Etching composition, etching method, method for manufacturing semiconductor device, and method for manufacturing gate-all-around transistor
The etching composition with nitric acid and organic acid enhances silicon germanium solubility, addressing fin collapse and performance issues in transistors by promoting selective etching.
Patent Information
- Application Number
- JP2024145378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-12-15
AI Technical Summary
Existing etching compositions for silicon germanium do not provide sufficient selective solubility, leading to issues such as fin collapse during processing and inadequate performance in Fin-type and Gate-All-Around transistors.
An etching composition comprising nitric acid as an oxidizing agent, an organic acid, and optionally a fluorine-containing compound, with specific mass ratios, that selectively dissolves silicon germanium while minimizing silicon dissolution.
The composition achieves high selective solubility of silicon germanium, enabling precise etching and high yield manufacturing of semiconductor devices, particularly Gate-All-Around transistors.
Smart Images

Figure 2024155993000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an etching composition, an etching method, a method for manufacturing a semiconductor device, and a method for manufacturing a gate-all-around transistor. [Background technology]
[0002] In accordance with Moore's Law, integrated circuits are becoming increasingly miniaturized. In recent years, in addition to reducing the size of conventional planar transistors, research is being conducted to improve performance by changing the structure, such as with fin transistors (fin FETs) and gate-all-around transistors (GAA FETs), while also promoting further miniaturization and integration.
[0003] In fin-type FETs, by forming fins vertically to the silicon substrate, not only does it increase the number of transistors per unit area, but it also exhibits excellent performance in ON / OFF control at low voltages. However, in order to further improve performance, it is necessary to devise ways to increase the aspect ratio of the fins, but if the aspect ratio is too large, there are issues such as the fins collapsing during the cleaning and drying processes used for fin formation.
[0004] On the other hand, in GAA FETs, the nanosheet or nanowire that forms the channel is covered with a gate electrode, increasing the contact area between the channel and gate electrode, thereby improving the transistor performance per unit area.
[0005] In order to form a GAA FET, an etching composition is required for selectively etching silicon germanium from a structure in which silicon and silicon germanium are alternately stacked. As such an etching composition, Patent Document 1 discloses a composition containing acetic acid. Patent Document 2 discloses a composition containing hydrogen peroxide. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-303305 A [Patent Document 2] JP 2019-050365 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the etching composition disclosed in Patent Document 1 has a low content of acetic acid, and the selective solubility of silicon germanium relative to silicon is not sufficient. Moreover, the etching composition containing hydrogen peroxide disclosed in Patent Document 2 also does not have sufficient selective solubility of silicon germanium relative to silicon.
[0008] As described in Patent Documents 1 and 2, etching compositions containing various components have been investigated in the past, but none of them have been found to have sufficient selective solubility of silicon germanium relative to silicon.
[0009] The present invention has been made in view of the above problems, and an object of the present invention is to provide an etching composition that suppresses dissolution of silicon, promotes dissolution of silicon germanium, and has excellent selective solubility of silicon germanium relative to silicon. Another object of the present invention is to provide an etching method using the etching composition, a method for manufacturing a semiconductor device, and a method for manufacturing a gate-all-around transistor. [Means for solving the problem]
[0010] As a result of extensive research, the present inventors have found that the etching composition of the present invention described below inhibits the dissolution of silicon, promotes the dissolution of silicon germanium, and has excellent selective solubility of silicon germanium relative to silicon.
[0011] That is, the gist of the present invention is as follows. [1] An etching composition which selectively dissolves silicon germanium relative to silicon, comprising an oxidizing agent (A) and an organic acid (B), wherein the oxidizing agent (A) contains nitric acid, and the content of the organic acid (B) is 50 mass% or more in 100 mass% of the etching composition. [2] The etching composition according to [1], wherein the organic acid (B) contains at least one compound selected from the group consisting of acetic acid, propionic acid, oxalic acid and citric acid. [3] The etching composition according to [1] or [2], further comprising a fluorine-containing compound (C). [4] The etching composition according to [3], wherein the fluorine-containing compound (C) contains at least one compound selected from the group consisting of hydrofluoric acid, ammonium fluoride, and hexafluorosilicic acid. [5] The etching composition according to [3] or [4], wherein the content of the fluorine-containing compound (C) is 5 mass% or less in 100 mass% of the etching composition. [6] The etching composition according to any one of [1] to [5], further comprising water (D). [7] The etching composition according to [6], wherein the content of water (D) is 20 mass% or less in 100 mass% of the etching composition. [8] An etching method comprising etching a structure containing silicon and silicon germanium by using the etching composition according to any one of [1] to [7]. [9] A method for manufacturing a semiconductor device, comprising a step of etching a structure containing silicon and silicon germanium using the etching composition according to any one of [1] to [7].
