Electrolyte and lithium ion battery

The electrolyte solution with cyclic carbonate and lithium Bis(fluorosulfonyl)imide addresses the low temperature performance issues of lithium-ion batteries by maintaining low melting points and high ionic conductivity, thereby improving energy density and power density.

JP2024155701AInactive Publication Date: 2024-10-31ENVISION DYNAMICS TECH (JIANGSU) CO LTD +3
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023208469
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2023-12-11
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium-ion batteries experience significant decreases in energy density and power density under low temperature conditions due to the high melting point and high viscosity of commonly used solvents, leading to precipitation and increased impedance, which affects ionic conductivity and overall performance.

Method used

An electrolyte solution comprising a solvent mixture of cyclic carbonate, ethyl acetate, and lithium Bis(fluorosulfonyl)imide, with specific mass percentages, is used to maintain low melting points and high ionic conductivity, improving battery performance at low temperatures.

Benefits of technology

The electrolyte solution achieves low melting points, high ionic conductivity, and reduced battery DC resistance, enhancing energy density and power density even at -20°C, with improved lithium salt solubility and discharge rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155701000001
    Figure 2024155701000001
  • Figure 2024155701000002
    Figure 2024155701000002
Patent Text Reader

Abstract

PURPOSE: To provide an electrolyte and a lithium ion battery which resolve the issues of high electrolyte melting point, low ionic conductivity, and poor performance under low temperatures.SOLUTION: An electrolyte contains: a solvent; a lithium salt; and an additive agent. The solvent contains cyclic carbonate; and an ethyl acetate. The cyclic carbonate contains ethylene carbonate. The lithium salt contains a lithium bis (fluorosulfonyl) imide. The mass percentage of the cyclic carbonate occupies 5% to 20% of the total amount of the solvent, the mass percentage of the ethyl acetate occupies 20% to 95% of the total amount of the solvent, and the mass percentage of the lithium bis (fluorosulfonyl) imide occupies 8% to 20% of the total amount of the electrolyte. The electrolyte provided by the present invention has a low fusion point, a high ionic conductivity, and a low battery DCR when it is used for the lithium ion battery, and can improve performance at a low temperature.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolyte and a lithium-ion battery. [Background technology]

[0002] Currently, a common problem with lithium-ion batteries is the significant decrease in energy density and power density under low temperature conditions. Common lithium-ion batteries employ cyclic carbonates (e.g., ethylene carbonate (EC) and propylene carbonate (PC)) and linear carbonates (e.g., dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC)) as solvents, and generally employ lithium hexafluorophosphate as the lithium salt. Because the solvents have high melting points and high viscosities, electrolytes with such combinations usually perform poorly at low temperatures.

[0003] Ethylene carbonate (EC) is a cyclic carbonate solvent commonly employed in the electrolyte of lithium-ion batteries. The dielectric constant of ethylene carbonate is 89, which is greater than that of propylene carbonate (65). The addition of ethylene carbonate promotes the dissociation of lithium hexafluorophosphate and improves the ionic conductivity of the electrolyte. In addition, ethylene carbonate has a higher decomposition potential on the negative electrode side than propylene carbonate and can preferentially participate in the formation of the solid electrolyte membrane SEI, thereby significantly improving the cycle performance of lithium-ion batteries. Therefore, ethylene carbonate has become an essential solvent component of conventional commercial electrolytes.

[0004] However, ethylene carbonate has a high freezing point (its melting point is 35°C to 38°C). Under low temperature conditions such as minus 40°C, it is very likely that ethylene carbonate will precipitate, blocking the pores of the separator film or electrode sheet, thereby increasing the impedance and affecting the performance of the battery. In addition, the precipitation of ethylene carbonate also reduces the relative dielectric constant of the mixed solvent, reducing the dissociation of lithium hexafluorophosphate. To solve this problem, some linear carbonates with low melting points are commonly adopted, such as dimethyl carbonate (its melting point is 4.6°C), ethyl methyl carbonate EMC (its melting point is -53°C), or diethyl carbonate (its melting point is -74.3°C) to partially replace EC, thereby lowering the melting point of the mixed solvent. However, the dielectric constants of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate are only 3.12, 2.96, and 2.82, respectively. The introduction of a large amount of low dielectric constant solvent is obviously not conducive to the dissociation of lithium hexafluorophosphate, and therefore reduces the ionic conductivity of the electrolyte, affecting the performance of the battery at low temperatures.

