Grip for golf club

The golf club grip with a porous inner layer and specific properties addresses the issue of mechanical strength and wear by enhancing resistance to settling and fatigue across temperature variations.

JP2024157786APending Publication Date: 2024-11-08SUMITOMO RUBBER INDUSTRIES LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023072363
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Golf club grips with porous structures face a decrease in mechanical strength and increased compression set, particularly under high temperatures, leading to wear and tear.

Method used

A golf club grip with a cylindrical inner layer having a porous structure and specific density and storage modulus ranges, combined with a cylindrical outer layer, to enhance resistance to settling at room and high temperatures.

Benefits of technology

The grip exhibits improved resistance to settling and fatigue, maintaining mechanical integrity under varying temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157786000001_ABST
    Figure 2024157786000001_ABST
Patent Text Reader

Abstract

To provide a grip for a golf club which shows improved settling resistance of an inner layer at a normal temperature and an increased temperature by improving a material forming a porous structure in a grip having the porous structure in the inner layer.SOLUTION: A grip for a golf club includes a cylindrical part having a cylindrical inner layer and a cylindrical outer layer for covering the inner layer, and the inner layer has a porous structure. In the inner layer, density (D) is 0.30 g / cm3 to 0.90 g / cm3, a storage elastic modulus (E'25) at 25°C, while measuring with a dynamic viscoelasticity measuring apparatus under measuring conditions of an oscillation frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode is 9.0 MPa or less, and a storage elastic modulus (E'60) at 60°C is 7.0 MPa or less. A ratio (E'25 / D) of the storage elastic modulus (E'25) (MPa) to the density (D) (g / cm3) is 10.5 or less, and a ratio (E'60 / D) of the storage elastic modulus (E'60) (MPa) to the density (D) (g / cm3) is 9.5 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grip for a golf club. [Background technology]

[0002] Rubber grips are often used as grips attached to golf clubs. As such rubber grips, golf club grips using acrylonitrile-butadiene rubber as the base rubber have been proposed. In addition, golf club grips with a multi-layered cylindrical portion and a porous inner layer have also been proposed (Patent Document 1 (Tables 3 to 5)). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-162635 A Summary of the Invention [Problem to be solved by the invention]

[0004] Golf club grips may have a porous structure in order to reduce the weight of the grip and improve its cushioning. However, the porous structure tends to reduce the mechanical strength of the grip, and in particular tends to increase the compression set caused by compression deformation. For example, if a golf bag containing golf clubs is left lying down for a long time, the grip may become worn. In particular, if the bag is left in a high-temperature environment such as the inside of a car in summer for a long time, the grip is likely to become worn.

[0005] The present invention has been made in consideration of the above circumstances, and has an object to provide a golf club grip in which the inner layer has a porous structure, and in which the material that forms the porous structure is improved to improve the resistance of the inner layer to wear at room temperature and at high temperatures. [Means for solving the problem]

[0006] The golf club grip of the present invention, which has been able to solve the above problems, has a cylindrical portion composed of a cylindrical inner layer and a cylindrical outer layer covering the inner layer, the inner layer having a porous structure, and a density (D) of the inner layer of 0.30 g / cm 3 ~0.90g / cm 3 The inner layer had a storage modulus (E') at 25°C measured using a dynamic viscoelasticity device under the following measurement conditions: vibration frequency 10Hz, strain amplitude 0.05%, tensile mode. 25 ) is 9.0MPa or less, and the storage modulus at 60℃ (E' 60 ) is 7.0 MPa or less, and the storage modulus at 25°C (E' 25 ) (MPa) and density (D) (g / cm 3 ) and the ratio (E' 25 / D) is 10.5 or less, and the storage modulus at 60°C (E' 60 ) (MPa) and density (D) (g / cm 3 ) and the ratio (E' 60 / D) is 9.5 or less. Effect of the Invention

[0007] According to the present invention, a golf club grip having an inner layer with excellent resistance to settling at room temperature and at high temperatures can be obtained. [Brief description of the drawings]

[0008] [Figure 1] 1 is a perspective view showing an example of a golf club grip of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing an example of a golf club grip of the present invention. [Diagram 3] 1 is a perspective view showing an example of a golf club equipped with a golf club grip of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Golf club grips] The golf club grip of the present invention has a cylindrical portion composed of a cylindrical inner layer and a cylindrical outer layer covering the inner layer, and the inner layer has a porous structure. The density (D) of the inner layer is 0.30 g / cm. 3 ~0.90g / cm 3 The inner layer has a storage modulus (E') at 25°C measured using a dynamic viscoelasticity device under the following measurement conditions: vibration frequency 10Hz, strain amplitude 0.05%, and tensile mode. 25 ) is 9.0MPa or less, and the storage modulus at 60℃ (E' 60 ) is 7.0 MPa or less, and the storage modulus at 25°C (E' 25 ) (MPa) and density (D) (g / cm 3 ) and the ratio (E' 25 / D) is 10.5 or less, and the storage modulus at 60°C (E' 60 ) (MPa) and density (D) (g / cm 3 ) and the ratio (E' 60 / D) is 9.5 or less.

[0010] In the present invention, the storage modulus (E' 25 ) is the temperature at which the grip is used, and the storage modulus (E' 60 ) is the storage modulus in a high temperature atmosphere. These storage moduli (E' 25 ) and storage modulus (E' 60 If the ratio (E') is within a certain range, the ratio of the force stored in the grip to the external force applied during deformation will be small. 25 / D) and ratio (E' 60 By controlling the thickness (D) within a specified range, distortion is less likely to remain and resistance to settling is improved regardless of the grip density.

[0011] The golf club grip has a cylindrical portion made of a cylindrical inner layer and a cylindrical outer layer covering the inner layer. The cylindrical portion may have a two-layer structure made of one inner layer and one outer layer, or may have a three-layer structure made of two inner layers and one outer layer.

[0012] [Inner layer] The inner layer has a porous structure. The porous structure is a structure in which a large number of pores (voids) are formed in the base rubber. By forming a large number of pores, the apparent density of the inner layer is reduced, and weight can be reduced. In addition, the porous structure makes it easier to deform in response to external forces, improving the cushioning properties of the grip.

[0013] (Physical Properties) The density (D) of the inner layer is 0.30 g / cm 3 More preferably, it is 0.35 g / cm or more. 3 More preferably, 0.40 g / cm 3 More than 0.90g / cm 3 Preferably less than 0.85 g / cm 3 More preferably, 0.80 g / cm 3 The density (D) is 0.30 g / cm or less. 3 If it is more than 0.90g / cm, the mechanical strength of the grip will be improved. 3 The grip can be made lighter if:

[0014] The hardness (Shore A hardness) of the inner layer is preferably 35 or more, more preferably 40 or more, and even more preferably 45 or more, and is preferably 65 or less, more preferably 60 or less. If the hardness (Shore A hardness) of the inner layer is 35 or more, the inner layer will not be too soft, and a feeling of firm fixation will be obtained when gripped, and if it is 65 or less, the inner layer will not be too hard, and a better grip feeling will be obtained when gripped.

[0015] The inner layer had a storage modulus (E') at 25°C measured using a dynamic viscoelasticity device under the following measurement conditions: vibration frequency 10 Hz, strain amplitude 0.05%, and tensile mode. 25 The storage elastic modulus (E') is preferably 3.0 MPa or more, more preferably 3.5 MPa or more, and even more preferably 4.0 MPa or more, and is preferably 9.0 MPa or less, more preferably 8.5 MPa or less, and even more preferably 8.0 MPa or less. 25If the compressive strength is 3.0 MPa or more, the grip will have good hardness and will have better operability, and if the compressive strength is 9.0 MPa or less, the grip will have better resistance to settling during actual use.

[0016] The inner layer was measured using a dynamic viscoelasticity device under the conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode, and had a loss tangent (tanδ) at 25°C. 25 ) is preferably 0.120 or more, more preferably 0.124 or more, and even more preferably 0.126 or more, and is preferably 0.200 or less, more preferably 0.195 or less, and even more preferably 0.190 or less. 25 If the ratio is 0.120 or more, the grip will have better resistance to settling during actual use, and if the ratio is 0.200 or less, the grip will have a better feeling.

