Method for producing modified recycled carbon black and modified recycled carbon black
By using controlled combustion and oxidation in a burner system, the method addresses the weak bonding issue of recycled carbon black, producing modified carbon black with enhanced reinforcing properties for rubber products.
Patent Information
- Application Number
- JP2023072019
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-26
AI Technical Summary
Recycled carbon black obtained from pyrolyzing rubber products like waste tires has weak reinforcing properties due to rubber residues adhering to its surface, which inhibit its bonding with rubber components, and existing methods are not efficient or continuous.
A method involving a main burner and optionally an auxiliary burner to oxidize and decompose rubber residues on recycled carbon black by controlling oxygen and fuel combustion rates, followed by a particle size adjustment and cooling process to produce modified recycled carbon black with enhanced bonding properties.
The method effectively removes rubber residues, enabling continuous production of recycled carbon black with improved reinforcing properties for rubber products, comparable to virgin carbon black.
Smart Images

Figure 2024157598000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to recycled carbon black having a modified surface state, a method for producing the same, and a rubber composition in which the same is used. [Background technology]
[0002] In recent years, efforts such as carbon neutrality and sustainability have been actively undertaken to reduce the burden on the global environment. In the carbon black industry, the use of recycled carbon black obtained by pyrolysis of waste tires is being considered as part of sustainability activities.
[0003] As a method for producing recycled carbon black by pyrolysis of waste tires and the like, for example, Patent Document 1 discloses a method in which nitrogen gas is circulated and waste tires are pyrolyzed at about 500°C, and Patent Document 2 discloses a method in which waste rubber is subjected to a two-stage pyrolysis process and the obtained material is pulverized. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5813985 [Patent Document 2] WO2013 / 095145A1 Summary of the Invention [Problem to be solved by the invention]
[0005] However, recycled carbon black, which is obtained by pyrolyzing rubber products such as waste tires, has rubber residues, mainly composed of rubber charcoal, adhering to its surface. When the recycled carbon black is mixed with a rubber composition, the rubber residues inhibit the adsorption of the recycled carbon black to the rubber component.
[0006] Therefore, recycled carbon black has a problem in that it has a low reinforcing effect on rubber products due to its weak bond with the rubber component.
[0007] Therefore, there is a demand for recycled carbon black with high reinforcing properties for rubber products. Furthermore, from an industrial point of view, a method for producing recycled carbon black with high reinforcing properties for rubber products continuously, rather than batchwise, is required.
[0008] Therefore, an object of the present invention is to provide a method for producing modified recycled carbon black, which can effectively remove rubber residue adhering to the surface of recycled carbon black and can be carried out continuously. [Means for solving the problem]
[0009] As a result of extensive research, the inventors have discovered that by continuously supplying main burner fuel, oxygen-containing gas, and recycled carbon black having charcoal adhering thereto to a main burner which burns fuel to generate a flame, and combusting the main burner fuel, while continuously generating a flame with the main burner, the recycled carbon black having rubber charcoal adhering thereto is introduced into the flame and passed through the flame, the rubber residue adhering to the surface of the recycled carbon black is quickly oxidized and decomposed by the high-temperature flame, which has led to the completion of the present invention.
[0010] That is, the present invention provides (1) A main burner modification process includes a main burner fuel, an oxygen-containing gas, and recycled carbon black having rubber carbonized particles attached thereto, which are continuously supplied to a main burner that burns fuel to generate a flame, and combusts the main burner fuel. While continuously generating a flame in the main burner, the recycled carbon black having rubber carbonized particles attached thereto is introduced into the flame and passed through the flame, The following formula (1): Main burner total carbon combustion rate (%) = (A / (B+C)) x 100 (1) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, and C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner.) The total carbon combustion rate of the main burner, expressed as: A method for producing modified recycled carbon black, comprising the steps of: (2) The main burner reforming process is carried out according to the following formula (2): Main burner flame combustion rate (%) = (A / C) x 100 (2) (In the formula, A refers to the amount of oxygen supplied to the main burner, and C refers to the theoretical amount of oxygen required to completely combust the main burner fuel supplied to the main burner.) A main burner reforming process (1) in which the main burner flame combustion rate represented by is 100.0% or more; A method for producing modified recycled carbon black according to claim 1. (3) The main burner reforming process is carried out in accordance with the following formula (2): Main burner flame combustion rate (%) = (A / C) x 100 (2) (In the formula, A refers to the amount of oxygen supplied to the main burner, and C refers to the theoretical amount of oxygen required to completely combust the main burner fuel supplied to the main burner.) A main burner reforming step (2) in which the main burner flame combustion rate represented by is less than 100.0%; A method for producing modified recycled carbon black according to (1), (4) an auxiliary burner for burning an auxiliary burner fuel to generate a flame is provided downstream of the main burner, and an auxiliary burner reforming step is provided in which, while a flame is continuously generated by the auxiliary burner, the recycled carbon black after the main burner reforming step (1) or (2) is introduced into the flame generated by the auxiliary burner and passed through the flame; The auxiliary burner reforming step is represented by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (In the formula, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner.) The auxiliary burner flame combustion rate represented by the following formula (4): is 100.0% or more. Total carbon combustion rate of all burners (%) = ((A+D) / (B+C+E)) x 100 (4) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required to completely combust the auxiliary burner fuel that is supplied to the auxiliary burner.) The auxiliary burner reforming step (1) is for making the total carbon combustion rate of all burners, represented by A method for producing modified recycled carbon black according to (2) or (3), (5) an auxiliary burner for burning an auxiliary burner fuel to generate a flame is provided downstream of the main burner, and an auxiliary burner reforming step is provided in which, while a flame is continuously generated by the auxiliary burner, the recycled carbon black after the main burner reforming step (1) or (2) is introduced into the flame generated by the auxiliary burner and passed through the flame; The auxiliary burner reforming step is represented by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) x 100 (3) (In the formula, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner.) The auxiliary burner flame combustion rate represented by the following formula (4): is less than 100.0%. Total carbon combustion rate of all burners (%) = ((A+D) / (B+C+E)) x 100 (4) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required to completely combust the auxiliary burner fuel that is supplied to the auxiliary burner.) an auxiliary burner reforming step (2) for making the total carbon combustion rate of all burners represented by the formula (1) less than 100.0%; A method for producing modified recycled carbon black according to (2) or (3), (6) an auxiliary fuel pyrolysis step of providing a fuel nozzle downstream of the main burner and introducing auxiliary fuel from the fuel nozzle into or near the flame generated by the main burner, The following formula (5): Total carbon burn rate (%) of all reactions = (A / (B+C+F)) x 100 (5) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner, and F indicates the theoretical amount of oxygen required to completely combust the auxiliary fuel that is supplied from the fuel nozzle.) an auxiliary fuel pyrolysis process in which the total reaction total carbon combustion rate represented by A method for producing modified recycled carbon black according to (2) or (3), (7) A method for producing modified recycled carbon black as described in claim 1, characterized in that it includes a particle size adjustment process of pulverizing and / or classifying the recycled carbon black to which the rubber carbonized material is attached before carrying out the main burner modification process. (8) Modified recycled carbon black obtained by carrying out any one of the methods for producing modified recycled carbon black described in (1) to (7). This provides: Effect of the Invention
[0011] According to the present invention, it is possible to provide a method for producing modified recycled carbon black, which can effectively remove rubber residue adhering to the surface of recycled carbon black and can be carried out continuously. [Brief description of the drawings]
[0012] [Figure 1] 1 is a modified recycled carbon black production apparatus according to an embodiment of the modified recycled carbon black production method of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a main burner reforming process. [Diagram 3] FIG. 2 is a schematic diagram showing an example of a main burner reforming step and an auxiliary burner reforming step. [Figure 4] FIG. 2 is a schematic end view showing the structure of an example main burner; [Diagram 5] FIG. 13 is a schematic end view showing the structure of another example of the main burner. [Figure 6] 1 is a Raman spectrum of an example of a modified recycled carbon black according to the present invention. [Figure 7] 1 is a Raman spectrum of an example morphology of recycled carbon black before modification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings as appropriate. The detailed description of the present invention below is an example of an embodiment, and the present invention is not to be construed as being limited to this embodiment.