[10] A method for manufacturing a gate-all-around transistor, comprising a step of etching a structure containing silicon and silicon germanium using the etching composition according to any one of [1] to [7]. Effect of the Invention
[0012] The etching composition of the present invention inhibits dissolution of silicon, promotes dissolution of silicon germanium, and has excellent selective solubility of silicon germanium relative to silicon. Furthermore, the etching method of the present invention using such an etching composition of the present invention, the manufacturing method of a semiconductor device of the present invention, and the manufacturing method of a gate-all-around transistor of the present invention suppress the dissolution of silicon and promote the dissolution of silicon germanium in the etching step, and due to the excellent selective solubility of silicon germanium relative to silicon, it is possible to perform highly accurate etching and manufacture desired products with good yields. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified and implemented in various ways within the scope of the gist. In addition, when the expression "~" is used in this specification, it is used as an expression including the numerical values or physical property values before and after it.
[0014] The etching composition of the present invention contains an oxidizing agent (A) (hereinafter, sometimes referred to as "component (A)") and an organic acid (B) (hereinafter, sometimes referred to as "component (B)"), and since the oxidizing agent (A) contains nitric acid and the content of the organic acid (B) is 50 mass% or more in 100 mass% of the etching composition, silicon germanium can be selectively dissolved relative to silicon.
[0015] <Component (A)> The component (A) is an oxidizing agent. By including an oxidizing agent in the etching composition, the effect of oxidizing the surface of silicon or silicon germanium is exhibited.
[0016] Examples of the oxidizing agent include nitric acid, hydrogen peroxide, permanganic acid, periodic acid, and perchloric acid. These oxidizing agents may be used alone or in combination of two or more. Among these oxidizing agents, nitric acid and hydrogen peroxide are preferred because they can remove metals that are a source of contamination, and nitric acid is more preferred because it has excellent selective oxidation properties for silicon germanium. Therefore, the etching composition of the present invention is characterized in that it contains at least nitric acid as the oxidizing agent of component (A).
[0017] The content of component (A) is preferably 5% by mass or more, and more preferably 10% by mass or more, in 100% by mass of the etching composition, because the component (A) has an excellent selective oxidation property for silicon germanium. The content of component (A) is preferably 50 mass % or less, and more preferably 40 mass % or less, in 100 mass % of the etching composition, because this is excellent in suppressing etching of silicon.
[0018] When an oxidizing agent other than nitric acid is used in combination as component (A), from the viewpoint of effectively obtaining the effect of selective oxidation of silicon germanium by using nitric acid, the content of nitric acid in 100 mass% of component (A) is preferably 50 mass% or more, and more preferably 80 to 100 mass%.
[0019] <Ingredient (B)> The component (B) is an organic acid. By including an organic acid in the etching composition, the effect of protecting silicon and an oxide film is exhibited.
[0020] Examples of organic acids include acetic acid, propionic acid, oxalic acid, and citric acid. These organic acids may be used alone or in combination of two or more. Among these organic acids, acetic acid, propionic acid, oxalic acid, and citric acid are preferred, and acetic acid is more preferred, because they are excellent in suppressing silicon etching.
[0021] The content of component (B) is 50 mass% or more, preferably 55 mass% or more, and more preferably 60 mass% or more, in 100 mass% of the etching composition, because it has excellent silicon etching suppression properties and excellent penetration into narrow spaces. The content of component (B) is preferably 95 mass % or less, more preferably 90 mass % or less, and even more preferably 75 mass % or less, in 100 mass % of the etching composition, because the component (B) has excellent selective oxidation properties for silicon germanium.
[0022] <Ingredient (C)> The etching composition of the present invention preferably contains a fluorine-containing compound (C) (hereinafter sometimes referred to as "component (C)") in addition to the components (A) and (B).
[0023] When the etching composition contains the fluorine-containing compound as component (C), it exerts the effect of etching the surface of oxidized silicon or the surface of silicon germanium.