[0017] The inner layer had a storage modulus (E') at 60°C measured using a dynamic viscoelasticity device under the conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode. 60 The storage elastic modulus (E') is preferably 2.0 MPa or more, more preferably 2.5 MPa or more, and even more preferably 3.0 MPa or more, and is preferably 7.0 MPa or less, more preferably 6.8 MPa or less, and even more preferably 6.6 MPa or less. 60 ) is 2.0 MPa or more, the grip hardness will be better and the operability will be better, and if it is 7.0 MPa or less, the resistance to settling during storage in a high-temperature atmosphere will be improved.

[0018] The inner layer was measured using a dynamic viscoelasticity device under the conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode, and had a loss tangent (tanδ) at 60°C. 60 ) is preferably 0.080 or more, more preferably 0.085 or more, and even more preferably 0.090 or more, and is preferably 0.180 or less, more preferably 0.175 or less, and even more preferably 0.170 or less. 60If the value is 0.080 or more, the resistance to settling during storage in a high-temperature atmosphere is improved, and if the value is 0.180 or less, the grip feeling is improved.

[0019] The storage modulus at 25° C. (E' 25 ) (MPa) and density (D) (g / cm 3 ) and the ratio (E' 25 The ratio (E' / D) is preferably 10.5 or less, more preferably 10.0 or less, and further preferably 9.5 or less. 25 If the ratio of the hardness to the stiffness of the grip is 10.5 or less, the grip will have better resistance to fatigue during actual use. The ratio (E' 25 The ratio (E' / D) is preferably 0.3 or more, more preferably 1.0 or more, and further preferably 2.0 or more. 25 If the ratio of 0.3 to 1, the grip has better hardness and is easier to handle.

[0020] The storage modulus at 60° C. (E' 60 ) (MPa) and density (D) (g / cm 3 ) and the ratio (E' 60 The ratio (E' / D) is preferably 9.5 or less, more preferably 9.0 or less, and further preferably 8.5 or less. 60 If the ratio of 0.1 to 9.5, the resistance to settling during storage in a high-temperature atmosphere is improved. The ratio (E' 60 The ratio (E' / D) is preferably 0.3 or more, more preferably 1.0 or more, and further preferably 2.0 or more. 60 If the ratio of 0.3 to 1, the grip has better hardness and is easier to handle.

[0021] The inner layer has an elongation at break (Eb) determined by a tensile test of preferably 300% or more, more preferably 350% or more, even more preferably 400% or more, and preferably 600% or less, more preferably 580% or less, even more preferably 550% or less. If the elongation at break (Eb) is 300% or more, tearing of the grip when inserting a shaft into the grip is more suppressed, and if it is 600% or less, the crosslinking strength of the crosslinked rubber constituting the grip is better.

[0022] The elongation at break (Eb) (%) and density (D) (g / cm 3 ) is preferably equal to or less than 660, more preferably equal to or less than 630, and further preferably equal to or less than 600. When the ratio (Eb / D) is equal to or less than 660, the crosslinking strength of the crosslinked rubber constituting the grip becomes better. The ratio (Eb / D) is preferably equal to or greater than 330, more preferably equal to or greater than 340, and even more preferably equal to or greater than 350. When the ratio (Eb / D) is equal to or greater than 330, the crosslinking strength of the crosslinked rubber constituting the grip becomes better.

[0023] The inner layer has a tensile stress at 25% elongation (Se 25 The tensile stress (Se) is preferably 0.5 MPa or more, more preferably 0.6 MPa or more, and even more preferably 0.7 MPa or more, and is preferably 1.4 MPa or less, more preferably 1.3 MPa or less, and even more preferably 1.2 MPa or less. 25 If the pressure is 0.5 MPa or more, the crosslinking strength of the crosslinked rubber constituting the grip will be better, and if it is 1.4 MPa or less, the feeling of the grip will be better.

[0024] The tensile stress at 25% elongation (Se 25 ) (MPa) and density (D) (g / cm 3 ) and the ratio (Se 25The ratio (Se / D) is preferably 0.7 or more, more preferably 0.75 or more, and even more preferably 0.80 or more, and is preferably 1.5 or less, more preferably 1.45 or less, and even more preferably 1.40 or less. 25 If the ratio (R / D) is 0.7 or more, the crosslinking strength of the crosslinked rubber constituting the grip will be better, and if the ratio (R / D) is 1.5 or less, the feeling of the grip will be better.

[0025] The rubber composition for the inner layer that forms the inner layer preferably has a maximum torque (MH) in a vulcanization curve measured at a vulcanization temperature of 165° C. of 0.91 N·m or more, more preferably 0.93 N·m or more, even more preferably 0.95 N·m or more, and preferably 1.5 N·m or less, more preferably 1.4 N·m or less, and even more preferably 1.3 N·m or less. If the maximum torque is 0.91 N·m or more, the crosslinking strength of the crosslinked rubber that constitutes the grip will be better, and if it is 1.5 N·m or less, poor appearance of the two-layer structure grip after molding can be further reduced.

[0026] The maximum torque (MH) (N·m) and the loss tangent (tanδ 25 ) and its product (tan δ 25 ×MH) is preferably 0.1 or more, more preferably 0.11 or more, and further preferably 0.12 or more. 25 If the ratio of the hardness (H) to the hardness (H) is 0.1 or more, the grip will have better resistance to fatigue during actual use. The product (tan δ 25 ×MH) is preferably 0.28 or less, more preferably 0.26 or less, and further preferably 0.24 or less. 25 ×MH) is 0.28 or less, the grip feeling is better.

[0027] The maximum torque (MH) (N·m) and the loss tangent (tanδ 60 ) and its product (tan δ 60 ×MH) is preferably 0.1 or more, more preferably 0.11 or more, and further preferably 0.12 or more. 60When the ratio (M × MH) is 0.1 or more, the resistance to settling during storage in a high-temperature atmosphere is further improved. The product (tan δ 60 ×MH) is preferably 0.24 or less, more preferably 0.22 or less, and further preferably 0.21 or less. 60 ×MH) is 0.24 or less, the grip feeling is better.

[0028] The maximum torque (MH) and loss tangent (tanδ 25 , tan δ 60 ) improves sag resistance, but it is thought to be as follows. In the vulcanization curve, maximum torque (MH) is an index of crosslink density. Also, the larger the loss tangent (tan δ), the easier it is for the external force applied during deformation to be released when the deformation is released. In other words, the larger the loss tangent (tan δ), the less likely strain will remain during compressive deformation. Therefore, by controlling the product of maximum torque (MH), which is an index of crosslink density, and loss tangent (tan δ), which is an index of strain, it is possible to improve the compression set rate at the temperature during use or in a high-temperature atmosphere, and it is thought that sag resistance will improve.

[0029] The physical properties and vulcanization characteristics of the inner layer can be controlled by adjusting the raw materials and compounding amounts of the rubber composition constituting the inner layer. In particular, the density of the inner layer can be controlled mainly by the foaming agent content, crosslinking agent content, vulcanization accelerator content, and vulcanization conditions. The viscoelastic properties of the inner layer can be controlled mainly by the type and content of the base rubber, the filler content, and the coupling agent content.

[0030] The inner layer has a porous structure. Methods for producing the porous layer include a balloon foaming method, a chemical foaming method, a supercritical carbon dioxide injection molding method, a salt extraction method, and a solvent removal method. In the balloon foaming method, microballoons are contained in a rubber composition, and the microballoons are expanded by heating to form a foam. The expanded microballoons may be blended into the rubber composition and molded. In the chemical foaming method, a foaming agent (azodicarbonamide, azobisisobutyronitrile, N,N-dinitrosopentamethylenetetramine, p-toluenesulfonylhydrazine, p-oxybis(benzenesulfohydrazide), etc.) or a foaming assistant is contained in the rubber composition, and gas (carbon dioxide gas, nitrogen gas, etc.) is generated by a chemical reaction to form the foam. In the supercritical carbon dioxide injection molding, carbon dioxide in a supercritical state under high pressure is impregnated into the rubber composition, and the rubber composition is injected under normal pressure, and the carbon dioxide is vaporized to form the foam. In the salt extraction method, a soluble salt (boric acid, calcium chloride, etc.) is added to the rubber composition, and the salt is dissolved and extracted after molding to form pores. In the solvent removal method, a solvent is added to the rubber composition, and the solvent is removed after molding to form pores.

