Ultrahigh-strength concrete

The formulation of ultra-high strength concrete with specific components and properties improves pumpability, enabling use of standard equipment and maintaining high compressive strength.

JP2024156516APending Publication Date: 2024-11-06TAISEI CORP
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
JP2023071042
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

Ultra-high strength concrete, such as UFC, has high viscosity, making it difficult to pump using standard equipment, necessitating high-pressure systems or special pumps.

Method used

Formulation of ultra-high strength concrete with specific components and properties, including compressive strength, slump flow value, and steel fiber content, to enhance pumpability.

Benefits of technology

The concrete achieves excellent pumpability, allowing use of general pump trucks and piping without special equipment, while maintaining high compressive strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156516000001_ABST
    Figure 2024156516000001_ABST
Patent Text Reader

Abstract

To provide an ultrahigh-strength concrete having excellent pumpability.SOLUTION: An ultrahigh-strength concrete according to the present invention has a compression strength of 100 N / mm2 or over and includes normal Portland cements, silica fume, water, water-reducing agents, fine aggregates, coarse aggregates, and steel fibers, wherein the maximum size of the coarse aggregates is 20 mm or under, a content of the steel fibers is 0.5-1.5%, a slump flow value according to the JIS A1150 slump flow test method is 550-750 mm, and a 500-mm flow arrival time is 20.0 s or under.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to ultra-high strength concrete. [Background technology]

[0002] Compressive strength is 100N / mm 2 An example of the above ultra-high strength concrete is ultra-high strength fiber reinforced concrete (UFC) which contains steel fibers. Although UFC has excellent material properties such as compressive strength, tensile strength, and durability, its extremely high viscosity means that it is difficult to say that it is a material suitable for pumping. For this reason, various studies have been conducted on the pumpability of ultra-high strength concrete such as UFC. For example, Non-Patent Document 1 confirms that it is possible to pump even ultra-high strength concrete by using a pump with a high maximum discharge pressure and high-pressure piping. In addition, in Non-Patent Document 2, a pumping test was carried out using UFC, and the presence or absence of defects during pumping and changes in fresh properties before and after pumping were investigated. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Masanori Kono "Pumping of 150N / mm2 class ultra-high strength concrete" Construction planning '10.5 Estimation of bridge construction work (2010 edition) Japan Construction Mechanization Association [Non-Patent Document 2] Yoshikazu Ishiseki et al. "Pumping Test and Field Construction of Room Temperature Curing UFC" Abstracts of Lectures at the 66th Annual Academic Conference of the Japan Society of Civil Engineers (2011) Summary of the Invention [Problem to be solved by the invention]

[0004] Figure 2 in Non-Patent Document 1 shows the relationship between the pipe pressure and the pumping distance when pumping ultra-high strength concrete, and from this figure it can be seen that the pipe pressure is 10 MPa or more or 8 MPa or more when pumping of ultra-high strength concrete starts. Also, Figure 1 in Non-Patent Document 2 shows the relationship between the discharge rate and the pipe pressure when pumping UFC, and from this figure it can be seen that if the discharge rate is reduced, the pipe pressure will be lower, but will still be 6 MPa or more. Considering that the pressure inside the pipes when pumping regular concrete is approximately 5 MPa or less, when using ultra-high strength concrete, it is necessary to use special pump trucks or high-pressure piping, or to use the concrete without pumping it. Therefore, the inventors considered that if the pumpability of ultra-high strength concrete could be improved, it would be possible to pump it using ordinary pump trucks and piping, and it would be possible to expand into a variety of applications without being restricted to extremely specific usage patterns (such as those requiring special pump trucks or high-pressure piping, or those for use in small-scale construction projects).

[0005] From this viewpoint, an object of the present invention is to provide an ultra-high strength concrete with excellent pumpability. [Means for solving the problem]

