Substrate for magnetic disk, magnetic disk, and hard disk drive
A high-modulus, thin magnetic disk substrate with specific properties addresses the challenge of increased HDD storage capacity by minimizing vibrations and particle generation, ensuring disk integrity and reliability.
Patent Information
- Application Number
- JP2024141833
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-01-24
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2039-08-07
AI Technical Summary
The miniaturization of magnetic particles in magnetic disks is approaching its limit, and increasing the storage capacity of HDDs by adding more disks leads to issues with substrate rigidity, vibrations, and particle generation due to external shocks, especially in large substrates like 3.5-inch disks, which can damage the disks and reduce HDD reliability.
A magnetic disk substrate with a diameter of 85 mm or more and a thickness of 0.6 mm or less, made from materials with a Young's modulus of 90 GPa or more, featuring specific properties such as high glass transition temperature, low linear expansion coefficient, and chamfered edges to minimize vibrations and particle generation.
The solution effectively suppresses particle generation and vibration-induced contact, enhancing HDD reliability by reducing the likelihood of substrate contact with internal components and maintaining disk integrity under external impacts.
Smart Images

Figure 2024157052000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a magnetic disk substrate and a magnetic disk. [Background technology]
[0002] Glass substrates and aluminum alloy substrates have been used as substrates for magnetic disks. Magnetic films are formed on the main surfaces of these substrates to form magnetic disks. It is desirable for magnetic disks to have few surface defects, to have no hindrance to reading and writing information, and to be capable of reading and writing large amounts of information. In addition, in response to the demand for increased storage capacity in hard disk drive devices (hereinafter referred to as HDDs), efforts are being made to increase the density of magnetic recording.
[0003] For example, a method for manufacturing a glass substrate for a magnetic disk is known in which the surface roughness (arithmetic mean roughness Ra) of the glass substrate for a magnetic disk is reduced so that reading and writing can be performed without hindrance using a magnetic head (DFH head) equipped with a DFH (Dynamic Flying Height) mechanism when increasing the density of magnetic recording (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2014 / 051153 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, the hard disk drive industry has been reaching the limit of miniaturization of magnetic particles in magnetic disks, and the speed of improvement in recording density has been slowing down. On the other hand, the demand for increased storage capacity of HDDs is becoming increasingly intense for big data analysis and other purposes. As a result, there are considerations of increasing the number of magnetic disks installed in one HDD. To store such large amounts of data, HDDs with a nominal size of 3.5 inches are usually used. When trying to increase the storage capacity by increasing the number of magnetic disks incorporated in a HDD, it is necessary to reduce the thickness of the magnetic disk substrate, which accounts for most of the thickness of the magnetic disks in the limited space inside the HDD. Furthermore, in order to increase the storage capacity, it is also desirable to increase the size of the magnetic disks.
[0006] It has been found that increasing the diameter of the magnetic disk substrate and reducing its thickness reduces the rigidity of the substrate, making it more susceptible to large vibrations and making it difficult to contain those vibrations. For example, cloud data centers use a huge number of HDDs, and HDDs are frequently replaced due to failure. It has been found that the shock of installing a new HDD in the rack can cause the HDD to fail or shorten the time until failure. Further detailed investigation has revealed that when the HDD receives an external shock, it can be damaged even though the magnetic disk is not rotating because the HDD is not yet receiving power.
[0007] The vibration caused by the external impact decays over time, unlike the steady-state flutter vibration caused by the rotating magnetic disk and the air flow around it in the steady rotation state. However, if the amplitude of this vibration is large, it is likely to come into contact with the ramp in the HDD and also with the adjacent magnetic disks. Furthermore, the magnetic disk located at the top of the multiple magnetic disks arranged at a certain interval may come into contact with the ceiling surface of the magnetic disk storage container of the HDD. Such contact may cause the contacted part of the magnetic disk to chip, generating particles. Particles may also be generated by rubbing or scraping. The generated particles are scattered inside the storage container and often adhere to the read / write area (main surface) of the magnetic disk, which has a large area. In this way, by increasing the diameter of the magnetic disk substrate and decreasing the plate thickness, vibrations due to external shocks and the accompanying generation of particles, which did not previously pose a problem, can no longer be ignored. In particular, for large magnetic disk substrates with magnetic disks of nominal size 3.5 inches (e.g., diameter 95 mm) or more, the problem of particles generated by the above-mentioned contact due to substrate vibration cannot be ignored.
[0008] Therefore, an object of the present invention is to provide a magnetic disk substrate and a magnetic disk that can suppress the generation of particles caused by external impact even if the diameter of the magnetic disk substrate is increased and the plate thickness is reduced. [Means for solving the problem]
[0009] One aspect of the present invention is a substrate for a disk-shaped magnetic disk. The diameter D of the substrate is 85 mm or more, and the thickness T of the substrate is 0.6 mm or less; The substrate is made of a material having a Young's modulus E of 90 GPa or more.
[0010] The diameter D is preferably 90 mm or more. It is preferable that when an impact of 70 [G] is applied to the substrate in the normal direction to the main surface of the substrate with the inner peripheral edge of the substrate fixed for 2 [ms], the maximum amplitude due to vibration in the thickness direction of the outer peripheral edge of the substrate is 0.25 mm or less.
[0011] Another aspect of the present invention is a disk-shaped magnetic disk substrate. The diameter D of the substrate is 85 mm or more, and the thickness T of the substrate is 0.6 mm or less; When an impact of 70 [G] is applied to the substrate in the normal direction to the main surface of the substrate with the inner peripheral edge of the substrate fixed for 2 [ms], the maximum amplitude of vibration in the thickness direction of the outer peripheral edge of the substrate is 0.25 mm or less.
[0012] The diameter D is preferably 90 mm or more. The substrate is preferably a glass substrate made of glass having a glass transition point of 650° C. or higher.
[0013] It is preferable that the change in flatness of the substrate after heating at 730° C. and the flatness of the substrate before heating is 4 μm or less.
[0014] The substrate has a linear expansion coefficient of 70×10 -7 It is preferable that the material be made of a material having a thickness of 1 / K or less.
[0015] The Vickers hardness Hv of the substrate is 650 [kgf / mm 2 ] or more.
[0016] The Knoop hardness Hk of the substrate is 600 [kgf / mm 2 ] or more.
[0017] At least a surface of the outer peripheral end of the substrate is provided with a chamfered surface; It is preferable that a ratio W1 / R of a width W1 of the chamfered surface along the radial direction of the substrate to a radius R of the substrate is 0.0025 or less.
[0018] It is preferable that the ratio (2·W2) / T of twice the width W2 of the chamfered surface in the thickness direction of the substrate to the thickness T is 0.4 or less.
