Semiconductor storage device and method of manufacturing semiconductor storage device

By employing a crystalline semiconductor layer with additives and metal-induced lateral crystallization, the semiconductor memory device achieves reduced resistance and noise in the channel layer, enhancing memory cell performance.

JP2024157748AInactive Publication Date: 2024-11-08KIOXIA CORP

Patent Information

Application Number
JP2023072292
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing semiconductor memory devices face challenges in achieving low resistance and reducing noise in the channel layer, which affects the electrical characteristics of memory cells.

Method used

A semiconductor memory device with a crystalline semiconductor layer as the channel layer, incorporating additives like carbon, nitrogen, oxygen, and fluorine to minimize grain boundaries, and using metal-induced lateral crystallization to achieve a substantially single-crystal channel layer.

Benefits of technology

The solution results in lower resistance and reduced noise in the channel layer, improving the electrical performance of memory cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157748000001_ABST
    Figure 2024157748000001_ABST
Patent Text Reader

Abstract

To reduce a resistance of a channel layer and reduce a noise derived from the channel layer to improve electrical characteristics of a memory cell.SOLUTION: A semiconductor storage device according to an embodiment includes: a stacked body including a plurality of conductive layers and a plurality of insulating layers alternately stacked; and a plurality of pillars each including a core material extending in the stacked body in a first direction intersecting a surface of each of the plurality of conductive layers, a semiconductor layer covering a side surface of the core material, and a multi-layered insulating layer stacked on a side surface of the semiconductor layer, the semiconductor layer being crystalline, and the multi-layered insulating layer including a charge storage layer. Each of the semiconductor layers includes a crystal structure in which the appearance number of crystal grain boundaries per 1 μm in the first direction is less than 2 near to at least a first end in the first direction, and an additive that includes one or more of carbon, nitrogen, oxygen, and fluorine.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD Embodiments of the present invention relate to a semiconductor memory device and a method for manufacturing a semiconductor memory device. [Background technology]

[0002] In a three-dimensional nonvolatile memory, for example, a pillar having a semiconductor layer as a channel layer and a multilayer insulating layer as a memory layer penetrates a stack of multiple conductive layers. The semiconductor layer as the channel layer is preferably single crystalline over the entire extension direction of the pillar. This reduces the resistance of the channel layer and reduces noise originating from the channel layer, thereby improving the electrical characteristics of the memory cell formed at the intersection with the multiple conductive layers. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-103742 A [Patent Document 2] JP 2004-165185 A [Patent Document 3] JP 2009-194259 A [Patent Document 4] JP 2020-141008 A Summary of the Invention [Problem to be solved by the invention]

[0004] One embodiment aims to provide a semiconductor memory device and a method for manufacturing a semiconductor memory device that can reduce the resistance of a channel layer and noise originating from the channel layer, thereby improving the electrical characteristics of a memory cell. [Means for solving the problem]

[0005] The semiconductor memory device of the embodiment comprises a stack in which a plurality of conductive layers and a plurality of insulating layers are alternately stacked, and a plurality of pillars each including a core material extending within the stack in a first direction intersecting each of the faces of the plurality of conductive layers, a crystalline semiconductor layer covering a side of the core material, and a multilayer insulating layer stacked on a side of the semiconductor layer including a charge storage layer, and each of the semiconductor layers has a crystal structure in which the number of crystal grain boundaries per μm in the first direction is less than two, at least on a first end side in the first direction, and contains one or more additives selected from the group consisting of carbon, nitrogen, oxygen, and fluorine. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a block diagram of a semiconductor memory device according to an embodiment. [Diagram 2] FIG. 2 is an equivalent circuit diagram showing an example of a configuration of a memory cell array included in the semiconductor memory device according to the embodiment. [Diagram 3] 1 is a cross-sectional view showing a schematic configuration example of a semiconductor memory device according to an embodiment. [Figure 4] FIG. 1 is a diagram showing an example of a configuration of a semiconductor memory device according to an embodiment. [Diagram 5] 3A and 3B are schematic diagrams showing the crystal structure of channel layers included in multiple pillars of the semiconductor memory device according to the embodiment. [Figure 6] 1A to 1C are diagrams illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to an embodiment. [Figure 7] 1A to 1C are diagrams illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to an embodiment. [Figure 8] 1A to 1C are diagrams illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to an embodiment. [Figure 9] 1A to 1C are diagrams illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to an embodiment. [Figure 10] 1A to 1C are diagrams illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to an embodiment. [Figure 11] 1A to 1C are diagrams illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to an embodiment. [Figure 12] 1A to 1C are diagrams illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to an embodiment. [Figure 13] 1A to 1C are diagrams illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to an embodiment. [Figure 14] 11 is an enlarged cross-sectional view of a memory hole showing how an amorphous channel layer is converted into a crystalline channel layer according to a comparative example. [Figure 15] 4 is a graph showing an appropriate position of a doped layer introduced into a channel layer according to an embodiment. [Figure 16] 10A to 10C are enlarged cross-sectional views illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to a modified example of the embodiment in order. [Figure 17] 10A to 10C are enlarged cross-sectional views illustrating a part of a procedure of a manufacturing method of a semiconductor memory device according to a modified example of the embodiment in order. [Figure 18] FIG. 13 is a cross-sectional view showing an example of a configuration of a semiconductor memory device according to another modified example of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to the following embodiment. In addition, the components in the following embodiment include those that a person skilled in the art can easily imagine or that are substantially the same.

[0008] (Functional configuration of semiconductor memory device) 1 is a block diagram of a semiconductor memory device 1 according to an embodiment. As shown in FIG. 1, the semiconductor memory device 1 includes an input / output circuit 310, a logic control circuit 320, a status register 330, an address register 340, a command register 350, a sequencer 360, a ready / busy circuit 370, a voltage generating circuit 380, a memory cell array 510, a row decoder 520, a sense amplifier module 530, a data register 540, and a column decoder 550.

[0009] The input / output circuit 310 controls input / output of a signal DQ to / from an external device such as a memory controller (not shown) that controls the semiconductor memory device 1. The input / output circuit 310 includes an input circuit and an output circuit (not shown).

[0010] The input circuit transmits data DAT, such as write data WD received from an external device, to the data register 540 , transmits an address ADD to the address register 340 , and transmits a command CMD to the command register 350 .

[0011] The output circuit transmits the status information STS received from the status register 330, the data DAT such as the read data RD received from the data register 540, and the address ADD received from the address register 340 to an external device.

[0012] The logic control circuit 320 receives, for example, a chip enable signal CEn, a command latch enable signal CLE, an address latch enable signal ALE, a write enable signal WEn, and a read enable signal REn from an external device. The logic control circuit 320 also controls the input / output circuit 310 and the sequencer 360 in response to the received signals.

[0013] The status register 330 temporarily holds status information STS for, for example, data write, read, and erase operations, and notifies an external device as to whether or not the operation has ended normally.

[0014] The address register 340 temporarily holds an address ADD received from an external device via the input / output circuit 310. The address register 340 also transfers a row address RA to a row decoder 520 and a column address CA to a column decoder 550.

[0015] The command register 350 temporarily stores a command CMD received from an external device via the input / output circuit 310 , and transfers the command CMD to the sequencer 360 .

[0016] The sequencer 360 controls the overall operation of the semiconductor memory device 1. More specifically, the sequencer 360 controls, for example, the status register 330, the ready / busy circuit 370, the voltage generating circuit 380, the row decoder 520, the sense amplifier module 530, the data register 540, and the column decoder 550 in response to the command CMD held by the command register 350, and executes a write operation, a read operation, an erase operation, and the like.

[0017] The ready / busy circuit 370 transmits a ready / busy signal R / Bn to an external device according to the operating status of the sequencer 360 .

[0018] The voltage generation circuit 380 generates voltages necessary for write, read, and erase operations under the control of the sequencer 360, and supplies the generated voltages to, for example, the memory cell array 510, the row decoder 520, and the sense amplifier module 530. The row decoder 520 and the sense amplifier module 530 apply the voltages supplied from the voltage generation circuit 380 to the memory cells in the memory cell array 510.

[0019] The memory cell array 510 includes a plurality of blocks BLK (BLK0 to BLKn), where n is an integer equal to or greater than 2. A block BLK is a set of a plurality of memory cells associated with bit lines and word lines, and serves as, for example, a data erase unit. The memory cells are configured as, for example, transistors, and hold non-volatile data.

[0020] By including such memory cells, the semiconductor memory device 1 is configured as, for example, a NAND type nonvolatile memory.

[0021] The row decoder 520 decodes the row address RA, selects one of the blocks BLK based on the result of the decoding, and applies a required voltage to the block BLK.

[0022] During a read operation, the sense amplifier module 530 senses data read from the memory cell array 510. In addition, the sense amplifier module 530 transmits read data RD to the data register 540. During a write operation, the sense amplifier module 530 transmits write data WD to the memory cell array 510.

[0023] The data register 540 includes a plurality of latch circuits. The latch circuits hold write data WD and read data RRD. For example, in a write operation, the data register 540 temporarily holds the write data WD received from the input / output circuit 310 and transmits it to the sense amplifier module 530. For example, in a read operation, the data register 540 temporarily holds the read data RD received from the sense amplifier module 530 and transmits it to the input / output circuit 310.

[0024] The column decoder 550 decodes a column address CA during, for example, a write operation, a read operation, or an erase operation, and selects a latch circuit in the data register 540 according to the decoded result.

