Coating agent and resin member

A UV-activated coating agent using silsesquioxane and (meth)acrylate simplifies the formation of a durable, scratch-resistant film on resin surfaces by segregating inorganic and organic layers, addressing the complexity and cost issues of existing two-layer film processes.

JP2024157456AActive Publication Date: 2024-11-07TOYOTA INDUSTRIES CORP

Patent Information

Application Number
JP2023071841
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07
Estimated Expiration
2043-04-25

AI Technical Summary

Technical Problem

The formation of a two-layer film structure with a primer and hard coat layer on organic material surfaces is complex and costly, increasing the operational complexity and cost of forming a durable coating.

Method used

A coating agent comprising silsesquioxane and (meth)acrylate, which generates bases and radicals upon UV irradiation, allowing simultaneous sol-gel and radical polymerization, forming a coating film with a segregated inorganic surface layer and organic inner layer for enhanced adhesion and durability.

Benefits of technology

The coating agent simplifies the coating process by forming a durable, scratch-resistant film with excellent adhesion to resin substrates through UV irradiation, reducing complexity and cost while improving durability and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157456000001_ABST
    Figure 2024157456000001_ABST
Patent Text Reader

Abstract

To provide a coating agent which enables formation of a coating film that is excellent in adhesion to a base material composed of a resin and has high durability to scratches by simple work, and a resin member having a coating film formed from the coating agent.SOLUTION: A coating agent contains a film formation component containing silsesquioxane having a Ta structural unit and a TC structural unit represented by the following composition formulae, and (meth)acrylate (excluding silsesquioxane), and a film curing component. The molar ratio of the content of the Ta structural unit to the total of the content of the Ta structural unit and the content of the Tc structural unit in the silsesquioxane exceeds 0 mol% and 45 mol% or less. The weight average molecular weight of the silsesquioxane is 2,000 or more. Ta structural unit: (R1SiO3 / 2). Tc structural unit: (R2SiO3 / 2). In the formulae, R1 is a (meth)acryloyl group, and R2 is a monovalent hydrocarbon group.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating agent and a resin member. [Background technology]

[0002] Traditionally, inorganic materials such as steel, aluminum, and glass have been used for the components that make up vehicles such as automobiles and trains. In recent years, in order to reduce the weight of vehicles, there has been a trend to replace inorganic parts with organic parts such as plastics. However, while organic materials are lighter than inorganic materials, they are softer and more easily scratched.

[0003] Therefore, in order to improve the durability of parts made of organic materials against scratches, a technique for forming a hard coating on the surface of the part has been proposed. For example, Patent Document 1 describes a coated member having a resin base material, a primer layer formed on the surface of the resin base material, and a hard coat layer formed on the primer layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-240294 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when forming a coating having a two-layer structure of a primer layer and a hard coat layer, as in the coated member of Patent Document 1, it is necessary to sequentially carry out a step of applying a primer onto a resin substrate, a step of drying the primer to form a primer layer, a step of applying a coating agent onto the primer layer, and a step of curing the coating agent to form a hard coat layer. This makes the coating formation process complicated and leads to an increase in the cost required for the coating formation process.

[0006] The present invention has been made in view of the above background, and aims to provide a coating agent that can form, by simple operations, a coating film that has excellent adhesion to a resin substrate and is highly resistant to scratches, and a resin member having a coating film formed from this coating agent. [Means for solving the problem]

[0007] One aspect of the present invention is a silsesquioxane having a Ta structural unit represented by the following composition formula (1) and a Tc structural unit represented by the following composition formula (2), A film-forming component including a (meth)acrylate (excluding the silsesquioxane); A film-curing component configured to generate a base and a radical when irradiated with ultraviolet light; the molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the Tc structural unit in the silsesquioxane is more than 0 mol % and 45 mol % or less; The coating agent is characterized in that the weight average molecular weight of the silsesquioxane is 2,000 or more. (R 1 SiO 3 / 2 ) ···(1) (R 2 SiO 3 / 2 ) ···(2)

[0008] However, R in the composition formula (1) 1 is an acryloyl group or a methacryloyl group, and R in the composition formula (2) 2 is a monovalent hydrocarbon group.

[0009] Another aspect of the present invention is a substrate made of a resin, A resin member having a coating film formed on the substrate, The coating film is made of a cured product of the coating agent of the above embodiment, The coating film is on a resin member having a surface layer exposed on a surface of the resin member and an inner layer interposed between the surface layer and the base material, and the average concentration of Si atoms in the surface layer is higher than the average concentration of Si atoms in the inner layer. Effect of the Invention

[0010] The film-forming component in the coating agent includes the specific silsesquioxane and (meth)acrylate. The film-curing component in the coating agent is configured to generate a base and a radical when irradiated with ultraviolet light. When such a coating agent is irradiated with ultraviolet light, a base and a radical are generated from the film-curing component. The base generated from the film-curing component can condense the silsesquioxane by a sol-gel reaction. The radical generated from the film-curing component can polymerize the (meth)acrylate and the silsesquioxane by radical polymerization.

[0011] Therefore, by irradiating the coating agent with ultraviolet light, the sol-gel reaction and the radical polymerization can proceed in parallel. As a result, inorganic components derived from silsesquioxane are segregated on the surface of the coating film, improving durability against scratches, and organic components are segregated in the vicinity of the substrate in the coating film, improving adhesion to the substrate. In addition, the coating agent can form a coating film that has excellent adhesion to the substrate made of resin and high durability against scratches by a simple operation of applying the coating agent to the substrate and then irradiating ultraviolet light.

[0012] As described above, according to the above-mentioned aspects, it is possible to provide a coating agent capable of forming a coating film that has excellent adhesion to a substrate made of a resin and is highly resistant to scratches through a simple operation, and a resin member having a coating film formed from this coating agent. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a mapping image of Si atoms of a test piece produced using coating agent A1 in Experimental Example 1. [Diagram 2] FIG. 2 is a mapping image of Si atoms of the test piece produced using coating agent A2 in Experimental Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] (Coating agent) The coating agent has a film-forming component that forms a coating film by curing, and a film-hardening component for hardening the film-forming component. The composition of each component contained in the coating material will be described below.