[0019] With respect to the Young's modulus E of the substrate and the thickness T of the substrate, E·T 3 The value is 3 to 18 [GPa mm 3 It is preferable that:
[0020] The Q value of the material at 3000 Hz at room temperature is preferably 1500 or less.
[0021] ρ is the density of the material at room temperature [g / cm 3 ], Q is the Q value of the material at room temperature at 3000 Hz, E is the Young's modulus of the material at room temperature [GPa], and ν is the Poisson's ratio of the material at room temperature, and ρ (1-ν) of the material 2 Q / E value is 25 [g / cm 3 / GPa] or less.
[0022] Another aspect of the present invention is a magnetic disk having at least a magnetic film on the surface of the magnetic disk substrate. Effect of the Invention
[0023] According to the magnetic disk substrate and magnetic disk described above, even if the diameter of the magnetic disk substrate is increased and the plate thickness is reduced, the generation of particles caused by an external impact can be suppressed. [Brief description of the drawings]
[0024] [Figure 1] 1 is a diagram showing an example of an external shape of a magnetic disk substrate according to an embodiment; [Diagram 2] 1A and 1B are diagrams illustrating an example of vibration of a magnetic disk substrate according to an embodiment. [Diagram 3] FIG. 2 is a diagram illustrating an example of an outer circumferential end portion of a magnetic disk according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The magnetic disk substrate of the present invention will be described in detail below. In the following description, a magnetic disk glass substrate will be used, but the magnetic disk substrate may be a non-magnetic metal substrate in addition to a glass substrate. In the case of a glass substrate, the glass that can be used may be aluminosilicate glass, soda-lime glass, borosilicate glass, etc. In particular, amorphous aluminosilicate glass can be preferably used, since it can be chemically strengthened as necessary and can produce a glass substrate for a magnetic disk excellent in flatness of the main surface and strength of the substrate. Examples of materials that can be used for the metal substrate include aluminum alloys, titanium alloys, and single crystal silicon. A magnetic disk is produced by forming at least a magnetic film on the surface of the magnetic disk substrate.
[0026] Fig. 1 is a diagram showing the external shape of a magnetic disk substrate of this embodiment. As shown in Fig. 1, a magnetic disk substrate 1 in this embodiment (hereinafter simply referred to as substrate 1) is a disk-shaped thin plate substrate formed with an inner hole 2. A magnetic disk is produced by forming films such as a magnetic film, an undercoat film, and a soft magnetic layer on this substrate 1. There is no restriction on the size of the substrate 1 as long as the diameter D is 85 mm or more, preferably 90 mm or more, but the substrate 1 is suitably applicable to, for example, a magnetic disk substrate having a nominal diameter of 3.5 inches. In the case of a magnetic disk substrate having a nominal diameter of 3.5 inches, the diameter D (outer diameter) of the disk shape is 85 mm or more, preferably 90 mm or more. Specifically, the nominal value of the outer diameter of the disk shape is 95 mm or 97 mm. As described above, the amplitude of vibration of the magnetic disk caused by an external shock different from flutter vibration increases and becomes more difficult to attenuate as the outer diameter of the substrate 1 increases. Therefore, the substrate 1 of this embodiment is preferable when used for magnetic disks with a nominal size of 3.5 inches or more.
[0027] The diameter D of the substrate 1 in this embodiment is 85 mm or more, preferably 90 mm or more, and the thickness T of the substrate 1 is 0.6 mm or less. Furthermore, the substrate 1 is made of a material with a Young's modulus E of 90 GPa or more. The substrate 1 has a shape with a larger diameter D and a thinner thickness T than the conventional shape. This allows the number of magnetic disks to be incorporated in the HDD to be increased, and the storage capacity to be increased. At this time, since the diameter D of the substrate 1 is large and the thickness T is thin, as described above, the magnetic disk comes into contact with the ramp in the HDD due to the vibration of the substrate 1 caused by the impact when the HDD is installed, and also the magnetic disk is likely to come into contact with the magnetic disks arranged next to each other in the HDD. Furthermore, the magnetic disk located at the top of the magnetic disks may come into contact with the ceiling surface of the magnetic disk storage container of the HDD. The upper limit of the diameter D of the substrate 1 is, for example, 100 mm in consideration of the standard size of a nominal 3.5-inch HDD. The lower limit of the thickness T of the substrate 1 is, for example, 0.30 mm in consideration of suppressing arcing when a bias voltage is applied during the film formation process. There is no particular need to set an upper limit for the Young's modulus E, but it is, for example, 120 GPa in consideration of ease of processing.
[0028] FIG. 2 is a diagram showing an example of vibration of the substrate 1 caused by the above-mentioned shock. Such vibration is different from the steady-state flutter vibration caused in a steady rotation state caused by the rotating magnetic disk and the air flow around it. The vibration caused by the shock is a vibration in which the main surface of the substrate 1 is displaced in an out-of-plane direction relative to the main surface. In particular, in a HDD, the inner peripheral end is fixed to the spindle, while the outer peripheral end is a free end and displaces in an out-of-plane direction relative to the main surface. Such vibration displaced in an out-of-plane direction of the main surface (vibration in the plate thickness direction) causes contact with the ramp in the HDD, contact with the adjacent magnetic disk, and further contact with the ceiling surface of the magnetic disk storage container. Such contact may cause the contacted portion of the magnetic disk to chip, generating particles. The generated particles often scatter in the storage container and adhere to the read / write area of the magnetic disk. For this reason, in this embodiment, a material with a Young's modulus of 90 GPa or more is used for the substrate 1.
[0029] When the substrate 1 is a glass substrate, for example, the following glass composition can provide an amorphous oxide glass having a Young's modulus of 90 GPa or more.
[0030] (Glass 1) SiO2 56-80 mol%, LiO 1 to 10 mol%, B2O3 0-4 mol%, The total content of MgO and CaO (MgO+CaO) is 9 to 40 mol%, It is. The specific gravity of glass 1 is 2.75 g / cm 3 Hereinafter, the glass transition temperature Tg is 650° C. or higher.
[0031] (Glass 2) SiO2 56-80 mol%, LiO 1 to 10 mol%, B2O3 0-4 mol%, The total content of MgO and CaO (MgO+CaO) is 9 to 40 mol%, and The molar ratio of the total content of SiO2 and ZrO2 to the content of Al2O3 ((SiO2+ZrO2) / Al2O3) is 2 to 13. It is. The glass transition temperature Tg of glass 2 is 650° C. or higher.
