Calculation method for thickness of inner oxide layer of martensitic heat-resistant steel in steam environment
A method for calculating the inner oxide layer thickness in martensitic heat-resistant steel considering steam temperature and pressure enhances prediction accuracy, reducing the risk of pipe rupture and extending component life.
Patent Information
- Application Number
- JP2023087183
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2023-05-26
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Current steam oxidation kinetic models for martensitic heat-resistant steels fail to accurately predict the thickness of the oxide layer due to neglecting the influence of steam pressure, leading to inaccurate evaluation of component life and increased risk of pipe rupture.
A method to calculate the inner layer thickness of the oxide layer in martensitic heat-resistant steel considering both steam temperature and pressure, using a formula that integrates these factors with fitting coefficients to enhance prediction accuracy.
The method allows for precise estimation of the oxide layer thickness, reducing the risk of pipe rupture by improving prediction accuracy to within 6% error, thus ensuring safe operation and extending the service life of high-temperature components.
Smart Images

Figure 2024155649000015 
Figure 2024155649000016 
Figure 2024155649000017
Abstract
Description
[Technical field]
[0001] The present invention belongs to the technical field of martensitic heat-resistant steel, and more particularly to a method for calculating the thickness of the inner oxide layer of martensitic heat-resistant steel in a steam environment. [Background technology]
[0002] Martensitic heat-resistant steels include 9-12%Cr heat-resistant steels such as T / P91, T / P92, E911, T / P93 (9Cr-3W-3Co), T / P122, etc. Martensitic heat-resistant steels have excellent high-temperature creep strength, good thermal conductivity and low linear expansion coefficient, and are widely applied to important high-temperature components such as main steam pipes, headers, superheaters, reheaters, etc. for manufacturing ultra-(super)critical units. With the improvement of the operating steam pressure of the unit, the steam oxidation resistance performance of martensitic heat-resistant steels becomes one of the important factors affecting the service life of high-temperature components. In the long-term operation process of high-temperature components, the thickness of the oxidation layer increases, so the effective thickness of the tube wall decreases, and the stress of the tube wall also increases correspondingly, and the oxidation layer also causes the deterioration of the thermal conductivity performance of the tube wall, improves the average operating temperature of the tube wall, and when the tube wall is in a long-term overheating service state and develops to a certain extent, it will eventually lead to the occurrence of a tube rupture accident. Therefore, it is very necessary to predict the thickness of the oxide layer of steam-serviced components such as superheaters, reheaters, etc., in order to evaluate the service life of the components, realize early warning, and reduce the occurrence of accidents.
[0003] The calculation of the thickness of the inner layer of the oxide film requires the use of the oxidation kinetic model of heat-resistant steel in a steam environment. At present, the steam oxidation kinetic models of martensitic heat-resistant steels at home and abroad generally only consider the effect of steam temperature, and rarely consider the effect of the change in steam pressure, especially without considering the comprehensive effect of the combined action of the two. In reality, the parameters of steam temperature and steam pressure in different components of a unit are significantly different, for example, the steam temperature of the high-temperature reheater is higher than that of the superheater, but the steam pressure is obviously lower than that of the superheater. Therefore, only by considering the comprehensive effect of steam temperature and steam pressure can the thickness of the oxide layer of different components be accurately predicted, and even their remaining service life be predicted. In addition, at present, the steam oxidation kinetic models of martensitic heat-resistant steels are obtained based on the experimental results of the oxidation gravimetric method, and the thickness of the oxide layer cannot be directly calculated. A few documents have reported high-temperature steam oxidation kinetic models of martensitic heat-resistant steels based on the increase in the thickness of the oxide layer, but the oxide layer includes the inner layer and the outer layer, and these documents do not distinguish between the thickness of the outer layer and the thickness of the inner layer. According to the applicant's research, predicting the thickness of the inner oxide layer has more practical meaning, since only an increase in the thickness of the inner oxide layer will result in thinning of the tube wall, which will affect the service life of the tube. Summary of the Invention [Problem to be solved by the invention]
[0004] In order to solve the problems existing in the prior art, the present invention provides a method for calculating the thickness of the inner oxide layer of martensitic heat-resistant steel in a steam environment, which can easily and quickly calculate the thickness of the inner oxide layer of 9%Cr martensitic heat-resistant steel in steam based on the steam temperature, steam pressure and operation time, significantly improving the calculation accuracy, and enabling the evaluation of the remaining service life of high-temperature components by measuring without cutting the tubes during the actual operation of the power plant, which ensures the safe operation of the unit, reduces costs, and has important industrial application value. [Means for solving the problem]
[0005] In order to achieve the above object, the technical means used in the present invention are as follows.