[0006] The ultra-high strength concrete according to the present invention for solving the above problems has a compressive strength of 100 N / mm 2 The above ultra-high strength concrete contains ordinary Portland cement, silica fume, water, a water reducing agent, fine aggregate, coarse aggregate, and steel fibers, the maximum dimension of the coarse aggregate is 20 mm or less, the steel fiber content is 0.5 to 1.5%, and the slump flow value in the JIS A 1150 slump flow test method is 550 to 750 mm, and the 500 mm flow time is 20.0 seconds or less. According to the present invention, the ultra-high strength concrete is made of a predetermined material, has a slump flow value within a predetermined range, and has a 500 mm flow time of less than a predetermined value. Therefore, the compressive strength is 100 N / mm2 Despite the above, it has excellent pumpability. In addition, the ultra-high strength concrete according to the present invention preferably has a water-binder ratio of 18.0 to 20.0%. In addition, the ultra-high strength concrete according to the present invention has an absolute volume of the coarse aggregate of 0.245 m 3 / m 3 Preferably, the ultra-high strength concrete according to the present invention has a content of the water reducing agent of 0.50 to 2.00% when the mass of the binder is taken as 100%. Preferably, the ultra-high strength concrete according to the present invention has a steel fiber coarse aggregate volume ratio (= absolute volume of the steel fibers / absolute volume of the coarse aggregate x 100) of 5 to 10%. According to the present invention, it is possible to more reliably provide ultra-high strength concrete with excellent pumpability. Effect of the Invention

[0007] The ultra-high strength concrete according to the present invention can exhibit excellent pumpability. [Brief description of the drawings]

[0008] [Figure 1] 1 is a graph showing the relationship between the slump flow value and the 500 mm passing time for each sample used in the examples. [Diagram 2] This is an overall schematic diagram of the piping and pump vehicle used in the pumping test. [Diagram 3] 1 is a graph showing the relationship between pumping distance and internal pipe pressure obtained in a pump pumping test. [Figure 4] 1 is a graph showing the relationship between the pressure loss in the pipe and the discharge amount calculated from the test results of a pump pressure test. [Diagram 5] 1 is a graph showing the relationship between shear stress and plastic viscosity of certain sample mortars used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment for carrying out ultra-high strength concrete according to the present invention (ultra-high strength concrete according to this embodiment) will be described. [Ultra-high strength concrete] The ultra-high strength concrete according to this embodiment has a compressive strength equal to or greater than a predetermined value, and contains ordinary Portland cement, silica fume, water, a water reducing agent, fine aggregate, coarse aggregate, and steel fibers. The ultra-high strength concrete according to this embodiment also has a maximum dimension of the coarse aggregate equal to or less than a predetermined value, a steel fiber content within a predetermined range, a slump flow value within a predetermined range, and a 500 mm flow time equal to or less than a predetermined value. Each of the constituent elements will be described in detail below.

[0010] (Compressive strength) In this specification, "ultra-high strength concrete" refers to concrete with a compressive strength of 100 N / mm 2 The above concrete is used. The ultra-high strength concrete according to this embodiment has a compressive strength of 100 N / mm 2 Although more than this is acceptable, from the viewpoint of ensuring high compressive strength, 110N / mm 2 The above is preferred. The compressive strength is the value of the compressive strength at 28 days of age, and may be measured using the method described in "Testing method for compressive strength of concrete" in JISA1108:2018.

[0011] (ordinary Portland cement) Ordinary Portland cement is a common type of cement that conforms to the regulations set forth in JIS R 5210:2009. Although low-heat Portland cement or moderate-heat Portland cement is generally considered to be preferable as the cement used for ultra-high strength concrete (Non-Patent Document 1, paragraph 0011 of JP 2019-214504 A, etc.), the ultra-high strength concrete according to this embodiment uses ordinary Portland cement. By using ordinary Portland cement and satisfying the other constituent requirements described below, it is possible to achieve both high compressive strength and excellent pumpability. The content (mixture) of ordinary Portland cement in ultra-high strength concrete is, for example, 600 kg / m 3 More than 900kg / m 3 The following is the result.

[0012] (Silica fume) Silica fume is an ultrafine particle obtained by collecting dust in the exhaust gas generated during the production of metal silicon, ferrosilicon, etc., and is defined in JISA 6207:2016. The content (mixture amount) of silica fume in ultra-high strength concrete is, for example, 100 kg / m 3 More than 200kg / m 3 The following is the result. The quality of the silica fume, such as the particle size and specific surface area, is not particularly limited.

[0013] (Slag gypsum admixture) Slag-gypsum-based admixture is an admixture made by mixing ground granulated blast furnace slag and gypsum. Ground granulated blast furnace slag is defined in JISA6206:2013, and gypsum is defined in JISR9151:2009. The ultra-high strength concrete according to the present embodiment may contain a slag gypsum admixture, although this is not essential. As the slag gypsum admixture, for example, Cerapower CPSI (manufactured by DC Corporation) can be used.

