Ceiling material and manufacturing method of the ceiling material
The ceiling material with a base material layer, base coating, and inkjet printed pattern layer addresses the inefficiencies of conventional designs by enabling easy and durable decorative integration, reducing construction costs and improving adhesion and durability.
Patent Information
- Application Number
- JP2023070604
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
Conventional ceiling materials lack design flexibility and require skilled labor for decoration, leading to high construction costs and inefficiencies.
A ceiling material comprising a base material layer made of gypsum, calcium silicate, or rock wool, with a base coating layer containing a binder resin and white pigment, and a pattern layer formed through inkjet printing, allowing for easy design integration and improved adhesion and durability.
The solution enables high-quality, durable designs on ceilings with reduced construction effort and cost, while maintaining nonflammability and resistance to impact, with the inkjet printing layer providing long-lasting design quality and reduced ink bleeding.
Smart Images

Figure 2024156275000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to ceiling materials and methods for manufacturing ceiling materials. [Background technology]
[0002] Conventionally, gypsum boards, calcium silicate boards, rock wool boards, glass wool boards, etc. have been used as ceiling materials for buildings and other structures. Ceilings made from these ceiling materials have poor design, and most of them have only a moth-eaten pattern of depressions (for example, Patent Document 1 below). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-154514 A Summary of the Invention [Problem to be solved by the invention]
[0004] When adding design to a ceiling, there has been a method of attaching commercially available tack sheets, decorative paper for surface decoration, or wallpaper to the ceiling material. However, such methods are difficult to apply to the ceiling surface, making it difficult to secure skilled workers and to make the application efficient, and therefore have not been widely adopted, resulting in high application costs.
[0005] The present disclosure has been made in consideration of the above circumstances, and aims to provide a ceiling material that makes it possible to easily improve the design of a ceiling, and a manufacturing method thereof. [Means for solving the problem]
[0006] The present disclosure relates to the following ceiling material and method for manufacturing the ceiling material.
[0007] [1] A ceiling material comprising a base layer, a base coat layer provided on the base layer, and a pattern layer provided on the base coat layer, the base layer comprising at least one inorganic material selected from the group consisting of gypsum, calcium silicate, and rock wool, the base coat layer containing a binder resin and a white pigment, and the pattern layer being an inkjet printed layer. [2] In a heat release test based on the ISO 5660 cone calorimeter method, the total heat release rate after 20 minutes from the start of heating is 8 MJ / m 2 A ceiling material as described in [1] above, which is as follows: [3] The ceiling material according to [1] or [2] above, wherein the binder resin contains at least one resin selected from the group consisting of acid-modified olefin resins, acrylic resins, and vinyl acetate resins, and the white pigment contains at least one of calcium carbonate and titanium oxide. [4] The ceiling material according to any one of [1] to [3] above, wherein the content of the binder resin in the undercoat layer is 5 to 50 parts by mass per 100 parts by mass of the total content of the binder resin and the white pigment. [5] The ceiling material according to any one of the above [1] to [4], further comprising a protective layer on the pattern layer. [6] The ceiling material according to the above [5], wherein the protective layer contains at least one additive selected from the group consisting of ultraviolet absorbers and light stabilizers. [7] A method for producing a ceiling material according to any one of the above items [1] to [6], comprising the steps of: preparing a laminate having a base layer containing at least one inorganic material selected from the group consisting of gypsum, calcium silicate, and rock wool; and a base coat layer containing a binder resin and a white pigment and provided on the base layer; and forming a pattern layer on the base coat layer of the laminate by an inkjet printing method. [8] The method for producing a ceiling material according to the above [7], wherein in the printing step, a solventless ultraviolet-curable ink is used as the inkjet printing ink. [9] The method for manufacturing a ceiling material described in [8] above, wherein in the printing process, the pattern layer is formed by multi-pass printing of four or more passes.
[0008] The ceiling material according to the above [1] has a pre-applied pattern layer, so that the ceiling material can be given a design at the same time as it is installed. In addition, the ceiling material according to the above [1] has a base layer containing a general-purpose material, but the pattern layer is an inkjet printed layer that is applied via the above-mentioned undercoat layer, so that a high-quality pattern can be formed regardless of the uneven shape of the base layer surface. Therefore, the ceiling material according to the above [1] can easily improve the design of the ceiling.