[0031] The inner layer is preferably a foamed layer formed from a rubber composition for the inner layer containing a foaming agent. In particular, it is preferably a foamed layer produced by a balloon foaming method. That is, the inner layer is preferably a foamed layer formed from a rubber composition for the inner layer containing microballoons. By using microballoons, it becomes easier to maintain the mechanical strength of the inner layer and to control the physical properties of the inner layer.

[0032] (Rubber composition for inner layer) The rubber composition for the inner layer constituting the inner layer may be, for example, a rubber composition containing (A) a base rubber, (B) a crosslinking agent, and (C) a reinforcing material.

[0033] (A) Base rubber The content of the base rubber (A) in the rubber composition for the inner layer is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 60% by mass or more. Examples of the base rubber (A) include natural rubber (NR), ethylene-propylene-diene rubber (EPDM), butyl rubber (IIR), acrylonitrile-butadiene rubber (NBR), hydrogenated acrylonitrile-butadiene rubber (HNBR), carboxy-modified acrylonitrile-butadiene rubber (XNBR), butadiene rubber (BR), styrene-butadiene rubber (SBR), polyurethane rubber (PU), isoprene rubber (IR), chloroprene rubber (CR), and ethylene-propylene rubber (EPM). These base rubbers may be used alone or in combination of two or more.

[0034] The base rubber (A) preferably contains an acrylonitrile-butadiene rubber. The acrylonitrile-butadiene rubber is preferably at least one selected from the group consisting of acrylonitrile-butadiene rubber (NBR), carboxy-modified acrylonitrile-butadiene rubber (XNBR), hydrogenated acrylonitrile-butadiene rubber (HNBR), and carboxy-modified hydrogenated acrylonitrile-butadiene rubber (HXNBR). The XNBR is a copolymer of a monomer having a carboxy group, acrylonitrile, and butadiene. The HNBR is a hydrogenated product of acrylonitrile-butadiene rubber. The HXNBR is a hydrogenated product of a copolymer of a monomer having a carboxy group, acrylonitrile, and butadiene.

[0035] The content of the acrylonitrile-butadiene rubber in the base rubber (A) is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. It is also preferable that the rubber composition for the inner layer contains only the acrylonitrile-butadiene rubber as the base rubber (A).

[0036] The (A) base rubber preferably contains at least one selected from the group consisting of NBR, XNBR, HNBR and HXNBR, and more preferably contains HNBR. By blending HNBR as the (A) base rubber, the weather resistance of the grip is further improved.

[0037] The content of HNBR in the base rubber (A) is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. The rubber composition may contain only HNBR as the base rubber (A). When the content of HNBR in the base rubber (A) is 20% by mass or more, the weather resistance of the grip is further improved.

[0038] The acrylonitrile content of the HNBR is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, and is preferably 40% by mass or less, more preferably 39% by mass or less, and even more preferably 38% by mass or less. If the acrylonitrile content of the NBR is 10% by mass or more, the mechanical strength of the grip is further improved, and if it is 40% by mass or less, the compression set during deformation is smaller.

[0039] The double bond content of the HNBR is preferably 0.09 mmol / g or more, more preferably 0.2 mmol / g or more, and is preferably 2.5 mmol / g or less, more preferably 2.0 mmol / g or less, and even more preferably 1.5 mmol / g or less. If the double bond content is 0.09 mmol / g or more, a crosslinked structure is more easily formed when sulfur is used as a crosslinking agent, and if it is 2.5 mmol / g or less, the weather resistance and mechanical strength of the grip are better. The double bond content can be adjusted by the butadiene content in the copolymer and the amount of hydrogen added to the copolymer.

[0040] The rubber composition for the inner layer preferably contains HNBR and NBR as the base rubber (A). In addition, by blending NBR to increase the amount of double bonds in the base rubber, the crosslink density is improved and the compression set of the inner layer can be further reduced.

[0041] The acrylonitrile content of the NBR is preferably 10% by mass or more, more preferably 12% by mass or more, and even more preferably 14% by mass or more, and is preferably 40% by mass or less, more preferably 38% by mass or less, and even more preferably 36% by mass or less. If the acrylonitrile content of the NBR is 10% by mass or more, the compatibility with the HNBR is improved, and if it is 40% by mass or less, the compression set during deformation is small.

[0042] When the rubber composition for the inner layer contains NBR as the base rubber (A), the content of NBR in the base rubber (A) is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, and is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. If the content of HNBR in the base rubber (A) is 20% by mass or more, the compression set rate is good, and if it is 80% by mass or less, the weather resistance of the grip is further improved.

[0043] When the (A) base rubber contains HNBR and NBR, the mass ratio of HNBR to NBR in the (A) base rubber (HNBR / NBR) is preferably 0.30 or more, more preferably 0.35 or more, and even more preferably 0.40 or more, and is preferably 2.4 or less, more preferably 2.0 or less, and even more preferably 1.5 or less. If the mass ratio (HNBR / NBR) is 0.30 or more, the weather resistance of the grip will be better, and if it is 2.4 or less, the compression set rate will be better.

[0044] (B) Crosslinking agent As the (B) crosslinking agent, a sulfur-based crosslinking agent or an organic peroxide can be used. The crosslinking agent may be used alone or in combination of two or more. As the crosslinking agent, a sulfur-based crosslinking agent is preferable, and elemental sulfur is more preferable. As the sulfur-based crosslinking agent, elemental sulfur and a sulfur donor type compound can be mentioned.

[0045] The elemental sulfur may be powdered sulfur, precipitated sulfur, colloidal sulfur, or insoluble sulfur. The sulfur donor compound may be a morpholine-based sulfur donor compound, such as 4,4'-dithiodimorpholine. Examples of the organic peroxide include dicumyl peroxide, α,α'-bis(t-butylperoxy-m-diisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane.

[0046] The inner layer rubber composition preferably contains elemental sulfur and a morpholine-based sulfur donor compound as the crosslinking agent (B).

[0047] The amount of the (B) crosslinking agent used, relative to 100 parts by mass of the (A) base rubber, is preferably 0.2 parts by mass or more, more preferably 0.4 parts by mass or more, and even more preferably 0.6 parts by mass or more, and is preferably 4.0 parts by mass or less, more preferably 3.5 parts by mass or less, and even more preferably 3.0 parts by mass or less.

[0048] (C) Reinforcement Examples of the (C) reinforcing material include carbon black and silica, with carbon black being preferred. The content of the (C) reinforcing material is preferably 2.0 parts by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 4.0 parts by mass or more, relative to 100 parts by mass of the (A) base rubber, and is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less. If the content of the (C) reinforcing material is 2.0 parts by mass or more, the reinforcing effect of the grip is further improved, and if it is 50 parts by mass or less, the feeling of the grip is better.

[0049] resin The rubber composition for the inner layer may further contain a resin. By containing a resin, the tackiness of the inner layer is increased, and the occurrence of air entrapment can be suppressed when the inner layer and the outer layer in the two-layer structure grip are bonded together. The resin preferably has a softening point of 120° C. or less.

[0050] Examples of the resin include rosin ester, ethylene-vinyl acetate copolymer, coumarone resin, and phenol resin.

[0051] The rosin ester is an ester compound obtained by reacting rosin with alcohols. Rosin is a natural resin containing abietic acid, neoabietic acid, palustric acid, pimaric acid, isopimaric acid, and dehydroabietic acid. As the alcohols, dihydric or higher polyhydric alcohols are preferred, and glycerin is more preferred.

[0052] The rosin ester includes hydrogenated rosin ester and disproportionated rosin ester. The hydrogenated rosin ester is an ester compound in which the portion derived from rosin of the rosin ester is hydrogenated. The disproportionated rosin ester is an ester compound in which the portion derived from rosin of the rosin ester is disproportionated.