[0014] FIG. 1 is a schematic diagram of a modified recycled carbon black manufacturing apparatus of an embodiment for carrying out the modified recycled carbon black manufacturing method of the present invention. In FIG. 1, the modified recycled carbon black manufacturing apparatus 1 has a burner reforming section 2 in which a main burner 3, an auxiliary burner 4, and a cooling water supply pipe 5 are installed, and a collection section 7 in which a bag filter is installed. The burner reforming section 2 and the collection section 7 are connected by a connecting pipe 6. The main burner 3 is installed above the burner reforming section 2, and the main burner 3 is connected to a supply pipe for main burner fuel 11, a supply pipe for oxygen-containing gas 12, and a supply pipe for raw recycled carbon black and carrier gas 13. In addition, the auxiliary burner 4 is connected to a supply pipe for auxiliary burner fuel 14 and oxygen-containing gas 15.
[0015] As shown in FIG. 2, in the burner reforming section 2, the main burner 3 burns fuel to generate a flame 21, and while the flame 21 is generated in the main burner 3, the main burner fuel 11, the oxygen-containing gas 12, the raw recycled carbon black, and the carrier gas 13 are continuously supplied to the main burner 3 from the fuel supply side to the flame 21. While the flame 21 is continuously generated in the main burner 3, the raw recycled carbon black is introduced from the fuel supply side into the flame 21 generated by the main burner 3 and passes through the flame 21. When the raw recycled carbon black passes through the flame 21 generated by the main burner 3, the surface of the recycled carbon black is modified. FIG. 2 shows the movement direction 22 of the raw recycled carbon black, and the recycled carbon black moves from the fuel supply side to the tip side of the flame 21 generated by the main burner 3.
[0016] As shown in FIG. 3, in the burner reforming section 2, in addition to reforming using the main burner 3, reforming using the auxiliary burner 4 can be performed. As in FIG. 2, recycled carbon black is introduced into the flame 21 generated by the main burner 3, and after passing through the flame 21, the auxiliary burner 4 burns fuel to generate a flame 23. With the flame 23 generated by the auxiliary burner 4, the recycled carbon black that has passed through the flame 21 generated by the main burner 3 is introduced into the flame 23 generated by the auxiliary burner 4 and passes through the flame 23. Then, when the recycled carbon black that has passed through the flame 21 generated by the main burner 3 passes through the flame 23 generated by the auxiliary burner 4, the surface of the recycled carbon black is further modified. FIG. 3 shows the moving direction 22 of the recycled carbon black, and after passing through the flame 21 generated by the main burner 3, the recycled carbon black is introduced into the flame 23 generated by the auxiliary burner 4 and passes through the flame 23.
[0017] In the burner reforming section 2, the reforming of the recycled carbon black is always carried out using the main burner 3, and the reforming of the recycled carbon black is also carried out using the auxiliary burner 4 as required.
[0018] After the raw recycled carbon black is passed through the flame generated by the main burner 3 in the burner reforming section 2, or after it is passed through the flame generated by the main burner 3 and the flame generated by the auxiliary burner 4, cooling water is supplied into the burner reforming section 2 from a cooling water supply pipe 5 installed below the burner reforming section 2, and the recycled carbon black is brought into contact with the cooling water 16 to be cooled.
[0019] Next, the cooled recycled carbon black and gases such as combustion gas, decomposition gas, and water vapor are introduced into the collection section 7 via the connecting pipe 6, and separated into gas 17 and modified recycled carbon black 18 by a bag filter installed in the collection section 7, thereby obtaining modified recycled carbon black 18.
[0020] The method for producing modified recycled carbon black of the present invention includes a main burner modification step of continuously supplying a main burner fuel, an oxygen-containing gas, and recycled carbon black having rubber carbonized particles adhered thereto to a main burner which is burning a fuel to generate a flame, thereby combusting the main burner fuel, and continuously introducing the recycled carbon black having rubber carbonized particles adhered thereto into the flame while generating a flame in the main burner, and passing the recycled carbon black through the flame; The following formula (1): Main burner total carbon combustion rate (%) = (A / (B+C)) x 100 (1) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, and C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner.) The total carbon combustion rate of the main burner, expressed as: It is characterized by:
[0021] The main burner modification step in the method for producing modified recycled carbon black of the present invention is a step of modifying the surface of the recycled carbon black to which carbides are attached by continuously supplying main burner fuel, oxygen-containing gas, and recycled carbon black to which carbides are attached to a main burner that burns fuel to generate a flame.
[0022] In the main burner reforming process, recycled carbon black (hereinafter also referred to as raw recycled carbon black) having carbide attached thereto, which is the raw material for reforming, is carbon black obtained by pyrolyzing rubber products such as waste tires, and is carbon black having rubber residues, mainly composed of rubber charcoal, attached to its surface. Examples of raw recycled carbon black, which is the raw material for reforming, include PB365 manufactured by Enrestec, BolderBlack manufactured by Bolder Industries, DE-Black manufactured by Delta Energy, and MondoBlack manufactured by ECOLOMONDO. Such raw recycled carbon black may be manufactured by any manufacturing method, and is not particularly limited, but may be, for example, the method described in Patent Document 2.
[0023] The raw recycled carbon black has a Raman spectrum of 1350±10cm when measured by laser Raman spectroscopy at an excitation wavelength of 532 nm. -1 When the peak intensity of the peak (D band) having a peak top in the range of 1580 ± 20 cm is taken as 100, -1 The peak intensity of a peak (G band) having a peak top in this range (hereinafter also referred to as the G band intensity when the D band intensity is taken as 100) is 112 to 200, preferably 112 to 190. The G band intensity when the D band intensity is taken as 100 will be described later.
[0024] Raw recycled carbon black is obtained by modifying recycled carbon black obtained by pyrolysis of rubber products such as waste tires, and therefore the ash content of raw recycled carbon black is, for example, 3.0% or more and 50.0% or less, preferably 5.0% or more and 35.0% or less.
[0025] In the present invention, the ash content means a value measured by the method specified in JIS K 6218-2.
[0026] The main burner fuel in the main burner reforming process is not particularly limited as long as it burns with the oxygen in the oxygen-containing gas when it comes into contact with the flame generated by the main burner and generates a flame. For example, hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, acetylene, etc., hydrogen, ammonia, mixed gases thereof, gases generated by thermal decomposition of rubber and plastics, etc., and also liquid fuels such as aromatic hydrocarbons such as naphthalene and anthracene, coal-based hydrocarbons such as creosote oil and tar oil, petroleum-based heavy oils such as FCC residual oil and ethylene heavy end oil, acetylenic unsaturated hydrocarbons, aliphatic hydrocarbons such as hexane, vegetable oils such as rapeseed oil and soybean oil, and oils generated by thermal decomposition of rubber and plastics. Hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, and acetylene are preferred in that they produce a higher flame temperature.
[0027] The oxygen-containing gas in the main burner reforming step may be oxygen gas, a gas containing oxygen, air, or the like, with air being preferred from the viewpoint of economy.
[0028] In the main burner reforming process, the main burner fuel, oxygen-containing gas, and recycled carbon black having carbide attached thereto are continuously supplied from the fuel supply side to the main burner, which is burning the main burner fuel to generate a flame, thereby burning the main burner fuel, and while continuously generating a flame in the main burner, the raw recycled carbon black is introduced into the flame generated by the main burner and allowed to pass through the flame.
[0029] In the main burner reforming step, the raw recycled carbon black is supplied to the main burner using a carrier gas. The carrier gas may be an inert gas such as nitrogen gas, argon gas, or helium gas, or an oxygen-containing gas such as oxygen gas, a gas containing oxygen, or air. As the carrier gas, an oxygen-containing gas is preferred because it makes the raw recycled carbon black more easily oxidized.