[0015] [Film forming component] The film-forming components include a silsesquioxane and a (meth)acrylate.

[0016] Silsesquioxane The silsesquioxane contained in the film-forming component has a Ta structural unit represented by the following composition formula (1) and a Tc structural unit represented by the following composition formula (2). (R 1 SiO 3 / 2 ) ···(1) (R 2 SiO 3 / 2 ) ···(2)

[0017] However, R in the composition formula (1) 1 is an acryloyl group or a methacryloyl group, and R in the composition formula (2) 2 R in the composition formula (2) is a monovalent hydrocarbon group. 2 More specifically, R may be a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, etc. From the viewpoint of more reliably obtaining the above-mentioned effects, R 2is preferably a monovalent saturated hydrocarbon group, more preferably a saturated hydrocarbon group having 18 or less carbon atoms, further preferably a methyl group or an ethyl group, and particularly preferably a methyl group.

[0018] A hydroxyl group (-OH) or an alkoxy group (-OR) is bonded to a part of the Si atom in the silsesquioxane. Therefore, the silsesquioxane can be condensed by a base generated from the film hardening component to form an inorganic component in the coating film. In addition, the (meth)acryloyl group in the silsesquioxane can be polymerized together with the (meth)acryloyl group in the (meth)acrylate by a radical generated from the film hardening component.

[0019] The molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the Tc structural unit in the silsesquioxane is more than 0 mol% and 45 mol% or less. The weight average molecular weight of the silsesquioxane is 2,000 or more. By setting the content of the Ta structural unit in the silsesquioxane within the specific range and setting the weight average molecular weight of the silsesquioxane within the specific range, inorganic components derived from the silsesquioxane can be segregated on the surface of the coating film after curing. As a result, a surface layer mainly composed of inorganic components can be formed on the surface of the coating film, and an inner layer mainly composed of organic components can be formed between the surface layer and the substrate. The coating film having such a two-layer structure has excellent adhesion to the substrate made of resin and durability against scratches.

[0020] If the content of Ta structural units in the silsesquioxane is more than 45 mol% relative to the total content of Ta structural units and Tc structural units, the inorganic components are likely to be uniformly distributed throughout the entire coating film after curing, which may lead to a decrease in durability against scratches. In addition, in this case, wrinkles are likely to occur on the surface of the coating film, which may lead to a deterioration in the appearance of the resin member on which the coating film is formed. In order to avoid these problems, the content of Ta structural units in the silsesquioxane is set to 45 mol% or less relative to the total content of Ta structural units and Tc structural units.

[0021] The content of Ta structural unit in silsesquioxane is preferably 5 mol% or more, more preferably 10 mol% or more, even more preferably 15 mol% or more, particularly preferably 20 mol% or more, and most preferably 25 mol% or more, based on the total content of Ta structural unit and Tc structural unit. In this case, the wear resistance of the coating film can be further improved.

[0022] When forming the preferred range of the content of the Ta structural unit in the silsesquioxane, the upper limit and the lower limit of the content of the Ta structural unit described above can be combined arbitrarily.For example, the preferred range of the content of the Ta structural unit in the silsesquioxane may be 5 mol% or more and 45 mol% or less, 10 mol% or more and 45 mol% or less, 15 mol% or more and 45 mol% or less, 20 mol% or more and 45 mol% or less, or 25 mol% or more and 45 mol% or less, based on the total content of the Ta structural unit and the Tc structural unit.

[0023] If the weight-average molecular weight of silsesquioxane is less than 2,000, the inorganic components tend to be uniformly distributed throughout the entire coating film after curing, which may lead to a decrease in durability against scratches. In addition, in this case, the abrasion resistance of the coating film may also be decreased. By making the weight-average molecular weight of silsesquioxane 2,000 or more, preferably 2,500 or more, more preferably 3,000 or more, even more preferably 3,500 or more, and particularly preferably 4,000 or more, these problems can be easily avoided.

[0024] On the other hand, if the weight-average molecular weight of the silsesquioxane is too large, the viscosity of the coating agent will increase too much, which may lead to deterioration of the workability in applying the coating agent. In order to avoid such problems, the weight-average molecular weight of the silsesquioxane is preferably 25,000 or less, more preferably 20,000 or less, even more preferably 15,000 or less, and particularly preferably 13,000 or less.

[0025] When forming the preferred range of the weight-average molecular weight of silsesquioxane, the upper limit and the lower limit of the weight-average molecular weight of silsesquioxane described above can be combined arbitrarily.For example, the preferred range of the weight-average molecular weight of silsesquioxane may be 2,000 or more and 25,000 or less, 2,000 or more and 20,000 or less, 2,500 or more and 15,000 or less, 3,000 or more and 15,000 or less, 4,000 or more and 15,000 or less, or 4,000 or more and 13,000 or less.

[0026] The silsesquioxane may further contain a Q structural unit represented by the following composition formula (3): In this case, the molar ratio of the content of the Q structural unit to the total content of the Ta structural unit, the Tc structural unit, and the Q structural unit in the silsesquioxane is preferably more than 0 mol% and 25 mol% or less. (SiO 4 / 2 ) ···(3)

[0027] By introducing Q structural unit into silsesquioxane, the abrasion resistance of coating film can be further improved.From the viewpoint of improving the abrasion resistance of coating film, the content of Q structural unit in silsesquioxane is preferably 1 mol% or more, more preferably 2 mol% or more, and even more preferably 3 mol% or more, based on the total of the content of Ta structural unit, the content of Tc structural unit and the content of Q structural unit.