[0005] Therefore, how to ensure that the melting point of the electrolyte meets the requirements for practical application, while at the same time improving the ionic conductivity of the electrolyte and the performance of the battery at low temperatures, has become an urgent problem to be solved. Summary of the Invention [Problem to be solved by the invention]

[0006] Provided is an electrolyte and a lithium ion battery capable of overcoming the problems of electrolytes having a high melting point, low ionic conductivity, and poor performance at low temperatures. [Means for solving the problem]

[0007] The technical problem that the present invention aims to solve is to overcome the problems of high melting point, low ionic conductivity, and poor performance at low temperature of the electrolyte in the prior art. The present invention provides an electrolyte and a lithium ion battery. The electrolyte provided by the present invention has a low melting point, high ionic conductivity, low battery DCR, and can improve the performance at low temperature when used in a lithium ion battery.

[0008] The present invention solves the above technical problems through the following technical solutions.

[0009] The present invention provides an electrolyte solution including a solvent, a lithium salt, and an additive, wherein the solvent includes a cyclic carbonate and ethyl acetate, the cyclic carbonate includes ethylene carbonate, and the lithium salt includes lithium bis(fluorosulfonyl)imide.

[0010] The mass percentage of the cyclic carbonate is 5% to 20% of the total amount of the solvent, and the mass percentage of the ethyl acetate is 20% to 95% of the total amount of the solvent.

[0011] The mass percentage of lithium bis(fluorosulfonyl)imide is 8% to 20% of the total amount of the electrolyte.

[0012] The present invention further provides a negative electrode, a positive electrode, a separator, and a lithium ion battery each containing the above-mentioned electrolyte solution. Effect of the Invention

[0013] The advantageous effects of the present invention are as follows:

[0014] The electrolyte provided by the present invention, when employed in lithium ion batteries, has a low melting point, high ionic conductivity, low battery DCR, improves performance at low temperatures, and has high energy and power densities even at temperatures down to -20°C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In the present invention, the mass percentage of ethyl acetate may be 20%, 40%, 60%, 75%, 80%, 90%, or 95% of the total amount of the solvent, and preferably 50% to 95%.

[0016] In the present invention, under the condition that the mass percentage of ethyl acetate is 20%-95% of the total amount of the solvent, the electrolyte not only has excellent lithium salt solubility when used in a lithium ion battery, but also has excellent DCR at 25° C., DCR at −20° C., and discharge rate at −20° C. Under the condition that the mass percentage of ethyl acetate is 50%-95% of the total amount of the solvent, the DCR at −20° C. and the discharge rate at −20° C. are even better.

[0017] In the present invention, the mass percentage of the cyclic carbonate may be 5%, 10%, 15%, or 20% of the total amount of the solvent, and preferably 5% to 10%.

[0018] In the present invention, under the condition that the mass percentage of the cyclic carbonate is 5% to 20% of the total amount of the solvent, the electrolyte not only has excellent lithium salt solubility when used in a lithium ion battery, but also has excellent DCR at 25° C., DCR at −20° C., and discharge rate at −20° C. Under the condition that the mass percentage of the cyclic carbonate is 5% to 10% of the total amount of the solvent, the DCR at −20° C. and the discharge rate at −20° C. are further improved.

[0019] In the present invention, the mass percentage of ethylene carbonate preferably accounts for 5% to 20%, for example, 5%, 10%, 15%, or 20%, of the total amount of the solvent.

[0020] In the present invention, the cyclic carbonate further includes propylene carbonate. The mass percentage of propylene carbonate is preferably 0% to 10%, for example 10%, of the total amount of the solvent.

[0021] In the present invention, the mass percentage of lithium fluorosulfonylimide may be 8%, 10%, 14%, 16%, 18%, or 20% of the total amount of the electrolyte, and preferably 12% to 20%.

[0022] In the present invention, under the condition that the mass percentage of lithium fluorosulfonylimide is 8% to 20% of the total amount of the electrolyte, the electrolyte not only has excellent lithium salt solubility when used in a lithium ion battery, but also has excellent DCR at 25° C., DCR at −20° C., and discharge rate at −20° C. Under the condition that the mass percentage of lithium fluorosulfonylimide is 12% to 20% of the total amount of the electrolyte, the DCR at 25° C., DCR at −20° C., and discharge rate at −20° C. are further improved.

[0023] In the present invention, the mass percentage of the lithium salt preferably accounts for 12% to 20%, for example, 12%, 18%, or 20%, of the total amount of the electrolyte.