[0030] In the main burner reforming process, the raw recycled carbon black transported in the carrier gas, the oxidizing gas, and the fuel for the main burner can be supplied to the main burner through separate routes. Also, in the main burner reforming process, the raw recycled carbon black and the oxidizing gas can be mixed first, and the resulting mixed flow and the fuel for the main burner can be supplied to the main burner.
[0031] In the main burner reforming step, when the raw recycled carbon black and the oxygen-containing gas are introduced into the flame, they are introduced into the flame as a mixed flow of the raw recycled carbon black and the oxygen-containing gas. This allows the oxygen-containing gas to be present in the vicinity of the raw recycled carbon black when it is introduced into the flame. This makes it possible to prioritize contact between the raw recycled carbon black and the oxygen-containing gas over contact between the raw recycled carbon black and the fuel gas, making it easier for oxidation of the raw recycled carbon black to occur.
[0032] In the main burner reforming step, (i) when the raw recycled carbon black, the carrier gas, the oxygen-containing gas, and the main burner fuel are introduced into the flame, the raw recycled carbon black is present at the center when viewed in a plane perpendicular to the moving direction of the raw recycled carbon black, the oxygen-containing gas is present surrounding the raw recycled carbon black, and the main burner fuel is present surrounding the oxygen-containing gas, and the raw recycled carbon black, the carrier gas, the oxygen-containing gas, and the main burner fuel can be introduced into the flame, and (ii) when the raw recycled carbon black, the carrier gas, the oxygen-containing gas, and the main burner fuel are introduced into the flame, the main burner fuel is present at the center when viewed in a plane perpendicular to the moving direction of the raw recycled carbon black. (iii) when the raw material recycled carbon black, the carrier gas, the oxygen-containing gas, and the main burner fuel are introduced into the flame, when viewed on a plane perpendicular to the moving direction of the raw material recycled carbon black, the raw material recycled carbon black can be present at the center, the main burner fuel can be present surrounding the raw material recycled carbon black, the oxygen-containing gas can be present surrounding the main burner fuel, and the raw material recycled carbon black, the carrier gas, the oxygen-containing gas, and the main burner fuel can be introduced into the flame. Of these, (i) and (ii) are preferred in that they allow an oxygen-containing gas to be present in the vicinity of the raw recycled carbon black when it is introduced into the flame, thereby allowing contact between the raw recycled carbon black and the oxygen-containing gas to take precedence over contact between the raw recycled carbon black and the fuel gas, thereby facilitating oxidation of the raw recycled carbon black.
[0033] In the main burner reforming process, the temperature of the flame generated by the main burner is high, so when the raw recycled carbon black passes through the flame generated by the main burner, the rubber residue, mainly composed of rubber charcoal, adhering to the surface of the raw recycled carbon black is quickly oxidized and decomposed and removed. In the main burner reforming process, the raw recycled carbon black is supplied to the main burner together with the main burner fuel and oxygen-containing gas, and is exposed to high temperatures only while passing through the flame generated by the main burner, so the time of exposure to high temperatures is short. Therefore, the surface of the raw recycled carbon black is selectively oxidized.
[0034] On the other hand, when the raw recycled carbon black is supplied to a heating furnace together with an oxidizing gas and oxidized in the heating furnace, the temperature to which the raw recycled carbon black is exposed does not become as high as the temperature of the flame, and the time for which the raw recycled carbon black is heated becomes long. If the temperature to which the raw recycled carbon black is exposed is low, oxidation will proceed from the parts that are easily oxidized and decomposed, but if the time is long, oxidation will proceed to the inside of the raw recycled carbon black particles, forming pores in the raw recycled carbon black.
[0035] In the main burner reforming process, the following formula (1): Main burner total carbon combustion rate (%) = (A / (B+C)) x 100 (1) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, and C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner.) The main burner total carbon combustion rate represented by the following formula is set to be less than 100.0%. Note that A is the amount of oxygen supplied to the main burner per unit time, B is the amount of theoretical oxygen required per unit time to completely combust the carbon content calculated by regarding all components excluding ash of the recycled carbon black to which rubber carbonized material is attached that is supplied to the main burner as carbon, and C is the amount of theoretical oxygen required per unit time to completely combust the main burner fuel that is supplied to the main burner.
[0036] In the main burner reforming step, controlling the main burner total carbon combustion rate to less than 100.0% means that the main burner fuel and the raw recycled carbon black supplied to the main burner are not completely burned. If the main burner fuel and the raw recycled carbon black supplied to the main burner were completely burned, the recycled carbon black would be oxidized and lost, and reformed recycled carbon black would not be obtained. Therefore, by making the main burner total carbon combustion rate less than 100.0%, it is possible to reform the raw recycled carbon black by oxidative decomposition of its surface. From the viewpoint of the balance between the amount of reformed particles recovered and the amount of rubber char that needs to be removed, the main burner total carbon combustion rate is preferably 10.0% or more and 90.0% or less, more preferably 15.0% or more and 80.0% or less.
[0037] In the method for producing the modified recycled carbon black of the present invention, the main burner modification step is carried out by reacting the carbon black with the carbon black having a fluorine atom or a fluorine atom in an amount of 1:1 or more. Main burner flame combustion rate (%) = (A / C) x 100 (2) (In the formula, A refers to the amount of oxygen supplied to the main burner, and C refers to the theoretical amount of oxygen required to completely combust the main burner fuel supplied to the main burner.) The main burner reforming step (1) is to make the main burner flame combustion rate, represented by
[0038] In the main burner reforming step (1), controlling the main burner flame combustion rate to 100.0% or more means that the main burner fuel supplied to the main burner is completely burned. In the main burner reforming step (1), by setting the main burner flame combustion rate to 100.0% or more, the surface of the raw recycled carbon black is easily oxidized, so that the oxidative removal of the residual rubber adhering to the raw recycled carbon black can be improved. From the viewpoint of the balance between the flame temperature and the amount of rubber char that needs to be removed, the main burner flame combustion rate is preferably 105.0% or more and 500.0% or less, and more preferably 110.0% or more and 400.0% or less. Note that since the main burner reforming step (1) is one form of the main burner reforming step, the main burner total carbon combustion rate is less than 100.0%, preferably 15.0% or more and 90.0% or less, and more preferably 20.0% or more and 80.0% or less.
[0039] In the method for producing the modified recycled carbon black of the present invention, the main burner modification step is carried out by reacting the carbon black with the carbon black having a fluorine atom or a fluorine atom in an amount of 1:1 or more. Main burner flame combustion rate (%) = (A / C) x 100 (2) (In the formula, A refers to the amount of oxygen supplied to the main burner, and C refers to the theoretical amount of oxygen required to completely combust the main burner fuel supplied to the main burner.) The main burner reforming step (2) is to make the main burner flame combustion rate, represented by
[0040] In the main burner reforming step (2), controlling the main burner flame combustion rate to less than 100.0% means that the main burner fuel supplied to the main burner is prevented from being completely burned. When the main burner fuel is heated under conditions that prevent the main burner fuel supplied to the main burner from being completely burned, the main burner fuel is pyrolyzed to generate charcoal, and the generated charcoal is attached to the surface-modified recycled carbon black when it passes through the flame generated by the main burner, thereby adjusting the specific surface area of the modified recycled carbon black. From the viewpoint of the appropriate value of the specific surface area for improving the reinforcing properties of rubber, the main burner flame combustion rate is preferably 20.0% or more and 99.0% or less, more preferably 30.0% or more and 95.0% or less. Since the main burner reforming step (2) is one form of the main burner reforming step, the main burner total carbon combustion rate is less than 100.0%, preferably 15.0% or more and 90.0% or less, and more preferably 20.0% or more and 80.0% or less.
[0041] In the method for producing modified recycled carbon black of the present invention, an auxiliary burner for burning auxiliary burner fuel to generate a flame is provided downstream of the main burner, and an auxiliary burner reforming step is continuously performed in which the recycled carbon black after the main burner reforming step is introduced into the flame generated by the auxiliary burner while the flame is continuously generated by the auxiliary burner and passed through the flame. In the method for producing modified recycled carbon black of the present invention, the auxiliary burner reforming step is performed as necessary.
