the both surfaces 22a and 22b by bonding or the like. In this case, a voltage can be applied between the metal film layer 23a on one side and the electrode member 61 on the opposite side.
[0030] By the way, as described above, the ion conductor of the membrane main body 2 included in the lithium selective permeable membrane 1 contains a sintered body of an oxide represented by the general formula (I): A 2 / 3-x Li 3x TiO3. In the general formula (I), x satisfies 0.04 < x < 0.14, and A is one or more elements selected from lanthanoids. Since such a sintered body of an oxide exhibits high ionic conductivity and has excellent chemical stability, it may be effectively used in the lithium concentration device 51.
[0031] In particular, it is preferable that the ion conductor of the membrane main body 2 contains an oxide of La 2 / 3-x Li 3x TiO3 (0.04 < x < 0.14) in which A in the general formula (I) is La. The composite oxide having a perovskite crystal structure in which A in the general formula (I) is La may also be referred to as LLTO (registered trademark). For example, the general formula (I-a): La x Li 2-3x TiO 3-a SrTiO3, the general formula (I-b): La x Li 2-3x TiO 3-a La 0.5 K 0.5 TiO3, the general formula (I-c): La x Li 2-3x Ti 1-a M a O 3-a , or the general formula (I-d): Sr x-1.5a La a Li 1.5-2x Ti 0.5 Ta 0.5% or less, and the SiO2 content is 0.1% or less.
[0032] The fact that the film body 2 contains the oxide represented by the above general formula (I) can be confirmed by performing an X-ray diffraction method on the film body 2. In the X-ray diffraction method, the X-ray diffraction pattern of the film body 2 obtained by PANalytical X'pert Pro is compared with the ICDD database (PANalytical Example Database and PDF-4+ 2019RDB) to identify the oxide represented by the above general formula (I) contained in the film body 2.
[0033] Here, the X-ray diffraction pattern of the film main body 2 obtained by X-ray diffraction method and from which noise has been removed is compared with the ICDD database, and if it is determined that the X-ray diffraction pattern of the oxide represented by the general formula (I) is present in the X-ray diffraction pattern of the film main body 2, it is determined that the film main body 2 contains the oxide represented by the general formula (I). On the other hand, if it is determined that the X-ray diffraction pattern of the oxide represented by the general formula (I) is not present in the X-ray diffraction pattern of the film main body 2 by similarly comparing with the ICDD database, it is determined that the film main body 2 does not contain the oxide represented by the general formula (I).
[0034] In the oxide represented by the general formula (I) in the membrane body 2, a part of oxygen may be replaced by other elements such as F or Cl, or a part of transition metal may be replaced by other metals such as Fe, Cr, Ti, Nb, W, Mo, Na, K, Mg, or Ca. In addition, Li or oxygen may be excessive or deficient with respect to the stoichiometric composition of the oxide represented by the general formula (I). In addition, the crystal structure of the oxide represented by the general formula (I) in the membrane body 2 may be distorted. Even when a constituent element is substituted, deficient, or excessive with respect to the stoichiometric composition of the oxide as described above, or when a crystal structure is distorted, it is acceptable as the oxide represented by the general formula (I) as long as it does not significantly affect the properties of the membrane body 2 as an ion conductor. When the X-ray diffraction patterns of oxides lacking constituent elements or oxides with excess constituent elements are compared with the ICDD database, there is a possibility that the peaks may shift from the X-ray diffraction pattern of the oxide represented by the general formula (I). If such a peak shift is within ±10% of the reference value in the ICDD database, it is considered that the oxide represented by the general formula (I) is contained in the film body 2.
[0035] The oxide represented by the general formula (I) is preferably contained in the film body 2 at 99.0% by mass or more, and more preferably at 99.5% by mass or more. The oxide content is preferably as high as possible, and there is no particular upper limit, but it may be, for example, 99.999% by mass or less, typically 99.99% by mass or less. The oxide content is measured by ICP (Inductively Coupled Plasma). In addition to the oxide represented by the general formula (I), the film body 2 may contain at least one impurity selected from the group consisting of Si, Al, and Fe. The impurity content in the film body 2 is preferably 1.0% by mass or less, more preferably 0.5% by mass or less.