[0032] (Glass 3) In mole percent, SiO2 56-65%, Al2O3 5-20%, B2O30-4%, MgO 3-28%, Li2O 1~10%, and The total content of SiO2 and Al2O3 (SiO2+Al2O3) is 65-80%, The total content of MgO and CaO (MgO+CaO) is 11~30%. The total content of MgO, CaO, SrO and BaO (MgO+CaO+SrO+BaO) is 12~30%, Sum of MgO content, 0.7×CaO content, Li2O content, TiO2 content and ZrO2 content (MgO+0.7CaO+Li2O+TiO2+ZrO2) 16% or more, 5×Li2O content, 3×Na2O content, 3×K2O content, 2×B2O3 content, MgO content, 2×CaO content, 3×SrO content and sum of BaO content (5Li2O+3Na2O+3K2O+2B2O3+MgO+2CaO+3SrO+BaO) 32~58%, Sum of SiO2 content, Al2O3 content, B2O3 content, P2O5 content, 1.5×Na2O content, 1.5×K2O content, 2×SrO content, 3×BaO content and ZnO content (SiO2+Al2O3+B2O3+P2O5+1.5Na2O+1.5K2O+2SrO+3BaO+ZnO) 86% or less, and Sum of SiO2 content, Al2O3 content, B2O3 content, P2O5 content, Na2O content, K2O content, CaO content, 2×SrO content and 3×BaO content (SiO2+Al2O3+B2O3+P2O5+Na2O+K2O+CaO+2SrO+3BaO) 92% or less, and The molar ratio of CaO to MgO (CaO / MgO) is 2.5 or less; The molar ratio of the Na2O content to the Li2O content (Na2O / Li2O) is 5 or less; The molar ratio of the Li2O content to the total content of MgO and CaO (Li2O / (MgO+CaO)) is 0.03 to 0.4. The molar ratio of the SiO2 content to the total content of Li2O, Na2O and K2O (SiO2 / (Li2O+Na2O+K2O)) is 4 to 22, The molar ratio of the total content of SiO2 and ZrO2 to Al2O3 ((SiO2+ZrO2) / Al2O3) is 2 to 10. The molar ratio of the total content of TiO2 and Al2O3 to the total content of MgO and CaO ((TiO2+Al2O3) / (MgO+CaO)) is 0.35 to 2. The molar ratio of the total content of MgO and CaO to the total content of MgO, CaO, SrO and BaO ((MgO+CaO) / (MgO+CaO+SrO+BaO)) is 0.7 to 1, The molar ratio of the BaO content to the total content of MgO, CaO, SrO and BaO (BaO / (MgO+CaO+SrO+BaO)) is 0.1 or less; The molar ratio of the P2O5 content to the total content of B2O3, SiO2, Al2O3 and P2O5 (P2O5 / (B2O3+SiO2+Al2O3+P2O5)) is 0.005 or less; and Glass transition temperature is 670℃ or higher and Young's modulus is 90GPa or higher. Specific gravity is 2.75 or less, The average linear expansion coefficient at 100 to 300°C is 40×10 -7 ~70×10 -7 / °C range.
[0033] In this case, when an impact (acceleration) of 70 [G] is applied to the substrate 1 in the normal direction of the main surface of the substrate 1 for 2 [ms] with the inner peripheral edge of the substrate 1 fixed, it is preferable that the maximum amplitude of the vibration in the thickness direction of the outer peripheral edge of the substrate 1 is 0.25 mm or less. By making the maximum amplitude 0.25 mm or less in this way, the above-mentioned contact can be prevented. The above-mentioned impact test was carried out using an AVEX-SM-110-MP type testing machine manufactured by Air Brown Co., Ltd. Therefore, in one embodiment, the diameter D of the substrate 1 is 85 mm or more, and preferably 90 mm or more, the thickness T of the substrate 1 is 0.6 mm or less, and when an impact of 70 [G] is applied to the substrate 1 for 2 [ms] in the normal direction to the main surface of the substrate 1 with the inner peripheral end of the substrate 1 fixed, the maximum amplitude due to vibration in the thickness direction of the outer peripheral end of the substrate 1 is 0.25 mm or less.
[0034] According to one embodiment, the substrate 1 is preferably made of glass having a glass transition temperature Tg of 650° C. or higher, and more preferably has a glass transition temperature Tg of 680° C. or higher. The higher the glass transition temperature Tg, the higher the thermal durability, and the more likely it is that deformation of the substrate, such as flatness, that occurs when the substrate 1 is heat-treated can be suppressed. In consideration of the heat treatment when forming a magnetic film of a magnetic disk or the like on the substrate 1, the glass transition temperature Tg is preferably set to 650° C. or higher in order to suppress thermal deformation. Specifically, when a metal film including a magnetic film and the like is formed on the substrate 1 to a thickness of about 30 nm to produce a magnetic disk, the substrate 1 is heated. During this heating process, the substrate 1 is easily deformed due to thermal history. For this reason, according to one embodiment, it is preferable that the change in flatness of the substrate 1 after heating at 730° C. and the flatness of the substrate 1 before heating (flatness after heating−flatness before heating) is 4 μm or less. By limiting the change in flatness in this way, a flat magnetic disk can be obtained, and micro-vibrations during rotation of the magnetic disk can be reduced.
[0035] According to one embodiment, the substrate 1 has a linear expansion coefficient of 70×10 -7 [1 / K] or less, and more preferably, the linear expansion coefficient is 60×10 -7 The lower limit of the linear expansion coefficient of the substrate 1 is, for example, 40×10 -7 [1 / K]. The linear expansion coefficient here is the linear expansion coefficient calculated from the difference in thermal expansion between 100°C and 300°C. By using such a linear expansion coefficient, it is possible to suppress thermal expansion during the heat treatment for forming a magnetic film, etc., and to suppress thermal distortion of the substrate 1 around the gripped portion when the gripping member of the film forming apparatus fixes and grips the surface of the outer periphery end (hereinafter referred to as the outer periphery end face). For example, the linear expansion coefficient of a conventional aluminum alloy substrate is 242×10 -7 [1 / K], whereas for conventional glass substrates, it is 95×10 -7 [1 / K] or more, whereas the linear expansion coefficient of the glass substrate 1 of one embodiment is 51×10 -7[1 / K]. On the other hand, there is no particular need to set a lower limit for the linear expansion coefficient of the substrate 1, but if the linear expansion coefficient of the substrate 1 becomes too small, when the temperature inside the HDD rises, the spindle expands and comes into contact with and presses against the circular hole of the substrate, which may cause deformation of the substrate. Therefore, for example, the lower limit of the linear expansion coefficient is set to 20×10 -7 It is even more preferable to set it to [1 / K].