[0006] A method for calculating the thickness of an inner oxide layer of a martensitic heat-resistant steel in a steam environment is provided, the martensitic heat-resistant steel being a 9% Cr heat-resistant steel, and the calculation formula for the thickness of the inner oxide layer in the steam environment is Y=ω×Y T +(1-ω)×Y p (1) Where:
[0007]
number
[0008] In the above technical means, the steam temperature ranges from 550 to 650° C., and the steam pressure ranges from 5.0 to 25.0 MPa.
[0009] In the above technical means, the time range is 1000 to 150000 hours.
[0010] In the above technical means, in the calculation formula of Y, When the steam temperature T<600° C., the value of ω is 0.1682±0.1136; When the steam temperature T≧600° C., the value of ω is 0.6891±0.2269.
[0011] In the above technical means, the Y T In the calculation formula for the thickness of the inner layer of the steam oxidation layer of the martensitic heat resistant steel, n=0.25.
[0012] In the above technical means, the Y T In the formula, the mathematical relationship between the k and the temperature T is k = 1.01 × 10 -42 T 14.68 It is.
[0013] In the above technical means, the Y T In the formula, the mathematical relationship between the activation energy Q and the time t is Q = 106661.33557 - 0.36498t + 3.07915 × 10 -6 t 2 It is.
[0014] In the above technical means, the Y p In the above formula, the value of the fitting coefficient a is 22.21, the value of the fitting coefficient b is 0.0009334, the value of the fitting coefficient c is −0.8198, and the value of the fitting coefficient d is −7.655×10 -10 and the value of the fitting coefficient h is 1.79×10 -5 and the value of the fitting coefficient i is 0.1152.
[0015] The application of the above calculation method in evaluating the service life of martensitic heat-resistant steel components operating with steam in power plants is provided.
[0016] In the above technical means, the steam temperature is 550 to 650° C., and the steam pressure is 5.0 to 25.0 MPa.
[0017] In the present invention, the relationship between the thickness Y of the inner oxide layer and the steam temperature T or steam pressure p is first studied separately, and then a weight analysis is carried out on the magnitude and degree of the influence of temperature and pressure on the thickness of the inner oxide layer. It is found that the weight of the influence of temperature on the thickness of the inner oxide layer is different in different temperature ranges due to the combined action of steam temperature and pressure. Finally, the formula is mathematically corrected based on the traditional exponential model by combining actual data, and a calculation formula for the thickness of the inner oxide layer of 9%Cr martensitic heat-resistant steel steam is provided, which integrates three factors, namely, steam temperature, steam pressure and operation time. There is no need to cut the tube to measure, which reduces costs and realizes the estimation of the thickness of the oxide layer of the tube without affecting operation. In addition, the calculation of the thickness of the inner oxide layer of 9%Cr martensitic heat-resistant steel using this formula can accurately reflect the degree of oxidation corrosion of the inner wall of the tube, and provides basic data for calculating the remaining service life of the component. Effect of the Invention
[0018] The beneficial effects of the present invention are as follows:
[0019] 1. According to the present invention, the thickness of the inner oxide layer of martensitic heat-resistant steel in a supercritical steam environment is first studied, and the thickness of the inner oxide layer of 9%Cr martensitic heat-resistant steel in a supercritical steam environment can be easily and quickly calculated by combining three factors, namely, steam temperature, steam pressure and operating time, which greatly improves the prediction accuracy and controls the error within 6%. Furthermore, the thickness of the inner oxide layer can be measured without cutting the tube during the operation of an actual power plant, which reduces costs and improves work efficiency, and is of great practical value.
[0020] 2. The present invention can calculate the thickness of the inner oxide layer of martensitic heat-resistant steel in a supercritical steam environment with high accuracy, thereby fully detecting the degree of corrosion and thinning caused by oxidation on the inner wall of martensitic heat-resistant steel pipe, evaluating the remaining service life of components, and ensuring the safe operation of units, and has important industrial application value.
