Flame retardant composition

A flame retardant composition with a dispersion medium, silica particles, and silicone surfactant addresses the aggregation issue of powdered flame retardants, ensuring stable mixing and improved resin foam production.

JP2024155941AInactive Publication Date: 2024-10-31INOAC TECHN CENT
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024134639
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The aggregation of powdered flame retardants, such as red phosphorus, in flame retardant compositions over time causes issues during use, affecting the performance and stability of resin foams.

Method used

A flame retardant composition comprising a dispersion medium, silica particles, and a silicone surfactant, with a specific weight ratio, is used to prevent aggregation of powder flame retardants, including red phosphorus, phosphates, phosphinates, cellulose, and expanded graphite, while maintaining thixotropy and viscosity properties.

Benefits of technology

The composition effectively prevents powder flame retardant aggregation, ensuring stable mixing and handling properties, and enhances the production of resin foams with improved flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155941000001
    Figure 2024155941000001
  • Figure 2024155941000002
    Figure 2024155941000002
  • Figure 2024155941000003
    Figure 2024155941000003
Patent Text Reader

Abstract

To provide a flame retardant composition in which the powder in the composition does not easily settle.SOLUTION: A flame retardant composition comprises a dispersion medium, a powder flame retardant, a silica-based particle, and a silicone-based surfactant, and is characterized in that it is used for producing a resin foam.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flame retardant composition. [Background technology]

[0002] 2. Description of the Related Art Resin foams such as polyurethane foams are used as construction materials, heat retaining materials and insulating materials for ships for transporting oil and gas, and for electrical appliances such as refrigerators.

[0003] Here, polyurethane foam alone has low flame retardancy, and therefore, studies have been made to improve the flame retardancy of polyurethane foam.

[0004] Prior Art Document 1 discloses a technology that uses multiple flame retardants including red phosphorus to improve the flame retardancy of polyurethane foam and suppress shrinkage, expansion, and deformation during combustion. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6329235 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0006] However, in the conventional technology, when a large amount of a powder flame retardant such as red phosphorus is used, aggregation of the powder flame retardant occurs over time in the flame retardant composition, which causes problems during use.

[0007] Therefore, an object of the present invention is to provide a flame retardant composition in which the powder flame retardant is less likely to aggregate. [Means for solving the problem]

[0008] The present inventors have conducted extensive research and found that the above problems can be solved by a specific flame retardant composition, and have completed the present invention.

[0009] The present invention is a flame retardant composition for producing a resin foam, the flame retardant composition comprising a dispersion medium, a powder flame retardant, silica-based particles, and a silicone-based surfactant. The weight ratio of the silicone-based surfactant to the silica-based particles (the silicone-based surfactant:the silica-based particles) may be 1:1 to 1:150. The dispersion medium may contain a polyol compound and / or a phosphoric acid ester. The silica-based particles may include fumed silica. The silicone surfactant may have an HLB value of 3 to 19, and may have a molecular structure in which a polyalkylsilyl ether and a polyoxyalkylene ether are graft-copolymerized or a molecular structure in which a linear block copolymerization is performed. The powder flame retardant may include one or more selected from red phosphorus, phosphates, phosphinates, cellulose, and expandable graphite. The flame retardant composition may have a thixotropy index value at 25° C. of 2.0 or more and 5.0 or less.

[0010] The present invention may also be a method for producing a resin foam, comprising a step of foaming a raw material composition containing the flame retardant composition. Effect of the Invention

[0011] According to the present invention, it is possible to provide a flame retardant composition in which the powder flame retardant is less likely to aggregate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The composition, physical properties / characteristics, production method, applications, etc. of the flame retardant composition will be described below, but the present invention is not limited to the following in any way.

[0013] When an upper limit and a lower limit are separately described for a certain element, the upper limit and the lower limit can be freely combined as appropriate to form a new numerical range. In addition, "greater than" and "less than" can be freely interpreted.

[0014] When isomers exist in the described compounds, all possible isomers can be used unless otherwise specified.