[0024] Examples of fluorine-containing compounds include hydrofluoric acid, ammonium fluoride, and hexafluorosilicic acid. These fluorine-containing compounds may be used alone or in combination of two or more. Among these fluorine-containing compounds, hydrofluoric acid, ammonium fluoride, and hexafluorosilicic acid are preferred, and hydrofluoric acid is more preferred, because they have excellent selective solubility of silicon germanium.
[0025] The content of the component (C) is preferably 0.01 mass % or more, and more preferably 0.1 mass % or more, in 100 mass % of the etching composition, because the component (C) has excellent solubility for silicon germanium. From the viewpoint of reducing damage to silicon, the content of the component (C) is preferably 5 mass % or less, and more preferably 3 mass % or less, in 100 mass % of the etching composition.
[0026] <Ingredient (D)> The etching composition of the present invention preferably contains water (D) (hereinafter sometimes referred to as "component (D)") in addition to the components (A), (B) and (C).
[0027] When the etching composition contains water as the component (D), it exerts the effect of inhibiting etching of silicon.
[0028] The content of the component (D) is preferably 5% by mass or more, and more preferably 10% by mass or more, in 100% by mass of the etching composition, because the etching composition is easy to produce. The content of the component (D) is preferably 30 mass % or less, and more preferably 20 mass % or less, in 100 mass % of the etching composition, because the etch rate can be improved.
[0029] <Other ingredients> The etching composition of the present invention may contain other components in addition to the component (A), the component (B), the component (C) and the component (D).
[0030] <Mass ratio of each component> The mass ratio of component (B) to component (A) in the etching composition of the present invention (mass of component (B) / mass of component (A), hereinafter referred to as "(B) / (A)") is preferably 1 to 10, and more preferably 2 to 5, since this provides an excellent balance between the effect of oxidizing the surface of silicon or silicon germanium and the effect of protecting silicon or an oxide film.
[0031] The mass ratio of component (C) to component (A) in the etching composition of the present invention (mass of component (C) / mass of component (A), hereinafter referred to as "(C) / (A)") is preferably 0.005 to 0.1, and more preferably 0.01 to 0.05, because this provides an excellent balance between the effect of oxidizing the surface of silicon or silicon germanium and the effect of etching the surface of oxidized silicon or silicon germanium.
[0032] The mass ratio of component (C) to component (B) in the etching composition of the present invention (mass of component (C) / mass of component (B), hereinafter referred to as "(C) / (B)") is preferably 0.001 to 0.05, and more preferably 0.002 to 0.025, since this provides an excellent balance between the effect of protecting silicon or an oxide film and the effect of etching the surface of oxidized silicon or the surface of silicon germanium.
[0033] <Method of manufacturing the etching composition> The method for producing the etching composition of the present invention is not particularly limited, and the composition can be produced by mixing component (A) and component (B), and, if necessary, component (C), component (D), and other components. The order of mixing is not particularly limited, and all of the components may be mixed at once, or some of the components may be mixed in advance and then the remaining components may be mixed.
[0034] <Physical properties of etching composition> The silicon etch rate ER of the etching composition of the present invention Si Since the selective solubility of silicon germanium in silicon is excellent, the rate is preferably 1.0 nm / min or less, more preferably 0.5 nm / min or less, and even more preferably 0.3 nm / min or less.
[0035] The silicon germanium etch rate ER of the etching composition of the present invention SiGe Since the selective solubility of silicon germanium in silicon is excellent, the rate is preferably 0.5 nm / min or more, more preferably 1.0 nm / min or more, and even more preferably 2.0 nm / min or more.
[0036] The dissolution selectivity DSR (ER) of the etching composition of the present invention between silicon and silicon germanium SiGe / ER Si ) is preferably 10 or more, and more preferably 15 or more, because the selective solubility of silicon germanium in silicon is excellent.
[0037] Since silicon oxide may be exposed in a structure containing silicon and silicon germanium, it is preferable to suppress dissolution of the silicon oxide. The etch rate ER of silicon oxide of the etching composition of the present invention SiOx is preferably 50 nm / min or less, more preferably 40 nm / min or less, and even more preferably 30 nm / min or less.
[0038] In addition, the etch rate ER Si , etch rate ER SiGe , Dissolution selectivity DSR, Etch rate ER SiOx is measured and calculated by the method described in the Examples section below.