[0009] The ceiling material according to [2] above can provide the ceiling with non-combustibility. The ceiling material according to [3] above can have an inkjet printing layer with high ink adhesion and suppressed ink bleeding, and can provide the ceiling with high designability for a long period of time. The ceiling material according to [4] above can provide the undercoat layer with a good balance of adhesion, white concealment, and non-combustibility. The ceiling materials according to [5] and [6] above can further improve the durability of the pattern layer. The provision of the protective layer can reduce the pattern fading due to impact, etc., when handled at the construction site, and can not only improve the design but also reduce the labor required for repair work.
[0010] According to the method for manufacturing a ceiling material according to [7] above, the ceiling material according to any one of [1] to [6] above can be efficiently manufactured. According to the method for manufacturing a ceiling material according to [8] above, the ink can be cured during printing, which highly suppresses the seepage and bleeding of the ink after printing, thereby obtaining a ceiling material having a higher quality pattern layer. According to the method for manufacturing a ceiling material according to [9] above, it becomes easy to increase the amount of ink in the pattern layer while sufficiently curing the ultraviolet-curable ink, making it possible to improve the quality of the pattern by high-density printing. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide a ceiling material that makes it possible to easily improve the design of a ceiling, and a manufacturing method thereof. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a ceiling material according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, embodiments of the present disclosure will be described in detail.
[0014] <Ceiling material> The ceiling material of the present embodiment comprises a base layer, a base coating layer provided on the base layer, and a pattern layer provided on the base coating layer.
[0015] Fig. 1 is a schematic cross-sectional view showing one embodiment of the ceiling material of the present disclosure. The ceiling material 1 shown in Fig. 1 includes a base layer 10, a base coating layer 20 provided on the surface of the base layer 10, a pattern layer 30 provided on the base coating layer 20, and a protective layer 40 provided on the pattern layer 30. The pattern layer 30 is an inkjet printing layer. The protective layer 40 may not be provided, or may have a laminated structure of two or more layers.
[0016] (base material layer) The substrate layer may be made of at least one inorganic material selected from the group consisting of gypsum, calcium silicate, and rock wool. The substrate layer may be a gypsum board, a calcium silicate board, or a rock wool board. These may be made from raw materials or may be commercially available products.
[0017] The gypsum board may contain, for example, calcium sulfate, starch, and various additives. Such a gypsum board can be obtained by mixing the above components and then solidifying and molding them. The additives include a dispersant, a foaming agent, a water repellent, and a mineral aggregate.
[0018] From the viewpoints of flame retardancy and strength, the content of calcium sulfate in the gypsum board may be 90 to 98 parts by mass with respect to 100 parts by mass of the total mass of the gypsum board.
[0019] From the viewpoints of flame retardancy and binding property, the content of starch may be 0.1 to 2.0 parts by mass with respect to 100 parts by mass of the total mass of calcium sulfate.
[0020] The gypsum board may be an ordinary gypsum board (GB-R) specified in JIS A 6901, a decorative gypsum board (GB-D) specified in JIS A 6911, a waterproof gypsum board (GB-S) specified in JIS A 6912, a reinforced gypsum board (GB-F) specified in JIS A 6913, a sound-absorbing gypsum board (GB-P) specified in JIS A 6301, or the like.
[0021] The calcium silicate board may be a calcium silicate board, which is a type of fiber reinforced cement board specified in JIS A 5430.
[0022] The rock wool board may be a building insulation material specified in JIS A 9521.
[0023] The thickness of the base material layer may be 4 to 10 mm, or 4 to 8 mm, from the viewpoint of maintaining the shape and suppressing the amount of heat generated in a heat generation test. The standard mass of the base material layer is 4 to 6 kg / m 2 and 4.5 to 5.5 kg / m 2 may be also possible.
[0024] (Base coat layer) The undercoat layer may contain a binder resin and a white pigment.