[0036] The thickness of the membrane body 2 may be, for example, 0.1 mm to 10.0 mm, typically 0.2 mm to 2.0 mm. By making the membrane body 2 to have a certain thickness, the occurrence of defects can be suppressed and the required strength can be ensured, and by not making it too thick, lithium ions can permeate at a good speed. The thickness of the membrane body 2 can be measured with a vernier caliper.
[0037] Moreover, each of the metal coating layers 3a and 3b preferably contains at least one selected from platinum group elements (ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir) and platinum (Pt)). This is because platinum group elements have high corrosion resistance even when a voltage is applied. When a plurality of platinum group elements are contained, the total content of the platinum group elements in the metal coating layers 3a and 3b is preferably 80% by mass to 100% by mass. Each of the metal coating layers 3a and 3b preferably contains platinum (Pt) among the platinum group elements. This is because platinum has particularly high corrosion resistance and effectively adheres to the membrane body 2 containing the ion conductor. If the content of the platinum group elements or platinum is too small, the corrosion resistance may decrease and the layers may peel off. The metal coating layers 3a and 3b containing a platinum group element may further contain at least one selected from the group consisting of nickel (Ni), cobalt (Co), boron (B), carbon (C), nitrogen (N), oxygen (O), phosphorus (P) and sulfur (S) in an amount of 0.1% by mass to 30% by mass.
[0038] The presence of platinum group elements in the metal coating layers 3a and 3b can be confirmed by X-ray fluorescence spectroscopy (XRF), energy dispersive X-ray spectroscopy (EDX) or X-ray diffraction (XRD), and the content can be measured by analysis using X-ray fluorescence spectroscopy (XRF) or energy dispersive X-ray spectroscopy (EDX). In the metal coating layers 3a and 3b containing one or more elements of the platinum group elements, the elements may often exist in the form of a simple metal or an alloy, but are not limited thereto.
[0039] The thickness of the metal coating layers 3a, 3b may be, for example, 0.01 μm to 20 μm, typically 0.05 μm or more and less than 10 μm. This is to suppress costs by not making the layers too thick, while making them thick to a certain extent to improve conduction. The thickness of the metal coating layers 3a, 3b can be measured by X-ray fluorescence spectroscopy (XRF). The lithium permselective membrane 1 manufactured by a manufacturing method including a plating step as described below may have the metal coating layers 3a and 3b formed as plating layers on at least one of both sides 2a and 2b of the membrane body 2.
[0040] (Manufacturing method) To manufacture the lithium permselective membrane as described above, for example, a plating step and an annealing step may be sequentially performed on a membrane member containing an ion conductor for lithium ions.
[0041] The ion conductor of the membrane member is represented by the above-mentioned general formula (I): A 2 / 3-x Li 3x It includes a sintered body of an oxide represented by TiO3. The film member may be obtained by purchasing a pre-fabricated one, or may be fabricated as described below. However, the fabrication method is not limited to this.
[0042] Lithium compounds such as lithium hydroxide and lithium carbonate are used as lithium raw materials, and titanium compounds such as titanium oxide, metatitanic acid, and orthotitanic acid are used as titanium raw materials (for example, average particle size D50: 0.1 μm to 1.0 μm, BET specific surface area: 5.0 m 2 / g~100.0m 2 In this case, powders of lanthanum oxide are prepared as a lanthanum raw material, and if necessary, hydroxide, chloride and / or carbonate of at least one element selected from the group consisting of Sr, K, Fe, Ga and Ta are also prepared.
[0043] Next, in the first wet grinding step, the lithium raw material, titanium raw material, lanthanum raw material, and other raw materials are mixed in a predetermined molar ratio with a mixed solvent such as pure water and ethanol in a ball mill or the like and ground. After grinding, the mixture is dried using a spray dryer, fluidized bed dryer, tumbling granulator dryer, freeze dryer, hot air dryer, or the like to obtain a first ground powder.
[0044] Then, in the calcination step, the first pulverized powder is heated at 1000° C. to 1200° C. for 1 hour to 12 hours in an oxygen or air atmosphere or an inert gas atmosphere such as nitrogen, thereby obtaining a calcined powder.
[0045] Then, in the second wet pulverization step, the calcined powder is pulverized with the addition of a solvent in a ball mill or the like and then dried to obtain a second pulverized powder. Then, in the dry pulverization step, the second pulverized powder is dry pulverized using a ball mill or the like, and further, if necessary, microparticulated using a dry or wet jet mill or the like to obtain an oxide powder.