[0053] The vinyl acetate content of the ethylene-vinyl acetate copolymer is preferably 10% by mass or more, more preferably 12% by mass or more, and even more preferably 15% by mass or more, and is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. If the vinyl acetate content is 10% by mass or more, the grip feeling is better. If the content is 80% by mass or less, the wear resistance of the grip is further improved.

[0054] The coumarone resin is a resin containing coumarones as monomer components. The coumarone resin is preferably a coumaron-indene resin. The coumaron-indene resin is a copolymer containing coumarones and indenes as monomer components, and the total content of coumarones and indenes in the total monomer components is 50 mass% or more. Examples of the coumarones include coumarones, methylcoumarones, etc. Examples of the indenes include indene, methylindene, etc.

[0055] The phenolic resin may be, for example, a condensate of a phenol and formaldehyde. Examples of the phenol include phenol, m-cresol, etc. The phenolic resin may also include resol obtained by addition reaction of a phenol and formaldehyde with an alkali catalyst; novolac obtained by condensation reaction with an acid catalyst, etc. The phenolic resin may also include rosin phenolic resin obtained by adding a phenol to rosin with an acid catalyst and thermally polymerizing the mixture.

[0056] When the resin is blended, the content of the resin is preferably 5 parts by mass or more, more preferably 6 parts by mass or more, and even more preferably 7 parts by mass or more, and is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and even more preferably 16 parts by mass or less, relative to 100 parts by mass of the (A) base rubber. If the content of the resin is 5 parts by mass or more, the tackiness of the inner layer is increased, and the occurrence of air entrapment when the inner layer and the outer layer are bonded together can be further suppressed, and if it is 20 parts by mass or less, the mechanical strength of the grip is improved.

[0057] Filler Coupling Agent The rubber composition for the inner layer may further contain a filler coupling agent. By containing a filler coupling agent, the crosslink density of the inner layer is mainly improved.

[0058] The filler coupling agent improves the dispersibility of the (C) reinforcing material in the (A) base rubber. The type of the filler coupling agent is not particularly limited, and may be appropriately selected depending on the reinforcing material to be blended. For example, when carbon black is used as the (C) reinforcing material, it is preferable that the filler coupling agent contains a carbon coupling agent. Examples of the carbon coupling agent include a compound represented by formula (1) and a compound represented by formula (2).

[0059] [ka] [In formula (1), n ​​represents an integer of 2 to 10.]

[0060] n is preferably an integer of 2 to 6. Examples of the compound represented by the formula (1) include S-(3-aminopropyl)thiosulfuric acid, S-(4-aminobutyl)thiosulfuric acid, S-(5-aminopentyl)thiosulfuric acid, S-(6-aminohexyl)thiosulfuric acid, S-(7-aminoheptyl)thiosulfuric acid, S-(8-aminooctyl)thiosulfuric acid, S-(9-aminononyl)thiosulfuric acid, and S-(9-aminodecyl)thiosulfuric acid.

[0061] [ka] [In formula (2), R 1 R represents an alkylene group having 1 to 12 carbon atoms or an arylene group having 6 to 12 carbon atoms. 2 , R 3 are the same or different and represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, a hydroxy group, or an alkoxy group having 1 to 6 carbon atoms. X represents -NH- or -O-. Z represents a hydrogen atom or a metal atom.]

[0062] R 1 is preferably an arylene group having 6 to 12 carbon atoms, and more preferably a phenylene group. R 2 and R 3is preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and more preferably a hydrogen atom. The Z is preferably a metal atom, more preferably an alkali metal such as sodium or potassium. The above X is preferably -NH-.

[0063] An example of the compound represented by the formula (2) is sodium (2Z)-4-[(4-aminophenyl)amino]-4-oxo-2-butenoate.

[0064] When the filler coupling agent is blended, the content of the filler coupling agent in the inner layer rubber composition is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.0 parts by mass or more, and is preferably 3.0 parts by mass or less, more preferably 2.8 parts by mass or less, and even more preferably 2.6 parts by mass or less, relative to 100 parts by mass of the (C) reinforcing material. If the content of the filler coupling agent is 0.5 parts by mass or more, the crosslinking strength of the crosslinked rubber constituting the grip becomes better, and if it is 3.0 parts by mass or less, the effect on other physical properties can be further reduced.

[0065] The rubber composition for the inner layer may further contain a vulcanization accelerator and a vulcanization activator.

[0066] (Vulcanization accelerator) Examples of the vulcanization accelerator include thiuram-based vulcanization accelerators, guanidine-based vulcanization accelerators, dithiocarbamate-based vulcanization accelerators, thiourea-based vulcanization accelerators, thiazole-based vulcanization accelerators, sulfenamide-based vulcanization accelerators, etc. These vulcanization accelerators may be used alone or in combination of two or more kinds.

[0067] The inner layer rubber composition preferably contains two or more vulcanization accelerators. If the inner layer rubber composition contains two or more vulcanization accelerators, the vulcanization rate can be adjusted more precisely and the occurrence of bloom can be reduced. The inner layer rubber composition may contain a thiuram-based vulcanization accelerator, a thiourea-based vulcanization accelerator, a thiazole-based vulcanization accelerator, and a guanidine-based vulcanization accelerator.

[0068] Examples of the thiuram vulcanization accelerator include tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), tetramethylthiuram monosulfide (TMTM), dipentamethylenethiuram tetrasulfide, and tetrakis(2-ethylhexyl)thiuram disulfide. Examples of the thiourea-based vulcanization accelerator include trimethylthiourea and N,N'-diethylthiourea. Examples of the thiazole vulcanization accelerator include mercaptobenzothiazole (MBT) and benzothiazole disulfide. The guanidine vulcanization accelerator includes diphenyl guanidine (DPG) and the like. Examples of the dithiocarbamate vulcanization accelerator include zinc dimethyldithiocarbamate (ZnPDC) and zinc dibutyldithiocarbamate. Examples of the sulfenamide salt vulcanization accelerator include N-cyclohexyl-2-benzothiazolylsulfenamide (CBS) and Nt-butyl-2-benzothiazolylsulfenamide (BBS).

[0069] When the vulcanization accelerator is blended, the total content of the vulcanization accelerator is preferably 4.0 parts by mass or more, more preferably 4.2 parts by mass or more, and even more preferably 4.4 parts by mass or more, and is preferably 6.0 parts by mass or less, more preferably 5.8 parts by mass or less, and even more preferably 5.6 parts by mass or less, per 100 parts by mass of the (A) base rubber. If the total content of the vulcanization accelerator is 4.0 parts by mass or more, when a rubber having few double bonds such as HNBR is used as the base rubber, the vulcanization speed can be increased, and if it is 6.0 parts by mass or less, the occurrence of bloom can be further suppressed.

[0070] (Vulcanization activator) Examples of the vulcanization activator include metal oxides, metal peroxides, and fatty acids. Examples of the metal oxides include zinc oxide, magnesium oxide, and lead oxide. Examples of the metal peroxides include zinc peroxide, chromium peroxide, magnesium peroxide, and calcium peroxide. Examples of the fatty acids include stearic acid, oleic acid, and palmitic acid. These vulcanization activators may be used alone or in combination of two or more.

[0071] When the vulcanization activators are blended, the total content of the vulcanization activators is, per 100 parts by mass of the (A) base rubber, preferably 0.5 parts by mass or more, more preferably 0.6 parts by mass or more, and even more preferably 0.7 parts by mass or more, and is preferably 10.0 parts by mass or less, more preferably 9.5 parts by mass or less, and even more preferably 9.0 parts by mass or less.

[0072] The inner layer rubber composition may further contain antioxidants, softeners, scorch inhibitors, colorants, etc., as required.

[0073] Examples of the antiaging agents include imidazoles, amines, phenols, and thioureas. Examples of the imidazoles include nickel dibutyldithiocarbamate (NDIBC), 2-mercaptobenzimidazole, and zinc salt of 2-mercaptobenzimidazole. Examples of the amines include phenyl-α-naphthylamine. Examples of the phenols include 2,2'-methylenebis(4-methyl-6-t-butylphenol) (MBMBP), and 2,6-di-tert-butyl-4-methylphenol. Examples of the thioureas include tributylthiourea and 1,3-bis(dimethylaminopropyl)-2-thiourea. These antiaging agents may be used alone or in combination of two or more.