[0042] The auxiliary burner reforming step in the method for producing modified recycled carbon black of the present invention is a step in which a flame is generated by burning auxiliary burner fuel downstream of the flame generated by the main burner, and the recycled carbon black after the main burner reforming step is continuously supplied so as to be introduced into the flame generated by the auxiliary burner and passed through the flame, thereby modifying the surface of the recycled carbon black.
[0043] What is reformed in the auxiliary burner reforming step is the recycled carbon black after the main burner reforming step, i.e., the recycled carbon black that has passed through the flame generated by the main burner or the recycled carbon black that has passed near the tip of the flame generated by the main burner.
[0044] In the auxiliary burner reforming step, auxiliary burner fuel and oxygen-containing gas are continuously supplied to the auxiliary burner to continuously generate a flame. The position of the flame generated by the auxiliary burner is the tip of the flame generated by the main burner, inside the flame generated by the main burner and near the tip of the flame, outside the flame generated by the main burner and near the tip of the flame, and preferably outside the flame generated by the main burner and near the tip of the flame.
[0045] The fuel for the auxiliary burner in the auxiliary burner reforming process is not particularly limited as long as it burns with the oxygen in the oxygen-containing gas when it comes into contact with the flame generated by the auxiliary burner and generates a flame. For example, hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, acetylene, etc., hydrogen, ammonia, mixed gases thereof, gases generated by thermal decomposition of rubber and plastics, etc., and also, as liquid fuels, aromatic hydrocarbons such as naphthalene and anthracene, coal-based hydrocarbons such as creosote oil and tar oil, petroleum-based heavy oils such as FCC residual oil and ethylene heavy end oil, acetylenic unsaturated hydrocarbons, aliphatic hydrocarbons such as hexane, vegetable oils such as rapeseed oil and soybean oil, and oils generated by thermal decomposition of rubber and plastics. Hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, and acetylene are preferred in that the temperature of the flame is higher.
[0046] Examples of the oxygen-containing gas involved in the auxiliary burner reforming step include oxygen gas, a gas containing oxygen, and air, with air being preferred from the viewpoint of economy.
[0047] In the auxiliary burner reforming process, the fuel for the auxiliary burner is burned to generate a flame in the auxiliary burner, and while continuously generating a flame in the auxiliary burner, the recycled carbon black after the main burner reforming process is introduced into the flame generated by the auxiliary burner and passed through the flame.
[0048] The auxiliary burner reforming process is carried out according to the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) x 100 (3) (In the formula, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner.) The auxiliary burner flame combustion rate represented by the following formula (4): is 100.0% or more. Total carbon combustion rate of all burners (%) = ((A+D) / (B+C+E)) x 100 (4) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required to completely combust the auxiliary burner fuel that is supplied to the auxiliary burner.) The auxiliary burner reforming step (1) is for making the total carbon combustion rate of all burners, represented by the formula: D = D / E / E+100.0%, less than 100.0%. Here, D is the amount of oxygen supplied to the auxiliary burner per unit time, and E is the theoretical amount of oxygen required per unit time to completely combust the auxiliary burner fuel supplied to the auxiliary burner.
[0049] In the auxiliary burner reforming step (1), controlling the total carbon combustion rate of all burners to less than 100.0% means that the auxiliary burner fuel and recycled carbon black supplied to the auxiliary burner are not completely burned. If the auxiliary burner fuel and recycled carbon black supplied to the auxiliary burner were completely burned, the recycled carbon black would be oxidized and lost, and modified recycled carbon black would not be obtained. From the viewpoint of the balance between the amount of recovered modified particles obtained and the amount of rubber carbonized matter that needs to be removed, the total carbon combustion rate of all burners is preferably 15.0% or more and 90.0% or less, more preferably 20.0% or more and 80.0% or less.
[0050] In the auxiliary burner reforming step (1), controlling the auxiliary burner flame combustion rate to 100.0% or more means that the auxiliary burner fuel supplied to the auxiliary burner is completely burned. In the auxiliary burner reforming step (1), by setting the auxiliary burner flame combustion rate to 100.0% or more, the surface of the recycled carbon black after the main burner reforming step is easily oxidized, so that the oxidative removal property of the residual rubber adhering to the recycled carbon black after the main burner reforming step can be improved. In other words, the auxiliary burner reforming step (1) can improve the oxidative removal property of the residual rubber that could not be completely removed even by the main burner reforming step (1). From the viewpoint of the balance between the temperature of the flame and the amount of rubber carbonized matter that needs to be removed, the auxiliary burner flame combustion rate is preferably 105.0% or more and 600.0% or less, and more preferably 110.0% or more and 500.0% or less. Since the auxiliary burner reforming step (1) is one form of the auxiliary burner reforming step, the total carbon combustion rate of all burners is less than 100.0%, preferably 15.0% or more and 90.0% or less, and more preferably 20.0% or more and 80.0% or less.
[0051] The auxiliary burner reforming process is carried out according to the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) x 100 (3) (In the formula, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner.) The auxiliary burner flame combustion rate represented by the following formula (4): is less than 100.0%. Total carbon combustion rate of all burners (%) = ((A+D) / (B+C+E)) x 100 (4) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required to completely combust the auxiliary burner fuel that is supplied to the auxiliary burner.) The total carbon combustion rate of all burners, represented by the formula (2), is less than 100.0%.
[0052] In the auxiliary burner reforming step (2), controlling the total carbon combustion rate of all burners to less than 100.0% means that the auxiliary burner fuel and recycled carbon black supplied to the auxiliary burner are not completely burned. If the auxiliary burner fuel and recycled carbon black supplied to the auxiliary burner were completely burned, the recycled carbon black would be oxidized and lost, and modified recycled carbon black would not be obtained. From the viewpoint of the balance between the amount of recovered modified particles obtained and the amount of rubber carbonized matter that needs to be removed, the total carbon combustion rate of all burners is preferably 15.0% or more and 90.0% or less, more preferably 20.0% or more and 80.0% or less.
[0053] In the auxiliary burner reforming step (2), controlling the auxiliary burner flame combustion rate to less than 100.0% means that the auxiliary burner fuel supplied to the auxiliary burner is prevented from being completely burned. When the auxiliary burner fuel is heated under conditions that prevent the auxiliary burner fuel supplied to the auxiliary burner from being completely burned, the auxiliary burner fuel is thermally decomposed to generate charcoal. When the auxiliary burner fuel passes through the flame generated by the auxiliary burner, the generated charcoal is attached to the surface-modified recycled carbon black, thereby adjusting the specific surface area of the modified recycled carbon black. From the viewpoint of the appropriate value of the specific surface area for improving the reinforcing properties of rubber, the auxiliary burner flame combustion rate is preferably 2.0% or more and 90.0% or less, more preferably 5.0% or more and 80.0% or less. Since the auxiliary burner reforming step (2) is one form of the auxiliary burner reforming step, the total carbon combustion rate of all burners is less than 100.0%, preferably 15.0% or more and 90.0% or less, and more preferably 20.0% or more and 80.0% or less.
[0054] The method for producing the modified recycled carbon black of the present invention may include an auxiliary fuel pyrolysis step in which a fuel nozzle is provided downstream of the main burner and the auxiliary fuel is introduced into or near the flame generated by the main burner to pyrolyze the auxiliary fuel. In the method for producing the modified recycled carbon black of the present invention, an auxiliary fuel pyrolysis step is carried out as necessary.
[0055] Among the methods for producing modified recycled carbon black according to the present invention, an apparatus for carrying out an embodiment having an auxiliary fuel pyrolysis step may be, for example, the modified recycled carbon black production apparatus 1 shown in FIG. 1 , which does not have an auxiliary burner and has a fuel nozzle for introducing auxiliary fuel into or near the flame generated by the main burner.
[0056] The auxiliary fuel pyrolysis step in the manufacturing method of the modified recycled carbon black of the present invention is a step of introducing an auxiliary fuel into or near a flame generated by a main burner, pyrolyzing the auxiliary fuel to generate char, and using the generated char to modify the surface of the recycled carbon black after the main burner reforming step. The auxiliary fuel is supplied to the tip of the flame generated by the main burner, inside the flame generated by the main burner and near the tip of the flame, or outside the flame generated by the main burner and near the tip of the flame.
