Method of preparing modified propylene-based polymer and modified propylene-based polymer prepared thereby
The method of modifying propylene polymers using a radical initiator in a solution state addresses the issue of main chain scission and high xylene solubles by achieving uniform long chain branching and improved properties at lower temperatures.
Patent Information
- Application Number
- JP2023184905
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2023-10-27
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional methods for introducing long chain branches into propylene polymers often result in main chain scission due to high reaction temperatures, leading to deterioration of physical properties and high xylene solubles content.
A method involving a radical initiator in a solution state is used to modify propylene polymers by reacting a mixture of propylene polymer, diene compound, and radical initiator in a solvent, performed at lower temperatures to achieve uniform long chain branching and reduce xylene solubles content.
The modified propylene polymer exhibits improved processability, productivity, and physical properties with reduced xylene solubles, resulting in enhanced melt strength and rheological properties.
Smart Images

Figure 2024157507000001 
Figure 2024157507000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a modified propylene-based polymer and the modified propylene-based polymer produced thereby. [Background technology]
[0002] Propylene polymer (Polypropylene, PP) is composed only of carbon and hydrogen and has low density, making it easy to reproduce and providing excellent chemical resistance and high tensile modulus at a relatively low cost. In order to further improve the physical properties of propylene polymer, a method has been used to introduce long chain branching (LCB) into the main chain of the polymer.
[0003] As a technique for adding long chain branches to the propylene main chain, methods such as solid-state reaction, reactive extrusion, electron beam irradiation, etc. have been reported. However, the conventional technique using reactive extrusion has a problem that the main chain often breaks due to the relatively high reaction temperature, resulting in deterioration of physical properties. Summary of the Invention [Problem to be solved by the invention]
[0004] An object of one embodiment is to provide a method for modifying a propylene-based polymer using a radical initiator in a solution state, and a modified propylene-based polymer produced thereby.
[0005] Another embodiment aims to provide a modified propylene-based polymer having reduced xylene solubles content.
[0006] Another embodiment aims to provide a foaming composition including the modified propylene-based polymer according to the above embodiment. [Means for solving the problem]
[0007] One embodiment provides a method for producing a modified propylene-based polymer, the method including the steps of: preparing a mixture by adding a propylene-based polymer, a diene compound, and a radical initiator to a solvent; and subjecting the mixture to a radical reaction.
[0008] Another embodiment provides a modified propylene-based polymer produced by the method according to the above embodiment.
[0009] Another embodiment provides a modified propylene-based polymer having a xylene solubles content adjusted to 2.0% by weight or less.
[0010] Another embodiment provides a foaming composition including the modified propylene-based polymer produced by the method according to the above embodiment. Effect of the Invention
[0011] The present disclosure relates to a method for producing a modified propylene-based polymer using a radical initiator in a solution state, and a modified propylene-based polymer produced by the method. The modified propylene-based polymer produced by the method according to one embodiment has a low content of xylene flammables and uniformly contains long chain branched (LCB), thereby improving processability and productivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The embodiments described herein may be modified into various other forms, and therefore the technology according to one embodiment is not limited to the embodiments described below. Furthermore, throughout this specification, "including," "comprising," "including," or "having" a certain element means that it can further include other elements, but does not exclude other elements, materials, or processes not further recited, unless otherwise specified to the contrary.
[0013] Numerical ranges used herein include lower and upper limits and all values within the range, increments logically derived from the form and width of the range defined, all values that are doubly limited, and all possible combinations of upper and lower limits of numerical ranges limited in different forms. As an example, if the content of a composition is limited to 10-80% or 20-50%, the numerical ranges of 10-50% or 50-80% should also be interpreted as being described herein. Unless otherwise specified in the present specification, values outside the numerical range that may occur due to experimental error or rounding of values are also included in the defined numerical range.
[0014] Hereinafter, unless otherwise defined in this specification, "about" can be considered to mean a value within 30%, 25%, 20%, 15%, 10% or 5% of the stated value.