[0025] The group of circuits arranged around the memory cell array 510 is also called peripheral circuits. The peripheral circuits include at least a row decoder 520, a sense amplifier module 530, a data register 540, and a column decoder 550. The peripheral circuits may include a status register 330, an address register 340, a command register 350, and a sequencer 360, and may further include an input / output circuit 310, a logic control circuit 320, a ready / busy circuit 370, and a voltage generation circuit 380.

[0026] Thus, the semiconductor memory device 1 includes a memory cell array 510 including a plurality of memory cells, and a peripheral circuit that operates the plurality of memory cells.

[0027] FIG. 2 is an equivalent circuit diagram showing an example of the configuration of the memory cell array 510 included in the semiconductor memory device 1 according to the embodiment.

[0028] As described above, the memory cell array 510 includes a plurality of blocks BLK. Each of the plurality of blocks BLK includes a plurality of string units SU. Each of the plurality of string units SU includes a plurality of memory strings MS. One end of each of the plurality of memory strings MS is connected to a peripheral circuit such as a sense amplifier module 530 via a bit line BL. The other end of each of the plurality of memory strings MS is connected to the peripheral circuit via a common source line SL.

[0029] The memory string MS includes a drain select transistor STD connected in series between a bit line BL and a source line SL, a plurality of memory cells MC, and a source select transistor STS. Hereinafter, the drain select transistor STD and the source select transistor STS may be simply referred to as select transistors (STD, STS).

[0030] The memory cells MC are, for example, field effect transistors (FETs) that include a charge storage layer in a gate insulating layer. The threshold voltage of the memory cells MC varies depending on the amount of charge in the charge storage layer. By providing one or more threshold voltages, the memory cells MC may be able to store one or more bits of data. A word line WL is connected to each of the gate electrodes of the memory cells MC corresponding to one memory string MS. Each of these word lines WL is commonly connected to all the memory strings MS in one block BLK.

[0031] The selection transistors (STD, STS) are, for example, field effect transistors. Selection gate lines (SGD, SGS) are connected to the gate electrodes of the selection transistors (STD, STS), respectively. The drain selection line SGD connected to the drain selection transistor STD is provided corresponding to the string unit SU, and is commonly connected to all the memory strings MS in one string unit SU. The source selection line SGS connected to the source selection transistor STS is commonly connected to all the memory strings MS in one block BLK.

[0032] One end of each of the word lines WL and the select gate lines (SGD, SGS) is connected to peripheral circuits such as a row decoder 520.

[0033] (Physical configuration of semiconductor memory device) 3 is a cross-sectional view showing an example of a schematic physical configuration of the semiconductor memory device 1 according to the embodiment, in which hatching is omitted for ease of viewing.

[0034] 3, the semiconductor memory device 1 includes, from the bottom of the page, an electrode layer EL, a source line SL, a select gate line SGD, a plurality of word lines WL, and a select gate line SGS. The semiconductor memory device 1 also includes a peripheral circuit CBA provided on a semiconductor substrate SB above the select gate line SGD.

[0035] A source line SL is disposed on the electrode layer EL via an insulating layer 60. A plurality of plugs PG are disposed in the insulating layer 60, and the source line SL and the electrode layer EL are kept electrically conductive via the plugs PG. This allows a source potential to be applied to the source line SL from the above-mentioned voltage generating circuit 380 (see FIG. 1) via the electrode layer EL and the plugs PG.

[0036] On the source line SL, one or more select gate lines SGD, a plurality of word lines WL, and one or more select gate lines SGS are stacked in this order. A memory region MR is arranged on the word lines WL, and a contact region ER is arranged at the end of the word lines WL in the direction in which they extend.

[0037] In the memory region MR, a plurality of pillars PL are arranged, which penetrate the word lines WL in the stacking direction. A plurality of memory cells MC (see FIG. 2) are formed at the intersections between the pillars PL and the word lines WL. This allows the semiconductor memory device 1 to be configured as, for example, a three-dimensional nonvolatile memory in which the memory cells MC are arranged three-dimensionally in the memory region MR.

[0038] Thus, the memory region MR is an example of a physical configuration corresponding to the above-mentioned memory cell array 510 (see FIG. 2). Also, the pillar PL is an example of a physical configuration corresponding to the above-mentioned memory string MS (see FIG. 2) in which memory cells MC and the like are connected in series.

[0039] In the physical configuration of the semiconductor memory device 1, the pillars PL are electrically connected to the peripheral circuit CBA via bit lines BL arranged above the pillars PL.

[0040] In the contact region ER, a plurality of contacts CC are arranged, which are connected to the plurality of word lines WL and the selection gate lines SGD, SGS, respectively.

[0041] A write voltage, a read voltage, etc. are applied to the memory cells MC included in the memory region MR at the center in the direction in which the word lines WL extend through the contacts CC via the word lines WL at the same height as the memory cells MC. In this way, the word lines WL and the select gate lines SGD, SGS, which are stacked in multiple layers, are individually drawn out by these contacts CC.

[0042] The word lines WL, the select gate lines SGD, SGS, the pillars PL, and the contacts CC are covered with an insulating layer 50. The insulating layer 50 also extends around the word lines WL and the like.

[0043] The semiconductor substrate SB above the insulating layer 50 is, for example, a silicon substrate. On the surface of the semiconductor substrate SB, the peripheral circuit CBA, such as the row decoder 520 including the transistors TR and wiring, and the sense amplifier module 530 (see FIG. 1), are arranged. Various voltages applied to the memory cells MC from the contacts CC are controlled by the peripheral circuit CBA, which is electrically connected to these contacts CC. Data read from the memory cells MC aligned in the height direction of the pillar PL is read to the sense amplifier module 530 of the peripheral circuit CBA. In this way, the peripheral circuit CBA controls the electrical operation of the memory cells MC.

[0044] The peripheral circuit CBA is covered with an insulating layer 40, and by joining this insulating layer 40 to an insulating layer 50 covering a plurality of word lines WL, etc., a semiconductor memory device 1 is formed that includes a configuration of a plurality of word lines WL, select gate lines SGD, SGS, pillars PL, contacts CC, etc., and the peripheral circuit CBA.

[0045] Next, a detailed configuration example of the semiconductor memory device 1 will be described with reference to FIGS.

[0046] FIG. 4 is a diagram showing an example of a configuration of the semiconductor memory device 1 according to the embodiment.

[0047] More specifically, Fig. 4(a) is a cross-sectional view along the Y direction including the memory region MR of the semiconductor memory device 1. In Fig. 4(a), the structure above the insulating layer 53, which is a part of the insulating layer 50, and the structure below the source line SL are omitted.

[0048] Fig. 4(b) is a cross-sectional view of the pillar PL in the Y direction at the height of any select gate line SGD. Fig. 4(c) is a cross-sectional view of the pillar PL in the Y direction at the height of any word line WL. Fig. 4(d) is a cross-sectional view of the pillar PL in the Y direction at the height of any select gate line SGS.

[0049] In this specification, the X and Y directions are both directions along the plane of the word lines WL, and are perpendicular to each other. The stacking direction of the word lines WL is sometimes called the first direction, and this first direction is a direction that intersects with the X and Y directions.

[0050] In addition, in this specification, the side where the drain side select gate line SGD is arranged is the upper side of the semiconductor memory device 1, and the side where the source side select gate line SGS is arranged is the lower side of the semiconductor memory device 1. Such a vertical direction of the semiconductor memory device 1 also coincides with the penetration direction of the pillar PL in the manufacturing method of the semiconductor memory device 1 described later. In other words, the upper end of the pillar PL in the penetration direction is the upper side of the semiconductor memory device 1, and the lower end of the pillar PL in the penetration direction is the lower side of the semiconductor memory device 1.

[0051] 4, a stacked body LM is disposed on a source line SL, which is, for example, a conductive polysilicon layer, via an insulating layer 55, for example. The stacked body LM has a configuration in which a plurality of word lines WL and a plurality of insulating layers OL are alternately stacked one by one. Furthermore, one or more select gate lines SGD are disposed on an insulating layer OL above the top word line WL. Furthermore, one or more select gate lines SGS are disposed on an insulating layer OL below the bottom word line WL.

[0052] That is, the select gate line SGS shown in Fig. 4(d) is disposed on the source line SL via, for example, an insulating layer 55, and insulating layers 51, 52, and 53 covering the upper surface of the laminate LM are disposed in this order above the select gate line SGD shown in Fig. 4(b). Note that these insulating layers 51 to 53, 55 constitute a part of the insulating layer 50 (see Fig. 3) described above.

[0053] Here, the number of stacked word lines WL and select gate lines SGD, SGS as the multiple conductive layers in the laminate LM is arbitrary. As an example, the number of stacked word lines WL and select gate lines SGD, SGS in the laminate LM can be several tens to several hundreds. The word lines WL and select gate lines SGD, SGS are, for example, tungsten layers or molybdenum layers. The insulating layers OL, 51 to 53, 55 are, for example, silicon oxide layers.

[0054] The laminate LM is divided in the Y direction by a number of plate-shaped portions PT. Fig. 4(a) shows one of the plate-shaped portions PT.

[0055] The plate-shaped portions PT are aligned in the Y direction and extend in the stacking direction and the X direction of the laminate LM. More specifically, the plate-shaped portions PT penetrate the insulating layers 52 and 51, the laminate LM, and the insulating layer 55 to reach the source line SL, and extend continuously within the laminate LM from one end to the other end in the X direction of the laminate LM. Each of the plate-shaped portions PT is formed as a single unit of the insulating layer 54, such as a silicon oxide layer.