[0057] What is reformed in the auxiliary fuel pyrolysis step is the recycled carbon black after the main burner reforming step, i.e., the recycled carbon black that has passed through the flame generated by the main burner or the recycled carbon black that has passed through the flame generated by the main burner.
[0058] In the auxiliary fuel pyrolysis process, the auxiliary fuel is introduced from a fuel nozzle provided downstream of the main burner. At this time, when the auxiliary fuel is supplied to the fuel nozzle and introduced from the fuel nozzle to the flame generated by the main burner or its vicinity, the auxiliary fuel supplied to the fuel nozzle is not mixed with an oxygen-containing gas. The auxiliary fuel for the auxiliary fuel pyrolysis step is not particularly limited as long as it is pyrolyzed by the heat of the flame of the main burner. Examples of the auxiliary fuel include hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, acetylene, etc., mixed gases of these, gases generated by the pyrolysis of rubber or plastics, and also, as liquid fuels, aromatic hydrocarbons such as naphthalene and anthracene, coal-based hydrocarbons such as creosote oil and tar oil, petroleum-based heavy oils such as FCC residual oil and ethylene heavy end oil, acetylenic unsaturated hydrocarbons, aliphatic hydrocarbons such as hexane, vegetable oils such as rapeseed oil and soybean oil, and oils generated by the pyrolysis of rubber or plastics. From the viewpoint of uniformly modifying the recycled carbon black, hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, acetylene, etc. are preferred.
[0059] In the auxiliary fuel pyrolysis process, the following formula (5): Total carbon burn rate (%) of all reactions = (A / (B+C+F)) x 100 (5) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required to completely combust the recycled carbon black with rubber carbonized material attached that is supplied to the main burner, C indicates the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner, and F indicates the theoretical amount of oxygen required to completely combust the auxiliary fuel that is supplied from the fuel nozzle.) The total carbon combustion rate of all reactions, expressed as: Here, F is the theoretical amount of oxygen required per unit time to completely combust the auxiliary fuel supplied from the fuel nozzle.
[0060] In the auxiliary fuel pyrolysis step, controlling the total reaction carbon combustion rate to less than 100.0% means that the main burner fuel, recycled carbon black, and auxiliary fuel supplied to the main burner are not completely burned. If the main burner fuel, recycled carbon black, and auxiliary fuel supplied to the main burner were completely burned, the recycled carbon black would be oxidized and lost, and modified recycled carbon black would not be obtained. In addition, the auxiliary fuel supplied from the auxiliary nozzle is heated under conditions that do not completely burn the auxiliary fuel, so that the auxiliary fuel is pyrolyzed to generate charcoal, and the generated charcoal can be attached to the surface-modified recycled carbon black to adjust the specific surface area of the modified recycled carbon black. From the viewpoint of the balance between the amount of recovery of the modified particles obtained and the amount of rubber charcoal that needs to be removed, the total reaction carbon combustion rate is preferably 15.0% or more and 90.0% or less, more preferably 20.0% or more and 80.0% or less.
[0061] In the main burner reforming step, the feed rates of raw recycled carbon black, oxygen-containing gas, and main burner fuel are appropriately selected to provide a desired main burner total carbon burn rate. In the main burner reforming step (1), the main burner total carbon burn rate and main burner flame burn rate are appropriately selected to obtain a predetermined total carbon burn rate and a predetermined flame burn rate. For example, the amount of air supplied as the oxygen-containing gas is 100.0 Nm 3 / hour, the supply of city gas (composition: methane 88%, ethane 6%, propane 5%, butane 1%) as fuel for the main burner is 1.8 Nm 3 / hour over 8.7Nm 3 / hour or less, preferably 2.3Nm 3 / hour over 8.3Nm 3 / hour or less, and the supply rate of the raw recycled carbon black is 3 kg / hour or more and 80 kg / hour or less, preferably 5 kg / hour or more and 60 kg / hour or less. In the main burner reforming step (2), the main burner total carbon burn rate and main burner flame burn rate are appropriately selected to obtain a predetermined total carbon burn rate and a predetermined flame burn rate. For example, the amount of air supplied as the oxygen-containing gas is set to 100.0 Nm 3 / hour, the supply of city gas as fuel for the main burner is 9.2 Nm 3 / hour over 45.0Nm 3 / hour or less, preferably 9.6 Nm 3 / hour over 30Nm 3 / hour or less, and the supply rate of the raw recycled carbon black is 2 kg / hour or more and 75 kg / hour or less, preferably 3 kg / hour or more and 55 kg / hour or less.
[0062] In the auxiliary burner reforming step, the supply amounts of the oxygen-containing gas and the auxiliary burner fuel are appropriately selected so as to achieve a predetermined total carbon combustion rate of all burners and a predetermined auxiliary burner flame combustion rate. In the auxiliary burner reforming step (1), the total carbon combustion rate of all burners and the flame combustion rate of the auxiliary burner are appropriately selected. For example, the amount of air supplied as the oxygen-containing gas for the main burner is set to 100.0 Nm 3 / hour, the supply of air as oxygen-containing gas for the auxiliary burner is 5.0 Nm 3 / hour over 100.0Nm 3 / hour or less, preferably 10.0Nm 3 / hour over 90.0Nm 3 / hour or less, and the supply of city gas as fuel for the auxiliary burner is 0.2 Nm 3 / hour over 8.7Nm 3 / hour or less, preferably 0.5 Nm 3 / hour over 7.5Nm 3 / hours or less. In the auxiliary burner reforming step (2), the total carbon combustion rate of all burners and the flame combustion rate of the auxiliary burner are appropriately selected. For example, the amount of air supplied as the oxygen-containing gas for the main burner is set to 100.0 Nm 3 / hour, the supply of air as oxygen-containing gas for the auxiliary burner is 2Nm 3 / hour more than 50.0Nm 3 / hour or less, preferably 5.0 Nm 3 / hour over 40.0Nm 3 / hour or less, and the supply of city gas as fuel for the auxiliary burner is 0.5Nm 3 / hour more than 50.0Nm 3 / hour or less, preferably 1.0 Nm 3 / hour over 30.0Nm 3 / hours or less. In the auxiliary fuel pyrolysis step, the amount of air supplied as oxygen-containing gas for the main burner is appropriately selected so as to obtain a predetermined total reaction carbon combustion rate. For example, the amount of air supplied as oxygen-containing gas for the main burner is set to 100.0 Nm 3 / hour, the supply of city gas as auxiliary fuel is 0.5Nm 3 / hour more than 50.0Nm 3 / hour or less, preferably 1.0 Nm 3 / hour over 30.0Nm 3 / hours or less.
[0063] When the auxiliary burner reforming step is not performed or the auxiliary fuel pyrolysis step is not performed, the reformed recycled carbon black obtained after the main burner reforming step, i.e., by passing through the flame generated by the main burner, is cooled by contacting it with water, nitrogen gas, a metal wall of a heat exchanger, etc. When the auxiliary burner reforming step is performed, the reformed recycled carbon black obtained after the main burner reforming step and the auxiliary burner reforming step, i.e., by passing through the flame generated by the main burner and the flame generated by the auxiliary burner, is cooled by contacting it with water, nitrogen gas, a metal wall of a heat exchanger, etc. When the auxiliary fuel pyrolysis step is performed, the reformed recycled carbon black obtained after the main burner reforming step and the auxiliary fuel pyrolysis step, i.e., by passing through the flame generated by the main burner and by performing the auxiliary fuel pyrolysis step, is cooled by contacting it with water, nitrogen gas, a metal wall of a heat exchanger, etc. At this time, since the modified recycled carbon black is at a high temperature after passing through the flame, when it comes into contact with water, the water turns into steam.
[0064] After the modified recycled carbon black is cooled, the cooled modified recycled carbon black is separated from gases such as combustion gas, decomposition gas, and water vapor using a solid / gas separator such as a bag filter or a cyclone to obtain the modified recycled carbon black.