[0039] <Target to be etched by etching composition> The etching composition of the present invention suppresses dissolution of silicon, promotes dissolution of silicon germanium, and has excellent selective solubility of silicon germanium relative to silicon. Therefore, the etching composition of the present invention is suitable for etching structures containing silicon and silicon germanium, such as semiconductor devices, and is particularly suitable for structures in which silicon and silicon germanium are alternately stacked, which are necessary for forming a GAA type FET.
[0040] The silicon content in the silicon germanium to be etched is preferably 10 mass % or more, and more preferably 20 mass % or more, based on 100 mass % of silicon germanium, since this is suitable for etching with the etching composition of the present invention. On the other hand, the silicon content in silicon germanium is preferably 95 mass % or less, and more preferably 85 mass % or less, in 100 mass % of silicon germanium, because this is suitable for etching with the etching composition of the present invention. Furthermore, the germanium content in silicon germanium is preferably 5 mass % or more, and more preferably 15 mass % or more, based on 100 mass % of silicon germanium, since this is suitable for etching with the etching composition of the present invention. On the other hand, the germanium content in silicon germanium is preferably 90 mass % or less, and more preferably 80 mass % or less, in 100 mass % of silicon germanium, because this is suitable for etching with the etching composition of the present invention.
[0041] The silicon germanium alloy film may be produced by deposition using a known method, but is preferably produced by deposition using a crystal growth method, since this provides excellent mobility of electrons and holes after the formation of a transistor.
[0042] In a structure containing silicon and silicon germanium or a structure in which silicon and silicon germanium are alternately laminated, silicon oxide may be exposed.
[0043] <Etching method> The etching method of the present invention is a method for etching a structure containing silicon and silicon germanium using the etching composition of the present invention.
[0044] The etching method may be a known method, such as a batch method or a single wafer method.
[0045] The temperature during etching is preferably 15° C. or higher, and more preferably 20° C. or higher, since this allows the etching rate to be improved. The temperature during etching is preferably 100° C. or less, and more preferably 80° C. or less, from the viewpoints of reducing damage to the substrate and ensuring etching stability. Here, the temperature during etching corresponds to the temperature of the etching composition during etching.
[0046] <Application> The etching composition and the etching method of the present invention can be suitably used in the manufacture of semiconductor devices, which includes a step of etching a structure containing silicon and silicon germanium, and can be particularly suitably used in the manufacture of GAA type FETs, which includes a step of etching a structure containing silicon and silicon germanium, since the etching composition and the etching method of the present invention suppress the dissolution of silicon, promote the dissolution of silicon germanium, and have excellent selective solubility of silicon germanium relative to silicon. EXAMPLES
[0047] The present invention will be described in more detail below using examples. However, the present invention is not limited to the description of the following examples as long as it does not deviate from the gist of the present invention.
[0048] <Raw materials> In the following Examples and Comparative Examples, the following materials were used as raw materials for producing the etching compositions. Ingredient (A-1): Nitric acid Ingredient (A'-1): Hydrogen peroxide Ingredient (B-1): Acetic acid Component (C-1): Hydrofluoric acid Ingredient (D-1): Water
[0049] <Method of measuring silicon etch rate> A silicon substrate cut to 7 cm x 7 cm and having a thickness of about 0.7 mm was immersed in the etching composition obtained in the examples and comparative examples at 25°C for 60 minutes or more. The mass of the silicon substrate before and after immersion was measured using a balance, and the silicon etch rate ER was calculated from the change in mass using the following formula (1). Si [nm / min] was calculated. ER Si [nm / min] = mass change of silicon substrate ÷ (density of silicon substrate × surface area of silicon substrate × immersion time of silicon substrate) (1)
[0050] <Method of measuring the etch rate of silicon germanium> A silicon substrate having a silicon germanium alloy film (thickness 50 nm) having a germanium content of 25 mass% formed on its surface was immersed in the etching compositions obtained in the Examples and Comparative Examples at 25° C., and the change in film thickness was measured using a spectroscopic ellipsometer (model name "UVISEL ER", manufactured by Horiba, Ltd.). The etch rate ER of silicon germanium was calculated using the following formula (2). SiGe [nm / min] was calculated. ER SiGe [nm / min] = change in thickness of silicon germanium alloy film ÷ immersion time of silicon substrate (2)
[0051] <Dissolution selectivity between silicon and silicon germanium> The dissolution selectivity ratio DSR of silicon and silicon germanium was calculated using the following formula (3). DSR=ER SiGe [nm / min]÷ER Si [nm / min] (3)
[0052] <Method of measuring silicon oxide etch rate> A silicon substrate having a silicon oxide film (thickness 280 nm) formed on its surface was immersed in the etching composition obtained in the examples and comparative examples at 25° C., and the change in film thickness was measured using a reflection spectroscopic film thickness meter (model name "FE-3000", manufactured by Otsuka Electronics Co., Ltd.). The etch rate ER of silicon oxide was calculated using the following formula (4). SiOx [nm / min] was calculated. ER SiOx [nm / min] = change in thickness of silicon oxide film ÷ immersion time of silicon substrate (4)
[0053] [Example 1] The etching composition was obtained by mixing the components so that, based on 100 mass% of the etching composition, the components (A-1) were 21.0 mass%, the component (B-1) was 62.5 mass%, the component (C-1) was 1.0 mass%, and the component (D-1) was 15.5 mass%. The evaluation results of the obtained etching compositions are shown in Table 1.