[0028] On the other hand, if the content of the Q structural unit in the silsesquioxane is excessively large, silsesquioxane aggregates are likely to occur in the coating film, which may lead to deterioration of the appearance of the coating film and deterioration of the abrasion resistance, etc. These problems can be easily avoided by setting the content of the Q structural unit in the silsesquioxane to preferably 25 mol % or less, more preferably 20 mol % or less, even more preferably 15 mol % or less, particularly preferably 10 mol % or less, and most preferably 8 mol % or less, based on the total content of the Ta structural unit, the Tc structural unit, and the Q structural unit.

[0029] When forming the preferred range of the content of the Q structural unit in the silsesquioxane, the upper limit and the lower limit of the content of the Q structural unit described above can be combined arbitrarily.For example, the preferred range of the content of the Q structural unit in the silsesquioxane may be 1 mol% or more and 20 mol% or less, 1 mol% or more and 15 mol% or less, 2 mol% or more and 10 mol% or less, 2 mol% or more and 8 mol% or less, or 3 mol% or more and 8 mol% or less, based on the total of the content of the Ta structural unit, the content of the Tc structural unit, and the content of the Q structural unit.

[0030] The content of silsesquioxane in the coating agent is preferably 30 parts by mass or more and 150 parts by mass or less, more preferably 40 parts by mass or more and 125 parts by mass or less, and even more preferably 50 parts by mass or more and 100 parts by mass or less, relative to 100 parts by mass of (meth)acrylate. In this case, the effect of improving hardness by the inorganic component and the effects of improving adhesion and flexibility by the organic component can be obtained in a better balance.

[0031] The silsesquioxane used in the coating agent can be obtained, for example, by condensing a plurality of alkoxysilanes including a (meth)acryloxyalkyltrialkoxysilane which becomes a Ta structural unit and an alkyltrialkoxysilane which becomes a Tc structural unit.

[0032] Examples of (meth)acryloxyalkyltrialkoxysilanes that are Ta structural units include 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-methacryloxypropyltriethoxysilane. These (meth)acryloxyalkyltrialkoxysilanes may be used alone to synthesize silsesquioxanes. In addition, two or more (meth)acryloxyalkyltrialkoxysilanes may be used in combination to synthesize silsesquioxanes.

[0033] As the alkyltrialkoxysilane that is the Tc structural unit, for example, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, isopropyltrimethoxysilane, n-butyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltriethoxysilane, isopropyltriethoxysilane, n-butyltriethoxysilane, etc. can be used. These alkyltrialkoxysilanes may be used alone to synthesize silsesquioxane. In addition, two or more kinds of alkyltrialkoxysilanes can be used in combination to synthesize silsesquioxane.

[0034] When introducing a Q structural unit into silsesquioxane, tetraalkoxysilane may be used to synthesize the silsesquioxane in addition to the above-mentioned trialkoxysilane. As the tetraalkoxysilane that becomes the Q structural unit, for example, tetramethoxysilane, tetraethoxysilane, etc. may be used. These tetraalkoxysilanes may be used alone to synthesize the silsesquioxane. In addition, two or more kinds of tetraalkoxysilanes may be used in combination to synthesize the silsesquioxane.

[0035] The reaction conditions for synthesizing silsesquioxane using alkoxysilane are not particularly limited, and alkoxysilane may be condensed by a known method.

[0036] (Meth)acrylates In this specification, (meth)acrylate refers to acrylic acid ester and methacrylic acid ester. However, the above-mentioned silsesquioxane is excluded from (meth)acrylate. The (meth)acrylate contained in the film-forming component can be radically polymerized by the radical generated from the film-curing component to form an organic component in the coating film. In addition, the (meth)acrylate can react with the (meth)acryloyl group contained in the silsesquioxane and bond to the silsesquioxane.

[0037] By incorporating a (meth)acrylate into the coating agent, an inner layer mainly composed of an organic component can be formed in the coating film, which can further improve the adhesion between the substrate and the coating film.

[0038] The film-forming component may contain one type of (meth)acrylate selected from the group consisting of acrylates and methacrylates, or may contain two or more types of (meth)acrylates. Examples of the (meth)acrylate contained in the film-forming component include (meth)acrylic acid monoesters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, 1-methylethyl (meth)acrylate, butyl (meth)acrylate, 2-methylpropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 2-hydroxypropyl (meth)acrylate; (meth)acrylic acid diesters such as 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and isocyanuric acid ethylene oxide-modified di(meth)acrylate; and (meth)acrylic acid esters having three or more (meth)acryloyl groups such as trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and isocyanuric acid ethylene oxide-modified tri(meth)acrylate. The (meth)acrylate may be a monomer of the above-mentioned compound, or may be an oligomer in which a plurality of monomers are polymerized in advance.

[0039] The (meth)acrylate preferably has three or more (meth)acryloyl groups per molecule. In this case, the structural unit derived from the (meth)acrylate and the structural unit derived from the silsesquioxane can be polymerized in a network shape. As a result, the hardness of the coating film can be increased, and the durability against scratches can be improved. In addition, from the viewpoint of further improving weather resistance, the (meth)acrylate preferably has an isocyanuric ring.

[0040] [Film curing component] The coating agent contains a film-curing component for promoting the curing reaction of the film-forming component. The film-curing component is configured to generate both a base and a radical when irradiated with ultraviolet light. For example, the film-curing component may contain a photobase generator configured to generate both a base and a radical when irradiated with ultraviolet light. In addition, the film-curing component may contain both a photobase generator configured to generate a base when irradiated with ultraviolet light, and a photoradical polymerization initiator configured to generate radicals when irradiated with ultraviolet light.

[0041] Photobase generator The photobase generator may be configured to generate at least a base when irradiated with ultraviolet light. That is, the photobase generator may be a compound that generates only a base when irradiated with ultraviolet light. The photobase generator may also be a compound that generates both a base and a radical when irradiated with ultraviolet light.

