Antirust coating steel material, method for manufacturing antirust coating steel material and method for improving antirust performance
By applying a water-based inorganic zinc-based paint directly to steel with intact black scale, a composite film is formed that penetrates into cracks, addressing inefficiencies and costs of traditional surface treatments, achieving superior rust prevention.
Patent Information
- Application Number
- JP2023071808
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for improving rust prevention on steel surfaces require costly and time-consuming surface treatments to remove black scale (oxide film) before painting, which is inefficient and prone to localized corrosion due to minute pinholes.
Applying a water-based inorganic zinc-based paint directly onto the steel surface with an intact black scale, forming a composite film that penetrates into the cracks of the oxide film, using zinc silicate particles for enhanced adhesion and rust prevention.
The method reduces costs and time associated with surface treatments by forming a composite film that effectively prevents rust while maintaining strong adhesion, even in the presence of cracks, outperforming conventional methods in rust prevention performance.
Smart Images

Figure 2024157438000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to anti-rust coated steel material, a manufacturing method for anti-rust coated steel material, and a method for improving anti-rust performance, and more particularly to anti-rust coated steel material that exhibits anti-rust performance, a manufacturing method for anti-rust coated steel material, and a method for improving anti-rust performance. [Background technology]
[0002] 2. Description of the Related Art In the field of architecture and civil engineering, for example, in the case of steel materials used in steel bridges and the like, paint exhibiting rust-preventive properties has been conventionally applied to the surface of the steel materials in order to improve the rust-preventive (corrosion-resistant) performance. Specifically, steel material having a black surface (oxide film) is formed by hot rolling, the surface of the steel material is sandblasted (a type of scraping process) to remove the black surface, and a paint having anti-rust properties is applied to the surface of the steel material within a certain period of time after the sandblasting process, and the paint is then dried to produce anti-rust coated steel material. Known examples of paints having the above-mentioned rust-preventing properties include inorganic zinc-based paints such as inorganic zinc-rich paints (see, for example, Patent Document 1).
[0003] In the corrosion-resistant coated steel material described in Patent Document 1, the surface of the steel material is blasted to remove the black scale, and then an inorganic zinc-based paint is applied to the surface of the steel material to form a coating film (first layer), and then the steel material is immersed in a chloride aqueous solution containing magnesium and calcium and dried to form a second layer. It is disclosed that by forming the first and second layers, dissolution of granular zinc in the first layer can be suppressed, providing a sacrificial corrosion protection effect. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-103123 A Summary of the Invention [Problem to be solved by the invention]
[0005] As mentioned above, when painting the surface of steel material, a process for removing the black scale (oxide film) is carried out by blasting or the like as a preparatory process before painting in order to improve the adhesion of the paint and the rust prevention after painting. "Black scale (oxide film)" is also known as mill scale, and is black rust made mainly of triiron tetraoxide. Black scale protects the surface of steel from corrosion, but because tiny pinholes (cracks) form on the surface of the black scale, localized corrosion often occurs relatively quickly. Therefore, although black scale is a benign form of rust that prevents corrosion, it is not useful as a protective film to protect steel (it does not adhere well to steel). For these reasons, in order to manufacture coated steel products, it is necessary to first carry out surface treatment (black scale removal treatment) by blasting, grinding or polishing, which requires cost and time.
[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a novel anti-rust coated steel material, a method for manufacturing anti-rust coated steel material, and a method for improving anti-rust performance. Another object of the present invention is to provide an anti-rust coated steel material that is capable of exhibiting anti-rust performance while reducing the cost and time burden associated with surface treatment of the steel material, a method for manufacturing the anti-rust coated steel material, and a method for improving the anti-rust performance. [Means for solving the problem]
[0007] As a result of intensive research, the inventors have discovered that it is possible to manufacture anti-rust coated steel material that exhibits anti-rust performance by directly applying an aqueous inorganic zinc-based paint to the surface of the steel material (black surface) without first removing the black surface (oxide film), and then drying the paint to form an "oxide film" and a "coating film" with anti-rust performance on the surface of the steel material (by forming a "composite film"). In more detail, it was discovered that by forming an aqueous inorganic zinc-based coating on the surface of steel (black surface), the coating adheres closely to the black surface, the coating penetrates into cracks in the black surface, and the zinc particles (zinc oxide particles) filled in the coating reach and fill the interior of the cracks.