[0024] In the present invention, the lithium salt further includes lithium hexafluorophosphate.

[0025] The mass percentage of lithium hexafluorophosphate preferably accounts for 2% to 10%, for example 2%, 4%, 8%, or 10%, of the total amount of the electrolyte.

[0026] In the present invention, the solvent further comprises a linear carbonate.

[0027] The linear carbonate is preferably one or more of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.

[0028] When the linear carbonate includes dimethyl carbonate, the mass percentage of dimethyl carbonate can account for 20% to 30% of the total amount of the solvent.

[0029] When the linear carbonate includes ethyl methyl carbonate, the mass percentage of ethyl methyl carbonate can account for 15% to 30% of the total amount of the solvent.

[0030] The mass percentage of the linear carbonate preferably accounts for 20% to 60% of the total amount of the solvent, for example, 20%, 30%, 45%, or 60%.

[0031] In the present invention, the additive is preferably one or more of vinylene carbonate, fluoroethylene carbonate, ethylene sulfate, and 1,3-propane sultone.

[0032] When the additive includes vinylene carbonate, the mass percentage of the vinylene carbonate accounts for 0.5% to 3% of the total amount of the electrolyte.

[0033] When the additive contains fluoroethylene carbonate, the mass percentage of the fluoroethylene carbonate accounts for 1% to 5% of the total amount of the electrolyte.

[0034] In the present invention, the mass percentage of the additive preferably accounts for 2% to 5%, for example 3%, of the total amount of the electrolyte.

[0035] In a preferred embodiment, the additive is 1% vinylene carbonate and 2% fluoroethylene carbonate.

[0036] In the present invention, the negative electrode preferably comprises a negative electrode current collector and a negative electrode active material applied to the negative electrode current collector.

[0037] The negative electrode active material preferably comprises a graphite material or a graphite material-silicon material composite.

[0038] The negative electrode current collector can be made of conductive materials that do not cause chemical changes, such as copper, stainless steel, aluminum, nickel, titanium, sintered carbon, aluminum-cadmium alloy, or "copper, stainless steel material, or aluminum-cadmium alloy surface-treated with carbon, nickel, titanium, or silver." In addition, micro-embossing may be formed on the surface of the negative electrode current collector to enhance the adhesion of the negative electrode active material. The negative electrode current collector can have various shapes, such as a film, sheet, foil, mesh, porous body, foam body, nonwoven fabric body, etc.

[0039] In the present invention, the thickness of the negative electrode current collector may be 4.5 μm to 10 μm, for example, 6 μm or 8 μm.

[0040] In the present invention, the negative electrode further comprises a conductive agent, a binder, and a thickener.

[0041] The binder is a component provided to bind the active material to the conductive agent. For example, one or more of SBR, PAA, CMC, and PVDF can be used as the binder.

[0042] The conductive agent is not particularly limited as long as the conductive agent exhibits high conductivity without causing a chemical change in the battery to which the conductive agent is applied. For example, carbon nanotubes, carbon black, or graphene can be used as the conductive material.

[0043] The thickener is not particularly limited. The addition of the thickener can increase the system viscosity of each component of the negative electrode active material layer. In general, the thickener can be selected as a sodium carboxymethyl cellulose solution.

[0044] In a preferred embodiment, the negative electrode satisfies the following conditions: the negative electrode active material is artificial graphite, the conductive agent is Super P, the thickener is sodium carboxymethyl cellulose, and the binder is styrene-butadiene rubber. The mass ratio of the negative electrode active material, the conductive agent, the thickener, and the binder is 96:1:1:2.

[0045] In the present invention, the positive electrode preferably comprises a positive electrode current collector and a positive electrode active material applied to the positive electrode current collector.

[0046] The positive electrode active material preferably includes one or more of lithium iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.

[0047] The positive electrode current collector may be made of any material having high electrical conductivity without chemical change, such as stainless steel, aluminum, nickel, titanium, calcined carbon, aluminum or stainless steel material generally surface-treated with carbon, nickel, titanium, silver, etc., without limitation. In order to enhance the adhesion of the positive electrode active material, a micro-embossment may be formed on the surface of the positive electrode current collector. The positive electrode current collector may have various shapes, such as a film, sheet, foil, mesh, porous body, foam body, nonwoven fabric body, etc.

[0048] In the present invention, the thickness of the positive electrode current collector may be a common thickness in this technical field, such as 16 μm or 13 μm.