[0015] Unless otherwise defined herein, a "polymer" refers to a molecule of relatively high molecular weight, whose structure may include multiple repeats of units derived from a molecule of lower molecular weight. In one embodiment, the polymer may be an alternating copolymer, a block copolymer, a random copolymer, a graft copolymer, a gradient copolymer, a branched copolymer, a crosslinked copolymer, or any of the above copolymers (e.g., a polymer containing one or more monomers). In another embodiment, the polymer may be a homopolymer (e.g., a polymer containing one monomer).
[0016] As used herein, a "propylene-based polymer" is a polymer polymerized from a monomer containing propylene. The monomer used for producing a propylene-based polymer according to the present invention necessarily contains propylene, but there is no limitation on the type of other monomers that can be used. For example, the propylene-based polymer may be a polymer polymerized from a monomer containing propylene and an additional aliphatic unsaturated hydrocarbon (olefin, diene), etc. Meanwhile, the term "propylene-based polymer" as used herein may also be used as "propylene polymer" at the discretion of a person skilled in the art.
[0017] An embodiment provides a method for producing a modified propylene-based polymer (or a method for modifying a propylene-based polymer) using a radical reaction in a solution state. The method for producing a modified propylene-based polymer provided in an embodiment is performed at a lower temperature than a conventional method using reactive extrusion, thereby improving the uniformity of the reaction. The modified propylene-based polymer produced by the method according to an embodiment may be a propylene polymer (long chain branched polypropylene, LCBPP) having uniform long long chain branches. The modified propylene-based polymer according to an embodiment has a plurality of types of long chain branches evenly distributed and has a low content of xylene solubles, and therefore has excellent physical properties such as high melt strength, processability, and productivity.
[0018] Hereinafter, a method for producing a modified propylene-based polymer according to one embodiment and a modified propylene-based polymer produced therefrom will be specifically described.
[0019] One embodiment provides a method for producing a modified propylene-based polymer, the method including: preparing a mixture by adding a propylene-based polymer, a diene compound, and a radical initiator to a solvent; and subjecting the mixture to a radical reaction.
[0020] In one embodiment, the step of preparing the mixture may specifically include a step of dissolving a propylene polymer in a solvent, and a step of adding a diene compound and a radical initiator to the solution in which the propylene polymer is dissolved, and then mixing the resulting mixture.
[0021] In one embodiment, the step of preparing the mixture and / or the step of carrying out the radical reaction can be carried out at a temperature of 80 to 200° C., 80 to 180° C., 100 to 150° C., or about 130° C. The above temperature ranges are merely examples, and the present invention is not necessarily limited to these ranges.
[0022] In one embodiment, the step of preparing the mixture and the step of carrying out the radical reaction can be carried out under the same temperature conditions. Specifically, the step of dissolving the propylene polymer in a solvent, the step of adding the diene compound and the radical initiator and then mixing them, and the step of carrying out the radical reaction can all be carried out under the same conditions.
[0023] The process for producing a modified propylene-based polymer according to one embodiment can be carried out at a lower temperature than the conventional process for producing a modified propylene-based polymer by reactive extrusion, improving the economics of the reaction.
[0024] In one embodiment, the propylene polymer (i.e., the polymer before modification) may be an isotactic propylene polymer (iPP), a syndiotactic propylene polymer (sPP), or an atactic propylene polymer (aPP). Without wishing to be bound by any particular theory, an isotactic propylene polymer may be more suitable due to its better crystallinity. The isotactic propylene polymer may be produced using a Zigler-Natta catalyst or a metallocene catalyst.