[0065] The method for producing modified recycled carbon black of the present invention may include a particle size adjustment step of pulverizing and / or classifying the raw recycled carbon black before carrying out the main burner modification step. By carrying out the particle size adjustment step before carrying out the main burner modification step, the variation in particle size of the raw recycled carbon black supplied to the main burner modification step is reduced, so that the variation in the surface modification of the raw recycled carbon black in the main burner modification step can be reduced.
[0066] The pulverizing device used in the particle size adjustment step is not particularly limited, and examples thereof include a roller mill, a jet mill, a hammer mill, a pin mill, a cutter mill, a roll crusher, a stamp mill, a ring mill, etc. The classifying device used in the particle size adjustment step is not particularly limited, and examples thereof include a mechanical classifier equipped with a classification rotor or the like to realize centrifugal classification, a classifier that realizes centrifugal classification by a swirling flow (free vortex or semi-free vortex) generated by supplying a high-speed air flow, and a classifier that utilizes the inertial force of particles accelerated by a bending high-speed air flow and the Coanda effect.
[0067] There are no particular limitations on the main burner, so long as it is capable of burning a main burner fuel to generate a flame, and is capable of continuously supplying the main burner fuel, oxygen-containing gas, and raw recycled carbon black from the fuel supply side to burn the main burner fuel, and is capable of continuously introducing the raw recycled carbon black into the flame while generating a flame with the main burner, and allowing the raw recycled carbon black to pass through the flame.
[0068] For example, the main burner may be of the form shown in FIG. 4. FIG. 4 is a schematic end view of the form of the main burner. In FIG. 4, the main burner 30a has a supply path 33 for the raw recycled carbon black and the carrier gas in the center of the burner, and a nozzle 37 for the raw recycled carbon black and the carrier gas is formed on the flame generation side. The main burner 30a also has a supply path 32 for the oxygen-containing gas so as to surround the supply path 33 for the raw recycled carbon black and the carrier gas, and a nozzle 36 for the oxygen-containing gas is formed on the flame generation side. The main burner 30a also has a supply path 31 for the main burner fuel so as to surround the supply path 32 for the oxygen-containing gas, and a nozzle 35 for the main burner fuel is formed on the flame generation side. When viewed on a plane perpendicular to the moving direction of the raw recycled carbon black, a circular supply path for the raw recycled carbon black and carrier gas is formed in the center, a cylindrical supply formation for oxygen-containing gas is formed so as to surround the supply path for the raw recycled carbon black and carrier gas, and a cylindrical supply formation for main burner fuel is formed so as to surround the supply path for oxygen-containing gas. In the embodiment shown in Fig. 4, the supply path for the raw recycled carbon black and carrier gas, the supply path for oxygen-containing gas, and the supply path for main burner fuel are opened at the end of the main burner on the flame side.
[0069] By supplying the raw recycled carbon black, the carrier gas, the oxygen-containing gas, and the main burner fuel from the fuel supply side of the main burner 30a, the raw recycled carbon black is placed at the center of the flame, the oxygen-containing gas is placed surrounding the raw recycled carbon black, and the main burner fuel is placed surrounding the oxygen-containing gas, and the raw recycled carbon black, the carrier gas, the oxygen-containing gas, and the main burner fuel can be introduced. By using the main burner 30a, when the raw recycled carbon black, the carrier gas, the oxygen-containing gas, and the main burner fuel are introduced into the flame, the oxygen-containing gas can be placed near the raw recycled carbon black, so that the contact between the raw recycled carbon black and the oxygen-containing gas can be prioritized over the contact between the raw recycled carbon black and the fuel gas, which makes it easier for the raw recycled carbon black to be oxidized.
[0070] As the main burner, there is a main burner of an embodiment shown in FIG. 5. FIG. 5 is a schematic end view of an embodiment of the main burner. In FIG. 5, the main burner 30b has a supply path 33 for the raw recycled carbon black and the carrier gas in the center of the burner, and a nozzle 37 for the raw recycled carbon black and the carrier gas is formed on the flame generation side. The main burner 30b also has a supply path 32 for the oxygen-containing gas so as to surround the supply path 33 for the raw recycled carbon black and the carrier gas, and a nozzle 36 for the oxygen-containing gas is formed on the flame generation side. The main burner 30b also has a supply path 31 for the main burner fuel so as to surround the supply path 32 for the oxygen-containing gas, and a nozzle 35 for the main burner fuel is formed on the flame generation side. Then, the outlet 37 for the raw recycled carbon black and carrier gas, the outlet 36 for the oxygen-containing gas, and the outlet 35 for the main burner fuel open to a mixing chamber 38, and the mixed flow is ejected from the mixing chamber 38 toward the flame. In the embodiment shown in Fig. 5, the supply paths for the raw recycled carbon black and carrier gas, the supply path for the oxygen-containing gas, and the supply path for the main burner fuel open to a mixing chamber formed at the end of the main burner on the flame side, which is located just before the end of the main burner on the flame side, and the mixing chamber opens to the end of the main burner on the flame side.
[0071] In addition, examples of the structure of the main burner include the burner structures described in Japanese Patent No. 3001561, Japanese Patent No. 5367471, Japanese Patent No. 3312228, Japanese Patent No. 4769276, Japanese Patent Application Publication No. 2021-50897, Japanese Patent Application Publication No. 2010-156025, and Japanese Patent Application Publication No. 6580710.
[0072] In the method for producing modified recycled carbon black of the present invention, by performing the main burner modification step, or by performing the main burner modification step and the auxiliary burner modification step, modified recycled carbon black can be obtained whose G band intensity and nitrogen adsorption specific surface area N2SA are in the ranges shown below when the D band intensity of the modified recycled carbon black is taken as 100. Modified recycled carbon black whose G band intensity and nitrogen adsorption specific surface area N2SA are in the ranges shown below when the D band intensity is taken as 100 has strong bonds with the rubber component and is not too cohesive, so that it has high reinforcing properties for rubber products. Therefore, the method for producing modified recycled carbon black of the present invention can continuously produce modified recycled carbon black that can increase the reinforcing properties of rubber products.
[0073] The modified recycled carbon black obtained by carrying out the method for producing modified recycled carbon black of the present invention is a surface-modified recycled carbon black obtained by pyrolyzing rubber products such as waste tires, etc. More specifically, the modified recycled carbon black of the present invention is a recycled carbon black obtained by pyrolyzing rubber products such as waste tires, etc., from which all or a part of the rubber residues mainly composed of rubber charcoal that were attached to the surface of the recycled carbon black have been removed.
[0074] Recycled carbon black with rubber carbonized material on its surface has a Raman spectrum of 1350±10cm when measured with laser Raman spectroscopy at an excitation wavelength of 532 nm. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The peak intensity of the peak having a peak top in the range is 112 or more.
[0075] In contrast to such recycled carbon black with rubber charcoal adhering to the surface, modified recycled carbon black has the rubber residue, mainly composed of rubber charcoal, removed from the surface. In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, the peak intensity is 1350±10 cm -1 When the peak intensity of the peak (D band) having a peak top in the range of 1580 ± 20 cm is taken as 100, -1 The peak intensity of the peak (G band) having a peak top in the range is 84 or more and 111 or less. When the G band intensity is within the above range when the D band intensity of the recycled carbon black is taken as 100, there is no or very little rubber residue adhering to the surface of the recycled carbon black, and the bond between the recycled carbon black and the rubber component is high, so that the reinforcing property of the rubber product is high. From the viewpoint of appropriately reacting with the rubber and improving the reinforcing property, the G band intensity when the D band intensity is taken as 100 is preferably 85 or more and 110 or less, more preferably 90 or more and 105 or less. On the other hand, when the G band intensity when the D band intensity of the recycled carbon black is taken as 100 exceeds the above range, there is a lot of rubber residue adhering to the surface of the recycled carbon black, and the bond between the recycled carbon black and the rubber component is low. On the other hand, when the G band intensity is less than the above range, there are many defects in the graphite structure on the surface of the carbon black, and the surface activity is too high, which promotes the aggregation of the carbon blacks in the rubber, and reduces the reinforcing property of the rubber.