[0042] More specifically, as the photobase generator, a compound can be used that has an ultraviolet light absorbing portion that contains an aromatic ring such as a benzene ring, a naphthalene ring, a phenanthrene ring, an anthracene ring, an anthraquinone ring, a xanthene ring, or a thioxanthene ring in its molecular structure and absorbs ultraviolet light, and a base portion bonded to the ultraviolet light absorbing portion and that contains a structural unit that becomes a base when detached from the ultraviolet light absorbing portion, such as a primary to tertiary amino group, a quaternary ammonium cation, a carbamoyl group, a carbamate bond, an imino bond, or a nitrogen-containing heterocycle.

[0043] Examples of such compounds include 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidinium=n-butyltriphenylborate, (Z)-{[bis(dimethylamino)methylidene]amino}-N-cyclohexyl(cyclohexylamino)methaniminium=tetrakis(3-fluorophenyl)borate, 1,2-diisopropyl-3-[bis(dimethylamino)methylene]guanidinium=2-(3-benzoylphenyl)propionate, N,N-diethylcarbamate 9-anthrylmethyl, (E)-1-piperidino-3-(2-hydroxyphenyl)-2-propen-1-one, imidazole-1-carboxylic acid 1-carboxylate, and the like. -(anthraquinone-2-yl)ethyl, 4-(methacryloyloxy)piperidine-1-carboxylate (2-nitrophenyl)methyl, cyclohexylcarbamate 1,2-bis(4-methoxyphenyl)-2-oxoethyl, cyclohexylcarbamate 2-nitrobenzyl, 2-(9-oxoxoxanthen-2-yl)propionic acid 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 2-(9-oxoxoxanthen-2-yl)propionic acid 1,5-diazabicyclo[4.3.0]non-5-ene, 2-(9-oxoxoxanthen-2-yl)propionic acid 1,8-diazabicyclo[5.4.0]undec-7-ene, acetophenone O-benzoyloxime, 2-(piperidine-1-carbonyl)benzaldehyde, nifedipine, and the like. Among these, the photobase generator is preferably one or more compounds selected from the group consisting of 1,2-bis(4-methoxyphenyl)-2-oxoethyl cyclohexylcarbamate, 2-nitrobenzyl cyclohexylcarbamate, 1,5,7-triazabicyclo[4.4.0]dec-5-ene 2-(9-oxoxanthen-2-yl)propionic acid, 1,5-diazabicyclo[4.3.0]non-5-ene 2-(9-oxoxanthen-2-yl)propionic acid, and 1,8-diazabicyclo[5.4.0]undec-7-ene 2-(9-oxoxanthen-2-yl)propionic acid.

[0044] Photoradical polymerization initiator The film-hardening component may contain a photoradical polymerization initiator. The photoradical polymerization initiator is configured to generate radicals when the coating agent is irradiated with ultraviolet light. By blending the photoradical polymerization initiator in the coating agent, radical polymerization of the film-forming component can be advanced, and an organic component can be formed in the coating film.

[0045] Examples of the photoradical polymerization initiator that can be used include acetophenone-based compounds, benzophenone-based compounds, α-ketoester-based compounds, phosphine oxide-based compounds, benzoin compounds, titanocene-based compounds, acetophenone / benzophenone hybrid-based photoinitiators, oxime ester-based photoinitiators, and camphorquinone.

[0046] Examples of acetophenone compounds include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, diethoxyacetophenone, oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone} and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one.

[0047] Examples of the benzophenone compounds include benzophenone, 4-phenylbenzophenone, 2,4,6-trimethylbenzophenone, and 4-benzoyl-4'-methyldiphenyl sulfide, etc. Examples of the α-ketoester compounds include methylbenzoyl formate, 2-(2-oxo-2-phenylacetoxyethoxy)ethyl ester of oxyphenylacetic acid, and 2-(2-hydroxyethoxy)ethyl ester of oxyphenylacetic acid, etc.

[0048] Examples of phosphine oxide compounds include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. Examples of benzoin compounds include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether. Examples of acetophenone / benzophenone hybrid photoinitiators include 1-[4-(4-benzoylphenylsulfanyl)phenyl]-2-methyl-2-(4-methylphenylsulfinyl)propan-1-one. Examples of oxime ester photopolymerization initiators include 2-(O-benzoyloxime)-1-[4-(phenylthio)]-1,2-octanedione.

[0049] As the photoradical polymerization initiator, one compound selected from these compounds may be used, or two or more compounds may be used in combination.

[0050] The content of the film-hardening component in the coating agent and the ratio of the photobase generator to the photoradical polymerization initiator may be appropriately set according to the composition of the film-hardening component, etc. For example, the content of the film-hardening component in the coating agent may be appropriately set within the range of 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the film-forming component.

[0051] [Other additives] In addition to the film-forming component and the film-hardening component, the coating agent may contain additives known for coating agents within a range that does not impair the hardening of the coating agent.For example, the coating agent may contain additives for suppressing deterioration of the coating film, such as ultraviolet absorbers, radical scavengers, and hindered amine-based light stabilizers.By using these additives, it is expected to improve the weather resistance of the coating film.

[0052] The coating agent may contain, as an additive, a surface conditioner such as a leveling agent or a defoaming agent. By using these additives, the thickness of the coating agent can be made uniform when the coating agent is applied to a substrate. As a result, it is expected that the durability of the resin member provided with the coating film against scratches can be further improved.

[0053] (Resin material) The coating agent is applied onto a substrate made of a resin, and then cured to obtain a resin member. The resin member thus obtained is A base material made of resin; A coating film formed on the substrate, The coating film is composed of a cured product of the coating agent. The coating film includes a surface layer exposed on the surface of the resin member, An inner layer is interposed between the surface layer and the base material, The average concentration of Si atoms in the surface layer is higher than the average concentration of Si atoms in the inner layer.

[0054] The coating film is made of the cured product of the coating agent, and therefore has a surface layer mainly derived from silsesquioxane and an inner layer mainly derived from (meth)acrylate. Therefore, the resin member has excellent durability against scratches. In addition, the coating film has excellent adhesion to the substrate.