[0025] In one embodiment, the Ziegler-Natta catalyst (or Ziegler-Natta type catalyst) may include a transition metal compound containing an element of Group 4, Group 5, or Group 6 of the periodic table, and an organometallic compound containing an element of Group 13 of the periodic table. The transition metal compound may be a compound containing at least one of magnesium, titanium, a halogen element, and an internal electron donor as a main catalyst of the Ziegler-Natta catalyst. The organometallic compound may be an organoaluminum compound as a co-catalyst of the Ziegler-Natta catalyst, and may include at least one of trialkylaluminum, dialkylaluminum halide, alkylaluminum dihalide, aluminum dialkyl hydride, and alkylaluminum sesquihalide. Specifically, for example, the organoaluminum compound may be Al(C 2 H 5 ) 3 , Al(C 2 H 5 ) 2 H, Al(C 3 H 7 ) 3 , Al(C 3 H 7 ) 2 H, Al(iC 4 H 9 ) 2 H, Al(C 8 H 17 ) 3 , Al(C 12 H 25 ) 3 , Al(C 2 H 5 )(C 12 H 25 ) 2 , Al(iC 4 H 9 )(C 12 H 25 ) 2 , Al(iC 4 H 9 ) 2 H, Al(iC 4 H 9 ) 3 , (C 2 H 5 ) 2 AlCl, (iC3 H 9 ) 2 AlCl, or (C 2 H 5 ) 3 Al 2 Cl 3 It may be also possible.
[0026] In addition, a recycled propylene polymer can also be used as the propylene polymer before modification that is fed in one embodiment.
[0027] In one embodiment, the propylene polymer is homo or random, specifically, homoisotactic propylene polymer or random isotactic propylene polymer. The homo type has inherent mobility, and the random type has a low melting point. Meanwhile, the homo or random propylene polymer has a problem that it is difficult to use commercially because the xylene soluble matter (which can be understood as the content of isotactic propylene polymer contained in isotactic polymer) is usually more than 5%. In response to this, one embodiment provides a method for modifying propylene polymer that can effectively reduce the xylene content.
[0028] In one embodiment, the solvent may contain at least one of an aliphatic hydrocarbon compound and an aromatic hydrocarbon compound as a solvent for dissolving the propylene polymer. For example, the aliphatic hydrocarbon compound may be 3-20 Aliphatic hydrocarbon compounds, C 5-15 Aliphatic hydrocarbon compounds of C 5-10 The aliphatic hydrocarbon compound may be an aliphatic hydrocarbon compound having a structure such as butane, pentane, hexane, heptane, octane, nonane, decane, cyclopentane, cyclohexane, C 1-5 Cyclopentane substituted with an alkyl group of C 1-5The aromatic hydrocarbon compound may be, for example, a cyclohexane having an alkyl group substituted with C 5-20 Aromatic hydrocarbon compounds, C 6-20 Aromatic hydrocarbon compounds, C 6-15 Aromatic hydrocarbon compounds, C 6-10 Aromatic hydrocarbon compounds of C 6-8 The aromatic hydrocarbon compound may be any of the aromatic hydrocarbon compounds, which may be substituted or unsubstituted. Specifically, the aromatic hydrocarbon compound may be benzene, toluene, xylene, cresol, anisole, catechol, naphthalene, styrene, aniline, and xylenol.
[0029] In one embodiment, the diene compound may be added in an amount of 0.1 to 20.0 wt%, 0.5 to 15.0 wt%, 1.0 to 20.0 wt%, 1.0 to 15.0 wt%, 2.0 to 15.0 wt%, 3.0 to 15.0 wt%, 3.0 to 13.0 wt%, 5.0 to 20.0 wt%, 5.0 to 15.0 wt%, or 5.0 to 10.0 wt%, based on the weight of the added propylene polymer (i.e., when the weight of the added propylene polymer is 100 wt%). However, the weight ranges are only examples and are not necessarily limited thereto.
[0030] In one embodiment, the radical initiator may be added in an amount of 0.1 to 5.0 wt%, 0.1 to 3.0 wt%, 0.1 to 2.0 wt%, 0.1 to 1.0 wt%, 0.3 to 1.2 wt%, or about 0.5 wt% based on the weight of the added propylene polymer, although the weight ranges are merely examples and are not necessarily limited thereto.