[0074] When the antioxidant is blended, the content of the antioxidant, per 100 parts by mass of the (A) base rubber, is preferably at least 0.2 parts by mass, more preferably at least 0.3 parts by mass, and even more preferably at least 0.4 parts by mass, and is preferably at most 5.0 parts by mass, more preferably at most 4.8 parts by mass, and even more preferably at most 4.6 parts by mass.

[0075] The softener may be a mineral oil or a plasticizer. The mineral oil may be paraffin oil, naphthene oil, aromatic oil, etc. The plasticizer may be dioctyl phthalate, dibutyl phthalate, dioctyl sebacate, dioctyl adipate, etc.

[0076] Examples of the scorch inhibitor include organic acids, nitroso compounds, etc. Examples of the organic acids include phthalic anhydride, pyromellitic anhydride, trimellitic anhydride, benzoic acid, salicylic acid, malic acid, etc. Examples of the nitroso compounds include N-nitroso diphenylamine, N-(cyclohexylthio)phthalimide, sulfonamide derivatives, diphenylurea, bis(tridecyl)pentaerythritol diphosphite, 2-mercaptobenzimidazole, etc.

[0077] When the inner layer is made porous by a balloon foaming method, the rubber composition for the inner layer contains microballoons. As the microballoons, either organic microballoons or inorganic microballoons can be used. As organic microballoons, hollow particles made of thermoplastic resins, resin capsules in which low-boiling point hydrocarbons are encapsulated in a shell of a thermoplastic resin, and the like can be mentioned. Specific examples of the resin capsules include Expancel manufactured by Akzo Nobel and Matsumoto Microsphere (registered trademark) manufactured by Matsumoto Yushi Seiyaku Co., Ltd. As inorganic microballoons, hollow glass particles (silica balloons, alumina balloons, etc.), hollow ceramic particles, and the like can be mentioned.

[0078] The volume average particle size of the resin capsules (before expansion) is preferably 5 μm or more, more preferably 6 μm or more, and even more preferably 9 μm or more, and is preferably 90 μm or less, more preferably 70 μm or less, and even more preferably 60 μm or less.

[0079] When the inner layer is produced by the balloon foaming method, the content of microballoons in the rubber composition for the inner layer is preferably 6 parts by mass or more, more preferably 7 parts by mass or more, even more preferably 8 parts by mass or more, and preferably 16 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 14 parts by mass or less, relative to 100 parts by mass of the base rubber. If the content of the microballoons is 6 parts by mass or more, foaming during the formation of the porous layer becomes more uniform, and if it is 16 parts by mass or less, poor appearance of the grip after molding can be further suppressed.

[0080] The rubber composition for the inner layer can be prepared by a conventional method. For example, it can be prepared by kneading each raw material using a kneading machine such as a Banbury mixer, a kneader, or an open roll. When the rubber composition for the inner layer contains microballoons, it is preferable to knead the components other than the microballoons in advance, and then knead the kneaded mixture with the microballoons. The material temperature when kneading the kneaded mixture with the microballoons is preferably set to a temperature lower than the expansion start temperature of the microballoons.

[0081] The Mooney viscosity (ML 1+4 (100°C)) is preferably 30 or more, more preferably 32 or more, and even more preferably 34 or more, and is preferably 70 or less, more preferably 60 or less, and even more preferably 50 or less. 1+4 If the (100° C.)) is 30 or more, the handling property is improved and the sheet can be extruded by a calendar roll, and if it is 70 or less, the formation of a porous structure by the foaming agent becomes easier.

[0082] The density of the rubber composition for the inner layer (density before vulcanization) is 1.00 g / cm 3More preferably, it is 1.02 g / cm 3 More than 1.10g / cm 3 Preferably, it is less than 1.08 g / cm 3 The following is the result.

[0083] [Outer layer] In the present invention, the material forming the inner layer is improved to improve the settling resistance of the inner layer, and the structure of the outer layer and the material forming the outer layer are not particularly limited.

[0084] The outer layer may be a solid layer or a porous layer. If the outer layer is a porous layer, the weight of the golf club grip can be reduced. If the outer layer is a porous layer, the apparent density of the outer layer is reduced, and the weight can be reduced.

[0085] Examples of materials for forming the outer layer include a rubber composition for an outer layer and a resin composition. The outer layer is preferably formed from a rubber composition for an outer layer.

[0086] The outer layer rubber composition preferably contains a base rubber and a crosslinking agent. The content of the base rubber in the outer layer rubber composition is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 60% by mass or more.

[0087] Examples of the base rubber include natural rubber (NR), ethylene-propylene-diene rubber (EPDM), butyl rubber (IIR), acrylonitrile-butadiene rubber (NBR), hydrogenated acrylonitrile-butadiene rubber (HNBR), carboxy-modified acrylonitrile-butadiene rubber (XNBR), carboxy-modified hydrogenated acrylonitrile-butadiene rubber (HXNBR), butadiene rubber (BR), styrene-butadiene rubber (SBR), polyurethane rubber (PU), isoprene rubber (IR), chloroprene rubber (CR), and ethylene-propylene rubber (EPM).

[0088] The outer layer rubber composition preferably contains an acrylonitrile-butadiene rubber as a base rubber. By containing an acrylonitrile-butadiene rubber, the mechanical strength of the outer layer is improved. In addition, when the inner layer rubber composition contains an acrylonitrile-butadiene rubber as the base rubber (A), the adhesion between the inner layer and the outer layer is improved.

[0089] The content of the acrylonitrile-butadiene rubber in the base rubber is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. It is also preferable that the outer layer rubber composition contains only the acrylonitrile-butadiene rubber as the base rubber.

[0090] The base rubber is preferably at least one selected from the group consisting of XNBR, HNBR and HXNBR, and particularly preferably HXNBR. That is, the outer layer preferably contains at least one selected from the group consisting of carboxy-modified acrylonitrile-butadiene rubber (XNBR), hydrogenated acrylonitrile-butadiene rubber (HNBR) and carboxy-modified hydrogenated acrylonitrile-butadiene rubber (HXNBR), and more preferably contains HXNBR. When the outer layer contains these rubbers as the base rubber, the wear resistance and weather resistance of the grip are improved.

[0091] In the XNBR, HNBR, and HXNBR used in the outer layer, the acrylonitrile content is preferably 15% by mass or more, more preferably 18% by mass or more, and even more preferably 21% by mass or more, and is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less. If the acrylonitrile content is 15% by mass or more, the abrasion resistance is good, and if it is 50% by mass or less, the grip feel in cold regions and in winter is good.

[0092] In the HNBR and HXNBR, the double bond content is preferably 0.09 mmol / g or more, more preferably 0.2 mmol / g or more, and preferably 2.5 mmol / g or less, more preferably 2.0 mmol / g or less, and even more preferably 1.5 mmol / g or less. If the double bond content is 0.09 mmol / g or more, vulcanization during molding is facilitated and the tensile strength of the grip is improved, and if it is 2.5 mmol / g or less, the durability (weather resistance) and tensile strength of the grip are improved. The double bond content can be adjusted by the butadiene content in the copolymer and the amount of hydrogen added to the copolymer.

[0093] In the XNBR and HXNBR, examples of the monomer having a carboxy group include acrylic acid, methacrylic acid, fumaric acid, and maleic acid. In the XNBR and HXNBR, the content of the monomer containing a carboxy group is preferably 1.0 mass% or more, more preferably 2.0 mass% or more, and even more preferably 3.5 mass% or more, and is preferably 30 mass% or less, more preferably 25 mass% or less, and even more preferably 20 mass% or less. If the content of the monomer containing a carboxy group is 1.0 mass% or more, the wear resistance is better, and if it is 30 mass% or less, the tactile feel of the grip in cold regions and winter is better.

[0094] In the XNBR and HXNBR, the carboxyl group content is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, and even more preferably 3.5% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. If the carboxyl group content is 1.0% by mass or more, the abrasion resistance is improved, and if it is 30% by mass or less, the grip feel in cold regions and in winter is improved.