[0055] Since the coating film formed by curing the coating agent is transparent, for example, by applying the coating agent to the surface of a transparent window component, i.e., a component made of an inorganic material that serves as a substitute for window glass, a transparent window component that is lighter than glass made of an inorganic material can be obtained.

[0056] For example, the coating agent can be applied to the surface of a body panel to form a clear coat layer on the surface of the body panel. If necessary, a colorant such as a pigment can be added to the coating agent to color the coating film.

[0057] In the resin member, the resin constituting the substrate can be appropriately selected according to the application of the resin member. For example, when the resin member is used as a transparent window member, a polycarbonate resin can be used as the substrate. Polycarbonate resin is excellent in various properties required for a transparent window member, such as weather resistance, strength, and transparency. Therefore, by forming the transparent coating film on a substrate made of polycarbonate resin, a resin member suitable as a transparent window member can be obtained.

[0058] The resin member may include, for example, a preparation step of preparing a base material made of resin; A coating step of applying the coating agent onto a surface of a substrate; a curing step of irradiating the coating agent with ultraviolet light to form a coating film made of a cured product of the coating agent on the surface of the substrate; The present invention can be produced by a production method having the steps of:

[0059] In the production method, for applying the coating agent in the application step, an appropriate device can be selected and used from known application devices such as a spray coater, a flow coater, a spin coater, a dip coater, a bar coater, and an applicator depending on the desired film thickness, the shape of the equipment, and the like.

[0060] After the application step, a step of heating and drying the coating agent may be carried out as necessary.

[0061] For the irradiation of ultraviolet light in the curing step, an appropriate light source can be selected from known light sources capable of generating ultraviolet light, such as a mercury lamp, a metal halide lamp, a light-emitting diode, an excimer lamp, etc., depending on the absorption wavelength of the film curing component and the required light amount. In the curing step, ultraviolet light may be irradiated in an air atmosphere or in a nitrogen atmosphere. If necessary, the coating agent may be heated to promote the reaction while irradiating ultraviolet light.

[0062] After the curing step, a step of heating the coating film to promote curing may be carried out as necessary. EXAMPLES

[0063] An example of the coating agent will be described. The coating agent of this example includes a film-forming component including silsesquioxane having a Ta structural unit represented by the following composition formula (1) and a Tc structural unit represented by the following composition formula (2), (meth)acrylate (excluding the silsesquioxane), and a film-curing component configured to generate a base and a radical when irradiated with ultraviolet light. In addition, the molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the Tc structural unit in the silsesquioxane is more than 0 mol% and 45 mol% or less, and the weight-average molecular weight of the silsesquioxane is 2,000 or more. (R 1 SiO 3 / 2 ) ···(1) (R 2 SiO 3 / 2 ) ···(2)

[0064] However, R in the composition formula (1) 1 is an acryloyl group or a methacryloyl group, and R in the composition formula (2) 2 is a monovalent hydrocarbon group.

[0065] The silsesquioxanes used in this example are as follows:

[0066] Silsesquioxane Silsesquioxanes A1 to A12 shown in Tables 1 and 2 were synthesized by condensing a plurality of types of alkoxysilanes including alkyltrialkoxysilane and (meth)acryloxyalkyltrialkoxysilane by a known method. The (meth)acryloxyalkyltrialkoxysilane used in this example is specifically either methacryloxypropyltriethoxysilane (MAcSi(OEt)3) or methacryloxypropyltrimethoxysilane (MAcSi(OMe)3). The alkyltrialkoxysilane used in this example is specifically methyltriethoxysilane (MeSi(OEt)3). The tetraalkoxysilane used in this example is specifically tetraethoxysilane (Si(OEt)4).

[0067] (Meth)acryloxyalkyltrialkoxysilane becomes the Ta structural unit in silsesquioxane. Therefore, the "Ta structural unit" column in Tables 1 and 2 lists the molar ratio of the (meth)acryloxyalkyltrialkoxysilane used in the synthesis of silsesquioxane. Similarly, the "Tc structural unit" column in Tables 1 and 2 lists the molar ratio of the alkyltrialkoxysilane that becomes the Tc structural unit in silsesquioxane, and the "Q structural unit" column lists the molar ratio of the tetraalkoxysilane that becomes the Q structural unit in silsesquioxane. In addition, the "Ta / (Ta+Tc)" column in Table 1 lists the molar ratio of the content of the Ta structural unit to the total of the content of the Ta structural unit and the content of the Tc structural unit, and the "Q / (Ta+Tc+Q)" column lists the molar ratio of the content of the Q structural unit to the total of the content of the Ta structural unit, the content of the Tc structural unit, and the content of the Q structural unit.

[0068] In addition, the column "Weight average molecular weight" in Tables 1 and 2 lists the weight average molecular weight in terms of polyethylene obtained by gel permeation chromatography.

[0069] [Table 1]

[0070] [Table 2]

[0071] (Experimental Example 1) In this example, silsesquioxanes having different weight average molecular weights were used to prepare three types of coating agents (coating agents B1 to B3) shown in Table 3. The coating agent in this example has a film-forming component containing 100 parts by mass of (meth)acrylate and 75 parts by mass of silsesquioxane, a film-curing component containing 3 parts by mass of a photobase generator, and a solvent that dissolves the film-forming component and the film-curing component.

[0072] Specifically, the (meth)acrylate used in this example is a mixture containing ethylene oxide isocyanurate modified triacrylate ("M-315" manufactured by Toagosei Co., Ltd.). The silsesquioxane used in this example is any one of silsesquioxanes A1 to A3 as shown in Table 3. The photobase generator used in this example is 1,2-diisopropyl-3-[bis(dimethylamino)methylene]guanidium=2-(3-benzoylphenyl)propionate.

[0073] In this example, coating agents B1 to B3 shown in Table 3 were prepared by dissolving the above-mentioned compounds in a solvent.