[0021] 3. According to the present invention, in different temperature intervals, different weights of the influence of temperature on the thickness of the inner layer of the oxide layer are determined, which further improves the accuracy of the calculation. [Brief description of the drawings]
[0022] [Figure 1] FIG. 2 is a fitting curve diagram of the thickness YT of the inner oxide layer and Z in an embodiment of the present invention. [Diagram 2] FIG. 2 is a graph showing the relationship between the thickness Yp of the inner oxide layer and the selected pressure p and time t in an embodiment of the present invention. [Diagram 3] FIG. 1 is a graph showing the thickness Yp of the inner oxide layer in an embodiment of the present invention and a fitting verification diagram of three repeated measurements of actual data at a selected pressure p and time t. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The technical means of the present invention will be further illustrated by the following specific examples.
[0024] 1) Thickness Y of the inner oxide layer T and temperature T The effect of temperature T and time t on the oxide layer on the high-temperature heat receiving surface of a power plant boiler was investigated, and the thickness Y of the oxide layer under high-temperature operating conditions was measured. T conforms to the exponential model law of equation (1) below.
[0025]
number
[0026] In the embodiment of the present invention, a large amount of actual operation data from a power plant and laboratory simulation experimental data are collected, including data on the thickness of the inner oxide layer of 9%Cr heat-resistant steels such as T / P91 and T / P92 at temperatures of 550°C to 650°C, steam pressures of 5.0 to 25.0 MPa, and oxidation times of 1000 to 150000 h, and the parameters n, Q, and k in formula (1) are calculated using the above data. The calculation method is as follows: Steps 1 to 3.
[0027] Step 1 is to find n. Taking a particular temperature T,
[0028]
number
[0029] Regarding the first group, If T=550°C, Y T =5.3307±0.36426t 0.25745±0.00604 and If T=575°C, Y T =3.8695±0.25881t 0.32759±0.00588 and If T = 600°C, Y T =7.4295±0.57287t 0.29728±0.00675 and If T=625°C, Y T =16.0928±1.29516t 0.24991±0.0071 and If T=650°C, Y T =31.4784±1.91864t 0.21077±0.0054 and Regarding the second set, If T=550°C, Y T =5.1523±0.76277t 0.26299±0.01301 and If T=575°C, Y T=3.9382±0.52155t 0.33434±0.01156 and If T = 600°C, Y T =5.66428±0.63578t 0.33218±0.00987 and If T=625°C, Y T =5.52665±0.39467t 0.36569±0.00628 and If T=650°C, Y T =2.47527±0.14564t 0.37688±0.00511 and It can be found that the range of n value is about 0.21 to 0.35 and fluctuates around 0.25. To explain that the oxidation kinetics of 9% Cr heat-resistant steel substantially conforms to the cube law, if n is set to 0.25, formula (1) is modified to the following formula (2).
[0030]
number
[0031] In step 2, the activation energy Q is calculated. Taking the logarithm of both sides of equation (2) gives us:
[0032]
number
[0033]
number
[0034] When t=1000h, 10000h, 50000h, 100000h, 150000h, the experimental data is substituted into the fitting equation obtained in step 1 to calculate the lnY values when T=550℃, 575℃, 600℃, 625℃, 650℃ respectively, and then substituted into equation (3) to calculate the activation energy Q values at different times t, as shown in Table 1.
[0035] [Table 1]
[0036] As can be seen from Table 1, the Q value at different times is different, which explains the different activation energies of the oxidation reaction at different times. Through research, it is found that the oxidation reaction of 9%Cr heat-resistant steel is a complex, dynamically changing process, and the reaction mechanism, the composition and structure of the products and oxides change at different stages of oxidation. Therefore, in the present invention, a mathematical model is used to fit the time change of the activation energy, and the obtained activation energy Q and time t are highly consistent with the following mathematical model, which is expressed as follows: Q=106661.33557-0.36498t+3.07915×10 -6 t 2 (4)
[0037] Substituting equation (4) into equation (2) gives the corrected thickness equation, which is:
[0038]
number
[0039] In step 3, the coefficient k is calculated. By selecting a specific temperature T value and operating time t,
[0040]
number
[0041] As can be seen, with the increase in temperature, the k value becomes larger and larger. This explains that the higher the temperature, the greater the effect of temperature on the thickness of the inner oxide layer. Therefore, the final thickness Y of the inner oxide layer obtained T and the temperature T are fitted as shown in Equation (7) below.
[0042]
number
[0043] In the above formula, the unit of temperature T is K, the unit of time t is h, and the calculated inner oxide layer thickness Y T The unit is μm.