[0095] The crosslinking agent for the rubber composition for the outer layer may be the same as that used for the rubber composition for the inner layer, and elemental sulfur is preferred. The rubber composition for the outer layer preferably further contains a vulcanization accelerator and a vulcanization activator. The vulcanization accelerator and the vulcanization activator may be the same as those used for the rubber composition for the inner layer. The vulcanization accelerator is preferably a thiuram vulcanization accelerator or a thiourea vulcanization accelerator. The vulcanization activator is preferably zinc oxide or stearic acid.

[0096] The outer layer rubber composition may further contain, as necessary, a reinforcing material, an antioxidant, a softener, a colorant, a scorch inhibitor, a foaming agent (microballoons, etc.), etc. Examples of the reinforcing material, the antioxidant, and the colorant include the same materials as those used in the inner layer rubber composition. As the reinforcing material, carbon black and silica are preferred.

[0097] The rubber composition for the outer layer can be prepared by a conventional method. For example, it can be prepared by kneading the raw materials using a kneading machine such as a Banbury mixer, a kneader, or an open roll. The temperature during kneading (material temperature) is preferably 70°C to 160°C. When the rubber composition for the outer layer contains microballoons, it is preferable to knead the materials at a temperature lower than the expansion start temperature of the microballoons.

[0098] The resin composition contains a base resin, such as a polyurethane resin, a polystyrene resin, a polyethylene resin, a polypropylene resin, an ethylene-vinyl acetate copolymer resin, or a polyethylene terephthalate resin.

[0099] (Golf club grip structure) The golf club grip has a cylindrical portion composed of a cylindrical inner layer and a cylindrical outer layer covering the inner layer.

[0100] Examples of the combination of the outer layer and the inner layer include a solid outer layer and a porous inner layer, and a porous outer layer and a porous inner layer.

[0101] The grip for golf clubs is obtained, for example, by molding the rubber composition in a mold. Examples of molding methods include press molding and injection molding. The grip for golf clubs is obtained, for example, by press molding a laminate of an unvulcanized rubber sheet formed from the rubber composition for the outer layer and an unvulcanized rubber sheet formed from the rubber composition for the inner layer in a mold. When press molding is employed, the mold temperature is preferably 140°C to 200°C, the molding time is preferably 5 minutes to 40 minutes, and the molding pressure is preferably 0.1 MPa to 100 MPa.

[0102] The shape of the golf club grip can be, for example, a shape having a cylindrical portion into which a shaft is inserted and a cap portion integrally formed so as to cover the opening at the rear end of the cylindrical portion. The cylindrical portion has a laminated structure of an inner layer and an outer layer.

[0103] The thickness of the cylindrical portion is preferably 0.5 mm or more, more preferably 1.0 mm or more, and even more preferably 1.5 mm or more, and is preferably 17.0 mm or less, more preferably 10.0 mm or less, and even more preferably 8.0 mm or less.

[0104] When the thickness of the cylindrical portion is 0.5 mm to 17.0 mm, the thickness of the inner layer is preferably more than 0 mm, more preferably 0.6 mm or more, even more preferably 0.8 mm or more, and is preferably 16.5 mm or less, more preferably 16.4 mm or less, and even more preferably 16.3 mm or less. If the thickness of the inner layer is 0.2 mm or more, the effect of reducing the weight of the grip is greater, and if it is 16.5 mm or less, the thickness of the surface layer becomes relatively thick, and the mechanical strength of the grip is further improved.

[0105] The percentage of the thickness of the inner layer relative to the thickness of the cylindrical portion ((thickness of inner layer / thickness of cylindrical portion)×100) is preferably greater than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and is preferably 97% or less, more preferably 96% or less, and even more preferably 95% or less. If the percentage is greater than 0%, the effect of reducing the weight of the grip will be greater, and if it is 97% or less, the thickness of the surface layer will be relatively thick, and the mechanical strength of the grip will be improved.

[0106] The thickness of the outer layer and the inner layer may be uniform or may vary. For example, they may be formed so as to gradually become thicker from one end to the other end in the axial direction of the cylindrical grip. The thickness of the outer layer is preferably uniform. The thickness of the cylindrical portion may be formed so as to be constant over the entire circumferential direction, or a convex portion (so-called back line) may be provided in a portion. Grooves may be provided on the surface of the cylindrical portion. The grooves suppress the formation of a water film between the golfer's hand and the grip, further improving the grip performance in wet conditions. Furthermore, reinforcing cords may be disposed within the grip from the viewpoint of the grip's anti-slip performance and abrasion resistance.

[0107] The mass of the golf club grip is preferably 16 g or more, more preferably 18 g or more, and even more preferably 20 g or more, and is preferably 35 g or less, more preferably 32 g or less, and even more preferably 30 g or less.

[0108] [Golf clubs] The present invention also includes a golf club using the golf club grip. The golf club includes a shaft, a head attached to one end of the shaft, and a grip attached to the other end of the shaft, and the grip is the golf club grip. The shaft can be made of stainless steel or carbon fiber reinforced resin. Examples of the head include wood type, utility type, and iron type. The material constituting the head is not particularly limited, and examples thereof include titanium, titanium alloy, carbon fiber reinforced plastic, stainless steel, maraging steel, and soft iron.

[0109] Hereinafter, a golf club grip and a golf club will be described with reference to the drawings. Fig. 1 is a perspective view showing an example of a golf club grip. Grip 1 has a cylindrical portion 2 into which a shaft is inserted, and a cap portion 3 integrally formed so as to cover an opening at the rear end of the cylindrical portion.

[0110] Fig. 2 is a schematic cross-sectional view showing an example of a grip for a golf club. The cylindrical portion 2 is composed of an inner layer 2a and an outer layer 2b. The outer layer 2b is formed to have a uniform thickness from the tip to the rear end. The inner layer 2a is formed to have a gradually increasing thickness from the tip to the rear end. In the grip 1 shown in Fig. 2, the cap portion 3 is formed from the same rubber composition as the outer layer 2b.

[0111] 3 is a perspective view showing an example of a golf club equipped with a golf club grip of the present invention. Golf club 4 includes shaft 5, head 6 attached to one end of shaft 5, and grip 1 attached to the other end of shaft 4. The rear end of shaft 5 is fitted into cylindrical portion 2 of grip 1. EXAMPLES

[0112] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.

[0113] [Evaluation method] (1) Acrylonitrile content The acrylonitrile content was measured according to ISO 24698-1(2008) on the acrylonitrile-butadiene rubber before hydrogenation.

[0114] (2) Double bond content (mmol / g) The double bond content was calculated from the butadiene content (mass%) and the amount of remaining double bonds (%) in the copolymer. The amount of remaining double bonds is the mass ratio of the double bonds in the copolymer before hydrogenation to the double bonds in the copolymer after hydrogenation (amount of double bonds after hydrogenation / amount of double bonds before hydrogenation), and can be measured by infrared spectroscopy. When the acrylonitrile-butadiene rubber is an acrylonitrile-butadiene binary copolymer, the butadiene content in the copolymer can be calculated by subtracting the acrylonitrile content (mass%) from 100. Amount of double bonds = {butadiene content / 54} x amount of remaining double bonds x 10

[0115] (3) Content of monomers containing carboxyl groups 1 g of hydrogenated acrylonitrile-butadiene rubber was weighed out and dissolved in 50 mL of chloroform, to which thymol blue indicator was added dropwise. While stirring this solution, a 0.05 mol / L methanol solution of sodium hydroxide was added dropwise, and the amount of dripping (V mL) until the first color change was recorded. As a blank, 50 mL of chloroform containing no hydrogenated acrylonitrile-butadiene rubber was also dripped with a 0.05 mol / L methanol solution of sodium hydroxide using thymol blue as an indicator, and the amount of dripping (B mL) until the first color change was recorded. The carboxyl group content was calculated using the following formula. Carboxylic group-containing monomer content = {0.05 × (VB) × PM} / (10 × X) (In the formula, V is the amount of sodium hydroxide solution dropped as the test solution (mL), B is the amount of sodium hydroxide solution dropped as the blank (mL), PM is the molecular weight of the carboxyl group-containing monomer, and X is the valence of the carboxyl group-containing monomer.)