[0046] The oxide powder is then subjected to a molding process in which it is uniaxially compressed at, for example, 80 MPa to 120 MPa, preferably 100 MPa to 120 MPa, to obtain a green body. This green body is then subjected to a sintering process in which it is heated to, for example, 1300°C to 1450°C, preferably 1350°C to 1450°C. As a result, a compound represented by the general formula (I):A 2 / 3-x Li 3x A film member containing a sintered body of an oxide represented by TiO3 is obtained.
[0047] In the plating step, the film-like member is subjected to electroless plating using a plating solution containing metal ions, a complexing agent, and a reducing agent, whereby metal is precipitated on at least one of both surfaces of the film-like member to form a metal coating layer as a plating layer.
[0048] The metal ions contained in the plating solution can be appropriately determined according to the composition of the metal coating layer of the lithium selective permeable membrane to be manufactured. When forming a metal coating layer containing at least one selected from platinum group elements (ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir) and platinum (Pt)), the plating solution contains at least one soluble salt selected from the platinum group elements. In particular, when forming a metal coating layer containing platinum (Pt), a plating solution containing a platinum salt is used.
[0049] When the plating solution contains at least one soluble salt selected from platinum group elements, the metal ion concentration of the platinum group elements is preferably 0.01 g / L to 20 g / L in total when multiple types are contained. When the plating solution contains platinum salt, the platinum ion concentration is preferably 0.1 g / L to 5 g / L. If the concentration of the platinum group elements or platinum is too low, the plating speed may decrease, and if it is too high, there is a concern that the plating solution will be expensive.
[0050] The reducing agent contained in the plating solution is preferably at least one selected from the group consisting of boron hydride compounds, aminoborane compounds, hydrazine compounds, hypophosphorous compounds, phosphorous compounds, formic acid compounds, and formaldehyde. This is because these compounds act as reducing agents that can provide a sufficient plating speed at low cost. The reducing agent is preferably contained in the plating solution at 0.01 g / L to 100 g / L. If the amount of the reducing agent is too small, there is a concern that the plating speed will decrease. On the other hand, if the amount of the reducing agent is too large, the stability of the plating solution may decrease. Depending on the type of reducing agent, the metal film layer formed on the film-like member may contain boron, nitrogen, and / or phosphorus.
[0051] The complexing agent contained in the plating solution is preferably at least one selected from the group consisting of polyamine compounds (compounds having multiple amino groups (-NH2)) such as ethylenediamine, propanediamine, diethylenetriamine, tetraethylenepentamine, and pentaethylenehexamine, and ammonia. These compounds are also preferable from the viewpoints of good electroless plating performance, ease of dissolution in water, ease of availability, low cost, and the like. The complexing agent is preferably contained in the plating solution in an amount that can be coordinated to the metal ions in the plating solution in an equivalent amount or more, specifically, 0.1 g / L to 300 g / L. If the amount of the complexing agent is too small, there is a concern that the stability of the plating solution will decrease. On the other hand, if the amount of the complexing agent is too large, the plating speed may decrease.
[0052] The anti-pattern deposition agent to be added to the plating solution is preferably a hydroxymethyl compound and / or a salt thereof represented by the general formula (II): R1-CH2-OH (R1: an atomic group having an aldehyde group or a ketone group). This prevents the plating film from protruding from the area other than the area to which the catalyst is applied, and plating is performed only in the required area, so that a metal film layer can be formed as a suitable pattern electrode. Specific examples include sugar, ascorbic acid, erythorbic acid, and the like. The anti-pattern deposition agent is preferably added to the plating solution at 0.01 g / L to 10 g / L. If the amount of the anti-pattern deposition agent is too small, there is a concern that the pattern formation may be defective. On the other hand, if the amount of the anti-pattern deposition agent is too large, the plating speed may decrease. In addition, when a metal film layer is formed on the entire surface of the film-like member, rather than in a pattern shape, it is not necessary to add the anti-pattern deposition agent to the plating solution.
[0053] The pH of the plating solution is preferably 7 or higher. If the pH is too low, the plating speed may decrease. Typically, the pH of the plating solution may be 9 to 14.
[0054] Electroless plating using such a plating solution can be carried out according to a known method. For example, a film-like member is immersed in the plating solution. Then, metal ions are precipitated on the surface of the film-like member by the action of a reducing agent in the plating solution, and a metal coating layer having a composition corresponding to the metal ions is formed on the surface. For example, by applying a mask, it is possible to select whether to form a metal coating layer on one or both of the two surfaces of the film-like member.