[0015] In the following, the term "particle" refers to any particle that can be generally determined to be a "particle" and may be, for example, spherical, ellipsoidal, plate-like, scaly, needle-like, hollow, etc., in shape (e.g., aspect ratio).

[0016] Unless otherwise specified, the average particle size (average particle size) is the D50 value of the particle size distribution measured by laser diffraction method.

[0017] <<<<<Flame retardant composition>>>> <<<Ingredients>>> The flame retardant composition contains a dispersion medium, a powder flame retardant, silica-based particles, and a silicone-based surfactant. The flame retardant composition may also contain other components.

[0018] <<Dispersion medium>> The dispersion medium is not particularly limited as long as it is a liquid medium capable of dispersing each component, and preferably contains a polyol compound and / or a phosphoric acid ester.

[0019] Examples of the polyol compound include those usable as polyurethane foaming raw materials, such as polyester polyol, polycarbonate polyol, polyether polyol, and polyester ether polyol.

[0020] As the phosphoric acid ester, for example, a phosphoric acid ester-based flame retardant that is liquid at normal temperature and normal pressure can be used, and examples thereof include aliphatic phosphoric acid esters such as trimethyl phosphate and triethyl phosphate, aromatic phosphoric acid esters such as tricresyl phosphate and cresyl diphenyl phosphate, aromatic condensed phosphoric acid esters such as resorcinol polyphosphate, halogenated phosphoric acid esters such as tris(chloropropyl)phosphate, etc. In addition, since the phosphoric acid ester may be any that is liquid at normal temperature and normal pressure, in addition to the above phosphates, phosphonates such as diethyl-N,N-bis(2-hydroxyethyl)aminomethylphosphonate, phosphinates, phosphites, etc. can also be used.

[0021] Other dispersion media include halogenated paraffins such as chlorinated paraffins, brominated carboxylate compounds such as brominated dialkyl phthalates, halogenated poly(oxyalkylene) compounds such as halogenated polyether polyols, petroleum-based lubricating oils such as paraffinic oils and naphthenic oils, natural lubricating oils such as castor oil and rapeseed oil, hindered amines, poly(oxyethylene)-poly(oxypropylene) copolymers derived from low molecular weight active hydrogen compounds (monoalcohols, glycols, phenolic compounds, amine compounds), and poly(oxyethylene)-poly(oxypropylene) copolymers derived from polyhydric alcohols such as glycerin and sugars, and other nonionic surfactants, active hydrogen compounds such as epoxy compounds, polyamine compounds, and polythiol compounds, isocyanate compounds, acrylate compounds, methacrylate compounds, vinyl toluene compounds, and vinyl acetate compounds.

[0022] The dispersion medium may be used alone or in combination of two or more.

[0023] <<Powder flame retardants>> The powder flame retardant is not particularly limited, and for example, a conventionally known powder flame retardant can be used, and preferably contains one or more selected from red phosphorus, phosphates, phosphinates, cellulose, and expandable graphite. The powder flame retardant may also contain other components (for example, other powder flame retardants).

[0024] <Red phosphorus> The red phosphorus is not particularly limited, and may be untreated red phosphorus or surface-treated or surface-coated red phosphorus.

[0025] The average diameter of the red phosphorus is preferably 300 μm or less, 200 μm or less, or 100 μm or less, and is preferably 25 μm or more, 50 μm or more, or 75 μm or more.

[0026] <Phosphate> The phosphate is not particularly limited, and may be a monophosphate or a polyphosphate.