[0008] Therefore, according to the present invention, the above-mentioned problems are solved by providing an anti-rust painted steel material that exhibits anti-rust performance, comprising a steel material, an oxide coating film provided on the surface of the steel material, and a coating film that is formed on the surface of the oxide coating and has anti-rust performance, wherein the coating film is an aqueous inorganic zinc-based coating film that is provided directly on the surface of the oxide coating and is in close contact with the surface of the oxide coating.
[0009] In this case, a plurality of cracks are formed on the surface of the oxide coating, the coating is a zinc-based coating containing an aqueous inorganic binder and no organic solvent-based binder, and the coating penetrates into the cracks formed on the surface of the oxide coating, and the zinc particles filled in the coating reach and fill the interior of the cracks. The coating film is preferably filled with zinc silicate particles, and exhibits rust-preventing performance by inhibiting the passage of red rust and white rust associated with zinc through the coating film.
[0010] Furthermore, according to the present invention, the above-mentioned problem is also solved by a manufacturing method for anti-rust coated steel material that exhibits anti-rust performance, which includes a steel material forming step of forming steel material having an oxide film on its surface by hot rolling processing, and a coating step of coating the surface of the steel material with a paint having anti-rust performance, in which the coating step directly coats the surface of the steel material with the water-based inorganic zinc-based paint and dries the paint to form the oxide film and a coating film having anti-rust performance on the surface of the steel material.
[0011] In this case, in the steel material formation process, the oxide film is not removed, and the steel material is formed with the oxide film remaining on its surface, and in the painting process, the zinc-based paint containing an aqueous inorganic binder and no organic solvent-based binder is directly painted onto the surface of the steel material, forming a composite film on the surface of the steel material that integrates the oxide film and the paint film. In addition, the paint is an aqueous ceramic zinc-rich paint, and is composed of a mixture of an aqueous inorganic binder and zinc powder, and the coating film is a coating film filled with zinc silicate particles, and the zinc silicate particles preferably reach the inside of cracks formed on the surface of the oxide coating and fill the inside of the cracks. In addition, the anti-rust painted steel material preferably exhibits higher anti-rust performance than painted steel material obtained by applying the paint to the surface of steel material from which the oxide coating has been removed by blast preparation (rust removal degree of Sa2.5 or higher according to ISO8501-1).
[0012] According to the present invention, the above-mentioned problems are also solved by a method for improving rust-prevention performance, which comprises directly painting an aqueous inorganic zinc-based paint on a surface of a steel material having an oxide film on its surface without removing the oxide film, thereby forming the oxide film and a coating film having rust-prevention performance on the surface of the steel material. Effect of the Invention
[0013] According to the present invention, it is possible to provide a novel anti-rust coated steel material that exhibits anti-rust performance, a method for producing an anti-rust coated steel material, and a method for improving the anti-rust performance. Furthermore, it is possible to provide anti-rust coated steel material that is capable of exhibiting anti-rust performance while reducing the cost and time burden associated with surface treatment of steel material, a method for manufacturing anti-rust coated steel material, and a method for improving anti-rust performance. [Brief description of the drawings]
[0014] [Figure 1] 1 is a cross-sectional view of an anti-rust coated steel material according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view of an anti-rust coated steel material according to a first conventional example. [Diagram 3] FIG. 1 is a cross-sectional view of an anti-rust coated steel material according to a second conventional example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described with reference to FIGS. This embodiment relates to a "manufacturing method for anti-rust coated steel material" that includes a "steel material forming process" for forming steel material having an oxide coating on the surface thereof, and a "painting process" for directly painting an aqueous inorganic zinc-based paint onto the surface of the steel material, and that makes it possible to produce anti-rust coated steel material that exhibits anti-rust performance without performing an oxide coating removal process. The present invention also relates to an "anti-rust coated steel material" produced by the above production method.