[0025] Examples of the binder resin include an acid-modified olefin resin, an acrylic resin, and a vinyl acetate resin. The binder resin may be used alone or in combination of two or more kinds.
[0026] As the acid-modified olefin resin, commercially available products such as "CHEMIPEARL" and "UNISTOR" (both trade names manufactured by Mitsui Chemicals, Inc.) can be used.
[0027] Examples of the acrylic resin include those obtained by polymerizing one or more acrylic monomers, and those obtained by copolymerizing one or more acrylic monomers with one or more other comonomers.
[0028] Examples of acrylic monomers include: Alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, methylcyclohexyl (meth)acrylate, bornyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, and octadecyl (meth)acrylate; hydroxyl group-containing alkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate; (Meth)acrylic acid hydroxyalkyl esters such as 8-hydroxyoctyl (meth)acrylate; glycol mono(meth)acrylates such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and 1,4-cyclohexanedimethanol mono(meth)acrylate; Carboxyl group-containing acrylic monomers such as (meth)acrylic acid, monohydroxyethyl phthalate acrylate, p-carboxybenzyl acrylate, ethylene oxide-modified (number of moles added: 2 to 18) acrylate phthalate, monohydroxypropyl phthalate, monohydroxyethyl acrylate succinate, β-carboxyethyl acrylate, and 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate; Amide bond group-containing acrylic monomers such as N-isopropyl(meth)acrylamide, N,N-diethylacrylamide, and hydroxyethylacrylamide; Amino group-containing acrylic monomers such as monomethylaminoethyl (meth)acrylate, monoethylaminoethyl (meth)acrylate, monomethylaminopropyl (meth)acrylate, and monoethylaminopropyl (meth)acrylate; and 2-methoxyethyl acrylate, 2-ethoxyethyl acrylate, 2-phenoxyethyl acrylate, methoxypolyethylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, ethoxypolypropylene glycol (meth)acrylate, caprolactone-modified (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, phenoxypolypropylene glycol (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxymethyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, glycidyl (meth)acrylate, α-methylglycidyl acrylate, α-methylglycidyl methacrylate, 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, and the like.
[0029] Examples of vinyl acetate resins include polyvinyl acetate, ethylene-vinyl acetate copolymer, vinyl chloride-vinyl acetate copolymer, etc. From the viewpoint of suppressing bleeding of the pattern in the inkjet printing layer and improving ink adhesion, the undercoat layer may contain a vinyl acetate resin as a binder resin.
[0030] Examples of the white pigment include calcium carbonate and titanium oxide. The white pigment may be used alone or in combination of two or more.
[0031] The total content of the binder resin and the white pigment in the base coating layer may be 97% by mass or more, or 99% by mass or more, based on the total mass of the base coating layer.
[0032] The content of the binder resin in the undercoat layer may be 5 to 50 parts by mass, 10 to 40 parts by mass, or 20 to 30 parts by mass, based on 100 parts by mass of the total of the binder resin and the white pigment, from the viewpoints of adhesion, white hiding power, and non-combustibility. Also, the content of the binder resin in the undercoat layer may be 30 to 55 parts by mass, or 45 to 55 parts by mass, based on 100 parts by mass of the total of the binder resin and the white pigment, from the viewpoints of weather resistance, white hiding power, and non-combustibility.
[0033] The undercoat layer may contain additives such as dispersants (surfactants), ultraviolet absorbers, radical scavengers, antioxidants, wetting agents, fluorescent whitening agents, thickeners, viscosity reducers, hydrolysis inhibitors, and heat stabilizers.
[0034] The thickness of the base coating layer may be 20 μm or more, or 30 μm or more, from the standpoint of design (concealment), and may be 200 μm or less, or 150 μm or less, from the standpoint of making it easier to obtain fireproof certification as incombustible.
[0035] (Picture layer) The design layer is an inkjet printing layer formed by inkjet printing, and contains an ink for inkjet printing or a cured product thereof.