[0027] Examples of monophosphates include: Ammonium salts such as ammonium phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate; Sodium salts such as monosodium phosphate, disodium phosphate, trisodium phosphate, monosodium phosphite, disodium phosphite, and sodium hypophosphite; Potassium salts such as monopotassium phosphate, dipotassium phosphate, tripotassium phosphate, monopotassium phosphite, dipotassium phosphite, and potassium hypophosphite; Lithium salts such as lithium monophosphate, lithium diphosphate, lithium triphosphate, lithium monophosphite, lithium diphosphite, and lithium hypophosphite; barium salts such as barium dihydrogen phosphate, barium hydrogen phosphate, barium triphosphate, and barium hypophosphite; magnesium salts such as magnesium monohydrogen phosphate, magnesium hydrogen phosphate, magnesium trimagnesium phosphate, and magnesium hypophosphite; Calcium salts such as calcium dihydrogen phosphate, calcium hydrogen phosphate, tricalcium phosphate, calcium hypophosphite; zinc salts such as zinc phosphate, zinc phosphite, zinc hypophosphite, etc., aluminum salts such as aluminum monophosphate, aluminum diphosphate, aluminum triphosphate, aluminum phosphite, aluminum hypophosphite, etc.; etc. can be mentioned.

[0028] Examples of the polyphosphate include ammonium polyphosphate, piperazine polyphosphate, melamine polyphosphate, ammonium amide polyphosphate, and aluminum polyphosphate.

[0029] The phosphates may be used alone or in combination.

[0030] The average diameter of the phosphate is preferably 1 to 100 μm.

[0031] <Phosphinate> The phosphinate is not particularly limited, and for example, a metal phosphinate represented by the following formula can be used.

[0032] [ka]

[0033] In the formula, R1 and R2 are each independently a hydrogen atom or a linear or branched, saturated or unsaturated hydrocarbon group. The hydrocarbon group can be, for example, an alkyl group having 1 to 6 carbon atoms, an alkenyl group, a cycloalkyl group, a phenyl group, a benzyl group, a tolyl group, or the like.

[0034] In the formula, M represents a metal ion having a valence of n. The metal ion M can be Mg, Ca, Al, Sb, Sn, Ge, Ti, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K, etc. M is preferably Al.

[0035] The phosphinates may be used alone or in combination.

[0036] The average diameter of the phosphinate is preferably 1 to 100 μm.

[0037] <Cellulose> The cellulose is not particularly limited, and for example, a component derived from a general natural product can be used, and microcellulose, cellulose nanofiber (CNF), etc. can be used. For example, cellulose obtained by subjecting a raw material (e.g., pulp) to defibration treatment (mechanical treatment / chemical treatment) by a known method can be used. In addition, the cellulose may be modified. When CNF is used, it may be further surface-treated.

[0038] The average diameter of the cellulose is preferably 15 to 35 μm. The average diameter of the cellulose can be measured by a laser diffraction method. The average length of the cellulose is preferably 10 to 1000 μm. The average length of the cellulose can be a value measured based on ISO 16065-1:2001.

[0039] <Expanded graphite> The expandable graphite is not particularly limited, and any known expandable graphite can be used, for example, graphite obtained by immersing natural graphite in a mixture of sulfuric acid, nitric acid, etc. and adding an oxidizing agent such as hydrogen peroxide or hydrochloric acid.

[0040] The expandable graphite that can be used has an expansion start temperature of about 130 to 300° C. and an expansion volume of 50 to 300 cc / g.

[0041] The average diameter of the expanded graphite before expansion is preferably 50 to 500 μm.

[0042] <Other powder flame retardants> Other powder flame retardants include solid phosphate ester-based flame retardants, boron-containing flame retardants, needle-like fillers, bromine-containing flame retardants, nitrogen-based flame retardants, antimony-containing flame retardants, and metal hydroxides.

[0043] <<Silica-based particles>> The silica-based particles are not particularly limited, and known particles can be used, including wet silica such as precipitated silica, sol-gel silica, and colloidal silica, and dry silica such as deflagration silica and fumed silica. As the silica-based particles, fumed silica is preferred because it can improve the dispersibility of the powder flame retardant.

[0044] The silica-based particles preferably have an average diameter of 50 to 300 μm, and more preferably 150 to 250 μm.

[0045] The ratio of the average diameter of the powder flame retardant to the average diameter of the silica-based particles (average diameter of the powder flame retardant / average diameter of the silica-based particles) is preferably 2 / 1 to 1 / 20, 3 / 2 to 1 / 15, or 1 / 1 to 1 / 10.