[0044] 2) Thickness Y of the inner oxide layer p and steam pressure p In order to investigate the effect of pressure p and time t on the oxide layer of the high-temperature heat-receiving surface of the power plant boiler, the experimental data of the thickness of the inner oxide layer of 9%Cr martensitic heat-resistant steel at different times t and different pressures p were selected and processed, and the results are shown in Table 2.
[0045] [Table 2]
[0046] The above data was plotted to obtain the thickness of the inner oxide layer Y shown in Figure 2. p A relationship diagram of the selected pressure p and time t is obtained.
[0047] Thickness Y p It can be found that there exists a two-dimensional quadratic relationship between pressure p and time t, and by three-dimensional nonlinear surface fitting, the following Equation (8) is obtained. Y p =a+bt+cp+dt 2 +hpt+ip 2 (8)
[0048] In step 1, the coefficients i, h, and c including the p term are found. By selecting a particular time t, the terms involving t become constants, and equation (8) can be transformed into a parabolic equation in p, and by substituting the data and fitting, the coefficients i, h, and c involving the p term can be obtained. i=0.1152±0.03315 h=1.79×10 -5 ±4.74×10 -6 c=-0.8198±1.0842
[0049] In step 2, the coefficients d and b including the t term are found. Similarly, by selecting a particular pressure p, the terms involving p become constants, and equation (8) can be transformed into a parabolic equation in t, and by substituting the data and fitting, the coefficients d and b involving the t term can be obtained. d=-7.655×10 -10 ±7.7735×10-10 b=0.0009334±0.0001543
[0050] In step 3, after determining the five coefficients, the coefficient a needs to be determined last. The coefficient obtained above is substituted into equation (8), and then all the data is substituted and three-dimensional nonlinear surface fitting is performed to obtain the coefficient a = 22.21 ± 9.65. Therefore, equation (8) is rewritten as the following equation (9). Y p =22.21+0.0009334t+(-0.8198p)+(-7.655×10 -10 t 2 ) + 1.79 × 10 -5 tp+0.1152p 2 (9)
[0051] In step 4, the fitting is repeated for FIG. 2, and the error rate of each coefficient in formula (9) is verified. A surface diagram is made for the expression of formula (9), and then all data are substituted into the diagram. It is explained that when the data points are basically on the surface, the prediction result of formula (9) basically matches the actual result. Since each coefficient value has a certain variation range, three fittings are performed to improve the accuracy and reduce the error. Finally, the three repeated fitting prediction diagram of the actual data is obtained as shown in FIG. 3. It can be found that the data points under different operating conditions are basically on the three prediction surfaces (boundaries), and the average error rate is 5%, and the thickness Y under the actual operating conditions is 1.5%. p It is explained that the relationship between and pressure p and time t basically conforms to the function change law described in equation (9), and the coefficients of each are determined as follows: a=22.21 b=0.0009334 c=-0.8198 d=-7.655×10 -10 h=1.79×10 -5 i=0.1152
[0052] The final thickness of the oxide layer is Y pand the fitting equation for the steam pressure p is given by the following equation (10). Y p =22.21+0.0009334t+(-0.8198p)+(-7.655×10 -10 t 2 ) + 1.79 × 10 -5 tp+0.1152p 2 (10)
[0053] In the above formula, the unit of time t is h, the unit of steam pressure p is MPa, and the thickness of the inner oxide layer Y p The unit is μm.
[0054] 3) The relationship between the total thickness Y of the inner oxide layer, the steam temperature T, and the steam pressure p In the process of fitting the experimental data, it is found that when the data of T and p are introduced at the same time and the fitting process is performed, the results are not consistent with the actual one, and the error rate is high. After analysis, the possible reasons are as follows: When the temperature and pressure are introduced into a system at the same time, the two physical quantities of temperature and pressure themselves also affect each other and change, so that the closed-loop repeatability error occurs in the system, and the difference between the fitting result and the actual situation becomes large. As mentioned above, the relationship between the thickness of the inner layer of the oxide layer and the steam temperature T or the steam pressure p has been obtained, and the weighting coefficient for both thicknesses is currently studied, and the calculation formula of the total thickness of the inner layer of the oxide layer including T and p is determined.