[0054] [Examples 2 to 4, Comparative Examples 1 to 3] The same procedure as in Example 1 was carried out except that the types and contents of the raw materials were as shown in Table 1, to obtain etching compositions. The evaluation results of the obtained etching compositions are shown in Table 1.
[0055] [Table 1]
[0056] As can be seen from Table 1, the etching compositions obtained in Examples 1 to 4 suppress the dissolution of silicon, promote the dissolution of silicon germanium, and are excellent in the selective solubility of silicon germanium relative to silicon.
[0057] The etching composition obtained in Comparative Example 1, which contained less component (B) and more component (D), suppressed the dissolution of silicon, but also suppressed the dissolution of silicon germanium, and was therefore inferior in the selective solubility of silicon germanium relative to silicon.
[0058] The etching composition obtained in Comparative Example 2, which contains less component (B) and more component (A), promoted the dissolution of silicon germanium, but also promoted the dissolution of silicon, resulting in poor selective solubility of silicon germanium relative to silicon.
[0059] The etching composition obtained in Comparative Example 3, which used hydrogen peroxide as component (A), inhibited the dissolution of silicon to some extent and promoted the dissolution of silicon germanium to some extent, but was inferior in the selective solubility of silicon germanium relative to silicon. [Industrial Applicability]
[0060] The etching composition of the present invention and the etching method of the present invention using this etching composition suppress dissolution of silicon, promote dissolution of silicon germanium, and have excellent selective solubility of silicon germanium relative to silicon, and therefore can be suitably used in the manufacture of semiconductor devices, and in particular, can be suitably used in the manufacture of GAA type FETs.
Claims
1. An etching composition that selectively dissolves silicon germanium relative to silicon, comprising an oxidizing agent (A) and an organic acid (B), wherein the oxidizing agent (A) contains nitric acid, and the content of the organic acid (B) is 50 mass% or more in 100 mass% of the etching composition.
2. 2. The etching composition according to claim 1, wherein the organic acid (B) comprises at least one compound selected from the group consisting of acetic acid, propionic acid, oxalic acid and citric acid.
3. The etching composition according to claim 1 or 2, further comprising a fluorine-containing compound (C).
4. 4. The etching composition according to claim 3, wherein the fluorine-containing compound (C) comprises at least one compound selected from the group consisting of hydrofluoric acid, ammonium fluoride, and hexafluorosilicic acid.
5. The etching composition according to claim 3 or 4, wherein the content of the fluorine-containing compound (C) is 5 mass% or less in 100 mass% of the etching composition.
6. The etching composition according to any one of claims 1 to 5, further comprising water (D).
7. The etching composition according to claim 6, wherein the content of water (D) is 20 mass% or less in 100 mass% of the etching composition.
8. An etching method for etching a structure containing silicon and silicon germanium using the etching composition according to any one of claims 1 to 7.
9. A method for manufacturing a semiconductor device, comprising a step of etching a structure containing silicon and silicon germanium with the etching composition according to any one of claims 1 to 7.
10. A method for manufacturing a gate-all-around transistor, comprising the step of etching a structure containing silicon and silicon germanium with the etching composition according to any one of claims 1 to 7.
Citation Information
Patent Citations
Method for selectively patterning silicon germanium layer by ion implantation
JP2005033202A
Etchant for selective removal of silicon-germanium alloy from silicon-germanium / silicon stack during semiconductor device fabrication
JP2019050365A
Formulations for selectively etching silicon germanium relative to silicon
JP2020517108A
Etching composition
JP2022512116A
Method for semiconductor selective etching and BSI image sensor