[0056] In the memory region MR, a plurality of isolation layers SHE are disposed between the plate-like portions PT adjacent in the Y direction, penetrating the upper layer portion of the laminate LM and extending in the X direction. These isolation layers SHE are insulating layers 56 such as silicon oxide layers that penetrate the select gate lines SGD and reach the insulating layers OL directly below.

[0057] In other words, these separation layers SHE penetrating the upper part of the laminate LM extend in the X direction within the memory region MR between the plate-shaped portions PT, thereby dividing the upper part of the laminate LM into the above-mentioned select gate lines SGD.

[0058] The region between adjacent plate-like portions PT in the Y direction is an example of a physical configuration corresponding to one block BLK (see FIG. 2) described above. Also, the region between adjacent plate-like portions PT, partitioned into a pattern of the select gate line SGD by the separation layer SHE, is an example of a physical configuration corresponding to the string unit SU (see FIG. 2) described above.

[0059] In the memory region MR of the laminate LM, a plurality of pillars PL are distributed and arranged, which penetrate the insulating layer 51, the laminate LM, and the insulating layer 55 to reach the source line SL.

[0060] The pillars PL are arranged, for example, in a staggered pattern when viewed from the stacking direction of the laminate LM. Each pillar PL has a cross-sectional shape, for example, a circular, elliptical, oval, or the like, in the direction along the layer direction of the laminate LM, i.e., the direction along the XY plane.

[0061] Each of these pillars PL has a tapered shape in which the cross-sectional area and diameter along the XY plane become smaller from the upper end to the lower end. Alternatively, each of these pillars PL has a bowing shape in which the cross-sectional area and diameter along the XY plane are smaller at the lower end than at the upper end and the cross-sectional area and diameter along the XY plane are maximum between the upper end and the lower end. Such a shape of the pillars PL is obtained according to the penetration direction of the pillars PL in the manufacturing method of the semiconductor memory device 1 described later.

[0062] In other words, the penetration direction of the pillars PL can also be determined by the shape of the pillars PL. That is, the side with a larger cross-sectional area and diameter along the XY plane is generally the upper end in the penetration direction of the pillar PL, and the side with a smaller cross-sectional area and diameter is generally the lower end in the penetration direction of the pillar PL.

[0063] Each of the multiple pillars PL has a core layer CR that extends in the stacking direction within the laminate LM and serves as the core material of the pillar PL, a channel layer CN that covers the side surfaces of the core layer CR and has an upper cap layer CP and a lower cap layer EP arranged at both vertical and horizontal ends, and a memory layer ME that covers the side surfaces of the upper cap layer CP, the channel layer CN, and the lower cap layer EP.

[0064] As shown in Figures 4(b) to 4(d), the memory layer ME is a multi-layer insulating layer in which a block insulating layer BK, a charge storage layer CT, and a tunnel insulating layer TN are stacked in this order from the outer periphery of the pillar PL. The channel layer CN is inside the memory layer ME and extends in the stacking direction within the stacked body LM. A core layer CR is filled further inside the channel layer CN.

[0065] The lower cap layer EP is disposed at the lower end of the channel layer CN, and is connected to the source line SL below the stack LM. In this manner, the lower cap layer EP connects the channel layer CN and the source line SL.

[0066] The upper cap layer CP is disposed on the upper end of the channel layer CN, and is connected to the bit line BL disposed in the insulating layer 53 via a plug CH disposed in the insulating layers 52 and 53. In this manner, the channel layer CN and the bit line BL are connected by the upper cap layer CP. The bit line BL extends above the stacked body LM in a direction, for example, along the Y direction, so as to intersect with the lead-out direction of the word line WL.

[0067] In Fig. 4(a), in the section separated by the separation layer SHE, a plug CH is connected to only one pillar PL. The other pillars PL are connected to other bit lines BL extending in the Y direction parallel to the bit lines BL shown in Fig. 4(a) at positions different from the cross section shown in Fig. 4(a) via plugs CH not shown in Fig. 4(a).

[0068] The block insulating layer BK and the tunnel insulating layer TN of the memory layer ME, and the core layer CR are, for example, silicon oxide layers, etc. The charge storage layer CT of the memory layer ME is, for example, a silicon nitride layer, etc. The channel layer CN, the upper cap layer CP, and the lower cap layer EP are semiconductor layers such as silicon layers, and the lower cap layer EP further contains an N-type dopant (impurity) such as phosphorus.

[0069] More specifically, the channel layer CN is a crystalline semiconductor layer that is substantially entirely single crystal. The channel layer CN may partially contain polycrystals. The upper cap layer CP and the lower cap layer EP are amorphous silicon layers or polysilicon layers, etc. Alternatively, the upper cap layer CP and the lower cap layer EP may contain a mixture of amorphous and polycrystalline portions at a predetermined ratio. The upper cap layer CP and the lower cap layer EP may partially be single crystallized.

[0070] With the above-described configuration, memory cells MC are formed on the side surfaces of the pillars PL in portions facing the individual word lines WL. When a predetermined voltage is applied from the word lines WL, data is written to and read from the memory cells MC.

[0071] In addition, with the above-mentioned configuration, a select gate STD is formed where the side of the pillar PL faces the select gate line SGD arranged in the upper layer of the word line WL, and a select gate STS is formed where the side of the pillar PL faces the select gate line SGS arranged in the lower layer of the word line WL.

[0072] By applying a predetermined voltage from the select gate lines SGD, SGS, respectively, the select gates STD, STS are turned on or off, so that the memory cell MC of the pillar PL to which the select gates STD, STS belong can be placed in a selected or unselected state.

[0073] Here, the channel layer CN contains a predetermined additive. The additive contained in the channel layer CN is an electrically inactive element different from the impurity element that imparts the P-type or N-type conductivity to the semiconductor layer, and has a property of inhibiting crystallization of a semiconductor layer such as the channel layer CN. As an example, the additive may be at least one of carbon, nitrogen, oxygen, and fluorine.

[0074] The channel layer CN may contain at least one metal element selected from the group consisting of nickel, palladium, and aluminum.

[0075] These additives and metal elements may be unevenly distributed in the channel layer CN. An example of such a case is shown in Figures 4(b) to 4(d).

[0076] The region CNb near the core layer CR shown in Figures 4(b) to 4(d) is a region where the above-mentioned additive has a peak concentration, and the region CNa near the tunnel layer TN shown in Figures 4(b) to 4(d) is a region where the above-mentioned metal element may be included.

[0077] More specifically, the concentration of the additive increases from the tunnel insulating layer TN side to the core layer CR side in the thickness direction of the channel layer CN. Therefore, these additives may be diffused not only in the region CNb but also throughout the channel layer CN. However, apart from nitrogen, oxygen, fluorine, and the like that tend to diffuse in the channel layer CN, when the additive is carbon, etc., the additive may have a peak concentration at least in the region CNb.

[0078] In addition, the metal element that may be contained in the region CNa may also be diffused throughout the channel layer CN. However, it is considered that the metal element is likely to be detected in a portion adjacent to the peak concentration position of the additive in the region CNa in the thickness direction of the channel layer CN.

[0079] As described above, the channel layer CN is substantially entirely made of single crystal, and the fact that it has the regions CNa and CNb does not mean that the channel layer CN is divided into these regions CNa and CNb.

[0080] FIG. 5 is a schematic diagram showing the crystal structure of the channel layers CN included in the pillars PL of the semiconductor memory device 1 according to the embodiment.

[0081] 5(a) is an XY cross-sectional view of the lower end side of multiple pillars PL, and shows a schematic diagram of the crystal analysis result of the channel layer CN of the pillar PL. Such crystal analysis can be performed using, for example, a BF-STEM (Bright-Field Scanning Transmission Electron Microscope) or the like.

[0082] Fig. 5(b) is a cross-sectional view along the extension direction of a pillar PL having a channel layer CN containing polycrystals, and Fig. 5(c) is a cross-sectional view along the extension direction of a pillar PL having a channel layer CN not containing polycrystals.

[0083] 5(a) show the XY cross section of the channel layer CN of each pillar PL. That is, the outer edge of the donut-shaped ring is the outer wall part of the channel layer CN that contacts the memory layer ME, and the inner edge of the donut-shaped ring is the inner wall part of the channel layer CN that contacts the core layer CR.

[0084] As shown in Fig. 5(a), the channel layer CN of many pillars PL is made of a single crystal. On the other hand, in some pillars PL, the ring representing the channel layer CN is divided into multiple parts, which indicates that the channel layer CN is polycrystallized at least in the cross section of Fig. 5(a). Thus, among the multiple pillars PL, a certain ratio of pillars PL exist as first pillars having a channel layer CN that is partially polycrystallized.

[0085] As shown in FIG. 5(b), in such a pillar PL, the channel layer CN is more likely to be polycrystallized from the upper end side as the first end toward the lower end side as the second end.

[0086] That is, in such pillars PL, the average grain size of the crystals contained in the channel layer CN decreases from the upper end to the lower end. The average grain size of the crystals in the channel layer CN at this time is, for example, 1 μm or more on the upper end side. The average grain size of the crystals in the channel layer CN at this time is, for example, 5 nm to 100 nm, typically, for example, 20 nm to 30 nm, on the lower end side.

[0087] Therefore, as described above, the ratio of the pillars PL in which a part of the channel layer CN is polycrystallized tends to increase from the upper end side to the lower end side of the pillars PL.