[0074] Next, a 5 mm thick substrate made of polycarbonate resin was prepared, and one of the coating agents B1 to B3 was applied to the surface of the substrate using a bar coater. After the coating agent was applied to the substrate, the substrate was prebaked by heating it for 3 minutes in a hot air drying oven set at a temperature of 100°C.

[0075] After the pre-baking, a curing step was carried out in which the coating agent was irradiated with ultraviolet light to form a coating film made of a cured product of the coating agent on the surface of the substrate. In this example, the ultraviolet light was irradiated in a nitrogen atmosphere. A high-pressure mercury lamp was used as the source of the ultraviolet light. The illuminance of the ultraviolet light was 250 mW / cm. 2 The exposure dose was 2500 mJ / cm 2 It was decided.

[0076] After irradiation with ultraviolet light, the coating film was post-baked by heating it for 10 minutes using a hot air drying oven set at a temperature of 130°C. A test piece was obtained as described above. The obtained test piece was colorless and transparent. The thickness of the coating film formed on the substrate was about 50 μm.

[0077] Using the test pieces thus obtained, the layer structure, appearance and abrasion resistance of the coating film were evaluated.

[0078] [Layer structure of coating film] After exposing the cross section of the test piece, a mapping image of Si atoms in the cross section of the test piece was obtained by scanning secondary electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX). Then, based on the mapping image of Si atoms, it was determined whether the layer structure of the coating film was a layer-separated structure separated into a surface layer and an inner layer, or a single-layer structure consisting of a single layer. As an example, FIG. 1 shows a cross section of test piece 1a made using coating agent B1. FIG. 2 shows a cross section of test piece 1b made using coating agent B2. Note that the brightly displayed areas in FIG. 1 and FIG. 2 are areas with a high concentration of Si atoms.

[0079] As shown in FIG. 1, the coating film 2a made of the cured product of the coating agent B1 has a surface layer 21 that is exposed on the surface 10 of the test piece 1a and is displayed relatively brightly, and an inner layer 22 that is interposed between the surface layer 21 and the substrate 3 and is displayed darker than the surface layer 21. From FIG. 1, it can be seen that the surface layer 21 and the inner layer 22 are clearly separated in the coating film 2a. Furthermore, the surface layer 21 is displayed brighter than the inner layer 22, and the average concentration of Si atoms in the surface layer 21 is higher than the average concentration of Si atoms in the inner layer. From these results, it can be seen that the coating film 2a made of the cured product of the coating agent B1 has a structure separated into two layers, the surface layer 21 and the inner layer 22.

[0080] On the other hand, as shown in Fig. 2, the coating film 2b made of the cured product of coating agent B2 is composed of a single layer. Also, according to Fig. 2, the entire area from the boundary with the substrate 3 to the surface 10 is displayed with uniform brightness, and it can be seen that Si atoms are distributed throughout the coating film 2b. From these results, it can be seen that the coating film made of the cured product of coating agent B1 is composed of a single layer.

[0081] The layer structure thus determined based on the mapping image of Si atoms is shown in the “Layer structure” column of Table 3.

[0082] 〔exterior〕 The appearance of the coating film was evaluated visually. If the coating film was transparent and had a smooth surface, it was recorded as "Good" in the "Appearance" column of Table 3. If the coating film was opaque or had wrinkles or other irregularities on the surface, it was recorded as "Poor."

[0083] [Wear resistance] A Taber abrasion tester was used to perform an abrasion test on the coating film, and the abrasion resistance was evaluated based on the increase in haze value ΔH (unit: %) after the abrasion test. More specifically, the haze value of the test piece before the abrasion test was measured, and then the test piece was attached to the Taber abrasion tester. The abrasion test was performed by abrading the coating film of the test piece with an abrasion wheel. The abrasion wheel of the Taber abrasion tester in this example was CS-10F. The load in the abrasion test was 500 gf, and the number of rotations was 1000.

[0084] After the abrasion test was performed under the above conditions, the haze value of the test piece after the test was measured using a haze meter. The increase in haze value was calculated by subtracting the haze value of the test piece before the test from the haze value of the test piece after the test. The "Abrasion Resistance" column in Table 3 shows the increase in haze value ΔH (unit: %) for the coating film obtained using each coating agent.

[0085] [Table 3]

[0086] The film-forming components of coating agent B1 and coating agent B3 include (meth)acrylate and silsesquioxane. As shown in Table 3, the weight-average molecular weight of the silsesquioxane used in these coating agents and the molar ratio of the Ta structural unit content to the total of the Ta structural unit content and the Tc structural unit content are all within the above-mentioned specific range. Therefore, the coating film formed using coating agent B1 and coating agent B3 has a two-layer structure consisting of a surface layer and an inner layer, and is excellent in durability against scratches. In addition, the coating film formed using these coating agents has a good appearance and is also excellent in abrasion resistance.

[0087] On the other hand, the coating agent B2 uses silsesquioxane A2 whose weight average molecular weight is smaller than the specific range. Therefore, the coating film formed using the coating agent B2 is composed of a single layer in which the inorganic component is uniformly distributed, and has poor durability against scratches.

[0088] (Experimental Example 2) In this example, four types of coating agents (coating agents C1 to C4) shown in Table 4 were prepared using silsesquioxanes with different contents of Ta structural units. The specific configurations of coating agents C1 to C4 are the same as those of the coating agent in Experimental Example 1, except that one of silsesquioxanes A4 to A7 was used to prepare the coating agents as shown in Table 4, and that 2 parts by mass of a photoradical polymerization initiator was further contained in the film curing component. The photoradical polymerization initiators used in this example were Omnirad819 and Omnirad754 (both manufactured by IGM Resins BV). "Omnirad" is a registered trademark of IGM Group BV.