[0049] In the present invention, the positive electrode further contains a binder and a conductive agent.

[0050] In a preferred embodiment, the positive electrode satisfies the following conditions: the positive electrode active material is lithium iron phosphate, the binder is polyvinylidene fluoride, and the conductive agent is Super P. The mass ratio of the positive electrode active material, the binder, and the conductive agent is 98:1:1.

[0051] In the present invention, a separator film is used, which is an insulating film having high ion permeability and mechanical strength. The pore size of the separator film is generally 0.01 μm to 10 μm, and the thickness is generally 5 μm to 300 μm. Examples of the separator film include a sheet or nonwoven fabric made of an olefin polymer such as polypropylene, which is chemically resistant and water repellent, glass fiber, polyethylene, etc. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte may be used as the separator.

[0052] In a preferred embodiment, the separator film is a polypropylene separator film having a thickness of 12 μm.

[0053] On the one hand, in the present invention, by using a large amount of linear carbonate and carboxylic acid ester, the amount of cyclic carbonate with high melting point and high viscosity in the electrolyte solvent can be reduced, thereby effectively solving the problem of solidification at low temperature and large increase in viscosity of the electrolyte. In addition, by combining a large amount of lithium bis(fluorosulfonyl)imide (LiFSI) as the main lithium salt, LiFSI can be completely dissolved and dissociated in linear carbonate and carboxylic acid ester with low dielectric constant due to the high dissociation ability of LiFSI, thereby providing high ionic conductivity. On the other hand, the electrolyte using LiFSI as the lithium salt has a wide liquid phase range and can avoid solidification of the electrolyte at low temperature. The combination of a large amount of linear carbonate, carboxylic acid ester, and a large amount of LiFSI ensures that the battery has low impedance and high capacity retention even at low temperature. Compared with the conventional combination of a small amount of linear carbonate and lithium hexafluorophosphate, the present invention uses a specific combination of a large amount of linear carbonate, ethyl acetate, and lithium bis(fluorosulfonyl)imide to effectively reduce the freezing point and viscosity of the electrolyte, and improve the ionic conductivity and lithium ion mobility of the electrolyte, thereby helping to form a low impedance SEI, and greatly improving the rate performance of the battery at low temperature.

[0054] All the reagents and raw materials employed in the present invention are commercially available products.

[0055] Based on general knowledge in the art, the above preferred conditions can be freely combined to obtain preferred embodiments of the present invention.

[0056] The present invention will be further described below with reference to examples, but the present invention is not limited to the scope of the described examples. In the following examples, the experimental methods without specific conditions should be selected based on conventional methods and conditions or based on the product specifications.

[0057] Example 1

[0058] Preparation of electrodes:

[0059] In a glove box with an argon atmosphere and a water content of 10 ppm, battery grade ethylene carbonate (EC) and ethyl acetate (EA) were mixed in a mass ratio of 2:8 to form an organic solvent. Lithium salt and anode additive were added quantitatively according to the electrolyte composition listed in Table 1, and mixed uniformly to obtain an electrolyte. The lithium salts were LiPF6 and LiFSI, the mass fraction of LiPF6 was 10%, and the mass fraction of LiFSI was 8%. The anode additives were vinylene carbonate (VC) and fluoroethylene carbonate (FEC), the mass fraction of VC was 1%, and the mass fraction of FEC was 2%. In Table 1, the content of each component other than the solvent is a mass percentage calculated based on the total mass of the electrolyte, and the mass content of each component in the solvent is the amount present in a total amount of 10 parts of the solvent.

[0060] Examples 2 to 13 and Comparative Examples 1 to 6

[0061] Electrolyte solutions were prepared according to the experimental parameters in Table 1. The electrolyte compositions of Examples 2-13 and Comparative Examples 1-6 were the same as Example 1, except that the ingredients were added according to the ratios in Table 1.

[0062] Example of effect

[0063] 1. The method for producing a secondary lithium battery is as follows:

[0064] (1) Preparation of lithium iron phosphate positive electrode:

[0065] The positive electrode active material (lithium iron phosphate), polyvinylidene fluoride used as a binder, and Super P used as a conductive agent were mixed in a weight ratio of 98:1:1, and an appropriate amount of N-methylpyrrolidone (NMP) was added, and the above mixture was stirred under the action of a vacuum mixer until the system became uniform and transparent to obtain a positive electrode slurry. The positive electrode slurry was uniformly applied to an aluminum foil with a thickness of 13 μm, and the aluminum foil was dried at room temperature, transferred to an oven for drying, and then cold-rolled and cut to obtain a positive electrode (electrode sheet).