[0036] According to one embodiment, the Vickers hardness Hv of the substrate 1 is 650 [kgf / mm 2 According to one embodiment, the Knoop hardness Hk of the substrate 1 is preferably 600 [kgf / mm 2 ] or more. By increasing the Vickers hardness Hv or Knoop hardness Hk, it is possible to suppress chipping of the substrate 1 and generation of particles even when the substrate 1 comes into contact with another substrate 1 or with another member due to vibration caused by an external impact. In addition, when the outer peripheral end face is gripped by a gripping member of a film-forming apparatus during film formation, for example, a magnetic film, the outer peripheral end face may be chipped due to gripping, generating particles, and this can be prevented from adhering to the main surface of the substrate 1. For example, the Vickers hardness Hv of an aluminum alloy substrate is 128 [kgf / mm 2 ], whereas for a conventional glass substrate, it is 620 [kgf / mm 2 ], whereas the glass substrate 1 of the embodiment has a resistance of 741 [kgf / mm 2 ].
[0037] Fig. 3 is an enlarged view of an example of an end portion of a magnetic disk. Fig. 3 shows two adjacent magnetic disks in a HDD. In Fig. 3, the film thickness of the magnetic film, etc. is overwhelmingly smaller than the plate thickness of the substrate 1, about several tens of nm, so the magnetic film, etc. are not shown. The substrate 1 has a pair of main surfaces 3, side wall surfaces 4 arranged along a direction perpendicular to the pair of main surfaces 3, and a pair of chamfered surfaces 5 arranged between the pair of main surfaces 3 and the side wall surfaces 4. The side wall surfaces 4 and the chamfered surfaces 5 are formed on the outer circumferential edge and the inner circumferential edge of the substrate 1, respectively.
[0038] In an HDD, magnetic disks 10 with a magnetic film or the like (not shown) formed on the surface of a substrate 1 are arranged next to each other as shown in Fig. 3. When the magnetic disks 10 vibrate in the normal direction of the main surface 3 and come into contact with the adjacent magnetic disks 10, corners 6 that are connection points between the main surface 3 and the chamfered surface 5 at the outer periphery are likely to come into contact. This contact causes a large impact on the chamfered surface 5 near the corners 6. The chamfered surface 5 is formed by grinding with a grindstone and then polishing the edge with a brush or the like. In the case of a substrate made of a glass material with a Young's modulus E of 90 GPa or more, it has been found that there are more latent cracks or fine cracks on the surface of the chamfered surface 5 than in the case of a conventional glass substrate with a low Young's modulus. The reason for this is not entirely clear, but it is presumed that, for example, glass with a high Young's modulus is generally hard, so that the load during grinding is large, causing deeper cracks than in the past, and some of these cracks remain as latent cracks or fine cracks after polishing. In this state, if the corner 6 is subjected to an impact due to contact with a ramp member or the like, the latent cracks or fine cracks will progress, and as a result, the corner 6 or part of the chamfered surface 5 of the substrate 1 in the magnetic disk 10 may chip, generating particles together with the magnetic film thereon. In such a case, the larger the width W1 described later, the more likely it is that the corner 6 or part of the chamfered surface 5 will chip. Particles generated at the corners 6 or the chamfered surfaces 5 often scatter within the HDD housing and adhere to the read / write area of the magnetic disk 10 .
[0039] For this reason, according to one embodiment, in the chamfering process, it is preferable to reduce the machining allowance when forming the chamfered surface 5. When the diameter of the magnetic disk 10 is large, 85 mm or more, preferably 90 mm or more, and the plate thickness is thin, 0.600 mm or less, the corner 6 is easily brought into contact by vibration, so it is preferable to reduce the machining allowance when forming the chamfered surface 5 to reduce the number of latent cracks and fine cracks. By doing so, even if the corner 6 of the magnetic disk 10 comes into contact with a ramp member or the like due to large vibration, it is possible to suppress the generation of particles. Here, the machining allowance when forming the chamfered surface 5 refers to the value of the width W1 described later. In addition, there are cases where the outer diameter is adjusted by cutting a certain amount of the outer periphery at the beginning of grinding, but according to the research of the present inventor, such an initial machining allowance does not affect latent cracks, etc. It is presumed that the reason for this is that latent cracks, etc. generated by the initial machining allowance disappear due to the effect of the final machining allowance. Specifically, at least the outer peripheral end face of the substrate 1 is provided with the chamfered surface 5. At this time, the width W1 (see FIG. 3) of the chamfered surface 5 along the radial direction of the substrate 1 is preferably 120 μm or less. More preferably, the width W1 is 90 μm or less. By adjusting the machining allowance when forming the chamfered surface 5 so that the width W1 is 120 μm or less, the number of latent cracks or fine cracks on the chamfered surface 5 can be reduced even when the diameter of the magnetic disk 10 using the high Young's modulus glass substrate is large and the plate thickness is thin, making the corners 6 more likely to come into contact due to vibration. Therefore, even if the corners 6 come into contact, it is possible to suppress the chipping of the corners 6 or the chamfered surface 5 and the generation of particles. The lower limit of the width W1 is, for example, 20 μm. If the width W1 is less than 20 μm, the chamfered surface 5 is too small, and chipping may occur in the substrate manufacturing process after shape processing, the film formation process, and the like. As shown in Fig. 3, the chamfered surface 5 may have a linear shape or an outwardly convex arc or curved shape in a cross section cut in the radial direction through the center of the magnetic disk 10. In this case, the chamfered surface 5 refers to a portion where the inclination angle of the tangent at each position with respect to the side wall surface 4 and the main surface 3 is 5 to 85 degrees. Fig. 3 shows the chamfered surface 5 with a constant inclination angle θ1 with respect to the main surface 3.
[0040] According to one embodiment, the ratio (2·W2) / T of twice the width W2 (see FIG. 3) of chamfered surface 5 on the outer periphery of substrate 1 along the thickness direction of substrate 1 to the thickness T is preferably 0.4 or less. The ratio (2·W2) / T is more preferably 0.3 or less. If the ratio (2·W2) / T exceeds 0.4, side wall surface 4 becomes too small, and the outer peripheral edge may be chipped or cracked due to gripping or application of a bias voltage when forming a magnetic film or the like.
[0041] Furthermore, according to one embodiment, the Young's modulus E [GPa] and the plate thickness T [mm] are expressed as follows: E·T 3 The value is 3 to 18 [GPa / mm 3 ], and 3 to 16 [GPa / mm 3 ], and more preferably 5 to 15 [GPa / mm 3 It is particularly preferred that E·T 3 If the value of E·T is in this range, contact of the magnetic disk 10 due to vibration can be suppressed. 3 The value is 3 [GPa / mm 3 If the distance is less than 1 / 2 mm, the magnetic disk 10 is likely to come into contact with the magnetic disk 10 due to vibration. 3 The value is 18 [GPa / mm 3 ], the plate thickness cannot be increased in order to ensure the number of magnetic disks 10 built into the HDD, and so Young's modulus E is increased. In this case, as Young's modulus E increases, substrate 1 tends to become harder than necessary, and the polishing time for main surface 3 becomes longer, which is undesirable in terms of the production efficiency of magnetic disk substrate 1. According to one embodiment, Young's modulus E [GPa] and density ρ [g / cm 3 ], the specific elastic modulus calculated by E / ρ is 36 [GPa cm 3 / g] or more. Even if the Young's modulus is high, if the density is high, the weight of the substrate itself may cause large vibrations. There is no need to set an upper limit on the specific elastic modulus, but from the viewpoint of productivity, it is preferable to set it to, for example, 41 [GPa cm 3 / g] may also be used.