[0031] In one embodiment, the weight ratio of the radical initiator to the diene compound may be 1:1 to 1:50, 1:1 to 1:30, 1:1 to 1:20, 1:2 to 1:20, 1:5 to 1:20, 1:8 to 1:20, or 1:10 to 1:20. However, the weight ratio is only an example and is not necessarily limited thereto.
[0032] The diene compound according to one embodiment is not particularly limited as long as it is a compound containing two double bonds, and may be, for example, a compound containing 2 to 20 carbon atoms, 5 to 10 carbon atoms, 5 to 15 carbon atoms, or 5 to 10 carbon atoms. Specifically, for example, the diene compound may contain one or more of 1,3-butadiene, 1,4-pentadiene, 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, 1,8-nonadiene, 1,9-decadiene, 1,10-undecadiene, 1,11-dodecadiene, 1,12-tridecadiene, 1,13-tetradecadiene, chloroprene, cyclohexadiene, cyclopentadiene, 2,3-dimethylbutadiene, isoprene, and o-divinylbenzene, m-divinylbenzene, and p-divinylbenzene. As an example, the divinylbenzene (DVB) used in the following examples is a mixture of m-DVB and p-DVB.
[0033] The radical initiator according to an embodiment may be any known radical initiator without limitation, and may include, for example, any one or more selected from the group consisting of acyl peroxides, alkyl peroxides, hydroperoxides, peresters, and peroxycarbonates.
[0034] The acyl peroxide may be, for example, benzoyl peroxide, 4-chlorobenzoyl peroxide, 3-methoxybenzoyl peroxide, and / or methylbenzoyl peroxide.
[0035] The alkyl peroxide may be, for example, allyl t-butyl peroxide, 2,2-bis(t-butylperoxybutane), 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(t-butylperoxy)valerate, diisopropylaminomethyl-t-amyl peroxide, dimethylaminomethyl-t-amyl peroxide, diethylaminomethyl-t-butyl peroxide, dimethylaminomethyl-t-butyl peroxide, 1,1-di(t-amylperoxy)cyclohexane, t-amyl peroxide, t-butylcumyl peroxide, t-butyl peroxide and / or 1-hydroxybutyl n-butyl peroxide.
[0036] Peresters and peroxycarbonates include, for example, butyl peracetate, cumyl peracetate, cumyl perpionate, cyclohexyl peracetate, di-t-butyl peradipate, di-t-butyl perazelate, di-t-butyl perglutarate, di-t-butyl persalate, di-t-butyl persebacate, 4-nitrocumyl perpropionate, 1-phenylethyl peroxybenzoate, 1-phenylethyl 4-nitro-peroxybenzoate, t-butyl bicyclo-(2,2,1)heptane peroxycarboxylate, t-butyl-4-carbomethoxyperoxybutyrate, t-butyl cyclobutane peroxycarboxylate, t-butyl cyclohexyl peroxycarboxylate, t-butyl cyclopentyl peroxycarboxylate, t-butyl cyclopropane peroxycarboxylate, t-butyl dimethyl percinnamate, t-butyl- The peroxybenzoate may be 2-(2,2-diphenylvinyl)peroxybenzoate, t-butyl-4-methoxyperoxybenzoate, t-butylperoxybenzoate, t-butylperoxyisopropylcarbonate, t-butylpertoluate, t-butyl-1-phenylcyclopropylperoxycarboxylate, t-butyl-2-propylperpenten-2-oate, t-butyl-1-methylcyclopropylperoxycarboxylate, t-butyl-4-nitrophenylperacetate, t-butylnitrophenylperoxycarbamate, t-butyl-N-succinimideperoxycarboxylate, t-butylpercrotonate, t-butylpermalic acid, t-butylpermethacrylate, t-butylperoctoate, t-butylperoxyisopropylcarbonate, t-butylperisobutyrate, t-butylperacrylate and / or t-butylperpropionate.