[0014] (Water reducing agent) A water-reducing agent is a chemical admixture that reduces the amount of water required to obtain a desired slump, and is defined in JISA6204:2011. Examples of the water reducing agent include high performance water reducing agents, AE water reducing agents, and high performance AE water reducing agents, with the high performance water reducing agents being preferred. The mass ratio (B×%) of the water-reducing agent when the mass of the binder in the ultra-high strength concrete is taken as 100% is, for example, not less than 0.50% and not more than 2.00%.

[0015] (fine aggregate, coarse aggregate) Examples of fine aggregates include mountain sand, river sand, sea sand, crushed sand, silica sand, and lime sand, and examples of coarse aggregates include mountain gravel, river gravel, and sea gravel, all of which comply with JIS A 5005:2020. The content (mixture) of fine aggregate in ultra-high strength concrete is, for example, 500 kg / m 3 More than 800kg / m 3 The content (mixture) of coarse aggregate in ultra-high strength concrete is, for example, 400 kg / m 3 More than 700kg / m 3 The following is the result. The maximum dimension of the coarse aggregate is preferably 20 mm or less, and more preferably 15 mm or less. By restricting the maximum dimension of the coarse aggregate to a predetermined value or less, pumpability can be reliably improved.

[0016] The absolute volume (Vg) of coarse aggregate is, for example, 0.140 m 3 / m 3 Above 0.280m 3 / m 3 The following is the result. The fine aggregate ratio (s / a) is, for example, 40% or more and 65% or less. The fine aggregate powder ratio (S / B) is, for example, 45% or more and 65% or less.

[0017] (Steel Fiber) Steel fibers are fibers made of steel used to reinforce concrete. The shape of the steel fiber may be a hook type, a straight type, or a straight type, but the hook type is preferred from the viewpoint of anchoring power to concrete. The length of the steel fiber is, for example, 10 to 40 mm (preferably 30 to 40 mm). The diameter of the steel fiber is, for example, 0.1 to 0.8 mm (preferably 0.38 to 0.75 mm). The content (mixture amount) of steel fibers in ultra-high strength concrete is 0.5 vol.% or more and 1.5 vol.% or less from the viewpoint of ensuring high compressive strength while providing excellent pumpability. The steel fiber / coarse aggregate volume ratio in ultra-high strength concrete (= absolute volume of steel fibers / absolute volume of coarse aggregate × 100) is 5% or more and 10% or less, from the viewpoint of ensuring high compressive strength while also providing excellent pumpability. As the steel fibers, commercially available steel fibers for steel fiber reinforced concrete may be used, for example, Dramix (registered trademark) steel fiber manufactured by Bekaert Japan KK may be used.

[0018] (water) The ultra-high strength concrete according to the present embodiment contains water. The water content (mixture amount) is not particularly limited, but is, for example, 160 kg / m 3 Above 220kg / m 3 The following is the result. The water-binder ratio (W / B) is, for example, 17.0% or more from the viewpoint of ensuring excellent pumpability, and is 20.0% or less from the viewpoint of ensuring high compressive strength. The water is not particularly limited, and tap water, sludge water, etc. can be used.

[0019] (Slump flow test: slump flow value, time to reach 500mm flow) The ultra-high strength concrete according to this embodiment has a slump flow value of 550 to 750 mm and a 500 mm flow time of 20.0 seconds or less according to the slump flow test method of JIS A 1150: 2020. By having the slump flow value in a predetermined range and the 500 mm flow time of a predetermined value or less, it is possible to achieve both high compressive strength and excellent pumpability. The slump flow value is more preferably 600 mm or more, and more preferably 750 mm or less. The lower limit of the 500 mm flow reaching time is not particularly limited, but is, for example, 4.5 seconds or more.

[0020] (others) The ultra-high strength concrete according to this embodiment may contain, as appropriate, conventionally known materials (such as chemical admixtures, fibers, etc.) used in concrete, as long as the desired effects of the present invention are not impaired. Examples of chemical admixtures include, in addition to the water-reducing agents described above, separation reducing agents, air content regulators, antifoaming agents, shrinkage reducing agents, setting retarders, setting accelerators, air-entraining agents, air-entraining water-reducing agents, high-performance air-entraining water-reducing agents, etc. Any one of the chemical admixtures may be used alone, or two or more may be used in combination. Examples of the fibers include metal fibers, organic fibers, and composite fibers that are a mixture of organic fibers and metal fibers. Examples of the metal fibers include the above-mentioned steel fibers, as well as stainless steel fibers, titanium fibers, and aluminum fibers. Examples of the organic fibers include polypropylene fibers, polyvinyl alcohol fibers, aramid fibers, polyethylene fibers, ultra-high strength polyethylene fibers, polyethylene terephthalate fibers, rayon fibers, nylon fibers, polyvinyl chloride fibers, polyester fibers, acrylic fibers, and alkali-resistant glass fibers. EXAMPLES