[0046] <<Silicone surfactants>> The silicone-based surfactant is a surfactant containing a siloxane bond as the skeleton, and typically, a polyether-modified silicone can be used.

[0047] The silicone surfactant preferably has a molecular structure in which a polyalkylsilyl ether (e.g., polydimethylsiloxane) and a polyoxyalkylene ether (e.g., polyethers such as polyethylene glycol and polypropylene glycol) are graft-copolymerized or linear-block-copolymerized. The silicone surfactant may be appropriately modified.

[0048] The silicone surfactant is particularly preferably a component represented by the following formula:

[0049] [ka]

[0050] [ka]

[0051] In the formula, R represents an alkyl group having 1 or more and 10 or less carbon atoms (preferably 1 or more and 3 or less, preferably 1), m represents an integer of 0 or more, n represents an integer of 1 or more, c and d are both 0 or more and represent integers such that c+d is 1 or more (preferably, c is 1 or more).

[0052] As the silicone surfactant, commercially available products can also be used. As commercially available products, DOWSIL SH-192, DOWSIL SH-193, DOWSIL SF-2904, DOWSIL SF-2936, DOWSIL SF-2937, DOWSIL SF-2938, DOWSIL SZ-1333, DOWSIL SZ-1671, DOWSIL SZ-1718, DOWSIL SZ-580, DOWSIL manufactured by Dow Toray SRX-298, DOWSIL SZ-1142, DOWSIL SZ-1968, DOWSIL 8868 additive; Momentive Performance Materials: Niax L-6887, Niax L-6888, Niax L-6120, Niax L-5420, Niax Y-16248, Niax L-6978, Niax L-6100, Niax L-626, Niax L-540, Niax L-580, Niax L-618, Niax L-620, Niax L-639; Evonik: TEGOSTAB B8481, TEGOSTAB B84817, TEGOSTAB B8465, TEGOSTAB B8462, TEGOSTAB B8460, TEGOSTAB B84711, TEGOSTAB B8450, TEGOSTAB B8110, TEGOSTAB BF2470, TEGOSTAB B8266, TEGOSTAB B8255; Shin-Etsu Chemical Co., Ltd.'s X-22-4952, X-22-4972, KF-6123, KF-6000, KF-6001, KF-6002, KF-6003, KF-9701, X-22-170BX, KF-945, KF-6011, X-22-2516, and KF-6004; etc.

[0053] The silicone surfactant preferably has an HLB value of 3 or more, 3.5 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 11 or more, or 12 or more, and preferably has an HLB value of 19 or less, 18.5 or less, 18 or less, 17 or less, 16 or less, 15 or less, or 14 or less. For example, the HLB value is preferably 3 to 19, 3.5 to 19, 5 to 18.5, 7 to 17, or 10 to 15.

[0054] The silicone surfactant that can be used has a weight average molecular weight of 300 to 100,000 (preferably 1,000 to 50,000). The weight average molecular weight is a value measured by GPC and converted into standard polystyrene.

[0055] According to the composition of the present invention, by using the powder flame retardant in combination with the silica-based particles and the silicone-based surfactant, the particles are wetted with the dispersion medium, which makes it easier to mix with the resin raw material (such as polyol, etc.), and furthermore, the aggregation (secondary aggregation) of the powder flame retardant particles can be suppressed. Furthermore, according to the composition of the present invention, the composition is appropriately thickened, which makes it possible to prevent the sedimentation of solids and the occurrence of caking over time. Furthermore, according to the composition of the present invention, it is possible to improve the handleability and the ease of mixing with the raw material composition of the resin foam.

[0056] <<Other ingredients>> The flame retardant composition may optionally contain other ingredients.

[0057] Other components include known dispersants, such as amine salt dispersants, carboxylic acid polymer dispersants, ester polymer dispersants, and phosphoric acid dispersants.

[0058] The other components may contain other known additives, and the other known additives may be additives that are necessary for producing a resin foam or that are effective when the resin foam is produced. Examples of the other known additives include a foam stabilizer, an antioxidant, an ultraviolet absorber, an antibacterial agent, a catalyst, etc.