[0088] For this reason, it can be seen that the channel layers CN of some of the pillars PL are polycrystallized at the bottom end side of the multiple pillars PL shown in Fig. 5(a). In this way, the ratio of the pillars PL in which grain boundaries appear in the channel layers CN due to the channel layers CN being polycrystallized in a part near the bottom end, etc., is, for example, 4% or less of the entire multiple pillars PL. In addition, the lower limit of the ratio of the pillars PL in which grain boundaries appear in the channel layers CN is, for example, 0.1% or more, preferably 0.05% or more, and more preferably 0.01% or more.

[0089] On the other hand, at the upper end side of the multiple pillars PL, the ratio of the pillars PL in which grain boundaries appear in the channel layer CN among all the multiple pillars PL is, for example, less than 1%.Also, near the center in the extension direction of the multiple pillars PL, the ratio of the pillars PL in which grain boundaries appear in the channel layer CN among all the multiple pillars PL is, for example, less than 2%.

[0090] Here, when the extension distance of the pillars PL is, for example, several μm to 10 μm, the upper end side of these pillars PL is, for example, a height position 0.5 μm lower than the upper end of the pillar PL, and the lower end side of these pillars PL is, for example, a height position 0.5 μm higher than the lower end of the pillar PL.

[0091] However, as described later, the distance from the bottom end of the pillar PL at which the channel layer CN has the above-mentioned crystal structure may vary depending on the treatment that the channel layer CN undergoes after the formation of the channel layer CN.

[0092] 5(b) and 5(c), the crystal structure of the channel layer CN of the pillar PL can be defined from a different perspective. That is, the crystal structure of the channel layer CN can be defined by the number of grain boundaries (CNg in FIG. 5(b)) that appear in the channel layer CN within a given distance in the extension direction of the pillars PL.

[0093] In this case, in the channel layer CN at least on the upper end side of the multiple pillars PL, the number of grain boundaries per 1 μm in the extension direction of the pillars PL is, for example, less than 0.5. In other words, when observing the crystal structure of the channel layer CN at the upper end side of the multiple pillars PL for a distance of 1 μm along the extension direction of the pillars PL, less than 0.5 grain boundaries can be observed in the channel layer CN.

[0094] On the other hand, in the case of a pillar PL having a channel layer CN partially polycrystallized, the number of crystal grain boundaries appearing per 1 μm in the extension direction of the pillar PL in the channel layer CN on the lower end side of the pillar PL may be, for example, 10 or more, and typically is, for example, 20 to 30.

[0095] (Method of manufacturing semiconductor memory device) Next, a method for manufacturing the semiconductor memory device 1 according to the embodiment will be described with reference to Figures 6 to 13. Figures 6 to 13 are diagrams illustrating, in order, some of the steps of the method for manufacturing the semiconductor memory device 1 according to the embodiment.

[0096] First, a state in which a memory hole MH is formed in a laminated body LMs before the word line WL is formed is shown in Fig. 6. Fig. 6 is a cross-sectional view along the Y direction of a region that will later become a memory region MR.

[0097] 6(a), an insulating layer 55 such as a silicon oxide layer is formed on a support substrate SS. As the support substrate SS, a semiconductor substrate such as a silicon substrate, an insulating substrate such as a ceramic substrate, or a conductive substrate such as an alumina substrate can be used.

[0098] A laminate LMs in which insulating layers NL as a plurality of first insulating layers and insulating layers OL as a plurality of second insulating layers are alternately laminated is formed on the insulating layer 55. The insulating layers NL are, for example, silicon nitride layers, and function as sacrificial layers that are later replaced with a conductive material to become the word lines WL or the select gate lines SGD, SGS.

[0099] Moreover, an insulating layer 51 such as a silicon oxide layer is formed to cover the upper surface of the laminated body LMs.

[0100] 6(b), a plurality of memory holes MH are formed in the laminate LMs, extending in the lamination direction. The memory holes MH are formed in regions that will later become memory regions MR, and penetrate the insulating layer 51, the laminate LMs, and the insulating layer 55 to reach the support substrate SS.

[0101] Here, the memory hole MH usually has a tapered shape in which the cross-sectional area and diameter along the XY plane become smaller in the penetration direction in the laminate LMs, that is, from the upper end to the lower end, or a bowing shape in which the cross-sectional area and diameter along the XY plane become maximum between the upper and lower ends. Such a shape of the memory hole MH is also maintained in the pillar PL formed from the memory hole MH. Thereby, in the semiconductor memory device 1 finally obtained, it may be possible to distinguish the penetration direction of the pillar PL.

[0102] In FIG. 6(b), the portion of the laminate LMs on the left side of the drawing where the memory hole MH is not formed is a region where the plate-shaped portion PT will be formed later.

[0103] As shown in Fig. 6(c), a block insulating layer BK, a charge storage layer CT, and a tunnel insulating layer TN (see Figs. 4(b) to (d)) are stacked in this order in each of the memory holes MH to form a memory layer ME that covers the side walls and bottom surfaces of the memory holes MH. The memory layer ME is also formed on the upper surface of the insulating layer 51.

[0104] Next, a state in which a channel layer CNs, a part of which will later become the above-mentioned channel layer CN (see FIG. 4), is formed in the memory hole MH is shown in FIG. 7. FIG. 7 is an enlarged cross-sectional view of the memory hole MH in which the memory layer ME is formed.

[0105] 7(a) to 7(c), a raw material gas for a semiconductor layer such as a silicon layer is supplied to form a channel layer CNs that covers the memory layer ME already formed in the memory hole MH. The channel layer CNs as a first semiconductor layer is a non-crystalline semiconductor layer such as an amorphous silicon layer, and is formed to be thicker than the above-mentioned channel layer CN.

[0106] 7(a), a non-doped layer CNsa is initially formed to cover the memory layer ME by using a raw material gas that does not contain additives, etc. The non-doped layer CNsa is preferably formed to have a thickness that is less than 5% or at most 25% of the thickness that the amorphous channel layer CNs will ultimately have.

[0107] At the interface with the memory layer ME, the structure of the non-doped layer CNsa, which is an amorphous silicon layer, may be disturbed. Such a structural disturbance of the non-doped layer CNsa may be, for example, a portion where the density of silicon atoms is higher than in other portions, and may become a crystal nucleus CNn when the amorphous channel layer CNs is crystallized later.

[0108] 7B, after the non-doped layer CNsa is formed, the supply of the source gas is continued while adding at least one of carbon, nitrogen, oxygen, and fluorine, so that the doped layer CNsb to which the additive is added is formed so as to cover the non-doped layer CNsa. 19 More than 1×10 21 atoms / cm 3 The following applies.

[0109] The doped layer CNsb is formed so that the thickness thereof, including the non-doped layer CNsa, is less than 50% of the thickness that the amorphous channel layer CNs will ultimately have, and more preferably is 5% or more and less than 25%.

[0110] 7(c), even after the addition of the additive is stopped, the supply of the raw material gas is continued for a predetermined period of time, so that the non-doped layer CNsc is formed so as to cover the doped layer CNsb. When the non-doped layer CNsc becomes thicker than the above-mentioned channel layer CN, the formation of the channel layer CNs is completed.

[0111] The above numerical values ​​for the thicknesses of the non-doped layer CNsa, the doped layer CNsb, and the non-doped layer CNsc are merely approximate values, not taking into account the volume change accompanying the conversion of the crystal structure from amorphous to crystalline. Furthermore, the additive added during the formation of the doped layer CNsb may be at least partially diffused into the non-doped layers CNsa and CNsc through subsequent processing. Even in this case, it is preferable that the additive has a peak concentration in the doped layer CNsb.

[0112] As a result of the above, an amorphous channel layer CNs is formed that covers the sidewall and bottom surface of the memory hole MH via the memory layer ME. The channel layer CNs is also formed on the upper surface of the insulating layer 51 via the memory layer ME.

[0113] However, in the above, for convenience of explanation, the channel layer CNs has a non-doped layer CNsa, a doped layer CNsb, and a non-doped layer CNsc, but the channel layer CNs is formed by adding an additive at a predetermined timing for a predetermined period while continuing to supply a raw material gas. Therefore, the non-doped layer CNsa, the doped layer CNsb, and the non-doped layer CNsc may be seamlessly formed in the channel layer CNs.

[0114] Next, the state in which the amorphous channel layer CNs is crystallized to form the channel layer CN is shown in Fig. 8. Fig. 8 is a cross-sectional view along the Y direction of a region that will later become the memory region MR, similar to Fig. 6 described above.

[0115] FIG. 8(a) shows a state in which the channel layer CNs is formed on the sidewall and bottom surface of the memory hole MH and on the upper surface of the insulating layer 51 via the memory layer ME.

[0116] As shown in FIG. 8(b), the inside of the channel layer CNs of the memory hole MH is filled with a core layer CRs. The core layer CRs is, for example, a silicon oxide layer, and functions as a sacrificial layer that is removed in a later process. The core layer CRs is also formed on the upper surface of the insulating layer 51 via the channel layer CNs and the memory layer ME.

[0117] 8(c), the core layer CRs is etched back and removed from the upper surface of the insulating layer 51 and the upper end of the memory hole MH. This exposes the channel layer CNs on the upper surface of the insulating layer 51. In addition, the upper end of the core layer CRs is positioned at a predetermined depth within the memory hole MH, and a recess RCc is formed above the core layer CRs.

[0118] The recess RCc in the memory hole MH can be obtained by continuing overetching for a predetermined time even after the core layer CRs on the upper surface of the insulating layer 51 is removed, for example.