[0042] When such substrates 1 are mounted on an HDD, the number of substrates 1 mounted on the HDD depends on the thickness T of the substrates 1. The thickness of the magnetic film formed on the substrate 1 is several tens of nm, which is thin enough to be ignored compared to the thickness T of the substrate 1. For example, when the thickness T of the substrate 1 is 0.635 mm, nine or more substrates 1 can be mounted; when the thickness T of the substrate 1 is 0.5 mm, ten or more substrates 1 can be mounted; and when the thickness T of the substrate 1 is 0.38 mm, twelve or more substrates 1 can be mounted. In this way, the number of substrates 1 mounted varies depending on the thickness T of the substrate 1. Therefore, the storage capacity can be increased by reducing the thickness T of the substrate 1 and increasing the number of substrates mounted. In this case, as described above, the substrate 1 of this embodiment is less likely to come into contact with other substrates 1 or components due to vibration even if the thickness T is reduced. Furthermore, according to one embodiment, it is preferable that the substrate 1 is not damaged in an impact test in which the inner peripheral edge of the substrate 1 is fixed to reproduce the clamping of a magnetic disk and an impact of 600 G is applied to the substrate 1 for 2 ms. Such a substrate 1 is preferable from the viewpoint of improving durability, since the substrate 1 is not damaged even if a large impact is applied to the HDD. This substrate 1 can be achieved, for example, by using the above-mentioned glasses 1 to 3.
[0043] According to one embodiment, the material of the substrate 1 preferably has a Q value (quality factor) of 1500 or less at room temperature (25° C.) and 3000 Hz. The Q value is the vibration energy stored in the substrate 1 vibrating during one period divided by the energy dissipated from the vibrating substrate 1, and the smaller this value is, the greater the vibration damping. Therefore, the smaller the Q value of a material is used, the faster the vibration damping can be. Therefore, the number of contacts with adjacent substrates 1 or lamps in the HDD can be reduced, and the impact at the time of contact can be mitigated, making it possible to suppress adverse effects such as the generation of particles due to contact. The Q value at room temperature and 3000 Hz is more preferably 1300 or less. The Q value at 3000 Hz was obtained as follows. First, a laser Doppler vibrometer (LDV) was used to generate vibrations on the substrate 1 rotated by a spin stand, and the vibrations were measured by applying a laser to the approximate outer peripheral edge of the substrate 1. The obtained data was appropriately Fourier transformed to obtain a frequency response function (horizontal axis: frequency (unit: Hz), vertical axis: NRRO (Non Repeatable Runout) Amplitude (unit: nm)). Next, for each peak observed in the frequency response function, the Q value (= f0 / (f2-f1)) was obtained using the half-width method (a method of calculation using frequencies f1 and f2 (> f1) corresponding to a value 3 dB lower than the peak value of NRRO and the frequency f0 (resonance frequency) corresponding to the peak value). The obtained measurement results were plotted on an XY plane with frequency on the horizontal axis and Q value on the vertical axis, and a linear approximation was performed by the least squares method to obtain an approximate straight line. The Q value at 3000 Hz was obtained on the obtained approximate straight line or by extrapolating the approximate straight line as necessary. The substrate 1 used for evaluation with the laser Doppler vibrometer had an outer diameter of 95 mm, an inner diameter of 25 mm, and a thickness of 0.635 mm. The substrate rotation speed was 6900 rpm, the measurement position was a radial position of 46.5 mm from the substrate center (1 mm inside from the outer edge), and the measurement was performed at room temperature.
[0044] According to one embodiment, ρ is defined as the density at room temperature of the material of the substrate 1 [g / cm 3 ], Q is the Q value of the material of substrate 1 at 3000 Hz at room temperature, E is the Young's modulus [GPa] of the material of substrate 1 at room temperature, and ν is the Poisson's ratio of the material at room temperature. The material of substrate 1 is then expressed as ρ·(1-ν) 2 Q / E value is 25 [g / cm 3 / Gpa]. The amplitude at the outer peripheral edge of the substrate 1 is preferably less than ρ·(1-ν) 2 The amplitude is proportional to / E / ξ (ξ is the damping ratio of the material of the substrate 1), and the damping ratio ξ is expressed as 1 / (2·Q) (Q is the Q value), so the amplitude is 2·ρ·(1-ν) 2 Proportional to Q / E, where 2 ρ(1-ν) 2 Q / E is 25 [g / cm 3 / Gpa], it was found that the amplitude of vibration in a specific frequency band can be efficiently reduced, that is, the RSS (root of sum of flutter vibration amounts: root of sum of squares) of flutter vibration in the range of 1000 to 4000 Hz can be made less than 80 nm. Specifically, the RSS in the range of 1000 to 4000 Hz is the square root of the integrated value of the square of the amplitude of flutter vibration from 1000 Hz to 4000 Hz. In other words, 2·ρ(1-ν) 2 Q / E is 25 [g / cm 3 / GPa], the RSS in the range from 1000Hz to 4000Hz can be reduced. 2 Q / E is 20 [g / cm 3 / Gpa] or less, the RSS in the range from 1000 Hz to 4000 Hz can be made 68 nm or less, which is more preferable. In addition, the impact of flutter vibration in the frequency band below 1000Hz is becoming less due to recent advances in head servo technology, while flutter vibration in the band above 4000Hz is small to begin with. Therefore, it is becoming important to reduce flutter vibration in the 1000 to 4000Hz band. The substrate 1 of this embodiment has such characteristics.
[0045] Such a substrate 1 is produced, for example, as follows. Here, as an example, a case where a glass substrate is used as the substrate 1 will be described. First, a forming process is performed on a glass blank, which is a material for a plate-shaped magnetic disk substrate having a pair of main surfaces. Next, the glass blank is roughly ground. After that, the glass blank is subjected to shape processing and end face polishing. After that, fine grinding is performed on the main surface of the substrate obtained from the glass blank using fixed abrasive grains. After that, the substrate is subjected to first polishing of the main surface, chemical strengthening, and second polishing of the main surface. In this embodiment, the substrate is produced in the above-mentioned flow, but it is not necessary to always perform the above-mentioned processes, and the order of these processes may be appropriately changed or omitted. For example, among the above, fine grinding, first polishing, and chemical strengthening may not be performed. Each process will be described below.