[0116] (4) Mooney viscosity The Mooney viscosity of the rubber composition was measured in accordance with JIS K 6300-1 (2013). The measurement was performed with an L-shaped roller, a measurement temperature of 100°C, a preheating time of 1 minute, and a rotor rotation time of 4 minutes.

[0117] (5) Vulcanization test The rubber composition was subjected to a vulcanization test at the vulcanization temperature shown in Table 2 using a vulcanization tester (Curastometer (registered trademark) Type 7, manufactured by JSR Trading Co., Ltd.). According to "9. Die vulcanization test A" of "Method of determining vulcanization characteristics using a vibration vulcanization tester" of JIS K6300-2 (2001), a sine wave vibration of a low amplitude that does not break the rubber test piece was applied from the lower die, and the torque transmitted from the test piece to the upper die was measured from unvulcanized to overvulcanized. The measurement conditions were a vulcanization temperature of 165°C, a torsional vibration frequency of 100 times per minute, an amplitude angle of 1°, and a measurement time of 30 minutes. The maximum torque (MH) was obtained from the obtained vulcanization curve.

[0118] (6) Hardness (Shore A hardness) The rubber composition was used to prepare a sheet having a thickness of 2 mm by hot pressing under the same conditions as those for manufacturing the grip. The sheet was stored at 23°C for 2 weeks, and the hardness was measured using an automatic hardness tester (Digitest II, manufactured by H. Burleith Co.) in a state where three sheets were stacked so as not to be affected by the measurement substrate, etc. The detector used was "Shore A".

[0119] (7) Density The rubber composition was used to prepare a sheet having a thickness of 2 mm and a square of 13 cm by hot pressing under the same conditions as those for manufacturing the grip. A test piece was prepared by punching out a square of 2 cm from the sheet. The density of the obtained test piece was measured using an automatic specific gravity meter (MS Tech Co., Ltd., SP-GR1, Archimedes' principle).

[0120] (8) Tensile test The tensile test was performed in accordance with JIS K 6251 (2017). Specifically, the rubber composition was hot-pressed under the same conditions as those for manufacturing the grip to produce a sheet with a thickness of 1 mm, which was then punched into a dumbbell shape (dumbbell shape No. 3) to produce a test piece. The physical properties were measured using a tensile test measuring device (Shimadzu Corporation, Autograph AGS-D) (measurement temperature 23°C, tensile speed 500 mm / min). The tensile stress at 25% elongation (Se 25 ) and elongation at break (Eb) were determined.

[0121] (9) Viscoelasticity Loss tangent (tan δ) and storage modulus (E') were measured using a dynamic viscoelasticity measuring device (UBM Corporation). The measurements were performed using a Rheogel-E4000 manufactured by Epson. The test samples were prepared by slicing the grips in the thickness direction to a thickness of 2 mm and punching them to a specified size. The measurement conditions were: temperature; -100°C to 100°C, heating rate; 3°C / min, measurement interval; 3°C, frequency; 10Hz, strain amplitude; 10%, jig; tension, sample shape; width 4mm, thickness 2mm, length 40mm. Tan δ and E' at 25°C and 60°C were obtained from the viscoelasticity spectrum obtained by dynamic viscoelasticity measurement.

[0122] (10) Resistance to wear The sag resistance was measured by measuring the compression set in accordance with JIS K 6262 (2013), and the reciprocal of this compression set was taken as the sag resistance. Cylindrical plugs were prepared from the inner layer formulation containing the foaming agent, and cylindrical test specimens with a diameter of 29 mm and a thickness of 12.5 mm were prepared with a 2x expansion ratio. The test piece and spacer (thickness 9.38 mm) were sandwiched between compression plates, and the test piece was compressed until the compression plates were in close contact with the spacer, and the compression plates were fixed in this state. The compression plates with the test piece compressed were left in a thermostatic chamber (25°C, 60°C) for 22 hours. After 22 hours, the test piece was removed from the thermostatic chamber and the test piece was immediately removed from the compression plates. The test piece released from compression was left at 23°C for 30 minutes, and then the thickness was measured. The compression set (CS) was calculated using the following formula. CS=(t0-t2) / (t0-t1)×100 [CS: Compression set (%) t0: thickness of test piece before test (mm) t1: Spacer thickness (mm) t2: thickness of test piece 30 minutes after release from compression (mm)] Next, the reciprocal of the compression set obtained above was calculated and this was taken as the settling resistance. The larger the settling resistance value, the smaller the compression set. In Table 3, the settling resistance of Grip No. 4 was set at 100, and the values ​​were expressed as an index.

[0123] (11) Grip pressure test A 1 kg weight (50 mm wide, 108 mm long) was placed 5 cm from the butt of the grip inserted into the shaft, and the club was left for one month in an atmosphere at 25°C or 60°C, after which the appearance was visually observed and evaluated. 5 points: Very little sagging. 4 points: Little sagging. 3 points: The sagging was quite severe. 2 points: It was very worn out. 1 point: Significant sagging.

[0124] [Grip Creation] The raw materials were kneaded according to the formulations shown in Tables 1 and 2 to prepare the rubber compositions for the outer layer and the rubber compositions for the inner layer. For the rubber composition for the outer layer, all the raw materials were kneaded in a Banbury mixer. For the rubber composition for the inner layer, the raw materials other than the microballoons were kneaded in a Banbury mixer, and then the microballoons were blended using a roll. The material temperatures during kneading of the rubber composition for the inner layer in the Banbury mixer and during blending of the microballoons with the roll were lower than the expansion start temperature of the microballoons. The density of the rubber composition for the inner layer was 1.02 g / cm 3 ~1.08g / cm 3 It was.

[0125] [Table 1]

[0126] [Table 2]

[0127] The materials used in Tables 1 and 2 are as follows: HXNBR: Hydrogenated carboxy-modified acrylonitrile-butadiene rubber (ARANXEO, THERBAN (registered trademark) XT VPKA 8889 (residual double bond amount 3.5%, acrylonitrile content 33.0 mass%, double bond content 0.40 mmol / g, carboxy group-containing monomer content 5.0 mass%) HNBR: Hydrogenated acrylonitrile-butadiene rubber (ARANXEO, THERBAN AT 3443 VP (residual double bond content 4.0%, acrylonitrile content 34% by mass, double bond content 0.59 mmol / g)) NBR-1: Acrylonitrile-butadiene rubber (JSR Corporation, N240S (acrylonitrile content: 26% by mass)) NBR-2: acrylonitrile-butadiene rubber (Nipol DN401LL (acrylonitrile content: 18.0% by mass), manufactured by Zeon Corporation) Sulfur: Tsurumi Chemical Industry Co., Ltd., 5% oil-filled fine sulfur (200 mesh) Valnoc (registered trademark) R: 4,4'-dithiodimorpholine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Carbon black: SEAST (registered trademark) 3, manufactured by Tokai Carbon Co., Ltd. EVA: Ethylene-vinyl acetate copolymer (manufactured by ARANXEO, Levapren (registered trademark) 500 (vinyl acetate content 50 mass%, melting point 100 ± 5 ° C., Mooney viscosity (ML 1+4 (100℃))27) SYLVATAC RE-5S: Made by Arizona Chemical, rosin ester (melting point below 25°C) Carbon coupling agent: Sumilink (registered trademark) 100, manufactured by Sumitomo Chemical Co., Ltd. TBzTD: Sansela (registered trademark) TBzTD (tetrabenzyl thiuram disulfide) manufactured by Sanshin Chemical Industry Co., Ltd. TOT-N: "Noccela (registered trademark) TOT-N" (tetrakis(2-ethylhexyl)thiuram disulfide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. EUR: "Noccela EUR" (N,N'-diethylthiourea) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. MBTS: Ouchi Shinko Chemical Industry Co., Ltd., "Noccela DM-P" (di-2-benzothiazole disulfide) DPG: Noccela D (1,3-diphenylguanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Zinc peroxide: Struktol ZP 1014 (zinc peroxide content 29% by mass) manufactured by Struktol Zinc oxide: Toho Zinc Co., Ltd., Ginrei R Microballoons: Akzo Nobel's "Expancel (registered trademark) 909-80DU" (resin capsules with low boiling point hydrocarbons encapsulated in a thermoplastic resin shell, volume average particle size 18 μm to 24 μm, expansion start temperature 120°C to 130°C)

[0128] Using the rubber composition for the outer layer, an unvulcanized rubber sheet and a cap member in a fan-shaped shape were produced. The rubber sheet for the outer layer was molded to have a constant thickness. Using the rubber composition for the inner layer, an unvulcanized rubber sheet in a rectangular shape was produced. The rubber sheet for the inner layer was formed to be gradually thicker from one end to the other end. The rubber sheet for the inner layer was wound around a mandrel, and the rubber sheet for the outer layer was superimposed and wound on top of it. The mandrel and the cap member around which the rubber sheets were wound were placed in a mold having a groove pattern on the cavity surface. Then, a heat treatment was performed at a mold temperature of 160°C for a heating time of 15 minutes to obtain a grip for a golf club. The thickness of the cylindrical part of the obtained grip for a golf club was 1.5 mm at the thinnest part (end on the head side) and 6.7 mm at the thickest part (end on the grip end side). The surface of the obtained grip was buffed with abrasive paper (#80). The evaluation results of each grip are shown in Table 3.