[0119] 8(d), a cap layer CPs is formed to cover the channel layer CNs on the upper surface of the insulating layer 51. The cap layer CPs is a sacrificial layer such as an amorphous silicon layer, and is removed in a later process. The cap layer CPs is also filled in the recess RCc in the memory hole MH.

[0120] As shown in Fig. 8(e), a metal layer SR is formed to cover the cap layer CPs on the channel layer CNs. The metal layer SR is a silicide layer or the like in which one or more metals selected from nickel, palladium, and aluminum are silicided by the surface layer of the cap layer CPs, which is an amorphous silicon layer or the like. Such a metal layer SR is formed by sputtering one or more metals selected from nickel, palladium, and aluminum.

[0121] Furthermore, the channel layer CNs and the cap layer CPs are crystallized by a metal-assisted annealing process or the like to form a substantially single-crystallized channel layer CN.

[0122] That is, with the metal layer SR formed on the cap layer CPs, annealing is performed at a temperature between 500°C and 600°C, which is a temperature at which an amorphous silicon layer does not usually crystallize, for example, 550°C. As a result, the metal layer SR on the cap layer CPs acts as a catalyst, and the cap layer CPs and the channel layer CNs are almost entirely single-crystallized. At this time, some of the metal layer SR that acted as a catalyst for single crystallization become finely divided metal fragments SRf, and segregate to the lower end side of the channel layer CN.

[0123] As shown in FIG. 8(f), a gettering layer GT such as an amorphous silicon layer is formed on the upper surface of the channel layer CN, and annealing is performed at a temperature of 500° C. or higher. As a result, the metal fragments SRf that have been segregated in the channel layer CN move into the gettering layer GT. Therefore, most of the metal fragments SRf in the channel layer CN can be removed.

[0124] Here, a more detailed state of the above-mentioned process for converting the amorphous channel layer CNs into the crystalline channel layer CN is shown in Fig. 9. Fig. 9 is an enlarged cross-sectional view of a memory hole MH in which a memory layer ME is formed, similar to Fig. 7 described above.

[0125] 9(a), the metal layer SR on the cap layer CPs serves as a catalyst to cause crystallization to proceed from the upper surface of the cap layer CPs toward the lower end of the channel layer CNs. When the cap layer CPs and the channel layer CNs are crystallized and a region of the channel layer CN that has become substantially single crystal appears, at least a part of the metal layer SR on the upper surface of the cap layer CPs becomes finely chopped metal fragments SRf and migrates downward in the cap layer CPs and the channel layer CNs.

[0126] On the other hand, the crystal nuclei CNn in the non-doped layer CNsa generated at the interface with the memory layer ME may form into microcrystals even when annealed at a temperature at which the amorphous silicon layer does not crystallize without metal assistance, and may inhibit the crystallization of the above-mentioned channel layer CNs by metal assistance.

[0127] However, the channel layer CNs includes a doped layer CNsb formed in contact with the non-doped layer CNsa. As described above, the additives in the doped layer CNsb have the property of inhibiting the crystallization of the channel layer CNs. This causes the doped layer CNsb to have local crystal defects, and the crystal nuclei CNn in the non-doped layer CNsa are easily trapped in the doped layer CNsb. This prevents the crystal nuclei CNn from disappearing without becoming microcrystals, which inhibits the crystallization of the channel layer CNs from being hindered.

[0128] In this way, the additive in the doped layer CNsb has the function of gettering the crystal nuclei CNn in the non-doped layer CNsa. The additive in the doped layer CNsb also slows down the crystallization rate of the channel layer CNs by metal assistance.

[0129] As shown in Fig. 9(b), as the metal fragments SRf move, the crystallization also progresses in the depth direction of the channel layer CNs. As a result, the cap layer CPs and the channel layer CNs are substantially entirely crystallized, and the channel layer CN is formed as a second semiconductor layer including the regions CNa, CNb, and CNc. After that, the metal fragments SRf that have been contained in the channel layer CN by migration are removed by the process shown in Fig. 8(f) above.

[0130] The region CNa of the channel layer CN is a portion where the non-doped layer CNsa is crystallized, the region CNb is a portion where the doped layer CNsb is crystallized, and the region CNc is a portion where the non-doped layer CNsc is crystallized.

[0131] Here, the additive in the doped layer CNsb has the function of gettering the metal element in the metal fragment SRf. Therefore, the metal element impregnated in the channel layer CNs by migration may segregate in the non-doped layer CNsa, including the surface of the doped layer CNsb in contact with the non-doped layer CNsa. As a result, even after the metal fragment SRf is removed, the metal element may remain in the region CNa of the channel layer CN.

[0132] As described above, the doped layer CNsb reduces the crystallization acceleration of the channel layer CNs, so that even after the annealing process using the metal assist, the amorphous channel layer CNs may remain on the lower side of a part of the channel layer CN. Therefore, after removing the metal fragment SRf, further annealing is performed at a temperature of, for example, more than 800° C. As a result, the remaining amorphous part undergoes solid phase growth and is incorporated into the part of the channel layer CN that is already single crystal.

[0133] FIG. 9(c) shows how the channel layer CN becomes substantially entirely single crystal through solid phase growth in a further annealing treatment.

[0134] As described above, the process of placing a metal layer SR as a catalyst on the upper ends of the cap layers CPs and channel layers CNs to be crystallized and progressing metal-assisted crystallization from top to bottom is also called MILC (Metal Induced Lateral Crystallization) annealing process.

[0135] The above-mentioned MILC annealing process provides the channel layer CN with the above-mentioned crystal structure. That is, among the multiple memory holes MH, the ratio of the memory holes MH in which the crystal grain boundaries appear in the cross section along the XY plane of the channel layer CN is, for example, less than 1% at the upper end side of the memory hole MH, i.e., at a height position, for example, 0.5 μm lower than the upper end of the memory hole MH, and, for example, less than 2% at the center of the memory hole MH in the extension direction, and, for example, 4% or less at the lower end side of the memory hole MH, i.e., at a height position, for example, 0.5 μm higher than the lower end of the memory hole MH. The lower limit of the ratio at the lower end side of the memory hole MH is, for example, 0.1% or more, preferably 0.05% or more, and more preferably 0.01% or more.

[0136] Next, the state in which the channel layer CN is further processed to form pillars PL is shown in Figures 10 and 11. Figures 10 and 11 are cross-sectional views along the Y direction of a region that will later become the memory region MR, similar to Figure 8 described above.

[0137] FIG. 10(a) shows a cross section of the entire pillar PL in which a crystalline channel layer CN is formed.

[0138] 10(b), the channel layer CN and the memory layer ME are etched back and removed from the upper surface of the insulating layer 51. This exposes the upper surface of the insulating layer 51. At this time, the channel layer CN and the core layer CRs are also etched back in the memory hole MH. As a result, the upper ends of the channel layer CN and the core layer CRs are positioned at a predetermined depth in the memory hole MH, and a recess RCm is formed above the channel layer CN and the core layer CRs.

[0139] The recess RCm in the memory hole MH can be obtained by continuing overetching for a predetermined time even after the channel layer CN on the upper surface of the insulating layer 51 is removed. At this time, the overetching time and the like are controlled to maintain the upper ends of the channel layer CN and the core layer CRs at a height position at least higher than the uppermost insulating layer NL of the stack LMs. By leaving the channel layer CN at the height position of the uppermost insulating layer NL that will later become the select gate line SGD, the pillar PL in this portion can function as the select gate STD.

[0140] As shown in FIG. 11(a), a sidewall layer SW is formed to cover the upper surface of the insulating layer 51. The sidewall layer SW is also formed in the recess RCm at the upper end of the memory hole MH so as to cover the side wall of the memory hole MH, and protects the memory layer ME in a slimming process of the channel layer CN, which will be described later. The sidewall layer SW is, for example, an amorphous silicon layer. Note that the thickness of the sidewall layer SW is adjusted by controlling the processing time, etc., so that the recess RCm is not completely blocked.

[0141] As shown in Fig. 11(b), the core layer CRs in the memory hole MH is removed and the channel layer CN is thinned by wet etching, isotropic dry etching, etc. At this time, the memory layer ME on the side wall of the memory hole MH is protected by the sidewall layer SW.

[0142] By the slimming process for thinning the channel layer CN, among the regions CNa, CNb, and CNc of the channel layer CN, the region CNc is almost completely removed. Also, a part of the region CNb may be removed. At this time, in the layer thickness direction of the channel layer CN, for example, the region CNb may be removed until a portion in the region CNb where the additive has a peak concentration is exposed as a new surface of the channel layer CN. As a result, the above-mentioned channel layer CN having the regions CNa and CNb but not the region CNc is formed.

[0143] In this way, the crystallization of the channel layer CNs is easily promoted by initially forming a thick channel layer CNs and then performing an annealing process, etc. Also, by slimming the crystallized channel layer CN, the depletion layer can be made thinner compared to the length of the channel layer CN in the stacking direction, which corresponds to the gate length, and the short channel effect can be suppressed.

[0144] As shown in Fig. 11(c), the core layer CRs is removed, and the gap in the memory hole MH resulting from the slimming of the channel layer CN is filled with a silicon oxide layer or the like to form the core layer CR. At this time, the height position of the upper end of the core layer CR is adjusted so that it is equal to or higher than the height position of the upper end of the channel layer CN. By maintaining the shape of the channel layer CN at the height position of the top insulating layer NL, which will later become the select gate line SGD, as a circular ring, the pillar PL in this portion can function as the select gate STD.