[0046] (a) Forming of glass blanks In forming the glass blank, for example, a press molding method can be used. A circular glass blank can be obtained by the press molding method. Furthermore, the glass blank can be manufactured by using a known manufacturing method such as a down-draw method, a re-draw method, or a fusion method. The plate-shaped glass blank manufactured by these known manufacturing methods is appropriately shaped to obtain a disk-shaped substrate that is the base of the magnetic disk substrate.
[0047] (b)Rough grinding In the rough grinding, grinding is performed on both main surfaces of the glass blank. For example, loose abrasive grains are used as the grinding material. In the rough grinding, the glass blank is ground so as to approximate the target plate thickness dimension and the target flatness of the main surface. Note that the rough grinding is performed according to the dimensional accuracy or surface roughness of the molded glass blank, and may not be performed in some cases.
[0048] (c) Shape processing Next, shaping is performed. In shaping, first, after molding the glass blank, a circular hole and an outer periphery are formed using a known processing method to obtain a disk-shaped substrate with a circular hole (circular hole forming process). Then, the end surface of the substrate is chamfered (chamfering process). As a result, a side wall surface 4 perpendicular to the main surface 3 and a chamfered surface 5 inclined with respect to the main surface 3 are formed on the end surface of the substrate between the side wall surface 4 and the main surface 3 on both sides. In the chamfering process, the side wall surface 4 and the two chamfered surfaces 5 may be formed simultaneously by grinding the end surface of the substrate using a forming grindstone.
[0049] (d) Edge polishing Next, the edge surface of the substrate is polished. Edge surface polishing is a process in which, for example, a polishing liquid containing free abrasive grains is supplied between the polishing brush and the outer peripheral edge surface (side wall surface 4 and chamfered surface 5) and the inner peripheral edge surface (side wall surface 4 and chamfered surface 5) of the substrate, and the polishing brush and the substrate are moved relatively. In edge surface polishing, the inner peripheral edge surface and the outer peripheral edge surface of the substrate are polished to a mirror finish.
[0050] (e) Fine grinding Next, the main surface of the substrate is subjected to precision grinding. For example, a double-sided grinding device with a planetary gear mechanism is used to grind the main surface 3 of the substrate. In this case, for example, fixed abrasive grains are provided on a surface plate for grinding. Alternatively, grinding using free abrasive grains can also be performed. Note that precision grinding may not be performed in some cases.
[0051] (f) First polishing Next, the main surface 3 of the substrate is subjected to a first polishing. In the first polishing, a polishing pad attached to a surface plate is used with free abrasive grains. The first polishing removes cracks and distortions remaining on the main surface 3 when precision grinding is performed with fixed abrasive grains, for example. In the first polishing, the surface roughness of the main surface 3, for example the arithmetic mean roughness Ra, can be reduced while preventing the shape of the edge of the main surface 3 from being excessively depressed or protruded. The free abrasive grains used in the first polishing are not particularly limited, but for example, cerium oxide abrasive grains, zirconia abrasive grains, etc. may be used. Note that the first polishing may not be performed in some cases.
[0052] (g)Chemical strengthening Depending on the embodiment of the substrate 1, the substrate may be appropriately chemically strengthened. When chemically strengthening is performed, for example, a molten liquid obtained by heating potassium nitrate, sodium nitrate, or a mixture thereof can be used as the chemical strengthening liquid. By immersing the substrate in the chemical strengthening liquid, lithium ions and sodium ions in the glass composition on the surface layer of the substrate are replaced by sodium ions and potassium ions, which have relatively large ionic radii, respectively, in the chemical strengthening liquid, forming a compressive stress layer in the surface layer portion, and the substrate is strengthened. The timing of chemical strengthening can be determined as appropriate, but it is particularly preferable to perform polishing after chemical strengthening, as this not only smoothes the surface but also removes any foreign matter that has adhered to the surface of the substrate due to the chemical strengthening.
[0053] (h) Second polishing (mirror polishing) Next, the substrate after chemical strengthening is subjected to a second polishing. The second polishing is aimed at mirror-polishing the main surface 3. The second polishing is also performed using a polishing device having the same configuration as the first polishing. In the second polishing, the type and particle size of the free abrasive grains are changed from those in the first polishing, and a resin polisher with a soft hardness is used as a polishing pad to perform mirror polishing. This makes it possible to reduce the roughness of the main surface 3 while preventing the shape of the edge of the main surface 3 from being excessively depressed or protruded. The roughness of the main surface 3 is preferably 0.2 nm or less in terms of arithmetic mean roughness Ra (JIS B 0601 2001). Thereafter, the substrate is washed, and thus the substrate 1 can be obtained.
[0054] (Examples, Comparative Examples, Conventional Examples) In order to examine the effect of the substrate 1, various substrates were prepared (Conventional Examples 1 and 2, Comparative Examples 1 and 2, Examples 1 to 12, Examples 61 to 67, Examples 81 to 84, Examples 111 to 114, and Examples 121 to 124). The substrate was a glass substrate or an aluminum alloy substrate. The substrate of Conventional Example 1 and Comparative Example 1 was made of glass 4 having the following composition. The substrate 1 of Examples 1 and 2 was made of glass 1 described above, the substrate 1 of Examples 3 to 5 was made of glass 2 described above, the substrate 1 of Examples 6 to 10 was made of glass 3 described above, the substrate 1 of Examples 11 and 12 was made of glass 5 and 6, which are amorphous aluminosilicate glasses having compositions different from glass 1 to 4 and a Young's modulus E of 100 [GPa] or more, and the substrate 1 of Examples 61 to 67 and Examples 81 to 84 was made of glass 3 described above. The substrate 1 of Examples 111 to 114 was made of glass 5, and the substrate 1 of Examples 121 to 124 was made of glass 6. Chemical strengthening was not performed on any of the substrates. In addition, glasses 1 to 3, 5, and 6 have a specific elastic modulus of 36 [GPa cm 3 / g] or more. Glass 4 is less than 36.