[0037] The modified propylene-based polymer produced by the method according to an embodiment may contain xylene solubles (XS) of 2.0 wt% or less, 1.5 wt% or less, 1.0 wt% or less, 0.8 wt% or less, 0.7 wt% or less, 0.5 wt% or less, 0.3 wt% or less, or 0.1 wt% or less. The lower limit may be, for example, 0.1 wt%, 0.05 wt%, or 0.01 wt%. The xylene solubles refer to the portion of the components contained in the polymer that is soluble in cold xylene, and can be measured by dissolving the polymer in xylene and then determining the insoluble portion (residue) from the cooled solution. Specifically, the xylene solubles can be calculated by the following Equation 1.
[0038] [Formula 1] Xylene solubles (XS, % (wt%)) = {(m 0 -m 1 ) / m 0}×100
[0039] In the above formula 1, m 0 is the initial weight of the polymer (g), m 1 is the weight of the residue (g). The xylene solubles contain polymer chains with low stereoregularity and are an indicator of the amount of non-crystalline regions.
[0040] The modified propylene-based polymer produced by the production method according to one embodiment has significantly reduced xylene solubles, and thus has excellent processability and productivity.
[0041] Another embodiment provides a modified propylene-based polymer produced by the method for producing a modified propylene-based polymer according to the above embodiment.
[0042] The modified propylene-based polymer according to one embodiment may be a multi-branched propylene-based polymer, i.e., the propylene backbone (main chain) may have multiple side chains, some of which may themselves have additional side chains.
[0043] In addition, the modified propylene-based polymer according to an embodiment may be a propylene-based polymer having long chain branches (long chain branched polypropylene (LCBPP)). The modified polymer according to an embodiment may have excellent rheological properties such as flow, shear, and extension due to the long chain branches.
[0044] When the modified propylene-based polymer according to an embodiment is analyzed by gel permeation chromatography (GPC), it can have a molecular weight distribution that is equal to or wider than that of commercially available LCBPP.
[0045] That is, the modified propylene-based polymers according to one embodiment are not separated from each other and are homogeneously distributed.
[0046] The modified propylene-based polymer according to one embodiment may have a xylene solubles (XS) calculated according to Equation 1 of 2.0 wt% or less, 1.5 wt% or less, 1.0 wt% or less, 0.8 wt% or less, 0.7 wt% or less, 0.5 wt% or less, 0.3 wt% or less, or 0.1 wt% or less.
[0047] The modified propylene-based polymer according to one embodiment has high melt strength and can be used in a variety of applications, such as blown film, extrusion coating, foam extrusion, and blow-molding. In addition, the high melt strength allows for greatly improved processability and productivity, which is useful, and the increased melt strength at high temperatures allows for foam molding at high temperatures. In addition, the modified propylene-based polymer can be recycled, making it useful for use as an environmentally friendly lightweight material.
[0048] The modified propylene-based polymer according to an embodiment has high melt strength and excellent physical properties, and therefore can be used to manufacture foamed articles such as laminated and non-laminated sheets, beads, and release agents. In addition, the modified propylene-based polymer according to an embodiment can be used to form articles by thermoforming, injection molding, blow molding, extrusion coating, or melting. In addition, the modified propylene-based polymer according to an embodiment can be effectively applied to various fields such as adhesives, films, and packaging materials.
[0049] Another embodiment provides a modified propylene-based polymer having a xylene solubles content of 2.0 wt.% or less.
[0050] The modified propylene-based polymer according to the embodiment has excellent physical properties, specifically, excellent productivity and processability, since the xylene solubles content (calculated by the above mathematical formula 1) is significantly reduced.
[0051] The modified propylene-based polymer according to one embodiment may have a xylene solubles content of 1.5% by weight or less, 1.0% by weight or less, 0.8% by weight or less, 0.7% by weight or less, 0.5% by weight or less, 0.3% by weight or less, or 0.1% by weight or less, where the lower limit may be, for example, 0.01% by weight, 0.05% by weight, or 0.01% by weight.