[0066] (2) Preparation of graphite anode:

[0067] Artificial graphite was used as the negative electrode active material, Super P was used as the conductive agent, sodium carboxymethyl cellulose (CMC-Na) was used as the thickener, and styrene-butadiene rubber (SBR) was used as the binder. All of the above were mixed in a mass ratio of 96:1:1:2, and then deionized water was added and stirred under the action of a vacuum mixer to obtain a negative electrode slurry. The negative electrode slurry was uniformly applied to a negative electrode current collector copper foil with a thickness of 8 μm, and the copper foil was dried at room temperature, transferred to an oven for drying, and then cold-rolled and cut to obtain a negative electrode (electrode sheet).

[0068] (3) Preparation of electrolyte:

[0069] For preparation of the electrolyte, see Example 1.

[0070] (4) Preparation of separator film:

[0071] A polypropylene film was used as the separator film.

[0072] (5) Preparation of lithium-ion secondary battery:

[0073] A 12 μm thick polypropylene film (PP) was used as a separator film, and the positive electrode, separator film, and negative electrode prepared above were laminated in order so that the separator film was between the positive electrode and the negative electrode, separating the positive electrode and the negative electrode. Next, all of the above was wrapped in an aluminum plastic film, transferred to a vacuum oven and dried at 120 ° C., and 3.0 g / Ah of the electrolyte prepared above was injected, and the electrolyte was chemically converted and then sealed. Finally, a soft pack battery (lithium ion battery) with a capacity of 1 Ah was obtained.

[0074] 2.Performance test method:

[0075] (1) Testing the DC resistance (DCR) of lithium-ion secondary batteries

[0076] At the specified temperature, the battery was discharged to 50% SOC (state of charge reflecting the remaining capacity of the battery) at a current of 1C, the current was increased to 4C and maintained for 30 seconds, the difference between the updated stable voltage and the original platform voltage was detected, and the ratio of the difference value to the current value of 4C was the DC resistance of the battery. The DCR test result performed after the battery was first fully charged was the initial DCR of the battery.

[0077] (2) Discharge capacity retention test for lithium-ion secondary batteries at low temperatures

[0078] After the lithium-ion secondary battery was fully charged, the battery was placed in a thermostatic box at -20° C. After being sufficiently cooled, the battery was discharged at a rate of 1 C to the cut-off voltage, and the percentage of the battery capacity relative to the initial discharge capacity was compared.

[0079] For the lithium iron phosphate / graphite battery, the charge and discharge cut-off voltages were between 2.5V and 3.65V.

[0080] Electrolyte composition of Examples 1 to 13 and Comparative Examples 1 to 6 [Table 1]

[0081] Performance test results of Examples 1 to 13 and Comparative Examples 1 to 6 [Table 2]

[0082] Table 2 shows the performance test results of Examples 1-13 and Comparative Examples 1-6. As can be seen from Examples 1 and 2 and Comparative Examples 1 and 2, when the amount of EC is within the range of 0.5 / 10-2 / 10 (i.e., when the mass percentage of the cyclic carbonate accounts for 5%-20% of the total amount of the solvent), the performance of the battery is optimal at low temperature. When the amount of EC is higher than 2 / 10 (see Comparative Example 1), its DCR is much higher than that of Example 1, and the low-temperature discharge rate is significantly reduced, which indicates that too much cyclic carbonate increases the melting point of the electrolyte, increases the viscosity of the electrolyte at low temperature, and reduces the conductivity of the electrolyte, resulting in deterioration of the battery performance at low temperature. When the amount of EC is less than 0.5 / 10 (see Comparative Example 2, that is, when the mass percentage of the cyclic carbonate in the total amount of the solvent is less than 5%), the electrolyte does not have a solvent with a sufficiently high dielectric constant, so that the lithium salt does not dissolve completely, resulting in an extremely high DCR at room temperature and an extremely poor performance at low temperature. In the present invention, EC may be replaced with an appropriate amount of other cyclic carbonates (e.g., PC), and EA may be replaced with an appropriate amount of other linear carbonates (e.g., EMC, DMC). As can be seen from Examples 6 to 9, when the amount of cyclic carbonate is 0.5 / 10 to 2 / 10 (i.e., when the mass percentage of cyclic carbonate is 5% to 20% of the total amount of the solvent), as the amount of cyclic carbonate decreases and the amount of EA increases, the DCR of the battery at normal temperature decreases slightly, the DCR at low temperature decreases significantly, and the low temperature discharge rate increases, which indicates that the viscosity of the electrolyte decreases and the conductivity of the electrolyte increases due to the decrease in the amount of cyclic carbonate and the increase in the amount of EA, thereby improving the performance of the battery at low temperature. When the amount of EA is 0 (see Comparative Example 3), the viscosity of the electrolyte is high, so the performance of Comparative Example 3 at low temperature is worse than that of the electrolyte containing EA. As can be seen from Examples 3, 4, 5 and Comparative Examples 4 and 5, when the amount of LiFSI is 8% to 20%, the battery has optimal performance at low temperature.When the amount of LiFSI is lower than 8% (see Comparative Example 4), the DCR and low temperature performance of the battery are significantly deteriorated, and when the amount of LiFSI is higher than 20% (see Comparative Example 5), the concentration of lithium salt is too high, so the viscosity of the electrolyte increases and the dissociation degree of the lithium salt decreases, thereby deteriorating the performance of the battery at low temperature.