[0055] (Glass 4) SiO2, Al2O3, one or more alkali metal oxides selected from the group consisting of Li2O, Na2O, and K2O, one or more alkaline earth metal oxides selected from the group consisting of MgO, CaO, SrO, and BaO, and ZrO2, HfO2, Nb2O5, Ta2O5, La2O3, and Y2O 3、 and one or more oxides selected from the group consisting of TiO2, SiO2 50 mol% or more, Al2O3 3 mol% or more, and the total content of SiO2 and Al2O3 is 70 to 85 mol%; Contains Li2O and Na2O, and contains 4.3 mol% or more of Li2O; Na2O 5 mol% or more, and the total content of Li2O and Na2O is 24 mol% or less; The total content of the alkali metal oxide and the alkaline earth metal oxide is 8 mol % or more; Contains the molar ratio of the total content of the oxides to the total content of the alkali metal oxides and the alkaline earth metal oxides ((ZrO2+HfO2+Nb2O5+Ta2O5+La2O3+Y2O3+TiO2) / (Li2O+Na2O+K2O+MgO+CaO+SrO+BaO)) is 0.035 or more; Contains MgO and CaO, MgO less than 3 mol %; CaO 4 mol% or less, and the molar ratio of the MgO content to the CaO content (MgO / CaO) is 0.130 to 0.700; This is an amorphous glass.
[0056] The size of the fabricated substrate is an outer diameter (diameter) of 85 mm to 97 mm, and an inner diameter (circular hole diameter) of 25 mm. The specifications of this chamfered surface are a width W1 along the radial direction of 60 μm to 150 μm, and a width W2 along the plate thickness direction of 60 μm to 150 μm. Specifically, for Conventional Examples 1 and 2, in which the plate thickness exceeds 0.6 mm, the width W1 along the radial direction of the chamfered surface is 150 μm, and the width W2 along the plate thickness direction is 150 μm. And, for Comparative Examples 1 and 2 and Examples 1 to 12, in which the plate thickness is 0.6 mm or less, the width W1 is 100 μm, and the width W2 is 100 μm. The widths W1 and W2 of Examples 61 to 67 and 81 to 84 are shown in Tables 3A to 3D below. Therefore, when the widths W1 and W2 are equal, the inclination angle θ1 (see FIG. 3) is 45 degrees. In the shaping process, when forming the outer periphery of the substrate, a diamond scriber was used to make a vertical cut, which was then extended to the opposite side before being cut. In the subsequent chamfering process, a chamfered surface was formed using a grindstone.
[0057] (Experiment 1) The substrates of Conventional Examples 1 and 2, Comparative Examples 1 and 2, and Examples 1 to 12 were attached to an evaluation device equipped with a high-speed camera to determine the maximum amplitude. This evaluation device can apply an external impact (acceleration) of any magnitude, and can capture the accompanying movement (vibration) of the outer peripheral edge of the substrate as a video. The video can then be analyzed to measure the displacement of the outer peripheral edge in the normal direction of the main surface. Using this evaluation device, an impact test was performed in which a 70G impact was applied to the substrate for 2 ms in the normal direction to the substrate's main surface, and the vibration of the outer edge in the normal direction to the main surface was measured. The measurement results are shown as waveform data as shown in Figure 2. From this waveform data, the maximum displacement in either direction in the normal direction relative to the center where the displacement of the outer edge of the substrate is 0 was calculated as the maximum amplitude.
[0058] In addition, in an actual HDD, a ramp for the ramp load mechanism of the magnetic head is built in, and when each magnetic disk is mounted, a gap of 0.25 mm is provided from both main surfaces. In other words, the gap between the ramps for the magnetic disk to fit in is the thickness of the magnetic disk + 0.5 mm. In an actual HDD, this gap is designed to be constant even if the thickness of the substrate changes. On the other hand, the evaluation device does not have this ramp. Therefore, whether or not the vibration of the substrate will cause contact with other components such as a ramp (adjacent substrate, ramp, or HDD container) in an actual HDD is determined by the maximum amplitude of the substrate vibration, and if the maximum amplitude is 0.25 mm or less, it can be determined that there will be no contact with the ramp. If the maximum amplitude exceeds 0.25 mm, there is a very high possibility of contact with another component. The maximum amplitude was measured for three substrates, and the average value of the maximum amplitude was used. In this evaluation, the substrate was not rotated and was evaluated in a stationary state. The thickness of the magnetic film and the like formed in the media process is approximately 100 nm or less on the main surface and can therefore be substantially ignored.
[0059] The evaluation results of the maximum amplitude are shown in Tables 1, 2A, and 2B below. The aluminum alloys ("Al alloys") of Conventional Example 2 and Comparative Example 2 are Al-Mg alloys having the following composition: In mass%, Mg: 3.5-5%, Si: 0-0.05%, Fe: 0-0.1%, Cu: 0-0.12%, Mn: 0-0.3%, Cr: 0-0.1%, Zn: 0-0.5%, Ti: 0-0.1%, and the balance is Al. Furthermore, a film of Ni-P alloy (P: 10 mass%, the balance Ni) was formed on the surface of a substrate made of an Al-Mg alloy by electroless plating so as to cover the entire surface of the substrate. The plate thickness of the substrate on which the plated film is formed refers to the plate thickness including the film.
[0060] [Table 1]
[0061] According to Table 1, in Conventional Examples 1 and 2 in which the plate thickness T exceeds 0.6 mm, even if the Young's modulus is less than 90 [GPa], the plate thickness T is large, so the maximum amplitude is small and the substrate does not come into contact with other members. However, as shown in Comparative Examples 1 and 2, when the plate thickness T is 0.6 mm or less, the maximum amplitude exceeds 0.25 mm, and there is a very high possibility that the substrate will come into contact with other members. In contrast, in Examples 1 and 2, even if the plate thickness T is 0.6 mm or less, the Young's modulus is 90 [GPa] or more, so the maximum amplitude is 0.25 mm or less.
[0062] [Table 2A]
[0063] [Table 2B]
[0064] In Examples 3 to 12, similarly to Examples 1 and 2, even if the plate thickness T is 0.6 mm or less, the Young's modulus is 90 [GPa] or more, so that the maximum amplitude is 0.25 mm or less.
[0065] From the above, according to Table 1 and Tables 2A and 2B, even if the diameter D of the substrate 1 is 85 mm or more and the thickness T of the substrate 1 is 0.6 mm or less, if the Young's modulus E of the material of the substrate 1 is 90 GPa or more, the maximum amplitude will be 0.25 mm or less, so that the substrate 1 will not come into contact with other members due to vibrations caused by external shocks. This makes it possible to suppress the generation of particles inside the HDD.