[0016] <Anti-rust coated steel> As shown in FIG. 1, the anti-rust coated steel material 1 is a coated steel material that exhibits anti-rust performance, and comprises a steel material 10, an oxide coating 20 provided on the surface of the steel material 10, and a coating film 30 that is formed on the surface of the oxide coating 20 and has anti-rust performance. Anti-rust coated steel material 1 is widely used in the fields of construction and civil engineering, and is a steel material in which a coating film 30 is formed on the surface of steel material 10 for the purpose of improving rust prevention performance, corrosion prevention performance, and weather resistance. The rust-proof coated steel material 1 is also called a coated steel material or a colored steel material. In the case of the anti-rust coated steel material 1, when a coating film 30 is formed on the surface of the steel material 10, the oxide film 20 formed on the surface of the steel material 10 is not removed (no surface preparation is performed), and the coating film 30 is formed as is.
[0017] The steel material 10 is steel processed from an iron and steel material into a plate, a bar, a tube, or the like, and has an oxide film 20 on its surface. Specifically, the steel material 10 is formed by hot rolling the iron and steel material, and has an oxide film 20 on its surface. The steel material 10 is also called black-skin material or black-skin steel material, and includes thick steel plate, thin steel plate, shaped steel, steel pipe, steel bar, steel wire, and the like. "Hot rolling" refers to rolling at a temperature above the recrystallization temperature at which metal does not harden due to processing. During rolling, the hot material surface combines with oxygen in the air to form an oxide film (black scale).
[0018] The oxide film 20 is also called black scale, black rust, or mill scale, and is a non-uniform film mainly made of triiron tetroxide, which covers the surface of the steel material 10. In detail, the oxide film 20 is composed of FeO, Fe 3 O 4 , Fe 2 O 3 The film is composed of oxide layers in this order. A plurality of fine cracks 21 are formed on the surface of the oxide coating 20. The cracks 21 are formed as minute irregularities, cracks, or minute pinholes. The steel material 10 covered with the oxide film 20 (black scale material) is a material that has been hot-rolled and can be obtained relatively cheaply, but its surface is relatively rough and it is said that it has poor adhesion to paint. Therefore, the oxide film 20 (black scale material) is generally removed from the steel material 10 (black scale material).
[0019] The coating film 30 is a water-based inorganic zinc-based coating film that is applied directly to the surface of the oxide film 20 and adheres closely to the surface of the oxide film 20 . More specifically, the coating film 30 is a zinc-based coating film that contains an aqueous inorganic binder and does not contain any organic solvent-based binder, and covers the entire oxide film 20 . The coating film 30 is formed by directly coating the surface of the steel material 10 (the surface of the oxide film 20) with a water-based inorganic zinc-based paint, which will be described later. As shown in FIG. 1, the coating film 30 is a film (cured surface film) in which zinc particles (zinc silicate particles) are densely packed.
[0020] In the above configuration, as shown in FIG. 1, the coating film 30 penetrates into the inside of the crack 21 formed on the surface of the oxide coating 20, and the zinc particles filled in the coating film 30 reach the inside of the crack 21 and fill the inside of the crack. Therefore, the coating film 30 can be adhered to the oxide film 20 in an appropriate manner. In particular, when zinc silicate particles are filled in the coating film 30, the coating film 30 can adhere more strongly to the oxide film 20.
[0021] In the above-mentioned configuration, as shown in FIG. 1, zinc particles are uniformly packed in the coating film 30 so as to be spread out. Therefore, the passage of red rust caused by the steel material 10 and white rust caused by zinc within the coating film 30 can be suppressed, and the coating film 30 can exhibit suitable rust prevention performance. In particular, when zinc silicate particles are packed into the coating film 30, the passage of red rust and white rust can be further inhibited.
[0022] <Method of manufacturing anti-rust coated steel products> Next, the "steel material forming process" and "painting process" performed by the manufacturing method of this embodiment will be described in detail. Note that for the other processes, known techniques may be appropriately adopted.