[0059] <<<Content of each ingredient>>> The amount of the dispersion medium in the flame retardant composition is taken as 100 parts by weight. The content of the powder flame retardant in the flame retardant composition is preferably 40 parts by weight or more, 50 parts by weight or more, 60 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, or 90 parts by weight or more, and is preferably 99 parts by weight or less, 98 parts by weight or less, or 97 parts by weight or less. The content of the silica-based particles in the flame retardant composition is preferably 0.1 parts by weight or more, 0.2 parts by weight or more, 0.5 parts by weight or more, 1 part by weight or more, 2 parts by weight or more, or 5 parts by weight or more, and is preferably 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less. The content of the silicone surfactant in the flame retardant composition is preferably 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.15 parts by weight or more, and is preferably 5 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.5 parts by weight or less. The other components may be considered as the remainder.

[0060] The weight ratio of the silicone-based surfactant to the silica-based particles (silicone-based surfactant:silica-based particles) is preferably 2:1 to 1:200, 1:1 to 1:150, 1:2 to 1:100, 1:5 to 1:50, or 1:20 to 1:50.

[0061] The content of the dispersion medium in the flame retardant composition may be appropriately adjusted depending on the type of the dispersion medium and the composition / physical properties of the raw material composition of the resin foam used. For example, when the total content of the powdered flame retardant, the silica-based particles, and the silicone-based surfactant in the flame retardant composition is 100 parts by weight, the content of the dispersion medium is preferably 50 to 500 parts by weight or 50 to 200 parts by weight.

[0062] <<<<<Physical properties / properties of flame retardant compositions>>>> <<<Thixotropy index value at 25℃>>> The flame retardant composition preferably has a thixotropy index value at 25° C. (25° C. TI value) of 1.0 to 6.0, 1.5 to 5.5, or 2.0 to 5.0.

[0063] The 25°C TI value can be measured by the following method. 50 mL of the sample was transferred to a sample bottle, and then placed in a thermostatic bath at 25°C to maintain the sample at 25°C. The viscosity was measured at rotation speeds of 1 rpm and 10 rpm using a B-type viscometer (Brookfield, rotor No. 4). The viscosity ratio (viscosity at rotation speed of 1 rpm / viscosity at rotation speed of 10 rpm) was defined as the 25°C TI.

[0064] The 25° C. TI value of the flame retardant composition can be adjusted to fall within the above range by adjusting the ratio of the silica particles to the silicone surfactant within an appropriate range or by adjusting the amount of the dispersion medium.

[0065] <<<25℃ viscosity>>> The flame retardant composition preferably has a viscosity at 25°C of 12,000 mPa·s or more, 15,000 mPa·s or more, or 20,000 mPa·s or more, and preferably 100,000 mPa·s or less, 75,000 mPa·s or less, or 50,000 mPa·s or less.

[0066] The 25° C. viscosity can be measured by the following method. 50 mL of the sample is transferred to a sample bottle, and then the bottle is placed in a thermostatic chamber at 25° C. to maintain the sample at 25° C. The viscosity is measured using a B-type viscometer (Brookfield, rotor No. 4) at a rotation speed of 6 rpm.

[0067] The viscosity at 25° C. of the flame retardant composition can be adjusted to fall within the above range by adjusting the ratio of the silica particles to the silicone surfactant within an appropriate range or by adjusting the amount of the dispersion medium.

[0068] <<<<<Method of manufacturing flame retardant composition>>>> The method for producing the flame retardant composition is not particularly limited, and for example, the composition containing various components is stirred and mixed with a stirrer or the like, and degassed as necessary. The various components may be added to the composition simultaneously, or may be added to the composition separately in an appropriate order. For example, the solid component and the liquid component may be prepared separately and mixed.

[0069] <<<<<Applications of flame retardant compositions>>>> The flame retardant composition can be used for producing a resin foam. More specifically, the flame retardant composition can be used for producing a resin foam raw material composition.