[0066] (Experiment 2) Furthermore, using the substrates 1 of Examples 6, 8, 11, and 12 as references, the quality of the substrates 1 after impact tests was evaluated using substrates 1 (Examples 61-67, Examples 81-84, Examples 111-114, and Examples 121-124) in which the widths W1 and W2 of the chamfered surface 5 were variously changed. The widths W1 and W2 were variously changed by variously changing the grindstone shape and processing conditions when performing chamfering using a shaped grindstone. Examples 61 to 67 are examples in which the widths W1 and W2 of the substrate 1 of Example 6 are changed, Examples 81 to 84 are examples in which the widths W1 and W2 of the substrate 1 of Example 8 are changed, Examples 111 to 114 are examples in which the widths W1 and W2 of the substrate 1 of Example 11 are changed, and Examples 121 to 124 are examples in which the widths W1 and W2 of the substrate 1 of Example 12 are changed. Therefore, the material, Young's modulus E, plate thickness, and outer diameter of Examples 61 to 67 are the same as those of Example 6, the material, Young's modulus E, plate thickness, and outer diameter of Examples 81 to 84 are the same as those of Example 8, the material, Young's modulus E, plate thickness, and outer diameter of Examples 111 to 114 are the same as those of Example 11, and the material, Young's modulus E, plate thickness, and outer diameter of Examples 121 to 124 are the same as those of Example 12.
[0067] The quality evaluation of the fabricated substrate 1 was carried out by disassembling a commercially available HDD, attaching the substrate 1 and spacer of each embodiment to a spindle, and further attaching a simulated ramp member made of engineering plastic to the substrate surface so that it protruded. The gap between the ramp member and the substrate was set to 0.25 mm. Then, while the substrate 1 was held in place, an impact test was carried out in which an impact of 200 [G] was applied in the normal direction of the main surface of the substrate 1 for 2 [ms]. This test is an accelerated test in which the outer peripheral edge of the substrate 1 and the ramp member are intentionally collided several times or more. After that, the particle distribution around the surface of the substrate 1 that came into contact with the ramp member was observed. Note that, due to the difficulty of quantifying, a relative evaluation was performed. Rank 1: Almost no particles Rank 2: Medium number of particles Rank 3: High number of particles The evaluation results are shown in Tables 3A to 3D below. The lower the rank value, the better the quality evaluation, with rank 1 representing the highest evaluation.
[0068] [Table 3A]
[0069] [Table 3B]
[0070] [Table 3C]
[0071] [Table 3D]
[0072] It can be seen from Tables 3A to 3D that the number of particles can be reduced by setting width W1 to 120 μm or less. It can also be seen that the number of particles can be further reduced by setting width W1 to 90 μm or less. Therefore, when the diameter D of substrate 1 is 85 mm or more, the thickness T of substrate 1 is 0.6 mm or less, and a material having a Young's modulus E of 90 [GPa] or more is used for substrate 1, the number of particles adhering to the main surface of substrate 1 in the HDD can be further suppressed by setting width W1 to 120 μm or less.
[0073] The magnetic disk substrate and magnetic disk of the present invention have been described in detail above, but the present invention is not limited to the above-mentioned embodiments and examples, and various improvements and modifications may be made without departing from the spirit and scope of the present invention. [Explanation of symbols]
[0074] 1 Magnetic disk substrate 2 Inner hole 3 Main surface 4 Side wall 5 Chamfered surface 6 angles 10 Magnetic Disks
Claims
1. A disk-shaped magnetic disk substrate, The diameter D of the substrate is 85 mm or more, and the thickness T of the substrate is 0.6 mm or less, A magnetic disk substrate, characterized in that the substrate is made of a material having a Young's modulus E of 90 GPa or more.
2. 2. The magnetic disk substrate according to claim 1, wherein the diameter D is 90 mm or more.
3. 3. The magnetic disk substrate according to claim 1, wherein when an impact of 70 [G] is applied to the substrate in a normal direction to a main surface of the substrate for 2 [ms] with the inner peripheral edge of the substrate fixed, the maximum amplitude due to vibration in the thickness direction of the outer peripheral edge of the substrate is 0.25 mm or less.
4. A disk-shaped magnetic disk substrate, The diameter D of the substrate is 85 mm or more, and the thickness T of the substrate is 0.6 mm or less, A magnetic disk substrate, characterized in that when an impact of 70 [G] is applied to the substrate for 2 [ms] in a normal direction to a main surface of the substrate while the inner peripheral edge of the substrate is fixed, the maximum amplitude due to vibration in the thickness direction of the outer peripheral edge of the substrate is 0.25 mm or less.
5. 5. The magnetic disk substrate according to claim 4, wherein the diameter D is 90 mm or more.
6. 6. The magnetic disk substrate according to claim 1, wherein the substrate is a glass substrate made of glass having a glass transition point of 650° C. or higher.
7. 7. The magnetic disk substrate according to claim 1, wherein the change in flatness of the substrate after heating at 730° C. and the flatness of the substrate before heating is 4 μm or less.
8. The substrate has a linear expansion coefficient of 70×10 -78. The magnetic disk substrate according to claim 1, which is made of a material having a viscosity of 1 / K or less.
9. The Vickers hardness Hv of the substrate is 650 [kgf / mm 2 9. The magnetic disk substrate according to claim 1, wherein the thickness of the magnetic disk substrate is 100 nm or more.
10. The Knoop hardness Hk of the substrate is 600 [kgf / mm 2 10. The magnetic disk substrate according to claim 1, wherein the thickness of the magnetic disk substrate is 100 nm or more.
11. At least a surface of the outer peripheral end of the substrate is provided with a chamfered surface; The width W of the chamfered surface along the radial direction of the substrate 1 The magnetic disk substrate according to any one of claims 1 to 10, wherein the thickness of the first layer is 120 µm or less.
12. The width W of the chamfered surface along the thickness direction of the substrate 2 The ratio of the thickness T to the thickness T is twice that (2.W 2 12. The magnetic disk substrate according to claim 1, wherein the ratio of the thickness of the magnetic disk to the thickness of the substrate is 0.4 or less.
13. With respect to the Young's modulus E and the plate thickness T of the substrate, E·T 3 The value is 3 to 18 [GPa mm 3 13. The magnetic disk substrate according to claim 1, wherein
14. 14. The magnetic disk substrate according to claim 1, wherein the material has a Q value of 1500 or less at 3000 Hz at room temperature.
15. ρ is the density of the material at room temperature [g / cm 3 ], Q is the Q value of the material at room temperature at 3000 Hz, E is the Young's modulus of the material at room temperature [GPa], and ν is the Poisson's ratio of the material at room temperature, and ρ (1-ν) of the material is 2 ・Q / E value is 25 [g / cm 315. The magnetic disk substrate according to claim 1, wherein the modulus of elasticity is less than [. / GPa].
16. A magnetic disk having at least a magnetic film on the surface of the magnetic disk substrate according to any one of claims 1 to 15.
Citation Information
Patent Citations
Substrate for information recording medium comprising crystallized glass and the information recording medium
JP2001180975A
Glass substrate for information recording medium and magnetic information recording medium using the same
JP2005302289A
Information storage medium and device
JP2008097821A
Magnetic-disc glass substrate and magnetic disc
WO2014051153A1