[0023] In the "steel material forming process," steel material (black steel material) having an oxide film (black scale) on its surface is formed by hot rolling. More specifically, hot rolling is performed at a rolling temperature of 800 to 1200° C., and at the end of the process, temperature control is performed by cooling water curing to form a steel material (black skin steel material). At this time, the sudden temperature change causes contraction, which results in the formation of fine cracks on the surface of the oxide film.
[0024] In this embodiment, the oxide film is not removed, and a steel material is formed with the oxide film remaining on the surface. "Removal treatment (black scale removal treatment)" refers to a process for removing an oxide film from the surface of a steel material, and includes a physical removal method such as blasting, and a chemical removal method such as acid treatment. Methods for physical removal include sandblasting, shot blasting, grinding, polishing, etc. For example, in the case of blasting, it is recommended to carry out the treatment so that the degree of rust removal according to ISO8501-1 is Sa2.5 (Sa2 1 / 2 according to JIS Z 0313) or more.
[0025] In the "painting process," anti-rust paint is applied to the surface of the steel material. More specifically, a water-based inorganic zinc paint is directly applied to the surface of the steel material, and the paint is dried to form an oxide film and a coating film having rust-preventing properties on the surface of the steel material. At this time, a composite film is formed on the surface of the steel material, which is an integrated film of the oxide film and the paint film.
[0026] The "paint" is a water-based inorganic zinc-based paint, a zinc-rich paint that contains a water-based inorganic binder and does not contain an organic solvent-based binder. In other words, water-based means that it does not use organic solvents. Specifically, the paint is a one liquid, one powder mix (mixed in a weight ratio of 20:80) and is an alkaline zinc-rich paint (zinc-rich paint) that is a mixture of an "aqueous inorganic binder (ceramic binder)" and "zinc powder." The "aqueous inorganic binder" contains silica (colloidal silica) as the main component, fine powder of the mineral zinc as a pigment, water as a solvent, and an amine salt as a catalyst. The "zinc powder" used may be fine zinc powder having a particle size of, for example, 0.1 to 10 μm, preferably 0.1 to 5 μm, and more preferably 0.1 to 1 μm. The paint is not limited to the above, and various water-based inorganic zinc-based paints can be used.
[0027] The paint can be applied to the surface of the steel material (the surface of the oxide film) and then dried for 3 to 6 hours at a temperature of 20° C., for example, to harden the coating. For complete hardening, it is recommended to leave it to cure for about 10 to 30 days. By using the above coating material, a coating film (breathing film) having a thickness of 40 to 60 μm and a pencil hardness of 3 to 5H can be formed over the entire surface.
[0028] The formed coating film is a hydrophilic film in which zinc silicate particles are densely packed, and the gaps between the zinc silicate particles are small (few voids). Specifically, because the main component of the "water-based inorganic binder" is silica (silicon dioxide), when it is applied to the surface of steel and hardens, a coating film that is like a coating of zinc silicate particles is formed. As a result, the cracks in the oxide film are filled with zinc silicate particles. Furthermore, by not using organic solvents, the zinc silicate particles are not covered with resin, the contact area between the zinc silicate particles and the oxide film is increased, and the adhesion of the coating film to the oxide film can be improved. For these reasons, the passage of oxides such as red rust and white rust through minute gaps in the coating film can be suppressed, and the growth of these oxides can be prevented. In addition, even if water ingress occurs due to wind and rain, the formation of water channels within the coating film can be prevented.
[0029] The paint may be a combination of the zinc-rich paint (undercoat paint) and the water-based silicate paint (topcoat paint). By further applying a water-based silicate paint, a ceramic film can be formed on the surface of the zinc silicate layer, which is filled with zinc silicate particles, preventing the zinc from leaching out and further improving the rust prevention performance. The main components of water-based silicate paint are colloidal silica, inorganic extender pigments, inorganic color pigments, water, etc. Water-based silicate paint uses silicate (silicate salt) as a binder, and forms an amorphous film by promoting a dehydration condensation reaction. Specifically, silica is in a state where there is Si-OH on the surface of SiO2, and the surface of the substrate is in a state of HO-substrate or HOO-substrate due to moisture in the air and carbon dioxide gas. By applying water-based silicate paint, a dehydration condensation reaction occurs between Si-OH and the active parts of the substrate, HO and HOO, forming covalent bonds of the Si-O substrate, resulting in strong adhesion.