[0089] Using the coating agent thus prepared, the layer structure, appearance and abrasion resistance of the coating film were evaluated in the same manner as in Experimental Example 1. The results are shown in Table 4. The coating agent of this example is different from the coating agent of Experimental Example 1 in that the film curing component contains a photoradical polymerization initiator. In addition, the value of the increase in haze value ΔH obtained by the abrasion test is also greatly affected by the condition of the abrasion wheel used in the abrasion test. The condition of the abrasion wheel used in the abrasion test of this example is different from the condition of the abrasion wheel used in the abrasion test of Experimental Example 1. For these reasons, the value of the increase in haze value ΔH obtained in this example cannot be directly compared with the value of ΔH obtained in Experimental Example 1.

[0090] [Table 4]

[0091] As shown in Table 4, the weight average molecular weight of the silsesquioxane used in the coating agent C3 and the coating agent C4 and the molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the content of the Tc structural unit are all within the above-mentioned specific range. Therefore, the coating film formed using the coating agent C3 and the coating agent C4 has a structure consisting of two layers, a surface layer and an inner layer, and is excellent in durability against scratches. In addition, the coating film formed using these coating agents has a good appearance. Among these coating agents, the coating agent C3 has a moderately high content of the Ta structural unit, so that the wear resistance of the coating film can be further improved compared to the coating agent C4.

[0092] On the other hand, coating agents C1 and C2 use silsesquioxanes with an excessively high content of Ta structural units. Therefore, the coating films formed using these coating agents are composed of a single layer in which inorganic components are uniformly distributed, and have poor resistance to scratches. In addition, the coating films formed using these coating agents have wrinkles on the surface, resulting in poor appearance. In addition, the coating films formed using coating agents C1 and C2 have wrinkles on the surface, so the increase in haze value ΔH after the abrasion test cannot be compared with ΔH for coating films with smooth surfaces. Therefore, the "abrasion resistance" column for coating agents C1 and C2 states "unassessable."

[0093] (Experimental Example 3) In this example, silsesquioxanes having different contents of Q structural units were used to prepare three types of coating agents (coating agents D1 to D3) shown in Table 5. The specific configurations of coating agents D1 to D3 are the same as those of the coating agent in Experimental Example 1, except that one of silsesquioxanes A3, A8, and A11 was used to prepare the coating agents, as shown in Table 5.

[0094] Using the coating agent thus prepared, the layer structure, appearance, and abrasion resistance of the coating film were evaluated in the same manner as in Experimental Example 1. The results are shown in Table 5. Note that, for the same reason as in Experimental Example 2, the value of the increase in haze value ΔH obtained in this example cannot be directly compared with the values ​​of ΔH obtained in other Experimental Examples.

[0095] [Table 5]

[0096] As shown in Table 5, the weight average molecular weight of the silsesquioxane used in the coating agent D1 and the coating agent D3 and the molar ratio of the Ta structural unit content to the total of the Ta structural unit content and the Tc structural unit content are all within the specific range. Therefore, the coating film formed using the coating agent D1 and the coating agent D3 has a two-layer structure consisting of a surface layer and an inner layer, and is excellent in durability against scratches. In addition, the coating film formed using these coating agents has a good appearance. Among these coating agents, the coating agent D3 has a Q structural unit content within the specific range, so that the abrasion resistance of the coating film can be further improved compared to the coating agent D1 that does not contain the Q structural unit.

[0097] On the other hand, coating agent D2 uses silsesquioxane A8 with an excessively high content of Q structural units. Therefore, the coating film formed using coating agent D2 had an opaque appearance due to the formation of aggregates of inorganic components. In addition, since the coating film formed using coating agent D2 had aggregates of inorganic components, the increase in haze value ΔH of the coating film formed using coating agent D2 cannot be compared with the increase in haze value ΔH of a coating film with a smooth surface. Therefore, the "Abrasion resistance" column for coating agent D2 states "Unassessable."

[0098] (Experimental Example 4) In this example, silsesquioxanes containing Q structural units and differing in the amount of Ta structural units were used to prepare four types of coating agents (coating agents E1 to E4) shown in Table 6. The specific configurations of coating agents E1 to E4 are the same as those of the coating agent in Experimental Example 2, except that one of silsesquioxanes A9 to A12 was used to prepare the coating agents, as shown in Table 6.

[0099] Using the coating agent thus prepared, the layer structure, appearance, and abrasion resistance of the coating film were evaluated in the same manner as in Experimental Example 1. The results are shown in Table 6. Note that, for the same reason as in Experimental Example 2, the value of the increase in haze value ΔH obtained in this example cannot be directly compared with the values ​​of ΔH obtained in other Experimental Examples.

[0100] [Table 6]

[0101] As shown in Table 6, the weight average molecular weight of the silsesquioxane used in the coating agents E2 to E4 and the molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the Tc structural unit are all within the above-mentioned specific range. Therefore, the coating film formed using the coating agents E2 to E4 has a two-layer structure consisting of a surface layer and an inner layer, and is excellent in durability against scratches. In addition, the coating film formed using these coating agents has a good appearance. Among these coating agents, the coating agents E2 and E3 have a moderately high content of the Ta structural unit, and therefore the abrasion resistance of the coating film can be further improved compared to the coating agent E4 having a low content of the Ta structural unit.

[0102] On the other hand, coating agent E1 uses silsesquioxane with an excessively high content of Ta structural units. Therefore, the coating film formed using coating agent E1 is composed of a single layer and has poor resistance to scratches. In addition, the coating film formed using coating agent E1 has wrinkles on the surface, resulting in a poor appearance. Furthermore, since the coating film formed using coating agent E1 has wrinkles on the surface, the increase in haze value ΔH after the abrasion test cannot be compared with ΔH for a coating film with a smooth surface. Therefore, the "Abrasion Resistance" column for coating agent E1 states "Cannot be evaluated."

[0103] Although the embodiments of the coating agent and resin member according to the present invention have been described above based on Experimental Examples 1 to 4, the specific embodiments of the coating agent and resin member according to the present invention are not limited to those of the Experimental Examples, and the configurations can be appropriately changed within the scope of the present invention without departing from the spirit and scope of the present invention.