[0021] [Sample preparation] The materials shown in Table 1 were used and mixed according to the ratio shown in Table 2 to prepare samples (concrete specimens). The symbols in Table 2 are as follows: Gmax: Maximum size of coarse aggregate (mm) W / B: Water binding material ratio (%) s / a: Fine aggregate ratio (%) S / B: Fine aggregate powder ratio (%) Vg: Unit coarse aggregate absolute volume (m 3 / m 3 ) Vf: Unit steel fiber absolute volume (m 3 / m 3 ) Vf / Fg: Steel fiber coarse aggregate volume ratio

[0022] [Table 1]

[0023] [Table 2]

[0024] [Measurement method] (Slump flow value and 500mm passing time) For each sample, the slump flow value and 500 mm passing time were measured according to JIS A 1150:2020 "Test method for slump flow of concrete". The 500 mm passing time was measured only for samples whose slump flow value was 500 mm or more. (Air volume) For each sample, the air content was measured according to JIS A 1128:2019 "Pressure test method for air content of fresh concrete - Air chamber pressure method". (temperature) The temperature of each sample was measured in accordance with JISA1156:2014 "Method of measuring temperature of fresh concrete." (Compressive strength) Specimens (cylinders with a diameter of 10 cm and a height of 20 cm) were taken from each sample. The specimens were left in a sealed state in a temperature- and humidity-controlled room at 20°C, and after one day, they were removed from the mold and standard curing (underwater curing at 20°C) was started. Then, a compressive strength test was carried out on the specimens at an age of 28 days, and the compressive strength was calculated. The compressive strength tests were conducted in accordance with JISA1108:2018 "Test method for compressive strength of concrete." The compressive strength was measured only for samples that had a slump flow value of 500 mm or more and a 500 mm passing time of 20.0 seconds or less.

[0025] [Table 3]

[0026] [Pump pressure test details] Figure 2 shows an overall schematic diagram of the piping and pump vehicle used in the pumping test. In the pumping test, each sample was pumped from pump vehicle C, and the pressure inside the pipes was measured when each sample flowed through the pipes using pressure measurement pipes P1 to P8 provided at predetermined locations in the pipes. The pumping test was carried out using samples 1, 2, 7, and 8, which are examples of the present invention. Samples 2 and 7 had a pump discharge of 15 m 3 / h, and samples 1 and 8 had a pump discharge of 30 m 3 The experiment was carried out at / h. The detailed configuration of the piping is shown in Table 4. The measurement results for each pressure measurement pipe are shown in Table 5.

[0027] [Table 4]

[0028] [Table 5]

[0029] [Pressure loss calculation] From the measurement results of each sample shown in Table 5, the pressure loss per unit distance in pipe 4B (horizontal pipe between P7 and P8) was calculated and designated as "4B pipe pressure loss." In detail, the calculation formula used was "(P8 pipe pressure - P7 pipe pressure) / distance between P8 and P7." In addition, from the measurement results of each sample shown in Table 5, the pressure loss in pipe 5B (the horizontal pipe between P3 and P4, and the horizontal pipe between P5 and P6) was calculated (using the same calculation formula as above), and the average value was taken as the "pipe 5B pressure loss."

[0030] [Table 6]

[0031] [Measurement of plastic viscosity and shear stress of mortar] The plastic viscosity and shear stress of the mortar that was the base for samples 2 and 8 were measured using a rheometer (a rotational rheometer manufactured by NETZSCH Japan). For comparison, similar measurements were also carried out on a typical UFC mortar with the composition shown below. Water: 216kg / m 3 Cement: 852kg / m 3 Admixture: 568kg / m 3 Silica sand: 650kg / m 3 High-performance water reducer: 20kg / m 3 Water powder ratio (W / P): 15.2%

[0032] [Consideration of the results] Fig. 1 is a graph showing the relationship between the slump flow value and the 500 mm passing time for each sample, where ◯ in Fig. 1 indicates the results for the samples of the embodiment, and × indicates the results for the samples of the comparative example. 1 and Table 3, it was confirmed that Samples 1 to 8, which are examples, meet both the slump flow value (550 to 750 mm) and the 500 mm flow time (20.0 seconds or less) specified in the present invention. Also, according to Table 3, Samples 1 to 8 have a compressive strength of 100 N / m 2 As a result, it was also confirmed that this corresponds to ultra-high strength concrete. On the other hand, it was confirmed that Samples 9 to 35, which are comparative examples, did not satisfy at least one of the requirements for the slump flow value and the requirements for the 500 mm flow arrival time specified in the present invention.