[0030] As described above, through the "steel material forming process", the "painting process", and other processing processes, anti-rust coated steel material that exhibits anti-rust performance can be manufactured. In particular, since the process of removing the oxide film is no longer necessary, it is possible to produce anti-rust coated steel material that is capable of exhibiting anti-rust performance while reducing the cost and time associated with surface treatment of the steel material.
[0031] <Differences from other zinc-rich paints> Next, the differences in coating films formed when various zinc-rich paints are applied to the surface of a steel material (surface of an oxide film) will be described with reference to Figs. 1 to 3. FIG. 1 is a cross-sectional view of an anticorrosive coated steel material 1 of this embodiment, which is coated with a water-based inorganic zinc-rich paint (one that does not use organic solvents). FIG. 2 is a cross-sectional view of a coated steel material, which is Conventional Example 1, that has been coated with an organic zinc-rich paint. FIG. 3 is a cross-sectional view of a coated steel material, which is Conventional Example 2, that has been coated with an inorganic zinc-rich paint (using an organic solvent).
[0032] As shown in Figure 1, the coating film 30 on the anti-corrosive coated steel material 1 is a film filled with water-soluble zinc silicate particles, and because the gaps between the zinc silicate particles are small, the zinc silicate particles reach the cracks 21 in the oxide coating 20 and fill the cracks 21. In addition, the contact area between the zinc silicate particles and the oxide coating is large, which provides strong adhesion (adhesion) to the oxide coating 20. For this reason, even if paint is applied directly to the surface of the oxide film 20 of the steel material 10 without removing the oxide film 20, it is possible to realize an anti-rust coated steel material 1 with a coating film 30 firmly adhered thereto.
[0033] On the other hand, in Figure 2, organic zinc-rich paint is applied, but the paint contains resin (such as epoxy resin) as a binder, and most of the zinc particles are covered with resin. Therefore, the contact area between the zinc particles and the oxide film is small, and the adhesion of the paint to the oxide film is weak. In addition, the coating film forms an environmental barrier film, and because the presence of resin (carbon) makes the film highly viscous and less fluid, the zinc particles do not penetrate into the cracks and do not fill the cracks (if a viscous material is used, a film with many voids will be formed). This weakens the adhesion of the coating film to the oxide film.
[0034] In Figure 3, when an inorganic zinc-rich paint is applied, the zinc particles in the coating film formed by the paint become large, and the voids between the particles also become large. In addition, because it contains an organic solvent (carbon), the zinc particles are covered with resin, reducing the contact area between the zinc particles and the oxide film. The presence of carbon results in a high viscosity film with poor fluidity. Therefore, the zinc particles do not penetrate into the cracks in the oxide film and do not fill the cracks, which weakens the adhesion of the coating to the oxide film.
[0035] As described above, in order to effectively apply zinc-rich paint to the surface of an oxide film on steel, it is recommended to use a "water-based inorganic zinc-rich paint," to use a water-based inorganic binder whose main component is "silica (silicon dioxide)," and to use "paint that does not use organic solvents (carbon)." In other words, when using organic zinc-rich paints or inorganic zinc-rich paints (those that use organic solvents), it is necessary to remove the oxide film from the surface of the steel, as has been done in the past. EXAMPLES
[0036] EXAMPLES The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0037] <Example 1: Anti-rust coated steel material> Based on the above-mentioned manufacturing method, an anti-rust coated steel material was prepared in which a "water-based inorganic zinc-based coating film" was formed on the surface of the oxide film of the steel material. As the "water-based inorganic zinc-rich paint", a water-based ceramic zinc-rich paint (manufactured by Ceratec Co., Ltd., product name: Tough Zinc 11) was used. In addition, in Test Example 1, a steel plate with an oxide film remaining was used as the "steel material," and in Test Example 2, a reinforcing bar with an oxide film remaining was used. The same applies to Example 2.