[0070] Specifically, the flame retardant composition can be used as a component further added to the raw material composition when a resin foam is produced by carrying out a step of foaming the raw material composition. More specifically, a flame-retardant resin foam can be produced by mixing the raw material of the resin foam and the flame retardant composition to prepare a raw material composition, foaming and curing the raw material composition, and processing it as necessary.

[0071] The type of resin foam to which the flame retardant composition is applied is not particularly limited, but is preferably a urethane foam or a polyisocyanurate foam. The flame retardant composition can also be applied to polyurea foam, polyester foam, polystyrene foam, polyolefin foam, polyacrylate foam, epoxy resin foam, etc.

[0072] The resin foam may be produced by spraying. When the resin foam is produced by spraying, the raw material composition may be divided into a plurality of compositions and stored, for example, as a two-liquid composition. In such a case, the flame retardant composition may be added simultaneously when these compositions are mixed, or may be added to any of the compositions in advance. EXAMPLES

[0073] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following.

[0074] <<<Raw materials>>> <<Dispersion medium>> <Phosphate ester 1> Chlorinated phosphate esters <Phosphate ester 2> Aromatic phosphate ester <Polyol compound> Aromatic ester polyol

[0075] <<Powder flame retardants>> <fr-1> Red phosphorus Exolit RP607 (Clariant) Average diameter: 100μm <fr-2> Ammonium Polyphosphate Exolit Ap-422 (Clariant) Average diameter: 50μm <fr-3> Aluminum diethylphosphinate Exolit OP-930 (Clariant) Average diameter: 20μm <fr-4> Expanded graphite 9550250 (Ito Graphite Co., Ltd.) Average diameter: 300μm

[0076] <<Silicone surfactants>> <s-1> DOWSIL SF-2937F (Dow Toray) PDMS-PPG / PEG copolymer, pendant type, HLB:13.0 Weight average molecular weight: 8878 <s-2> DOWSIL SH-192 (Dow Toray) PDMS-PPG / PEG copolymer, pendant type, HLB:18.0 Weight average molecular weight: 19891 <s-3> DOWSIL SH-193 (Dow Toray) PDMS-PPG / PEG copolymer, pendant type, HLB:19.0 Weight average molecular weight: 2789 <s-4> DOWSIL SZ-1333 (Dow Toray) PDMS-PPG / PEG copolymer, linear type, HLB: 3.5 Weight average molecular weight: 24381 <<Non-silicone surfactants>> <s-5> Sannix LP-3000 (manufactured by Sanyo Chemical Industries, Ltd.) Higher alcohol-added PEG-PPG copolymer HLB: 17.2 Weight average molecular weight: 17348

[0077] <<Silica-based particles>> <hs-1> AEROSIL #200 (fumed silica, particle size: 200 μm) <hs-2> AEROSIL #100 (fumed silica, particle size: 100 μm)

[0078] <<Dispersant>> <d-1> Unsaturated Carboxylic Acid Polymer (BYK P-105) <d-2> Polyether phosphate ester (Disparlon AQ-330) <d-3> Ammonium polyacrylate (SN Dispersant 5027)

[0079] <<<Preparation of flame retardant composition>>> Flame retardant compositions according to the respective Examples and Comparative Examples were prepared as follows. The amounts of each raw material used in the flame retardant composition are as shown in the table. The dispersion medium and dispersant were added to a disposable cup, and the mixture was stirred at 1,000 rpm for 10 minutes using a stirrer. The powdered flame retardant was added and mixed until uniform. The surfactant was added and mixed until uniform. The composition was degassed under reduced pressure using a vacuum pump.

[0080] <<<Evaluation>>> For each flame retardant composition, the change in viscosity at 25°C, the TI value at 25°C, the amount of residue on filtration, and the appearance and caking were evaluated.

[0081] <<Change in viscosity at 25℃>> The rate of change in viscosity at 25°C of the flame retardant composition which had been left to stand in a heating furnace at 40°C for one month after production relative to the viscosity at 25°C of the flame retardant composition immediately after production was measured. The viscosity at 25°C was measured according to the above-mentioned method.