[0036] As the ink for inkjet printing, ultraviolet curable ink, electron beam curable ink, one-component curable ink, etc. can be used. Furthermore, the ink for inkjet printing may be water-based, solvent-based, or solventless. Incidentally, solventless means that no solvent (organic solvent, water, etc.) is used as a solvent for dispersing pigments, etc. Furthermore, the ink for inkjet printing may be acrylic or ester-based. From the viewpoint of suppressing the penetration and bleeding of the ink and forming a higher quality picture layer, ultraviolet curable ink may be used, or a solventless ultraviolet curable ink may be used.
[0037] Inkjet printing can be carried out under the printing conditions described below.
[0038] (protective layer) Examples of the main component constituting the protective layer include resin materials such as acrylic, polyurethane, acrylic silicone, fluorine, epoxy, vinyl, polyester, melamine, aminoalkyd, urea, etc. The content of the resin material in the protective layer may be 80% by mass or more, 90% by mass or more, or 99% by mass or more based on the total mass of the protective layer.
[0039] In order to improve the surface hardness, a resin that is cured by active energy rays such as ultraviolet rays and electron beams may be used. Examples of such resins include acrylic resins and epoxy resins.
[0040] The protective layer may contain at least one additive selected from the group consisting of ultraviolet absorbers and light stabilizers. In this case, the weather resistance of the ceiling material can be improved, and the ink adhesion of the inkjet printing layer can be easily maintained for a longer period of time. The protective layer containing the ultraviolet absorber has increased resistance to ultraviolet rays (e.g., reflected light from a wall or floor surface), and can improve the durability of the pattern layer. The protective layer containing the light stabilizer can have excellent durability (especially weather resistance). From these viewpoints, the protective layer may contain an ultraviolet absorber and a light stabilizer. As additives other than those mentioned above, matting agents, antioxidants, fluorescent whitening agents, slip agents, etc. may be used.
[0041] Examples of ultraviolet absorbing agents include benzotriazole-based, benzoate-based, benzophenone-based, and triazine-based compounds. From the viewpoint of the balance between cost and performance, a benzotriazole-based compound may be blended as an ultraviolet absorbing agent. Examples of such compounds include Benzenepropanoic acid, 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-, C7-9-branched and linear alkyl esters, etc.
[0042] Examples of the light stabilizer include hindered amine and phenol compounds. From the viewpoint of effect persistence, a hindered amine compound may be blended as the light stabilizer. The hindered amine compound can capture radicals, which makes it easy to improve the durability (particularly weather resistance) of the protective layer.
[0043] The content of the additive in the protective layer may be 0.1 to 10 parts by mass, or may be 0.5 to 7 parts by mass, relative to 100 parts by mass of the resin material.
[0044] The thickness of the protective layer may be 3 μm or more, or 6 μm or more, from the viewpoint of providing weather resistance, and may be 20 μm or less, or 10 μm or less, from the viewpoint of suppressing the amount of heat generated by combustion and making it easier to obtain fire protection certification.
[0045] The ceiling material of this embodiment may satisfy the following condition 1, or may satisfy the following conditions 1 and 2, or may satisfy all of the following conditions 1 to 3, in a heat generation test based on the cone calorimeter method of ISO 5660. Condition 1: The total heat generated over the first 20 minutes after heating is 8 MJ / m 2 The following is the result. Condition 2: 20 minutes after the start of heating, no cracks or holes with a maximum diameter exceeding 0.5 mm that penetrate to the back surface are observed. Condition 3: For 20 minutes after the start of heating, the heat generation rate is 200 kW / m for 10 seconds or more. 2 not exceed.
[0046] In the ceiling material of this embodiment, the configurations of the base layer, undercoat layer, pattern layer, and, if necessary, protective layer may be adjusted so as to satisfy the above condition 1. For example, the total heat generation can be adjusted to be smaller by reducing the content of organic material in the base layer and undercoat layer, and by reducing the thickness of the pattern layer and protective layer.
[0047] <Manufacturing method for ceiling materials> The method for producing the ceiling material of this embodiment is a method for producing the ceiling material of this embodiment described above, and includes a printing step of preparing a laminate having a base layer containing at least one inorganic material selected from the group consisting of gypsum, calcium silicate, and rock wool, and a base coat layer containing a binder resin and a white pigment provided on the base layer, and forming a pattern layer on the base coat layer of the laminate by an inkjet printing method. If the ceiling material of this embodiment has a protective layer, a protective layer forming step of forming a protective layer on the pattern layer can be further provided after the printing step.