[0052] The modified propylene polymer according to one embodiment may have a crystallization temperature (Tc) of 110° C. to 124° C., or 110° C. to 120° C., or 110° C. to 118° C., as measured under DSC measurement conditions in the following Experimental Examples.
[0053] The modified propylene-based polymer according to one embodiment may have a number average molecular weight (Mn) of 60,000 g / mol to 110,000 g / mol, or 70,000 g / mol to 110,000 g / mol, as measured under GPC measurement conditions in the following experimental examples.
[0054] According to one embodiment, the modified propylene-based polymer has a melting point of 1.0 s at 180° C. -1 The strain hardening index (SHI) measured in a range of a Hencky rate (dε / dt) of 0.2 or more, 0.3 or more, 0.5 or more, 1.0 or more, 1.5 or more, 1.8 or more, or 1.9 or more, may be 0.2 or more, 0.3 or more, 0.5 or more, 1.0 or more, 1.5 or more, 1.8 or more, or 1.9 or more. The upper limit may be, for example, 5.0, 4.0, 3.0, or 2.74. The strain hardening index is defined by the slope value (c2) of the common logarithm (log(ε)) function of the Hencky strain defined by the following mathematical formula 2.
[0055] [Formula 2] η E =c1×ε c2
[0056] In the above formula 2, η E is the elongation viscosity (Pa-s), ε is the Hencky strain, and c1 and c2 are parameters.
[0057] The modified propylene-based polymer according to an embodiment exhibits an excellent strain hardening index comparable to that of existing developed products, which indicates that the modified propylene-based polymer according to an embodiment contains various long chain branches. Therefore, the propylene-based polymer according to an embodiment can effectively maintain a stable state during processing.
[0058] The modified propylene-based polymer according to one embodiment is produced by copolymerizing a diene copolymer, and the above description of the diene compound may be applied thereto.
[0059] Another embodiment provides a foaming composition including the modified propylene-based polymer according to the above embodiment, and a foamed molded article formed using the same, and the use of the molded article is not particularly limited.
[0060] Examples and experimental examples are specifically illustrated below. However, the examples and experimental examples described below are merely illustrative of a part of one embodiment, and therefore the technology described in this specification should not be construed as being limited thereto.
[0061] <Example 1> In a 500mL 3-neck round bottom flask, 15g of propylene polymer (isotacic polypropylene, iPP) and a magnetic bar were placed, and 300mL of n-octane solvent was added, followed by refluxing with nitrogen gas at 120°C. After the propylene polymer was completely dissolved, 1.0wt% of octadiene and 1.0wt% of DVB (Sigma-Aldrich) were added as diene monomers (diene compounds), and 0.5wt% of TBPB as a radical initiator, and the mixture was stirred at the same temperature for 1 hour. After cooling to room temperature, the mixture was washed with acetone, filtered and dried to obtain a modified propylene polymer.
[0062] <Examples 2 to 7> The propylene-based polymer was modified by the method of Example 1, except that the solvent, radical initiator and diene compound shown in Table 1 below were used.
[0063] [Table 1] (The weight percent is based on the weight of the propylene polymer.) TBPB: t-Butyl peroxybenzoate LP: Lauroyl peroxide DVB: Divinylbenzene
[0064] <Comparative Example 1> The unmodified propylene polymer (isotacic polypropylene, iPP) used in Example 1 was prepared.
[0065] <Comparative Example 2> A high melt strength polypropylene (HMSPP), WB140HMS (Borealis), was prepared. WB140HMS was a product produced by reactive extrusion.
[0066] <Experimental Example 1> Xylene solubles (XS) content measurement The xylene solubles content was measured using Crystex. Specifically, the modified propylene polymer was dissolved in xylene, and the insoluble portion (residue) was determined from the cooled solution. The xylene solubles content was calculated using the following formula 1. The results are shown in Table 2 below.