[0145] 11(d), a cap layer CPa is formed to cover the sidewall layer SW on the upper surface of the insulating layer 51. The cap layer CPa is an amorphous silicon layer or the like that will be crystallized later to become the upper cap layer CP. The cap layer CPa is also filled into the recess RCm at the upper end of the memory hole MH.

[0146] 11(e), the cap layer CPa and the sidewall layer SW are etched back and removed from the upper surface of the insulating layer 51. At this time, the amount of overetching is suppressed and controlled so that the cap layer CPa and the sidewall layer SW in the memory hole MH are not also removed.

[0147] 11(f), the remaining cap layer CPa and sidewall layer SW are crystallized by, for example, annealing to form an upper cap layer CP. The degree of crystallization in the upper cap layer CP does not need to be as high as that of the above-mentioned channel layer CN, and the upper cap layer CP may be, for example, a polysilicon layer. An amorphous silicon layer may remain in part of the upper cap layer CP, and a part of the upper cap layer CP may be monocrystalline.

[0148] In this manner, the pillars PL are formed. However, at this point in time, the lower cap layer EP has not yet been formed on the lower end of the channel layer CN of the pillars PL.

[0149] Next, a state in which a laminated body LM is formed by replacing a plurality of insulating layers NL with word lines WL, etc. is shown in Fig. 12. Fig. 12 is a cross-sectional view along the Y direction of a region that will later become a memory region MR, similar to Figs. 10 and 11 described above.

[0150] 12(a), an insulating layer 52 is formed on an insulating layer 51. A slit ST is formed penetrating the insulating layers 52 and 51, the laminate LMs, and the insulating layer 55 to reach the support substrate SS. The slit ST also extends in the laminate LMs in the X direction.

[0151] 12(b), a remover such as hot phosphoric acid is poured from above the slit ST to remove the insulating layer NL in the laminate LMs exposed on the side surface of the slit ST, thereby forming a laminate LMg having gaps between a plurality of insulating layers OL.

[0152] As shown in Fig. 12(c), a raw material gas that is a raw material for conductors, etc. is injected from above the slit ST, and the gap is filled with a conductive layer to form the word line WL and the select gate lines SGD, SGS. This forms a stacked body LM in which multiple word lines WL and select gate lines SGD, SGS are stacked. However, at this point, the select gate line SGD is not yet separated into multiple sections.

[0153] The process of removing the insulating layer NL and forming the word lines WL and the like is also called a replacement process.

[0154] As shown in FIG. 12(d), the slit ST is filled with an insulating layer 54 to form a plate-shaped portion PT.

[0155] 12(e), in order to form the separation layer SHE, a groove GR is formed which penetrates the insulating layers 52 and 51 and the select gate line SGD and extends in the X direction. In other words, the groove GR is made to penetrate the conductive layer which is to function as the select gate line SGD among the conductive layers in the laminate LM, and the conductive layer is separated into a pattern of a plurality of select gate lines SGD.

[0156] As shown in FIG. 12(f), an insulating layer 56 is filled into the trench GR to form a separation layer SHE.

[0157] Thereafter, an insulating layer 53 is formed on the insulating layer 52, and a plug CH that penetrates the insulating layers 53 and 52 and is connected to the upper cap layer CP of the pillar PL, and a bit line BL that is connected to the plug CH are formed.

[0158] Next, a state in which the lower cap layer EP is formed on the lower end of the pillar PL is shown in Fig. 13. Fig. 13 is a cross-sectional view along the Y direction of a region that will later become the memory region MR, similar to Fig. 12 and the like described above.

[0159] 13(a) and 13(b), pillars PL are formed in the laminate LM, and a surface of a support substrate SS on which plugs CH and bit lines BL have been formed in insulating layers 52 and 53 covering the laminate LM is opposed to a surface of a semiconductor substrate SB separate from the support substrate SS on which a peripheral circuit CBA is formed. The peripheral circuit CBA is covered with an insulating layer 40, and contacts, vias, wiring, and the like electrically connected to the peripheral circuit CBA are formed in the insulating layer 40.

[0160] Thereafter, the insulating layer 50 including the insulating layers 51-53 on the support substrate SS side is bonded to the insulating layer 40 on the semiconductor substrate SB side. These insulating layers 50, 40 can be bonded by, for example, activating them in advance by plasma treatment or the like. When bonding the insulating layers 50, 40, the support substrate SS and the semiconductor substrate SB are aligned so that an electrode pad (not shown) formed on the surface of the insulating layer 50 and electrically connected to the pillars PL and the like overlaps with an electrode pad formed on the surface of the insulating layer 40 and electrically connected to the peripheral circuit CBA.

[0161] After the insulating layers 50 and 40 are bonded together, an annealing process is performed to bond the electrode pads together, for example, by Cu-Cu bonding, thereby bonding the support substrate SS and the semiconductor substrate SB together.

[0162] In addition, from here on, illustration of the configuration on the side of the semiconductor substrate SB bonded to the insulating layer 50 will be omitted.

[0163] 13(c), the entire support substrate SS above the laminate LM and part of the insulating layer 55 are removed by CMP (Chemical Mechanical Polishing) or the like. As a result, the upper ends of the pillar PL and the plate-like portion PT are exposed on the ground upper surface of the insulating layer 55. In addition, the entire memory layer ME that covered the upper surface of the pillar PL and a part of the upper end of the channel layer CN are removed, and the channel layer CN is exposed from the upper end of the pillar PL.

[0164] 13(d), recess etching is performed on the exposed channel layer CN while taking a selection ratio with respect to the memory layer ME on the sidewall of the pillar PL, and the upper end of the channel layer CN is recessed in the depth direction of the pillar PL, thereby forming a recess RCe at the upper end of the pillar PL.

[0165] During recess etching, by taking the selectivity with the memory layer ME, the insulating layer 55 containing the same material as the memory layer ME is prevented from being etched away. Also, by taking the selectivity with the memory layer ME, the core layer CR containing the same material as the memory layer ME may protrude into the recess RCe.

[0166] 13(e), the recesses RCE at the upper ends of the pillars PL are filled with a cap layer EPa such as an amorphous silicon layer or a polysilicon layer, and the cap layer EPa is doped with a dopant such as phosphorus by ion implantation or the like.

[0167] 13(f), the dopants in the cap layer EPa are activated by activation annealing, for example, by irradiating with laser light, thereby forming a lower cap layer EP in which the dopants in the cap layer EPa are activated.

[0168] In this manner, a pillar PL having the lower cap layer EP at its lower end is formed.

[0169] In addition, the above process of forming the lower cap layer EP at the lower end of the pillar PL removes a part of the lower end of the pillar PL including the memory layer ME and the channel layer CN. Depending on the amount of removal at this time, the distance from the lower end of the pillar PL to the part where the ratio of the pillar PL where the grain boundary appears is, for example, 4% or less in the cross section along the XY plane of the channel layer CN may vary slightly. In other words, in the above explanation, the lower end side of the pillar PL is a position 0.5 μm above the lower end of the pillar PL, but this distance is merely an example.

[0170] Thereafter, a source line SL is formed of a polysilicon layer or the like covering the lower end of the pillar PL on which the lower cap layer EP is formed and the insulating layer 55 on which the lower end of the plate-like portion PT is exposed. In addition, an electrode layer EL is formed above the source line SL via an insulating layer 60 on which a plug PG is formed.

[0171] In this manner, the semiconductor memory device 1 of the embodiment is manufactured.

[0172] (Overview) In semiconductor storage devices such as three-dimensional non-volatile memories, for example, a pillar having a channel layer and a memory layer is given the function of a memory cell. By appropriately controlling the crystal structure of the channel layer, which is a semiconductor layer, for example, by single-crystallizing the channel layer, the electrical resistance of the channel layer can be reduced, and the noise originating from the channel layer CN can be reduced to obtain a memory cell with good electrical characteristics.

[0173] Here, for example, when an amorphous channel layer is formed and crystallized by a simple annealing process, the channel layer has a crystal structure that is approximately 100% polycrystalline. In this case, the number of grain boundaries that appear in the channel layer throughout the entire pillar is, for example, one or more per 50 nm in the extension direction of the pillar.

[0174] Therefore, in order to crystallize the channel layer, a metal-assisted annealing process such as MILC annealing is used. However, crystal nuclei may be formed in the amorphous channel layer before crystallization, hindering the single crystallization of the channel layer by metal assistance. This is shown in Figure 14.

[0175] FIG. 14 is an enlarged cross-sectional view of a memory hole showing how an amorphous channel layer CNsx according to a comparative example is converted into a crystalline channel layer CNx.

[0176] 14(a), in the manufacturing process of the semiconductor memory device of the comparative example, a channel layer CNsx is formed which is an amorphous semiconductor layer such as an amorphous silicon layer and is a non-doped layer as a whole. Crystal nuclei CNn are formed in the vicinity of the interface between the channel layer CNsx and the memory layer ME due to the disorder of the structure of the channel layer CNsx.

[0177] 14(b), in a state where a metal layer, which is a silicide layer of nickel, palladium, aluminum, or the like, is formed on the upper side of the channel layer CNsx, an annealing process is performed at a temperature of 500° C. to 600° C. As a result, metal-assisted crystallization starts from the upper end side of the channel layer CNsx.

[0178] On the other hand, at this time, the crystal nuclei CNn in the channel layer CNsx grow into fine crystals, which inhibits homogeneous crystallization of the channel layer CNsx by metal assist.