[0055] After the plating process, an annealing process is performed to increase the adhesion of the metal coating layer to the film-like member. In the annealing process, the film-like member with the metal coating layer formed on at least one of its two sides is heated. Here, the total heating time from the start of heating to the end of cooling is set to 1 hour or more, and the maximum temperature reached during that time is set to 700°C or more.
[0056] If the maximum temperature in the annealing step is less than 700°C or if the total heating time is less than 1 hour, the adhesion of the metal coating layer to the film member cannot be improved significantly. On the other hand, if the maximum temperature is too high, the film member may be altered. For this reason, the maximum temperature is preferably 700°C to 1400°C. If the total heating time is too long, the adhesion will not increase any more, and the manufacturing efficiency will decrease. Therefore, the total heating time can be 0.5 hours to 10 hours, particularly 1 hour to 10 hours.
[0057] In the annealing step, for example, the temperature increase rate may be 1° C. / min to 20° C. / min, the holding time at the maximum temperature may be 0 minutes to 120 minutes, and the temperature decrease rate may be 1° C. / min to 20° C. / min.
[0058] By the annealing step, a metal coating layer is fixed to at least one of both sides of the film-like member, and a lithium selective permeable membrane is obtained with the film-like member as the film main body. However, the lithium selective permeable membrane may be manufactured by plating methods other than electroless plating, sputtering, various vapor deposition methods, and the like, and is not limited to the manufacturing method using electroless plating described in detail here. EXAMPLES
[0059] Next, a lithium permselective membrane according to the present invention was fabricated and its performance was confirmed, which will be described below, however, the description here is merely an example and is not intended to be limiting.
[0060] Example 1 The thickness is about 0.5 mm. 0.57 Li 0.29 An attempt was made to form a metal coating layer on a film-like member (LLTO (registered trademark) manufactured by Toho Titanium Co., Ltd.) containing a sintered body of an oxide represented by TiO3 as an ion conductor by electroless plating.
[0061] In the electroless plating, first, a few drops of a 30g / L aqueous solution of chloroplatinic acid were applied to the film-like member, and after drying, the member was immersed in a 10g / L aqueous solution of sodium borohydride to provide a platinum catalyst. The film-like member to which the catalyst was applied was immersed in a plating solution at 30°C for 20 hours, depositing platinum (Pt) to a thickness of 1μm on each side of the film-like member, forming a metal film layer on both sides. For this plating solution, plating solution A was used, which contained 0.2g / L of tetraammineplatinum (II) nitrate as platinum salt, 0.35mL / L of 80% hydrazine monohydrate, and 1mL / L of 25% ammonia, and had a pH of 12.2.
[0062] After electroless plating, tests were performed with or without annealing, and with varying maximum temperature when annealing was performed, as shown in Table 1. The annealing was performed with a temperature rise time of 1 hour, and immediately after reaching the maximum temperature, the temperature was lowered, resulting in a temperature drop time of 8 hours, and a total heating time of 9 hours. In this way, a lithium permselective membrane was produced with the membrane member as the membrane main body.
[0063] Comparative Example 1 A metal film layer was formed on the film member using Paste A (platinum paste (product name TR-7605, manufactured by Tanaka Kikinzoku Co., Ltd.)) to produce a lithium permselective membrane.
[0064] Specifically, first, 12 g of paste A was diluted with 7.2 g of ethanol. Then, a membrane member was set on a spin coater (ACT-300A II, manufactured by Active Co., Ltd.), and in an air atmosphere (temperature 20°C, humidity 30%), while dropping 0.5 g of platinum paste with a dropper, the membrane member was spin-coated under the conditions of 500 rpm for 10 seconds, then spin-coated under the conditions of 1000 rpm for 10 seconds, and further, spin-coated in three stages under the conditions of 3000 rpm for 30 seconds.
[0065] Then, drying was performed at 60°C for 2 hours with a dryer, heat treatment was performed at 400°C (heating rate: 1.7°C / min) for 2 hours, and then heat treatment was performed at 930°C (heating rate: 10°C / min) for 2 hours.
[0066] Through the above steps, a lithium selective permeation membrane provided with a metal film layer formed of platinum paste on a membrane member was manufactured.