[0067] [Formula 1] Xylene solubles (XS, % (wt%)) = {(m 0 -m 1 ) / m 0}×100
[0068] In the above formula 1, m 0 is the initial weight of the polymer (g), m 1 is the weight of the residue (g).
[0069] <Experimental Example 2> DSC (differential scanning calorimetry) analysis The crystallization temperature (Tc) and melting temperature (Tm) of the polymer were measured using differential scanning calorimetry (DSC). Polymer specimens for DSC analysis were prepared by pressing with a crimper press and then analyzed at temperatures from -50°C to 200°C at a heating rate of 10°C / min. The results are shown in Table 2 below.
[0070] <Experimental Example 3> GPC (Gel permeation chromatography) analysis The molecular weight distribution of the polymer was confirmed using gel permeation chromatography (GPC), and the results are shown in Table 2 below. The GPC analysis was performed using a Polymer Char GPC-IR device (standard sample: Easical PS1 Polystyrene, temperature: 160°C, solvent: 1,2,4-trichlorobenzene, viscosity constant: K, α of polypropylene). Approximately 1.5 mg of the polymer sample was placed in a 1.25 mL high-temperature GPC vial, and 1 mL of 1,2,4-trichlorobenzene (w / BHT) was added, and the polymer was dissolved at 150°C with stirring for more than 3 hours before being used for analysis.
[0071] <Experimental Example 4> Elongation viscosity analysis To confirm the strain hardening properties of the polymer, the extensional viscosity was measured as a function of time. The extensional viscosity analysis was performed using a TA Strain-Controlled Rheometer (ARES) at 180°C and a strain rate of 1.0 s. -1 The polymer was prepared into a test piece having a thickness of 8 mm and a width of 10.2 mm and the final Henky strain was set to 3.5.
[0072] In order to numerically confirm the strain hardening property of the polymer, the strain hardening index (SHI) defined as the gradient value (c2) of the common logarithm (log(ε)) function of the Hencky strain (ε) defined by the following Equation 2 was calculated, and the results are shown in Table 2 below.
[0073] [Formula 2] η E =c1×ε c2
[0074] In this case, η E is 1.0s at 180℃ -1is the elongation viscosity (Pa-s) measured at a Hencky rate (dε / dt) of 1000 Pa for a Hencky strain (ε) range of 1 to 3, where c1 and c2 are parameters. The parameters c1 and c2 are the common logarithm of the Hencky strain (log(η E ) = c2 × log(ε) + log(c1)) and validated by linear fitting the data using the least squares method.
[0075] [Table 2]
[0076] Through the above experiments, the propylene-based polymers modified according to the methods of the embodiments all had a xylene solubles content of about 1.0 wt% or less, which was significantly lower than that of the comparative examples. This confirmed that the polymer modification according to the embodiments can produce polymers with excellent crystallinity, heat resistance, and mechanical strength.
[0077] In addition, the propylene-based polymer modified by the method according to the embodiment exhibited a broad molecular weight distribution to the same extent as the commercially available propylene-based polymer (Comparative Example 2), which indicated that the polymers were not separated but were homogeneously distributed, resulting in a high polymer distribution.
[0078] In addition, it was confirmed that the propylene-based polymer modified by the method according to the embodiment is similar to a commercially available propylene-based polymer (Comparative Example 2) and exhibits a superior strain hardening index compared to the propylene-based polymer of Comparative Example 1. This confirmed that the polymer modification according to the embodiment can produce a polymer that has excellent strain hardening properties and can effectively maintain a stable state during processing.
[0079] Although an embodiment has been described in detail through examples and experimental examples, the scope of the embodiment should not be limited to the specific examples, but should be interpreted according to the appended claims.
Claims
1. A method for preparing a mixture by adding a propylene polymer, a diene compound, and a radical initiator to a solvent; subjecting the mixture to a radical reaction; A method for producing a modified propylene-based polymer, comprising the steps of:
2. The step of preparing the mixture comprises: Dissolving a propylene polymer in a solvent; adding a diene compound and a radical initiator and then mixing; The method for producing the modified propylene-based polymer according to claim 1, comprising:
3. The method for producing a modified propylene polymer according to claim 1, wherein the step of preparing the mixture and the step of carrying out the radical reaction are both carried out at a temperature of 80 to 200° C.