[0082] <Evaluation criteria> Less than 20% increase in viscosity: 2 points 20% to 30% thickening: 1 point Increase or decrease in viscosity by more than 30%: 0 points

[0083] <<25℃ TI value>> The 25°C TI value was measured for the flame retardant composition immediately after production and for the flame retardant composition which had been left to stand in a heating furnace at 40°C for one month after production. The 25°C TI value was measured according to the method described above.

[0084] <Evaluation criteria> 3.5 or more and 5.0 or less: 3 points 2.0~3.5 :1 point Less than 2.0 or more than 5.0: 0 points

[0085] <<Filtration residue>> 20 g of the flame retardant composition was collected and subjected to suction filtration using a 40 mesh filter. The amount of residue was calculated from the difference in weight of the filter before and after filtration (amount of composition remaining on the filter) and the weight of the sample used for filtration. The measurement of the amount of residue after filtration was performed on the flame retardant composition immediately after production and on the flame retardant composition which was left to stand for one month in a heating furnace at 40° C. after production. When the composition was separated into a liquid phase and a solid phase and the powder could not be filtered, it was determined that the amount of residue after filtration was not measurable.

[0086] <Evaluation criteria> 2.0% or less: 2 points More than 2.0% and less than 5.0%: 1 point Over 5.0% or not measurable: 0 points

[0087] <<Appearance>> After leaving the flame retardant composition in a heating furnace at 40° C. for one month, the appearance of the sample was visually checked to see if it had separated into a transparent liquid (phosphate ester) and a powder component.

[0088] <Evaluation criteria> No separation: 〇(2 points) Separation into solid and liquid phases: × (0 points)

[0089] <<Caking>> After leaving the flame retardant composition for one month in a heating oven at 40°C, the composition was palpated with a spoon to check whether the tip of the spoon could move.

[0090] <Evaluation criteria> The tip of the spoon moves freely without resistance (no caking): Good (2 points) Unable to move the tip of the medicine spoon: × (0 points)

[0091] <<Overall Judgment>> Based on each evaluation, the overall score was evaluated as follows: 15 points or more was indicated as ◎, 10 to 14 points as ○, 5 to 9 points as △, and 4 points or less as ×.

[0092]

Table 1

[0093]

Table 2

[0094]

Table 3

Claims

1. A flame retardant composition comprising a dispersion medium, a powder flame retardant, silica-based particles, and a silicone-based surfactant, the flame retardant composition being used for producing a resin foam.

2. The flame retardant composition according to claim 1, characterized in that a weight ratio of the silicone-based surfactant to the silica-based particles (the silicone-based surfactant:the silica-based particles) is 1:1 to 1:

150.

3. The flame retardant composition according to claim 1 or 2, wherein the dispersion medium contains a polyol compound and / or a phosphoric acid ester.

4. The flame retardant composition according to any one of claims 1 to 3, wherein the silica-based particles include fumed silica.

5. The silicone surfactant is HLB value is 3 to 19; It has a molecular structure in which polyalkylsilyl ether and polyoxyalkylene ether are graft-copolymerized or linear block-copolymerized. The flame retardant composition according to any one of claims 1 to 4.

6. The flame retardant composition according to any one of claims 1 to 5, characterized in that the powder flame retardant contains one or more selected from the group consisting of red phosphorus, phosphates, phosphinates, cellulose, and expandable graphite.

7. The flame retardant composition according to any one of claims 1 to 6, characterized in that the thixotropy index value at 25°C is 2.0 or more and 5.0 or less.

8. A method for producing a resin foam, comprising the steps of: A method for producing a resin foam, comprising a step of foaming a raw material composition containing the flame retardant composition according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Flame-retardant thermal and acoustic insulation material

    JP2004043747A

  • Flame-retardant filter foam

    JP2006083208A

  • Fire retardant sound barrier material

    JP2007044919A

  • Flame resistant heat insulation composition

    JP2015078357A

  • Polyol-containing composition, foamable polyurethane composition and polyurethane foam