[0048] (Preparation of laminate) The laminate can be obtained by preparing a coating liquid containing the above-mentioned binder resin and white pigment, and optionally additives, applying the coating liquid onto a substrate layer using a roll coater, flow coater, die coater, or other means, and drying to form a base coating layer. The coating liquid may contain a solvent. In this case, water or the like can be used as the solvent.
[0049] Drying conditions include a temperature of 40 to 100° C. and a time of 0.5 to 2 minutes.
[0050] (Printing process) Inkjet printing can be performed using the inkjet printing ink described above. Inkjet printing may be performed by multi-pass printing using a scanning or area type printer equipped with an ultraviolet irradiation device or the like. Note that multi-pass printing means that print data is divided into multiple pieces for a predetermined printing surface and printed in multiple passes. The number of passes in multi-pass printing may be 2 or more, 3 or more, or 4 or more.
[0051] The ultraviolet ray irradiation device may be attached to the side of the carriage on which the inkjet heads are arranged. In this case, ultraviolet ray irradiation can be performed almost simultaneously with the landing of the ejected ink on the substrate.
[0052] In this embodiment, by combining an inkjet printer equipped with an ultraviolet irradiation device, ultraviolet curable ink, and multi-pass printing, it is possible to improve the quality of the pattern by high density printing. In the case of single pass printing, if the ink ejection volume increases too much, the ink cannot be cured sufficiently with the amount of ultraviolet radiation irradiated once, making it difficult to print a high density pattern that requires a large amount of ink. In contrast, by using multi-pass printing, it is possible to increase the upper limit of the ink volume while sufficiently curing the ink. As a result, it is possible to improve the quality of the pattern by high density printing (for example, to expand the range of design expression).
[0053] (Protective layer formation process) The protective layer can be formed by preparing a coating liquid containing the components constituting the protective layer described above, applying the coating liquid onto the design layer using a means such as a flow coater, a roll coater, or a die coater, and drying the coating liquid. The coating liquid may contain the above-mentioned solvent.
[0054] Drying conditions include a temperature of 40 to 100° C. for 0.5 to 2 minutes. When a resin that is cured by active energy rays such as ultraviolet rays or electron beams is blended, irradiation with active energy rays may be performed. EXAMPLES
[0055] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these examples.
[0056] <Ceiling material production> Example 1 A coating liquid consisting of 8 parts by mass of "Unistol R-303Xe" (manufactured by Mitsui Chemicals, Inc., product name, acid-modified olefin resin) as a binder resin, 92 parts by mass of "Softon 400" (manufactured by Bihoku Funka Kogyo, product name, calcium carbonate, average particle size 13 μm) as a white pigment, and 2,000 parts by mass of xylene was applied to the surface of a 9.5 mm thick rock wool board using a roll coater, and the board was allowed to dry naturally to form a 50 μm thick undercoat coating layer.
[0057] Next, on the formed undercoat layer, a 4-pass multi-pass printing was performed using "LIOJET" (product name, water-based, manufactured by Toyo Ink Co., Ltd.) as the ink by an inkjet printing method using an inkjet printer PerformanceJet PJ-2508UF (product name, manufactured by Muto Industrial Co., Ltd.), and the resulting ink was naturally dried to form a pattern layer. The pattern had a colorless transparent portion for evaluating the hiding power, a pattern portion for evaluating the bleeding and density of the pattern, and a solid printed portion for evaluating the ink adhesion. In this way, a ceiling material was produced in which the undercoat layer and the pattern layer were laminated in this order on the base layer.
[0058] Example 2 A ceiling material was prepared in the same manner as in Example 1, except that a coating liquid was used to form the base coating layer, which consisted of 8 parts by weight of "7820" (product name, acrylic resin, manufactured by Japan Coating Resins Co., Ltd.) as a binder resin, 92 parts by weight of "Softon 400" (product name, calcium carbonate, average particle size 13 μm, manufactured by Bihoku Funka Kogyo Co., Ltd.) as a white pigment, and 400 parts by weight of dilution water.