[0104] For example, the coating agent according to the present invention may take the following forms (1) to (8).

[0105] [1] A silsesquioxane having a Ta structural unit represented by the following composition formula (1) and a Tc structural unit represented by the following composition formula (2), A film-forming component including a (meth)acrylate (excluding the silsesquioxane); A film-curing component configured to generate a base and a radical when irradiated with ultraviolet light; the molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the Tc structural unit in the silsesquioxane is more than 0 mol % and 45 mol % or less; The coating agent, wherein the silsesquioxane has a weight average molecular weight of 2,000 or more. (R 1 SiO 3 / 2 ) ···(1) (R 2 SiO 3 / 2 ) ···(2) (However, R in the composition formula (1) 1 is an acryloyl group or a methacryloyl group, and R in the composition formula (2) 2 is a monovalent hydrocarbon group.

[0106] [2] The coating agent according to [1], wherein the molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the Tc structural unit in the silsesquioxane is 20 mol% or more and 45 mol% or less. [3] The coating agent according to [1] or [2], wherein the weight average molecular weight of the silsesquioxane is 2,000 or more and 15,000 or less.

[0107] [4] The coating agent according to any one of [1] to [3], wherein the silsesquioxane further contains a Q structural unit represented by the following composition formula (3), and a molar ratio of the content of the Q structural unit to the total content of the Ta structural unit, the Tc structural unit, and the Q structural unit in the silsesquioxane is more than 0 mol % and 25 mol % or less. (SiO 4 / 2 ) ···(3) [5] The coating agent according to any one of [1] to [4], wherein the content of the silsesquioxane is 30 parts by mass or more and 150 parts by mass or less per 100 parts by mass of the (meth)acrylate.

[0108] [6] The coating agent according to any one of [1] to [5], wherein the film-curing component contains a photobase generator configured to generate both a base and a radical when irradiated with ultraviolet light. [7] The coating agent according to any one of [1] to [5], wherein the film-curing component contains a photobase generator configured to be capable of generating a base when irradiated with ultraviolet light, and a photoradical polymerization initiator configured to be capable of generating radicals when irradiated with ultraviolet light. [8] The coating agent according to any one of [1] to [7], wherein the (meth)acrylate has an isocyanuric ring.

[0109] Moreover, the resin member according to the present invention may have the following aspect [9].

[0110] [9] A substrate made of a resin; A resin member having a coating film formed on the substrate, The coating film is made of a cured product of the coating agent according to any one of [1] to [8], The coating film has a surface layer exposed on a surface of the resin member, An inner layer is interposed between the surface layer and the base material, The resin member, wherein an average concentration of Si atoms in the surface layer is higher than an average concentration of Si atoms in the inner layer. [Explanation of symbols]

[0111] 1a Test piece 2a Coating film 21 Surface layer 22 Inner layer 3 Base material

Claims

1. A silsesquioxane having a Ta structural unit represented by the following composition formula (1) and a Tc structural unit represented by the following composition formula (2); a film-forming component comprising a (meth)acrylate (excluding the silsesquioxane); A film-curing component configured to generate a base and a radical when irradiated with ultraviolet light; the molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the Tc structural unit in the silsesquioxane is more than 0 mol % and 45 mol % or less; The coating agent, wherein the silsesquioxane has a weight average molecular weight of 2,000 or more. (R 1 SiO 3/2 ) ... (1) (R 2 SiO 3/2 ) ... (2) (However, R in the composition formula (1) 1 is an acryloyl group or a methacryloyl group, and R in the composition formula (2) 2 is a monovalent hydrocarbon group.

2. 2. The coating agent according to claim 1, wherein a molar ratio of the content of the Ta structural unit to the total content of the Ta structural unit and the Tc structural unit in the silsesquioxane is 20 mol % or more and 45 mol % or less.

3. 2. The coating agent according to claim 1, wherein the weight average molecular weight of the silsesquioxane is 2,000 or more and 15,000 or less.

4. The silsesquioxane further contains a Q structural unit represented by the following composition formula (3), and a molar ratio of the content of the Q structural unit to the total content of the Ta structural unit, the Tc structural unit, and the Q structural unit in the silsesquioxane is more than 0 mol% and 25 mol% or less. (SiO 4/2 ) ... (3)

5. The coating agent according to claim 1, wherein the content of the silsesquioxane is 30 parts by mass or more and 150 parts by mass or less with respect to 100 parts by mass of the (meth)acrylate.

6. The coating agent according to claim 1 , wherein the film-hardening component comprises a photobase generator configured to generate both a base and a radical when irradiated with ultraviolet light.

7. 2. The coating agent according to claim 1, wherein the film-hardening component comprises: a photobase generator configured to be capable of generating a base when irradiated with ultraviolet light; and a photoradical polymerization initiator configured to be capable of generating radicals when irradiated with ultraviolet light.

8. The coating agent according to claim 1 , wherein the (meth)acrylate has an isocyanuric ring.

9. A base material made of resin; A resin member having a coating film formed on the substrate, The coating film is made of a cured product of the coating agent according to any one of claims 1 to 8, The coating film has a surface layer exposed on a surface of the resin member, An inner layer is interposed between the surface layer and the base material, The resin member, wherein an average concentration of Si atoms in the surface layer is higher than an average concentration of Si atoms in the inner layer.

Citation Information

Patent Citations

  • Ultraviolet-curable composition

    JP1991281616A

  • Siloxane polymer composition, cured film and method for forming cured film

    JP2012068417A

  • Colorant dispersion liquid, photosensitive resin composition, cured product, organic el element, patterning method, and method for producing photosensitive resin composition

    JP2018070695A

  • organopolysiloxane

    JP2018127619A

  • Negative photosensitive resin composition and cured film

    WO2018216570A1

Cited By

  • Coating agent and resin member

    WO2026196759A1