[0038] <Example 2: Anti-rust coated steel material> Based on the above-mentioned manufacturing method, an anti-rust coated steel material was prepared in which a "water-based inorganic zinc-based coating film" was formed on the surface of the oxide film of the steel material. The "undercoat paint" and "topcoat paint" were used together as the "water-based inorganic zinc-rich paint." The "undercoat paint" was a water-based ceramic zinc-rich paint (manufactured by Ceratec Co., Ltd., product name: Tough Zinc 11), and the "topcoat paint" was a water-based silicate paint (manufactured by Ceratec Co., Ltd., product name: SSA-1000).
[0039] <Test Example 1: Coating adhesion test (cross-cut test)> The rust-proof coated steel materials of Examples 1 and 2 were subjected to a cross-cut test based on JIS K 5600:1999 to confirm the adhesion of the coating.
[0040] Test specimens measuring 70 mm x 150 mm were prepared as Examples 1 and 2, and the coating film of each test specimen was cut in a grid pattern (cross cut). Since an oxide film and a coating film were formed and the film thickness was relatively thick, the cut interval was set to 3 mm. After cutting into a grid pattern, cellophane tape was applied to the cut surface (grid surface) of each specimen, and the edge of the cellophane tape was peeled off at an angle of about 45 degrees. The condition of the cut surface after peeling was evaluated based on the following criteria.
[0041] The criteria for judgment are as follows: Category 0: None of the grids have come off. Category 1: There is small peeling of the paint at the intersection of the cuts. Category 2: The coating has peeled off at the intersection along the cut line. Category 3: The coating has peeled off partially or completely along the cut line. Category 4: The coating has peeled off in large areas, either partially or completely, along the cut line. Classification 5: Classification 4 or higher.
[0042] (Results and discussion of Test Example 1) Example 1 was categorized as 0. In other words, the edges of the cuts were completely smooth, and no peeling occurred in any of the lattice meshes. Example 2 was categorized as Class 2, meaning the coating had peeled off along the cut lines and at the intersections. The results of Test Example 1 show that in both Examples 1 and 2, even when the paint was applied directly to the oxide film of the steel material, there was no problem with the adhesion (bonding strength). In particular, it was found that Example 1 had a higher adhesive strength.
[0043] In addition, in Test Example 1, when organic zinc-rich paint or inorganic zinc-rich paint (using organic solvents) was used, the adhesion of the coating to the oxide film of the steel material was poor, meaning that the coating peeled off, as confirmed by the results of another test.
[0044] <Test Example 2: Rust prevention evaluation test (combined cyclic corrosion test)> Next, the rust-proof coated steel material of Example 1 was subjected to a cyclic corrosion test based on JIS K 5600-7-9:2006 (Cycle A of Annex C) to confirm the corrosiveness (rust prevention) of the test specimen.
[0045] The coated rebar of Example 1 was placed in a combined cycle tester as a test specimen, and the following test cycle (a combination of salt spray, dry, and wet) was repeatedly performed. The pH of the salt spray solution was 6.0 to 7.0. Test cycle details (1) Salt spray: 35°C ± 1°C, 2 hours (2) Drying: 60 degrees ± 1 degree, 20-30%RH, 4 hours (3) Humidity: 50°C ± 1°C, 95% RH or higher, 2 hours Three cycles were performed, each lasting a total of 8 hours. The timing of the check was set to during salt spray (one hour after the start of salt spray), as this is a time when the impact of salt adhesion is relatively small. After the test was completed, a section approximately 3 mm from the scratched area spaced 1 mm apart was cut and the extent of rust erosion (erosion depth) was observed under a 100x microscope.
[0046] (Results and discussion of Test Example 2) In Example 1, it was found that there was no rust on the inside of the coating film, and even in the areas where the coating film had peeled off, sacrificial corrosion protection worked to suppress the progression of rust. The results of Test Example 2 show that Example 1 exhibits rust prevention performance even when the paint is applied directly to the oxide film of the steel material.