[0055] In step 1, the formula for the total thickness of the inner oxide layer is determined as the following formula (11). Y=ω×Y T +(1-ω)×Y p (11) As can be seen from the above,
[0056]
number
[0057] In step 2, after substituting the measured data of the thickness of the inner layer of the oxide layer at T = 550 ° C, 575 ° C, 600 ° C, 625 ° C, and 650 ° C and fitting, it is found that when the temperature is low (T = 550 ° C, 575 ° C), the value of ω fluctuates within the range of 0.1 to 0.2. When the temperature is low, the effect of temperature on the thickness of the inner layer of the oxide layer is smaller than the effect of pressure. Finally, when the measured data is substituted and the value of the weighting coefficient ω of temperature T obtained by fitting is 0.1682 ± 0.1136, equation (11) is changed to the following equation (12). Y = (0.1682 ± 0.1136) × Y T +(0.8318±0.1136)×Y p (12)
[0058] When the temperature is high (T = 600°C, 625°C, 650°C), the ω value varies within the range of 0.6 to 0.8. When the temperature is high, the effect of temperature on the thickness of the oxide layer exceeds the effect of pressure. Finally, when the measured data is substituted and the value of the weighting coefficient ω for temperature T obtained by fitting is 0.6891 ± 0.2269, equation (11) is changed to the following equation (13). Y = (0.6891 ± 0.2269) × Y T +(0.3109±0.2269)×Y p (13)
[0059] As can be seen from the above steps, with the increase in temperature, the weighting coefficient ω becomes larger and larger, which is related to the relationship between temperature and the thickness of the inner oxide layer Y TAs mentioned above, the calculation formula for the total thickness Y of the inner oxide layer, the temperature T and the steam pressure p are as follows: If T<600℃, Y=(0.1682±0.1136)×Y T +(0.8318±0.1136)×Y p and When T≧600℃, Y=(0.6891±0.2269)×Y T +(0.3109±0.2269)×Y p ,
[0060]
number
[0061] In the above formula, the unit of the steam temperature T is K, the unit of the steam pressure p is MPa, the unit of the time t is h, and the unit of the thickness Y of the oxide layer is μm.
[0062] Example 1 The results of the calculation method according to the present invention are compared with the oxidation experiment results of T91 steel.
[0063] Nishimura et al. oxidized T91 steel at a steam temperature of 555 to 568°C and a steam pressure of 25 MPa for approximately 1451 hours, and found that the thickness of the inner oxide layer was approximately 71 μm. The thickness of the inner oxide layer obtained by calculating the thickness by substituting the experimental conditions into the formula (12) according to the embodiment of the present invention was approximately 70.8602 μm, with an error percentage of 0.19%.
[0064] Example 2 The results of the calculation method according to the present invention are compared with the oxidation experiment results of T92 steel.
[0065] Muraki et al. oxidized T92 steel at a steam temperature of 555 to 568°C and a steam pressure of 25 MPa for approximately 29,920 hours, and found that the thickness of the inner oxide layer was approximately 149 μm. By substituting the experimental conditions into the formula (12) according to the embodiment of the present invention, the thickness of the inner oxide layer was calculated to be approximately 140.2092 μm, with an error of 5.9%.
[0066] Example 3 1 is an application of the computational method according to the present invention in a real power plant environment.
[0067] The connecting tube material of the high-temperature reheater header of a power plant #6 unit was T92 steel, and after operating for 15,479 h and 19,037 h at a steam temperature of 615°C and a steam pressure of 5 MPa, the thickness of the inner oxide layer measured was 98 μm and 112 μm, respectively.
[0068] The steam temperature under the above operating parameters is Y T The thickness of the inner layer of the oxide layer obtained by substituting into (Equation 7) for 15479 hours was 105.8385 μm, and the error percentage was 7.9%. p The thickness of the inner layer of the oxide layer after 15479 hours was calculated by substituting the above two operating parameters into equation (13) proposed in the embodiment of the present invention, and the thickness of the inner layer of the oxide layer after 15479 hours was calculated to be 90.6411 μm, with an error percentage of 7.5%. The thickness of the inner layer of the oxide layer after 15479 hours was calculated to be 100.9753 μm, with an error percentage of 3.0%.
[0069] The steam temperature under the above operating parameters is Y T The thickness of the inner layer of the oxide layer obtained by substituting into (Equation 7) for 19037 h was 120.1865 μm, and the error percentage was 7.3%. pThe thickness of the inner layer of the oxide layer in the case of 19037 h obtained by substituting into (Equation 10) was 103.4091 μm, with an error percentage of 7.7%. The thickness of the inner layer of the oxide layer in the case of 19037 h obtained by substituting the above two operating parameters into Equation (13) proposed in the embodiment of the present invention was 114.8177 μm, with an error percentage of 2.5%.