[0129] [Table 3]

[0130] Grips No. 1 to 3 have an inner layer density (D) of 0.30 g / cm 3 ~0.90g / cm 3 and the storage modulus (E' 25 ) is 9.0MPa or less, storage modulus (E'60 ) is 7.0MPa or less, and the ratio (E' 25 / D) is 10.5 or less, and the ratio (E' 60 / D) was 9.5 or less. Grip Nos. 1 to 3 were inhibited from becoming worn at both 25°C and 60°C.

[0131] The present invention (1) has a cylindrical portion composed of a cylindrical inner layer and a cylindrical outer layer covering the inner layer, the inner layer having a porous structure, and a density (D) of the inner layer being 0.30 g / cm 3 ~0.90g / cm 3 The inner layer has a storage modulus (E') at 25°C measured using a dynamic viscoelasticity device under the following measurement conditions: vibration frequency 10Hz, strain amplitude 0.05%, and tensile mode. 25 ) is 9.0MPa or less, and the storage modulus at 60℃ (E' 60 ) is 7.0 MPa or less, and the storage modulus at 25°C (E' 25 ) (MPa) and density (D) (g / cm 3 ) and the ratio (E' 25 / D) is 10.5 or less, and the storage modulus at 60°C (E' 60 ) (MPa) and density (D) (g / cm 3 ) and the ratio (E' 60 / D) is 9.5 or less.

[0132] In the present invention (2), the maximum torque in the vulcanization curve measured at a vulcanization temperature of 165°C for the rubber composition for the inner layer forming the inner layer is defined as MH (N m), and the loss tangent at 25°C measured for the inner layer using a dynamic viscoelasticity device under the measurement conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode is defined as tanδ 25 , loss tangent at 60℃ is tanδ 60 When the maximum torque MH (N m) and the loss tangent (tanδ 25 ) and its product (tan δ 25 ×MH) is 0.1 or more, and the maximum torque MH (N m) and the loss tangent (tanδ 60 ) and its product (tan δ 60×MH) is 0.1 or more.

[0133] The present invention (3) is a golf club grip according to the present invention (1) or (2), wherein the inner layer rubber composition forming the inner layer has a maximum torque (MH) of 0.91 N m or more in a vulcanization curve measured at a vulcanization temperature of 165°C.

[0134] In the present invention (4), the inner layer has an elongation at break (Eb) (%) and a density (D) (g / cm 3 ) (Eb / D) is 660 or less.

[0135] In the present invention (5), the inner layer has a tensile stress at 25% elongation (Se 25 ) (MPa) and density (D) (g / cm 3 ) and the ratio (Se 25 The golf club grip according to any one of the aspects (1) to (4) of the present invention has a coefficient of curvature of 0.7 to 1.5.

[0136] The present invention (6) is characterized in that the ratio (E' 25 The golf club grip according to any one of the aspects (1) to (5) of the present invention has a coefficient of curvature of 0.3 to 10.5.

[0137] The present invention (7) is characterized in that the ratio (E' 60 / D) is 0.3 to 9.5.

[0138] The present invention (8) is a golf club grip according to any one of the present inventions (1) to (7), wherein the rubber composition for the inner layer forming the inner layer contains, as base rubber, acrylonitrile-butadiene rubber (NBR) and hydrogenated acrylonitrile-butadiene rubber (HNBR).

[0139] The present invention (9) is the golf club grip according to the present invention (8), wherein the rubber composition for the inner layer that forms the inner layer contains carbon black and a carbon coupling agent.

[0140] The present invention (10) is a golf club grip according to the present invention (8) or (9), wherein the rubber composition for the inner layer forming the inner layer contains, as a vulcanizing agent, elemental sulfur and a morpholine-based sulfur donor compound, and also contains two or more types of vulcanization accelerators. [Explanation of symbols]

[0141] 1: grip, 2: cylindrical portion, 2a: inner layer, 2b: outer layer, 3: cap portion, 4: golf club, 5: shaft, 6: head

Claims

1. A cylindrical portion including a cylindrical inner layer and a cylindrical outer layer covering the inner layer, The inner layer has a porous structure, The density (D) of the inner layer is 0.30 g / cm 3 ~0.90g / cm 3 and The inner layer had a storage modulus (E') at 25° C. measured using a dynamic viscoelasticity device under the measurement conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode. 25 ) is 9.0 MPa or less, and the storage modulus at 60° C. (E' 60 ) is 7.0 MPa or less, The storage modulus at 25° C. (E′ 25 ) (MPa) and density (D) (g / cm 3 ) to (E' 25 / D) is 10.5 or less, The storage modulus at 60° C. (E′ 60 ) (MPa) and density (D) (g / cm 3 ) to (E' 60 / D) is 9.5 or less.

2. Regarding the rubber composition for the inner layer forming the inner layer, the maximum torque in a vulcanization curve measured at a vulcanization temperature of 165° C. is defined as MH (N m); The inner layer was measured using a dynamic viscoelasticity device under the conditions of an excitation frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode. The loss tangent at 25° C. was calculated as tanδ. 25 , the loss tangent at 60°C is tan δ 60 When The maximum torque MH (N m) and the loss tangent (tan δ) at 25°C 25 ) and the product (tan δ 25 ×MH) is 0.1 or more, The maximum torque MH (N m) and the loss tangent (tan δ) at 60°C 60 ) and the product (tan δ 60 2. The golf club grip according to claim 1, wherein the ratio of the MH to the MH is 0.1 or more.

3. 3. The golf club grip according to claim 2, wherein the inner layer rubber composition forming the inner layer has a maximum torque (MH) of 0.91 N·m or more in a vulcanization curve measured at a vulcanization temperature of 165°C.

4. The inner layer has an elongation at break (Eb) (%) and a density (D) (g / cm 3 2. The grip for golf clubs according to claim 1, wherein a ratio (Eb / D) of Eb to D is 660 or less.

5. The inner layer has a tensile stress (Se) at an elongation of 25% determined by a tensile test. 25 ) (MPa) and density (D) (g / cm 3 ) and the ratio (Se 25 2. The golf club grip according to claim 1, wherein the ratio of the thickness of the groove to the groove width of the golf club is 0.7 to 1.

5.

6. The ratio (E' 25 2. The golf club grip according to claim 1, wherein the ratio of the thickness of the groove to the groove width of the golf club is 0.3 to 10.

5.

7. The ratio (E' 60 2. The golf club grip according to claim 1, wherein the ratio of the thickness of the groove to the groove width of the golf club is 0.3 to 9.

5.

8. 2. The golf club grip according to claim 1, wherein the rubber composition for the inner layer forming the inner layer contains, as base rubber, acrylonitrile-butadiene rubber (NBR) and hydrogenated acrylonitrile-butadiene rubber (HNBR).

9. 9. The golf club grip according to claim 8, wherein the rubber composition for the inner layer contains carbon black and a carbon coupling agent.

10. 9. The golf club grip according to claim 8, wherein the rubber composition for the inner layer forming the inner layer contains elemental sulfur and a morpholine-based sulfur donor compound as vulcanizing agents, and also contains two or more types of vulcanization accelerators.