[0179] As shown in Fig. 14(c), the crystal nuclei CNn are inhibited by the grown microcrystals to form a polycrystallized channel layer CNx, which results in the formation of many crystal grain boundaries CNg in the channel layer CNx.

[0180] Thus, even when metal-assisted annealing is used, the percentage of pillars in which grain boundaries appear in a cross section along the XY plane of the channel layer is about 1% even at the top end of the pillars.

[0181] According to the manufacturing method of the semiconductor memory device 1 of the embodiment, an additive, which is one or more of carbon, nitrogen, oxygen, and fluorine, is added to the channel layer CNs near the memory layer ME in the layer thickness direction. This traps the crystal nuclei CNn formed near the interface between the channel layer CNs and the memory layer ME, and prevents the channel layer CNs from being inhibited from being single-crystallized by the MILC annealing process.

[0182] According to the manufacturing method of the semiconductor memory device 1 of the embodiment, the additive is added so that the peak concentration is in a region where the distance from the memory layer ME is less than 50% of the total thickness of the channel layer CNs, more preferably 5% to 25%. This can enhance the trapping effect of the crystal nuclei CNn by the doped layer CNsb to which the additive is added.

[0183] FIG. 15 is a graph showing an appropriate position of a doped layer CNsb introduced into a channel layer CNs according to an embodiment.

[0184] The horizontal axis of the graph shown in FIG. 15 represents the concentration of carbon used as an additive, and the vertical axis of the graph represents the ratio of pillars in which the channel layer was completely amorphous in the XY cross section on the lower end side of multiple pillars.

[0185] The graph in FIG. 15 also shows data obtained when carbon is added to positions where the distance from the memory layer is 95%, 60%, and 20% of the thickness of the entire channel layer before slimming.

[0186] In the example shown in Fig. 15, the ratio of pillars in which the channel layer became amorphous was the highest when carbon was added at a position where the distance from the memory layer was 60% of the total thickness of the channel layer. It was also found that the ratio of pillars in which the channel layer became amorphous was the lowest when carbon was added at a position where the distance from the memory layer was 20% of the total thickness of the channel layer.

[0187] Thus, it can be seen that the trapping effect of the crystal nuclei is enhanced when the carbon is added near the memory layer. On the other hand, for example, if the carbon-added region is formed so as to contact the memory layer, the electrons flowing through the channel layer during electrical operation of the memory cell may be scattered or captured by the carbon-added region. This may result in a deterioration of the electrical characteristics of the memory cell.

[0188] In the embodiment, since the region CNb of the channel layer CN is not in contact with the memory layer ME, such scattering and trapping of electrons can be suppressed and the electrical characteristics of the memory cell can be maintained.

[0189] According to the semiconductor memory device 1 of the embodiment, at least on the upper end side of the pillar PL, the channel layer CN has a crystal structure in which the number of crystal grain boundaries per 1 μm in the extension direction of the pillar PL is less than 0.5.

[0190] According to the semiconductor memory device 1 of the embodiment, in a cross section along the XY plane at the center of the extension direction of the multiple pillars PL, the ratio of the multiple pillars PL in which crystal grain boundaries appear in the channel layer CN is less than 2%.

[0191] Furthermore, the ratio of the pillars PL having grain boundaries in the channel layer CN among the multiple pillars PL is less than 1% in the cross section on the upper end side of the pillar PL and is 4% or less in the cross section on the lower end side of the pillar PL. The lower limit of the ratio on the lower end side of the pillar is 0.1% or more, preferably 0.05% or more, and more preferably 0.01% or more.

[0192] In this way, when an additive is added to a part of the channel layer CNs and the annealing process is performed by metal assist, the degree of single crystallization of the channel layer CN can be increased compared to the case where the annealing process is performed without adding an additive to an amorphous channel layer. This makes it possible to lower the resistance of the channel layer CN and reduce noise derived from the channel layer CN, thereby improving the electrical characteristics of the memory cell MC.

[0193] (Modification) Next, a method for manufacturing a semiconductor memory device according to a modification of the embodiment will be described with reference to Figures 16 and 17. In the method for manufacturing a semiconductor memory device according to the modification, the method of annealing using a metal assist is different from that of the above-described embodiment.

[0194] In the following drawings, the same components as those in the above-described embodiment are denoted by the same reference numerals, and the description thereof may be omitted.

[0195] 16 and 17 are enlarged cross-sectional views sequentially illustrating a part of the procedure of a manufacturing method for a semiconductor memory device according to a modification of the embodiment.

[0196] 16(a) and 16(b), in the manufacturing method of the semiconductor memory device of the modified example, an amorphous channel layer CNs is formed in the same manner as in the above-mentioned embodiment. That is, the channel layer CNs includes a non-doped layer CNsa that may include crystal nuclei CNn, a doped layer CNsb that includes at least one additive of carbon, nitrogen, oxygen, and fluorine, and a non-doped layer CNsc, in this order from the memory layer ME side.

[0197] 16(c), a metal layer SRa is formed to cover the inner wall surface of the channel layer CNs. The metal layer SRa is a silicide layer or the like in which one or more metals of nickel, palladium, and aluminum are silicided by the surface layer portion of the channel layer CNs, which is an amorphous silicon layer or the like.

[0198] Thereafter, the void remaining in the memory hole MH is filled with the core layer CRs.

[0199] 17(a), annealing is started at a temperature of 500° C. to 600° C., for example, 550° C. As a result, the metal layer SRa on the inner wall surface of the channel layer CNs becomes shardened metal fragments SRfa, which infiltrate into different height positions in the channel layer CNs.

[0200] On the other hand, the crystal nuclei CNn contained in the non-doped layer CNsa of the channel layer CNs are trapped in the doped layer CNsb of the channel layer CNs and disappear.

[0201] As shown in Figure 17(b), by continuing the annealing process, crystallization of the channel layer CNs begins at different height positions in the channel layer CNs using the metal fragments SRfa as a catalyst, and crystalline channel layers CNp are formed and grow in various places.

[0202] As shown in FIG. 17(c), a channel layer CNp that is almost entirely single-crystallized is formed by annealing using a metal assist and then additional annealing at 800° C. or higher. The channel layer CNp includes regions CNna, CNnb, and CNnc in which the non-doped layer CNsa, the doped layer CNsb, and the non-doped layer CNsc of the channel layer CNs are crystallized, respectively. As in the above-described embodiment, the region CNna of the channel layer CNp may contain the metal element used for the metal assist. Also, the peak concentration of the additive is located, for example, in the region CNnb.

[0203] The process of providing a metal layer SRa as a catalyst on the side of the channel layer CNs and promoting crystallization by metal assistance at different height positions in the channel layer CNs is also called MIC (Metal Induced Crystallization) annealing. In the MIC annealing, crystallization progresses at various points in the channel layer CNs, so the number of crystal grain boundaries CNg that appear in the finally obtained channel layer CNp may increase slightly more than in the case of crystallization by the above-mentioned MILC annealing.

[0204] Even in this case, the difference in quality between the channel layer CNp formed by the MIC annealing process and the channel layer CN of the above embodiment formed by the MILC annealing process is very small. For example, in the case of the channel layer CNp by the MIC annealing process, the number of grain boundaries per 1 μm in the extension direction of the pillars in the channel layer CNp at least on the upper end side of the multiple pillars is, for example, less than 2.

[0205] The other crystal structure characteristics of the channel layer CNp are substantially the same as those of the channel layer CN of the above embodiment. That is, the ratio of the pillars in which the grain boundaries appear in the cross section of the channel layer CNp along the XY plane among the plurality of pillars is, for example, less than 1% at the upper end side of the pillar, i.e., at a height position, for example, 0.5 μm lower than the upper end of the pillar, and is, for example, less than 2% at the center of the extension direction of the pillar, and is, for example, 4% or less at the lower end side of the pillar, i.e., at a height position, for example, 0.5 μm higher than the lower end of the pillar. The lower limit value of the ratio at the lower end side of the pillar is, for example, 0.1% or more, preferably 0.05% or more, and more preferably 0.01% or more.

[0206] The semiconductor memory device of the modified example and the manufacturing method thereof provide the same effects as those of the semiconductor memory device 1 of the above-described embodiment and the manufacturing method thereof.

[0207] (Other variations) In the above-mentioned embodiment and modified example, the lower end of the pillar PL is ground away to provide a lower cap layer EP connected to the source line SL. However, the method of connecting the pillar and the source line is not limited to this. For example, the lower end of the pillar may be extended into the source line, the memory layer may be removed from the side of the pillar in the source line, and the side of the channel layer may be connected to the source line. In this case, since the lower end of the pillar is not ground away, the pillar after the crystalline channel layer is formed is maintained substantially as it is.

[0208] In the above-described embodiment and modified examples, the semiconductor memory device 1 is provided with MONOS (Metal Oxide Nitride Oxide Silicon) type memory cells MC equipped with a charge storage layer CT, etc. However, even if the semiconductor memory device is provided with FG (Floating Gate) type memory cells equipped with a floating gate, etc., the channel layers CN, CNp of the above-described embodiment and modified examples can be applied.

[0209] The FG type memory cell has a floating gate between control gates as a plurality of conductive layers, which is electrically floating from the control gates. The floating gate is sandwiched between a tunnel insulating layer provided on the channel layer side and an inter-control gate insulating layer provided on the opposite side of the tunnel insulating layer, and data can be retained by storing electric charge in the floating gate. Thus, the FG type memory cell also has a structure in which the sidewall of the channel layer is covered by a multi-layer insulating layer of the tunnel insulating layer and the inter-control gate insulating layer, which includes the floating gate as a charge storage layer.