[0067] (Comparative Example 2) A lithium selective permeation membrane was manufactured in the same manner as in Comparative Example 1, except that paste A in Comparative Example 1 was replaced with paste B (product name: TR-7905, manufactured by Tanaka Kikinzoku Kogyo K.K.).
[0068] (Comparative Example 3) La 2 / 3-x Li 3x A membrane member containing a sintered body of an oxide represented by TiO3 (0.04 < x < 0.14) as an ion conductor (LLTO (registered trademark) manufactured by Toho Titanium Co., Ltd.) was used as the lithium selective permeation membrane without forming a metal film layer on the membrane member.
[0069] (Comparative Example 4) As the membrane member, Li 6.25 La3Zr2Al 0.25 O 12 A membrane member containing a sintered body of an oxide represented by (so-called LLZO) as an ion conductor (Li 6.25 La3Zr2Al 0.25 O 12A lithium permselective membrane was produced in the same manner as in Example 1, except that LLZO (cubic) was used. LLZO is an unstable substance in air, and its surface reacts with moisture in the air to become lithium hydroxide, which then reacts with carbon dioxide in the air to become covered with a layer of lithium carbonate. To eliminate this effect, in Comparative Example 4, the LLZO surface was polished with #1200 commercially available abrasive paper before electroless plating to expose a fresh LLZO surface.
[0070] (evaluation) It was confirmed whether or not a metal coating layer could be formed on both sides of the film-like member by each method of Example 1 and Comparative Examples 1, 2, and 4. The results are shown in Table 1. In Table 1, "◯" means that a metal coating layer was formed, and "×" means that the entire surface of the film-like member was exposed after plating, and a metal coating layer could not be formed.
[0071] As shown in Table 1, in Example 1, a metal coating layer could be formed on both sides of the film member without annealing and when the maximum temperature reached during annealing after electroless plating was set to 600° C. or higher. In Comparative Examples 1 and 2, when no annealing was performed and when the maximum annealing temperature was set to 600° C. or higher and 930° C. or lower, a metal coating layer could be formed on both sides of the film member. A metal coating layer could not be formed in Comparative Example 4. This is believed to be because when the film-like member containing LLZO was immersed in the plating solution, the plating solution was strongly alkaline, and thus hydroxides and lithium platinum oxide (Li2PtO3) were formed on the LLZO surface, preventing the formation of a metal coating layer.
[0072] For each of the lithium selective permeable membranes manufactured as described above, a peel test was performed to confirm the adhesion of the metal coating layer from the membrane body, and ion conductivity was measured. The results are shown in Tables 1 and 2. In Comparative Example 3, the membrane member was used as the lithium selective permeable membrane as it was, so the above-mentioned adhesion confirmation measurement was not performed. In Comparative Example 4, the metal coating layer could not be formed, so the above-mentioned adhesion confirmation and ion conductivity measurement were not performed.
[0073] In the peel test, a transparent adhesive tape manufactured by 3M was attached to the surface of the metal coating layer formed on the membrane body of the lithium selective permeable membrane, and the tape was pulled in the direction of peeling the metal coating layer from the membrane body to confirm whether the metal coating layer peeled off from the membrane body. In Table 1, "◯" means that the metal coating layer did not peel off at all from the membrane body, "△" means that only a small part of the metal coating layer peeled off from the membrane body, but at a level that is not problematic in practical use, and "×" means that the metal coating layer peeled off entirely from the membrane body, at a level that is problematic in practical use. For reference, photographs of each lithium selective permeable membrane after the peel test in Example 1 and Comparative Examples 1 and 2 are shown in Figures 5 to 7.
[0074] The ion conductivity was measured as follows. A metal coating layer was attached to both sides of a lithium permselective membrane plate (Φ12 mm) in Examples 1, Comparative Examples 1 and 2, and a Pt vapor deposition film was attached to the other in Comparative Example 3, and the result was sandwiched between stainless steel electrodes. Here, the metal coating layer and the Pt vapor deposition film were used as electrodes. Then, using an impedance analyzer E4990A (manufactured by Keysight Technologies), Nyquist plots were measured at a measurement frequency of 20 Hz to 20 MHz, and the resistance values of the grains and grain boundaries were read from the measurement data. The lithium ion conductivity was calculated using the following formula. Lithium ion conductivity (Scm -1 )=1 / (Rb+Rgb)×(L / S) Rb: Resistance value within the grain (Ω) Rgb: Resistance of grain boundary (Ω) L: Thickness of the plate-shaped lithium lanthanum titanium oxide (cm) S: electrode area (cm 2 )
[0075] As can be seen from Table 2, the lithium permselective membrane of Example 1 exhibited higher ionic conductivity than those of Comparative Examples 1 and 2. For this reason, it is expected that the lithium permselective membrane of Example 1 can be suitably used in a lithium concentrating device.