[0047] In addition, in Test Example 2, when organic zinc-rich paint and inorganic zinc-rich paint (using organic solvents) were used, the results of another test confirmed that rust had progressed deep into the inner part of the paint film.
[0048] In addition, when the anti-rust painted steel of Example 1 was compared with a painted steel (comparative painted steel) made by painting the same paint on the surface of steel from which the oxide coating had been removed by blasting (rust removal degree of ISO8501-1: Sa2.5 or higher), the results of another test confirmed that the anti-rust painted steel of Example 1 exhibited higher anti-rust performance than the comparative painted steel. This suggests that, for example, zinc silicate particles in the coating reach and fill the cracks in the oxide coating, and that the contact area between the zinc silicate particles and the oxide coating is large, resulting in strong adhesion of the coating to the steel and the oxide coating. [Explanation of symbols]
[0049] 1. Anti-rust painted steel 10 Steel material 20 Oxide coating (black skin) 21 Crack 30 Paint film
Claims
1. A rust-proof coated steel material that exhibits rust-proofing performance, Steel and An oxide coating provided on a surface of the steel material; A coating film having anti-rust properties is formed on the surface of the oxide coating film, The coating film is a water-based inorganic zinc-based coating film that is provided directly on the surface of the oxide film and adheres closely to the surface of the oxide film.
2. A plurality of cracks are formed on the surface of the oxide coating, The coating film is a zinc-based coating film containing an aqueous inorganic binder and not containing an organic solvent-based binder, The coating film penetrates into the cracks formed on the surface of the oxide coating, 2. The rust-proof coated steel material according to claim 1, characterized in that the zinc particles filled in the coating reach and fill the inside of the cracks.
3. The anti-rust coated steel material according to claim 2, characterized in that the coating film is filled with zinc silicate particles and exhibits anti-rust performance by inhibiting the passage of red rust and white rust associated with zinc within the coating film.
4. A method for producing a rust-preventive coated steel material that exhibits rust-preventive performance, comprising the steps of: a steel material forming step of forming a steel material having an oxide film on a surface thereof by hot rolling; A coating process for coating a surface of the steel material with a paint having anti-rust properties, The method for producing anti-rust coated steel material is characterized in that in the painting process, the aqueous inorganic zinc-based paint is directly painted onto the surface of the steel material, and the paint is dried to form the oxide coating and a coating film having anti-rust properties on the surface of the steel material.
5. In the steel material forming step, the oxide film is not removed, and the steel material is formed with the oxide film remaining on the surface thereof; The method for producing anti-rust coated steel material according to claim 4, characterized in that in the painting process, a zinc-based paint containing an aqueous inorganic binder and no organic solvent-based binder is directly painted onto the surface of the steel material, forming a composite film on the surface of the steel material that integrates the oxide film and the paint film.
6. The paint is an aqueous ceramic zinc-rich paint, and is made by mixing an aqueous inorganic binder with zinc powder; The coating is a coating filled with zinc silicate particles, The method for manufacturing anti-rust coated steel material according to claim 5, characterized in that the zinc silicate particles reach and fill the interior of cracks formed on the surface of the oxide coating.
7. The method for producing anti-rust coated steel material according to any one of claims 4 to 6, characterized in that the anti-rust coated steel material exhibits higher anti-rust performance than a painted steel material obtained by painting the paint on a surface of a steel material from which an oxide coating has been removed by blast pretreatment (rust removal degree Sa of 2.5 or more according to ISO 8501-1).
8. A method for improving rust-preventing performance, comprising directly painting an aqueous inorganic zinc-based paint on a surface of a steel material having an oxide film on its surface without removing the oxide film, thereby forming the oxide film and a coating film having rust-preventing performance on the surface of the steel material.
Citation Information
Patent Citations
Corrosion proof coated steel material, manufacturing method for the same, and corrosion proof method for coated steel material
JP2018103123A