[0033] FIG. 3 is a graph showing the relationship between the pumping distance and the pressure inside the pipe obtained in the pumping test. According to FIG. 3 and Table 5, for the samples 1, 2, 7, and 8, which are examples, the maximum pressure inside the pipe is 3N / mm2 for a pumping distance of 80m. 2Therefore, it was found that Samples 1, 2, 7, and 8, which are examples, have excellent pumpability because they can be pumped with a general pump (pump vehicle) without using a special pump vehicle or high-pressure piping. Figure 4 is a graph showing the relationship between the pressure loss in the pipe and the discharge rate calculated from the results of the pumping test. Figure 4 also shows data on the pressure loss in 4B and 5B pipes for normal concrete (normal concrete) with a slump of 8 cm (SL8) as described in the Standard Specifications for Concrete [Standard Edition]. According to Figure 4 and Table 6, the discharge volume of pipe 5B is 15 m 3 The pressure loss in the pipes at 30 m3 / h was the same as that for ordinary concrete in all examples. 3 The pressure loss in the pipes per hour for the example with a W / B of 18% was about 1.6 times that of ordinary concrete, but for the example with a W / B of 19% it was about the same as that of ordinary concrete. In addition, the discharge volume of pipe 4B is 15 m 3 The pressure loss in the pipes was about 1.6 times that of normal concrete in the example with a W / B of 18%, and about the same as that of normal concrete in the example with a W / B of 20%. 3 The pipe pressure loss per hour was larger in both the 18% W / B and 19% W / B examples than in the normal concrete, with the 18% W / B example being about 1.9 times that of the normal concrete. From these results, it was confirmed that the pressure loss inside the pipes of the ultra-high strength concrete of the embodiment was approximately 1.0 to 1.6 times in the 5B pipe and approximately 1.0 to 1.9 times in the 4B pipe compared to the pressure loss inside the pipes of ordinary concrete, which is within the acceptable range for pressure loss inside the pipes during pumping.

[0034] Fig. 5 is a graph showing the relationship between the shear stress and the plastic viscosity of the mortars of Samples 2 and 8 used in the examples. In Fig. 5, ◯ indicates the results of the mortars of Samples 2 and 8, and × indicates the results of the UFC mortar. According to Fig. 5, it was confirmed that in the case of general UFC mortar, as the shear stress increases, the plastic viscosity also increases in proportion (thick arrow in Fig. 5). On the other hand, it was confirmed that in the case of the mortars of Samples 2 and 8, which are examples, as the shear stress increases, the plastic viscosity decreases (thin arrow in Fig. 5). From these results, it is speculated that one of the factors that allows the ultra-high-strength concrete of the present invention to have excellent pumpability while maintaining high compressive strength is that it has the above-mentioned special property in the mortar state (when the shear stress increases, the plastic viscosity decreases).

Claims

1. Compressive strength is 100N / mm 2 The above ultra-high strength concrete, Contains ordinary Portland cement, silica fume, water, a water reducing agent, fine aggregate, coarse aggregate, and steel fiber, The maximum dimension of the coarse aggregate is 20 mm or less, The steel fiber content is 0.5 to 1.5%, An ultra-high strength concrete having a slump flow value of 550 to 750 mm in the slump flow test method of JIS A 1150 and a 500 mm flow arrival time of 20.0 seconds or less.

2. The ultra-high strength concrete according to claim 1, characterized in that the water-binder ratio is 18.0 to 20.0%.

3. The absolute volume of the coarse aggregate is 0.245 m 3 / m 3 3. The ultra-high strength concrete according to claim 1, wherein the following is satisfied:

4. 3. The ultra-high strength concrete according to claim 1, wherein the content of the water reducing agent is 0.50 to 2.00% when the mass of the binder is 100%.

5. 3. The ultra-high strength concrete according to claim 1, characterized in that the steel fiber coarse aggregate volume ratio (= absolute volume of the steel fibers / absolute volume of the coarse aggregate x 100) is 5 to 10%.

Citation Information

Cited By

  • High-strength concrete

    JP2023180864A

  • High-Strength Concrete

    JP7799565B2