[0210] In the above-described embodiment and modified example, the semiconductor memory device 1 has a one-tier stack LM. However, the semiconductor memory device may have a two-tier or more stack LM by stacking a plurality of stacks LMs. In this case, since memory holes MH and the like can be formed for each tier, the final number of stacks of the stack LM can be increased. FIG. 18 below shows an example of the configuration of a semiconductor memory device having two-tier stacks LMa and LMb.

[0211] FIG. 18 is a cross-sectional view showing an example of a configuration of a semiconductor memory device according to another modified example of the embodiment.

[0212] 18, the semiconductor memory device of the other modification includes a stack LMa arranged on the source line SL via an insulating layer 55, and a stack LMb arranged on the stack LMa via an insulating layer OLj. In this case, the above-mentioned drain side select gate line SGD is included in the upper stack LMb and is arranged in a layer above the top word line WL of the stack LMb. Also, the above-mentioned source side select gate line SGS is included in the lower stack LMa and is arranged in a layer below the bottom word line WL of the stack LMa.

[0213] The pillars PL extending in the stacking direction of the stacks LMa and LMb include pillars PLa that penetrate the stack LMa and insulating layer 55 to reach the source line SL, and pillars PLb that penetrate the insulating layer 52 and stack LMb to reach the insulating layer OLj. The upper ends of the corresponding pillars PLa and the lower ends of the pillars PLb are connected via junctions PLj disposed in the insulating layer OLj, for example. The sectional area and diameter of the junctions PLj along the XY plane are larger than those of the other parts of the pillar PL.

[0214] The semiconductor memory device of the other modified example shown in FIG. 18 is manufactured, for example, as follows.

[0215] That is, a stack that will become the stack LMa by replacement is formed on the insulating layer 55, an insulating layer OLj is formed to cover the stack, a memory hole that penetrates the insulating layer OLj, the stack, and the insulating layer 55 to reach the source line SL is formed, and the diameter of the memory hole in the insulating layer OLj is enlarged. This forms the portions that will later become the pillars PLa and the junctions PLj.

[0216] Moreover, a stack that will become the stack LMb by replacement is formed on the insulating layer OLj, an insulating layer 52 is formed to cover the stack, and a memory hole is formed that penetrates the insulating layer 52 and the stack and connects to the enlarged portion in the insulating layer OLj of the memory hole formed in the stack below. This forms the portion that will later become the pillar PLb.

[0217] As described above, by expanding the diameter of the upper end of the memory hole on the lower layer, the memory holes on the upper and lower layers can be more reliably connected even if the memory hole on the upper layer is formed slightly out of position.

[0218] A pillar PL is formed by carrying out the processes shown in Fig. 7 to Fig. 11 of the above-mentioned embodiment on the memory hole penetrating the entire stack of upper and lower layers via the expanded diameter portion in the insulating layer OLj. However, the crystallization of the amorphous channel layer CNs may be carried out by the MIC annealing process shown in Fig. 16 and Fig. 17 of the above-mentioned modified example, instead of the MILC annealing process shown in Fig. 7 and Fig. 9.

[0219] Thus, in the manufacturing method of a semiconductor memory device having a stack of multiple tiers, a memory hole is formed for each tier, and the formation of the memory layer ME, channel layer CN, core layer CR, etc. within the memory hole is performed collectively after the formation of the memory hole that penetrates the entire multiple tiers.

[0220] Thereafter, similarly to the above-described embodiment, the processes in and after FIG. 12 are carried out to manufacture the semiconductor memory device of the other modified example.

[0221] As described above, the joints PLj of the pillars PL are formed to ensure a margin for misalignment of the memory holes in the upper and lower layers. However, when the alignment accuracy of the memory holes in the upper and lower layers is sufficiently high, the upper end of the memory hole in the lower layer does not need to be enlarged. In that case, even a pillar PL with a multi-tier structure does not need to have the joints PLj.

[0222] Additionally, in the above-described embodiment and modified example, the contact region ER is arranged at the end of the laminate LM in the X direction. However, the contact region ER may be arranged in the center of the laminate LM in the X direction. In this case, the memory regions MR can be arranged on both sides of the contact region ER in the X direction. Also, instead of arranging a plurality of contacts CC connected to a plurality of word lines WL together in the contact region ER, the contacts CC can be distributed in the memory region MR, etc.

[0223] In the above-described embodiment and modified examples, the peripheral circuit CBA is arranged above the stack LM, but the peripheral circuit may be arranged below the stack or at the same layer as the stack.

[0224] When the peripheral circuit is disposed below the stack, the source line and the stack can be formed, for example, on an insulating layer of a semiconductor substrate having the peripheral circuit covered with the insulating layer. When the peripheral circuit is disposed at the same layer as the stack, the stack can be formed at a different position from the peripheral circuit on the semiconductor substrate on which the peripheral circuit is formed.

[0225] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0226] 1...semiconductor memory device, CN, CNp, CNs...channel layer, CNa, CNb, CNc, CNpa, CNpb, CNpc...region, CP...upper cap layer, CR...core layer, EP...lower cap layer, LM, LMg, LMs...stacked body, MC...memory cell, ME...memory layer, MR...memory region, NL, OL...insulating layer, PL...pillar, SGD, SGS...select gate line, STD, STS...select gate, WL...word line.

Claims

1. a laminate in which a plurality of conductive layers and a plurality of insulating layers are alternately laminated; a core extending within the stack in a first direction intersecting with the surfaces of the conductive layers, a crystalline semiconductor layer covering a side surface of the core, and a plurality of pillars each including a multilayer insulating layer including a charge storage layer stacked on a side surface of the semiconductor layer; Each of the semiconductor layers is At least on a first end side in the first direction, the crystal structure has less than two crystal grain boundaries per 1 μm in the first direction; containing an additive which is one or more of carbon, nitrogen, oxygen, and fluorine; Semiconductor memory device.

2. The plurality of pillars include a first pillar having the semiconductor layer with an average grain size that decreases from a first end in the first direction to a second end opposite the first end; 2. The semiconductor memory device according to claim 1.

3. The semiconductor layer of the first pillar has The second end portion has a crystal structure in which the number of crystal grain boundaries per 1 μm in the first direction is 10 or more.

3. The semiconductor memory device according to claim 2.

4. A ratio of the first pillars included in the plurality of pillars is 4% or less.

4. The semiconductor memory device according to claim 3.

5. a laminate in which a plurality of conductive layers and a plurality of insulating layers are alternately laminated; a core extending within the stack in a first direction intersecting with the surfaces of the conductive layers, a crystalline semiconductor layer covering a side surface of the core, and a plurality of pillars each including a multilayer insulating layer including a charge storage layer stacked on a side surface of the semiconductor layer; the semiconductor layer includes an additive that is one or more of carbon, nitrogen, oxygen, and fluorine; In a cross section in a direction intersecting the first direction, the cross section is at a center of the plurality of pillars in the first direction, and a ratio of the pillars in which a grain boundary appears in the semiconductor layer among the plurality of pillars is less than 2%. Semiconductor memory device.

6. forming a laminate in which a plurality of first insulating layers and a plurality of second insulating layers are alternately laminated; forming a plurality of holes extending within the stack in a first direction intersecting the surfaces of each of the plurality of first insulating layers; forming a multi-layer insulating layer including a charge storage layer and covering sidewalls of the plurality of holes; forming an amorphous first semiconductor layer covering each of the side walls of the holes via the multilayer insulating layer; crystallizing the first semiconductor layer by a metal-assisted annealing process to form a crystalline second semiconductor layer; filling the holes surrounded by the second semiconductor layer with a core material; When the first semiconductor layer is formed, adding an additive, which is one or more of carbon, nitrogen, oxygen, and fluorine, to the first semiconductor layer toward the multilayer insulating layer in a layer thickness direction; A method for manufacturing a semiconductor memory device.

7. When the first semiconductor layer is formed, adding the additive so that the additive has a peak concentration in a region where the distance from the multilayer insulating layer is less than 50% of the layer thickness of the first semiconductor layer; 7. The method for manufacturing a semiconductor memory device according to claim 6.

8. When the first semiconductor layer is formed, the additive is added so that the additive has a peak concentration in a region where the distance from the multilayer insulating layer is 5% or more and less than 25% of the thickness of the first semiconductor layer; The method for manufacturing a semiconductor memory device according to claim 7 .

9. When the first semiconductor layer is formed, Peak concentration is 5 x 10 19 Above 1 x 10 21 atoms / cm 3 Add the additives so that The method for manufacturing a semiconductor memory device according to claim 7 .

10. Before filling the core material into the plurality of holes, Etching the second semiconductor layer in a thickness direction to thin it; 7. The method for manufacturing a semiconductor memory device according to claim 6.

Citation Information

Patent Citations

  • Semiconductor film and its manufacturing method, and semiconductor device and its manufacturing method

    JP2004165185A

  • Crystallization method for silicon, junction structure, method of manufacturing semiconductor device and semiconductor device

    JP2009194259A

  • Method for manufacturing semiconductor device

    JP2015103742A

  • Semiconductor storage device and manufacturing method of the same

    JP2020141008A

Cited By

  • Semiconductor memory device and method for manufacturing a semiconductor memory device

    JP2026144307A

  • Semiconductor memory

    JP2026163742A