[0076] In the present invention, the G band intensity and the D band intensity, when the D band intensity is taken as 100, refer to values calculated from a Raman spectrum obtained by performing measurement under the measurement conditions of (1) below and then performing data processing of (2). (1) Using a laser Raman spectrometer, HR-800 manufactured by Horiba, Ltd., several grains of the carbon black sample to be measured are placed on a slide glass and rubbed several times with a spatula to make the surface flat. Measurement is performed under the following measurement conditions. YAG laser (excitation wavelength): 532 nm Number of grooves: 600gr / mm Filter: D0.6 Objective lens magnification: 100x Exposure time: 150 seconds Number of times: 2 (2) Measurement wavelength of the obtained spectrum (Raman Shift) 2100cm -1 The signal intensity at the measurement wavelength of 1350±10 cm was set to 0, and the average value was calculated for each of the 39 adjacent data points constituting the spectrum. Then, a spectral curve connecting the average values was obtained by smoothing. -1 The peak top intensity observed in this range is taken as 100. An example of the spectrum obtained in this case is shown in Figure 6.
[0077] As shown in FIG. 6, the modified recycled carbon black has a Raman spectrum of 1350±10 cm in the Raman spectrum measured at an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 A peak with a peak top in the range of 1580 ± 20 cm (D band) -1 A peak (G band) having a peak top in the range of
[0078] Then, from the values of the peak intensity of the D band and the peak intensity of the G band, the peak intensity of the G band is calculated when the peak intensity of the D band is set to 100. According to the studies of the present inventors, the greater the amount of rubber charcoal attached to the recycled carbon black, the greater the intensity of the G band, and therefore it was found that the state of removal of the rubber charcoal from the recycled carbon black can be grasped based on the magnitude of the peak intensity of the G band compared with the peak intensity of the D band.
[0079] Fig. 6 is a Raman spectrum of an example of modified recycled carbon black, in which the peak intensity of the G band is 93 when the peak intensity of the D band is 100, which is in the range of 84 to 111. On the other hand, Fig. 7 is a Raman spectrum of an example of recycled carbon black before modification, in which the peak intensity of the G band is 113 when the peak intensity of the D band is 100, which is outside the range of 84 to 111. It can be seen that the recycled carbon black before modification shown in Fig. 7 has rubber charcoal attached to its surface, and the modified recycled carbon black shown in Fig. 6 has the rubber charcoal attached to its surface removed by modification.
[0080] The nitrogen adsorption specific surface area (N2SA) of modified recycled carbon black is 15m 2 / g or more 350m 2 / g or less. By having the nitrogen adsorption specific surface area N2SA of the recycled carbon black in the above range, the cohesive force of the recycled carbon black is kept low, and the reinforcing properties of rubber products are enhanced. From the viewpoint of optimizing the contact area with the rubber and improving the reinforcing properties of the rubber, the nitrogen adsorption specific surface area N2SA of the recycled carbon black is preferably 20 m 2 / g or more 300m 2 / g or less, more preferably 30m 2 / g or more 250m 2 On the other hand, if the nitrogen adsorption specific surface area N2SA of the recycled carbon black is less than the above range, the surface area in contact with the rubber is small, and the reinforcing effect is not fully exerted, resulting in a decrease in the reinforcing property of the rubber, whereas if it exceeds the above range, the cohesive force of the recycled carbon black becomes too high, resulting in a decrease in the reinforcing property of the rubber product.
[0081] In the present invention, the nitrogen adsorption specific surface area N2SA means a value measured by the amount of nitrogen adsorption in accordance with the method specified in JIS K6217-2 2001 "Testing method for basic performance of carbon black for rubber".
[0082] The DBP (Dibutylphthalate) absorption capacity of the modified recycled carbon black is 60 cm 3 / 100g or more 200cm 3 / 100g or less is preferable, and 70cm 3 / 100g or more 195cm 3 / 100g or less is preferable, and 80cm 3 / 100g or more 190cm 3 On the other hand, if the DBP absorption is less than the above range, the dispersibility of the carbon black deteriorates when the carbon black is compounded in a rubber composition, and the reinforcing properties of the resulting rubber tend to decrease, while if the DBP absorption exceeds the above range, the processability of the resulting rubber may decrease when the carbon black is compounded in a rubber composition.
[0083] In the present invention, the DBP absorption amount means a value measured by the method specified in JIS K6217-4 "Carbon black for rubber - Basic properties - Part 4, Determination of DBP absorption amount".
[0084] Modified recycled carbon black is obtained by modifying recycled carbon black, which is obtained by pyrolysis of rubber products such as waste tires. Therefore, the ash content of the modified recycled carbon black is 3.0% or more and 50.0% or less, and more preferably 5.0% or more and 35.0% or less.
[0085] In the present invention, the ash content means a value measured by the method specified in JIS K 6218-2. EXAMPLES
[0086] The invention will now be illustrated by the following examples.
[0087] Example 1 The modified recycled carbon black manufacturing apparatus 1 shown in FIG. 1 was used. First, city gas (composition: methane 88%, ethane 6%, propane 5%, butane 1%) was used as the fuel for the main burner at 16.0 Nm 3 / hour, with 215.0 Nm3 of air as oxygen-containing gas 3 / hour, the main burner was supplied with gas and air to generate a flame. Then, the supply of city gas and air was continued, and the flame generation was continued at 10.0 Nm 3 Using 15 kg / hour of conveying air, raw recycled carbon black was supplied to the main burner at 15 kg / hour and passed through the flame to carry out the main burner reforming process. The raw recycled carbon was crushed in advance using a cutter mixer. The reformed recycled carbon black that had passed through the flame was cooled with cooling water, and the gas was separated using a bag filter to obtain the reformed recycled carbon black. At this time, the main burner total carbon combustion rate was 79.0%. Also, the main burner flame combustion rate was 128.0%. Next, the nitrogen adsorption specific surface area N2SA of the modified recycled carbon black and the G band intensity were measured relative to the D band intensity of 100. As a result, the nitrogen adsorption specific surface area N2SA was 202 m 2 / g, and the G band intensity was 93 when the D band intensity was 100. In Example 1, the auxiliary burner reforming step was not performed.
[0088] ·Recycled raw carbon black Recycled carbon black obtained by pyrolysis of waste tires Enrestec PB365, Ash content: 18.6%, G band intensity when D band intensity is 100: 113 N2SA:76m 2 / g
[0089] Example 2 City gas 26.0Nm 3 / hour, 205.0 Nm3 of air as oxygen-containing gas 3 The reforming treatment was carried out under the same conditions as in Example 1, except that the feed rate was changed to 33 kg / hour and the raw recycled carbon black was changed to 33 kg / hour. At this time, the main burner total carbon combustion rate was 39.0%. Also, the main burner flame combustion rate was 72.0%. As a result, the nitrogen adsorption specific surface area N2SA was 62 m2 / g, and the G band intensity was 99 when the D band intensity was 100.
[0090] Example 3 In addition to the conditions in Example 2, 3.0 Nm of city gas was used as auxiliary fuel from the auxiliary burner. 3 / hour, 85.0Nm of air as oxygen-containing gas for auxiliary burner 3 / hour to generate a flame, and additional treatment was performed using the auxiliary burner flame. At this time, the main burner total carbon combustion rate was 39.0%. The main burner flame combustion rate was 72.0%. In addition, the auxiliary burner flame combustion rate was 258.0%, and the total carbon combustion rate of all burners was 52.0%. As a result, the nitrogen adsorption specific surface area N2SA was 162 m 2 / g, and the G band intensity was 94 when the D band intensity was 100. That is, in Example 3, a main burner reforming step and an auxiliary burner reforming step were performed.