[0076] [Table 1]
[0077] [Table 2]
[0078] From the above, it was suggested that the lithium permselective membrane of the present invention may enable the construction of a lithium concentrating device with a relatively simple structure. [Explanation of symbols]
[0079] 1, 21 Lithium permselective membrane 2, 22 Membrane body 2a, 2b, 22a, 22b Both sides of the membrane body 3a, 3b, 23a Metal coating layer 51 Lithium enrichment device 52 Concentrator 52a Stock solution room 52b Concentration room Ld stock solution Lc concentrate
Claims
1. A lithium permselective membrane that selectively allows lithium ions to pass through a liquid containing lithium ions by applying a voltage between electrodes, comprising: A membrane body portion including an ion conductor of lithium ions and a metal coating layer formed and fixed to at least one of both surfaces of the membrane body portion and used as the electrode, The ion conductor comprises a sintered body of an oxide represented by the following general formula (I): A 2 / 3-x Li 3x TiO 3 (I) (In the general formula (I), x satisfies 0.04<x<0.14, and A is one or more elements selected from the lanthanoids.)
2. 2. The lithium permselective membrane according to claim 1, wherein the metal coating layer contains at least one element selected from the platinum group metals.
3. 3. The lithium permselective membrane according to claim 2, wherein the metal coating layer contains platinum.
4. 4. The lithium permselective membrane according to claim 1, wherein the metal coating layer has a thickness of 0.05 μm or more and less than 10 μm.
5. 4. The lithium permselective membrane according to claim 1, wherein the metal coating layer is formed on both sides of the membrane body.
6. A method for producing a lithium permselective membrane that selectively allows lithium ions to pass through a liquid containing lithium ions by applying a voltage between electrodes, comprising the steps of: The method includes a plating step of electrolessly plating a film member including an ion conductor of lithium ions using a plating solution including metal ions, a complexing agent, and a reducing agent to deposit a metal on at least one of both surfaces of the film member to form a metal coating layer, and an annealing step of heating the film member having the metal coating layer formed on at least one of both surfaces after the plating step at a maximum temperature of 700° C. or higher for a total heating time of 1 hour or more, The ion conductor includes a sintered body of an oxide represented by the following general formula (I): A method for producing a lithium selective permeable membrane, comprising: producing a lithium selective permeable membrane having a membrane main body portion as the membrane-like member; and a metal coating layer formed and fixed to at least one of both surfaces of the membrane main body and used as the electrode. A 2 / 3-x Li 3x TiO 3 (I) (In the general formula (I), x satisfies 0.04<x<0.14, and A is one or more elements selected from the lanthanoids.)
7. 7. The method for producing a lithium permselective membrane according to claim 6, wherein the plating solution contains at least one compound selected from the group consisting of boron hydride compounds, aminoborane compounds, and hydrazine compounds.
8. The method for producing a lithium permselective membrane according to claim 6 or 7, wherein the plating solution further contains a hydroxymethyl compound represented by the following general formula (II) and / or a salt thereof: R1-CH 2 -OH (II) (In general formula (II), R1 is an atomic group having an aldehyde group or a ketone group.)
9. 8. The method for producing a lithium permselective membrane according to claim 6, wherein the plating solution contains at least one soluble salt selected from the platinum group elements.
10. The method for producing a lithium permselective membrane according to claim 9 , wherein the plating solution contains a platinum salt.
Citation Information
Patent Citations
Lithium permselective membrane, lithium recovery apparatus, lithium recovery method, hydrogen production method
JP2017131863A
Metal ion recovery device and metal ion recovery method
WO2015020121A1
Cited By
Preparation of lithium hydroxide by improved llto membrane dialysis
EP4813507A1
Llto membrane, its production and use
EP4813508A1
LLTO membrane, production thereof and use thereof
WO2026201710A1
Production of lithium hydroxide by improved LLTO membrane dialysis
WO2026201711A1