4. The method for producing a modified propylene polymer according to claim 1, wherein the solvent contains at least one of an aliphatic hydrocarbon compound and an aromatic hydrocarbon compound.
5. The aliphatic hydrocarbon compound is 3-20 The method for producing a modified propylene polymer according to claim 4, wherein the aliphatic hydrocarbon compound is one of the following:
6. The aromatic hydrocarbon compound is 5-20 The method for producing a modified propylene polymer according to claim 4, wherein the aromatic hydrocarbon compound is an aromatic hydrocarbon compound represented by the formula:
7. The method for producing a modified propylene polymer according to claim 1, wherein the diene compound is added in an amount of 0.1 to 20.0% by weight based on the weight of the propylene polymer added.
8. The method for producing a modified propylene polymer according to claim 1, wherein the diene compound is added in an amount of 5.0 to 15.0% by weight based on the weight of the propylene polymer added.
9. The method for producing a modified propylene polymer according to claim 1, wherein a weight ratio of the radical initiator to the diene compound is 1:1 to 1:
50.
10. The method for producing a modified propylene polymer according to claim 1, wherein the radical initiator is added in an amount of 0.1 to 5.0% by weight based on the weight of the propylene polymer added.
11. The method for producing a modified propylene polymer according to claim 1, wherein the diene compound is a compound having 2 to 20 carbon atoms.
12. The method for producing a modified propylene polymer according to claim 1, wherein the diene compound includes at least one selected from the group consisting of 1,3-butadiene, 1,4-pentadiene, 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, 1,8-nonadiene, 1,9-decadiene, 1,10-undecadiene, 1,11-dodecadiene, 1,12-tridecadiene, 1,13-tetradecadiene, chloroprene, cyclohexadiene, cyclopentadiene, 2,3-dimethylbutadiene, isoprene, o-divinylbenzene, m-divinylbenzene, and p-divinylbenzene.
13. The method for producing a modified propylene-based polymer according to claim 1, wherein the radical initiator comprises at least one selected from the group consisting of acyl peroxides, alkyl peroxides, hydroperoxides, hydroperoxides, peresters and hydroperoxides.
14. The method for producing a modified propylene polymer according to claim 1, wherein the modified propylene polymer has a xylene soluble matter content of 2.0% by weight or less.
15. A modified propylene polymer produced by the method for producing a modified propylene polymer according to any one of claims 1 to 14.
16. The modified propylene-based polymer according to claim 15, wherein the modified propylene-based polymer has 2.0 wt% or less of xylene solubles.
17. A modified propylene polymer having a xylene solubles content of 2.0% by weight or less.
18. The modified propylene polymer according to claim 17, wherein the modified propylene polymer has a crystallization temperature (Tc) of 110 to 124°C.
19. The modified propylene-based polymer according to claim 17, wherein the modified propylene-based polymer has a number average molecular weight (Mn) of 60,000 to 110,000 g / mol.
20. The modified propylene polymer has a melting point of 1.0 s at 180° C. -1 The modified propylene-based polymer according to claim 17, wherein the strain hardening index (SHI) measured at a Hencky rate (dε / dt) of 0.2 or more and a Hencky strain (ε) of 1 to 3 is 0.2 or more, and the strain hardening index is defined as a gradient value (c2) of a common logarithm (log(ε)) function of the Hencky strain defined by the following Equation 2: [Formula 2] or E =c1×e c2 However, in Equation 2, η E is the elongation viscosity (Pa-s), ε is the Hencky strain, and c1 and c2 are parameters.
21. The modified propylene-based polymer according to claim 17, wherein the modified propylene-based polymer is produced by copolymerizing a diene copolymer.
22. A foaming composition comprising the modified propylene-based polymer according to claim 15.