[0083] According to Example 3 and Examples 10-13, when the solvent system remains unchanged and the concentration of lithium salt is within the range of 12%-20%, by increasing the amount of LiFSI in the lithium salt, the DCR of the corresponding battery at normal temperature and low temperature is greatly reduced, and the low temperature discharge rate continues to increase. The reason is that LiFSI dissociates more easily than LiPF6, has higher solubility in the solvent, and has higher conductivity. Therefore, the more LiFSI is adopted, the better the performance of the battery at low temperature.

[0084] As can be seen from Comparative Example 6, when the amount of cyclic carbonate is 3 / 10 (i.e., when the mass percentage of cyclic carbonate accounts for 30% of the total amount of solvent), even if the amount of LiFSI is increased to 18%, the DCR and low temperature performance of the corresponding battery are much worse than those of the embodiment with a lower amount of cyclic carbonate, indicating that in order for the electrolyte to have good conductivity and low temperature performance, the amount of cyclic carbonate needs to be reduced to 2 / 10 or less (i.e., the mass percentage of cyclic carbonate in the total amount of solvent is 20% or less). [Industrial Applicability]

[0085] The electrolyte provided by the present invention, when employed in lithium ion batteries, can have a low melting point, high ionic conductivity, low battery DCR, and improve performance at low temperatures.

Claims

1. An electrolyte solution comprising a solvent, a lithium salt, and an additive, wherein the solvent comprises a cyclic carbonate and ethyl acetate, the cyclic carbonate comprises ethylene carbonate, and the lithium salt comprises lithium bis(fluorosulfonyl)imide; the weight percentage of the cyclic carbonate is 5% to 20% of the total amount of the solvent, and the weight percentage of the ethyl acetate is 20% to 95% of the total amount of the solvent; The mass percentage of the lithium bis(fluorosulfonyl)imide is 8% to 20% of the total amount of the electrolyte.

2. 2. The electrolyte of claim 1, wherein the weight percentage of ethyl acetate comprises 50% to 95% of the total amount of the solvent.

3. the lithium salt further comprises lithium hexafluorophosphate; The electrolyte according to claim 1 , wherein the solvent further comprises a linear carbonate.

4. 2. The electrolyte solution according to claim 1, wherein the cyclic carbonate further comprises propylene carbonate, and the mass percentage of the propylene carbonate is 0% to 10% of the total amount of the solvent.

5. 4. The electrolyte of claim 3, wherein the weight percentage of the lithium hexafluorophosphate comprises 2% to 10% of the total weight of the electrolyte.

6. 4. The electrolyte solution of claim 3, wherein the weight percentage of the linear carbonate is from 20% to 60% of the total amount of the solvent.

7. 2. The electrolyte of claim 1, wherein the weight percentage of the additive comprises 2% to 5% of the total weight of the electrolyte.

8. 2. The electrolyte of claim 1, wherein the additive is one or more of vinylene carbonate, fluoroethylene carbonate, ethylene sulfate, and 1,3-propane sultone.

9. 4. The electrolyte of claim 3, wherein the linear carbonate is one or more of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.

10. A lithium ion battery comprising a negative electrode, a positive electrode, a separator film, and the electrolyte of claim 1.

Citation Information

Patent Citations

  • Lithium ion secondary battery

    JP2015109224A