[0091] Example 4 In addition to the conditions in Example 1, 12.0 Nm3 of city gas was used as auxiliary fuel from the auxiliary burner. 3 / hour, 30.0Nm of air as oxygen-containing gas for auxiliary burner 3 / hour to generate a flame, and additional treatment was performed using the auxiliary burner flame. At this time, the main burner total carbon combustion rate was 79.0%. The main burner flame combustion rate was 128.0%. In addition, the auxiliary burner flame combustion rate was 23.0%, and the total carbon combustion rate of all burners was 61.0%. As a result, the nitrogen adsorption specific surface area N2SA was 113 m 2 / g, and the G band intensity was 97 when the D band intensity was 100. That is, in Example 4, a main burner reforming step and an auxiliary burner reforming step were performed.
[0092] Example 5 The modified recycled carbon black manufacturing apparatus 1 shown in FIG. 1 was used in place of the auxiliary burner 4 with a fuel nozzle. First, city gas (composition: methane 88%, ethane 6%, propane 5%, butane 1%) was used as the fuel for the main burner at 16.0 Nm 3 / hour, with 215.0 Nm3 of air as oxygen-containing gas 3 / hour, the main burner was supplied with gas and air to generate a flame. Then, the supply of city gas and air was continued, and the flame generation was continued at 10.0 Nm 3 Using conveying air for 10 min / h, raw recycled carbon black was fed to the main burner at 15 kg / h, passed through the flame, and the main burner reforming process was carried out. 12.0 Nm3 of city gas was fed as fuel from the fuel nozzle. 3 / h, the auxiliary fuel pyrolysis process was carried out. At this time, the main burner total carbon combustion rate was 79.0%. Also, the main burner flame combustion rate was 128.0%. In addition, the total carbon combustion rate of the entire reaction was 54.0%. As a result, the nitrogen adsorption specific surface area N2SA was 90m 2 / g, and the G band intensity was 96 when the D band intensity was 100. That is, in Example 5, a main burner reforming step and an auxiliary fuel pyrolysis step were carried out. [Industrial Applicability]
[0093] According to the present invention, recycled carbon black, which has strong bonds with rubber components and has high reinforcing properties for rubber products, can be continuously produced. Therefore, rubber products having performance equivalent to that of unused carbon black can be industrially advantageously produced using recycled carbon black obtained by pyrolysis of rubber products such as waste tires. [Explanation of symbols]
[0094] 1. Modified recycled carbon black manufacturing equipment 2 Burner reformer 3 Main Burner 4 Auxiliary Burner 5. Cooling water supply pipe 6 Connecting pipe 7 Collection section 11 Fuel for main burner 12, 15 Oxygen-containing gases 13 Raw material recycled carbon black and conveying gas 14 Fuel for auxiliary burner 16 Cooling water 17 Gas 18 Modified recycled carbon black 21 Flame generated by the main burner 22 Direction of movement of raw recycled carbon black 23 Flame generated by auxiliary burner 30a, 30b Main burner 31 Fuel supply line for main burner 32 Oxygen-containing gas supply route 33 Supply route of raw material recycled carbon black and carrier gas 35 Main burner fuel outlet 36 Oxygen-containing gas outlet 37 Raw material recycled carbon black and carrier gas outlet 38 Mixing room
Claims
1. a main burner modifying step of continuously supplying a main burner fuel, an oxygen-containing gas, and recycled carbon black having rubber carbonized particles adhered thereto to a main burner which burns fuel to generate a flame, and combusting the main burner fuel; and continuously generating a flame in the main burner, while introducing the recycled carbon black having rubber carbonized particles adhered thereto and passing the flame through the main burner; The following formula (1): Main burner total carbon combustion rate (%) = (A / (B+C)) x 100 (1) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required for complete combustion of the recycled carbon black to which the rubber carbonized material is attached, which is supplied to the main burner, and C indicates the theoretical amount of oxygen required for complete combustion of the main burner fuel, which is supplied to the main burner.) The main burner total carbon combustion rate represented by is less than 100.0%; A method for producing modified recycled carbon black, comprising the steps of:
2. The main burner reforming process is carried out according to the following formula (2): Main burner flame combustion rate (%) = (A / C) x 100 (2) (In the formula, A represents the amount of oxygen supplied to the main burner, and C represents the theoretical amount of oxygen required to completely combust the main burner fuel supplied to the main burner.) A main burner reforming step (1) in which the main burner flame combustion rate represented by is 100.0% or more; The method for producing the modified recycled carbon black according to claim 1,
3. The main burner reforming process is carried out according to the following formula (2): Main burner flame combustion rate (%) = (A / C) x 100 (2) (In the formula, A represents the amount of oxygen supplied to the main burner, and C represents the theoretical amount of oxygen required to completely combust the main burner fuel supplied to the main burner.) A main burner reforming step (2) in which the main burner flame combustion rate represented by is less than 100.0%; The method for producing the modified recycled carbon black according to claim 1,
4. an auxiliary burner reforming step is provided downstream of the main burner, which burns an auxiliary burner fuel to generate a flame, and the recycled carbon black after the main burner reforming step (1) or (2) is continuously introduced into the flame generated by the auxiliary burner while the flame is being generated by the auxiliary burner, and the recycled carbon black is passed through the flame; The auxiliary burner reforming step is represented by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (In the formula, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner.) The auxiliary burner flame combustion rate represented by the following formula (4): is 100.0% or more. Total carbon combustion rate (%) of all burners = ((A + D) / (B + C + E)) x 100 (4) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto, which is supplied to the main burner, C indicates the theoretical amount of oxygen required for complete combustion of the main burner fuel, which is supplied to the main burner, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel, which is supplied to the auxiliary burner.) The auxiliary burner reforming step (1) is for making the total carbon combustion rate of all burners represented by the formula (1) less than 100.0%; The method for producing the modified recycled carbon black according to claim 2 or 3,
5. an auxiliary burner reforming step is provided downstream of the main burner, which burns an auxiliary burner fuel to generate a flame, and the recycled carbon black after the main burner reforming step (1) or (2) is continuously introduced into the flame generated by the auxiliary burner while the flame is being generated by the auxiliary burner, and the recycled carbon black is passed through the flame; The auxiliary burner reforming step is represented by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (In the formula, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner.) The auxiliary burner flame combustion rate represented by the following formula (4): is less than 100.0%. Total carbon combustion rate (%) of all burners = ((A + D) / (B + C + E)) x 100 (4) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto, which is supplied to the main burner, C indicates the theoretical amount of oxygen required for complete combustion of the main burner fuel, which is supplied to the main burner, D indicates the amount of oxygen supplied to the auxiliary burner, and E indicates the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel, which is supplied to the auxiliary burner.) The auxiliary burner reforming step (2) is for making the total carbon combustion rate of all burners represented by the formula (1) less than 100.0%; The method for producing the modified recycled carbon black according to claim 2 or 3,
6. an auxiliary fuel pyrolysis step of providing a fuel nozzle downstream of the main burner and introducing auxiliary fuel from the fuel nozzle into a flame generated by the main burner or in the vicinity thereof, thereby pyrolyzing the auxiliary fuel; The following formula (5): Total reaction total carbon combustion rate (%) = (A / (B + C + F)) x 100 (5) (In the formula, A indicates the amount of oxygen supplied to the main burner, B indicates the theoretical amount of oxygen required for complete combustion of the recycled carbon black to which rubber carbonized material is attached, which is supplied to the main burner, C indicates the theoretical amount of oxygen required for complete combustion of the main burner fuel, which is supplied to the main burner, and F indicates the theoretical amount of oxygen required for complete combustion of the auxiliary fuel, which is supplied from the fuel nozzle.) an auxiliary fuel pyrolysis step in which the total reaction total carbon combustion rate represented by The method for producing the modified recycled carbon black according to claim 2 or 3,
7. 2. The method for producing modified recycled carbon black according to claim 1, further comprising a particle size adjustment step of pulverizing and / or classifying the recycled carbon black to which the rubber carbonized material is attached prior to the main burner modification step.
8. A modified recycled carbon black obtained by the method for producing modified recycled carbon black according to any one of claims 1 to 7.
Citation Information
Patent Citations
Fin tube for heat exchange used for tunnel kiln
JP1983013985A
A method for obtaining a carbon black powder by pyrolyzing scrap rubber, the carbon black thus obtained and the use thereof
WO2013095145A1