[0059] Example 3 A ceiling material was prepared in the same manner as in Example 1, except that a coating liquid was used to form the undercoat layer, which consisted of 8 parts by weight of "Viniblan 1157" (manufactured by Nissin Chemical Industry Co., Ltd., product name: polyvinyl acetate) as the binder resin, 92 parts by weight of "Softon 400" (manufactured by Bihoku Funka Kogyo Co., Ltd., product name: calcium carbonate, average particle size: 13 μm) as the white pigment, and 400 parts by weight of dilution water.
[0060] (Examples 4 to 6) The ceiling materials were prepared in the same manner as in Example 3, except that the binder resin and white pigment contents were changed to 20 parts by weight and 80 parts by weight, 40 parts by weight and 60 parts by weight, or 50 parts by weight and 50 parts by weight, respectively.
[0061] Example 7 A ceiling material was produced in the same manner as in Example 4, except that in forming the design layer, one pass of printing was performed using "PJUV110 (cyan, magenta, yellow, black, white)" (product name, solvent-free UV-curable ink, manufactured by Muto Industries Ltd.). The ink was cured immediately after printing by irradiating it with UV light under standard conditions of the inkjet printer.
[0062] (Examples 8 to 9) Each ceiling material was produced in the same manner as in Example 7, except that a 2-pass or 4-pass multi-pass printing was used to form the design layer. The ink was cured after each pass by irradiating it with ultraviolet light under standard conditions of the inkjet printer.
[0063] Example 10 The pattern layer was formed in the same manner as in Example 9, and then "Viewtop Silicon Clear" (product name, manufactured by Kikusui Chemical Industry Co., Ltd.) was applied onto the pattern layer using a flow coater. A 10 μm thick protective layer was then further formed by hot air drying at 60°C to produce a ceiling material.
[0064] Example 11 The pattern layer was formed in the same manner as in Example 9, and a coating liquid consisting of 100 parts by mass of "Viewtop Silicon Clear" (product name, manufactured by Kikusui Chemical Industry Co., Ltd.) and 5 parts by mass of "Tinuvin 9945-DW(N)" (product name, benzotriazole-based, manufactured by BASF Japan Ltd.) as an ultraviolet absorber was applied on the pattern layer using a flow coater, and a protective layer having a thickness of 10 μm was further formed by hot air drying at 60°C to produce a ceiling material.
[0065] Example 12 The pattern layer was formed in the same manner as in Example 9, and a coating liquid consisting of 100 parts by weight of "Viewtop Silicon Clear" (manufactured by Kikusui Chemical Industry Co., Ltd., product name), 5 parts by weight of "Tinuvin 9945-DW(N)" (manufactured by BASF Japan Ltd., product name, benzotriazole type) as an ultraviolet absorber, and 3 parts by weight of "Tinuvin 123-DW(N)" (manufactured by BASF Japan Ltd., product name, hindered amine type) as a light stabilizer was applied on the pattern layer using a flow coater, and a protective layer of 10 μm in thickness was further formed by hot air drying at 60°C to produce a ceiling material.
[0066] <Evaluation of ceiling materials> The ceiling materials produced in the examples and comparative examples were evaluated as follows.
[0067] [Pyrogenicity test] The heat generation test was conducted in accordance with the cone calorimeter method of ISO 5660-1:2002. In the heat generation test, a cone calorimeter tester manufactured by Toyo Seiki Seisakusho Co., Ltd. was used to heat the test specimens (3 pieces) with dimensions of 99 mm × 99 mm × 9.5 mm with a radiant electric heater at 50 kW / m 2The total heat generation amount for 20 minutes after the start of heating was measured, and the shape stability and heat generation rate were evaluated according to the following criteria. (Shape stability: Judgment criteria) A: 20 minutes after the start of heating, there are no cracks or holes with a maximum diameter exceeding 0.5 mm that penetrate to the back surface. B: 20 minutes after the start of heating, cracks or holes with a maximum diameter of more than 0.5 mm that penetrate to the back surface are observed. (Heat release rate: criteria) A: 20 minutes after the start of heating, the heat generation rate is 200 kW / m for 10 seconds or more. 2 not exceed. B: 20 minutes after the start of heating, the heat generation rate is 200 kW / m for 10 seconds or more. 2 Exceeds.