[0070] From the above, the error after comprehensively considering the temperature and pressure is smaller, and the prediction results are more accurate.
[0071] Example 4 1 is an application of the computational method according to the present invention in a real power plant environment.
[0072] A supercritical power boiler at a certain power plant had a steam temperature of approximately 571°C, a steam pressure of approximately 25.4 MPa, and T91 steel was used as the tube material. After operating for approximately 12,956 hours, the thickness of the inner oxide layer inside the tube was measured to be approximately 101 μm.
[0073] The steam temperature under the above operating parameters is Y T The thickness of the inner layer of the oxide layer obtained by substituting into (Equation 7) for 12956 h was 108.4956 μm, and the error percentage was 7.4%. p The thickness of the inner layer of the oxide layer after 12956 hours, calculated by substituting into (Equation 9), was 91.4774 μm, with an error percentage of 9.4%. The thickness of the inner layer of the oxide layer after 12956 hours, calculated by substituting the above two operating parameters into Equation (12) proposed in the embodiment of the present invention, was 102.8971 μm, with an error percentage of 1.8%.
[0074] From the above, the error after comprehensively considering the temperature and pressure is smaller, and the prediction results are more accurate.
[0075] In all of the above examples, it is explained that the thickness of the inner oxide layer of 9%Cr martensitic steel calculated by the method matches well with the actual measurement results, and the error is within 6%.
[0076] The technical means of the present invention are not limited to the above embodiments, and any technical means obtained by equivalent substitution is within the scope of the protection of the present invention.
Claims
1. A method for calculating the thickness of an inner oxide layer of a martensitic heat-resistant steel in a steam environment, the martensitic heat-resistant steel being a 9% Cr heat-resistant steel, and the calculation formula for the thickness of the inner oxide layer in the steam environment is Y=ω×Y T +(1-ω)×Y p where: [0010] Y p =a+bt+cp+dt 2 +hpt+ip 2 where Y is the thickness of the inner layer of the oxide layer in the steam environment, and Y T is a relationship between the temperature in the steam environment and the thickness of the inner layer of the oxide layer, and Y p is a relational expression between the pressure in the steam environment and the thickness of the inner layer of the oxide layer, all in units of μm, ω is a weighting coefficient, k, a, b, c, d, h, and i are fitting coefficients, and Q is an activation energy in units of J mol -1 where R is the gas constant, T is the vapor temperature in K, p is the vapor pressure in MPa, and t is time in h. A calculation method characterized by:
2. The steam temperature range is 550 to 650 ° C., and the steam pressure range is 5.0 to 25.0 MPa.
2. The method of claim 1 .
3. The operating time t of the martensitic heat-resistant steel in a steam environment is in the range of 1000 to 150000 h.
2. The method of claim 1 .
4. In the calculation formula of Y, When the steam temperature T<600° C., the value of ω is 0.1682±0.1136; When the steam temperature T≧600° C., the value of ω is 0.6891±0.2269; 2. The method of claim 1 .
5. The Y T In the calculation formula of the thickness of the inner layer of the steam oxidation layer of the martensitic heat resistant steel, n = 0.
25.
2. The method of claim 1 .
6. The Y T In the calculation formula, the mathematical relationship between the k and the steam temperature T is k = 1.01 x 10 -42 T 14.68 That is, 2. The method of claim 1 .
7. The Y T In the above formula, the mathematical relationship between the activation energy Q and the time t is Q = 106661.33557 - 0.36498t + 3.07915 x 10 -6 t 2 That is, 2. The method of claim 1 .
8. The Y p In the above formula, the value of the fitting coefficient a is 22.21, the value of the fitting coefficient b is 0.0009334, the value of the fitting coefficient c is −0.8198, and the value of the fitting coefficient d is −7.655×10 -10 and the value of the fitting coefficient h is 1.79×10 -5 2. The method of claim 1, wherein the value of the fitting coefficient i is 0.1152.
9. The application of the calculation method according to claim 1 in evaluating the service life of martensitic heat-resistant steel components operated by steam in a power plant.
Citation Information
Patent Citations
Continuous damage prediction method and system for high-temperature oxidation corrosion of high-chromium steel component
CN111581861A
Calculation method for predicting spring steel heating process oxide layer thickness
CN112597627A
Method for predicting service life of stainless steel oil well tubing
JP1997318586A
Overheat damage diagnosing method for boiler water- wall tube
JP2001082702A
Method and device to diagnose damage of boiler heat transfer pipe different material joint welding part