[0068] [Evaluation of the pattern layer] The pattern layer on which the test chart was printed was visually observed, and the bleeding and density of the pattern were evaluated according to the following criteria: The test chart used was No. 11 of the Color Facsimile Test Chart of the Institute of Image Electronics Engineers of Japan. Pattern bleeding) (Pattern bleeding: Evaluation criteria) A: No bleeding is observed. B: Slight bleeding is observed. C: A little bleeding is observed. D: Considerable bleeding is observed. (Pattern Density: Evaluation Criteria) The relative evaluation was made on a 5-point scale, with Example 9 having the highest concentration being given a score of 5 and Example 1 having the lowest concentration being given a score of 1.
[0069] [Evaluation of the base coat layer] The colorless and transparent portion of the design layer was visually observed, and the hiding power of the undercoat layer was evaluated according to the following criteria. (Concealment: Evaluation Criteria) A: The base layer is not visible. B: The base layer is slightly visible. C: The base layer is slightly visible.
[0070] [Ink adhesion after weathering test] The ceiling material was placed in a Sunshine Weather weathering tester (black panel 63°C, 18 minutes of water spraying out of 120 minutes) and removed after a set time (200 hours, 500 hours, 1000 hours). The ceiling material before and after the test were evaluated for ink adhesion according to the following cross-cut test method. (Cross-cut test method) 1. Using a cutter knife and cutter guide, make 6 cuts (2mm apart) reaching the base material layer on the surface of the ceiling material where the pattern layer is located, creating 25 grids. 2. Firmly press Scotch tape (registered trademark) onto the grid area and quickly peel off the end of the tape at a 45° angle. 3. Count the number of grids from which the pattern layer has peeled off.
[0071] [Table 1]
[0072] [Table 2] [Explanation of symbols]
[0073] 1...ceiling material, 10...base material layer, 20...primer coating layer, 30...pattern layer, 40...protective layer.
Claims
1. The present invention comprises a base layer, a base coating layer provided on the base layer, and a pattern layer provided on the base coating layer, The substrate layer comprises at least one inorganic material selected from the group consisting of gypsum, calcium silicate, and rock wool, The undercoat layer contains a binder resin and a white pigment, A ceiling material, wherein the pattern layer is an inkjet printed layer.
2. In a heat generation test based on the ISO 5660 cone calorimeter method, the total heat generation amount for 20 minutes after the start of heating was 8 MJ / m 2 2. The ceiling material according to claim 1, wherein:
3. the binder resin comprises at least one resin selected from the group consisting of an acid-modified olefin resin, an acrylic resin, and a vinyl acetate resin; The ceiling material according to claim 1 , wherein the white pigment comprises at least one of calcium carbonate and titanium oxide.
4. The ceiling material according to claim 1, wherein the content of the binder resin in the undercoat layer is 5 to 50 parts by mass per 100 parts by mass of the total content of the binder resin and the white pigment.
5. The ceiling material according to claim 1 , further comprising a protective layer on the pattern layer.
6. The ceiling material according to claim 5, wherein the protective layer comprises at least one additive selected from the group consisting of an ultraviolet absorber and a light stabilizer.
7. A method for producing a ceiling material according to any one of claims 1 to 6, comprising the steps of: A method for manufacturing a ceiling material, comprising: preparing a laminate having a base layer containing at least one inorganic material selected from the group consisting of gypsum, calcium silicate, and rock wool, and a base coat layer containing a binder resin and a white pigment provided on the base layer; and a printing step of forming a pattern layer on the base coat layer of the laminate by an inkjet printing method.
8. The method for manufacturing a ceiling material according to claim 7, wherein in the printing step, a solventless ultraviolet-curable ink is used as the inkjet printing ink.
9. The method for manufacturing a ceiling material according to claim 8 , wherein in the printing step, the pattern layer is formed by multi-pass printing of four or more passes.